Method for producing thermoplastic resin extruded foam board
A resin blend of polystyrene and polyethylene terephthalate copolymer with specific properties addresses the challenges of thermal conductivity and moldability in extruded foam boards, achieving low thermal conductivity and stable production with enhanced insulation and moldability.
Patent Information
- Application Number
- JP2023077682
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing methods for manufacturing thermoplastic resin extruded foam boards do not adequately address the need for low thermal conductivity and continuous moldability, particularly in forming plate shapes.
A method involving the extrusion and foaming of a resin melt composed of a mixture of polystyrene resin and polyethylene terephthalate copolymer, with specific ratios and properties, including glass transition temperatures and heat of fusion, to achieve a sea-island structure with the polystyrene as the continuous phase and polyethylene terephthalate as the dispersed phase, enhanced with additives like graphite for improved insulation and moldability.
The method results in an extruded foam board with low thermal conductivity and excellent continuous moldability, maintaining stability during production and preventing edge catching, while maintaining mechanical strength and insulation properties.
Smart Images

Figure 2024162307000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a technique for producing an extruded thermoplastic resin foam plate. [Background technology]
[0002] Thermoplastic resin extruded foam boards (hereinafter, simply referred to as "extruded foam boards") using polystyrene resin as a base resin have excellent heat insulating properties and mechanical strength and are therefore widely used as heat insulating materials. For example, extruded foam boards are suitably used as heat insulating materials for the walls, floors, roofs, and the like of buildings. Extruded foam boards are generally produced by heating and melting a thermoplastic resin in an extruder, and then injecting and kneading a physical foaming agent into the resulting molten material to obtain a foamable molten resin kneaded material, which is extruded into a low pressure region from a flat die or the like attached to the tip of the extruder to foam it, and then forming it into a plate shape using a molding tool.
[0003] In recent years, the demand for energy saving in houses and buildings has been increasing, and there is a demand for extruded foam boards with excellent thermal insulation. In order to improve the thermal insulation of an extruded foam board, it is necessary to reduce the thermal conductivity of the extruded foam board. For example, Patent Document 1 discloses that by using a mixture of polystyrene resin and a specific polyester resin as a base resin, an extruded foam board with low thermal conductivity and excellent long-term thermal insulation can be obtained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-219631 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the technique of Patent Document 1 leaves room for further improvement in terms of obtaining an extruded foam board with low thermal conductivity. Also, there is room for further improvement in the continuous moldability of continuously molding the extruded foam board into a plate. In consideration of the above circumstances, the present invention aims to provide a method for producing an extruded foam board with low thermal conductivity and excellent continuous moldability. [Means for solving the problem]
[0006] [1] A method for producing an extruded thermoplastic resin foam plate, comprising a step of extruding and foaming a foamable resin melt obtained by kneading a thermoplastic resin and a physical foaming agent into a plate, wherein the thermoplastic resin is a mixture of a polystyrene resin and a polyethylene terephthalate copolymer, the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer (polystyrene resin:polyethylene terephthalate copolymer) is 95:5 to 40:60, and the heat of fusion of the polyethylene terephthalate copolymer in a DSC curve obtained under the following <Condition 1> is 1 J / g or less (including 0). <Condition 1>: The polyethylene terephthalate copolymer is used as a test piece, and the test piece is kept at 200°C for 15 minutes and then allowed to stand at 145°C for 4 days, and then heat flux differential scanning calorimetry based on JIS K7122-1987 is performed to obtain a DSC curve at a heating rate of 10°C / min.
[0007] [2] The method for producing an extruded thermoplastic resin foam board according to [1], wherein the polyethylene terephthalate copolymer contains 5 mol % or more and 40 mol % or less of an isophthalic acid component as a dicarboxylic acid component.
[0008] [3] The method for producing an extruded thermoplastic resin foam plate according to [1] or [2], wherein the glass transition temperature Tg1 of the polyethylene terephthalate copolymer satisfies the following formula 1, and the glass transition temperature Tg1 of the polyethylene terephthalate copolymer and the glass transition temperature Tg2 of the polystyrene-based resin satisfy the following formula 2. 65℃≦Tg1≦95℃ (Formula 1) Tg1≦Tg2+10℃ (Formula 2)
[0009] [4] The method for producing an extruded thermoplastic resin foam plate according to any one of [1] to [3], wherein the foamable resin melt contains graphite, and the amount of the graphite added is 0.3 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the thermoplastic resin. Effect of the Invention
[0010] According to the production method of the present invention, an extruded foam board having low thermal conductivity and excellent continuous moldability can be obtained. [Brief description of the drawings]
[0011] [Figure 1] 1 is an electron microscope photograph taken for evaluation of morphology for Example 2. [Diagram 2] 1 is an electron microscope photograph taken for evaluation of morphology for Comparative Example 2. [Diagram 3] 1 is an electron microscope photograph taken for evaluation of morphology for Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Manufacturing method of extruded foam board> The manufacturing method according to the present invention is a method for producing an extruded thermoplastic resin foam board (hereinafter simply referred to as an "extruded foam board"), which includes a step of extruding and foaming a foamable resin molten material obtained by kneading a thermoplastic resin and a physical foaming agent into a plate (hereinafter referred to as the "molding step").
[0013] Specifically, in the manufacturing method according to the present invention, a thermoplastic resin, a flame retardant, and other additives added as required are first melted and kneaded in an extruder under heating to obtain a molten kneaded product, and a physical foaming agent is then pressed into the molten kneaded product, which is then further kneaded to obtain a foamable resin melt. The foamable resin melt is then adjusted to a temperature suitable for foaming, and extruded from the high-pressure extruder through a flat die to a low-pressure region to foam, and then passed through a forming tool (e.g., a forming mold or a forming roll) arranged at the outlet of the flat die to form a plate-shaped extruded foam plate.
[0014] The thermoplastic resin used in the present invention is a mixture of a polystyrene resin and a polyethylene terephthalate copolymer (hereinafter also referred to as a "resin mixture"). The content of the resin mixture in the thermoplastic resin is preferably 80% by mass or more, more preferably 90% by mass or less, and preferably 95% by mass or less, and it is particularly preferable that the thermoplastic resin is substantially composed of only the resin mixture.
[0015] In the cross section of the bubble membrane of the extruded thermoplastic resin foam board, the polystyrene resin or the polyethylene terephthalate copolymer may be a continuous phase, and the other may be a dispersed phase in the continuous phase to form an island structure, or the polystyrene resin and the polyethylene terephthalate copolymer may be a bicontinuous phase structure. It is preferable that the dispersed phase is dispersed in layers in the continuous phase in order to achieve even better long-term heat insulation. From the viewpoint of producing an extruded foam board with a high expansion ratio and a high thickness by the extrusion foaming method, it is preferable that the polystyrene resin is a continuous phase and the polyethylene terephthalate copolymer is a dispersed phase.
[0016] [Polystyrene resin] Examples of the polystyrene resin used in the production method of the present invention include polystyrene, styrene-methyl acrylate copolymers containing 50 mol% or more of styrene unit components, styrene-ethyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-maleic anhydride copolymers, styrene-polyphenylene ether copolymers, styrene-acrylonitrile copolymers, styrene-methylstyrene copolymers, styrene-dimethylstyrene copolymers, styrene-ethylstyrene copolymers, and styrene-diethylstyrene copolymers. Among these, polystyrene can be preferably used. In addition to the styrene unit components, polystyrene may contain unit components derived from a branching agent such as a polyfunctional monomer or a polyfunctional macromonomer. The content of the styrene component units in these copolymers is preferably 60 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more.
[0017] In addition, the polystyrene resin may be a recycled material obtained by recovering used polystyrene resin foam beads molded bodies used in commercial general-purpose polystyrene or fish boxes, or a recycled material obtained by recovering extruded polystyrene resin foam boards (e.g., scraps and crushed materials generated during the manufacture of extruded polystyrene resin foam boards). The recycled material described above can be reused as a polystyrene resin by, for example, crushing and melting the material to form pellets.
[0018] The density of the polystyrene resin is preferably 1000 kg / m 3 That's all. The density of polystyrene resin is approximately 1100 kg / m 3 The density is measured according to the method described in ISO 1183-3.
[0019] For polystyrene-based resins, the heat of fusion in a DSC (Differential Scanning Calorimetry) curve obtained under the following <Condition 1> is preferably 1 J / g or less (including 0), more preferably 0.5 J / g or less, and even more preferably 0 J / g or less.
[0020] <Condition 1> A polystyrene-based resin is used as a test piece, and the test piece is held at 200°C for 15 minutes and then allowed to stand at 145°C for 4 days. Then, heat flux differential scanning calorimetry based on JIS K7122-1987 is performed to obtain a DSC curve at a heating rate of 10°C / min.
[0021] The glass transition temperature Tg2 of the polystyrene resin is preferably 80°C or more and 110°C or less from the viewpoint of the manufacturing stability of the extruded foam board in the resin mixture. From the above viewpoint, the glass transition temperature Tg2 of the polystyrene resin is more preferably 85°C or more and 105°C or less. In particular, when the above-mentioned recycled raw material is used as the polystyrene resin, the glass transition temperature tends to be low. This is because, for example, when the crushed material obtained by crushing the polystyrene resin extruded foam board is used as the recycled raw material, the crushed material is heated, melted, and kneaded through a recycling process, and it is considered that the glass transition temperature of the recycled raw material is lower than that of virgin polystyrene due to the heat in the recycling process. When a polystyrene resin with a low glass transition temperature is used, it is necessary to lower the foaming temperature, extrude and foam, and shape it into a plate shape using a molding tool, and at that time, the width direction end of the extruded foam board is likely to get caught, and there are cases where the extruded foam board cannot be obtained stably. In the manufacturing method of the present invention, by using a specific polyethylene terephthalate copolymer described later in combination, there is an advantage that an extruded foam board can be obtained stably even when the glass transition temperature Tg2 of the polystyrene resin is low. The term "stuck at the widthwise end of the extruded foam plate" refers to the situation where the extruded foam plate is caught at the widthwise end of the molding die and rolled up due to the excessive solidification of a part of the foamed resin melt during extrusion foaming. If the widthwise end of the extruded foam plate is caught, the widthwise end of the extruded foam plate will not be smooth and will have a poor appearance. If the caught state is severe, the widthwise end of the extruded foam plate may crack, and the extruded foam plate may not have the desired widthwise length.
[0022] The glass transition temperature Tg2 of a polystyrene resin is the midpoint glass transition temperature measured based on a DSC curve obtained at a heating rate of 10°C / min using a heat flux differential scanning calorimeter (hereinafter referred to as DSC device) in accordance with "the case where the glass transition temperature is measured after a certain heat treatment" (the heating rate and cooling rate in conditioning the test piece are both 10°C / min) as described in JIS K7121-1987.
[0023] [Polyethylene terephthalate copolymer] The polyethylene terephthalate copolymer used in the production method of the present invention is a polyester resin having dicarboxylic acid component (a) units and diol component (b) units as main component units. The polyethylene terephthalate copolymer has terephthalic acid component units as the dicarboxylic acid component (a) and ethylene glycol component units as the diol component (b) as main component units, but in order to control the crystallinity of the polyethylene terephthalate copolymer, other component units than the terephthalic acid component units as the dicarboxylic acid component (a) and the ethylene glycol component units as the diol component (b) may be used.
[0024] As the dicarboxylic acid component (a) other than terephthalic acid, for example, dicarboxylic acid or its ester-forming derivative can be used. Examples of the ester-forming derivative include ester derivatives such as alkyl esters having about 1 to 4 carbon atoms, salts such as diammonium salts, and acid halides such as dichlorides. Examples of the dicarboxylic acid include aromatic dicarboxylic acids such as isophthalic acid, 2,6-naphthalenedicarboxylic acid, phthalic acid (1,2-benzenedicarboxylic acid), 4,4'-diphenyldicarboxylic acid, 3,4'-diphenyldicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid, or derivatives thereof such as acid anhydrides, or aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, and dodecanedioic acid, or derivatives thereof, or alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, decalindicarboxylic acid, and tetralindicarboxylic acid. The dicarboxylic acid components exemplified above may be used alone or in combination of two or more. As the dicarboxylic acid component other than terephthalic acid contained as the dicarboxylic acid component (a), isophthalic acid is preferable. When the polyethylene terephthalate copolymer contains an isophthalic acid component, the crystallinity of the copolymer decreases and the copolymer is easily dispersed in layers. From the above viewpoints, the content of the isophthalic acid component in the dicarboxylic acid component (a) is preferably 5 mol% or more and 50 mol% or less, more preferably 5 mol% or more and 40 mol% or less, even more preferably 10 mol% or more and 40 mol% or less, and particularly preferably 15 mol% or more and 30 mol% or less. The dicarboxylic acid component (a) is preferably such that the total ratio of the terephthalic acid component and the isophthalic acid component in the dicarboxylic acid component (a) is 90 mol% or more, more preferably 95 mol% or more, and is even more preferably substantially composed of only the terephthalic acid component and the isophthalic acid component.
[0025] As the diol component (b) other than ethylene glycol, aliphatic and aromatic diols (including dihydric phenols) or their ester-forming derivatives can be used, and specifically, aliphatic diols such as propylene glycol, trimethylene glycol, diethylene glycol, 1,4-butanediol, and neopentyl glycol, alicyclic diols such as 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,6-cyclohexanediol, aromatic diols such as bisphenol A, and glycols having a cyclic ether skeleton such as 3,9-bis(1,1-dimethyl-2-hydroxyethyl)2,4,8,10-tetraoxaspiro[5.5]undecane (hereinafter referred to as "spiroglycol") and (1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane (hereinafter referred to as dioxane glycol). The diol components exemplified above may be used alone or in combination of two or more kinds. Among the above diol components, neopentyl glycol and spiro glycol are preferred, and spiro glycol is more preferred. The content of glycol having a cyclic ether skeleton in diol component (b) is preferably 10 mol% or more and less than 30 mol%, more preferably 15 mol% or more and 25 mol% or less. The total ratio of ethylene glycol components and glycol components having a cyclic ether skeleton in diol component (b) is preferably 90 mol% or more, more preferably 95 mol% or more, and further preferably is substantially composed of only ethylene glycol components and glycol components having a cyclic ether skeleton.
[0026] The polyethylene terephthalate copolymer may have its molecular ends blocked with a small amount of component units derived from monofunctional compounds such as benzoic acid, benzoylbenzoic acid, methoxypolyethylene glycol, etc. Also, it may contain a small amount of component units derived from polyfunctional compounds such as pyromellitic acid, trimellitic acid, trimesic acid, glycerin, pentaerythritol, etc.
[0027] The density of the polyethylene terephthalate copolymer is preferably 1200 kg / m 3 More preferably, it is 1250 kg / m 3 More preferably, it is 1280 kg / m 3 That's all. The density of polyethylene terephthalate copolymer is approximately 1350 kg / m 3 The density of the polyethylene terephthalate copolymer is determined according to the method described in ISO 1183-3.
[0028] The air permeability coefficient of the polyethylene terephthalate copolymer is preferably 8.0×10 -17 [mol m / (m 2 s Pa)] or less, and more preferably 5.0 × 10 -17 [mol m / (m 2 s Pa)] or less, and more preferably 4.0 × 10 -17 [mol m / (m 2 The air permeability coefficient is measured using a known gas permeability tester (for example, a gas permeability tester BT-3 manufactured by Toyo Seiki Co., Ltd.) in accordance with JIS K7126-1:2006 Plastics - Films and sheets - Gas permeability test method - Part 1: Differential pressure method under a temperature condition of 23°C ± 2°C.
[0029] For the polyethylene terephthalate copolymer, the heat of fusion of the DSC curve obtained under the above <Condition 1> is 1 J / g or less (including 0). Regarding the above <Condition 1>, the test piece is a polyethylene terephthalate copolymer. When the heat of fusion of the polyethylene terephthalate copolymer is 1 J / g or less, the polyethylene terephthalate copolymer is easily dispersed in layers, and the thermal conductivity can be reduced. From the above viewpoints, the heat of fusion of the polyethylene terephthalate copolymer is preferably 1 J / g or less, and more preferably less than 0.5 J / g.
[0030] In the above <Condition 1>, the test piece is held in an oven at 200°C for 15 minutes to reset the change in the crystallization state of the resin and adjust the condition. After that, the test piece is left in an oven at 145°C for 4 days to promote the crystallization of the resin. In the present invention, it was found that even in the case of low-crystalline resins in which an endothermic peak was not observed by the conventional method of determining the heat amount of the endothermic peak, an endothermic peak may be observed by leaving the resin at 145°C for 4 days. Based on this knowledge, the production of extruded foam boards was studied, and it was found that in the present invention, when a polyethylene terephthalate copolymer having a heat of fusion of more than 1 J / g is used together with a polystyrene-based resin to continuously mold an extruded foam board in <Condition 1>, a snag occurs at the width direction edge, but when a polyethylene terephthalate copolymer having a heat of fusion of 1 J / g or less (including 0) is used together with a polystyrene-based resin to continuously mold an extruded foam board in <Condition 1>, the occurrence of a snag at the width direction edge can be suppressed. In addition, it has been found that an extruded foam board produced by using a polyethylene terephthalate copolymer having a heat of fusion of 1 J / g or less (including 0) together with a polystyrene resin under <Condition 1> can be an extruded foam board with better gas barrier properties than an extruded foam board produced by using a polyethylene terephthalate copolymer having a heat of fusion of more than 1 J / g together with a polystyrene resin under <Condition 1>, because the polyethylene terephthalate copolymer forms a dispersed phase throughout the bubble film. The relationship between the heat of fusion (i.e., the crystalline component of the resin) observed under <Condition 1> and the snagging at the widthwise end of the extruded foam board can be confirmed by cutting a test piece from the widthwise end of the extruded foam board and measuring the heat of fusion under <Condition 1>. In the present invention, it has been confirmed that the greater the heat of fusion determined under <Condition 1> using a test piece cut from the widthwise end of the extruded foam board, the more snagging at the widthwise end of the extruded foam board occurs, and it is considered that snagging at the widthwise end of the extruded foam board is more likely to occur due to the progress of crystallization of the resin during the production of the extruded foam board.A conventional method for determining the endothermic peak calorific value is, for example, a method for determining the endothermic peak calorific value associated with the melting of a resin based on a DSC curve obtained under the following <Condition 2>.
[0031] <Condition 2> "When the heat of fusion is measured after a certain heat treatment" described in JIS K7122-1987 (the heating rate and cooling rate in conditioning the test piece are both 10°C / min) is adopted, and a DSC curve is obtained at a heating rate of 10°C / min using a heat flux differential scanning calorimeter.
[0032] It is preferable that the glass transition temperature Tg1 of the polyethylene terephthalate copolymer satisfies the following formula 1, and that the glass transition temperature Tg1 of the polyethylene terephthalate copolymer and the glass transition temperature Tg2 of the polystyrene resin satisfy the following formula 2. 65℃≦Tg1≦95℃ (Formula 1) Tg1≦Tg2+10℃ (Formula 2) By using a resin with a high glass transition temperature, it becomes easier to obtain an extruded foam board with excellent compression properties. From the above viewpoint, the glass transition temperature Tg1 is preferably 65°C or more and 95°C or less, more preferably 75°C or more and 95°C or less, and even more preferably 80°C or more and 92°C or less, as described above. The glass transition temperature Tg1 of the polyethylene terephthalate copolymer is measured in the same manner as the glass transition temperature Tg2. When the glass transition temperature Tg1 of the polyethylene terephthalate copolymer and the glass transition temperature Tg2 of the polystyrene resin satisfy the formula 2, the polyethylene terephthalate copolymer has excellent compatibility with the polystyrene resin, and the morphology in which the polystyrene resin forms a continuous phase and the polyethylene terephthalate copolymer forms a dispersed phase is easily formed, so that an extruded foam board that can maintain a lower thermal conductivity can be easily obtained. From the above viewpoints, it is more preferable that the glass transition temperature Tg1 of the polyethylene terephthalate copolymer is +8°C or lower than the glass transition temperature Tg2 of the polystyrene resin (i.e., Tg1≦Tg2+8°C or lower), and more preferably +5°C or lower than the glass transition temperature Tg2 of the polystyrene resin (i.e., Tg1≦Tg2+5°C or lower). When the glass transition temperature Tg1 of the polyethylene terephthalate copolymer satisfies the formulas 1 and 2, an extruded foam board having excellent compression properties is easily obtained, and a morphology is formed in which the polystyrene resin forms a continuous phase and the polyethylene terephthalate copolymer forms a dispersed phase, making it easier to obtain an extruded foam board that can maintain a lower thermal conductivity.
[0033] The mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer (polystyrene resin:polyethylene terephthalate copolymer) is 95:5 to 40:60. When the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer is within the above range, an extruded foam board having low thermal conductivity and excellent continuous moldability can be obtained.
[0034] The morphology is such that the polystyrene resin forms the continuous phase and the polyethylene terephthalate copolymer forms the dispersed phase, making it easier to maintain low thermal conductivity, and the foaming state is good, so that even when continuously molded, there is no snagging at the width direction ends and continuous moldability is excellent. From these viewpoints, the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer is preferably 95:5 to 55:45, and more preferably 90:10 to 70:30.
[0035] The thermoplastic resin may contain polymers other than the polystyrene resin and the specific polyethylene terephthalate copolymer described above within the scope in which the object and effect of the present invention are achieved. Examples of other polymers include thermoplastic resins such as polyethylene resins (a mixture of one or more selected from the group consisting of ethylene homopolymers and ethylene copolymers having an ethylene unit content of 50 mol% or more), polypropylene resins (a mixture of one or more selected from the group consisting of propylene homopolymers and propylene copolymers having an ethylene unit content of 50 mol% or more), polyphenylene ether resins, and polymethyl methacrylate, as well as thermoplastic elastomers such as styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers, hydrogenated styrene-isoprene-styrene block copolymers, and styrene-ethylene copolymers.
[0036] [Physical foaming agent] The physical foaming agent used in the production method of the present invention is an organic physical foaming agent or an inorganic physical foaming agent. Examples of the organic physical foaming agent include aliphatic saturated hydrocarbons having 3 to 5 carbon atoms, aliphatic alcohols having 1 to 5 carbon atoms, hydrofluoroolefins (HFOs), ethers, and alkyl chlorides. Examples of the inorganic physical foaming agent include water, carbon dioxide, and nitrogen. These foaming agents can be used alone or in combination of two or more.
[0037] The physical foaming agent used in the manufacturing method of the present invention is preferably one that has zero or very low ozone depletion potential and low global warming potential. On the other hand, considering the long-term heat insulation of the extruded foam insulation board, it is preferable that the physical foaming agent contains a physical foaming agent that has a relatively slow gas permeation rate and is likely to remain in the extruded foam board. As a physical foaming agent that is likely to remain in the extruded foam insulation board, a hydrocarbon-based physical foaming agent that has a relatively slow gas permeation rate relative to the well-known polystyrene resin can be suitably used. In addition, the thermoplastic resin in the present invention is a mixture of a polystyrene resin and a polyethylene terephthalate copolymer, which improves the gas barrier property, so that the gas permeation rate of the physical foaming agent relative to the thermoplastic resin is further slowed, and as a result, the heat insulation performance is further improved.
[0038] In addition to the above physical foaming agents, physical foaming agents having a relatively high gas permeation rate can also be used as the physical foaming agent, and further, a physical foaming agent having a relatively low gas permeation rate and a physical foaming agent having a relatively high gas permeation rate can be used in combination. As physical foaming agents having a relatively high gas permeation rate, which have the effect of reducing the apparent density of the resulting extruded foam board and are effective in stabilizing the heat insulating performance and flame retardant performance of the foam board by being dispersed from the extruded foam board early, aliphatic alcohols having 1 to 5 carbon atoms, ethers, water and carbon dioxide can be suitably used.
[0039] From the viewpoints of safety during the production of the resulting extruded foam board and the flame retardancy of the extruded foam, it is preferable to use, as the physical foaming agent, a mixed foaming agent which combines the above-mentioned physical foaming agent having a relatively slow gas permeation rate with the above-mentioned physical foaming agent having a relatively fast gas permeation rate.
[0040] Specific examples of the above-mentioned hydrocarbon-based physical blowing agent having a relatively slow gas permeation rate include aliphatic hydrocarbons having 3 to 5 carbon atoms, such as propane, normal butane, isobutane, normal pentane, isopentane, and neopentane, alicyclic hydrocarbons having 3 to 6 carbon atoms, such as cyclobutane, cyclopentane, and cyclohexane, and hydrofluoroolefins, such as 1,3,3,3-tetrafluoropropene (HFO-1234ze), 1-chloro-3,3,3-trifluoropropene (HFO-1233zd), 1-chloro-2,3,3,3-tetrafluoropropene (HFO-1224yd), 2,3,3,3-tetrafluoropropene (HFO-1234yf), and 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz). These physical blowing agents can be used alone or in combination of two or more kinds. Among the aliphatic hydrocarbons having 3 to 5 carbon atoms, normal butane, isobutane, normal pentane, isopentane, and cyclopentane are preferred, as they have a slow gas permeation rate and are suitable as a foaming agent, and isobutane is particularly preferred. Among the hydrofluoroolefins, HFO-1233zd is preferred from the viewpoint of being excellent in long-term heat insulation and foaming properties, and of facilitating the production of a foamed board with a low apparent density.
[0041] The amount of the hydrocarbon-based physical blowing agent having a relatively slow gas permeation rate added is preferably 0.5 mol to 1.1 mol, more preferably 0.6 mol to 1 mol, and even more preferably 0.7 mol to 0.9 mol, per 1 kg of thermoplastic resin. By having the amount of the hydrocarbon-based physical blowing agent having a relatively slow gas permeation rate within the above range, an effective amount of the hydrocarbon-based physical blowing agent having a relatively slow gas permeation rate remains, resulting in an extruded foam board having excellent long-term thermal insulation properties.
[0042] The amount of the aliphatic saturated hydrocarbon having 3 to 5 carbon atoms added is, for example, 0.05 mol to 1 mol, preferably 0.1 mol to 0.8 mol, and more preferably 0.2 mol to 0.7 mol, per kg of thermoplastic resin. When the amount of the aliphatic saturated hydrocarbon having 3 to 5 carbon atoms added is within the above range, an extruded foam board having a low apparent density and a high closed cell ratio can be easily obtained.
[0043] The amount of HFO added is, for example, 0.05 mol to 0.5 mol, preferably 0.1 mol to 0.4 mol, and more preferably 0.15 mol to 0.3 mol per kg of thermoplastic resin. If the amount of HFO added is within the above range, an effective amount of HFO remains in the extruded foam plate after extrusion foaming, resulting in an extruded foam plate with longer-term heat insulation properties.
[0044] Examples of aliphatic alcohols having 1 to 5 carbon atoms include methyl alcohol (methanol), ethyl alcohol (ethanol), n-propyl alcohol, isopropyl alcohol, butyl alcohol, sec-butyl alcohol (isobutyl alcohol), tert-butyl alcohol, aryl alcohol, crotyl alcohol, propargyl alcohol, n-amyl alcohol, sec-amyl alcohol, isoamyl alcohol, tert-amyl alcohol, neopentyl alcohol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-2-butanol, etc. Among these, ethanol is preferred because of its excellent safety to the environment and the human body.
[0045] The amount of the aliphatic alcohol having 1 to 5 carbon atoms added is, for example, 0.01 mol or more and 0.5 mol or less, preferably 0.03 mol or more and 0.4 mol or less, and more preferably 0.05 mol or more and 0.25 mol or less, per 1 kg of the thermoplastic resin.
[0046] Examples of the ethers include dimethyl ether, diethyl ether, ethyl methyl ether, di-n-butyl ether, and diisopropyl ether.
[0047] Examples of alkyl chlorides include formate esters such as methyl formate, ethyl formate, and butyl formate, methyl chloride, and ethyl chloride.
[0048] The amount of water added is, for example, 0.05 to 0.5 mol, preferably 0.1 to 0.4 mol, and more preferably 0.15 to 0.25 mol, per kg of thermoplastic resin. By using water within the above range together with the aliphatic saturated hydrocarbon, HFO, and aliphatic alcohol, the expansion ratio of the resulting extruded foam plate can be further improved and the apparent density can be reduced.
[0049] The total amount of the physical foaming agent added is appropriately selected in relation to the desired apparent density, but is preferably 0.8 mol to 2 mol, more preferably 1 mol to 1.5 mol, per kg of thermoplastic resin.
[0050] [Flame retardant] The extruded foam board obtained by the production method of the present invention is used mainly as a heat insulating material for building materials, and flame retardancy is imparted to the thermoplastic resin by blending a flame retardant therewith.
[0051] The flame retardant is not particularly limited, but a brominated flame retardant is preferable. Examples of the brominated flame retardant include brominated butadiene-based polymers such as brominated butadiene-styrene copolymers, tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-S-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-F-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-A-bis(2,3-dibromopropyl ether), tetrabromobisphenol-B-bis(2,3-dibromopropyl ether), tetrabromobisphenol-C-bis(2,3-dibromopropyl ether), tetrabromobisphenol-D ... Examples of the brominated flame retardants include brominated bisphenol compounds such as tetrabromobisphenol-S-bis(2,3-dibromopropyl ether) and tetrabromobisphenol-F-bis(2,3-dibromopropyl ether), and brominated isocyanurates such as tris(2,3-dibromopropyl)isocyanurate, mono(2,3,4-tribromobutyl)isocyanurate, di(2,3,4-tribromobutyl)isocyanurate, and tris(2,3,4-tribromobutyl)isocyanurate. These brominated flame retardants may be used alone or in combination of two or more.
[0052] In addition to the bromine-based flame retardants, nitrogen-containing cyclic compounds such as cresyl di-2,6-xylenyl phosphate, antimony trioxide, diantimony pentoxide, ammonium sulfate, zinc stannate, cyanuric acid, pentabromotoluene, isocyanuric acid, triallyl isocyanurate, melamine cyanurate, melamine, melam, and melem, silicone-based compounds, inorganic compounds such as boron oxide, zinc borate, and zinc sulfide, phosphorus-based compounds such as phosphate esters represented by triphenyl phosphate, red phosphorus, ammonium polyphosphate, phosphazene, and hypophosphites, and the like can be used in combination.
[0053] Among the flame retardants exemplified above, it is preferable to use a flame retardant containing one or more of brominated butadiene-styrene copolymer, tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), and tris(2,3-dibromopropyl)isocyanurate, because it can impart high flame retardancy to the extruded foam board. Among these, it is more preferable to use a flame retardant containing a brominated butadiene-styrene copolymer, or a flame retardant using a combination of tetrabromobisphenol A-bis(2,3-dibromopropyl ether) and tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), because it can impart high flame retardancy, it is difficult to decompose the polystyrene resin during extrusion, and it is easy to stably obtain an extruded foam board even in the case of a low apparent density (high expansion ratio) and a large cross-sectional area.
[0054] The amount of the flame retardant is preferably 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 2 to 7 parts by mass, relative to 100 parts by mass of the thermoplastic resin, since the flame retardant can impart high flame retardancy to the extruded foam board and can also suppress deterioration of extrusion foamability and mechanical properties. If the amount of the flame retardant is within the above range, the flame retardant does not inhibit foamability, and an extruded foam board that has flame retardancy can be obtained.
[0055] [Flame retardant synergist] In the manufacturing method of the present invention, in order to further improve the flame retardancy of the extruded foam board, a flame retardant auxiliary can be used in combination with the above flame retardant. Examples of the flame retardant auxiliary include one or more selected from diphenylalkanes and diphenylalkenes such as 2,3-dimethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 2,4-diphenyl-4-methyl-1-pentene, and 2,4-diphenyl-4-ethyl-1-pentene, and polyalkylated aromatic compounds such as poly-1,4-diisopropylbenzene.
[0056] The blending amount of the flame retardant auxiliary is preferably 0.01 part by mass or more and 1 part by mass or less, and more preferably 0.05 part by mass or more and 0.5 part by mass or less, based on 100 parts by mass of the resin mixture.
[0057] [Radiation suppressant] In the production method of the present invention, a radiation suppressor can be added to the foamable resin melt composition in order to improve the heat insulating property by suppressing heat transfer due to infrared radiation.
[0058] The amount of the radiation suppressor added to the extruded foam board is, for example, 0.3 parts by mass or more and 10 parts by mass or less, preferably 0.5 parts by mass or more and 8 parts by mass or less, and more preferably 1.2 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin (A), from the viewpoint of improving the heat insulation while suppressing the influence on the production stability of the extruded foam board.
[0059] As the radiation suppressant, for example, graphite can be added. Examples of graphite include flake graphite, scaly graphite, artificial graphite, and earthy graphite, and it is preferable to use graphite whose main component is flake graphite. As described later, it is preferable to use graphite as a master batch in which the graphite is mixed at a high concentration with a polystyrene resin. Graphite having a fixed carbon content of 90% or more is preferable because it has good workability when producing a master batch and has an excellent effect of improving the heat insulation of the resulting extruded foam board. In order to further improve the heat insulation of the extruded foam board, graphite having a fixed carbon content of 93% or more is more preferable, and graphite having a fixed carbon content of 95% or more is even more preferable. The fixed carbon content of graphite refers to a value measured by the method described in JIS M8511:2014.
[0060] The amount of graphite added is, for example, 0.3 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the thermoplastic resin. When the amount of graphite added is within the above range, the heat insulation is improved, and an extruded foam board with a desired low thermal conductivity can be obtained. From the above viewpoints, the amount of graphite added is preferably 0.3 parts by mass or more and 3 parts by mass or less, more preferably 0.4 parts by mass or more and 2.5 parts by mass or less, and even more preferably 0.4 parts by mass or more and less than 1 part by mass relative to 100 parts by mass of the resin mixture.
[0061] In the case where the resin is a mixture, the addition of graphite tends to result in finer bubbles, making it difficult to produce an extruded foam plate. In contrast, the production method according to the present invention has the advantage that the mixture contains the specific polyethylene terephthalate copolymer described above, which provides excellent foaming stability, and therefore extruded foam plates can be stably produced even if the mixture contains graphite.
[0062] In order to further improve the heat insulating properties, the foamable resin melt composition may contain a component other than graphite as a radiation suppressant.
[0063] Examples of components other than graphite include one or more selected from metal oxides such as titanium oxide, metals such as aluminum, ceramics, carbon black, infrared shielding pigments, hydrotalcite, etc. The amount of each of these components added is preferably 0.5 parts by mass or more and 5 parts by mass or less, and more preferably 1 part by mass or more and 4 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin.
[0064] [Foam regulator] In the production method of the present invention, it is preferable to mix a cell regulator with the thermoplastic resin to form a foamable resin melt.
[0065] The bubble adjusting agent may be one or a mixture of two or more of inorganic powders such as talc, kaolin, mica, silica, calcium carbonate, barium sulfate, titanium oxide, clay, aluminum oxide, bentonite, diatomaceous earth, etc. Among these, talc is preferred because it is easy to adjust the bubble size and to reduce the bubble size without impairing flame retardancy, and fine talc with a 50% particle size (light transmission centrifugal sedimentation method) of 0.1 to 20 μm is particularly preferred, with fine talc with a 50% particle size (light transmission centrifugal sedimentation method) of 0.5 to 15 μm being preferred.
[0066] The amount of the bubble regulator added varies depending on the type of regulator, the desired bubble diameter, etc., but when talc is used as the bubble regulator, the amount is preferably 0.02 parts by mass or more and 7 parts by mass or less, more preferably 0.05 parts by mass or more and 5 parts by mass or less, and even more preferably 0.1 parts by mass or more and 3 parts by mass or less, per 100 parts by mass of the thermoplastic resin.
[0067] [Heat stabilizer] The heat stabilizer can improve the heat stability of the bromine-based flame retardant by blending it with raw materials or scraps when producing an extruded foam board or when recycling scraps of an extruded foam board to repelletize them. Examples of the heat stabilizer include one or more heat stabilizers selected from bisphenol-type epoxy compounds and novolac-type epoxy compounds such as DIC's EPICLON series, hindered phenol compounds such as n-octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and phosphite compounds such as (bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol-diphosphite).
[0068] In the manufacturing method of the present invention, as a method of blending a flame retardant and other additives with a thermoplastic resin, a method of feeding a predetermined ratio of the flame retardant and other additives together with the thermoplastic resin to a feed section provided upstream of the extruder and kneading them in the extruder can be adopted. In addition, a method of feeding the flame retardant and other additives into the molten resin from a feed section provided midway through the extruder can also be adopted. Specifically, a method of feeding a dry blend of the flame retardant, other additives, and the thermoplastic resin to the extruder and melt-kneading it, a method of feeding a melt-kneaded product obtained by kneading the flame retardant, other additives, and the thermoplastic resin with a kneader or the like to the extruder, a method of preparing a master batch in which a high concentration of the flame retardant and other additives is blended in advance with a polystyrene-based resin, feeding the master batch to the extruder and melt-kneading it with the thermoplastic resin, etc. can be adopted. In particular, from the viewpoint of dispersibility, it is preferable to adopt a method of preparing a flame retardant master batch and feeding it to the extruder.
[0069] In the manufacturing method of the present invention, other known additives can be appropriately blended into the thermoplastic resin as necessary. Examples of other additives include various additives such as colorants such as pigments or dyes, heat stabilizers, and fillers. The total blending amount of other additives is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, per 100 parts by mass of the thermoplastic resin.
[0070] In the molding step of the manufacturing method of the present invention, as described above, a foamable resin melt obtained by melting a thermoplastic resin, additives such as a radiation suppressant and a flame retardant, and a physical foaming agent is extruded and foamed under atmospheric pressure, and then shaped into a plate using a molding tool, thereby obtaining an extruded foam plate.
[0071] <Physical properties of extruded foam board> The extruded foam board obtained by the production method of the present invention will now be described.
[0072] [Cross-section area and dimensions] The extruded foam board according to the present invention is in the form of a plate. The cross-sectional area of the extruded foam board perpendicular to the extrusion direction is 100 cm 2 It is preferable that the length is more than 200 cm. 2 The upper limit of the cross-sectional area perpendicular to the extrusion direction of the extruded foam plate is, for example, 1500 cm 2 The cross-sectional area perpendicular to the extrusion direction refers to the area of the cross section of the extruded foam board perpendicular to the extrusion direction.
[0073] When the extruded foam board is used as a heat insulating material, the thickness of the extruded foam board is preferably 10 mm or more and 150 mm or less, and more preferably 15 mm or more and 120 mm or less.
[0074] The width of the extruded foam plate is preferably 800 mm or more, more preferably 900 mm or more, and the upper limit of the width of the extruded foam plate is, for example, 1200 mm.
[0075] [Apparent Density] The apparent density of the extruded foam board is preferably 20 kg / m 3 More than 50kg / m3 More preferably, it is 30 kg / m or less. 3 More than 45kg / m 3 When the apparent density is within the above range, the extruded foam board has sufficient mechanical strength and is lightweight, and can be suitably used, for example, as a heat insulating material. The apparent density is determined by measuring the mass of the extruded foam board and dividing the mass by the volume.
[0076] [Closed bubble rate] The closed cell ratio of the extruded foam board is preferably 85% or more, more preferably 90% or more, and even more preferably 93% or more. When the closed cell ratio is within the above range, the extruded foam board can have excellent long-term heat insulation properties and mechanical strength.
[0077] The closed cell ratio of the extruded foam board is measured according to procedure C of ASTM-D2856-70 using a Toshiba Beckman Co., Ltd. air comparison type specific gravity meter Model 930 (a cut sample without a molded skin cut into a size of 25 mm x 25 mm x 20 mm from the extruded foam board is placed in a sample cup and measured. However, if the thickness is too thin to cut a 20 mm cut sample in the thickness direction, for example, two cut samples of a size of 25 mm x 25 mm x 10 mm may be placed in the sample cup at the same time and measured.) using the true volume Vx of the extruded foam board (cut sample) and calculate the closed cell ratio S (%) using the following formula (1), and obtain the average value of N = 3.
[0078] S(%)=(Vx-W / ρ)×100 / (VA-W / ρ)···(1) Vx: True volume of cut sample (cm 3 ) (This corresponds to the sum of the volume of the resin that constitutes the cut sample of the extruded foam board and the total volume of the air bubbles in the closed cell portion of the cut sample.) VA: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used for measurement 3 ) W: Total weight of cut sample used for measurement (g) ρ: Density of the resin that composes the extruded foam board (g / cm3 )
[0079] [10% compressive strength] Compressive strength is measured by the following method. From the center of the width of the extruded foam board, a rectangular parallelepiped shape of 25 mm in the extrusion direction, 25 mm in the width direction, and 25 mm thick (excluding the skin layer) is cut out. In this case, the center of the width of the extruded foam board and the center of the width of the test piece are aligned. Next, the test piece is compressed at a speed of 10% x T mm / min (where T is the initial thickness of the test piece), and the maximum force reached within a deformation rate of 10% based on JIS K7220:2006 is calculated, and the compressive strength is calculated by dividing this by the pressure-receiving area of the test piece. The above operation is performed for each of the extrusion direction, width direction, and thickness direction of the test piece, and the arithmetic average value is taken as the 10% compressive strength.
[0080] [Thermal Conductivity] (44 days later) The thermal conductivity of the extruded foam board 44 days after production is preferably 0.029 W / m·K or less, more preferably 0.028 W / m·K or less, and even more preferably 0.025 W / m·K or less.
[0081] (after 250 days) The thermal conductivity of the extruded foam board 250 days after production is preferably 0.029 W / m·K or less, more preferably 0.028 W / m·K or less, and even more preferably 0.027 W / m·K or less.
[0082] The thermal conductivity of the extruded foam board can be measured based on the heat flow meter method described in JIS A1412-2:1999 (one test piece, symmetrical configuration, high temperature side 38°C, low temperature side 8°C, average temperature 23°C). EXAMPLES
[0083] The present invention will be described in detail with reference to examples, but the present invention is not limited to the examples.
[0084] In the examples and comparative examples, extruded foam boards were produced as follows. In the examples and comparative examples, a mixture of a polyethylene terephthalate copolymer shown in Table 1 and a polystyrene-based resin shown in Table 2 was used as the thermoplastic resin.
[0085] The air permeability coefficient, crystallinity, and glass transition temperature were measured for the polyethylene terephthalate copolymers in Table 1 and the polystyrene resins in Table 2. In Table 1, "TPA" is terephthalic acid, "IPA" is isophthalic acid, "EG" is ethylene glycol, "SPG" is spiro glycol, "CHDM" is 1,4-cyclohexanedimethanol, and "NPG" is neopentyl glycol.
[0086] Air permeability coefficient [mol m / (m 2 ·s·Pa) was measured using a gas permeability tester BT-3 manufactured by Toyo Seiki Co., Ltd., in accordance with JIS K7126-1:2006 Plastics - Films and sheets - Gas permeability test method - Part 1: Differential pressure method, at a temperature of 23±2°C.
[0087] Regarding crystallinity, the heat of fusion [J / g] of the DSC curve obtained as follows was measured. For the heat of fusion (condition 1), a polyethylene terephthalate copolymer or a polystyrene resin was used as a test piece, and the heat of fusion was obtained from the DSC curve obtained under the following <condition 1>. Regarding the end temperature of the measurement, if a melting peak was detected, the sample was heated to a temperature 30°C higher than the end of the melting peak to obtain a DSC curve. On the other hand, if a melting peak was not detected, the sample was heated to 250°C, and a DSC curve was obtained with 250°C as the end temperature.
[0088] <Condition 1>: A polyethylene terephthalate copolymer or a polystyrene-based resin was used as a test piece, and the test piece was held at 200°C for 15 minutes and then allowed to stand at 145°C for 4 days. Then, heat flux differential scanning calorimetry based on JIS K7122-1987 was performed, and the test piece was heated at a heating rate of 10°C / min to obtain a DSC curve.
[0089] The heat of fusion (condition 2) was determined from the DSC curve obtained under the following <condition 2> using polyethylene terephthalate copolymer or polystyrene resin as a test piece. Regarding the end temperature of the measurement, if a melting peak was detected, the sample was heated to a temperature 30°C higher than the end of the melting peak to obtain a DSC curve. On the other hand, if no melting peak was detected, the sample was heated to 250°C, and a DSC curve was obtained with 250°C as the end temperature.
[0090] <Condition 2>: "When the heat of fusion is measured after a certain heat treatment" described in JIS K7122-1987 (the heating rate and cooling rate in conditioning the test piece are both 10°C / min) was adopted, and a DSC curve was obtained at a heating rate of 10°C / min using a heat flux differential scanning calorimeter.
[0091] The glass transition temperature [°C] was determined according to "the case where the glass transition temperature is measured after a certain heat treatment" as described in JIS K7121 (1987) (the heating rate and cooling rate in the conditioning of the test piece are both 10°C / min), using a heat flux differential scanning calorimeter (hereinafter referred to as DSC device). The midpoint glass transition temperature measured based on a DSC curve obtained at a heating rate of 10°C / min was taken as the glass transition temperature in the present invention.
[0092] [Table 1]
[0093] [Table 2]
[0094] An extruded foam board was manufactured using the components shown in Table 3. Details of each component are as follows. The polyethylene terephthalate copolymer and polystyrene resin are as shown in Tables 1 and 2.
[0095] [Flame retardant] GR134BG: tetrabromobisphenol A bis(2,3-dibromo-2-methylpropyl ether) ("SR-130" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), tetrabromobisphenol A bis(2,3-dibromopropyl ether) ("SR-720" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), GR134BG (SR-130 / SR-720) = 60 / 40 (mass ratio) [Radiation suppressant] Graphite: manufactured by Resino Color Kogyo Co., Ltd., product name: SBF-T-1683, flake graphite powder, average particle size 17 μm Titanium oxide: "JR-405" manufactured by Teika Co., Ltd., primary particle size (d50) = 0.2 μm [bubble adjuster] Talc: Matsumura Sangyo Co., Ltd., product name: High Filler #12, particle size (d50) 7.5 μm [Physical foaming agent] i-Bu: Isobutane: Mitsui Chemicals HFO-1233zd: 1-chloro-3,3,3-trifluoropropene (manufactured by Honeywell, product name "Solstice 1233zd") DME: Dimethyl ether: Mitsubishi Gas Chemical Company, Inc. Ethanol: Yamaichi Chemical Industry Co., Ltd. water
[0096] Specifically, a thermoplastic resin (polystyrene resin + polyethylene terephthalate copolymer), a radiation suppressant, a bubble control agent, and a flame retardant master batch were fed to a first extruder in the formulation shown in Table 3, heated to 200°C and kneaded, and a physical foaming agent was fed from a physical foaming agent injection port provided in the first extruder in the amount shown in Table 3 at each foaming agent injection pressure, and further kneaded to form a foamable resin melt.
[0097] Next, the obtained foamable resin melt is transferred to a second extruder to adjust the resin temperature, and then extruded into a guider at a discharge rate of 400 kg / hr. The resin is foamed while passing through the guider to be molded (shaped) into a plate. The length is then adjusted by cutting to produce an extruded foam plate (width 1000 mm, length 1820 mm, thickness 30 mm, cross-sectional area perpendicular to the extrusion direction: 300 cm). 2 ) was manufactured.
[0098] For the examples and comparative examples, the closed cell ratio, apparent density, 10% compressive strength, thermal conductivity (after 44 days and 250 days), morphology, continuous moldability, and crystallization state of the product ends were evaluated as follows.
[0099] [Closed bubble rate] The closed cell ratio of the extruded foam board was measured according to procedure C of ASTM-D2856-70 using a Toshiba Beckman Co., Ltd. air comparison type specific gravity meter Model 930 (a cut sample without a molded skin cut into a size of 25 mm x 25 mm x 20 mm from the extruded foam board was placed in a sample cup and measured. However, if the thickness is too thin to cut a 20 mm cut sample in the thickness direction, for example, two cut samples with a size of 25 mm x 25 mm x 10 mm may be placed in the sample cup at the same time for measurement.) and the true volume Vx of the extruded foam board (cut sample) was used to calculate the closed cell ratio S (%) according to the following formula (1), and the average value of N = 3 was obtained.
[0100] S(%)=(Vx-W / ρ)×100 / (VA-W / ρ)···(1) Vx: True volume of cut sample (cm 3 ) (This corresponds to the sum of the volume of the resin that constitutes the cut sample of the extruded foam board and the total volume of the air bubbles in the closed cell portion of the cut sample.) VA: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used for measurement 3 ) W: Total weight of cut sample used for measurement (g) ρ: Density of the resin that composes the extruded foam board (g / cm 3 )
[0101] [Apparent Density] The apparent density of the foam board was determined by the following method: A rectangular parallelepiped sample of 50 mm length × 50 mm width × 20 mm thickness was cut from the position where the obtained foam board was divided into two equal parts in the length direction and from the center and both ends in the width direction of the obtained foam board, and the mass was measured and the apparent density of each sample was determined by dividing the mass by the volume, and the arithmetic average of the masses was regarded as the apparent density.
[0102] [10% compressive strength] The compressive strength is a value measured by the following method. From the center of the width direction of the extruded foam plate, a rectangular parallelepiped shape of 25 mm in the extrusion direction, 25 mm in the width direction, and 25 mm in thickness (excluding the skin layer) was cut out. In this case, the center of the width direction of the extruded foam plate and the center of the width direction of the test piece were made to coincide. Next, the compression speed of this test piece was set to 10% x Tmm / min (where T is the initial thickness of the test piece), and the maximum force reached within a deformation rate of 10% based on JIS K7220:2006 was calculated, and this was divided by the pressure-receiving area of the test piece to calculate the compressive strength. The above operation was performed for each of the extrusion direction, width direction, and thickness direction of the test piece, and the arithmetic average value thereof was determined as the 10% compressive strength.
[0103] [Thermal Conductivity] The thermal conductivity of the extruded foam board was measured by cutting a test piece without the skin, measuring 200 mm long x 200 mm wide x 10 mm, from the extruded foam board immediately after production and storing it in an atmosphere of 23°C and 50% humidity, according to the flat plate heat flow meter method described in JIS A1412-2:1999 (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C).
[0104] The thermal conductivity measurements for 44 and 250 days after manufacture were taken from extruded foam boards subjected to test method A of the accelerated long-term change test for thermal resistance in accordance with JIS A1486:2014. Specifically, the thermal conductivity measured 7 days after manufacture using a sample obtained by slicing a 25 mm-thick extruded foam board to a thickness of 10 mm was deemed equivalent to the thermal conductivity of the extruded foam board 44 days after manufacture, and the thermal conductivity measured 40 days after manufacture was deemed equivalent to the thermal conductivity of the extruded foam board 250 days after manufacture.
[0105] [Morphology] An ultrathin section was prepared from the extruded thermoplastic resin foam, and the morphology of the cross section of the bubble membrane was visually confirmed using a transmission electron detector attached to a scanning electron microscope. Specifically, the extruded foam cut to an appropriate size was first embedded in a UV-curable acrylate resin. After embedding, a surface perpendicular to the thickness direction was cut out using a glass knife or the like. The embedded resin piece with the cross section of the extruded foam exposed was fixed on a glass plate. The opening of an Erlenmeyer flask containing several ml of 0.2% RuO4 aqueous solution was blocked with the glass plate on which the embedded resin piece was fixed so that the embedded resin piece was inside the Erlenmeyer flask, and the flask was sealed at room temperature. The embedded resin piece was exposed to the generated RuO4 vapor and electronically stained for 15 minutes. An ultrathin section of the foam with a thickness of about 0.1 μm was cut out from the embedded resin piece with the cross section of the extruded foam exposed using a diamond knife or the like. The electronically stained ultrathin section of the foam was photographed using a transmission electron detector attached to a scanning electron microscope. In the electron microscope photograph, the polystyrene resin portion appears white, and the polyethylene terephthalate copolymer portion appears black.
[0106] The observation conditions using an electron microscope were as follows. Scanning electron microscope: Hitachi High-Tech Corporation's field emission scanning electron microscope "SU8220" Acceleration voltage: 30 kV Electron staining: ruthenium tetroxide Magnification: 5000x
[0107] The dispersion state (morphology) of the polyethylene terephthalate copolymer was evaluated according to the following criteria. ◎: Polyethylene terephthalate copolymer forms a dispersed phase throughout the bubble film. ◯: The polyethylene terephthalate copolymer forms a dispersed phase in most of the bubble film, but granular parts are observed in some parts. Δ: Polyethylene terephthalate copolymer is unevenly distributed in the form of particles.
[0108] [Continuous molding] The continuous moldability was evaluated visually according to the following criteria. ⊚: The foaming state was extremely good, and even when continuously molded, an extruded foam board with no catches at the width direction edges could be stably molded. ◯: The foaming state was good, but the width direction edges of the extruded foam plate were occasionally caught during continuous molding. Δ: The foaming state was slightly unstable, and catches were occasionally observed at the width direction edges of the extruded foam plate during continuous molding. ×: The foaming state was unstable, and the edges of the extruded foam plate in the width direction were frequently caught, making continuous molding impossible.
[0109] [Crystallization state] The degree of crystallization of the polyethylene terephthalate copolymer at the end of the extruded foam plate was evaluated by measuring the heat of fusion of the extruded foam plate. The heat of fusion of the extruded foam plate [J / g] was calculated from the melting peak area of the DSC curve and the sample weight by randomly cutting 3-5 mg test pieces from the end of the width direction of the extruded foam plate including the skin layer, and performing heat flux differential scanning calorimetry based on JIS K7122-1987, heating from 30°C to 250°C at a heating rate of 10°C / min.
[0110] [Table 3]
[0111] As can be seen from Table 3, in comparison with Comparative Examples 1 to 4, Examples 1 to 5 had low thermal conductivity and excellent continuous moldability.
[0112] [Table 4]
[0113] As can be seen from Table 4, in Example 6, Vylon 270 (density 1260 kg / m) was used as a polyethylene terephthalate copolymer. 3 , air permeability coefficient 1.3×10 -17 [mol m / (m 2 An extruded foam board was obtained in the same manner as in Example 2, except that 30 mass% of Vylon 270 (Hexafluoroethylene terephthalate / isophthalic acid), heat of fusion (Condition 1) and (Condition 2) both 0 J / g, glass transition temperature 68° C.) was used. Vylon 270 is a resin commercially available from Toyobo, and is known to contain dicarboxylic acid components (terephthalic acid / isophthalic acid) and diol components (ethylene glycol / neopentyl glycol). The above results confirmed that the effects of the present invention can be obtained even when neopentyl glycol is used as the diol component.
[0114] 1, 2 and 3 show electron microscope photographs taken for the evaluation of morphology for Example 2, Comparative Example 2 and Comparative Example 4, respectively. In Example 2, the polyethylene terephthalate copolymer (black part) was dispersed throughout the entire cross section and was dispersed in layers. As described above, it can be said that an extruded foam board with low thermal conductivity and excellent heat insulation was obtained by dispersing the polyethylene terephthalate copolymer. On the other hand, in Comparative Example 2, the polyethylene terephthalate copolymer formed a dispersed phase in most of the bubble film compared to Example 2, but granular parts were observed in some parts. In Comparative Example 4, the polyethylene terephthalate copolymer (black part) was localized in granular form and was not dispersed in layers.
[0115] As explained above, in the present invention, by using a specific polyethylene terephthalate copolymer in combination with a polystyrene-based resin, an extruded foam board having low thermal conductivity and excellent continuous moldability can be produced.
[0116] Next, the recycled raw material was also used as the polystyrene resin to produce extruded foam boards according to Example 7 and Comparative Example 5. The recycled raw material (recycled PS) had a density of 1050 kg / m 3 A polystyrene resin with a heat of fusion of 0 J / g and a glass transition temperature of 96°C under condition 1 was used. The glass transition temperature of the resin with HP600 / recovered PS=30 / 70 was 98°C.
[0117] [Table 5]
[0118] In Comparative Example 5, recycled raw material (recycled PS) was used, and the dispersion state of the polyethylene terephthalate copolymer was poor, making it difficult to stably produce extruded foam boards, and continuous moldability was poor. In contrast, in Example 7, despite using recycled raw material (recycled PS), a specific polyethylene terephthalate copolymer was used, which resulted in excellent dispersion state of the polyethylene terephthalate copolymer, good continuous moldability, and stable production of extruded foam boards.
Claims
1. A method for producing an extruded thermoplastic resin foam plate, comprising the steps of extruding and foaming a foamable resin melt obtained by kneading a thermoplastic resin and a physical foaming agent into a plate shape, The thermoplastic resin is a mixture of a polystyrene resin and a polyethylene terephthalate copolymer, the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer (polystyrene resin:polyethylene terephthalate copolymer) is 95:5 to 40:60, and the polyethylene terephthalate copolymer has a heat of fusion of 1 J / g or less (including 0) in a DSC curve obtained under the following <Condition 1>. <Condition 1>: A polyethylene terephthalate copolymer is used as a test piece, and the test piece is held at 200°C for 15 minutes and then allowed to stand at 145°C for 4 days. Then, heat flux differential scanning calorimetry based on JIS K7122-1987 is performed to obtain a DSC curve at a heating rate of 10°C / min.
2. 2. The method for producing an extruded thermoplastic resin foam board according to claim 1, wherein the polyethylene terephthalate copolymer contains 5 mol % or more and 40 mol % or less of isophthalic acid as a dicarboxylic acid component.
3. 3. The method for producing an extruded thermoplastic resin foam plate according to claim 1, wherein the glass transition temperature Tg1 of the polyethylene terephthalate copolymer satisfies the following formula 1, and the glass transition temperature Tg1 of the polyethylene terephthalate copolymer and the glass transition temperature Tg2 of the polystyrene resin satisfy the following formula 2. 65℃≦Tg1≦95℃ (Formula 1) Tg1≦Tg2+10℃ (Formula 2)
4. 3. The method for producing an extruded thermoplastic resin foam plate according to claim 1, wherein the foamable resin melt contains graphite, and the amount of the graphite added is 0.3 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the thermoplastic resin.
Citation Information
Patent Citations
Heat insulation plate of extruded thermoplastic resin foam
JP2011219631A