Bamboo powder-containing propylene resin composition and molded product
A propylene resin composition with a highly stereoregular propylene polymer and bamboo powder addresses the need for improved heat-resistant stiffness and low specific gravity, enhancing the durability and weight reduction of automotive parts.
Patent Information
- Application Number
- JP2023078632
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing propylene-based resin compositions lack sufficient heat-resistant stiffness while maintaining low specific gravity, which is essential for reducing vehicle weight and carbon emissions.
A propylene resin composition containing a highly stereoregular propylene polymer and bamboo powder, with specific particle size and content ratios, to achieve low specific gravity and high heat distortion temperature.
The composition achieves a balance of low specific gravity and excellent heat-resistant rigidity, suitable for automotive and other applications requiring lightweight, durable materials.
Smart Images

Figure 2024162761000001 
Figure 2024162761000002 
Figure 2024162761000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a propylene-based resin composition having a low specific gravity and excellent heat resistance and rigidity, and a molded article containing said composition. [Background technology]
[0002] Propylene-based polymers have a low specific gravity and excellent moldability and recyclability, and are therefore used in a variety of fields, including daily necessities, kitchen utensils, packaging films, home appliances, machine parts, electrical parts, and automobile parts. In automobile parts, the weight of vehicles tends to increase with improvements in automobile safety, livability, and comfort, and an increase in IT equipment, and so the proportion of propylene-based resin compositions containing propylene-based polymers used is increasing. In particular, propylene-based resin compositions consisting of propylene-based polymers, talc, and ethylene-α-olefin copolymer rubber are widely used in automobile interior and exterior parts such as bumpers and instrument panels, due to their excellent balance between rigidity and impact resistance (Patent Document 1, Patent Document 2).
[0003] Here, in recent years, in the context of global warming, efforts toward carbon neutrality have been emphasized, and low CO2 emissions are being sought from the perspective of LCA (Life Cycle Assessment) in propylene-based resin compositions as well. In order to reduce CO2 emissions from the raw material procurement to manufacturing process and as a lightweight filler, fillers derived from natural plants can be used, one of which is bamboo. In particular, bamboo powder obtained by crushing bamboo is considered to be more advantageous in terms of low CO2 emissions in the filler manufacturing process than bamboo fiber, which includes a fiber extraction process. As an example of using bamboo powder as a filler, a manufacturing method for a resin composition consisting of a propylene polymer and bamboo powder has been disclosed (Patent Document 3). However, the effect of improving heat resistance rigidity (heat distortion temperature) is insufficient, and there is a demand for the development of a propylene-based resin composition with low specific gravity and excellent heat resistance rigidity. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 3-250040 [Patent Document 2] Japanese Patent Application Publication No. 7-053843 [Patent Document 3] JP 2019-199099 A Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the above-mentioned conventional techniques, an object of the present invention is to provide a propylene-based resin composition having a low specific gravity and a high heat distortion temperature, and a molded article formed using the propylene-based resin composition. [Means for solving the problem]
[0006] As a result of intensive research to solve the above problems, the present inventors have found that a propylene-based resin composition containing a highly stereoregular propylene-based polymer and bamboo powder can provide a low specific gravity and a high heat distortion temperature, and have thus completed the present invention.
[0007] [1] 20 to 98% by mass of a propylene-based polymer (A) satisfying the following requirements (1) and (2); 0 to 50% by mass of an elastomer (B); 1 to 20 mass% of a modified propylene resin (C); 1 to 49% by mass of bamboo powder (D) having an average particle size (particle size at which the cumulative volume is 50% as measured by a laser diffraction scattering method in accordance with JIS R1629) of 10 μm or more and 2000 μm or less, and a content of particles with a particle size of 600 μm or more (weight ratio of sieve residue with 600 μm openings in a sieve analysis method in accordance with JIS K0069) of 30% or more; A propylene-based resin composition comprising the above components (A), (B), (C) and (D) in total being 100 mass%. (1) Melt flow rate (MFR) (ASTM D1238, 230°C, 2.16 kg load) is 0.5 to 1000 g / 10 min; (2) The melting point (Tm) measured by differential scanning calorimetry (DSC) is 150°C to 170°C. [2] The propylene-based resin composition according to item [1], wherein the propylene-based polymer (A) further satisfies the following requirements (3) and (4): (3) the isotactic mesopentad fraction (mmmm) is greater than 97.0% and less than or equal to 99.9%; (4) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is 4.0 to 20.0. [3] A molded article comprising the propylene-based resin composition according to items [1] or [2]. Effect of the Invention
[0008] According to the present invention, a bamboo powder-containing propylene-based resin composition having a low specific gravity and excellent heat resistance and rigidity can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below. [Propylene-based resin composition] The propylene-based resin composition of the present invention (hereinafter, simply referred to as the "composition of the present invention") contains 20-98% by mass of a propylene-based polymer (A), 0-50% by mass of an elastomer (B), 1-20% by mass of a modified propylene resin (C), and 1-49% by mass of bamboo powder (D) having an average particle size (particle size at which the cumulative volume is 50% as measured by a laser diffraction scattering method in accordance with JIS R1629) of 10 μm or more and 2000 μm or less, and a content of particles with a particle size of 600 μm or more (weight ratio of sieve residue with 600 μm opening in a sieve test method in accordance with JIS K0069) of 30% or more (wherein the total of the components (A), (B), (C) and (D) is 100% by mass). Each component will be described below.
[0010] [Propylene-based polymer (A)] The propylene polymer (A) satisfies the following requirements (1) and (2).
[0011] <Requirement (1)> The MFR (ASTM D1238, 230°C, 2.16 kg load) is 0.5 to 1000 g / 10 min, preferably 1.0 to 500 g / 10 min, more preferably 5 to 200 g / 10 min. When the MFR is within the above range, the composition of the present invention has an excellent balance between moldability and mechanical strength.
[0012] <Requirement (2)> The melting point (Tm) measured by a differential scanning calorimeter (DSC) is 150° C. to 170° C., preferably 155° C. to 170° C., and more preferably 160° C. to 170° C. When the melting point is within the above range, the composition of the present invention has an excellent balance between heat resistance and impact resistance.
[0013] The propylene polymer (A) preferably further satisfies either the following requirement (3) or (4), and more preferably satisfies both the following requirements (3) and (4).
[0014] <Requirement (3)> The isotactic mesopentad fraction (mmmm) is greater than 97.0% and less than 99.9%, preferably greater than 97.3% and less than 99.9%, more preferably greater than 97.5% and less than 99.9%. When the isotactic mesopentad fraction is within the above range, the heat resistance rigidity of the composition of the present invention is excellent.
[0015] Here, the isotactic mesopentad fraction indicates the proportion of pentad isotactic structures in a molecular chain, and is the fraction of propylene structural units at the center of a chain in which five consecutive propylene monomer units have a mesostructure. The isotactic mesopentad fraction can be determined by the method described below.
[0016] <Requirement (4)> The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is 4.0 to 20.0, preferably 4.5 to 15.0, and more preferably 4.8 to 10.0. When the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight is within the above range, the composition of the present invention has excellent heat resistance and moldability.
[0017] In one embodiment, the propylene polymer (A) is a propylene homopolymer (Ah).
[0018] In one embodiment, the propylene polymer (A) is a random copolymer, for example, a propylene-α-olefin random copolymer (Ar). In the case of a random copolymer, the content of structural units derived from propylene is preferably 90 mol % or more and less than 100 mol %, more preferably 93 mol % or more and 99 mol % or less, based on 100 mol % of all repeating structural units. The content can be determined, for example, by carbon nuclear magnetic resonance analysis ( 13 It can be measured by C-NMR.
[0019] The α-olefin may be, for example, an α-olefin having 2 to 20 carbon atoms other than propylene, such as ethylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene, with ethylene being preferred. These may be used alone or in combination of two or more.
[0020] In one embodiment, the propylene polymer (A) may be a propylene-based block copolymer (Ab) comprising a propylene homopolymer portion (Ah) and a propylene-α-olefin copolymer portion (Ac) that satisfies the requirements for the propylene polymer (A) according to the present invention.
[0021] The copolymer portion (Ac) is composed of a copolymer of propylene and an α-olefin other than propylene having a carbon number of 2 to 20. Specific examples of the α-olefin are as described above, and ethylene is preferable.
[0022] The copolymer portion (Ac) contains 40.0 to 75.0 mol %, preferably 45.0 to 70.0 mol %, and more preferably 50.0 to 65.0 mol % of structural units derived from propylene, and 25.0 to 60.0 mol %, preferably 30.0 to 55.0 mol %, and more preferably 35.0 to 50.0 mol % of structural units derived from an α-olefin having 2 to 20 carbon atoms other than propylene. However, the total of the structural units derived from propylene and the structural units derived from the α-olefin is taken as 100 mol %. The content ratio can be determined, for example, by carbon nuclear magnetic resonance analysis ( 13 It can be measured by C-NMR.
[0023] The propylene-based block copolymer (Ab) contains the homopolymer portion (Ah) in an amount of preferably 50 to 99% by mass, more preferably 60 to 99% by mass, and even more preferably 70 to 97% by mass, and contains the copolymer portion (Ac) in an amount of preferably 1 to 50% by mass, more preferably 1 to 40% by mass, and even more preferably 3 to 30% by mass, where the total of the homopolymer portion (Ah) and the copolymer portion (Ac) is taken as 100% by mass. The propylene-α-olefin copolymer portion (Ac) generally corresponds to the n-decane soluble component of the propylene-based block copolymer (Ab) at 23° C.
[0024] The copolymer portion (Ac) (n-decane soluble component at 23°C) of the propylene-based block copolymer (Ab) has an intrinsic viscosity [η] measured with decalin at 135°C of usually 1.0 to 12.0 dl / g, preferably 1.5 to 11.0 dl / g, and more preferably 2.0 to 10.0 dl / g.
[0025] The propylene polymer (A) may be used in the form of a composition consisting of one or more propylene polymers as long as the requirements of the present invention are satisfied.
[0026] The propylene-based polymer (A) according to the present invention may contain biomass-derived propylene. The propylene constituting the polymer may be only biomass-derived propylene, or may contain both biomass-derived propylene and fossil fuel-derived propylene. Biomass-derived propylene is propylene obtained from any renewable natural raw material, such as fungi, yeast, algae, and bacteria, or from an animal or plant source, or from its residue, and contains propylene as carbon. 14 C isotope 10 -12 The biomass-derived propylene is contained in a ratio of about 100 (pMC) as measured in accordance with ASTM D6866. Biomass-derived propylene can be obtained by a conventionally known method. It is preferable that the propylene-based polymer (A) according to the present invention contains biomass-derived propylene from the viewpoint of reducing the environmental load (mainly reducing greenhouse gas emissions). If the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, even if the raw material propylene contains biomass-derived propylene, 14 C isotope 10 -14 ~10 -12 Other than the proportion of propylene in the polymer, its molecular structure is the same as that of propylene homopolymers made from fossil fuel-derived propylene, and therefore its performance is said to be the same.
[0027] The propylene-based polymer (A) according to the present invention may contain propylene derived from chemical recycling. The propylene constituting the polymer may be only propylene derived from chemical recycling, or may contain propylene derived from chemical recycling and propylene derived from fossil fuel and / or propylene derived from biomass. The propylene derived from chemical recycling is obtained by a conventionally known method. It is preferable that the propylene-based polymer (A) according to the present invention contains propylene derived from chemical recycling from the viewpoint of reducing the environmental load (mainly reducing waste). Even if the raw material monomer contains a monomer derived from chemical recycling, the monomer derived from chemical recycling is a monomer obtained by depolymerizing or pyrolyzing a polymer such as waste plastic back to a monomer unit such as propylene, and a monomer produced using the monomer as a raw material. Therefore, if the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, the molecular structure is the same as that of a propylene homopolymer made of a monomer derived from a fossil fuel. Therefore, the performance is said to be the same.
[0028] <<Method for producing propylene polymer (A)>> The method for producing the propylene polymer (A) is not particularly limited, and for example, the propylene polymer (A) can be produced by homopolymerizing propylene or copolymerizing propylene with other monomers in the presence of a Ziegler-Natta catalyst or a metallocene catalyst. Examples of the catalyst include those described in JP 2014-214202 A, JP 2016-084387 A, WO 2019 / 004418 A, and JP 2007-224179 A.
[0029] [Elastomer (B)] The propylene-based resin composition of the present invention may contain an elastomer (B) as necessary. The type of the elastomer (B) is not particularly limited, but an ethylene-α-olefin copolymer or a styrene-based block copolymer is preferred.
[0030] The ethylene-α-olefin copolymer is obtained, for example, by copolymerizing ethylene with one or more α-olefins selected from α-olefins having 3 to 20 carbon atoms, preferably 3 to 10 carbon atoms. As the α-olefin, propylene, 1-butene, 1-hexene, and 1-octene are preferable, and 1-butene and 1-octene are particularly preferable. The α-olefins may be used alone or in combination of two or more kinds.
[0031] The melt flow rate (MFR) of the ethylene-α-olefin copolymer measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg is preferably 0.1 to 40 g / 10 min, more preferably 1 to 20 g / 10 min, and particularly preferably 1 to 10 g / 10 min. If the melt flow rate is 0.1 g / 10 min or more, the resin fluidity is unlikely to decrease and dispersion failure during kneading is unlikely to occur, and physical properties such as impact resistance of the molded product are unlikely to decrease. On the other hand, if it is 40 g / 10 min or less, the molded product tends to have sufficient impact resistance.
[0032] The content of structural units derived from an α-olefin in the ethylene-α-olefin copolymer is 5 to 50 mol %, preferably 5 to 40 mol %, more preferably 7 to 35 mol %, and particularly preferably 10 to 30 mol %, relative to all structural units in the copolymer, with the total of the structural units derived from ethylene and the structural units derived from an α-olefin being taken as 100 mol %.
[0033] As the styrene-based block copolymer, for example, a styrene-conjugated diene type diblock copolymer or a styrene-conjugated diene-styrene triblock copolymer can be used. In addition, an XY-Y' type triblock copolymer using a block Y' in which the vinyl bond amount of the conjugated diene is reduced in order to improve fluidity can also be used. As the hydrogenated product of the block copolymer, an XYX type triblock copolymer is particularly preferable. Here, X represents a structural unit derived from styrene, and Y represents a structural unit derived from a conjugated diene.
[0034] In the styrene-based block copolymer, the styrene content is preferably 10 to 25% by mass, and the MFR (ASTM D1238, 190° C., 2.16 kg load) is preferably 0.5 to 15 g / 10 min, more preferably 1 to 10 g / 10 min.
[0035] Specific examples of the styrene-based block copolymer include a styrene-ethylene-butene-styrene block copolymer, a styrene-ethylene-propylene-styrene block copolymer, and a styrene-ethylene-propylene block copolymer.
[0036] <Method for producing elastomer (B)> The method for producing the elastomer (B) is not particularly limited, but it can be produced, for example, by the method described in paragraphs
[0043] to
[0088] of WO2007 / 034920.
[0037] [Modified propylene resin (C)] As the modified propylene resin (C), from the viewpoint of improving the affinity between the bamboo powder (D) and the propylene-based polymer (A) and enhancing the strength and heat resistance, fatty acid anhydride-modified polypropylene is preferred, and maleic anhydride-modified polypropylene is more preferred.
[0038] Specific examples of the maleic anhydride-modified polypropylene that can be used include commercially available products such as Admer (registered trademark) manufactured by Mitsui Chemicals, Inc., Umex (registered trademark) manufactured by Sanyo Chemical Industries, Ltd., MZ series manufactured by DuPont, Exxelor (registered trademark) manufactured by Exxon, and Polybond 3200 manufactured by Addivant Japan Co., Ltd.
[0039] <Production method of modified propylene resin (C)> The modified propylene resin (C) can be obtained by modifying a propylene polymer with an acid, for example by graft modification or copolymerization.
[0040] The modifier used for modification includes unsaturated carboxylic acids and their derivatives. Specific examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, nadic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, sorbic acid, mesaconic acid, angelic acid, and phthalic acid. Examples of derivatives of unsaturated carboxylic acids include acid anhydrides, esters, amides, imides, and metal salts. Specific examples of such derivatives include maleic anhydride, itaconic anhydride, citraconic anhydride, nadic anhydride, phthalic anhydride, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, maleic acid monoethyl ester, acrylamide, maleic acid monoamide, maleimide, N-butylmaleimide, sodium acrylate, and sodium methacrylate. Among these, unsaturated dicarboxylic acids and their derivatives are preferred, and maleic anhydride and phthalic anhydride are more preferred.
[0041] The modified propylene resin (C) can be prepared by various known methods, for example, by dissolving a propylene polymer in an organic solvent, adding an unsaturated carboxylic acid or a derivative thereof and, if necessary, a radical initiator such as an organic peroxide to the resulting solution, and reacting the mixture at a temperature of usually 60 to 350°C, preferably 80 to 190°C, for 0.5 to 15 hours, preferably 1 to 10 hours; or by using an extruder or the like, adding a propylene polymer, an unsaturated carboxylic acid or a derivative thereof and, if necessary, a radical initiator such as an organic peroxide, without a solvent, and reacting the mixture at a temperature equal to or higher than the melting point of the propylene polymer, preferably 180 to 350°C, for 0.5 to 10 minutes.
[0042] [Bamboo powder (D)] The average particle size of the bamboo powder (D) (particle size at which the cumulative volume is 50% as measured by the laser diffraction scattering method according to JIS R1629) is 10 μm to 2000 μm, preferably 15 μm to 1000 μm. If the particle size of the bamboo powder is larger than 2000 μm, the impact resistance of the propylene-based resin composition may decrease. If the particle size of the bamboo powder is smaller than 10 μm, the rigidity of the propylene-based resin composition may decrease.
[0043] The bamboo powder (D) further has a particle content of more than 600 μm in diameter (weight ratio of sieve residue with 600 μm mesh size in sieving test method based on JIS K0069) of 30% or more. If the content of particles with a particle size of more than 600 μm is less than 30%, there is a risk of a decrease in heat distortion temperature.
[0044] The bamboo powder (D) is preferably processed into powder form using a chip saw-type cutting grinder, and then sieved before use. In addition, there is no restriction on the type of bamboo, and bamboo powder made from one or more types of bamboo can be used as long as the requirements of the present invention are met. The bamboo powder used in the present invention is preferably Moso bamboo that is 3 years old or older.
[0045] [Inorganic filler] In the propylene-based resin composition according to the present invention, inorganic fillers other than the above-mentioned components (A) to (D) may be added within a range that does not impair the object of the present invention. Examples of inorganic fillers include talc, clay, mica, calcium carbonate, magnesium hydroxide, ammonium phosphate, silicates, carbonates, carbon black, magnesium sulfate fiber, glass fiber, carbon fiber, etc. These may be used alone or in combination of two or more.
[0046] [Other ingredients] The composition of the present invention may contain other components, such as resins, rubbers, fillers, weather stabilizers, heat stabilizers, antistatic agents, antislip agents, antiblocking agents, antifogging agents, lubricants, pigments, dyes, plasticizers, antioxidants, hydrochloric acid absorbers, antioxidants, nucleating agents, etc., other than the above-mentioned components (A) to (D), within the scope of the present invention. These may be used alone or in combination of two or more.
[0047] [Embodiments of Propylene-Based Resin Composition] The propylene-based resin composition of the present invention contains a propylene-based polymer (A), an elastomer (B), a modified propylene resin (C), and bamboo powder (D). When the total of the components (A), (B), (C), and (D) is taken as 100% by mass, The component (A) is 20 to 98% by mass, preferably 30 to 98% by mass, and more preferably 40 to 90% by mass, The content of the component (B) is 0 to 50% by mass, preferably 0 to 40% by mass, and more preferably 0 to 30% by mass. The content of the component (C) is 1 to 20% by mass, preferably 1 to 15% by mass, and more preferably 1 to 10% by mass, The content of the component (D) is 1 to 49% by mass, preferably 5 to 49% by mass.
[0048] If the amount of component (C) used is less than the above range, the effect of improving the rigidity of the molded article may not be observed, whereas if the amount used is more than the above range, the impact strength of the molded article may decrease as a mechanical property.
[0049] <Method for producing propylene-based resin composition> The propylene-based resin composition of the present invention can be produced by blending the above-mentioned components. The components may be blended sequentially in any order, or may be mixed simultaneously. A multi-stage mixing method may be adopted in which some components are mixed and then other components are mixed. Examples of the method for blending the components include a method in which the components are mixed or melt-kneaded simultaneously or sequentially using a mixing device such as a Banbury mixer, a single-screw extruder, a twin-screw extruder, or a high-speed twin-screw extruder.
[0050] [Molded body] The molded article of the present invention is formed using the above-mentioned composition of the present invention. The molded article made of the composition of the present invention is lightweight and has excellent heat resistance and rigidity, and therefore can be suitably used in various fields such as automobile parts, home appliance parts, and food containers.
[0051] Examples of automobile parts include automobile exterior parts such as bumpers, side moldings, and aerodynamic undercovers; automobile interior parts such as instrument panels and interior trim; exterior panel parts such as fenders, door panels, and steps; and engine peripheral parts such as engine covers, fans, and fan shrouds.
[0052] Examples of food containers include food containers such as tableware, retort containers, freezer storage containers, retort pouches, microwave heat-resistant containers, frozen food containers, frozen dessert cups, cups, and beverage bottles, retort containers, and bottle containers.
[0053] Other uses of the molded article of the present invention include, for example, housings for home appliances, electric wire covering materials, insulators for high-voltage wires, tubes for cosmetic and perfume sprays, medical tubes, infusion tubes, pipes, wire harnesses, interior materials for motorcycles, railway cars, aircraft, ships, etc., instrument panel skins, door trim skins, rear package trim skins, ceiling skins, rear pillar skins, seat back garnishes, console boxes, armrests, airbag case lids, shift knobs, assist grips, side step mats, reclining covers, trunk seats, seat belt buckles, molding materials such as inner and outer moldings, roof moldings, and belt moldings, automotive sealing materials such as door seals and body seals, glass run channels, mudguards, kicking plates, step mats, license plate housings, automotive hose components, air duct hoses, air duct covers, air intake pipes, air dam skirts, timing belt cover seals, bonnet cushions, door cushions, and other automotive interior and exterior materials, special tires such as vibration-damping tires, static tires, car racing tires, and radio-controlled tires, packings, Automobile dust covers, lamp seals, automotive boot materials, rack and pinion boots, timing belts, wire harnesses, grommets, emblems, air filter packing, covering materials for furniture, footwear, clothing, bags, building materials, etc., architectural sealing materials, waterproof sheets, building material sheets, building material gaskets, building material window films, iron core protection materials, gaskets, doors, door frames, window frames, moldings, baseboards, opening frames, etc., flooring materials, ceiling materials, wallpaper, health products (e.g. anti-slip mats / sheets, fall prevention films / mats / sheets), health equipment parts, shock absorbing pads, protectors / protective equipment ( Examples: helmets, guards), sports goods (examples: sports grips, protectors), sports protective gear, rackets, mouth guards, balls, golf balls, transport equipment (examples: shock absorbing grips for transport, shock absorbing sheets), vibration-damping pallets, shock absorbing dampers, insulators, shock absorbing materials for footwear, shock absorbing foams, shock absorbing films and other shock absorbing materials, grip materials, miscellaneous goods, toys, midsoles, innersoles, and outsoles of shoes, sandals, suction cups, toothbrushes, flooring materials, gymnastics mats, power tool parts, agricultural machinery parts, heat dissipation materials, transparent substrates, soundproofing materials, cushioning materials,Examples include electric wires and cables, shape memory materials, gaskets, packing materials for high-temperature treatment such as high-pressure steam sterilization, industrial sealing materials, industrial sewing machine tables, license plate housings, cap liners such as PET bottle cap liners, stationery, office supplies, precision equipment and OA equipment support materials such as OA printer legs, FAX legs, sewing machine legs, motor support mats, audio vibration isolators, heat-resistant packing for OA, costume cases, desk mats, etc.
[0054] The molding method for the molded article of the present invention is not particularly limited, and various methods known as methods for molding polymers can be used, with injection molding, extrusion molding, and press molding being particularly preferred. EXAMPLES
[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring various physical properties described in the examples are as follows.
[0056] <Isotactic mesopentad fraction (mmmm)> The isotactic mesopentad fraction mmmm (%), which is one of the indices of the stereoregularity of a polymer and is used to examine its microtacticity, was assigned in propylene-based polymers based on Macromolecules 8,687 (1975). 13 It was calculated from the peak intensity ratio of the C-NMR spectrum. 13 C-NMR spectra were measured using a JEOL EX-400 instrument at 130° C. with TMS as the standard and o-dichlorobenzene as the solvent.
[0057] <Melting point> The melting points of the components eluted at a temperature of 122°C or higher by the temperature rising elution fractionation measurement (TREF) were measured under the following conditions using a differential scanning calorimeter (DSC, manufactured by PerkinElmer Co., Ltd.) The endothermic peak in the third step measured here was defined as the melting point (Tm). (Measurement conditions) First step: Raise the temperature to 240°C at 10°C / min and hold for 10 minutes. Second step: Lower the temperature to 60°C at 10°C / min. Third step: Raise the temperature to 240°C at 10°C / min.
[0058] <Weight average molecular weight (Mw) and number average molecular weight (Mn)> The Mw / Mn value, which is an index of molecular weight distribution, was obtained by analyzing a chromatogram measured under the following conditions by a known method. (Measurement conditions) Apparatus: Waters gel permeation chromatograph Alliance GPC2000 Column: Tosoh TSKgel GMH6-HT x2 + TSKgel GMH6-HTL x2 Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Flow rate: 1.0ml / min Temperature: 140℃ Column calibration: Tosoh monodisperse polystyrene Sample concentration: 0.15% (w / v) Injection volume: 0.4ml
[0059] <Maleic anhydride graft amount> Approximately 2 g of modified propylene resin was collected and completely dissolved in 500 ml of boiling p-xylene by heating. The p-xylene solution in which the modified propylene resin was dissolved was transferred to a 2 L beaker and allowed to cool for approximately 1 hour under a 23°C atmosphere. Then, 1200 ml of acetone was added to the beaker, and the polymer was precipitated while stirring. The precipitate was filtered and dried to remove the ungrafted portion, thereby obtaining a refined product of the modified propylene resin. A pressed film from this refined product was subjected to FT-IR measurement, and a peak at 1790 cm -1 and 974cm -1 The amount of maleic anhydride grafted into polypropylene was calculated in terms of wt % from the peak intensity ratio.
[0060] <Intrinsic viscosity [η]> The measurement was performed at 135°C using decalin solvent. Approximately 20 mg of sample was dissolved in 15 ml of decalin, and the specific viscosity [ηsp] was measured in an oil bath at 135°C. After diluting the decalin solution by adding 5 ml of decalin solvent, the specific viscosity [ηsp] was measured in the same manner. This dilution procedure was repeated two more times, and the value of [ηsp / C] when the concentration (C) was extrapolated to 0 was calculated as the limiting viscosity [η]. [η]=lim(ηsp / C) (C→0)
[0061] <Melt flow rate (MFR)> The test was performed in accordance with ASTM D1238E at a measurement temperature of 230°C and a load of 2.16 kg.
[0062] <Specific gravity> Measurements were performed at 23°C using the immersion method.
[0063] <Heat distortion temperature> The heat distortion temperature was measured under the following conditions in accordance with JIS K7191. (Measurement conditions) Test piece: 10mm (width) x 4mm (thickness) x 80mm (length) Load: 0.45MPa
[0064] [Production Example 1] <Production method of propylene homopolymer (Ah-1)> (1) Preparation of solid titanium catalyst component 95.2 g of anhydrous magnesium chloride, 442 ml of decane, and 390.6 g of 2-ethylhexyl alcohol were reacted by heating at 130°C for 2 hours to obtain a homogeneous solution, and then 21.3 g of phthalic anhydride was added to this solution, followed by stirring and mixing at 130°C for 1 hour to dissolve the phthalic anhydride.
[0065] The homogeneous solution thus obtained was cooled to room temperature, and then 75 ml of this homogeneous solution was added dropwise over one hour to 200 ml of titanium tetrachloride kept at -20° C. After the addition was completed, the temperature of this mixture was raised to 110° C. over four hours, and when it reached 110° C., 5.22 g of diisobutyl phthalate (DIBP) was added, and the mixture was stirred and kept at the same temperature for another two hours.
[0066] After the 2-hour reaction, the solid was collected by hot filtration, resuspended in 275 ml of titanium tetrachloride, and then heated again for 2 hours at 110° C. After the reaction was completed, the solid was collected again by hot filtration and thoroughly washed with decane and hexane at 110° C. until no free titanium compounds were detected in the solution.
[0067] The detection of the free titanium compounds was confirmed by the following method. 10 ml of the supernatant of the solid catalyst component was taken with a syringe and placed in a 100 ml sidearm Schlenk tube that had been previously substituted with nitrogen. Next, the solvent hexane was dried with a nitrogen stream, and then vacuum dried for 30 minutes. 40 ml of ion-exchanged water and 10 ml of (1+1) sulfuric acid were added and stirred for 30 minutes. This aqueous solution was transferred to a 100 ml measuring flask through a filter paper, followed by the addition of 1 ml of concentrated phosphoric acid aqueous solution as a masking agent for iron (II) ions and 5 ml of 3% hydrogen peroxide solution as a titanium coloring reagent, and the measuring flask was then filled to 100 ml with ion-exchanged water. The measuring flask was then shaken, and after 20 minutes, the absorbance at 420 nm was observed using UV, and the free titanium was washed and removed until this absorption was no longer observed.
[0068] The solid titanium catalyst component (A) prepared as above was stored as a decane slurry, and a part of it was dried for the purpose of examining the catalyst composition. The composition of the solid titanium catalyst component (A) thus obtained was 2.3% by weight of titanium, 61% by weight of chlorine, 19% by weight of magnesium, and 12.5% by weight of DIBP.
[0069] (2) Preparation of prepolymerization catalyst 100 g of the solid catalyst component, 39.3 mL of triethylaluminum, and 100 L of heptane were charged into a 200 L autoclave equipped with a stirrer, and 600 g of propylene was added while keeping the internal temperature at 15 to 20°C. The mixture was reacted for 60 minutes with stirring to obtain a catalyst slurry.
[0070] (3) Main Polymerization To a 58 L jacketed circulation tubular polymerization reactor, 43 kg / h of propylene, 177 NL / h of hydrogen, 0.58 g / h of the catalyst slurry produced in (2) as a solid catalyst component, 3.1 ml / h of triethylaluminum, and 3.3 ml / h of dicyclopentyldimethoxysilane were continuously fed, and polymerization was carried out in a liquid-filled state with no gas phase present. The temperature of the tubular polymerization reactor was 70°C, and the pressure was 3.53 MPa / G.
[0071] The obtained slurry was sent to a 100 L vessel polymerization reactor equipped with a stirrer, and further polymerization was carried out. Propylene was fed to the polymerization reactor at 45 kg / hour, and hydrogen was fed to the polymerization reactor so that the hydrogen concentration in the gas phase was 3.2 mol%. Polymerization was carried out at a polymerization temperature of 70°C and a pressure of 3.28 MPa / G.
[0072] The resulting propylene homopolymer (Ah-1) was vacuum dried at 80° C. The physical properties of the propylene homopolymer (Ah-1) are shown in Table 1.
[0073] [Table 1]
[0074] [Production Example 2] <Method for producing propylene-based block copolymer (Ab-1)> (1) Preparation of solid titanium catalyst component A solid titanium catalyst component was obtained in the same manner as in Production Example 1.
[0075] (2) Preparation of prepolymerization catalyst A catalyst slurry containing a prepolymerization catalyst component was obtained in the same manner as in Production Example 1.
[0076] (3) Main Polymerization To a 58 L jacketed circulation tubular polymerization reactor, 43 kg / hr of propylene, 300 NL / hr of hydrogen, 0.55 g / hr of the catalyst slurry produced in (2) as a solid catalyst component, 2.9 ml / hr of triethylaluminum, and 3.1 ml / hr of dicyclopentyldimethoxysilane were continuously fed, and polymerization was carried out in a liquid-filled state with no gas phase present. The temperature of the tubular polymerization reactor was 70° C., and the pressure was 3.74 MPa / G.
[0077] The obtained slurry was sent to a 100 L vessel polymerization reactor equipped with an agitator, and further polymerization was carried out. Propylene was fed to the polymerization reactor at 45 kg / hr, and hydrogen was fed to the polymerization reactor so that the hydrogen concentration in the gas phase was 8.7 mol%. Polymerization was carried out at a polymerization temperature of 70°C and a pressure of 3.49 MPa / G.
[0078] The obtained slurry was transferred to a 2.4L liquid transfer tube, gasified, and separated into gas and solid. The polypropylene homopolymer powder was then sent to a 480L gas-phase polymerization reactor, where ethylene-propylene block copolymerization was carried out. A portion of the powder was sampled before copolymerization to measure MFR and mmmm. Propylene, ethylene, and hydrogen were continuously fed into the gas-phase polymerization reactor so that the gas composition in the reactor was ethylene / (ethylene + propylene) 0.23 (molar ratio) and hydrogen / ethylene 0.031 (molar ratio). Polymerization was carried out at a polymerization temperature of 70°C and a pressure of 1.0MPa / G.
[0079] The resulting propylene-based block copolymer (Ab-1) was vacuum dried at 80° C. The physical properties of the resulting propylene-based block copolymer (Ab-1) are shown in Table 2.
[0080] [Table 2]
[0081] [Production Example 3] <Method for producing propylene-based random copolymer (Ar-1)> [Preparation of solid titanium catalyst component (a-1)] 95.2 g of anhydrous magnesium chloride, 442 ml of decane, and 390.6 g of 2-ethylhexyl alcohol were reacted by heating at 130°C for 2 hours to obtain a homogeneous solution, and then 21.3 g of phthalic anhydride was added to this solution, followed by stirring and mixing at 130°C for 1 hour to dissolve the phthalic anhydride.
[0082] The homogeneous solution thus obtained was cooled to room temperature, and then 75 ml of this homogeneous solution was added dropwise over one hour to 200 ml of titanium tetrachloride kept at -20° C. After the addition was completed, the temperature of this mixture was raised to 110° C. over four hours, and when it reached 110° C., 5.22 g of diisobutyl phthalate (DIBP) was added, and the mixture was stirred and kept at the same temperature for another two hours.
[0083] After the 2-hour reaction, the solid was collected by hot filtration, resuspended in 275 ml of titanium tetrachloride, and then heated again for 2 hours at 110° C. After the reaction was completed, the solid was collected again by hot filtration and thoroughly washed with decane and hexane at 110° C. until no free titanium compounds were detected in the solution.
[0084] The solid titanium catalyst component prepared as above was stored as a hexane slurry, and a portion of this was dried to examine the catalyst composition. The solid titanium catalyst component contained 2.3 wt% titanium, 61 wt% chlorine, 19 wt% magnesium, and 12.5 wt% DIBP.
[0085] [Production of prepolymerization catalyst (b-1)] 100g of transition metal catalyst component (a-1), 15.4mL of triethylaluminum, and 100L of heptane were charged into a 200L autoclave equipped with a stirrer, and 600g of propylene was added while maintaining the internal temperature at 5℃, and the reaction was carried out with stirring for 60 minutes. After the polymerization was completed, 4.1mL of titanium tetrachloride was charged to prepare prepolymerization catalyst (b-1). This prepolymerization catalyst (b-1) contained 6g of polypropylene per 1g of transition metal catalyst component.
[0086] [Production of propylene-based random copolymer (Ar-1)] To a 500L stirred vessel polymerization reactor, 130 kg / hour of propylene, 2.6 kg / hour of ethylene, 0.50 g / hour of prepolymerization catalyst (b-1) as a transition metal catalyst component, 5.2 mL / hour of triethylaluminum, and 2.8 mL / hour of dicyclopentyldimethoxysilane were continuously supplied, and hydrogen was supplied so that the hydrogen concentration in the gas phase was 6.0 mol%. The temperature of the stirred vessel polymerization reactor was 70°C, and the pressure was 3.25 MPa / G.
[0087] The obtained slurry was deactivated, and the propylene was evaporated to obtain a powdered propylene random copolymer, which had an MFR of 8.0 g / 10 min and an ethylene content of 4.2 wt%.
[0088] 100 parts by weight of the obtained propylene random copolymer was mixed with 0.1 parts by weight of heat stabilizer Hostanox P-EPQ (trademark of Clariant Chemicals Co., Ltd.), 0.1 parts by weight of calcium stearate, and 0.029 parts by weight of Kayahexa AD (trademark of Kayaku Nouryon Co., Ltd.) in a tumbler, and then melt-kneaded in a twin-screw extruder under the following conditions to prepare pellet-shaped propylene random copolymer (Ar-1). The physical properties of the propylene random copolymer (Ar-1) are shown in Table 3.
[0089] <Melt kneading conditions> Co-rotating twin-screw mixer: Model number KZW-15, manufactured by Technovel Co., Ltd. Mixing temperature: 210℃ Screw rotation speed: 500 rpm Feeder rotation speed: 40 rpm
[0090] [Table 3]
[0091] [Example 1] 69 parts by weight of the propylene homopolymer (Ah-1) produced in Production Example 1, 10 parts by weight of the elastomer (B-1) (Tafmer A-1050S (trademark of Mitsui Chemicals, Inc.)), 20 parts by weight of bamboo powder (D-1) (manufactured by Takex Laboratories Co., Ltd.) having an average particle diameter of 500 μm and a content of particles exceeding 600 μm of 32%, 1 part by weight of maleic anhydride-modified PP ([η]=0.43 dl / g, maleic anhydride graft amount = 3 wt%) (C-1), 0.1 part by weight of IRGANOX 1010 (trademark of Ciba Geigy Corporation), 0.1 part by weight of heat stabilizer IRGAFOS 168 (trademark of Ciba Geigy Corporation), and 0.1 part by weight of calcium stearate were mixed in a tumbler and then melt-kneaded under the following conditions using a twin-screw extruder to prepare a pelletized propylene-based resin composition, and test pieces were prepared under the following conditions using an injection molding machine. The physical properties of the obtained propylene-based resin composition are shown in Table 4.
[0092] <Melt-kneading conditions> Co-rotating twin-screw kneader: Model KZW-15, manufactured by Technovel Corporation Kneading temperature: 170 °C Screw rotation speed: 600 rpm Feeder rotation speed: 80 rpm
[0093] <JIS small test piece / Injection molding conditions> Injection molding machine: Model EC40, manufactured by Toshiba Machine Co., Ltd. Cylinder temperature: 190 °C Mold temperature: 40 °C Injection time - holding pressure time: 20 seconds (primary filling time: 1 second) Cooling time: 5 seconds
[0094] [Example 2] In Example 1, a propylene-based resin composition was obtained in the same manner as in Example 1, except that 79 parts by weight of the propylene block copolymer (Ab-1) produced in Production Example 2 was used instead of 69 parts by weight of the propylene homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1). The physical properties of the obtained composition are shown in Table 4.
[0095] [Example 3] A propylene-based resin composition was obtained in the same manner as in Example 1, except that 69 parts by weight of the propylene-based block copolymer (Ab-1) was used instead of 69 parts by weight of the propylene-based homopolymer (Ah-1) in Example 1. The physical properties of the obtained composition are shown in Table 4.
[0096] [Example 4] A propylene-based resin composition was obtained in the same manner as in Example 1, except that 69 parts by weight of the propylene-based homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1) were replaced with 39.5 parts by weight of the propylene-based homopolymer (Ah-1) and the propylene-based block copolymer (Ab-1), respectively, in place of 69 parts by weight of the propylene-based homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1). The physical properties of the obtained composition are shown in Table 4.
[0097] [Example 5] A propylene-based resin composition was obtained in the same manner as in Example 1, except that the propylene-based homopolymer (Ah-1) and the propylene-based block copolymer (Ab-1) were 37 parts by weight, respectively, instead of 69 parts by weight of the propylene-based homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1). The physical properties of the obtained composition are shown in Table 4.
[0098] [Example 6] A propylene-based resin composition was obtained in the same manner as in Example 1, except that 69 parts by weight of the propylene-based homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1) were replaced with 32 parts by weight of the propylene-based homopolymer (Ah-1) and 32 parts by weight of the propylene-based block copolymer (Ab-1), respectively, and 15 parts by weight of the elastomer (B-1). The physical properties of the obtained composition are shown in Table 4.
[0099] [Comparative Example 1] A propylene-based resin composition was obtained in the same manner as in Example 1, except that 79 parts by weight of the propylene-based random copolymer (Ar-1) produced in Production Example 3 was used instead of 69 parts by weight of the propylene-based homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1) in Example 1. The physical properties of the obtained composition are shown in Table 4.
[0100] [Comparative Example 2] 90 parts by weight of propylene-based homopolymer (Ah-1), 10 parts by weight of talc (JM-209 manufactured by Asada Flour Milling Co., Ltd.), 0.1 parts by weight of IRGANOX1010 (trademark of Ciba-Geigy Co., Ltd.), 0.1 parts by weight of heat stabilizer IRGAFOS168 (trademark of Ciba-Geigy Co., Ltd.), and 0.1 parts by weight of calcium stearate were mixed in a tumbler, and a propylene-based resin composition was obtained in the same manner as in Example 1. The physical properties of the obtained composition are shown in Table 4.
[0101] [Comparative Example 3] A propylene-based resin composition was obtained in the same manner as in Comparative Example 2, except that 80 parts by weight of the propylene-based homopolymer (Ah-1) and 10 parts by weight of the elastomer (B-1) were used instead of 90 parts by weight of the propylene-based homopolymer (Ah-1) in Comparative Example 2. The physical properties of the obtained composition are shown in Table 4.
[0102] [Comparative Example 4] A propylene-based resin composition was obtained in the same manner as in Comparative Example 2, except that 90 parts by weight of the propylene-based homopolymer (Ah-1) was replaced with 90 parts by weight of the propylene-based monoblock copolymer (Ab-1). The physical properties of the obtained composition are shown in Table 4.
[0103] [Table 4] [Industrial Applicability]
[0104] INDUSTRIAL APPLICABILITY The propylene-based resin composition of the present invention is lightweight and has excellent heat resistance and rigidity, and therefore can be suitably used in various fields such as automobile parts, home appliance parts, and food containers.
Claims
1. 20 to 98% by mass of a propylene-based polymer (A) satisfying the following requirements (1) and (2); 0 to 50% by mass of an elastomer (B); 1 to 20% by mass of a modified propylene resin (C); Bamboo powder (D) 1 to 49% by mass having an average particle size (particle size at which the cumulative volume is 50% as measured by a laser diffraction scattering method in accordance with JIS R1629) of 10 μm or more and 2000 μm or less, and a content of particles with a particle size of 600 μm or more (weight ratio of sieve residue with 600 μm openings in a sieve analysis method in accordance with JIS K0069) of 30% or more; A propylene-based resin composition comprising the following (wherein the total of the components (A), (B), (C) and (D) is 100 mass%): (1) A melt flow rate (MFR) (ASTM D1238, 230°C, 2.16 kg load) of 0.5 to 1000 g / 10 min; (2) The melting point (Tm) measured by differential scanning calorimetry (DSC) is 150° C. to 170° C.
2. The propylene-based resin composition according to claim 1, wherein the propylene-based polymer (A) further satisfies the following requirements (3) and (4): (3) the isotactic mesopentad fraction (mmmm) is greater than 97.0% and less than 99.9%; (4) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is 4.0 to 20.
0.
3. A molded article comprising the propylene-based resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Polyolefin resin composition and its injection molding
JP1991250040A
Thermoplastic polymer composition