Aluminum alloy wire material and method for producing the same
The aluminum alloy wire manufacturing process addresses the challenge of maintaining high tensile strength, elongation, and conductivity by employing a series of heat treatments and wire drawing steps to suppress undesirable phase formations, resulting in improved mechanical properties for wires with diameters less than 2 mm.
Patent Information
- Application Number
- JP2023079063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing aluminum alloy wires in the 6000 series (Al-Mg-Si series) struggle to maintain high tensile strength, elongation, and conductivity when the wire diameter is less than 2 mm, as they face issues with phase separation and precipitation of β″ phase, which degrade mechanical properties.
A manufacturing process involving solution treatment, quenching, pre-aging, first and second wire drawing, and multiple heat treatments is employed, with specific heat treatments at lower temperatures to suppress Cluster (1) formation and β″ phase precipitation, ensuring uniform internal structure and improved mechanical properties.
The process achieves an aluminum alloy wire with maximum tensile strength of 150 MPa or more, elongation of 8% or more, and electrical conductivity of 50% IACS or more, even at diameters less than 2 mm, by optimizing the microstructural stability and preventing undesirable phase formations.
Smart Images

Figure 2024163457000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum alloy wire rod belonging to the Aluminum 6000 series (Al-Mg-Si series) and a manufacturing method thereof, and more particularly to an aluminum alloy wire rod having a wire diameter of less than 2 mm and capable of obtaining good maximum tensile strength, elongation, and electrical conductivity, and a manufacturing method thereof. In the present invention, the aluminum alloy belonging to the aluminum 6000 series (Al-Mg-Si series) means a 6000 series aluminum alloy according to the JIS standard. [Background technology]
[0002] 2. Description of the Related Art As an aluminum alloy wire rod for a wire harness and a method for producing the same, the technique described in Patent Document 1 below is known. The aluminum alloy wire according to Patent Document 1 has a composition of 0.10-1.00 mass% Mg and 0.10-1.20 mass% Si, with an Mg / Si mass ratio of 0.4-0.8, and has a wire diameter of 0.5 mm or less, and is capable of ensuring tensile strength (200 MPa or more), elongation (13% or more), and electrical conductivity (45% IACS or more). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6462662 Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention aims to provide an aluminum alloy wire belonging to the Aluminum 6000 series (Al-Mg-Si series) that has good maximum tensile strength, elongation, and electrical conductivity, and a manufacturing method thereof, by a method different from that of Patent Document 1. [Means for solving the problem]
[0005] The present invention, which has been made to solve the above problems, includes at least the steps of (a) performing a solution treatment, (b) performing a quenching treatment, (c) performing a preliminary aging treatment, (e) performing a first wiredrawing treatment, (f) performing a heat treatment, (g) performing a second wiredrawing treatment, and (h) performing a heat treatment, for an Al-Mg-Si-based aluminum alloy wire, wherein the step (h) is a heat treatment that does not involve solution treatment of the aluminum alloy wire. Moreover, the present invention may further include a step (d) of performing a heat treatment between the step (c) and the step (e), and the step (d) may be configured as a heat treatment for suppressing the generation of Cluster (1) and suppressing the precipitation of the β″ phase. In addition, the present invention may further include a step of (i) performing a heat treatment after the step (h), and the step (i) may be configured to be a heat treatment that does not involve solution treatment of the aluminum alloy wire rod and is performed at a heating temperature lower than the heating temperature in the step (h). The aluminum alloy wire obtained by the method according to the present invention has properties of a wire diameter of less than 2 mm, an ultimate tensile strength of 150 MPa or more, more preferably 170 MPa or more, an elongation of 8% or more, and an electrical conductivity of 50% IACS or more. Effect of the Invention
[0006] According to the present invention, an aluminum alloy wire having good maximum tensile strength, elongation, and electrical conductivity can be obtained, and in particular, an aluminum alloy wire having good maximum tensile strength, elongation, and electrical conductivity can be obtained even when the wire diameter is less than 2 mm. [Brief description of the drawings]
[0007] [Figure 1] 1 is a flowchart showing steps of a method for producing an aluminum alloy wire according to the present invention. [Diagram 2] FIG. 4 is a diagram showing a history of processing and heat treatment of an aluminum alloy wire in Example 2. [Diagram 3] FIG. 13 shows the results of DSC measurement of each sample according to Example 2. [Figure 4] FIG. 11 shows IPF maps of each sample according to Example 2. [Diagram 5] FIG. 13 is a graph showing the breaking elongation and maximum tensile strength of each sample according to Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0009] <1> Overall configuration (Fig. 1) FIG. 1 is a flow chart showing steps of a method for producing an aluminum alloy wire rod (hereinafter, simply referred to as "wire rod") according to the present invention. As shown in FIG. 1, the method for producing an aluminum alloy wire according to the present invention includes steps (a) to (i) for an Al-Mg-Si alloy wire, among which steps (d) and (i) may be omitted as appropriate. In order to obtain the wire used in the step (a), the following known steps (melting step, wire forming step) may be carried out in advance. Each step will be described in detail below.
[0010] <2> Melting process (preliminary process) This process is a process for melting an aluminum alloy. The aluminum alloy melted in the present invention is an aluminum 6000 series (Al-Mg-Si series) aluminum alloy, and includes, for example, an aluminum alloy having a composition containing 0.40 to 0.55 mass% Mg, 0.45 to 0.65 mass% Si, with the balance being Al and unavoidable impurities (0.32 mass% or less Fe, 0.01 mass% or less Cu, 0.01 mass% or less Mn, 0.01 mass% or less Ti, 0.003 mass% or less V, etc.).
[0011] <3> Wire forming process (preliminary process) This process is a process in which the molten aluminum alloy melted in the melting process is cast to form a wire rod. Methods for forming wire rod include rolling methods such as the Properti method (continuous casting and rolling method), and a method in which a billet (cylindrical ingot) cast by a semi-continuous casting method is extruded to form a wire shape. In the present invention, the wire diameter of the wire formed in this step is, for example, φ8.0 to 10.0 mm.
[0012] <4> Step (a): Solution treatment (S100) Step (a) is a step of subjecting the wire to a solution treatment. In the present invention, the solution treatment refers to a treatment for dissolving alloy components (Mg, Si, etc.) that are not dissolved in the Al phase into solid solution. Through solution treatment, the compounds formed during casting (a typical compound in 6000 series aluminum alloys is "Mg2Si") are dissolved in the Al phase, resulting in a homogenous internal structure of the wire. In the present invention, the heating temperature and heating time in step (a) are generally within the following ranges.
[0013] <4.1>Heating temperature The heating temperature in this step is preferably 500 to 600°C. If the heating temperature is less than 500° C., phase separation occurs, which is not preferable. Moreover, if the heating temperature is higher than 600° C., partial melting occurs, which is undesirable.
[0014] <4.2> Heating time The heating time in this step is not particularly limited since the optimum time varies depending on the temperature, but for example, when the heating temperature is 500 to 600° C., the heating time is preferably about 0.5 to 10 hours. This is because partial melting occurs over 10 hours.
[0015] <5> Step (b): Quenching treatment (S200) Step (b) is a step of subjecting the wire material heated by the solution treatment to a rapid cooling treatment (quenching). This rapid cooling process prevents Mg, Si, etc., dissolved in the Al phase from precipitating as compounds, and maintains the supersaturated state of Mg and Si in the Al phase. If the rapid cooling treatment is not performed, not only will Mg-Si compounds precipitate, but they will also become coarse, which may cause a decrease in mechanical properties such as tensile strength and elongation. The quenching treatment involves immersing the wire in water at room temperature, allowing the wire to cool to room temperature and then pulling it out, and this procedure is the same in the present invention.
[0016] <6> Step (c): Pre-aging treatment (S300) Step (c) is a treatment for generating Cluster(1) out of two types of nanoclusters (Cluster(1) and Cluster(2)) that are formed as precursors for the precipitation of Mg2Si needle-like precipitates (β″ phase). This process generates Cluster(1) in advance, which consumes the Mg and Si that were supersaturated in the Al phase. This suppresses the precipitation of the β″ phase, which reduces ductility, and the generation of Cluster(2), which promotes the precipitation of the β″ phase, in the subsequent heat treatment process. In the present invention, the heating temperature and heating time in step (c) can be generally within the following ranges.
[0017] <6.1>Holding temperature The holding temperature in this step is 15° C. or lower, and preferably lower than 5° C. from the viewpoint of preventing precipitation of the β″ phase in the subsequent steps. Moreover, if the holding temperature is higher than 15°C, the formation of Cluster (2) also occurs at the same time, which is undesirable.
[0018] <6.2>Retention time The retention time in this step is not particularly limited since the optimum time varies depending on the temperature, but is preferably, for example, 7 to 10 days.
[0019] <7> Step (d): First heat treatment (S400) Step (d) is a step of subjecting the wire that has been subjected to step (c) to a heat treatment. This step is also generally called a drying treatment. By carrying out the heat treatment in this step, the generation of Cluster(1) is suppressed, and further the precipitation of the β″ phase is suppressed. In the present invention, the heating temperature in step (d) can be set within the range of about 50° C. to 200° C., and the heating time can be set within the range of about 5 minutes to 10 hours.
[0020] <8> Step (e): First wire drawing process (S500) Step (f) is a step of drawing the wire to form a drawn wire. This step can be carried out, for example, by drawing using a tapered die. The wire diameter of the drawn wire obtained in this step is, for example, φ2.0 to 3.0 mm.
[0021] <9> Step (f): Second heat treatment (S600) Step (h) is a step of subjecting the drawn wire material (intermediate drawn wire material) that has been subjected to step (e) to a heat treatment. This step is generally also called an intermediate heat treatment. By appropriately carrying out the heat treatment in this step, the strain introduced into the drawn wire material in step (e) is removed, the subsequent wiredrawability is improved, and the elongation of the finally obtained aluminum alloy wire is improved. During the heat treatment in this step, precipitation of the β″ phase also occurs, but since the Mg and Si dissolved in the Al phase are consumed and reduced by the preliminary aging treatment in step (c) described above, the amount of β″ phase precipitation is reduced. In the present invention, the heating temperature and heating time in step (f) can be generally within the following ranges.
[0022] <9.1>Heating temperature The heating temperature in this step is 180° C. or lower, preferably 110 to 130° C., for the purpose of reducing the amount of β″ phase precipitated in the subsequent steps.
[0023] <9.2> Heating time The heating time in this step is not particularly limited since the optimum time varies depending on the temperature, but is preferably about 7 hours or more. For example, when the heating temperature is 100 to 140° C., about 7 to 10 hours is preferable.
[0024] <10> Step (g): Second wire drawing process (S700) Step (g) is a step of drawing again the drawn wire material after step (f) to finally form a drawn wire material having a desired wire diameter. In this step, similarly to step (e), for example, drawing using a tapered die can be used. The wire diameter of the drawn wire obtained in this step is, for example, φ0.6 to 0.1 mm.
[0025] <11> Step (h): Third heat treatment (S800) Step (h) is a step of subjecting the drawn wire material after step (g) to a heat treatment again. This step is generally called the final heat treatment. It should be noted that this step does not involve the solution treatment (treatment for dissolving undissolved alloy components (Mg, Si, etc.) in the Al phase) in the step (a). By appropriately carrying out the heat treatment in this step, the strain introduced into the drawn wire material in the step (g) is removed, and the elongation of the finally obtained aluminum alloy wire is improved. The heating temperature and heating time in this step can be generally within the following ranges.
[0026] <11.1>Heating temperature The heating temperature in this step is 200 to 350°C, preferably 250 to 350°C, and more preferably 270 to 310°C.
[0027] <11.2> Heating time The heating time in this step is not particularly limited since the optimum time varies depending on the temperature, but is preferably about 5 minutes or more. For example, when the heating temperature is 300° C., about 5 to 20 minutes is preferable.
[0028] <12> Step (i): Fourth heat treatment (S900) The step (i) is a step of subjecting the drawn wire material that has been subjected to the previous step to a heat treatment again. This step can be defined as an additional heat treatment since step (h) is generally called the final heat treatment. It should be noted that this step does not involve the solution treatment (treatment for dissolving undissolved alloy components (Mg, Si, etc.) in the Al phase) in the step (a). By appropriately carrying out the heat treatment in this step, the strain in the wire can be restored and the elongation characteristics can be improved. The heating temperature and heating time in this step can be generally within the following ranges.
[0029] <12.1>Heating temperature The heating temperature in this step is 110 to 160° C., preferably 130 to 150° C., for the purpose of adjusting the final mechanical properties (elongation, tensile strength), and is lower than the heating temperature in step (h).
[0030] <12.2> Heating time The heating time in this step is not particularly limited since the optimum time varies depending on the temperature, but for example, when the heating temperature is 130° C. to 150° C., the heating time is preferably about 0.5 to 10 hours.
[0031] <12.3> Wire processing This step is not limited to being performed immediately after step (h). For example, this step may be performed on the wire rod after step (h) that has been subjected to a separate twisting process. EXAMPLES
[0032] Next, a first embodiment of the present invention will be described. In this embodiment, an alloy in which only Mg and Si are added to Al is used, but the 6000 series alloy in the present invention is not limited to this composition, and also includes the composition ranges of Mg, Si and other elements permitted in JIS standard 6000 series alloys.
[0033] <1> Experimental conditions An aluminum alloy containing 0.5% by mass of Mg, 0.6% by mass of Si, and the remainder being Al and unavoidable impurities, was melted and formed into a wire having a diameter of φ9.5 mm using the Properti method. The experimental conditions for each process were set as follows. In addition, for each step in the table, an "O" indicates that the step was performed under the fixed conditions described below, a "numeric value" indicates that the step was performed with the indicated numerical value, and an "X" indicates that the step was not performed.
[0034] (1) Fixation conditions (Table 1) The fixing conditions, that is, steps (a) to (e) and step (g), are shown in Table 1. [Table 1] TIFF2024163457000002.tif57150
[0035] (2) Variable conditions The variable conditions, that is, the heat treatment temperature and heat treatment time in steps (f), (h), and (i), were as shown in the numerical values in each column.
[0036] <2> Evaluation method (Table 2) The aluminum alloy wires obtained in each experimental example were measured for tensile strength, elongation, and electrical conductivity, and the properties for use in a wire harness were evaluated. The evaluation results for each experimental example are shown in Table 2 below. [Table 2] TIFF2024163457000003.tif41150
[0037] <3> Experimental results (Tables 3 to 7) The results and evaluations of each experimental example will be explained with reference to Tables 3 to 7.
[0038] (1) Comparison of wire diameters (Table 3) [Table 3] JPEG2024163457000004.jpg73164
[0039] As shown in Table 3, for wires with a wire diameter of φ2.0 mm that were subjected to the first wiredrawing process, some wires were given an evaluation of A, as in Experimental Examples 3 and 4. However, for wires that were reduced in diameter to φ0.31 mm by the second wiredrawing process (step (g)), a good elongation [%] could not be achieved, and they did not achieve an evaluation of A. This shows that as the wire diameter is reduced by the wiredrawing process, it tends to become more difficult to ensure the elongation [%].
[0040] (2) Step (h) omitted (Table 4) [Table 4] JPEG2024163457000005.jpg73164
[0041] As shown in Table 4, in the wire having a wire diameter of φ0.31 mm, the wires according to Experimental Examples 8 to 18 in which step (h) was not carried out were unable to obtain a good elongation [%] and did not reach the evaluation A. This shows that simply not carrying out step (h) and instead applying a heat treatment temperature similar to that in step (f) for a long period of time in step (i) will not result in an improvement in elongation [%].
[0042] (3) Comparison with and without step (i) (1) (Table 5) [Table 5] JPEG2024163457000006.jpg73164
[0043] As shown in Table 5, in the case of a wire having a wire diameter of φ0.31 mm, in Experimental Examples 23 to 28 in which step (i) was further added to step (h), the elongation [%] was improved and the wire was rated B. In addition, compared to Experimental Example 19 in which step (i) was omitted, the examples in which the heat treatment time for step (h) was extended (Experimental Example 20) and the heat treatment temperature for step (h) were increased (Experimental Example 21) did not achieve an evaluation of A. This shows that a combination of steps (h) and (i) after the wire drawing process in step (g) is likely to produce good results.
[0044] (4) Comparison with and without step (i) (2) (Table 6) Table 6 shows that the heat treatment temperature in step (f) in Table 5 is changed from 110°C to 130°C. [Table 6] JPEG2024163457000007.jpg73164
[0045] As shown in Table 6, in experimental examples 33 to 38, in which step (i) was added to step (h) for a wire having a wire diameter of φ0.31 mm, a further improvement in tensile strength [MPa] was observed compared to experimental examples 23 to 28, resulting in an evaluation of A. Moreover, Experimental Example 32, in which step (i) was omitted, was given an evaluation of B. In addition, compared to Experimental Example 29 in which step (i) was omitted, the experiments in which the heat treatment time in step (h) was extended (Experimental Example 30) and the heat treatment temperature in step (h) were increased (Experimental Example 31) did not achieve an evaluation of A.
[0046] (5) Steps (c) and (i) omitted (Table 7) [Table 7] JPEG2024163457000008.jpg73164
[0047] As shown in Table 7, for a wire having a diameter of φ0.31 mm, none of Experimental Examples 39 to 42, which did not involve steps (c) and (i), achieved an evaluation of A, but Experimental Examples 41 and 42 achieved an evaluation of B.
[0048] In addition, in Experimental Examples 39 to 42, the heat treatment temperature in step (f) was 120°C. Even if the heat treatment temperature was changed to 110°C or 130°C, there is a high possibility that an evaluation of A would not be achieved. This can be inferred from the fact that Experimental Examples 19, 20, 29, and 30, shown in Tables 5 and 6, did not yet achieve an evaluation of A. EXAMPLES
[0049] Next, a second embodiment of the present invention will be described.
[0050] <1> Experimental conditions (Figure 2) As a test material, a φ9.5 mm rough wire of an aluminum alloy containing 0.55 wt % Mg, 0.57 wt % Si, and the remainder being Al and unavoidable impurities was used, and the following steps were carried out. Step (a) Solution treatment at 540°C for 7.2ks (2 hours). Step (b) Quenching in water at room temperature. Step (c) Cluster (1) is formed by pre-aging at 4°C for 604.8ks (1 week). Step (d) Drying at 90°C for 10.8ks (3 hours). Step (e) Wire drawing to φ2.0 mm. Step (f) Heat treatment at 110°C for 86.4ks (24 hours). Step (g) Wire drawing to φ0.31 mm. Step (h) Recrystallize by heat treatment at 300°C for a maximum of 0.6ks (maximum of 5 minutes). Therefore, the steps according to this embodiment are equivalent to carrying out the steps (S100) to (S800) shown in FIG. FIG. 2 shows the processing and heat treatment history of the aluminum alloy wire that underwent this process (hereinafter referred to as “0.31 Annealed material”).
[0051] The aging precipitation behavior of these samples was analyzed by differential scanning calorimetry (DSC), the texture and recrystallization behavior were observed by electron backscatter diffraction (EBSD), and the mechanical properties were evaluated by tensile tests. Furthermore, the electrical conductivity was calculated and evaluated by measuring the electrical resistivity using a DC four-terminal method.
[0052] <2> Experimental results (Figs. 3 to 5) (1) DSC measurement results (Figure 3) Figure 3 shows the results of DSC measurements of a sample drawn to φ2.0 mm (hereafter referred to as 2.0H material), a sample that was subsequently heat-treated at 130°C (hereafter referred to as 2.0IHT material), a sample drawn to φ0.31 mm (hereafter referred to as 0.31H material), and a 0.31Annealed material. Exothermic peaks A, C, D, and E indicate the release of strain energy, the precipitation of the β″ phase, the precipitation of the β′ phase, and the precipitation of the β phase, respectively. Endothermic peak B indicates the restoration of Cluster(1). Since the exothermic peak C did not change in the 2.0 IHT material, it is considered that the formation of Cluster (1) during pre-aging suppressed the formation of Cluster (2) and the precipitation of the β″ phase. The endothermic peak B decreased as the degree of drawing during wire drawing increased, indicating that some of Cluster(1) was restored by wiredrawing. This is presumably because the dislocations introduced by the wire drawing process sheared Cluster(1), reducing the thermal stability of Cluster(1). In addition, since the endothermic peak B disappeared in the 0.3 Annealed material, it is considered that Cluster(1) was completely restored. Furthermore, since the exothermic peak C has also disappeared, it is considered that the precipitation of the β″ phase has also been completed. On the other hand, since no change was observed in exothermic peak D, it is inferred that no precipitation of the β′ phase occurred.
[0053] (2) EBSD measurement results (Fig. 4) Figure 4 shows the inverse pole figure orientation map (IPF map) of the crystal plane perpendicular to the wiredrawing direction (DD) based on the EBSD measurement results. In the 2.0H, 2.0IHT, and 0.31H materials, the wire drawing process is suspected to be the cause. <111> A fiber texture was observed. In the 0.31 Annealed material, recrystallization structure is formed, and the fiber texture is <111> Elongated grains that maintained their orientation and equiaxed grains with relatively random orientation were observed. The former is considered to be a continuous recrystallization structure in which new crystal grains are generated only during the substantial recovery process due to the Zenerdrag effect, in which the pinning effect of precipitates inhibits grain boundary migration during heat treatment. The latter is considered to be a discontinuous recrystallization in which new crystal grains are generated by grain boundary migration, using subgrains generated during the recovery process as nuclei. This suggests that in this heat treatment process, precipitation of the β″ phase occurs simultaneously with recrystallization, and that the precipitation state of the β″ phase affects the recrystallization behavior.
[0054] (3) Breaking elongation and maximum tensile strength measurements (Fig. 5) The breaking elongation and ultimate tensile strength of each sample are shown in FIG. The 0.31H material had a maximum tensile strength of 518 MPa and a breaking elongation of 2.6%, while the 0.31Annealed material had values of 157 MPa and 11.3%, respectively, showing a significant improvement in ductility. In addition, the electrical conductivity of the 0.31 Annealed material was 60% IACS, which was a very large value for an Al-Mg-Si alloy wire. This is presumably due to the formation of Cluster(1) and the coarse precipitation of the β″ phase caused by the 300°C heat treatment, which reduced the amount of solid solution in the Al matrix. Therefore, it is considered that short-time annealing at 300°C can simultaneously achieve both improved ductility due to the recrystallization of the fiber texture and improved electrical conductivity due to the coarse precipitation.
[0055] <3> summary The changes in nanoclusters and the recrystallization behavior of an Al-Mg-Si alloy wire in which Cluster(1) was formed by preliminary aging (step (c)) were investigated. As a result, it was found that the formation of Cluster(1) suppresses the precipitation of the β″ phase during intermediate heat treatment, and that if the wire drawing is large, part of Cluster(1) is restored. In addition, it was revealed that when heat treatment (step (h)) was performed at 300°C after wire drawing (step (g)), the restoration of Cluster(1) and the precipitation of the β″ phase were completed within 0.3ks, and recrystallization of the fiber texture began. Therefore, this process has the potential to significantly improve ductility and electrical conductivity.
[0056] The invention made by the inventor has been specifically described above based on an embodiment, but the present invention is not limited to the above embodiment and can be modified within the scope of the gist of the invention.
[0057] For example, the present invention can be applied to the case where an aluminum alloy other than that having the composition shown in the embodiment is used.
[0058] Furthermore, the embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Industrial Applicability]
[0059] According to the present invention, it is possible to obtain an aluminum alloy wire having properties particularly suitable for use in wire harnesses.
Claims
1. For Al-Mg-Si aluminum alloy wires, (a) performing a solution treatment; (b) performing a quenching treatment; (c) performing a preliminary aging treatment; (e) performing a first wiredrawing process; (f) subjecting the resultant to a heat treatment; (g) performing a second wire drawing process; (h) performing a heat treatment; At least The step (h) is a heat treatment that does not involve solution treatment of the aluminum alloy wire. A method for manufacturing aluminum alloy wire.
2. Between the step (c) and the step (e), (d) subjecting the resulting product to a heat treatment; The step (d) is a heat treatment for suppressing the generation of Cluster (1) and the precipitation of the β″ phase. The method for producing the aluminum alloy wire according to claim 1 .
3. After the step (h), (i) subjecting the resulting product to a heat treatment; The step (i) is a heat treatment that does not involve solution treatment of the aluminum alloy wire and is performed at a temperature lower than the heating temperature in the step (h). The method for producing the aluminum alloy wire according to claim 2 .
4. In the step (f), the heat treatment temperature is 180° C. or less, and the heat treatment time is 7 hours or more; In the step (h), the heat treatment temperature is 250 to 350° C., and the heat treatment time is 5 minutes or more; In the step (i), the heat treatment temperature is 130 to 150° C., and the heat treatment time is 30 minutes to 10 hours. The method for producing the aluminum alloy wire according to claim 3.
5. The aluminum alloy wire after the step (i) has a wire diameter of less than 2 mm, an ultimate tensile strength of 150 MPa or more, an elongation of 8% or more, and an electrical conductivity of 50% IACS or more. The method for producing an aluminum alloy wire according to claim 4.
6. An Al-Mg-Si based aluminum alloy wire, The wire has a wire diameter of less than 2 mm, an ultimate tensile strength of 150 MPa or more, an elongation of 8% or more, and an electrical conductivity of 50% IACS or more. Aluminum alloy wire.
Citation Information
Patent Citations
Supporting body having layered structure to be used for photoconductive member
JP1989062662A