Process oil for rubber
A poly-internal olefin-based process oil addresses the insufficient processability of conventional paraffin oil by enhancing kneading performance and compatibility with rubber materials through specific physical property adjustments.
Patent Information
- Application Number
- JP2024077287
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-22
AI Technical Summary
Conventional paraffin oil does not sufficiently improve the processability of rubber materials, particularly in applications like automobile tires.
A process oil for rubber is developed using a poly-internal olefin with specific average DBP values and carbon numbers, along with defined physical properties such as flash point, pour point, and kinematic viscosity, to enhance compatibility and processability.
The poly-internal olefin-based process oil significantly improves the processability of rubber compositions, leading to better kneading performance and compatibility with rubber materials.
Smart Images

Figure 2024163893000001 
Figure 2024163893000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a process oil for rubber. [Background technology]
[0002] Rubber materials used in automobile tires and the like are blended with extender oils, process oils, etc., for the purpose of improving processability, etc. It is known that paraffin oil is used as a process oil (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-25370 Summary of the Invention [Problem to be solved by the invention]
[0004] However, conventional paraffin oils do not sufficiently improve processability, and there is room for improvement.
[0005] An object of the present invention is to provide a process oil for rubber which is more excellent in improving processability than conventional paraffin oils. [Means for solving the problem]
[0006] The present invention relates to a process oil for rubber containing a polyinternal olefin, wherein the polyinternal olefin is an olefin polymer containing an internal olefin, the olefin has an average DBP value of 3 or more and 6 or less, and the olefin has an average carbon number of 16 or more and 20 or less. Effect of the Invention
[0007] According to the present invention, it is possible to provide a process oil for rubber which is more excellent in improving processability than conventional paraffin oils. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Rubber processing oil> The rubber process oil of this embodiment is a rubber process oil containing a polyinternal olefin, the polyinternal olefin being an olefin polymer containing an internal olefin, the olefin having an average DBP value of 3.0 or more and 6.0 or less, and the olefin having an average carbon number of 16 or more and 20 or less. The rubber process oil of this embodiment is superior in improving processability to conventional paraffin oils.
[0009] [Polyinternal olefin] The DBP average value (average value of double bond positions) in the olefin containing the internal olefin is 3.0 or more, preferably 3.2 or more, more preferably 3.4 or more, and even more preferably 3.8 or more, from the viewpoint of lowering the pour point, and is 6.0 or less, preferably 5.5 or less, more preferably 5.0 or less, and even more preferably 4.5 or less, from the viewpoint of reducing the torque during kneading. In this specification, the DBP average value in the olefin is measured by the method described in the Examples.
[0010] The average carbon number of the olefin containing the internal olefin is, from the viewpoint of compatibility with the rubber material, 16 or more, preferably 17 or more, and more preferably 18 or more, and from the same viewpoint, is 20 or less, and more preferably 18 or less.
[0011] From the viewpoint of the safety of the working environment, the flash point of the polyinternal olefin is preferably 250° C. or higher, and more preferably 260° C. or higher. The flash point of the polyinternal olefin is 300° C. or lower. In this specification, the flash point means a flash point measured in accordance with JIS K 2265.
[0012] The pour point of the polyinternal olefin is preferably −35° C. or higher, more preferably −30° C. or higher, and even more preferably −20° C. or higher from the viewpoint of compatibility with rubber materials, and is preferably 0° C. or lower, more preferably −10° C. or lower from the viewpoint of handling. In this specification, the pour point means the pour point measured in accordance with JIS K 2269.
[0013] The kinetic viscosity of the polyinternal olefin at 100°C is set to 40mm from the viewpoint of compatibility with rubber materials. 2 / s or more is preferable, 45mm 2 / s or more is preferable, and 50 mm 2 / s or more is more preferable, and from the viewpoint of handling, 75 mm 2 / s or less is preferable, 70 mm 2 / s or less is preferable, 65 mm 2 In this specification, the kinetic viscosity refers to a kinetic viscosity measured in accordance with JIS K 2283.
[0014] The kinetic viscosity of the polyinternal olefin at 40°C is 7.0 mm from the viewpoint of compatibility with rubber materials. 2 / s or more is preferable, 7.5 mm 2 / s or more is preferable, and 8.2 mm 2 / s or more is more preferable, and from the viewpoint of handling, 14.0 mm 2 / s or less is preferable, 12.0 mm 2 / s or less is preferable, and 10.5 mm 2 / s or less is even more preferable.
[0015] The density of the polyinternal olefin at 25° C. is 0.7 g / cm from the viewpoint of compatibility with rubber materials. 3 More than 0.8 g / cm is preferable. 3 More preferably, from the viewpoint of handling, 0.95 g / cm 3 Less than 0.90 g / cm is preferred. 3 The following is more preferred: In this specification, the density at 25° C. means the pour point measured in accordance with JIS K 2249-1.
[0016] The polyinternal olefin can be obtained by polymerizing an olefin containing the internal olefin by a known method. From the viewpoint of plasticization performance, the content of the internal olefin in the olefin containing the internal olefin is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 100% by mass. The polyinternal olefin may be hydrogenated.
[0017] From the viewpoint of plasticization performance, the content of the polyinternal olefin in the rubber process oil is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, still more preferably substantially 100% by mass, and even more preferably 100% by mass. In this specification, "substantially 100% by mass" refers to a state in which a trace amount of impurities and the like is inevitably contained.
[0018] <Rubber composition> The rubber composition of the present embodiment contains the above-mentioned rubber process oil as a process oil. The rubber contained in the rubber composition preferably contains a conjugated diene rubber from the viewpoints of moldability, heat resistance, abrasion resistance, mechanical strength, and the like of the rubber molded body.
[0019] The conjugated diene rubber may be one or more selected from the group consisting of butadiene rubber (BR), styrene-butadiene rubber (SBR), natural rubber (NR), isoprene rubber (IR), acrylonitrile-butadiene rubber (NBR), styrene-butadiene-isoprene rubber (SBIR), styrene-isoprene rubber (SIR), styrene-isoprene-butadiene rubber (SIBR), hydrogenated butadiene rubber, hydrogenated styrene-butadiene rubber, etc., and among these, one or more selected from the group consisting of natural rubber and styrene-butadiene rubber are preferred. That is, the rubber process oil may be one or more conjugated diene rubber process oils selected from the group consisting of natural rubber and styrene-butadiene rubber.
[0020] The content of the polyinternal olefin in the rubber composition is preferably 0.2 mass % or more, more preferably 5 mass % or more, from the viewpoint of plasticization performance, and is preferably 40 mass % or less, more preferably 30 mass % or less, from the viewpoint of suppressing bleed-out.
[0021] The rubber composition may further contain various reinforcing agents, fillers, vulcanization accelerators, vulcanization aids, etc., which are used in the rubber industry.
[0022] The rubber composition can be produced by a known method for producing a rubber composition, except for using the rubber process oil.
[0023] <Rubber molded body> The rubber molded article of the present embodiment is produced by crosslinking the rubber composition. The rubber molded article can be produced by crosslinking the rubber composition by a known method.
[0024] The rubber molded product can be suitably used for various applications, for example, as a material for various tire parts such as a cap tread, a base tread, a carcass, a sidewall, a bead portion, a hose, a belt, a mat, an anti-vibration rubber, a paint, and various other industrial products.
[0025] In relation to the above-mentioned embodiment, the present invention further discloses the following compositions, etc.
[0026] <1> A process oil for rubber containing polyinternal olefin, The polyinternal olefin is an olefin polymer containing an internal olefin, The DBP average value of the olefin is 3.0 or more and 6.0 or less, The average carbon number of the olefin is 16 or more and 20 or less. <2> The DBP average value (average value of double bond positions) in the olefin containing the internal olefin is 3.0 or more, preferably 3.2 or more, more preferably 3.4 or more, and even more preferably 3.8 or more, and is 6.0 or less, preferably 5.5 or less, more preferably 5.0 or less, and even more preferably 4.5 or less. <1> 2. The rubber process oil according to claim 1 . <3> The average carbon number of the olefin containing the internal olefin is 16 or more, preferably 17 or more, more preferably 18 or more, and is 20 or less, more preferably 18 or less. <1> or <2> 2. The rubber process oil according to claim 1 . <4> The flash point of the polyinternal olefin is preferably 250° C. or higher, more preferably 260° C. or higher, and is 300° C. or lower. <1> ~ <3> 10. The process oil for rubber according to claim 9 . <5> The pour point of the polyinternal olefin is preferably -35°C or higher, more preferably -30°C or higher, and even more preferably -20°C or higher, and is preferably 0°C or lower, and more preferably -10°C or lower. <1> ~ <4> 10. The process oil for rubber according to claim 9 . <6> The polyinternal olefin has a kinetic viscosity of 40 mm at 100°C. 2 / s or more is preferable, 45mm 2 / s or more is preferable, and 50 mm 2 / s or more is more preferable, and 75 mm 2 / s or less is preferable, 70 mm 2 / s or less is preferable, 65 mm 2 / s or less is more preferable, <1> ~ <5> 10. The process oil for rubber according to claim 9 . <7> The polyinternal olefin has a kinetic viscosity of 7.0 mm at 40°C. 2 / s or more is preferable, 7.5 mm 2 / s or more is preferable, and 8.2 mm 2 / s or more is more preferable, and 14.0 mm 2 / s or less is preferable, 12.0 mm 2 / s or less is preferable, and 10.5 mm 2 / s or less is more preferable, <1> ~ <6> 10. The process oil for rubber according to claim 9 . <8> The density of the polyinternal olefin at 25° C. is 0.7 g / cm 3 More than 0.8 g / cm is preferable. 3 More preferably, 0.95 g / cm 3 Less than 0.90 g / cm is preferred. 3 The following is more preferred: <1> ~ <7> 10. The process oil for rubber according to claim 9 . <9> The content of the internal olefin in the olefin containing the internal olefin is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and still more preferably 100% by mass. <1> ~ <8> 10. The process oil for rubber according to claim 9 . <10> The content of the polyinternal olefin in the rubber process oil is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, still more preferably substantially 100% by mass, and still more preferably 100% by mass. <1> ~ <9> 10. The process oil for rubber according to claim 9 . <11> The rubber process oil is a process oil for one or more conjugated diene rubbers selected from the group consisting of natural rubber and styrene-butadiene rubber. <1> ~ <10> 10. The process oil for rubber according to claim 9 . <12> <1> ~ <11> 2. A rubber composition comprising the rubber process oil according to claim 1 . <13> The content of the polyinternal olefin in the rubber composition is preferably 0.2% by mass or more, more preferably 5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less. <12> The rubber composition according to claim 1. <14> <12> or <13> A rubber molded article obtained by crosslinking the rubber composition described in claim 1. EXAMPLES
[0027] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Various measurement and evaluation methods are as follows.
[0028] <Measurement method> [Method for measuring the distribution of double bonds in olefins] The double bond distribution of olefins was measured by gas chromatography (hereinafter abbreviated as GC). Specifically, olefins were reacted with dimethyl disulfide to produce dithiolated derivatives, and each component was then separated by GC. The double bond distribution of olefins was determined from each peak area. The equipment and analytical conditions used for the measurement are as follows: GC device: Product name HP6890 (manufactured by Hewlett Packard) Column: Product name: Ultra-Alloy-1HT capillary column 30m x 250μm x 0.15μm (manufactured by Frontier Labs) Detector: Flame ionization detector (FID) Injection temperature: 300℃ Detector temperature: 350℃ Oven: 60℃ (0 min) → 2℃ / min → 225℃ → 20℃ / min → 350℃ → 350℃ (5.2 min)
[0029] [Calculation method for DBP average value (average value of double bond positions)] For example, if the double bond distribution is C1 position: a mass %, C2 position: b mass %, C3 position: c mass %, C4 position: d mass %, C5 position: e mass %, C6 position: f mass %, C7 position: g mass %, C8 position: h mass %, C9 position: i mass % (total 100 mass %), the DBP average value is (1×a+2×b+3×c+4×d+5×e+6×f+7×g+8×h+9×i) / 100 When multiple peaks overlap, the area was allocated equally to each peak and the average DBP value was calculated.
[0030] [Method for measuring the content ratio of structural isomers] Mix 0.05g of alkyl glyceryl ether, 0.2g of trifluoroacetic anhydride, and 1g of deuterated chloroform, 1 Measurement was performed by H-NMR under the following conditions: Nuclear magnetic resonance spectrometer: Agilent 400-MR DD2, manufactured by Agilent Technologies Observation range: 6410.3Hz Data points: 65536 Measurement mode: Presat Pulse width: 45° Pulse delay time: 10sec Number of times accumulated: 128 times
[0031] [Various physical properties related to polyinternal olefin] [Density at 25℃] Measurements were performed in accordance with JIS K 2249-1.
[0032] [Kinematic viscosity] The kinematic viscosity was evaluated using a Stabinger kinematic viscometer (SVM3000, manufactured by Anton Paar) that meets the accuracy requirements of ASTM D7042, and was measured at 40°C and 100°C (mm 2 / s) was measured.
[0033] [Pour point] Measurements were performed in accordance with JIS K 2269.
[0034] [flash point] Measurements were performed using the Cleveland open cup (COC) method in accordance with JIS K 2265.
[0035] <Production Example of Olefin Containing Internal Olefin> [Production Example of Olefin 1 Containing an Internal Olefin Having 18 Carbon Atoms] In a flask equipped with a stirrer, 7000g (25.9 moles) of 1-octadecanol (Kao Corporation, Kalcol 8098) as the raw material alcohol and 700g (10% by mass based on the raw material alcohol) of γ-alumina (STREM Chemicals, Inc.) as the solid acid catalyst were charged, and the reaction was carried out for 10 hours at 280°C while circulating nitrogen (7L / min) in the system under stirring. After the reaction was completed, the alcohol conversion rate was 100% and the C18 internal olefin purity was 98.2%. The obtained crude C18 internal olefin was transferred to a distillation flask and distilled at 148-158°C / 0.5mmHg to obtain an olefin (olefin 1) containing C18 internal olefin with an olefin purity of 100%. The double bond distribution of the obtained olefin 1 was 0.8% by mass at C1, 31.3% by mass at C2, 22.9% by mass at C3, 15.5% by mass at C4, 10.8% by mass at C5, 7.2% by mass at C6, 5.3% by mass at C7, and 6.2% by mass in total at C8 and C9. The average DBP value was about 3.8.
[0036] [Production Example of Olefin 2 Containing Internal Olefin of Carbon Number 16] In a flask equipped with a stirrer, 7000g (28.9 moles) of 1-hexadecanol (Kao Corporation, Kalcol 6098) as the raw material alcohol and 700g (10% by mass based on the raw material alcohol) of γ-alumina (STREM Chemicals, Inc.) as the solid acid catalyst were charged, and the reaction was carried out for 5 hours at 280°C while circulating nitrogen (7L / min) in the system under stirring. After the reaction was completed, the alcohol conversion rate was 100% and the C16 internal olefin purity was 99.7%. The obtained crude C16 internal olefin was transferred to a distillation flask and distilled at 136-160°C / 4.0mmHg to obtain an olefin (olefin 2) containing C16 internal olefin with an olefin purity of 100%. The double bond distribution of the obtained olefin 2 was 0.5% by mass at C1, 16.5% by mass at C2, 15.4% by mass at C3, 16.4% by mass at C4, 17.2% by mass at C5, 14.2% by mass at C6, and 19.8% by mass in total at C7 and C8. The average DBP value was about 4.7.
[0037] <Production example of polyinternal olefin> [Production Example of Polyinternal Olefin 1] A reactor equipped with a stirrer was charged with 2.21 moles of the olefin 1 and 0.11 moles of aluminum chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a catalyst, and the mixture was stirred at 120°C for 10 hours under a nitrogen atmosphere to carry out a reaction. Then, 88 g of a 15% by mass aqueous solution of sodium hydroxide was added and stirred to deactivate the catalyst, followed by washing with water. The light components were then removed at 180°C and 5 torr (gauge pressure) to obtain polyinternal olefin 1.
[0038] [Production Example of Hydrogenated Polyinternal Olefin 1] A reactor equipped with a stirrer was charged with 2207 g of the polyinternal olefin 1 and 225 g of nickel catalyst (manufactured by Nikko Rica Corporation), and the reaction was carried out for 10 hours with stirring at a rotation speed of 600 rpm under a hydrogen flow rate of 5.0 L / min, a pressure of 2.0 MPa, and 200° C. The catalyst was then removed by filtration to obtain hydrogenated polyinternal olefin 1.
[0039] [Production Example of Polyinternal Olefin 2] Polyinternal olefin 2 was prepared in the same manner as for polyinternal olefin 1, except that olefin 2 was used instead of olefin 1 as a raw material.
[0040] [Production Example of Hydrogenated Polyinternal Olefin 2] A reactor equipped with a stirrer was charged with 2448 g of polyinternal olefin 2 and 50 g of nickel catalyst (manufactured by Nikko Rica Corporation), and the reaction was carried out for 18 hours with stirring at a rotation speed of 600 rpm, a hydrogen flow rate of 5.0 L / min, a pressure of 2.0 MPa, and 200°C. The catalyst was then removed by filtration to obtain hydrogenated polyinternal olefin 2.
[0041] Various physical properties of the above polyinternal olefins and the like are shown in Table 1. In addition, Oil 1 and Oil 2 in Table 1 have the following meanings. Oil 1: Naphthenic process oil, manufactured by Nippon Sun Oil Co., Ltd., product name: SUNTHENE 410 Oil 2: Paraffin oil, manufactured by EXXONMOBIL, product name: PAO8
[0042] [Table 1]
[0043] <Production Examples of Rubber Composition and Rubber Molded Article> The components other than zinc oxide, sulfur, and vulcanization accelerator shown in Table 2 were mixed in the formulation shown in Table 2 using a Banbury mixer (manufactured by Toyo Seiki Co., Ltd., Labo Plastomill 10C100, capacity 600cc) at a rotation speed of 70 rpm and a maximum temperature of 150°C for 4 minutes (mixing 1), to obtain kneaded products according to each of the Examples and Comparative Examples. Zinc oxide, sulfur, and vulcanization accelerator were added to each of the kneaded products, and the mixture was kneaded for 2 minutes at a maximum temperature of 100°C, to obtain unvulcanized rubber compositions according to each of the Examples and Comparative Examples. The obtained unvulcanized rubber compositions were heated at 145°C for 20 minutes to obtain sheet-shaped vulcanized rubber moldings according to each of the Examples and Comparative Examples.
[0044] <Evaluation method> [Evaluation of processability] The torque at the end of kneading 1 was measured, and the torque was expressed as a relative value with the comparative example corresponding to each example being set at 100. Specifically, the values of Examples 1 to 4 are expressed as relative values to Comparative Example 1, and the values of Examples 5, 6 and Comparative Example 3 are expressed as relative values to Comparative Example 2. The smaller the value, the better the processability. The evaluation results are shown in Table 2.
[0045] [Table 2]
[0046] The notations in Table 2 have the following meanings: SBR: Zeon Corporation, emulsion-polymerized styrene-butadiene rubber, product name: NIPOL 1502, styrene content 23.5% by mass Natural rubber: RSS #3 Oil 1: Naphthenic process oil, manufactured by Nippon Sun Oil Co., Ltd., product name: SUNTHENE 410 Oil 2: Paraffin oil, manufactured by EXXONMOBIL, product name: PAO8 Silica: Tosoh Silica Corporation, product name: Nipsil AQ, BET specific surface area 205 m 2 / g Carbon black: HAF, manufactured by Tokai Carbon Co., Ltd., product name: Seast 3, DBP absorption capacity 101 cm 3 / 100g, N 2 AS:79m 2 / g Silane coupling agent: Bis(3-triethoxysilylpropyl)tetrasulfide, manufactured by Evonik, trade name: Si69 Antioxidant: N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name: Nocrac 6C Stearic acid: Kao Corporation, product name: Lunac S-70V Zinc oxide: Fujifilm Wako Pure Chemical Industries, zinc oxide (first grade) Sulfur: Fujifilm Wako Pure Chemical Industries, sulfur (powder, chemical grade) Vulcanization accelerator 1: Sulfenamide vulcanization accelerator, N-cyclohexyl-2-benzothiazolyl sulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name: Noccela CZ-G Vulcanization accelerator 2: Guanidine-based vulcanization accelerator, 1,3-diphenylguanidine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name: Noccelaer D
Claims
1. A process oil for rubber containing polyinternal olefin, The polyinternal olefin is an olefin polymer containing an internal olefin, The DBP average value of the olefin is 3.0 or more and 6.0 or less, The average carbon number of the olefin is 16 or more and 20 or less.
2. 2. The rubber process oil according to claim 1, wherein the content of the polyinternal olefin in the rubber process oil is 70 mass% or more.
3. 2. The process oil for rubber according to claim 1, wherein the pour point of the polyinternal olefin is from -35°C to 0°C.
4. The rubber process oil according to claim 1, wherein the rubber process oil is a process oil for one or more conjugated diene rubbers selected from the group consisting of natural rubber and styrene-butadiene rubber.
5. A rubber composition comprising the rubber process oil according to any one of claims 1 to 4.
6. The rubber composition according to claim 5 , wherein the content of the polyinternal olefin in the rubber composition is from 0.2% by mass to 40% by mass.
7. A rubber molded article obtained by crosslinking the rubber composition according to claim 5.