Resin composition, dielectric substrate, and microstrip antenna

The use of spherical titanium-based materials in resin compositions addresses the fluidity and moldability issues of conventional dielectric substrates, enabling improved productivity and performance of dielectric substrates and microstrip antennas for high-frequency communication equipment.

JP2024164519AInactive Publication Date: 2024-11-27SUMITOMO BAKELITE CO LTD

Patent Information

Application Number
JP2023080058
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional resin compositions used in dielectric substrates for antennas suffer from inadequate fluidity and moldability, which hinders the miniaturization and performance of communication equipment.

Method used

A resin composition containing a spherical titanium-based material, such as spherical calcium titanate or titanium oxide, with specific particle size and circularity ranges, along with a thermosetting resin and curing agents, to enhance fluidity and moldability, resulting in improved mechanical strength and dielectric properties.

Benefits of technology

The composition exhibits excellent fluidity and moldability, leading to enhanced productivity of dielectric substrates and microstrip antennas with balanced mechanical strength and dielectric performance, suitable for high-frequency applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164519000016
    Figure 2024164519000016
  • Figure 2024164519000017
    Figure 2024164519000017
  • Figure 2024164519000001
    Figure 2024164519000001
Patent Text Reader

Abstract

To provide a resin composition that offers superior fluidity and moldability, contributing to improving the productivity of a dielectric substrate and a microstrip antenna.SOLUTION: A resin composition contains an inorganic filler (A) containing spherical titanium materials (a). During torque measurement over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C, the minimum torque value is 2.0 N m or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a dielectric substrate, and a microstrip antenna. [Background technology]

[0002] In recent years, wireless communication has become faster, and there is a demand for higher performance and smaller communication devices. Furthermore, the capacity of wireless communication has increased dramatically in recent years, and the frequency of transmission signals is rapidly becoming wider and higher. As a result, the frequency band used by communication devices is no longer compatible with the microwave band that has been used traditionally, and is expanding to the millimeter wave band. Against this background, there is a strong demand for higher performance antennas installed in communication devices.

[0003] Communication devices can be made even smaller when the dielectric constant of the antenna material (dielectric substrate) incorporated inside the communication device is increased. As antenna materials become smaller, the resin composition used to form the antenna material is required to have excellent moldability.

[0004] Patent Document 1 discloses a molding resin composition used for sealing electronic components in high-frequency devices, which contains an epoxy resin, a curing agent, and an inorganic filler containing a predetermined amount of calcium titanate particles, strontium titanate particles, silica particles, or alumina particles. The document describes that a specific filler such as calcium titanate particles is amorphous, and reduces the fluidity and moldability of the resin composition (paragraph 0015). In addition, polyhedral calcium titanate particles are used in the examples (paragraph 0103).

[0005] Patent Document 2 discloses a resin composition containing a thermosetting resin and a high dielectric constant filler selected from calcium titanate, strontium titanate, etc. The document describes the shape of the high dielectric constant filler as granular, amorphous, or flaky (paragraph 0027). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 6870778 [Patent Document 2] International Publication No. 2022 / 202804 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the conventional techniques described in Patent Documents 1 and 2, there is room for improvement in the flowability and moldability of the resin composition. [Means for solving the problem]

[0008] The present inventors have found that a resin composition containing a spherical titanium-based material has improved flowability and moldability by satisfying certain characteristics, and have completed the present invention. That is, the present invention can be shown as follows.

[0009] [1] A resin composition containing an inorganic filler (A) including a spherical titanium-based material (a), A resin composition having a minimum torque value of 2.0 N·m or less when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C. [2] The resin composition according to [1], wherein the spherical titanium-based material (a) contains spherical calcium titanate (a1). [3] The resin composition according to [2], wherein the spherical titanium-based material (a) contains spherical titanium oxide (a2). [4] The resin composition according to any one of [1] to [3], wherein, when the cure torque value at 175°C is measured over time using a curastometer, the time from the start of measurement until the cure torque value reaches 1 kgf cm is 30 seconds or more and 80 seconds or less. [5] The resin composition according to any one of [1] to [4], which has a rectangular pressure of 0.5 MPa or less as measured by the following method. (method) Using a low pressure transfer molding machine, the mold temperature was 175℃ and the injection speed was 177mm. 3 The resin composition is injected into a rectangular flow path having a width of 13 mm, a thickness of 1 mm, and a length of 175 mm under the condition of 1 / sec. At this time, the change in pressure over time is measured with a pressure sensor embedded at a position 25 mm from the upstream end of the flow path, and the minimum pressure (MPa) during the flow of the resin composition is measured and defined as the rectangular pressure. [6] The resin composition according to any one of [1] to [5], wherein a linear expansion coefficient CTE1 at a temperature lower than the glass transition temperature of a cured product of the resin composition is 10 ppm / °C or more and 30 ppm / °C or less. [7] The resin composition according to any one of [1] to [6], wherein a linear expansion coefficient CTE2 at a temperature equal to or higher than the glass transition temperature of a cured product of the resin composition is 60 ppm / °C or more and 90 ppm / °C or less. [8] The resin composition according to any one of [1] to [7], wherein a cured product of the resin composition has a flexural strength of 1 MPa or more at 260°C. [9] The resin composition according to any one of [1] to [8], wherein the cured product of the resin composition has a flexural modulus at 260°C of 1000 MPa or less.

[10] The resin composition according to any one of [1] to [9], wherein a cured product of the resin composition has a dielectric constant of 12 or more and a dielectric loss tangent (tan δ) of 0.005 or less at a frequency of 1 MHz.

[11] The resin composition according to [2], wherein the spherical calcium titanate (a1) has an average circularity of 0.92 or more.

[12] The resin composition according to [3], wherein the spherical titanium oxide (a2) has an average circularity of 0.88 or more.

[13] The resin composition according to any one of [1] to

[12] , wherein the resin composition contains 78% by mass or more of an inorganic filler (A) per 100% by mass of the resin composition.

[14] The spherical calcium titanate (a1) has particle sizes D5, D6, and D7 at which the cumulative frequency is 5%, 50%, and 95%, respectively, in a volume-based cumulative frequency distribution curve measured using a laser diffraction particle size distribution measuring device. 50 , D 95 The resin composition according to [2], wherein the above range is satisfied. Particle size D5: 0.1μm or less Particle size D 50 :1.0μm or more and 8.0μm or less Particle size D 95 :15μm or more and 30μm or less

[15] The spherical titanium oxide (a2) has particle sizes D5 and D6 at which the cumulative frequency is 5%, 50%, and 95%, respectively, in a volume-based cumulative frequency distribution curve measured using a laser diffraction particle size distribution measuring device. 50 , D 95 The resin composition according to [3], wherein the content is within the following range. Particle size D5: 1.5μm or less Particle size D 50 :2.0μm or more and 9.0μm or less Particle size D 95 :10μm or more and 30μm or less

[16] The resin composition according to any one of [1] to

[15] , further comprising a thermosetting resin (B).

[17] Further comprising a curing agent (C), The resin composition according to any one of [1] to

[16] , wherein the curing agent includes at least one selected from an active ester curing agent and a phenol curing agent.

[18] The resin composition according to any one of [1] to

[17] , further comprising a curing catalyst (D).

[19] The resin composition according to any one of [1] to

[18] , which is used as a material for forming a microstrip antenna.

[20] The resin composition according to any one of [1] to

[18] , which is used as a material for forming a dielectric waveguide.

[21] The resin composition according to any one of [1] to

[18] , which is used as a material for forming an electromagnetic wave absorber.

[22] A dielectric substrate obtained by curing the resin composition according to any one of [1] to

[18] .

[23] A dielectric substrate according to

[22] , a radiating conductor plate provided on one surface of the dielectric substrate; a ground conductor plate provided on the other surface of the dielectric substrate; A microstrip antenna comprising:

[24] A dielectric substrate, a radiating conductor plate provided on one surface of the dielectric substrate; a ground conductor plate provided on the other surface of the dielectric substrate; a high dielectric material disposed opposite the radiation conductor plate; A microstrip antenna comprising: A microstrip antenna, wherein the high dielectric constant material is a dielectric substrate as described in

[22] . Effect of the Invention

[0010] The resin composition of the present invention has excellent flowability and moldability, and use of the composition provides excellent productivity for dielectric substrates and antenna materials such as microstrip antennas. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a top perspective view showing the microstrip antenna of the present embodiment. [Diagram 2] 10 is a cross-sectional view showing another aspect of the microstrip antenna of the present embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present invention will be described with reference to the drawings. In all drawings, the same components are denoted by the same reference numerals, and the description will be omitted as appropriate. For example, "1 to 10" means "1 or more and 10 or less" unless otherwise specified.

[0013] The resin composition of the present embodiment contains an inorganic filler (A) that includes a spherical titanium-based material (a), and when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175° C., the minimum torque value can be 2.0 N·m or less, preferably 1.5 N·m or less, more preferably 1.0 N·m or less, and even more preferably 0.8 N·m or less. There are no particular limitations on the lower limit of the minimum torque value, but it is at least 0.05 N·m.

[0014] Since the resin composition contains the spherical titanium-based material (a) and the minimum torque value is within the above range, the resin composition has excellent fluidity and moldability, and the use of the composition provides excellent productivity for antenna materials such as dielectric substrates and microstrip antennas.

[0015] In this embodiment, the minimum torque value of the resin composition can be controlled by appropriately selecting the types and amounts of each component contained in the resin composition, the preparation method of the resin composition, etc.

[0016] [Inorganic filler (A)] As the inorganic filler (A) contained in the resin composition of this embodiment, any known inorganic filler can be used as long as the effects of the present invention are achieved, but it is preferable that the resin composition contains a spherical titanium-based material (a).

[0017] Examples of the spherical titanium-based material (a) include spherical titanium-based materials composed of titanium oxide, calcium titanate, strontium titanate, magnesium titanate, bismuth titanate, zirconium titanate, zinc titanate, calcium titanate zirconate, lead titanate zirconate, barium titanate, etc. These spherical titanium-based materials may be used alone or in combination of two or more kinds.

[0018] In this embodiment, the resin composition contains the spherical titanium-based material (a), and thus the resin composition has excellent fluidity and moldability, and the resulting cured product has excellent mechanical strength. In other words, these properties are well balanced. In general, the content of inorganic filler is reduced to improve fluidity and moldability, but the resulting cured product has a reduced mechanical strength. In contrast, the resin composition contains the spherical titanium-based material (a) as in this embodiment, and thus the mechanical strength of the cured product can be improved.

[0019] In this embodiment, the spherical titanium-based material (a) may be spherical calcium titanate (a1) or spherical titanium oxide (a2), and it is more preferable that the material contains spherical calcium titanate (a1).

[0020] The average circularity of the spherical calcium titanate (a1) is preferably 0.92 or more, more preferably 0.94 or more, and even more preferably 0.96 or more. The upper limit of the average circularity is not particularly limited, but may be 0.99 or less. When the average circularity is within the above range, the spherical calcium titanate (a1) particles slide smoothly between each other, resulting in further excellent fluidity, and further improved moldability and filling properties.

[0021] The circularity can be measured by a commercially available flow-type particle image analyzer. It can also be determined from a micrograph taken by a scanning electron microscope (SEM) or the like using image analysis processing software as follows. A photograph of a calcium titanate (a1) sample is taken, and the area and perimeter of calcium titanate (a1) (two-dimensional projection) are measured. Assuming that calcium titanate (a1) is a perfect circle, the circumference of a perfect circle having the measured area is calculated. The circularity is determined by the formula: circularity = circumference / perimeter. A circularity of 1 is a perfect circle. In other words, the closer the circularity is to 1, the closer it is to a perfect circle. The average circularity is calculated as the average circularity measured for 100 or more particles.

[0022] In addition, the spherical calcium titanate (a1) has particle diameters D5 and D6 at which the cumulative frequency is 5%, 50%, and 95%, respectively, in a volume-based cumulative frequency distribution curve measured using a laser diffraction particle size distribution measuring device. 50 , D 95 is preferably within the following range:

[0023] Particle size D5: 0.1 μm or less, preferably 0.07 μm or less, more preferably 0.04 μm or less Particle size D 50 : 1.0 μm or more and 8.0 μm or less, preferably 2.0 μm or more and 7.0 μm or less, more preferably 3.0 μm or more and 6.0 μm or less Particle size D 95 : 15 μm or more and 30 μm or less, preferably 17 μm or more and 28 μm or less, more preferably 19 μm or more and 26 μm or less

[0024] Particle size D5, D 50 , D 95 The spherical calcium titanate (a1) having a particle size distribution in the above range has an excellent balance of particle distribution, and is excellent in fluidity and moldability. In addition, since the spaces between the particles are filled, the spherical calcium titanate (a1) also has excellent mechanical properties.

[0025] The spherical titanium-based material (a) preferably contains spherical calcium titanate (a1) and spherical titanium oxide (a2). From the viewpoint of mechanical strength of the resulting cured product, it is preferable that the average particle size of the spherical titanium oxide (a2) is different from the average particle size of the spherical calcium titanate (a1).

[0026] The average circularity of the spherical titanium oxide (a2) is preferably 0.88 or more, more preferably 0.90 or more, and even more preferably 0.92 or more. The upper limit of the average circularity is not particularly limited, but can be 0.99 or less. The average circularity can be measured by the above-mentioned measuring method. By using spherical titanium oxide (a2) having the above average circularity together with spherical calcium titanate (a1) having the above average circularity, the slip between particles is further improved, the fluidity is further improved, and the moldability and filling properties are further improved.

[0027] In addition, the spherical titanium oxide (a2) has particle diameters D5 and D6 at which the cumulative frequency is 5%, 50%, and 95%, respectively, in a volume-based cumulative frequency distribution curve measured using a laser diffraction particle size distribution measuring device. 50 , D 95 is preferably within the following range:

[0028] Particle size D5: 1.5 μm or less, preferably 1.3 μm or less, more preferably 1.1 μm or less Particle size D 50 : 2.0 μm or more and 9.0 μm or less, preferably 3.0 μm or more and 8.0 μm or less, more preferably 4.0 μm or more and 7.0 μm or less Particle size D 95 : 10 μm or more and 30 μm or less, preferably 12 μm or more and 28 μm or less, more preferably 14 μm or more and 26 μm or less

[0029] The inorganic filler (A) may contain a non-spherical titanium-based material in addition to the spherical titanium-based material (a). Examples of the non-spherical titanium-based material include non-spherical titanium-based materials composed of titanium oxide, calcium titanate, strontium titanate, magnesium titanate, bismuth titanate, zirconium titanate, zinc titanate, calcium titanate zirconate, lead titanate zirconate, barium titanate, etc.

[0030] The shape of the non-spherical titanium-based material may be granular, amorphous, flake-like, etc. The non-spherical titanium-based material has an average particle diameter D 50 is preferably 0.1 μm or more and 50 μm or less, more preferably 0.3 μm or more and 20 μm or less, and further preferably 0.5 μm or more and 10 μm or less.

[0031] In this embodiment, the inorganic filler (A) may be contained in an amount of preferably 78% by mass or more, more preferably 79% by mass or more, and even more preferably 80% by mass or more in 100% by mass of the resin composition. The upper limit of the content of the inorganic filler (A) is not particularly limited, but is 90% by mass or less.

[0032] In this embodiment, from the viewpoint of the effect of the present invention, the spherical titanium-based material (a) can be contained in an amount of preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more in 100% by mass of the inorganic filler (A). The upper limit is not particularly limited, but can be 100% by mass or less, preferably 90% by mass or less.

[0033] In addition, the inorganic filler (A) may contain spherical calcium titanate (a1) in an amount of preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more in 100% by mass of the inorganic filler (A). The upper limit is not particularly limited, but may be 100% by mass or less, preferably 90% by mass or less.

[0034] In addition, when spherical calcium titanate (a1) and spherical titanium oxide (a2) are used in combination, the amount of spherical titanium oxide (a2) can be preferably 1 part by mass or more and 300 parts by mass or less, and more preferably 5 parts by mass or more and 100 parts by mass or less, per 100 parts by mass of spherical calcium titanate (a1).

[0035] In addition, the non-spherical titanium-based material may be contained in an amount of preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on 100% by mass of the inorganic filler (A). The upper limit is not particularly limited, but may be 99% by mass or less.

[0036] The resin composition of the present embodiment may further contain other inorganic fillers in addition to the inorganic filler (A) in order to reduce moisture absorption, reduce the linear expansion coefficient, improve thermal conductivity, and improve strength.

[0037] Other inorganic fillers include powders such as fused silica, crystalline silica, alumina, calcium silicate, calcium carbonate, potassium titanate, silicon carbide, silicon nitride, aluminum nitride, boron nitride, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, etc., or beads obtained by sphering these, glass fibers, etc. These inorganic fillers may be used alone or in combination of two or more kinds.

[0038] [Thermosetting resin (B)] The resin composition of the present embodiment may further contain a thermosetting resin (B). As the thermosetting resin (B), any known thermosetting resin can be used within the scope of the effects of the present invention, but one or more selected from cyanate resins, epoxy resins, resins having two or more radically polymerizable carbon-carbon double bonds in one molecule, and maleimide resins can be used. Among these, from the viewpoint of improving the effects of the present invention and the adhesiveness of the thermal conductive paste, it is particularly preferable to contain an epoxy resin (A1).

[0039] As the epoxy resin (A1), any monomer, oligomer or polymer having two or more epoxy groups in one molecule can be used, and there are no limitations on the molecular weight or molecular structure.

[0040] Examples of the epoxy resin (A1) include biphenyl type epoxy resins; bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and tetramethylbisphenol F type epoxy resins; stilbene type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; polyfunctional epoxy resins such as trisphenol type epoxy resins exemplified by triphenol methane type epoxy resins and alkyl-modified triphenol methane type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, naphthol aralkyl type epoxy resins having a phenylene skeleton, and the like. The epoxy resin may include one or more types selected from the group consisting of epoxy resins, phenol aralkyl type epoxy resins such as phenol aralkyl type epoxy resins having a biphenylene skeleton, and naphthol aralkyl type epoxy resins having a biphenylene skeleton; naphthol type epoxy resins such as dihydroxynaphthalene type epoxy resins and epoxy resins obtained by glycidyl etherifying a dimer of dihydroxynaphthalene; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; and bridged cyclic hydrocarbon compound-modified phenol type epoxy resins such as dicyclopentadiene-modified phenol type epoxy resins.

[0041] From the viewpoint of the effects of the present invention, among these, novolac type epoxy resins, polyfunctional epoxy resins, and phenol aralkyl type epoxy resins can be preferably used. From the same viewpoint, the epoxy resin preferably contains one or more selected from the group consisting of orthocresol novolac type epoxy resins, phenol aralkyl type epoxy resins having a biphenylene skeleton, and triphenylmethane type epoxy resins, and more preferably contains one or more selected from the group consisting of orthocresol novolac type epoxy resins and phenol aralkyl type epoxy resins having a biphenylene skeleton.

[0042] From the viewpoint of the effects of the present invention, the epoxy resin (A1) is preferably contained in an amount of 3 mass% or more, more preferably 5 mass% or more, and even more preferably 10 mass% or more, based on the entire resin composition. The epoxy resin (A1) is typically contained in an amount of 20 mass% or less, more preferably 18 mass% or less, and even more preferably 15 mass% or less.

[0043] [Hardening agent (C)] The resin composition of the present embodiment may further contain a curing agent (C). As the curing agent (C), any known curing agent can be used as long as the effects of the present invention are achieved. However, it is preferable to use at least one selected from the group consisting of active ester curing agents (C1) and phenolic curing agents (C2).

[0044] [Active ester hardener (C1)] As the active ester curing agent (C1), a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester curing agent (C1), a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferred.

[0045] Preferred specific examples of the active ester curing agent (C1) include active ester curing agents containing a dicyclopentadiene-type diphenol structure, active ester curing agents containing a naphthalene structure, active ester curing agents containing an acetylated product of phenol novolac, and active ester curing agents containing a benzoylated product of phenol novolac, and at least one of them can be included. Among them, active ester curing agents containing a naphthalene structure and active ester curing agents containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.

[0046] In this embodiment, the active ester curing agent (C1) can be, for example, a resin having a structure represented by the following general formula (1).

[0047] [ka]

[0048] In general formula (1), "B" is a structure represented by general formula (B).

[0049] [ka]

[0050] In general formula (B), Ar is a substituted or unsubstituted arylene group. Examples of the substituent of the substituted arylene group include an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, and an aralkyl group.

[0051] Y is a single bond, a substituted or unsubstituted linear alkylene group having 1 to 6 carbon atoms, a substituted or unsubstituted cyclic alkylene group having 3 to 6 carbon atoms, a substituted or unsubstituted divalent aromatic hydrocarbon group, an ether bond, a carbonyl group, a carbonyloxy group, a sulfide group, or a sulfone group. Examples of the substituent of the above group include an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, and an aralkyl group.

[0052] Preferred examples of Y include a single bond, a methylene group, -CH(CH3)2-, an ether bond, an optionally substituted cycloalkylene group, and an optionally substituted 9,9-fluorenylene group. n is an integer of 0 to 4, and is preferably 0 or 1. Specifically, B is a structure represented by the following general formula (B1) or the following general formula (B2).

[0053] [ka]

[0054] In the above general formula (B1) and the above general formula (B2), Ar and Y have the same meanings as in the general formula (B). A is a substituted or unsubstituted arylene group linked via an aliphatic cyclic hydrocarbon group; Ar' is a substituted or unsubstituted aryl group; k is the average value of the repeating units and is in the range of 0.25 to 3.5.

[0055] The resin composition of the present embodiment contains a specific active ester curing agent, and thus the resulting cured product can have excellent dielectric properties and an excellent low dielectric tangent.

[0056] The active ester curing agent (C1) used in the resin composition of this embodiment has an active ester group represented by formula (B). In the curing reaction between the epoxy resin and the active ester curing agent, the active ester group of the active ester curing agent reacts with the epoxy group of the epoxy resin to generate a secondary hydroxyl group. This secondary hydroxyl group is blocked by the ester residue of the active ester curing agent. Therefore, the dielectric tangent of the cured product is reduced. In one embodiment, the structure represented by the above formula (B) is preferably at least one selected from the following formulae (B-1) to (B-6).

[0057] [ka]

[0058] In formulas (B-1) to (B-6), R 1 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, or an aralkyl group,

[0059] R 2each independently represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a phenyl group; X represents a linear alkylene group having 2 to 6 carbon atoms, an ether bond, a carbonyl group, a carbonyloxy group, a sulfide group, or a sulfone group; n is an integer of 0 to 4, and p is an integer of 1 to 4.

[0060] Since the structures represented by the above formulas (B-1) to (B-6) are all highly oriented structures, when an active ester curing agent containing such structures is used, the cured product of the resulting resin composition has a low dielectric tangent and excellent adhesion to metals, and therefore can be suitably used as a semiconductor encapsulation material.

[0061] Among them, from the viewpoint of low dielectric tangent, active ester curing agents having a structure represented by formula (B-2), formula (B-3) or formula (B-5) are preferred, and active ester curing agents having a structure in which n in formula (B-2) is 0, a structure in which X in formula (B-3) is an ether bond, or a structure in which two carbonyloxy groups are at the 4,4'-position in formula (B-5) are more preferred. 1 are preferably all hydrogen atoms.

[0062] In formula (1), "Ar'" is an aryl group, and may be, for example, a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 3,5-xylyl group, an o-biphenyl group, an m-biphenyl group, a p-biphenyl group, a 2-benzylphenyl group, a 4-benzylphenyl group, a 4-(α-cumyl)phenyl group, a 1-naphthyl group, a 2-naphthyl group, etc. Among these, a 1-naphthyl group or a 2-naphthyl group is preferable, since a cured product having a particularly low dielectric tangent can be obtained.

[0063] In this embodiment, "A" in the active ester curing agent represented by formula (1) is a substituted or unsubstituted arylene group linked via an aliphatic cyclic hydrocarbon group. Examples of such arylene groups include a structure obtained by a polyaddition reaction between an unsaturated aliphatic cyclic hydrocarbon compound containing two double bonds in one molecule and a phenolic compound.

[0064] Examples of the unsaturated aliphatic cyclic hydrocarbon compound containing two double bonds in one molecule include dicyclopentadiene, cyclopentadiene polymers, tetrahydroindene, 4-vinylcyclohexene, 5-vinyl-2-norbornene, and limonene, which may be used alone or in combination of two or more. Among these, dicyclopentadiene is preferred because it can provide a cured product with excellent heat resistance. Since dicyclopentadiene is contained in petroleum fractions, industrial dicyclopentadiene may contain cyclopentadiene polymers and other aliphatic or aromatic diene compounds as impurities, but considering performance such as heat resistance, curability, and moldability, it is desirable to use a product with a purity of 90% by mass or more of dicyclopentadiene.

[0065] On the other hand, the phenolic compound may be, for example, phenol, cresol, xylenol, ethylphenol, isopropylphenol, butylphenol, octylphenol, nonylphenol, vinylphenol, isopropenylphenol, allylphenol, phenylphenol, benzylphenol, chlorophenol, bromophenol, 1-naphthol, 2-naphthol, 1,4-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, etc., each of which may be used alone or in combination of two or more kinds. Among these, phenol is preferred because it is an active ester curing agent with high curing property and excellent dielectric properties in the cured product.

[0066] In a preferred embodiment, "A" in the active ester curing agent represented by formula (1) has a structure represented by formula (A). A resin composition containing an active ester curing agent in which "A" in formula (1) has the following structure has a cured product with a low dielectric tangent and excellent adhesion to insert products.

[0067] [ka]

[0068] In formula (A), R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, or an aralkyl group, l is 0 or 1, and m is an integer of 1 or more.

[0069] Among the active ester curing agents represented by formula (1), more preferred are resins represented by the following formulas (1-1), (1-2) and (1-3), and particularly preferred is the resin represented by the following formula (1-3).

[0070] [ka]

[0071] In formula (1-1), R 1 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, or an aralkyl group; Z represents a phenyl group, a naphthyl group, or a phenyl group or naphthyl group having 1 to 3 alkyl groups having 1 to 4 carbon atoms on the aromatic nucleus; l is 0 or 1; and k is the average of the repeating units and is 0.25 to 3.5.

[0072] [ka]

[0073] In formula (1-2), R 1 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, or an aralkyl group; Z represents a phenyl group, a naphthyl group, or a phenyl group or naphthyl group having 1 to 3 alkyl groups having 1 to 4 carbon atoms on the aromatic nucleus; l is 0 or 1; and k is the average of the repeating units and is 0.25 to 3.5.

[0074] [ka]

[0075] In formula (1-3), R 1 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a phenyl group, or an aralkyl group; Z represents a phenyl group, a naphthyl group, or a phenyl group or naphthyl group having 1 to 3 alkyl groups having 1 to 4 carbon atoms on the aromatic nucleus; l is 0 or 1; and k is the average of the repeating units and is 0.25 to 3.5.

[0076] The active ester curing agent (C1) used in the present invention can be produced by a known method of reacting a phenolic compound (a) having a structure in which a plurality of aryl groups each having a phenolic hydroxyl group are bonded via an aliphatic cyclic hydrocarbon group, an aromatic nucleus-containing dicarboxylic acid or its halide (b), and an aromatic monohydroxy compound (c).

[0077] The reaction ratio of the phenolic compound (a), aromatic nucleus-containing dicarboxylic acid or its halide (b), and aromatic monohydroxy compound (c) can be appropriately adjusted according to the desired molecular design. Among them, since an active ester curing agent having higher curing properties can be obtained, it is preferable to use each raw material in a ratio such that the phenolic hydroxyl group of the phenolic compound (a) is in the range of 0.25 to 0.90 moles and the hydroxyl group of the aromatic monohydroxy compound (c) is in the range of 0.10 to 0.75 moles per 1 mole of the total of the carboxyl group or acid halide group of the aromatic nucleus-containing dicarboxylic acid or its halide (b), and it is more preferable to use each raw material in a ratio such that the phenolic hydroxyl group of the phenolic compound (a) is in the range of 0.50 to 0.75 moles and the hydroxyl group of the aromatic monohydroxy compound (c) is in the range of 0.25 to 0.50 moles.

[0078] In addition, when the total number of arylcarbonyloxy groups and phenolic hydroxyl groups in the resin structure is taken as the number of functional groups of the resin, the functional group equivalent of the active ester curing agent (C1) is preferably in the range of 200 g / eq or more and 230 g / eq or less, and more preferably in the range of 210 g / eq or more and 220 g / eq or less, in order to obtain a cured product with excellent curability and low dielectric constant and dielectric dissipation factor.

[0079] In the resin composition of this embodiment, the amount of active ester curing agent (C1) and thermosetting resin is preferably such that the functional group of the thermosetting resin (epoxy group in the epoxy resin) is 0.8 to 1.2 equivalents per equivalent of the total active groups in the active ester curing agent (C1), since a cured product with excellent curability and low dielectric tangent can be obtained. Here, the active group in the active ester curing agent (C1) refers to an arylcarbonyloxy group and a phenolic hydroxyl group in the resin structure.

[0080] In the composition of this embodiment, the active ester curing agent (C1) is used in an amount of preferably 0.2 mass % or more and 15 mass % or less, more preferably 0.5 mass % or more and 10 mass % or less, and even more preferably 1.0 mass % or more and 7 mass % or less, based on the entire resin composition. By including the specific active ester curing agent in the above range, the resulting cured product can have better dielectric properties and is even more excellent in low dielectric tangent.

[0081] The resin blocker of this embodiment uses the active ester curing agent (C1) in combination with the above-mentioned titanium-based material (a), and thus has excellent high dielectric constant and low dielectric tangent, and these effects are also excellent in the high frequency band.

[0082] From the viewpoint of the above-mentioned effects, the active ester curing agent (C1) can be contained in an amount of preferably 1 part by mass or more and 30 parts by mass or less, more preferably 2 parts by mass or more and 20 parts by mass or less, and even more preferably 3 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the above-mentioned titanium-based material (a).

[0083] (Phenol hardener (C2)) Examples of the phenol curing agent (C2) include polyhydric phenol compounds such as phenol novolac resin, cresol novolac resin, aromatic hydrocarbon formaldehyde resin-modified phenol resin, dicyclopentadiene phenol addition type resin, phenol aralkyl resin, naphthol aralkyl resin, trimethylolmethane resin, tetraphenylolethane resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-cresol co-condensed novolac resin, biphenyl-modified phenol resin (a polyhydric phenol compound in which phenol nuclei are linked by bismethylene groups), biphenyl-modified naphthol resin (a polyhydric naphthol compound in which phenol nuclei are linked by bismethylene groups), and aminotriazine-modified phenol resin (a polyhydric phenol compound in which phenol nuclei are linked by melamine, benzoguanamine, or the like).

[0084] The amount of the phenol curing agent (C2) is preferably 20% by mass or more and 70% by mass or less based on the thermosetting resin (A). By using the curing agent in the amount within the above range, a resin composition having excellent curability can be obtained.

[0085] In the composition of this embodiment, the phenol curing agent (C2) is used in an amount of preferably 0.2 mass % or more and 15 mass % or less, more preferably 0.5 mass % or more and 10 mass % or less, and even more preferably 1.0 mass % or more and 7 mass % or less, based on the entire resin composition. By including the specific phenol curing agent (C2) in the above range, the obtained cured product can have better dielectric properties and is further superior in low dielectric tangent. The curing agent (B) of this embodiment may contain other curing agents besides the active ester curing agent (C1) and the phenolic curing agent (C2).

[0086] Examples of other curing agents include amine compounds such as diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, diaminodiphenylsulfone, isophoronediamine, imidazole, BF3-amine complex, and guanidine derivatives; amide compounds such as dicyandiamide and polyamide resins synthesized from a dimer of linoleic acid and ethylenediamine; and acid anhydrides such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.

[0087] [Curing catalyst (D)] The resin composition of the present embodiment may further contain a curing catalyst (D). The curing catalyst (D) may be called a curing accelerator, etc. The curing catalyst (D) is not particularly limited as long as it accelerates the curing reaction of the thermosetting resin (B) such as an epoxy resin, and any known curing catalyst can be used.

[0088] Specific examples of such compounds include phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds; imidazoles (imidazole-based curing accelerators) such as 2-methylimidazole and 2-phenylimidazole; and nitrogen atom-containing compounds such as amidines and tertiary amines, exemplified by 1,8-diazabicyclo[5.4.0]undecene-7 and benzyldimethylamine, and quaternary salts of amidines and amines. Only one type of compound may be used, or two or more types may be used.

[0089] Among these, from the viewpoint of ensuring a predetermined gel time, improving moldability, and obtaining a magnetic material excellent in mechanical strength such as bending strength, it is preferable to contain a phosphorus atom-containing compound, more preferably to contain one having latency such as a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, or an adduct of a phosphonium compound and a silane compound, and particularly preferably a tetra-substituted phosphonium compound, an adduct of a phosphine compound and a quinone compound, or an adduct of a phosphonium compound and a silane compound. By using a latent curing catalyst, a resin composition having excellent moldability can be obtained.

[0090] Examples of the organic phosphines include primary phosphines such as ethylphosphine and phenylphosphine; secondary phosphines such as dimethylphosphine and diphenylphosphine; and tertiary phosphines such as trimethylphosphine, triethylphosphine, tributylphosphine and triphenylphosphine. Examples of the tetra-substituted phosphonium compound include compounds represented by the following general formula (6).

[0091] [ka]

[0092] In general formula (6), P represents a phosphorus atom. R4 , R 5 , R 6 and R 7 each independently represents an aromatic group or an alkyl group. A represents an anion of an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on an aromatic ring. AH represents an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on an aromatic ring. x and y are 1 to 3, z is 0 to 3, and x=y. The compound represented by the general formula (6) can be obtained, for example, as follows.

[0093] First, a tetra-substituted phosphonium halide, an aromatic organic acid, and a base are mixed uniformly in an organic solvent to generate an aromatic organic acid anion in the solution system. Then, water is added to precipitate the compound represented by general formula (6). In the compound represented by general formula (6), R bonded to the phosphorus atom 4 , R 5 , R 6 and R 7 is preferably a phenyl group, AH is a compound having a hydroxyl group on an aromatic ring, i.e., a phenol, and A is an anion of the phenol. Examples of the phenol include monocyclic phenols such as phenol, cresol, resorcin, and catechol, condensed polycyclic phenols such as naphthol, dihydroxynaphthalene, and anthraquinol, bisphenols such as bisphenol A, bisphenol F, and bisphenol S, and polycyclic phenols such as phenylphenol and biphenol. Examples of the phosphobetaine compound include compounds represented by the following general formula (7).

[0094] [ka]

[0095] In general formula (7), P represents a phosphorus atom. R 8 is an alkyl group having 1 to 3 carbon atoms, R 9 represents a hydroxyl group. f is 0 to 5 and g is 0 to 3. The compound represented by the general formula (7) can be obtained, for example, as follows.

[0096] First, a triaromatic substituted phosphine, which is a tertiary phosphine, is contacted with a diazonium salt to substitute the diazonium group of the diazonium salt for the triaromatic substituted phosphine. Examples of the adduct of a phosphine compound and a quinone compound include compounds represented by the following general formula (8).

[0097] [ka]

[0098] In general formula (8), P represents a phosphorus atom. R 10 , R 11 and R 12 represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and may be the same or different.

[0099] R 13 , R 14 and R 15 represents a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, and may be the same or different; R 14 and R 15 may be bonded to form a cyclic structure.

[0100] The phosphine compound used in the adduct of the phosphine compound and the quinone compound is preferably, for example, triphenylphosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, trinaphthylphosphine, tris(benzyl)phosphine, etc., which is unsubstituted or has a substituent such as an alkyl group or an alkoxy group on the aromatic ring, and examples of the substituent such as the alkyl group or alkoxy group include those having a carbon number of 1 to 6. From the viewpoint of availability, triphenylphosphine is preferred.

[0101] As the quinone compound used in the adduct of the phosphine compound and the quinone compound, benzoquinone and anthraquinones can be mentioned, and among them, p-benzoquinone is preferred from the viewpoint of storage stability.

[0102] The method for producing an adduct of a phosphine compound and a quinone compound is to contact and mix the organic tertiary phosphine and the benzoquinone in a solvent in which both can dissolve, to obtain the adduct. The solvent is preferably a ketone such as acetone or methyl ethyl ketone, which has low solubility in the adduct, but is not limited thereto.

[0103] In the compound represented by the general formula (8), R, R, and R bonded to the phosphorus atom are phenyl groups, and R 13 , R 14 and R 15 is a hydrogen atom, that is, an addition compound of 1,4-benzoquinone and triphenylphosphine is preferred in that it reduces the hot elastic modulus of the cured resin composition. Examples of the adduct of a phosphonium compound and a silane compound include a compound represented by the following general formula (9).

[0104] [ka]

[0105] In general formula (9), P represents a phosphorus atom, and Si represents a silicon atom.

[0106] R 16 , R 17 , R 18 and R 19 each represents an organic group having an aromatic ring or a heterocycle, or an aliphatic group, and may be the same or different. R 20 is the group Y 2 and Y 3 It is an organic group that bonds to R 21 is the group Y 4 and Y 5 It is an organic group that bonds to

[0107] Y 2 and Y 3 represents a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure.

[0108] Y 4 and Y 5 represents a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. R 20 , and R 21 may be the same or different, and Y 2 , Y 3 , Y 4 and Y 5 may be the same or different from each other. Z1 is an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group.

[0109] In the general formula (9), R 16 , R 17 , R 18 and R 19Examples of the alkyl group include a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, a naphthyl group, a hydroxynaphthyl group, a benzyl group, a methyl group, an ethyl group, an n-butyl group, an n-octyl group, and a cyclohexyl group. Among these, an aromatic group having a substituent such as an alkyl group, an alkoxy group, or a hydroxyl group, such as a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, or a hydroxynaphthyl group, or an unsubstituted aromatic group is more preferable.

[0110] In the general formula (9), R 20 is Y 2 and Y 3 Similarly, R 21 is the group Y 4 and Y 5 It is an organic group that bonds with Y. 2 and Y 3 is a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure. 4 and Y 5 is a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. 20 and R 21 may be the same or different, and the group Y 2 , Y 3 , Y 4 and Y5 may be the same or different. 2 -R 20 -Y 3 - and Y 4 -R 21 -Y 5The group represented by - is composed of a group formed by releasing two protons from a proton donor. As the proton donor, an organic acid having at least two carboxyl groups or hydroxyl groups in the molecule is preferable, an aromatic compound having at least two carboxyl groups or hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferable, and an aromatic compound having at least two hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferable. Examples of the proton donor include catechol, pyrogallol, 1,2-dihydro- Examples of the hydroxynaphthalene include xynaphthalene, 2,3-dihydroxynaphthalene, 2,2'-biphenol, 1,1'-bi-2-naphthol, salicylic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, chloranilic acid, tannic acid, 2-hydroxybenzyl alcohol, 1,2-cyclohexanediol, 1,2-propanediol, and glycerin. Of these, catechol, 1,2-dihydroxynaphthalene, and 2,3-dihydroxynaphthalene are more preferred.

[0111] Z in general formula (9) 1 represents an organic group or an aliphatic group having an aromatic ring or a heterocyclic ring, and specific examples thereof include aliphatic hydrocarbon groups such as methyl group, ethyl group, propyl group, butyl group, hexyl group, and octyl group; aromatic hydrocarbon groups such as phenyl group, benzyl group, naphthyl group, and biphenyl group; glycidyloxy groups such as glycidyloxypropyl group, mercaptopropyl group, and aminopropyl group; mercapto group; and reactive substituents such as an alkyl group having an amino group and a vinyl group. Among these, the methyl group, the ethyl group, the phenyl group, the naphthyl group, and the biphenyl group are more preferable in terms of thermal stability. A method for producing an adduct of a phosphonium compound and a silane compound is, for example, as follows.

[0112] In a flask containing methanol, a silane compound such as phenyltrimethoxysilane and a proton donor such as 2,3-dihydroxynaphthalene are dissolved, and then a sodium methoxide-methanol solution is added dropwise at room temperature with stirring. A previously prepared solution of a tetra-substituted phosphonium halide such as tetraphenylphosphonium bromide dissolved in methanol is then added dropwise at room temperature with stirring, causing crystals to precipitate. The precipitated crystals are filtered, washed with water, and vacuum dried to obtain an adduct of the phosphonium compound and the silane compound.

[0113] When the curing catalyst (D) is used, its content is preferably 0.01 to 1 mass %, more preferably 0.02 to 0.8 mass %, based on the total mass of the resin composition. By setting the content within such a range, a sufficient curing acceleration effect can be obtained without excessively impairing other performances, and fluidity and moldability can be further improved.

[0114] [Silane coupling agent (E)] The resin composition of the present embodiment may further contain a silane coupling agent (E). By containing the silane coupling agent (E), the mechanical strength of a cured product (molded article) of the resin composition can be improved.

[0115] As the silane coupling agent (E), any known compound can be used as long as the effects of the present invention can be exhibited. It is preferable to use a silane coupling agent represented by the following general formula (2).

[0116] [ka]

[0117] In general formula (2), R each independently represents an alkoxy group having 1 to 3 carbon atoms or an alkyl group having 1 to 3 carbon atoms, and at least two R are alkoxy groups having 1 to 3 carbon atoms. All of R are preferably alkoxy groups having 1 to 3 carbon atoms, and more preferably alkoxy groups having 1 to 2 carbon atoms.

[0118] L represents a linear or branched alkylene group having 1 to 17 carbon atoms. L is preferably a linear or branched alkylene group having 2 to 15 carbon atoms, and more preferably a linear or branched alkylene group having 2 to 12 carbon atoms. It is presumed that when L is a long-chain alkylene group, the wettability of the resin to the surface of the soft magnetic particles is improved, improving moldability and flowability.

[0119] X represents a vinyl group, an epoxy group, a glycidyl ether group, an oxetanyl group, a (meth)acryloyl group, an amino group, a methyl group, or an anilino group. From the viewpoint of the effects of the present invention, X is preferably a vinyl group, an epoxy group, a glycidyl ether group, a methyl group, or an anilino group, and more preferably an epoxy group, a glycidyl ether group, a methyl group, or an anilino group. From the viewpoint of further improving the fluidity of the resin molding material when melted, X is preferably an epoxy group, a glycidyl ether group, or an anilino group.

[0120] Examples of the silane coupling agent (E) include KBM-1083 (octenyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), KBM-3103C (decyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), KBM-4803 (glycidoxyoctyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), KBM-5803 (methacryloxyoctyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), and CF-4083 (N-phenyl-γ-aminopropyltrimethoxysilane, manufactured by Dow Corning Toray Co., Ltd.).

[0121] The resin composition of the present embodiment may contain the silane coupling agent (E) in an amount of 0.05% by mass to 1% by mass, preferably 0.1 to 0.8% by mass, which provides the cured product (molded article) of the resin composition with superior mechanical strength.

[0122] [Other ingredients] The soft magnetic material of the present embodiment may contain components other than those described above, such as one or more of a release agent, a stress reducing agent, an adhesion aid, a colorant, an antioxidant, a corrosion resistant agent, a dye, a pigment, and a flame retardant.

[0123] Examples of the release agent include carnauba wax, stearic acid, montanic acid, montanic acid esters, metal stearates, polyethylene oxide, and a reaction product of a condensate of an alkene and maleic anhydride with stearyl alcohol, and the like. One or a combination of two or more selected from these may be used.

[0124] Examples of the low stress agent include polybutadiene compounds, acrylonitrile butadiene copolymer compounds, silicone oils, silicone rubbers, etc. When using a low stress agent, only one type may be used, or two or more types may be used in combination.

[0125] <Resin composition> The resin composition of the present embodiment can be produced by uniformly mixing the above-mentioned components. The production method includes a method in which a predetermined amount of raw materials is thoroughly mixed using a mixer or the like, then melt-kneaded using a mixing roll, kneader, extruder, or the like, and then cooled and pulverized. The obtained resin composition may be tableted to a size and mass suitable for molding conditions, as necessary.

[0126] The properties of the resin composition of the present embodiment are shown below. The properties can be controlled by appropriately selecting the types and amounts of each component contained in the resin composition, the method for preparing the resin composition, and the like.

[0127] When the cure torque value of the resin composition of this embodiment is measured over time at 175°C using a curastometer, the time from the start of measurement until the cure torque value reaches 1 kgf cm is 30 seconds or more and 80 seconds or less, preferably 35 seconds or more and 75 seconds or less. When the time is within the above range, the resin composition has superior fluidity and superior moldability.

[0128] The resin composition of the present embodiment has a square wave pressure of 0.5 MPa or less, preferably 0.4 MPa or less, measured by the following method. The lower limit of the square wave pressure is not particularly limited, but is 0.05 MPa or more. The square root pressure is a parameter of melt viscosity, and the smaller the value, the lower the melt viscosity. Since the square root pressure is in the above range, the resin composition of the present embodiment has excellent mold filling properties during molding.

[0129] (method) Using a low pressure transfer molding machine, the mold temperature was 175℃ and the injection speed was 177mm. 3 The resin composition is injected into a rectangular flow path having a width of 13 mm, a thickness of 1 mm, and a length of 175 mm under the condition of 1 / sec. At this time, the change in pressure over time is measured with a pressure sensor embedded at a position 25 mm from the upstream end of the flow path, and the minimum pressure (MPa) during the flow of the resin composition is measured and defined as the rectangular pressure.

[0130] The resin composition of the present embodiment can have a linear expansion coefficient CTE1 at a temperature below the glass transition temperature of a cured product of the resin composition, measured under the following conditions, of 10 ppm / °C or more and 30 ppm / °C or less, preferably 15 ppm / °C or more and 25 ppm / °C or less. By having the linear expansion coefficient (CTE1) (c) within the above range, the stress caused by the difference in the linear expansion coefficient with other antenna materials is further alleviated, and warping when used as an antenna material can be reduced.

[0131] (Method of measuring linear expansion coefficient) The resin composition is injected and molded using a transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and curing time of 180 seconds to obtain a test piece (cured product) with a long side of 15mm, a short side of 4mm, and a thickness of 4mm. The test piece is post-cured at 175°C for 4 hours, and then measured using a thermomechanical analyzer in compression mode under the conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / min. From the measurement results, the average linear expansion coefficient from 40°C to 80°C is calculated as CTE1, and the average linear expansion coefficient from 190°C to 230°C is CTE2.

[0132] The resin composition of the present embodiment can have a linear expansion coefficient CTE2 at a temperature equal to or higher than the glass transition temperature of the cured product of the resin composition, measured under the above conditions, of 60 ppm / ° C. to 90 ppm / ° C., preferably 65 ppm / ° C. to 80 ppm / ° C. This can reduce warping when used as an antenna material.

[0133] The resin composition of the present embodiment can provide a cured product of the resin composition with a bending strength of 1 MPa or more, preferably 2 MPa or more at 260° C. The upper limit is not particularly limited, but is 20 MPa or less. This provides the cured product with excellent mechanical strength, making it suitable for use as an antenna material.

[0134] The flexural modulus of the cured product of the resin composition at 260° C. can be 1000 MPa or less, preferably 300 MPa or less. The lower limit is not particularly limited, but is 50 MPa or more. This provides the cured product with excellent mechanical strength, making it suitable for use as an antenna material.

[0135] The resin composition of this embodiment has the following dielectric constant and dielectric tangent (tan δ) in a cured product obtained by heating at 175° C. for 180 seconds. The dielectric constant at 1 MHz as measured by the Q meter method can be made 12 or more, preferably 13 or more. The dielectric loss tangent (tan δ) at 1 MHz as measured by the Q meter method can be made 0.005 or less, preferably 0.004 or less.

[0136] The cured product obtained from the resin composition of the present embodiment has a high dielectric constant and a low dielectric tangent in the high frequency band, which enables higher frequencies, shorter circuits, and smaller communication devices. The cured product can be suitably used as a material for forming a microstrip antenna, a material for forming a dielectric waveguide, and a material for forming an electromagnetic wave absorber.

[0137] <Microstrip antenna> 1, the microstrip antenna 10 of this embodiment includes a dielectric substrate 12 formed by curing the above-mentioned resin composition, a radiating conductor plate (radiating element) 14 provided on one surface of the dielectric substrate 12, and a ground conductor plate 16 provided on the other surface of the dielectric substrate 12. At least a portion of the radiating conductor plate 12 is embedded in the dielectric substrate 12. The shape of the radiating conductor plate may be rectangular or circular, and in this embodiment, a rectangular radiating conductor plate 14 will be used as an example.

[0138] The radiation conductor plate 14 includes any one of a metal material, an alloy of a metal material, a hardened metal paste, and a conductive polymer. The metal material includes copper, silver, palladium, gold, platinum, aluminum, chromium, nickel, cadmium-lead, selenium, manganese, tin, vanadium, lithium, cobalt, and titanium. The alloy includes a plurality of metal materials. The metal paste agent includes a mixture of powder of a metal material with an organic solvent and a binder. The binder includes an epoxy resin, a polyester resin, a polyimide resin, a polyamide-imide resin, and a polyetherimide resin. The conductive polymer includes a polythiophene-based polymer, a polyacetylene-based polymer, a polyaniline-based polymer, a polypyrrole-based polymer, and the like.

[0139] 1, the microstrip antenna 10 of this embodiment has a radiating conductor plate 14 with a length L and a width W, and resonates at a frequency where L is an integer multiple of 1 / 2 the wavelength. When using a dielectric substrate 12 with a high dielectric constant as in this embodiment, the thickness h of the dielectric substrate 12 and the width W of the radiating conductor plate 14 are designed to be sufficiently small compared to the wavelength.

[0140] The ground conductor plate 16 is a thin plate made of a highly conductive metal such as copper, silver, gold, etc. Its thickness is sufficiently thin compared to the central operating frequency of the antenna device, and may be about 1 / 50 to 1 / 1000 of the wavelength of the central operating frequency.

[0141] Feed methods for microstrip antennas include direct feed methods such as back-coaxial feed and coplanar feed, and electromagnetic coupling feed methods such as slot coupling feed and proximity coupling feed. The rear coaxial feed can feed power from the rear of the antenna to the radiation conductor plate 14 using a coaxial line or connector that passes through the ground conductor plate 16 and the dielectric substrate 12 . The coplanar feed can feed the radiating conductor plate 14 with a microstrip line (not shown) disposed on the same plane as the radiating conductor plate 14 .

[0142] In the slot coupling feed, another dielectric substrate (not shown) is provided sandwiching the ground conductor plate 16, and the radiating conductor plate 14 and the microstrip line are formed on separate dielectric substrates. The radiating conductor plate 14 is excited by electromagnetically coupling the radiating conductor plate 14 and the microstrip line through a slot opened in the ground conductor plate 16.

[0143] In proximity coupling power supply, the dielectric substrate 12 has a laminated structure, and a dielectric substrate on which the radiating conductor plate 14 is formed is laminated with a dielectric substrate on which the strip conductor of the microstrip line and the ground conductor plate 16 are arranged.The strip conductor of the microstrip line is extended to the bottom of the radiating conductor plate 14, and the radiating conductor plate 14 and the microstrip line are electromagnetically coupled, thereby exciting the radiating conductor plate 14.

[0144] 2(a) and (b) show another embodiment of the microstrip antenna. Note that the same components as those in FIG. 1 are given the same reference numerals and the description will be omitted as appropriate.

[0145] 2(a), the microstrip antenna 20 includes a dielectric substrate 22, a radiating conductor plate 14 provided on one surface of the dielectric substrate 22, a ground conductor plate 16 provided on the other surface of the dielectric substrate 22, and a high dielectric substrate (high dielectric) 24 disposed opposite the radiating conductor plate 14. The dielectric substrate 22 and the radiating conductor plate 14 can be configured to be spaced a predetermined distance from the high dielectric substrate 24 via a spacer 26.

[0146] The dielectric substrate 22 is made of a substrate having a low dielectric constant, such as a Teflon substrate. The high dielectric substrate 24 is made of a dielectric material obtained by curing the above-mentioned resin composition. The gap between the dielectric substrate 22 and the high dielectric substrate 24 may be a space or may be filled with a dielectric material. Also, as shown in a microstrip antenna 20' in FIG. 2(b), a high dielectric substrate 24 may be abutted against the upper surface of the radiation conductor plate 14. In the microstrip antenna 20' shown in FIG.

[0147] <Dielectric Waveguide> In this embodiment, the dielectric waveguide includes a dielectric obtained by curing the resin composition of this embodiment and a conductor film covering the surface of the dielectric. The dielectric waveguide confines and transmits electromagnetic waves in a dielectric (dielectric medium). The conductive film can be made of a metal such as copper, or an oxide high-temperature superconductor.

[0148] <Electromagnetic wave absorber> In this embodiment, the electromagnetic wave absorber has a structure in which a support, a resistive film, a dielectric layer, and a reflective layer are laminated together. The electromagnetic wave absorber can be used as a λ / 4 type electromagnetic wave absorber having high electromagnetic wave absorbing performance.

[0149] The support may be a resin substrate, etc. The support can protect the resistive film and enhance the durability of the radio wave absorber. Examples of the resistive film include indium tin oxide and molybdenum-containing resistive films. The dielectric layer is formed by curing the resin composition of the present embodiment, and has a thickness of about 10 μm or more and 2000 μm or less. The reflective layer can function as a layer that reflects radio waves, and is, for example, a metal film.

[0150] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention. EXAMPLES

[0151] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0152] [Examples 1-2, Comparative Example 1] The following raw materials were mixed in the amounts shown in Table 1 at room temperature using a mixer, and then roll-kneaded at 70 to 100° C. The kneaded product was then cooled and pulverized to obtain a granular resin composition. The resin composition was then tableted under high pressure to obtain a tablet-shaped resin composition.

[0153] (Inorganic filler) Inorganic filler 1: Calcium titanate (spherical, average circularity 0.97, particle size D5: 0 μm, D 50 : 3.8μm, D 95 :21.6μm) Inorganic filler 2: Magnesium titanate (average particle size 0.8 μm) Inorganic filler 3: Calcium titanate (CT, average particle size 2.0 μm, manufactured by Fuji Titanium Co., Ltd.)

[0154] (Coloring agent) Colorant 1: Black titanium oxide (Ako Kasei Co., Ltd.) (Coupling Agent) Coupling agent 1: Phenylaminopropyltrimethoxysilane (CF4083, manufactured by Dow Corning Toray Co., Ltd.)

[0155] (Epoxy resin) Epoxy resin 1: Phenol aralkyl type epoxy resin containing biphenylene skeleton (NC3000L, manufactured by Nippon Kayaku Co., Ltd.)

[0156] (hardening agent) Hardener 1: Active ester hardener prepared according to the following method (Method for preparing active ester curing agent) In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 203.0 g of 1,3-benzenedicarboxylic acid dichloride (molar number of acid chloride groups: 2.0 mol) and 1338 g of toluene were charged, and the inside of the system was reduced pressure and replaced with nitrogen to dissolve. Next, 96.5 g (0.67 mol) of α-naphthol and 219.5 g of dicyclopentadiene phenol resin (molar number of phenolic hydroxyl groups: 1.33 mol) were charged, and the inside of the system was reduced pressure and replaced with nitrogen to dissolve. Thereafter, while applying nitrogen gas purge, the inside of the system was controlled to 60°C or less, and 400 g of 20% aqueous sodium hydroxide solution was dropped over 3 hours. Then, stirring was continued under these conditions for 1.0 hour. After the reaction was completed, the mixture was left to stand and separated, and the aqueous layer was removed. Furthermore, water was added to the toluene phase in which the reactants were dissolved, and the mixture was stirred and mixed for about 15 minutes, and the aqueous layer was left to stand and separated to remove. This operation was repeated until the pH of the aqueous layer reached 7. Thereafter, water was removed by decanting to obtain an active ester resin in a toluene solution state with a non-volatile content of 65%. When the structure of the obtained active ester resin was confirmed, it was found to be R 1 and R 3 The structure had a hydrogen atom, Z a naphthyl group, and l 0. The average value k of the repeating units of the active ester resin was in the range of 0.5 to 1.0, calculated from the reaction equivalent ratio. The obtained active ester resin specifically had a structure represented by the following chemical formula. In the following formula, the average value k of the repeating units was 0.5 to 1.0.

[0157] [ka]

[0158] (catalyst) Catalyst 1: Tetraphenylphosphonium-4,4'-sulfonyldiphenolate Catalyst 2: Tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate

[0159] (Release agent) Release agent 1: Glycerol trimontanate ester (Licorb WE-4, Clariant Japan)

[0160] The physical properties were measured by the following methods. (Labo Plastomill (minimum torque value)) Using a Labo Plastomill tester (4C150, manufactured by Toyo Seiki Seisakusho, Ltd.), the melt torque of the resin compositions obtained in each of the Examples and Comparative Examples was measured over time at a rotation speed of 30 rpm and a measurement temperature of 175°C, and the minimum torque value was obtained.

[0161] (Spiral Flow) Using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., "KTS-15"), the resin compositions obtained in each of the Examples and Comparative Examples were injected into a spiral flow measurement mold conforming to ANSI / ASTM D 3123-72 under conditions of 175°C, injection pressure of 7.0 MPa, and pressure retention time of 120 seconds, and the flow length was measured, which was defined as the spiral flow. The spiral flow is a parameter of fluidity, and the larger the value, the better the fluidity.

[0162] [Gel time (175℃)] Using a curastometer (JSR Curastometer IVPS type, manufactured by Orientec Co., Ltd.), the cure torque of the resin compositions obtained in each Example and Comparative Example was measured over time at a mold temperature of 175°C, and the time from the start of measurement until the cure torque value reached 1 kgf cm was recorded, which was taken as the gel time.

[0163] [Rectangular Pressure] Using a low pressure transfer molding machine (NEC "40 ton manual press"), the mold temperature was 175℃ and the injection speed was 177mm. 3 The resin compositions obtained in each of the Examples and Comparative Examples were injected into a rectangular flow path having a width of 13 mm, a thickness of 1 mm, and a length of 175 mm under conditions of 0.1 s / sec, and the change in pressure over time was measured using a pressure sensor embedded 25 mm from the upstream end of the flow path. The minimum pressure (MPa) during flow of the resin composition was measured and recorded as the rectangular pressure.

[0164] (glass transition temperature, linear expansion coefficient) Using a transfer molding machine (KOTAKISEIKI Co., Ltd., "KTS-15"), the resin compositions obtained in each of the Examples and Comparative Examples were injected and molded at a mold temperature of 175°C, injection pressure of 9.8MPa, and curing time of 180 seconds to obtain test pieces (cured products) with long sides of 15mm, short sides of 4mm, and thickness of 4mm. The test pieces were post-cured at 175°C for 4 hours, and then measured using a thermomechanical analyzer in compression mode under the conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / min. From the measurement results, the glass transition temperature (Tg) and the average linear expansion coefficient from 40°C to 80°C were calculated and designated as CTE1, and the average linear expansion coefficient from 190°C to 230°C was designated as CTE2.

[0165] (Evaluation of mechanical strength (flexural strength / flexural modulus)) The resin compositions obtained in each of the Examples and Comparative Examples were injected into a mold using a low-pressure transfer molding machine (KOTAKISEIKI Co., Ltd.'s "KTS-30") under the conditions of a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 180 seconds. This resulted in a molded product having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded product thus obtained was then post-cured at 175°C for 4 hours. This resulted in a test piece for evaluating mechanical strength. The flexural strength (MPa) and flexural modulus (MPa) of the test piece at room temperature (25°C) or 260°C were measured at a head speed of 5 mm / min in accordance with JIS K 6911.

[0166] (Evaluation of dielectric constant and dielectric loss tangent using Q-meter method) First, a test piece was obtained using the resin composition. Specifically, the resin compositions prepared in the examples and comparative examples were injected into a mold at a mold temperature of 175°C and a curing time of 180 seconds to prepare test pieces (diameter 50 mm, film thickness 3 mm). The measurement equipment used was a Q meter and a micrometer. The electrodes were set up by adhering tin foil with an inner diameter of 38 mm and a thickness of 22.5 μm to both sides of the test piece via a Vaseline coating layer (thin layer) so as to be positioned on the concentric axis of the test piece. The resonant frequency, 3 dB bandwidth, transmitted power ratio, etc. were measured at a frequency of 1 MHz with and without the above-mentioned double-sided tin foil test piece inserted. These measurement results were then analytically calculated using software to obtain the dielectric properties of the dielectric constant (Dk) and dielectric loss tangent (Df). The measurement mode was TE 011 The measurement method was the same as that specified in Section 5.14 of JIS K 6911.

[0167] [Table 1]

[0168] As shown in Table 1, the resin composition of the examples according to the present invention contained a spherical titanium-based material and had a predetermined minimum torque value of 2.0 N m or less, and therefore had a long spiral flow length, excellent fluidity, and excellent dielectric properties. In other words, the resin composition of the present invention had an excellent balance between filling properties and dielectric properties. [Explanation of symbols]

[0169] 10 Microstrip Antenna 12 Dielectric substrate 14 Radiating conductor plate 16 Grounding plate 20, 20' Microstrip Antenna 22 Dielectric Substrate 24 High dielectric substrate 26 Spacer a Cavity

Claims

1. A resin composition containing an inorganic filler (A) including a spherical titanium-based material (a), A resin composition having a minimum torque value of 2.0 N·m or less when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C.

2. The resin composition according to claim 1 , wherein the spherical titanium-based material (a) comprises spherical calcium titanate (a1).

3. The resin composition according to claim 2, wherein the spherical titanium-based material (a) comprises spherical titanium oxide (a2).

4. 2. The resin composition according to claim 1, wherein, when the curing torque value at 175°C is measured over time using a curastometer, the time from the start of measurement until the curing torque value reaches 1 kgf cm is 30 seconds or more and 80 seconds or less.

5. The resin composition according to claim 1, having a rectangular pressure of 0.5 MPa or less as measured by the following method. (method) Using a low pressure transfer molding machine, the mold temperature was 175°C and the injection speed was 177 mm 3 The resin composition is injected into a rectangular flow path having a width of 13 mm, a thickness of 1 mm, and a length of 175 mm under the condition of 1 / sec. At this time, the change in pressure over time is measured with a pressure sensor embedded at a position 25 mm from the upstream end of the flow path, and the minimum pressure (MPa) during the flow of the resin composition is measured and defined as the rectangular pressure.

6. The resin composition according to claim 1, wherein a linear expansion coefficient CTE1 at a temperature lower than a glass transition temperature of a cured product of the resin composition is 10 ppm / °C or more and 30 ppm / °C or less.

7. The resin composition according to claim 1, wherein a linear expansion coefficient CTE2 at a temperature equal to or higher than a glass transition temperature of a cured product of the resin composition is 60 ppm / °C or higher and 90 ppm / °C or lower.

8. The resin composition according to claim 1 , wherein the cured product of the resin composition has a flexural strength of 1 MPa or more at 260° C.

9. The resin composition according to claim 1, wherein the cured product of the resin composition has a flexural modulus at 260°C of 1000 MPa or less.

10. The resin composition according to claim 1, wherein a cured product of the resin composition has a dielectric constant of 12 or more and a dielectric loss tangent (tan δ) of 0.005 or less at a frequency of 1 MHz.

11. The resin composition according to claim 2, wherein the spherical calcium titanate (a1) has an average circularity of 0.92 or more.

12. The resin composition according to claim 3, wherein the spherical titanium oxide (a2) has an average circularity of 0.88 or more.

13. The resin composition according to claim 1 , wherein the resin composition contains 78% by mass or more of the inorganic filler (A) based on 100% by mass of the resin composition.

14. The spherical calcium titanate (a1) has a particle diameter D at which the cumulative frequency is 5%, 50%, and 95%, respectively, in a volume-based cumulative frequency distribution curve measured using a laser diffraction particle size distribution measuring device. 5 , D 50 , D 95 The resin composition according to claim 2, wherein the above range is satisfied. Particle diameter D 5 :0.1μm or less Particle diameter D 50 :1.0μm or more 8.0μm or less Particle diameter D 95 :15μm or more and 30μm or less

15. The spherical titanium oxide (a2) has a particle diameter D at which the cumulative frequency is 5%, 50%, and 95%, respectively, in a volume-based cumulative frequency distribution curve measured using a laser diffraction particle size distribution measuring device. 5 , D 50 , D 95 The resin composition according to claim 3, wherein the resin composition is within the following range. Particle diameter D 5 :1.5μm or less Particle diameter D 50 :2.0μm or more 9.0μm or less Particle diameter D 95 :10μm or more and 30μm or less

16. The resin composition according to claim 1 , further comprising a thermosetting resin (B).

17. Further comprising a curing agent (C), The resin composition according to claim 1 , wherein the curing agent comprises at least one selected from an active ester curing agent and a phenolic curing agent.

18. The resin composition according to claim 1 , further comprising a curing catalyst (D).

19. The resin composition according to claim 1 , which is used as a material for forming a microstrip antenna.

20. The resin composition according to claim 1 , which is used as a material for forming a dielectric waveguide.

21. The resin composition according to claim 1 , which is used as a material for forming an electromagnetic wave absorber.

22. A dielectric substrate obtained by curing the resin composition according to any one of claims 1 to 18.

23. A dielectric substrate according to claim 22; a radiating conductor plate provided on one surface of the dielectric substrate; a ground conductor plate provided on the other surface of the dielectric substrate; A microstrip antenna comprising:

24. A dielectric substrate; a radiating conductor plate provided on one surface of the dielectric substrate; a ground conductor plate provided on the other surface of the dielectric substrate; a high dielectric material disposed opposite the radiation conductor plate; A microstrip antenna comprising: A microstrip antenna, wherein the high dielectric is constituted by the dielectric substrate according to claim 22.

Citation Information

Patent Citations

  • Molding resin composition and electronic component device

    JP6870778B1

  • Thermosetting resin composition, dielectric substrate, and microstrip antenna

    WO2022202804A1

Cited By

  • Calcium titanate powder and composition

    WO2026211463A1