Lithium ion secondary battery and manufacturing method of lithium ion secondary battery

The lithium ion secondary battery design with optimized crater-shaped recesses and protrusions on the positive electrode surface addresses separator misalignment and lithium precipitation, enhancing battery performance and efficiency.

JP2024164954APending Publication Date: 2024-11-28TOYOTA BATTERY CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023080704
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face issues with separator misalignment and local precipitation of metallic lithium on the negative electrode due to surface protrusions on the positive electrode composite layer, leading to performance deterioration.

Method used

The battery design incorporates crater-shaped recesses with protrusions on the positive electrode composite layer surface, optimizing dimensions and distribution to enhance friction and lithium ion diffusion, thereby preventing separator misalignment and local lithium precipitation.

Benefits of technology

This configuration effectively suppresses separator misalignment and maintains high battery performance by ensuring efficient lithium ion diffusion and reducing local lithium precipitation on the negative electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164954000001_ABST
    Figure 2024164954000001_ABST
Patent Text Reader

Abstract

To suppress a position deviation of a separator while securing a high battery performance.SOLUTION: A secondary battery 1 as a lithium ion secondary battery comprises an electrode body into which electrode sheets 35 of positive and negative electrodes are laminated while nipping a separator. Each electrode sheet 35 is formed by laminating an electrode mixture layer 32 to a base material 36 that becomes a collector 31. Also, the secondary battery 1 comprises: a concave part 51 that is provided onto a front surface 50 of a positive electrode mixture layer 32P constructing an electrode sheet 35P on a positive electrode 3 side; and a ridge part 52 that is projected to the front surface 50 of the positive electrode mixture layer 32P in a peripheral edge part 51e of the concave part 51. Then, in this secondary battery 1, a cross sectional width W of the ridge part 52 in a radial direction of this concave part 51 becomes smaller than a diameter R1 of the concave part 51.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium ion secondary battery and a method for manufacturing a lithium ion secondary battery. [Background technology]

[0002] Conventionally, some lithium ion secondary batteries have positive and negative electrodes formed by using electrode sheets formed by laminating electrode mixture layers on a substrate serving as a current collector. That is, in such lithium ion secondary batteries, a separator is interposed between the positive electrode mixture layer and the negative electrode mixture layer. In many cases, the electrode body is formed with the electrode sheets and the separator wound.

[0003] In addition, in the above configuration, problems such as short circuit between electrodes may occur due to misalignment of the separator sandwiched between the positive and negative electrode sheets. The cause of such misalignment of the separator may be, for example, so-called misalignment when winding the electrode sheets and the separator. Therefore, it is possible to increase the friction coefficient by providing irregularities on the surface of the electrode mixture layer constituting the electrode sheet. This can suppress the occurrence of defects caused by the misalignment of the separator, such as short circuit.

[0004] For example, Patent Document 1 discloses a configuration in which the adhesion of an electrode mixture layer is enhanced by providing irregularities on the surface of a substrate, while Patent Documents 2 and 3 disclose a configuration in which irregularities are formed on the surface of the electrode mixture layer by using a rolling roller in a coating press process or the like. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-54871 A [Patent Document 2] JP 2013-187468 A [Patent Document 3] Japanese Patent Application Publication No. 11-176421 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in lithium ion secondary batteries, the presence of protrusions on the surface of a positive electrode mixture layer makes it easier for metallic lithium to precipitate on the surface of a negative electrode mixture layer that faces the positive electrode mixture layer across the separator, which can result in a decrease in battery performance. [Means for solving the problem]

[0007] Various aspects of a lithium ion secondary battery and a method for manufacturing a lithium ion secondary battery that solves the above problems will be described. Aspect 1 is a lithium ion secondary battery comprising an electrode body in which positive and negative electrode sheets are laminated with a separator sandwiched therebetween, and each of the electrode sheets is formed by laminating an electrode mixture layer on a substrate that serves as a current collector, the lithium ion secondary battery comprising a recess provided on the surface of the positive electrode mixture layer constituting the electrode sheet on the positive electrode side, and a protrusion protruding from the surface of the positive electrode mixture layer at the periphery of the recess, and the cross-sectional width of the protrusion in the radial direction of the recess is smaller than the diameter of the recess.

[0008] That is, by forming a protuberance on the surface of the positive electrode mixture layer, the friction coefficient can be increased. Furthermore, according to the above-mentioned configuration, during charging, the lithium ions that move from the positive electrode to the negative electrode can be diffused from the protuberance where the lithium ions move in a large amount to the recessed side adjacent to the protuberance where the lithium ions move in a small amount. This makes it possible to suppress localized lithium deposition on the surface of the negative electrode mixture layer. As a result, it is possible to suppress the positional displacement of the separator while ensuring high battery performance.

[0009] A second aspect of the present invention is the lithium ion secondary battery according to the first aspect, wherein a value obtained by dividing a diameter of the peripheral portion having the protrusions by a diameter of the recesses is 2.0 or less. That is, if the diameter of the recess is not large enough relative to the diameter of the peripheral portion having the raised portion, there is a possibility that the lithium ions moving from the formation position of the raised portion where a large amount of the positive electrode active material is present to the negative electrode side cannot be effectively diffused. In this respect, according to the above-mentioned configuration, a sufficiently large diameter can be secured for the recess adjacent to the raised portion. This effectively suppresses localized lithium precipitation on the surface of the negative electrode mixture layer.

[0010] A third aspect is the lithium ion secondary battery according to the first or second aspect, wherein a value obtained by dividing the depth of the recess by the height of the protrusion is 5 or more and 17 or less. That is, the capacity of the lithium ions that move from the positive electrode to the negative electrode during charging, which can diffuse from the position where the protuberance is formed to the adjacent recessed side, depends on the depth of the recess. Therefore, if the depth of the recess is not large enough relative to the height of the protuberance, it may not be possible to effectively diffuse the lithium ions that move from the position where the protuberance is formed to the negative electrode side. On the other hand, as the depth of the recess increases, the amount of positive electrode active material contained in the positive electrode mixture layer decreases. In other words, this may cause a decrease in battery performance. In this regard, according to the above configuration, it is possible to ensure sufficient diffusion capacity for the recessed portion adjacent to the protuberance while suppressing the performance decrease due to the decrease in the amount of positive electrode active material. This effectively suppresses localized lithium precipitation on the surface of the negative electrode mixture layer.

[0011] A fourth aspect of the present invention is the lithium ion secondary battery according to any one of the first to third aspects, wherein the height of the protrusion is 0.5 μm or more and 5 μm or less. That is, when the height of the raised portion is low, there is a possibility that a sufficient increase in the friction coefficient cannot be obtained. On the other hand, when the height of the raised portion is high, the thickness of the positive electrode mixture layer increases, which makes it easier for localized lithium deposition to occur. In this respect, according to the above-mentioned configuration, it is possible to effectively increase the friction coefficient of the surface of the positive electrode mixture layer while suppressing localized lithium deposition on the surface of the negative electrode mixture layer. This makes it possible to effectively suppress the positional displacement of the separator while ensuring high battery performance.

[0012] A fifth aspect is the lithium ion secondary battery according to any one of the first to fourth aspects, wherein the raised portion extends around the entire periphery of the recess. According to the above-mentioned configuration, the coefficient of friction of the surface of the positive electrode mixture layer on which the recesses and protrusions are provided can be effectively increased.

[0013] A sixth aspect is the lithium ion secondary battery according to any one of the first to fifth aspects, in which the electrode body has a configuration as a wound body. That is, when the positive and negative electrode sheets stacked with the separator sandwiched therebetween are wound, the separator is likely to be misaligned, which is called winding misalignment. Therefore, by applying the configurations of aspects 1 to 5 to such a configuration, more significant effects can be obtained.

[0014] A seventh aspect is a method for producing a lithium ion secondary battery comprising an electrode body in which positive and negative electrode sheets are laminated with a separator therebetween, and each of the electrode sheets is formed by laminating an electrode mixture layer on a substrate serving as a current collector, the method comprising the steps of: forming a positive electrode mixture layer laminated on the substrate by coating the substrate with a positive electrode mixture; and including the steps of: causing air bubbles to be contained in the positive electrode mixture before the coating; and forming recesses in the surface of the positive electrode mixture layer by bursting the air bubbles contained in the positive electrode mixture after the coating, and forming protrusions that protrude from the surface of the positive electrode mixture layer around the periphery of the recesses.

[0015] According to the above-mentioned configuration, it is possible to easily form a crater-shaped recess having a ridge on the periphery of the surface of the positive electrode mixture layer with a simple configuration. Furthermore, the number and particle size of the bubbles contained in the positive electrode mixture can be controlled by optimizing various adjustment parameters in the process of incorporating bubbles into the positive electrode mixture before coating. This makes it possible to easily control the shapes of the recesses and ridges formed on the surface of the positive electrode mixture layer by the bursting of the bubbles. Effect of the Invention

[0016] According to the present invention, it is possible to suppress the displacement of the separator while ensuring high battery performance. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a perspective view of a secondary battery. [Diagram 2] FIG. 2 is an exploded view of the electrode assembly. [Diagram 3] FIG. 3 is a side view of the secondary battery. [Figure 4] FIG. 4 is a cross-sectional view of a recess having a protruding portion on the periphery provided on the surface of a positive electrode mixture layer. [Diagram 5] FIG. 5 is a plan view of a recess having a protruding portion on the periphery provided on the surface of the positive electrode mixture layer. [Figure 6] FIG. 6 is a flowchart showing a manufacturing process of an electrode sheet and a method of forming recesses and protrusions on the surface of a positive electrode mixture layer. [Figure 7] FIG. 7 is an explanatory diagram that illustrates the movement of lithium ions in the secondary battery of the reference example. [Figure 8] FIG. 8 is an explanatory diagram that illustrates the movement of lithium ions in the secondary battery of the embodiment. [Figure 9] FIG. 9 is a table showing test results of secondary batteries having recesses and protrusions on the surface of the positive electrode mixture layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of a secondary battery will be described with reference to the drawings. (Lithium-ion secondary battery) 1, the secondary battery 1 includes an electrode assembly 10 in which a positive electrode 3, a negative electrode 4, and a separator 5 are integrated, and a case 20 that houses the electrode assembly 10. The secondary battery 1 of this embodiment has a configuration as a lithium ion secondary battery in which the electrode assembly 10 in the case 20 is impregnated with a non-aqueous electrolyte solution (not shown).

[0019] More specifically, in the secondary battery 1 of this embodiment, the positive electrode 3, the negative electrode 4, and the separator 5 are laminated with a sheet-like outer shape. Then, by winding up the laminate of the positive electrode 3, the negative electrode 4, and the separator 5, an electrode body 10 is formed in which the positive and negative electrodes and the separators 5 are alternately arranged in the radial direction with the separator 5 sandwiched between the positive electrode 3 and the negative electrode 4.

[0020] The case 20 of this embodiment includes a case body 21 having a flat, substantially rectangular box shape, and a lid member 22 that closes an open end 21x of the case body 21. The electrode body 10 of this embodiment has a flat outer shape that corresponds to the box shape of the case 20.

[0021] (Electrode sheet and electrode body) More specifically, as shown in FIG. 2, in the secondary battery 1 of this embodiment, the positive electrode 3 and the negative electrode 4 each have a configuration as an electrode sheet 35 including a current collector 31 having a sheet-like outer shape and an electrode mixture layer 32 laminated on this current collector 31.

[0022] Specifically, for the electrode sheet 35P for the positive electrode 3, a composite paste 37P containing a lithium transition metal oxide serving as a positive electrode active material is applied onto a substrate 36P made of aluminum or the like that constitutes the positive electrode current collector 31P. For the electrode sheet 35N for the negative electrode 4, a slurry-like composite paste 37N containing a carbon-based material serving as a negative electrode active material is applied onto a substrate 36N made of copper or the like that constitutes the negative electrode current collector 31N. Furthermore, each of these composite pastes 37P and 37N contains a binder. In the secondary battery 1 of this embodiment, the composite pastes 37P and 37N are dried to form the corresponding positive electrode composite layer 32P and negative electrode composite layer 32N for the positive and negative electrode sheets 35P and 35N, respectively.

[0023] Furthermore, in the secondary battery 1 of this embodiment, the positive and negative electrode sheets 35P, 35N are each shaped into a belt-like shape. The electrode body 10 of this embodiment has a configuration as a wound body 10X in which the positive and negative electrode sheets 35P, 35N stacked with the separator 5 sandwiched therebetween are wound around a winding axis 10x extending in the width direction of the belt-like shape (the left-right direction in FIG. 2).

[0024] 2, the separator 5 and each electrode sheet 35 are wound in such a manner that the electrode sheet 35P constituting the positive electrode 3 is wound inward. However, this figure is one example showing the structure of the electrode body 10, and the separator 5 and each electrode sheet 35 may be wound in such a manner that the electrode sheet 35N constituting the negative electrode 4 is wound inward. This determines whether the electrode sheet 35 arranged on the outermost shell of the electrode body 10 is the electrode sheet 35P constituting the positive electrode 3 or the electrode sheet 35N constituting the negative electrode 4.

[0025] 1 to 3, the cover member 22 of the case 20 is provided with a positive electrode terminal 38P and a negative electrode terminal 38N that protrude to the outside of the case 20. Furthermore, each electrode sheet 35 has an uncoated portion 39 where the electrode mixture layer 32 is not formed on the current collector 31. The secondary battery 1 of this embodiment is configured such that, by utilizing these uncoated portions 39, the electrode sheet 35P constituting the positive electrode 3 and the positive electrode terminal 38P are electrically connected, and the electrode sheet 35N constituting the negative electrode 4 and the negative electrode terminal 38N are electrically connected.

[0026] Specifically, the electrode body 10 of this embodiment is housed in the case 20 with its winding axis 10x aligned along the longitudinal direction (left-right direction in FIG. 1) of the cover member 22, which is an elongated, generally rectangular plate. Furthermore, in this state, an uncoated portion 39P of an electrode sheet 35P constituting the positive electrode 3 is connected to a positive electrode terminal 38P via a connecting member 40P. Similarly, an uncoated portion 39N of an electrode sheet 35N constituting the negative electrode 4 is connected to a negative electrode terminal 38N via a connecting member 40N.

[0027] Furthermore, an electrolyte solution 45 is injected into the case 20. That is, the electrolyte solution 45 of the secondary battery 1 having a configuration as a lithium ion secondary battery is one in which a lithium salt serving as a supporting salt is dissolved in an organic solvent. Thus, the secondary battery 1 of this embodiment is configured such that the electrode body 10 sealed in the case 20 is impregnated with the electrolyte solution 45.

[0028] (Uneven structure on the surface of the positive electrode mixture layer) As shown in Fig. 4 and Fig. 5, in the secondary battery 1 of this embodiment, a surface 50 of the positive electrode composite layer 32P constituting the electrode sheet 35P on the positive electrode 3 side has a plurality of recesses 51 that are recessed in a so-called crater shape. Specifically, each of these recesses 51 has a substantially circular planar shape. Also, each of these recesses 51 has a so-called mortar-shaped hole shape with a substantially semicircular cross section. And, in the secondary battery 1 of this embodiment, for example, five or more recesses 51 are provided per cell on the surface 50 of the positive electrode composite layer 32P.

[0029] Furthermore, at the peripheral portion 51e of each of these recesses 51, a protruding portion 52 is formed that protrudes from the surface 50 of the positive electrode mixture layer 32P. Specifically, these protruding portions 52 extend over the entire circumference of each recess 51. In this way, the secondary battery 1 of this embodiment increases the friction coefficient of the surface 50 of the positive electrode mixture layer 32P, thereby suppressing misalignment of the separator 5 sandwiched between the positive and negative electrode sheets 35P, 35N. More specifically, this configuration is capable of effectively suppressing so-called winding misalignment that occurs when the separator 5 and the electrode sheets 35P, 35N are wound into the electrode body 10 (see FIG. 2).

[0030] More specifically, the diameter R1 of the recess 51 is preferably set to, for example, 15.0 μm or less. In this case, the "diameter R1 of the recess 51" is the maximum diameter of the substantially circular planar shape, that is, the diameter at the position where the value is maximum. The dimensions of the recess 51 and the protrusion 52 including the diameter R1 can be measured by observing the cross section of the positive electrode composite layer 32P using, for example, an electron microscope or the like (hereinafter the same). In the secondary battery 1 of this embodiment, the diameter R1 of the recess 51 is set to, for example, about 2.0 μm or more and 12.0 μm or less.

[0031] In the secondary battery 1 of this embodiment, the cross-sectional width W of the raised portion 52 in the radial direction of the recess 51 is smaller than the diameter R1 of the recess 51 (R1>W). Furthermore, in the secondary battery 1 of this embodiment, the diameter R2 of the peripheral portion 51e having the raised portion 52 is set to, for example, about 3.0 μm or more and 13.0 μm or less. Thus, the secondary battery 1 of this embodiment is configured such that the value obtained by dividing the diameter R2 of the peripheral portion 51e having the raised portion 52 by the diameter R1 of the recess 51 is 2.0 or less (R2 / R1≦2.0).

[0032] That is, since the raised portion 52 exists at the peripheral edge portion 51e of the concave portion 51, the value obtained by dividing the diameter R2 of the peripheral edge portion 51e having the raised portion 52 by the diameter R1 of the concave portion 51 is greater than 1.0 (1.0 < R2 / R1). And when considering this, the value of "R2 / R1" may be, for example, 1.1 or more.

[0033] Furthermore, in the secondary battery 1 of the present embodiment, the depth D of the concave portion 51 has a value larger than the height H of the raised portion 52 (D > H). Specifically, in the secondary battery 1 of the present embodiment, the depth D of the concave portion 51 is set, for example, to be about 2.5 μm or more and 25 μm or less. Also, the height H of the raised portion 52 is set to be 0.5 μm or more and 5 μm or less. Note that the "height H" in this case is the "protrusion height" of the raised portion 52 with respect to the flat portion on the surface 50 of the positive electrode composite material layer 32P. And the secondary battery 1 of the present embodiment is configured such that the value obtained by dividing the depth D of the concave portion 51 by the height H of the raised portion 52 is 5 or more and 17 or less (5 ≤ (D / H) ≤ 17).

[0034] (Method for forming unevenness on the surface of the positive electrode composite material layer) As shown in FIG. 6, in the manufacturing process of the electrode sheet 35 constituting the secondary battery 1 of the present embodiment, first, kneading of the composite paste 37 as the electrode composite material to be coated on the base material 36 is performed (step 101). In the present embodiment, in this kneading step, the electrode active material, binder, thickener, etc., which are the raw materials of the composite paste 37, are put into the machine of the kneader, and thus the formulation and kneading are performed. Further, following this kneading step, a defoaming step for removing the bubbles mixed into the composite paste 37 by the kneading is executed (step 102). Furthermore, the composite paste 37 after being defoamed in this way is coated on the base material 36 (step 103). And then, a drying step of the composite paste 37 coated on the base material 36 is executed (step 104).

[0035] In the secondary battery 1 of this embodiment, during this drying process, the above-mentioned unevenness, that is, a crater-shaped recess 51 having a protrusion 52 at its peripheral portion 51e, is formed on the surface 50 of the positive electrode composite layer 32P constituting the electrode sheet 35P for the positive electrode 3.

[0036] More specifically, in the secondary battery 1 of this embodiment, when the electrode sheet 35P for the positive electrode 3 is manufactured, the air bubbles contained in the composite paste 37P as the positive electrode composite are not completely removed in the defoaming process of the above step 102. As a result, the air bubbles contained in the composite paste 37P burst in the drying process of the above step 104. As a result, the secondary battery 1 of this embodiment is configured such that a crater-shaped recess 51 having a protuberance 52 at its peripheral portion 51e is formed on the surface 50 of the positive electrode composite layer 32P.

[0037] More specifically, in the secondary battery 1 of this embodiment, the composite paste 37P serving as the positive electrode composite is stirred in the kneading process, so that air bubbles are mixed into the composite paste 37P. In other words, the kneading process is a process for incorporating air bubbles into the positive electrode composite before coating. At this time, the number and particle size of the air bubbles contained in the kneaded composite paste 37P are controlled by adjusting the degree of vacuum in the kneader and the viscosity of the composite paste 37P.

[0038] Specifically, for example, the lower the degree of vacuum in the kneader, that is, the closer the environment is to the atmosphere, the larger the air bubbles will be mixed into the composite paste 37P. Also, the higher the viscosity of the composite paste 37P, that is, the lower its fluidity, the larger the air bubbles will be contained in the composite paste 37P.

[0039] In the secondary battery 1 of this embodiment, the particle size of the bubbles contained in the composite paste 37P is also controlled in the subsequent defoaming step. Specifically, the higher the degree of vacuum, the less likely it is that bubbles with large particle size will be present in the composite paste 37P. In addition, in the secondary battery 1 of this embodiment, the number and particle size of the bubbles contained in the composite paste 37P for the positive electrode 3 are controlled by optimizing various other adjustment parameters in the kneading step and the defoaming step, such as temperature conditions.

[0040] That is, the number of recesses 51 and protuberances 52 formed on surface 50 of positive electrode composite layer 32P corresponds to the number of bubbles contained in composite paste 37P applied on substrate 36P. Furthermore, the shapes of these recesses 51 and protuberances 52, that is, the diameter R1 and depth D of recesses 51, the cross-sectional width W and height H of protuberances 52, and the diameter R2 of peripheral portion 51e having protuberances 52 correspond to the particle size of the bubbles contained in composite paste 37P. Thus, secondary battery 1 of this embodiment is configured such that the number and shapes of recesses 51 and protuberances 52 formed on surface 50 of positive electrode composite layer 32P are controlled.

[0041] (action) As in the secondary battery 1B of the reference example shown in Fig. 7, the friction coefficient can be increased simply by providing a protrusion 55 on the surface 50 of the positive electrode mixture layer 32P. For ease of explanation, the separator 5 sandwiched between the positive and negative electrode sheets 35P, 35N is not shown. This can suppress the positional displacement of the separator 5.

[0042] However, by providing such a protrusion 55, the thickness d' of the portion where the protrusion 55 exists is greater than the thickness d of the positive electrode composite material layer 32P in the flat portion (d < d'). That is, more positive electrode active material exists in this portion, so that during charging, more lithium ions move from the positive electrode 3 side to the negative electrode 4 side at the formation position of the protrusion 55. As a result, local lithium precipitation is likely to occur on the surface 60 of the negative electrode composite material layer 32N facing the protrusion 55 with a separator 5 (not shown) interposed therebetween, specifically, at a position directly facing the protrusion 55 provided on the surface 50 of the positive electrode composite material layer 32P.

[0043] In this regard, as shown in FIG. 8, in the case of the secondary battery 1 of the present embodiment, a raised portion 52 exists at the peripheral edge 51e of the recess 51 provided on the surface 50 of the positive electrode composite material layer 32P. That is, a recess 51 having a smaller thickness d exists adjacent to the raised portion 52 having a larger thickness d of the positive electrode composite material layer 32P (d1 < d < d2). Further, the cross-sectional width W of the raised portion 52 in the radial direction of the recess 51 is smaller than the diameter R1 of the recess 51. For this reason, during charging, lithium ions moving from the positive electrode 3 to the negative electrode 4 are likely to diffuse from a position directly facing the raised portion 52 where a large amount of the positive electrode active material exists to the adjacent recess 51 side. In the secondary battery 1 of the present embodiment, local lithium precipitation on the surface 60 of the negative electrode composite material layer 32N is thereby less likely to occur.

[0044] Next, the effects of the present embodiment will be described. (1) The secondary battery 1 as a lithium-ion secondary battery includes an electrode body 10 in which positive and negative electrode sheets 35 are laminated with a separator 5 interposed therebetween. Each electrode sheet 35 is formed by laminating an electrode composite material layer 32 on a base material 36 serving as a current collector 31. Further, the secondary battery 1 includes a recess 51 provided on the surface 50 of the positive electrode composite material layer 32P constituting the electrode sheet 35P on the positive electrode 3 side, and a raised portion 52 protruding from the surface 50 of the positive electrode composite material layer 32P at the peripheral edge 51e of the recess 51. In this secondary battery 1, the cross-sectional width W of the raised portion 52 in the radial direction of the recess 51 is smaller than the diameter R1 of the recess 51.

[0045] That is, by forming the raised portion 52 on the surface 50 of the positive electrode mixture layer 32P, the friction coefficient can be increased. Furthermore, according to the above configuration, lithium ions that move from the positive electrode 3 to the negative electrode 4 during charging can be diffused from the raised portion 52, where the amount of movement of the lithium ions is large, to the recessed portion 51 side adjacent to the raised portion 52, where the amount of movement of the lithium ions is small. This can suppress localized deposition of lithium on the surface 60 of the negative electrode mixture layer 32N. As a result, it is possible to suppress the positional displacement of the separator 5 while ensuring high battery performance.

[0046] (2) In the secondary battery 1, the value (R2 / R1) obtained by dividing the diameter R2 of the peripheral portion 51e having the protrusion 52 by the diameter R1 of the recess 51 is equal to or smaller than 2.0. That is, if the diameter R1 of the recess 51 is not sufficiently large relative to the diameter R2 of the peripheral portion 51e having the raised portion 52, there is a possibility that the lithium ions moving from the formation position of the raised portion 52, where a large amount of the positive electrode active material is present, to the negative electrode 4 side cannot be effectively diffused. In this regard, according to the above-mentioned configuration, a sufficiently large diameter R1 can be ensured for the recess 51 adjacent to the raised portion 52. This makes it possible to effectively suppress localized precipitation of lithium on the surface 60 of the negative electrode composite layer 32N.

[0047] (3) In the secondary battery 1, the value (D / H) obtained by dividing the depth D of the recess 51 by the height H of the protrusion 52 is 5 or more and 17 or less. That is, the capacity of the lithium ions that move from the positive electrode 3 to the negative electrode 4 during charging, which can diffuse from the position where the protuberance 52 is formed to the adjacent recessed portion 51 side, depends on the depth D of the recessed portion 51. Therefore, if the depth D of the recessed portion 51 is not large enough relative to the height H of the protuberance 52, there is a possibility that the lithium ions that move from the position where the protuberance 52, where a large amount of the positive electrode active material is present, to the negative electrode 4 side cannot be effectively diffused. On the other hand, as the depth D of the recessed portion 51 becomes deeper, the amount of the positive electrode active material contained in the positive electrode mixture layer 32P decreases. In other words, this may cause a decrease in battery performance. In this regard, according to the above-mentioned configuration, it is possible to ensure a sufficient diffusion capacity for the recessed portion 51 adjacent to the protuberance 52 while suppressing the performance decrease due to the decrease in the amount of the positive electrode active material. This effectively suppresses localized lithium precipitation on the surface 60 of the negative electrode mixture layer 32N.

[0048] (4) In the secondary battery 1, the height H of the protrusion 52 is not less than 0.5 μm and not more than 5 μm. That is, when the height H of the raised portion 52 is low, there is a possibility that a sufficient increase in the friction coefficient cannot be obtained. On the other hand, when the height H of the raised portion 52 is high, the thickness d of the positive electrode mixture layer 32P increases, and localized lithium precipitation is likely to occur. In this regard, according to the above-mentioned configuration, it is possible to effectively increase the friction coefficient of the surface 50 of the positive electrode mixture layer 32P while suppressing localized lithium precipitation on the surface 60 of the negative electrode mixture layer 32N. This makes it possible to effectively suppress the positional displacement of the separator 5 while ensuring high battery performance.

[0049] (5) In the secondary battery 1 , the protrusion 52 extends around the entire periphery of the recess 51 . According to the above configuration, the coefficient of friction of surface 50 of positive electrode mixture layer 32P on which recesses 51 and protrusions 52 are provided can be effectively increased.

[0050] (6) The secondary battery 1 has an electrode body 10 configured as a wound body 10X. That is, when the positive and negative electrode sheets 35P and 35N stacked with the separator 5 sandwiched therebetween are wound, the separator 5 is likely to be misaligned, which is called winding misalignment. Therefore, by applying the above configurations (1) to (5) to such a configuration, more significant effects can be obtained.

[0051] (7) The manufacturing process of the secondary battery 1 includes a step of forming a positive electrode composite layer 32P laminated on a base material 36P by applying a composite paste 37P as a positive electrode composite to the base material 36P. The manufacturing process of the secondary battery 1 also includes a step of making the composite paste 37P contain air bubbles before being applied to the base material 36P. The air bubbles contained in the composite paste 37P burst when the composite paste 37P is dried after application to the base material 36P. The manufacturing process of the secondary battery 1 also includes a step of forming recesses 51 on a surface 50 of the positive electrode composite layer 32P by the bursting of the air bubbles, and forming protrusions 52 protruding from the surface 50 of the positive electrode composite layer 32P at peripheral portions 51e of the recesses 51.

[0052] According to the above-mentioned configuration, it is possible to easily form crater-shaped recesses 51 having raised portions 52 at peripheral portions 51e on surface 50 of positive electrode composite layer 32P with a simple configuration. Furthermore, the number and particle size of bubbles contained in composite paste 37P can be controlled by optimizing various adjustment parameters in the process of incorporating bubbles into composite paste 37P before application. This makes it possible to easily control the shapes of recesses 51 and raised portions 52 formed on surface 50 of positive electrode composite layer 32P by the bursting of the bubbles.

[0053] The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.

[0054] The diameter R1 of the recess 51 and the cross-sectional width W of the raised portion 52 in the radial direction of the recess 51 are arbitrary. The diameter R2 of the peripheral portion 51e having the raised portion 52 is also arbitrary. However, it is preferable that the diameter R1 of the recess 51 is sufficiently larger than the cross-sectional width W of the raised portion 52. As described above, it is preferable that the value (R2 / R1) obtained by dividing the diameter R2 of the peripheral portion 51e having the raised portion 52 by the diameter R1 of the recess 51 is 2.0 or less.

[0055] Moreover, the depth D of recesses 51 and the height H of protrusions 52 are also arbitrary. However, it is preferable that the height H of protrusions 52 is 0.5 μm or more and 5 μm or less. Furthermore, as described above, it is preferable that the value (D / H) obtained by dividing the depth D of recesses 51 by the height H of protrusions 52 is 5 or more and 17 or less. The numbers of recesses 51 and protrusions 52 formed on surface 50 of positive electrode composite layer 32P may also be changed arbitrarily.

[0056] In the above embodiment, after the composite paste 37P as the positive electrode composite is applied to the substrate 36P, the crater-shaped recesses 51 having the protuberances 52 at the periphery 51e are formed on the surface 50 of the substrate 36P by bursting the bubbles contained in the composite paste 37P. However, the present invention is not limited to this, and the recesses 51 having the protuberances 52 at the periphery 51e may be formed by other methods. Furthermore, the aspects of the process of including bubbles in the positive electrode composite and the process of forming the recesses 51 and the protuberances 52 by bursting the bubbles may also be changed as desired. The forming method of the above embodiment may be used when forming irregularities on the surface 60 of the negative electrode composite layer 32N.

[0057] In the above embodiment, the raised portion 52 extends around the entire circumference of the recess 51, but a portion of the raised portion in the circumferential direction may be missing. In the above embodiment, the electrode body 10 has a configuration as a wound body 10X, but the positive and negative electrode sheets 35P, 35N stacked with the separator 5 sandwiched therebetween do not necessarily have to be wound.

[0058] The terminal shapes of the positive electrode terminal 38P and the negative electrode terminal 38N are not limited to the shapes shown in Fig. 1 and may be changed as desired. The shape of the case 20 that defines the outer shape of the secondary battery 1 is also not necessarily limited to a flat rectangular box shape and may be changed as desired, for example, to a cylindrical shape.

[0059] Next, the technical ideas that can be understood from the above embodiment and modified examples will be described. (i) A method for manufacturing an electrode body comprising positive and negative electrode sheets stacked with a separator therebetween, each of the electrode sheets being formed by stacking an electrode mixture layer on a substrate which serves as a current collector, the method comprising the steps of: forming the electrode mixture layer stacked on the substrate by applying an electrode mixture to the substrate; and incorporating air bubbles in the electrode mixture before the coating; and forming recesses in the surface of the electrode mixture layer by bursting the air bubbles contained in the electrode mixture after the coating, and forming protrusions that protrude from the surface of the electrode mixture layer around the periphery of the recesses. EXAMPLES

[0060] Examples will be described below to more specifically explain the configuration and effects of the present invention, but the present invention is not limited to these examples. FIG. 9 is a table showing test results when the diameter R1 of the recess 51 and the diameter R2 of the peripheral portion 51e having the raised portion 52, as well as the depth D of the recess 51 and the height H of the raised portion 52, are changed for the recess 51 and the raised portion 52 formed on the surface 50 of the positive electrode mixture layer 32P. In this evaluation test, the "friction coefficient" on the surface 50 of the positive electrode mixture layer 32P was measured as an index representing the "difficulty of misalignment" of the separator 5 stacked on the positive electrode mixture layer 32P. Furthermore, in this evaluation test, the maximum current (mA) at which lithium does not precipitate on the surface 60 of the negative electrode mixture layer 32N during charging of the secondary battery 1 was measured as an index representing the local "difficulty of lithium precipitation" on the surface 60. The precipitation of lithium can be confirmed, for example, by using an ESR (electron spin resonance) device. Then, by combining these two indices, the "resistance to misalignment" and the "resistance to lithium deposition" were comprehensively evaluated.

[0061] 9, "Comparative Example 1" is a case where surface 50 of positive electrode mixture layer 32P is flat and has no irregularities, and "Comparative Example 2" is a case where only recesses 51 are present. Moreover, "Example 1" to "Example 5" and "Comparative Example 3" to "Comparative Example 5" all have crater-shaped recesses 51 having raised portions 52 at peripheral portions 51e on surface 50 of positive electrode mixture layer 32P. Moreover, all of "Example 1" to "Example 5" satisfy the "three preferable ranges" described in the above embodiment.

[0062] That is, in all of "Example 1" to "Example 5", the height H of the raised portion 52 is within the range of 0.5 μm or more and 5 μm or less. Specifically, in these "Example 1" to "Example 5", "Example 4" has a minimum value of "0.5 μm", and "Example 3" has a maximum value of "5.0 μm". Also, in all of these "Example 1" to "Example 5", the value (D / H) obtained by dividing the depth D of the recess 51 by the height H of the raised portion 52 is within the range of 5 or more and 17 or less. Specifically, in these "Example 1" to "Example 5", "Example 3" has a minimum value of "5.0", and "Example 3" has a maximum value of "16.7". In each of "Example 1" to "Example 5," the value (R2 / R1) obtained by dividing the diameter R2 of the peripheral portion 51e having the raised portion 52 by the diameter R1 of the recessed portion 51 is within a range of 2.0 or less, with the maximum value being "2.0" in "Example 1." The minimum value of "R2 / R1" is "1.1" in "Example 4."

[0063] In addition, when comparing these "Example 1" to "Example 5" with "Comparative Example 1" and "Comparative Example 2", the "friction coefficient" of each of "Example 1" to "Example 5" is greater than that of "Comparative Example 1" and "Comparative Example 2". Furthermore, in each of "Example 1" to "Example 5", the "maximum current amount at which lithium does not deposit" is equal to or greater than that of "Comparative Example 1" and "Comparative Example 2". As a result, it can be confirmed that by satisfying the above-mentioned "three preferable ranges" regarding the recesses 51 and the protrusions 52 formed on the surface 50 of the positive electrode mixture layer 32P, it is possible to suppress the positional deviation of the separator 5 while ensuring high battery performance.

[0064] In contrast, in "Comparative Example 3," the value (D / H) obtained by dividing the depth D of the recesses 51 by the height H of the protrusions 52 is "1.9," which is lower than the preferred range, that is, the depth D of the recesses 51 is shallow. As a result, the "maximum amount of current at which lithium does not deposit" is lower than those in "Comparative Example 1" and "Comparative Example 2," that is, lithium is more likely to deposit on the surface 60 of the negative electrode mixture layer 32N.

[0065] Moreover, in "Comparative Example 4," the value (R2 / R1) obtained by dividing diameter R2 of peripheral portion 51e having raised portion 52 by diameter R1 of recessed portion 51 is "3.6," which is larger than the preferred range, that is, diameter R1 of recessed portion 51 is small. As a result, in this case as well, the "maximum amount of current at which lithium does not deposit" is lower than those in "Comparative Example 1" and "Comparative Example 2," that is, lithium is more likely to deposit on surface 60 of negative electrode mixture layer 32N.

[0066] Furthermore, "Comparative Example 5" has a configuration that deviates from all of the above-mentioned "three preferable ranges" regarding the recesses 51 and the protrusions 52. As a result, "Comparative Example 5" has a lower "friction coefficient" and a lower "maximum current amount at which lithium does not deposit" than "Comparative Example 1" and "Comparative Example 2."

[0067] However, in "Comparative Example 4," the value (R2 / R1) obtained by dividing the diameter R2 of the peripheral portion 51e having the raised portion 52 by the diameter R1 of the recessed portion 51 is a value that is significantly outside the preferred range. Also, in "Comparative Example 3" and "Comparative Example 5," the value (D / H) obtained by dividing the depth D of the recessed portion 51 by the height H of the raised portion 52 is a value that is significantly outside the preferred range. And, in "Comparative Example 5," the height H of the raised portion 52 is a value that is significantly outside the preferred range.

[0068] 8, it is presumed that when the deviation from the "three preferred ranges" is small, a certain degree of lithium deposition suppression effect can be obtained by making the diameter R1 of the recess 51 larger than the cross-sectional width W of the raised portion 52 (R1>W). Also, with regard to the "friction coefficient," which is an evaluation index for "resistance to misalignment," it is presumed that a value capable of suppressing misalignment can be obtained to a certain degree if the height H of the raised portion 52 is slightly smaller than the preferred range. [Explanation of symbols]

[0069] 1...Secondary battery (lithium ion secondary battery) 3...Positive electrode 4...Negative electrode 5…Separator 10...Electrode body 31...Current collector 32…Electrode composite material layer 32P…Positive electrode composite layer 35, 35P, 35N...Electrode sheet 36...Base material 50…Surface 51…Recess 51e…periphery 52...Protuberance R1…diameter W…Cross-sectional width

Claims

1. A lithium ion secondary battery comprising an electrode assembly in which positive and negative electrode sheets are laminated with a separator sandwiched therebetween, and each of the electrode sheets is formed by laminating an electrode mixture layer on a substrate serving as a current collector, a recess provided on a surface of a positive electrode mixture layer constituting the positive electrode side electrode sheet; a protruding portion protruding from a surface of the positive electrode mixture layer at a peripheral portion of the recess; In addition to providing The cross-sectional width of the protrusion in the radial direction of the recess is smaller than the diameter of the recess. Lithium-ion secondary battery.

2. A value obtained by dividing the diameter of the peripheral portion having the raised portion by the diameter of the recessed portion is 2. The lithium ion secondary battery according to claim 1, wherein the refractive index is 2.0 or less.

3. The depth of the recess divided by the height of the protrusion is 2. The lithium ion secondary battery according to claim 1, wherein the molecular weight is 5 or more and 17 or less.

4. The height of the protrusion is 0.5 μm or more and 5 μm or less. The lithium ion secondary battery according to any one of claims 1 to 3.

5. The raised portion extends around the entire circumference of the recess. The lithium ion secondary battery according to any one of claims 1 to 3.

6. The electrode body has a configuration as a wound body. The lithium ion secondary battery according to any one of claims 1 to 3.

7. A method for producing a lithium ion secondary battery comprising an electrode assembly in which positive and negative electrode sheets are laminated with a separator sandwiched therebetween, each of the electrode sheets being formed by laminating an electrode mixture layer on a substrate serving as a current collector, the method comprising the steps of: The positive electrode composite layer is formed by applying a positive electrode composite to the substrate, and A step of including air bubbles in the positive electrode mixture before the coating; and forming recesses in the surface of the positive electrode mixture layer by bursting the air bubbles contained in the positive electrode mixture after the coating, and forming protrusions that protrude from the surface of the positive electrode mixture layer around the periphery of the recesses.

Citation Information

Patent Citations

  • Lithium ion battery pole piece and lithium ion battery comprising pole piece

    CN103367702A

  • Nonaqueous electrolyte secondary battery and its manufacturing method

    JP2002298922A

  • Method for manufacturing electrode for lithium secondary battery, electrode for lithium secondary battery, and lithium secondary battery

    JP2013097925A

  • Nonaqueous electrolyte secondary battery

    JP1999176421A

  • Secondary battery and method for manufacturing the same

    JP2013054871A