Card and method for manufacturing card
The card design addresses glare issues in metallic cards by incorporating a matte-finished protective layer with controlled roughness and low gloss, ensuring a solid and calm appearance.
Patent Information
- Application Number
- JP2023080806
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional metallic cards exhibit excessive glare due to light reflection, lacking a design that provides a solid and calm impression while maintaining metallic texture and gloss.
A card design with a card base material, a metal vapor deposition layer, and a protective layer, where the protective layer has a matte finish with specific roughness and low gloss, and a peelable layer is interposed between the metal vapor deposition and protective layers to prevent glare.
The design suppresses glare and provides a solid, calm impression while maintaining metallic texture and gloss, with the matte finish effectively reducing light reflection.
Smart Images

Figure 2024165007000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a card and a method for manufacturing a card. [Background technology]
[0002] Cards such as IC cards and magnetic cards are used in various fields, such as cash cards, credit cards, ID cards, membership cards, etc. As one such card, Patent Document 1 discloses a metallic card in which a metal deposition layer and a protective layer are laminated in that order on a card substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5708109 Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional metallic cards have a strong gloss and a mirror-like metal vapor deposition layer, which causes a lot of glare due to reflected light. In recent years, there has been a demand for metallic cards with excellent design that maintain the texture of metal and the gloss of the mirror surface while suppressing glare, in order to give a heavy and calm impression.
[0005] In view of the above-mentioned problems, an object of the present invention is to provide a card and a method for manufacturing the card that, while being a metallic card, reduces glare caused by light reflection and gives a heavy, calm impression. [Means for solving the problem]
[0006] One aspect of the present invention is a card comprising a card substrate, and a metal deposition layer and a protective layer laminated in that order on the upper surface of the card substrate. The upper surface of the protective layer has an arithmetic mean roughness Ra of 0.2 μm or more, a ten-point mean roughness Rz of 1.5 μm or more, and a glossiness Gs(60°) of 150 or less.
[0007] One aspect of the present invention is a method for manufacturing a card, comprising the steps of preparing a transfer sheet substrate having a matte-finished uneven surface, and a protective layer transfer foil having the protective layer laminated on the uneven surface, overlaying the protective layer transfer foil on the metal vapor deposition layer laminated on the card substrate, thereby interposing the protective layer between the metal vapor deposition layer and the transfer sheet substrate, and peeling the transfer sheet substrate from the protective layer. Effect of the Invention
[0008] According to the present invention, it is possible to provide a card that, while being a metallic card, has reduced glare due to light reflection and gives a more solid and calm impression. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view showing a schematic view of a main part of a card according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a state before a metal layer transfer foil is superimposed on a card substrate in a card manufacturing method according to one embodiment of the present invention. [Diagram 3] 3 is a diagram showing the state after the metal layer transfer foil has been superimposed on the card substrate in a card manufacturing method according to one embodiment of the present invention. FIG. [Figure 4] This figure shows the state after the first transfer sheet substrate has been removed from the metal vapor deposition layer and before the protective layer transfer foil is superimposed on the metal vapor deposition layer in a card manufacturing method according to one embodiment of the present invention. [Diagram 5] 2 is a diagram showing the state after a protective layer transfer foil is superimposed on a metal vapor deposition layer in a card manufacturing method according to one embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the present invention will be described with reference to FIGS. As shown in FIG. 1, a card 1 of this embodiment includes a card substrate 2, a metal vapor deposition layer 3, and a protective layer 4.
[0011] The card substrate 2 of this embodiment is formed by laminating one or more layers of core sheets 21 and an over sheet 22. In Fig. 1, the card substrate 2 is formed by one layer of core sheet 21 and one layer of over sheet 22. Note that the card substrate 2 may be formed by providing the over sheets 22 on both sides of one layer of core sheet 21. The upper surface 2a of the card substrate 2, on which the metal vapor deposition layer 3 and protective layer 4 described later are laminated, is formed by the over sheet 22.
[0012] The core sheet 21 and the oversheet 22 are white sheets or light-transmitting sheets. Examples of materials that can be used for the core sheet 21 and the oversheet 22 include vinyl chloride materials, vinyl chloride-vinyl acetate copolymer materials, copolymer materials of terephthalic acid with cyclohexanedimethanol and ethylene glycol, amorphous polyester materials made of polymer alloys of the above-mentioned copolymers with polycarbonate and / or polyarylate, polyethylene terephthalate materials, polybutylene terephthalate materials, acrylonitrile-butadiene-styrene copolymer synthetic resin (ABS) materials, paper materials, impregnated paper materials, and the like.
[0013] In this embodiment, a magnetic stripe 5 (magnetic tape) is provided on the top surface 2a of the card substrate 2. The magnetic stripe 5 provides the card 1 with a magnetic function. The magnetic stripe 5 is provided on part of the top surface 2a of the card substrate 2. In FIG. 1, the magnetic stripe 5 is embedded in the card substrate 2 so as to be exposed on the top surface 2a of the card substrate 2. Specifically, the magnetic stripe 5 is embedded in an oversheet 22. From the viewpoint of magnetic reading, it is preferable that the film thickness of layers overlapping the magnetic stripe 5 (e.g., the metal deposition layer 3, the protective layer 4, etc.) be 10 μm or less in total.
[0014] The metal deposition layer 3 and the protective layer 4 are laminated in this order on the upper surface 2a of the card substrate 2. The metal deposition layer 3 is formed by depositing a metal by a vacuum deposition method or the like. The metal deposition layer 3 of this embodiment has insulating properties by forming the metal in an island-like shape. The metal deposition layer 3 may be formed, for example, by depositing a metal in an island-like shape, or by depositing a metal and then partially removing it to form an island-like shape. Fine linear lines may be formed on the upper surface of the metal deposition layer 3 by, for example, hairline processing (see Japanese Patent No. 5708109).
[0015] Metals such as aluminum, chromium, iron, cobalt, nickel, silver, tin, and gold, or compounds thereof, can be used as the metals constituting the metal deposition layer 3. The metal deposition layer 3 can be formed by a method such as a vacuum deposition method, a sputtering method, an ion plating method, and a plating method. The thickness of the metal vapor deposition layer 3 is preferably in the range of, for example, 10 nm to 100 nm. If the thickness of the metal vapor deposition layer 3 is less than 10 nm, the effect of metallic luster is lost. If the thickness of the metal vapor deposition layer 3 exceeds 100 nm, it takes a long time to form the metal vapor deposition layer 3, and the thickness becomes uneven. In addition, the metal vapor deposition layer 3 does not form an island-like shape, making it difficult to ensure insulation.
[0016] In the card 1 of this embodiment, a peel-off protective layer 32 is interposed between the metal vapor deposition layer 3 and a protective layer 4 described later. The peel-off protective layer 32 is in contact with an upper surface 2a of the metal vapor deposition layer 3. The peel-off protective layer 32 serves to peel off the transfer sheet substrate 31 (see Figs. 2 and 3) from the metal vapor deposition layer 3 in a manufacturing method of the card 1 described later. The peel-off protective layer 32 is transparent. This allows the metal vapor deposition layer 3 to be seen through from the peel-off protective layer 32 side. The material for the release protective layer 32 may be, for example, urethane resin, melamine resin, cellulose resin, epoxy resin, acrylic resin, butyral resin, vinyl chloride / vinyl acetate copolymer resin, etc. Furthermore, wax or the like may be used as the material for the release protective layer 32, if necessary. The thickness of the release protective layer 32 is preferably in the range of 1 μm to 3 μm. The total thickness of the above-mentioned metal deposition layer 3 and release protective layer 32 may be, for example, 6.0 μm or less.
[0017] The protective layer 4 laminated on the metal vapor deposition layer 3 is transparent. This allows the metal vapor deposition layer 3 to be seen through from the protective layer 4 side. The resin used for the protective layer 4 may be a thermoplastic resin, a thermosetting resin, an ultraviolet curable resin, an electron beam curable resin, or the like. Specific examples of the resin include, but are not limited to, vinyl chloride-vinyl acetate copolymer, positive vinyl alcohol, positive ester resin, polyurethane resin, acrylic resin, copolymers thereof, polymer alloy, and acrylic UV resin obtained by adding isocyanate to positive ester positive ol.
[0018] The upper surface 4a of the protective layer 4 superimposed on the metal vapor deposition layer 3 is an uneven surface. This gives the upper surface 4a of the protective layer 4 a matte finish. Specifically, the upper surface 4a of the protective layer 4, which is an uneven surface 41a, has an arithmetic mean roughness Ra of 0.2 μm or more, a ten-point mean roughness Rz of 1.5 μm or more, and a glossiness Gs (60°) of 150 or less.
[0019] In the card 1 of the present embodiment, a printed layer 42 is interposed between the metal vapor deposition layer 3 and the protective layer 4. The printed layer 42 is in contact with the protective layer 4. The printed layer 42 can be provided by a known printing method such as offset printing or screen printing. Any ink may be used for the printed layer 42. However, it is more preferable to use an ink with low concealing properties for the printed layer 42, which allows the metal vapor deposition layer 3 to be seen through from the printed layer 42 side. The thickness of the printed layer 42 is preferably 0.5 μm to 1.0 μm. This allows the printed layer 42 to be colored in any color while making the most of the gloss and texture of the metal vapor deposition layer 3. The printed layer 42 may be colorless and transparent, or may be colored and transparent, for example. The printed layer 42 may also include characters, symbols, patterns, and the like. The total thickness of the protective layer 4 and the printed layer 42 may be 1.5 μm to 3.0 μm.
[0020] Next, an example of a method for manufacturing the card 1 of this embodiment will be described with reference to FIGS. In manufacturing the card 1 shown in FIG. 1, first, the card substrate 2 and metal layer transfer foil 30 shown in FIG. 2, and the protective layer transfer foil 40 shown in FIG. 4 are prepared.
[0021] 2, the card substrate 2 is formed by laminating an oversheet 22, in which a magnetic stripe 5 is embedded, on the upper surface (one side) of a core sheet 21. In this state, the magnetic stripe 5 is exposed on the upper surface 2a of the card substrate 2 made of the oversheet 22.
[0022] The metal layer transfer foil 30 is formed by sequentially laminating a release protective layer 32 and a metal vapor deposition layer 3 on a transfer sheet substrate 31 (hereinafter referred to as the first transfer sheet substrate 31). As the first transfer sheet substrate 31, a film of polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene (PE), polypropylene (PP), polycarbonate, or polyimide can be used. The metal vapor deposition layer 3 is formed on the first transfer sheet substrate 31 so that the metal is formed in an island-like shape. The materials and thicknesses of the release protective layer 32 and the metal vapor deposition layer 3 are as described above.
[0023] 4, the protective layer transfer foil 40 is formed by sequentially laminating a protective layer 4 and a printed layer 42 on a transfer sheet substrate 41 (hereinafter referred to as the second transfer sheet substrate 41). As the second transfer sheet substrate 41, for example, the film exemplified for the first transfer sheet substrate 31 of the metal layer transfer foil 30 described above can be used. The materials, thicknesses, etc. of the protective layer 4 and the printed layer 42 are as described above. The second transfer sheet substrate 41 has a matte-finished uneven surface 41a. The protective layer 4 is laminated on the uneven surface 41a of the second transfer sheet substrate 41. As a result, the surface (upper surface 4a) of the protective layer 4 facing the second transfer sheet substrate 41 is matte-finished. The matte-finished surface (upper surface 4a) of the protective layer 4 has an arithmetic mean roughness Ra of 0.2 μm or more and a ten-point mean roughness Rz of 1.5 μm or more.
[0024] As shown in FIG. 2, after preparing the card substrate 2 and the metal layer transfer foil 30, the metal vapor deposition layer 3 is transferred to the card substrate 2. When transferring the metal vapor deposition layer 3, first, as shown in FIG. 3, the metal layer transfer foil 30 is placed on the card substrate 2, and the metal vapor deposition layer 3 is interposed between the card substrate 2 and the first transfer sheet substrate 31. Specifically, the metal vapor deposition layer 3 is placed on the upper surface 2a of the card substrate 2 on which the magnetic stripe 5 is exposed. Next, as shown in FIG. 4, the first transfer sheet substrate 31 is peeled off from the metal vapor deposition layer 3. Specifically, the first transfer sheet substrate 31 is peeled off from the peelable protective layer 32, and the peelable protective layer 32 remains on the metal vapor deposition layer 3 side. This completes the transfer of the metal vapor deposition layer 3 to the card substrate 2.
[0025] After the metal deposition layer 3 is transferred to the card substrate 2 and the protective layer transfer foil 40 is prepared, the protective layer 4 and the printed layer 42 are transferred onto the metal deposition layer 3. When transferring the protective layer 4 and the printed layer 42, the protective layer transfer foil 40 is first superimposed on the metal deposition layer 3 as shown in FIG. 5, and the protective layer 4 and the printed layer 42 are interposed between the metal deposition layer 3 and the second transfer sheet substrate 41. Specifically, the protective layer transfer foil 40 is superimposed on the peelable protective layer 32 on the metal deposition layer 3. In addition, the printed layer 42 and the protective layer 4 are arranged in order from the peelable protective layer 32 toward the second transfer sheet substrate 41. Next, as shown in FIG. 1, the second transfer sheet substrate 41 is peeled off from the protective layer 4. This completes the transfer of the protective layer 4 and the printed layer 42 onto the metal deposition layer 3. This completes the method for manufacturing the card 1 of this embodiment.
[0026] Upper surface 4a of protective layer 4 in manufactured card 1 has an arithmetic mean roughness Ra of 0.2 μm or more, a ten-point mean roughness Rz of 1.5 μm or more, and a gloss level Gs(60°) of 150 or less.
[0027] In the card 1 of this embodiment, the gloss level Gs (60°) of the upper surface 4a of the protective layer 4 is 150 or less, so that glare due to light reflection can be suppressed even if the metal vapor deposition layer 3 has a mirror-like finish. This makes it possible to provide a card 1 that gives a heavy and calm impression while maintaining the metallic texture and mirror-like gloss of the metal vapor deposition layer 3.
[0028] Furthermore, although the card 1 of this embodiment further includes a magnetic stripe 5 arranged on the upper surface 2a side of the card substrate 2 facing the metal vapor deposition layer 3, the gloss level Gs (60°) of the upper surface 4a of the protective layer 4 is 150 or less. This effectively prevents the magnetic stripe 5 from being visible from the upper surface 4a side of the protective layer 4. Therefore, a card 1 with an excellent design can be provided.
[0029] In addition, in the manufacturing method of the card 1 of this embodiment, the upper surface 4a of the protective layer 4 facing the second transfer sheet substrate 41 is matted simply by laminating the protective layer 4 on the uneven surface 41a of the second transfer sheet substrate 41. Therefore, after the second transfer sheet substrate 41 is peeled off from the protective layer 4, unevenness corresponding to the uneven surface 41a of the second transfer sheet substrate 41 appears on the upper surface 4a of the protective layer 4 that was in contact with the second transfer sheet substrate 41. As a result, the upper surface 4a of the protective layer 4 can be formed into an uneven surface with a desired surface roughness with fewer steps compared to the case where the uneven surface 41a is formed by matting the upper surface 4a of the protective layer 4 after transferring the protective layer 4 onto the metal deposition layer 3. Therefore, the card 1 can be manufactured efficiently. EXAMPLES
[0030] The card 1 of the above embodiment will be further described below with reference to Example 1, Example 2, and Comparative Example 1. The technical scope of the present invention is not limited in any way by the specific contents of Example 1, Example 2, and Comparative Example 1 shown below.
[0031] <Example 1> A card substrate 2 was obtained by laminating an oversheet 22 made of a 100 μm thick transparent PET-G substrate with an embedded magnetic stripe 5 on both sides of a core sheet 21 made of a 600 μm thick white PET-G substrate, with the magnetic stripe 5 positioned on the outer side. A metal vapor deposition layer 3 and a peelable protective layer 32 were transferred onto one oversheet 22 forming the upper surface 2a of the card substrate 2 using a metal layer transfer foil 30 described below, thereby laminating the metal vapor deposition layer 3 and the peelable protective layer 32 in that order on the upper surface 2a of the card substrate 2. Furthermore, a printed layer 42 and a protective layer 4 were transferred onto the peelable protective layer 32 using a protective layer transfer foil 40 described below, thereby laminating the printed layer 42 and the protective layer 4 in that order on the peelable protective layer 32. In this manner, the card of Example 1 was obtained.
[0032] (Metal layer transfer foil) A 2 μm-thick release protective layer 32 mainly composed of acrylic resin and a 40 nm-thick metal deposition layer 3 were laminated in this order on a first transfer sheet substrate 31 made of PET to produce a metal layer transfer foil 30. The metal deposition layer 3 was made insulating by forming tin (Sn) in a sea-island shape by a vacuum deposition method.
[0033] (Protective layer transfer foil) A matte textured finish (matte finish) was applied to the surface of the second transfer sheet substrate 41 made of PET with a thickness of 100 μm, which was in contact with the protective layer 4. Thereafter, a 1.4 μm thick protective layer 4 made mainly of acrylic resin and a 1.5 μm thick printed layer 42 made of colorless and transparent acrylic resin were laminated in this order on the second transfer sheet substrate 41 to produce a protective layer transfer foil 40.
[0034] (surface roughness and gloss) For the card of Example 1, the arithmetic mean roughness Ra and ten-point mean roughness Rz of the upper surface 4a of the protective layer 4 were measured using a surface roughness measuring device. In addition, the glossiness of the upper surface 4a of the protective layer 4 was measured using a glossmeter (handy glossmeter PG-II manufactured by Nippon Denshoku Industries Co., Ltd.). The light incident angle during the glossiness measurement was 60°, which is highly versatile. In the card of Example 1, the upper surface 4a of the protective layer 4 had an arithmetic mean roughness Ra of 0.28 μm, a ten-point mean roughness Rz of 2.02 μm, and a glossiness Gs (60°) of 137.5. The card of Example 1 had a metallic card surface, but reduced glare due to light reflection.
[0035] <Example 2> The card of Example 2 was obtained by the same method as in Example 1. However, in the card of Example 2, when the protective layer transfer foil 40 was produced, the surface of the second transfer sheet substrate 41 that contacted the protective layer 4 was subjected to an uneven processing with a larger matte texture than that of Example 1.
[0036] (surface roughness and gloss) For the card of Example 2, the arithmetic mean roughness Ra and ten-point mean roughness Rz of the upper surface 4a of the protective layer 4 were measured using the same surface roughness measuring device as in Example 1. In addition, the glossiness of the upper surface 4a of the protective layer 4 was measured using the same gloss meter as in Example 1 with the light incident angle set to 60°. In the card of Example 2, the arithmetic mean roughness Ra was 0.52 μm, the ten-point mean roughness Rz was 3.16 μm, and the glossiness Gs (60°) was 54.8 for the upper surface 4a of the protective layer 4. The card of Example 2 had a metallic card surface, but was a card with almost no glare due to light reflection.
[0037] <Comparative Example 1> The card of Comparative Example 1 was obtained in the same manner as in Example 1. However, in the card of Comparative Example 1, when the protective layer transfer foil 40 was produced, the protective layer 4 and the printed layer 42 were laminated in this order on the second transfer sheet substrate 41 without subjecting the second transfer sheet substrate 41 to the uneven processing as in Examples 1 and 2.
[0038] (surface roughness and gloss) For the card of Comparative Example 1, the arithmetic mean roughness Ra and ten-point mean roughness Rz of the upper surface 4a of the protective layer 4 were measured using the same surface roughness measuring device as in Example 1. In addition, the glossiness of the upper surface 4a of the protective layer 4 was measured using the same gloss meter as in Example 1 with the light incident angle set to 60°. In the card of Comparative Example 1, the upper surface 4a of the protective layer 4 had an arithmetic mean roughness Ra of 0.11 μm, a ten-point mean roughness Rz of 0.64 μm, and a glossiness Gs (60°) of 193.6. The card of Comparative Example 1 was a metallic card with a strong mirror gloss to the extent that reflections occurred on the card surface.
[0039] <Comparison results> Comparing the matte-finished card surfaces of Examples 1 and 2 with the card surface of Comparative Example 1, the glossiness of Examples 1 and 2 was lower than that of Comparative Example 1. Moreover, the card surface of Example 2, which was matte-finished to have a rougher matte grain than Example 1, had an even lower glossiness than the card surface of Example 1. The cards in Examples 1 and 2 had a lower gloss level, which reduced glare due to reflection, and while maintaining a metallic mirror gloss, gave a solid, calm impression. Furthermore, while the magnetic stripe 5 in Comparative Example 1 stood out, the magnetic stripe 5 in Examples 1 and 2 was less noticeable and blended in with the card surface.
[0040] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and can be modified as appropriate without departing from the spirit of the present invention.
[0041] In the present invention, the card substrate 2 may be composed of, for example, only a single-layer core sheet 21 .
[0042] The card of the present invention may not, for example, be provided with a magnetic stripe 5 .
[0043] The card of the present invention may not have, for example, the peelable protective layer 32. In this case, the first transfer sheet substrate 31 of the metal layer transfer foil 30 itself may have peelability. This allows the metal vapor deposition layer 3 to be peeled off from the first transfer sheet substrate 31 during card manufacture, as in the above embodiment.
[0044] The card of the present invention may not include the printed layer 42, for example. [Explanation of symbols]
[0045] 1 Card 2 Card substrate 2a Upper surface of card substrate 2 3 Metal vapor deposition layer 4 protective layer 4a Upper surface of protective layer 4 5 Magnetic Stripe 30 Metal layer transfer foil 31 First transfer sheet substrate 40 Protective layer transfer foil 41 Second transfer sheet base material (transfer sheet base material) 41a Uneven surface 42 Printing layer
Claims
1. A card substrate, and a metal deposition layer and a protective layer laminated in this order on an upper surface of the card substrate, The card has an upper surface of the protective layer having an arithmetic mean roughness Ra of 0.2 μm or more, a ten-point mean roughness Rz of 1.5 μm or more, and a gloss level Gs (60°) of 150 or less.
2. The card of claim 1 , further comprising a magnetic stripe disposed on the top side of the card substrate opposite the metallized layer.
3. A method for producing the card according to claim 1 or 2, comprising the steps of: A step of preparing a transfer sheet substrate having a matte-finished uneven surface, and a protective layer transfer foil having the protective layer laminated on the uneven surface; a step of overlapping the protective layer transfer foil on the metal vapor deposition layer laminated on the card substrate, so that the protective layer is interposed between the metal vapor deposition layer and the transfer sheet substrate; peeling the transfer sheet substrate from the protective layer; A method for manufacturing a card comprising the steps of:
Citation Information
Patent Citations
Forming method of expanded pipe socket
JP1982008109A