Laminate
The laminate's innovative surface layer design with controlled unevenness reduces gloss and fingerprint adherence, ensuring a matte finish and easy cleaning, addressing the issue of smudge-prone glossy surfaces.
Patent Information
- Application Number
- JP2023080999
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Existing laminates with uneven surfaces to reduce gloss tend to attract fingerprints due to increased surface area contact, leading to smudges and potential damage to the design.
A laminate design featuring a base material, a design layer, and a surface layer with a first and second layer, where the second layer is provided in a predetermined pattern with an uneven shape having a ratio of total surface area within 2.5 μm from the maximum height of 10% or less, and a maximum roughness of 12.5 μm or less, forming an irregular wrinkle structure to minimize gloss and fingerprint adherence.
The laminate effectively reduces gloss while minimizing fingerprint adherence and smudges, maintaining a matte appearance and ease of cleaning, with reduced risk of scratches and design damage.
Smart Images

Figure 2024165118000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate. [Background technology]
[0002] A laminate used as a decorative sheet, as described in Patent Document 1, is known. The laminate is used for the interior and exterior of buildings, the surfaces of fittings, furniture, home appliances, and the like, and the interior of vehicles. A surface layer for suppressing gloss is provided on the surface of the laminate. The surface layer forms an uneven shape on the surface of the laminate. Light incident on the laminate is diffusely reflected and diffused by the uneven shape, thereby reducing the gloss on the surface of the laminate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-165030 A Summary of the Invention [Problem to be solved by the invention]
[0004] The uneven shape increases the surface area of the laminate. When the surface of the laminate is touched with a finger, the contact area between the finger and the laminate is large, so sebum is likely to adhere to the surface of the laminate as fingerprints. Fingerprints are observed as stains. It is desirable that fingerprints are less likely to adhere to the surface of the laminate. The present disclosure aims to make it difficult for fingerprints to adhere to the surface of the laminate while suppressing gloss by the uneven shape of the surface of the laminate. [Means for solving the problem]
[0005] One embodiment of the present disclosure relates to the following [1] to [8]. [1] A laminate having a first surface and a second surface opposite the first surface, A substrate and a surface layer are provided in this order from the first surface to the second surface, the surface layer includes a first layer and a second layer provided closer to the second surface than to the first surface with respect to the first layer, the second layer is provided in a predetermined pattern; The second surface has an uneven shape formed thereon, A laminate, wherein the ratio of the total surface area of portions of the second surface having a height within 2.5 μm from the maximum height thereof to the surface area of the second surface is 10% or less. [2] The laminate according to [1], wherein the second surface has a maximum height roughness Rz defined in JIS B0601:2013 of 12.5 μm or less. [3] The laminate according to [1] or [2], wherein the uneven shape has an irregular wrinkled structure. [4] The laminate according to any one of [1] to [3], wherein the uneven shape is formed by linear convex portions and concave portions between the linear convex portions. [5] The laminate according to any one of [1] to [4], wherein the first layer has a thickness of 1 μm or more and 20 μm or less. [6] The laminate according to any one of [1] to [5], wherein the second layer has a thickness of 0.1 μm or more and 5 μm or less. [7] The laminate according to any one of [1] to [6], wherein the second surface has a 60° specular gloss, as defined in JIS Z8741:1997, of 10.0 or less. [8] A design layer is disposed between the substrate and the surface layer, The design layer includes a colored layer and a pattern layer provided closer to the second surface than the first surface with respect to the colored layer, The laminate according to any one of [1] to [7], wherein the design layer is provided in a pattern corresponding to the pattern of the second layer. Effect of the Invention
[0006] According to the present disclosure, the uneven shape of the surface of the laminate can suppress gloss while also making it difficult for fingerprints to adhere to the surface of the laminate. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a laminate. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of the laminate. [Diagram 3] FIG. 3 is a photograph of the second side of the laminate. [Figure 4] FIG. 4 is an enlarged cross-sectional view of the surface layer of the laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the drawings attached to this specification, the scale and the aspect ratio are appropriately changed and exaggerated from those of the actual objects for the convenience of illustration and understanding. Configurations shown in some drawings may be omitted in other drawings.
[0009] In this specification, terms specifying shapes or geometric conditions and their degrees, such as "parallel," "orthogonal," "same," and the like, as well as values of lengths and angles, are not limited to their strict meanings, but are interpreted to include a range within which similar functions can be expected.
[0010] In this specification, when multiple upper limit candidates and multiple lower limit candidates are listed for a parameter, the parameter may be a numerical range that combines any one of the upper limit candidates with any one of the lower limit candidates.
[0011] The laminate 10 according to an embodiment of the present disclosure is used as a decorative sheet. The laminate 10 may be used, for example, as a member constituting the outermost layer of the interior and exterior of buildings, the surfaces of fittings, furniture, and home appliances, the interior of vehicles, and the like. More specifically, the laminate 10 may be used, for example, as interior components of buildings such as walls, ceilings, and floors, exterior components such as exterior walls, eaves ceilings, roofs, fences, and fences, fittings or fixtures such as window frames, doors, door frames, handrails, baseboards, moldings, and other fittings or fixtures, general furniture such as chests of drawers, shelves, and desks, kitchen furniture such as dining tables and sinks, surface decorative panels such as cabinets for home appliances and office automation equipment, and interior and exterior components of vehicles. The laminate 10 may be used as packaging materials, anti-glare films for displays, whiteboards (whiteboards) or blackboards, various cards such as credit cards, cash cards, telephone cards, and various certificates, various keyboard keys, transparent panels (window glass, etc.) such as windows, doors, and partitions, and artificial leather.
[0012] The laminate 10 of the present embodiment may be overlaid on another member that serves as an adherend. The adherend may be, for example, a member that constitutes the interior and exterior of a building, a fitting, a surface of furniture, a home appliance, or a lower layer of a vehicle's interior. The adherend and the laminate 10 may constitute a decorative material.
[0013] The laminate 10 of this embodiment has a surface layer 40. The surface layer 40 forms an uneven shape 13 on the second surface 12 of the laminate 10. The uneven shape 13 makes the second surface 12 a matte surface. Light incident on the laminate 10 is diffused by the uneven shape 13 of the second surface 12. The surface layer 40 reduces the gloss on the second surface 12 of the laminate 10. By reducing the gloss, the second surface can be made to look more like a natural material such as natural wood. In this embodiment, a specific uneven shape 13 is formed on the second surface 12. The uneven shape 13 on the second surface 12 of the laminate 10 reduces the gloss while making it difficult for fingerprints to adhere to the second surface 12 of the laminate 10.
[0014] A laminate 10 according to an embodiment of the present disclosure will be described with reference to FIGS. 1 to 4. FIG. 1 is a cross-sectional view of an example of the laminate 10. FIG. 2 is a cross-sectional view of another example of the laminate 10. In the example shown in FIGS. 1 and 2, the laminate 10 has a first surface 11 and a second surface 12. The second surface 12 is the surface opposite to the first surface 11. The first surface 11 and the second surface 12 are the main surfaces of the laminate 10. When the laminate 10 is overlaid on another member that is to be an adherend, the first surface 11 faces the member. The second surface 12 of the laminate 10 is observed by an external observer. The laminate 10 displays a design on the second surface 12. The second surface 12 has an uneven shape 13 formed thereon. Due to the uneven shape 13, the gloss of the laminate 10 is reduced on the second surface 12. The uneven shape 13 has a wrinkled structure. The second surface 12 of the laminate 10 is provided with a textured surface 13 that provides a tactile sensation.
[0015] As shown in FIG. 1 and FIG. 2, the laminate 10 includes, from the first surface 11 to the second surface 12, a substrate 20, a design layer 30, and a surface layer 40. The design layer 30 is disposed between the substrate 20 and the surface layer 40. In the example shown in FIG. 2, the laminate 10 further includes a resin layer 50 disposed between the design layer 30 and the surface layer 40. The laminate 10 may include other layers intended to perform specific functions. For example, the laminate 10 may further include a primer layer between the surface layer 40 and the design layer 30 or the resin layer 50 in order to improve adhesion between the surface layer 40 and the design layer 30 or the resin layer 50.
[0016] The substrate 20 supports the design layer 30 and the surface layer 40. The substrate 20 is in the form of a film. The thickness of the substrate 20 may be 10 μm or more, or may be 20 μm or more. The thickness of the substrate 20 may be 1 mm or less, or may be 300 μm or less.
[0017] The material of the substrate 20 may be, for example, a resin material, a metal material, a non-metallic inorganic material, or a fibrous material. The resin material may be, for example, a polyester resin such as polyethylene terephthalate, an olefin resin such as polyethylene or polypropylene, a vinyl chloride resin such as polyvinyl chloride, or an acrylic resin. The metal material may be, for example, aluminum, iron, copper, gold, silver, chromium, nickel, cobalt, tin, titanium, or an alloy thereof. The non-metallic inorganic material may be, for example, a non-ceramic ceramic material such as cement, ALC (lightweight aerated concrete), gypsum, calcium silicate, or wood chip cement, a ceramic ceramic material such as pottery, earthenware, glass, or enamel, or a natural stone such as limestone, marble, granite, or andesite. The fibrous material may be, for example, paper, woven fabric, non-woven fabric, or a material impregnated with a resin. The substrate 20 may include only one layer made of these materials. The substrate 20 may include multiple layers made of these materials. The substrate 20 may include multiple layers made of different materials. The substrate 20 may include an adhesive layer or the like between the multiple layers.
[0018] The design layer 30 forms a design displayed on the second surface 12 of the laminate 10. The design formed by the design layer 30 may be, for example, a picture, a photograph, a figure, a pattern, a mark, a character, a color, or other picture pattern. More specifically, the design formed by the design layer 30 may be, for example, a wood grain pattern such as annual rings and vessel grooves on the surface of a wooden board; a stone grain pattern on the surface of a stone slab such as marble or granite; a fabric grain pattern on a cloth surface; a leather grain pattern on a leather surface; a tiled pattern including joint grooves; a brickwork pattern including joint grooves; a sand grain pattern; a matte pattern; a pattern formed by arranging a plurality of concave and convex ridges extending in parallel directions (so-called "line-like concave and convex pattern" or "ray carving pattern"); an abstract pattern such as a geometric pattern, a character, a figure, a polka dot, or a floral pattern; and the like.
[0019] The design layer 30 includes a colored layer 31 and a pattern layer 32. The pattern layer 32 is provided closer to the second surface 12 than the first surface 11 is to the colored layer 31. When observed from the second surface 12, the colored layer 31 and the pattern layer 32 are observed. The pattern layer 32 is provided in a pattern corresponding to the pattern of a second layer 42 of the surface layer 40, which will be described later. In the illustrated example, when observed from the second surface 12, the pattern layer 32 is provided in a portion where the second layer 42 of the surface layer 40 is not provided.
[0020] The colored layer 31 forms a base for the design formed by the design layer 30. The colored layer 31 displays a desired color on the entire surface of the laminate 10. The colored layer 31 is a so-called solid layer. The colored layer 31 may have a single color or a combination of multiple colors. The colored layer 31 is formed, for example, by a uniform monochromatic ink or a metal thin film. The pattern layer 32 forms a design in combination with the colored layer 31. The pattern layer 32 forms a pattern such as tree rings or vessel grooves on the surface of a wooden board, and forms a wood grain pattern in combination with the colored layer 31. The pattern layer 32 displays a desired color on a part of the laminate 10. The pattern layer 32 exhibits a color different from that of the colored layer 31. The pattern layer 32 exhibits, for example, a color darker than that of the colored layer 31. The pattern layer 32 is formed, for example, by an ink or a metal thin film printed on top of the colored layer 31. The thickness of the colored layer 31 and the design layer 32 may be 0.5 μm or more, 1 μm or more, or 2 μm or more. The thickness of the colored layer 31 and the design layer 32 may be 20 μm or less, 10 μm or less, or 5 μm or less.
[0021] The colored layer 31 and the design layer 32 may be inks obtained by appropriately mixing a coloring agent such as a pigment or a dye with a binder resin. The binder resin may be, for example, a urethane resin, an acrylic polyol resin, an acrylic resin, an ester resin, an amide resin, a butyral resin, a styrene resin, a urethane-acrylic copolymer, a vinyl chloride-vinyl acetate copolymer resin, a vinyl chloride-vinyl acetate-acrylic copolymer resin, a chlorinated propylene resin, a nitrocellulose resin, or a cellulose acetate resin. The coloring agent may be, for example, an inorganic pigment such as carbon black (ink), iron black, titanium white, antimony white, yellow lead, titanium yellow, red oxide, cadmium red, ultramarine blue, or cobalt blue; an organic pigment or dye such as quinacridone red, isoindolinone yellow, nickel azo complex, phthalocyanine blue, or azomethine azo black; a metal pigment made of scaly foil pieces such as aluminum or brass; or a pearlescent (pearl) pigment made of scaly foil pieces such as titanium dioxide-coated mica or basic lead carbonate; or the like. The colored layer 31 and the design layer 32 may be, for example, a thin film of a single metal element such as gold, silver, copper, tin, iron, nickel, chromium, cobalt, etc., or a thin film of an alloy containing two or more of the above metal elements, etc. The alloy may be, for example, brass, bronze, stainless steel, etc.
[0022] The resin layer 50 shown in FIG. 2 protects the design layer 30 and increases the strength of the laminate 10. The resin layer 50 is transparent. The material of the resin layer 50 may be, for example, a polyolefin resin, a polyester resin, a polycarbonate resin, an acrylonitrile-butadiene-styrene resin (ABS resin), an acrylic resin, a vinyl chloride resin, or the like. The thickness of the resin layer 50 may be 20 μm or more, 40 μm or more, or 60 μm or more. The thickness of the resin layer 50 may be 150 μm or less, 120 μm or less, or 100 μm or less.
[0023] In this specification, "transparent" means that the visible light transmittance is 40% or more, 70% or more, 80% or more, or 90% or more. The visible light transmittance is specified as the average value of the total light transmittance at each wavelength when measured at 1 nm intervals within a measurement wavelength range of 380 nm to 780 nm using a spectrophotometer (Shimadzu Corporation's "UV-3600i Plus", JIS K0115 compliant product). The incident angle when measuring the visible light transmittance is set to 0° when the transmission direction is not particularly specified. The incident angle is the angle that the traveling direction of the incident light makes with respect to the normal direction to the incident surface, and is a value less than 90°.
[0024] The surface layer 40 reduces the gloss on the second surface 12 of the laminate 10. The surface layer 40 forms the second surface 12 of the laminate 10. The surface layer 40 forms an uneven shape 13 on the second surface 12. The uneven shape 13 has an irregular wrinkle structure. Light incident on the second surface 12 is diffused by being diffusely reflected by the uneven shape 13 formed by the surface layer 40. The gloss on the second surface 12 of the laminate 10 is reduced.
[0025] The surface layer 40 includes a first layer 41 and a second layer 42. The second layer 42 is provided closer to the second surface 12 than the first surface 11 with respect to the first layer 41. The second layer 42 is provided in a predetermined pattern. The pattern of the second layer 42 corresponds to the design formed by the design layer 30. The second layer 42 allows the surface layer 40 to impart a tactile sensation corresponding to the design displayed by the laminate 10. In the illustrated example, the second layer 42 is provided in a portion of the design layer 30 where the design layer 32 is not provided when observed from the second surface 12. When the design layer 30 forms a design of a wood grain pattern such as annual rings and vessel grooves on the surface of a wooden board, and the design layer 32 forms a pattern such as annual rings and vessel grooves, the second layer 42 forms a recess on the second surface 12 corresponding to the pattern of annual rings and vessel grooves. In the portion displaying the pattern of tree rings or vessel grooves, the second layer 42 can impart a recessed feel to the second surface 12 of the laminate 10. Not limited to the example shown in the figure, the second layer 42 may be provided in the portion where the design layer 32 of the design layer 30 is provided when observed from the second surface 12.
[0026] The first layer 41 includes a binder resin 41a and a plurality of particles 41b. At least a portion of each particle 41b is located inside the binder resin 41a. The binder resin 41a forms a part of the uneven shape 13 having a wrinkled structure on the second surface 12. The first layer 41 reduces the gloss on a part of the second surface 12. The plurality of particles 41b are a wrinkle forming agent that forms a wrinkled structure in the binder resin 41a. The particles 41b control the shape of the wrinkled structure when a wrinkled structure is formed in the binder resin 41a using excimer light or the like.
[0027] The binder resin 41a includes a cured product of a resin composition. The resin composition may include an ionizing radiation curable resin. The ionizing radiation curable resin is a resin having an ionizing radiation curable functional group. The ionizing radiation curable functional group is a group that crosslinks by irradiation with ionizing radiation. The ionizing radiation curable functional group may be, for example, a functional group having an ethylenic double bond, such as a (meth)acryloyl group, a vinyl group, or an allyl group. In this specification, a (meth)acryloyl group refers to an acryloyl group or a methcroyl group. In this specification, a (meth)acrylate refers to an acrylate or a methacrylate. The ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing and / or crosslinking molecules. The ionizing radiation may be electromagnetic waves such as ultraviolet rays (UV), electron beams (EB), X-rays, and gamma rays, or charged particle beams such as alpha rays and ion beams.
[0028] The ionizing radiation curable resin may be an electron beam curable resin or an ultraviolet ray curable resin. The ionizing radiation curable resin may be appropriately selected from polymerizable monomers and polymerizable oligomers that have been conventionally used as ionizing radiation curable resins.
[0029] The polymerizable monomer may be a (meth)acrylate monomer having a radically polymerizable unsaturated group in the molecule. The polymerizable monomer may be a polyfunctional (meth)acrylate monomer. The polyfunctional (meth)acrylate monomer may be a (meth)acrylate monomer having two or more ionizing radiation curable functional groups in the molecule and having at least a (meth)acryloyl group as the functional group. The number of functional groups of the polyfunctional (meth)acrylate monomer may be 2 or more. The number of functional groups of the polyfunctional (meth)acrylate monomer may be 8 or less, or 6 or less. The polyfunctional (meth)acrylate may be used alone or in combination of two or more kinds.
[0030] The polymerizable oligomer may be, for example, a (meth)acrylate oligomer having two or more ionizing radiation curable functional groups in the molecule and having at least a (meth)acryloyl group as the functional group. The polymerizable oligomer may be, for example, a urethane (meth)acrylate oligomer, an epoxy (meth)acrylate oligomer, a polyester (meth)acrylate oligomer, a polyether (meth)acrylate oligomer, a polycarbonate (meth)acrylate oligomer, an acrylic (meth)acrylate oligomer, etc. Other examples of the polymerizable oligomer include highly hydrophobic polybutadiene (meth)acrylate oligomers having (meth)acrylate groups in the side chains of polybutadiene oligomers, silicone (meth)acrylate oligomers having polysiloxane bonds in the main chain, aminoplast resin (meth)acrylate oligomers obtained by modifying aminoplast resins having many reactive groups in a small molecule, and oligomers having cationically polymerizable functional groups in the molecule, such as novolac type epoxy resins, bisphenol type epoxy resins, aliphatic vinyl ethers, and aromatic vinyl ethers.
[0031] The polymerizable oligomer may be used alone or in combination of two or more kinds. The polymerizable oligomer may be a urethane (meth)acrylate oligomer, an epoxy (meth)acrylate oligomer, a polyester (meth)acrylate oligomer, a polyether (meth)acrylate oligomer, a polycarbonate (meth)acrylate oligomer, or an acrylic (meth)acrylate oligomer.
[0032] The number of functional groups of the polymerizable oligomer may be 2 or more. The number of functional groups of the polymerizable oligomer may be 8 or less, or 6 or less. The weight average molecular weight of the polymerizable oligomer may be 2500 or more, 3000 or more, or 3500 or more. The weight average molecular weight of the polymerizable oligomer may be 7500 or less, 7000 or less, or 6000 or less. The weight average molecular weight is an average molecular weight measured by GPC analysis and converted into standard polystyrene.
[0033] In the present embodiment, the binder resin 41a may be a combination of a polymerizable oligomer and a polymerizable monomer. The polymerizable oligomer may be a multifunctional urethane (meth)acrylate oligomer. The polymerizable monomer may be a multifunctional polymerizable monomer. The polymerizable monomer may be a multifunctional (meth)acrylate monomer. The mixing ratio of the polymerizable oligomer and the polymerizable monomer can be appropriately adjusted according to required characteristics.
[0034] In addition to the above-mentioned resins, the resin composition may contain other components depending on the desired performance, etc. For example, the resin composition may contain a monofunctional (meth)acrylate for the purpose of reducing the viscosity, etc. The monofunctional (meth)acrylate may be used alone or in combination of two or more kinds.
[0035] When the resin is an ultraviolet-curable resin that is cured by ultraviolet light, it may contain additives such as a photopolymerization initiator and a photopolymerization accelerator. The photopolymerization initiator may be, for example, one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc. The photopolymerization accelerator reduces polymerization inhibition caused by air during curing and increases the curing speed. The photopolymerization accelerator may be, for example, one or more selected from p-dimethylaminobenzoic acid isoamyl ester, p-dimethylaminobenzoic acid ethyl ester, etc.
[0036] The particles 41b may be, for example, organic particles or inorganic particles. The organic matter constituting the organic particles may be polymethyl methacrylate, acrylic-styrene copolymer resin, melamine resin, polycarbonate, polystyrene, polyvinyl chloride resin, benzoguanamine-melamine-formaldehyde condensate, silicone, fluorine-based resin, polyester-based resin, etc. The inorganic matter constituting the inorganic particles may be silica, alumina, calcium carbonate, aluminosilicate, barium sulfate, etc. The shape of the particles 41b may be, for example, spherical, polyhedral, scaly, amorphous, etc.
[0037] The average particle diameter of the particles 41b may be 1 μm or more, 1.3 μm or more, 1.5 μm or more, or 1.8 μm or more. The average particle diameter of the particles 41b may be 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The average particle diameter of the particles 41b may be equal to or less than the thickness of the binder resin 41a.
[0038] In this specification, the average particle diameter of the particles is the average particle diameter (arithmetic mean diameter) measured for 100 randomly selected non-aggregated particles when the cross section of the laminate 10 in the thickness direction is observed with a scanning electron microscope (SEM) under conditions of an acceleration voltage of 3.0 kV and a magnification of 50,000 times. The particle diameter is the value measured by measuring the distance between two parallel lines that is the maximum distance between the two lines when the cross section of the particle is sandwiched between the two lines.
[0039] The content of the particles 41b may be 0.5 parts by mass or more, 0.75 parts by mass or more, 1 part by mass or more, or 1.2 parts by mass or more, relative to 100 parts by mass of the resin forming the binder resin 41a. The content of the particles 41b may be 25 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, 7.5 parts by mass or less, or 6 parts by mass or less, relative to 100 parts by mass of the resin forming the binder resin 41a.
[0040] The thickness of the first layer 41 may be 1 μm or more, 2 μm or more, 3 μm or more, or 4 μm or more. The thickness of the first layer 41 may be 20 μm or less, 15 μm or less, or 10 μm or less. The thickness of the first layer 41 means the thickness of the first layer 41 excluding the particles 41b. The thickness of the first layer 41 is the thickness of the binder resin 41a.
[0041] In this specification, the thickness of each member of the laminate 10 is determined by measuring the thickness of the member at 20 points on an image taken with a scanning electron microscope (SEM) of a cross section of the laminate 10, and taking the arithmetic mean of the thickness values at 20 points. The accelerating voltage of the SEM is set to 3 kV, and the magnification is set according to the thickness.
[0042] The second layer 42 forms another part of the uneven shape 13 having a wrinkled structure on the second surface 12. The second layer 42 reduces the gloss on another part of the second surface 12. The uneven shape 13 formed by the second layer 42 is different from the uneven shape 13 formed by the first layer 41. The gloss reduced by the second layer 42 on the second surface 12 is different from the gloss reduced by the first layer 41 on the second surface 12. Since the second layer 42 is provided in a pattern corresponding to the pattern of the design layer 32 of the design layer 30, it is possible to reduce the gloss on the second surface 12 in accordance with the design displayed by the laminate 10, and it is possible to impart a tactile feel to the second surface 12 in accordance with the design displayed by the laminate 10.
[0043] The second layer 42 may contain a binder resin and a plurality of particles, similarly to the first layer 41. The binder resin may form another part of the uneven shape 13 having a wrinkled structure on the second surface 12. The material of the binder resin and the material of the particles may be the same as the material of the binder resin 41a of the first layer 41 and the material of the particles described above.
[0044] The second layer 42 may have a different configuration from the first layer 41. The second layer 42 includes a binder resin and a plurality of particles, but the binder resin does not have to form an uneven shape having a wrinkled structure. In the second layer 42, the plurality of particles may protrude from the binder resin to form another part of the uneven shape 13. The material of the binder resin and the material of the particles may be the same as the material of the binder resin 41a of the first layer 41 and the material of the particles described above.
[0045] When the binder resin forms another part of the uneven shape 13 having a wrinkled structure on the second surface 12, the content of particles relative to 100 parts by mass of the resin forming the binder resin in the second layer 42 is less than the content of particles 41b relative to 100 parts by mass of the resin forming the binder resin 41a in the first layer 41. When the binder resin forms another part of the uneven shape 13 having a wrinkled structure on the second surface 12, the content of particles relative to 100 parts by mass of the resin forming the binder resin in the second layer 42 may be 0.05 parts by mass or more, 0.25 parts by mass or more, or 0.5 parts by mass or more. The content of particles relative to 100 parts by mass of the resin forming the binder resin in the second layer 42 may be 24 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, 7.5 parts by mass or less, or 6 parts by mass or less.
[0046] In particular, when the particles form another part of the uneven shape 13 of the second surface 12, the thickness of the second layer 42 may be 0.1 μm or more, or 0.5 μm or more. The thickness of the second layer 42 may be 5 μm or less, or 3 μm or less. The thickness of the second layer 42 is the thickness of the binder resin.
[0047] Fig. 3 shows a top view of the second surface 12 on which the wrinkled uneven shape 13 is formed. As shown in Fig. 3, the wrinkled uneven shape 13 is formed by a plurality of linear protrusions 14 extending linearly and recesses 15 between the linear protrusions 14. The linear protrusions 14 and the recesses 15 have irregular shapes in a plan view and are irregularly arranged.
[0048] The linear convex portions 14 and the concave portions 15 in the concave-convex shape 13 having a wrinkled structure may be distinguished from each other, for example, by using the brightness difference of the image of the second surface 12 of the laminate 10. For example, the darkest part in the concentration distribution image of the second surface 12 of the laminate 10 is set to gradation 255, and the lightest part in the concentration distribution image is set to gradation 0, and the concentration of the concentration distribution image is divided into gradations 0 to 255. Gradations 0 to 127 may be distinguished as the concave portions 15, and gradations 128 to 255 as the linear convex portions 14, by performing a binarization process. The threshold value of the gradation for distinguishing the linear convex portions 14 and the concave portions 15 may be set to any value.
[0049] In the entire second surface 12, the ratio of the portion close to the maximum height of the uneven shape 13 is small. More specifically, the ratio of the total surface area of the portion having a height of 2.5 μm or less from the maximum height of the second surface 12 to the surface area of the second surface 12 is 10% or less, preferably 8% or less, and more preferably 5% or less. FIG. 4 shows an enlarged view of the vicinity of the second surface 12 in the cross-sectional view of the laminate 10 shown in FIG. 1 and FIG. 2. The dashed line shown in FIG. 4 indicates 2.5 μm from the maximum height of the second surface 12. The total surface area of the second surface 12 above the dashed line on the paper is the total surface area of the portion having a height of 2.5 μm or less from the maximum height of the second surface 12. The surface area of the second surface 12 is the area along the uneven shape 13.
[0050] The maximum height Rz of the second surface 12 as defined in JIS B0601:2013 may be 12.5 μm or less, or may be 6 μm or less.
[0051] The ratio of the total surface area of the portion having a height of 2.5 μm or less from the maximum height of the second surface 12 to the surface area of the second surface 12 and the maximum height Rz of the second surface 12 are calculated from the shape of the second surface 12 measured using a shape analysis laser microscope (Keyence Corporation, VK-X150 (control unit) / VK-X160 (measurement unit)). The size of the measured second surface 12 is 271 × 204 μm in plan view. 2The resolution for measuring the second surface 12 is 1024 x 768 pics. The ratio of the total surface area of the portions having a height of 2.5 μm or less from the maximum height of the second surface 12 to the surface area of the second surface 12 is the arithmetic mean of values calculated at any 10 points on the second surface 12. The maximum height Rz of the second surface 12 is the arithmetic mean of the values of the maximum height Rz measured at any 20 points on the second surface 12.
[0052] The 60° specular gloss of the second surface 12 as defined in JIS Z8741:1997 may be 10.0 or less, or may be 5 or less.
[0053] The specular gloss is measured in accordance with JIS Z8741:1997 using micro-TRI-gloss Cat. No. 4563 manufactured by BYK-Gardner. The 60° specular gloss is measured at an incident angle of 60° in accordance with Method 3 in JIS Z8741:1997. The specular gloss of the second surface 12 is measured in a square area of 1 cm on each side of the second surface 12 of the laminate 10. The specular gloss of the second surface 12 is measured in 10 square areas, and the average of the 10 areas is determined as the average of the specular gloss. The 10 areas at which the specular gloss is measured are randomly selected. The average of these is determined as the specular gloss of the second surface 12.
[0054] As an example of a method for manufacturing the laminate 10 of the present embodiment, a method for manufacturing the laminate 10 shown in Fig. 1 will be described. The method for manufacturing the laminate 10 includes a step of providing a design layer 30 on the base material 20, a step of providing a first layer 41 of the surface layer 40 on the design layer 30, and a step of providing a second layer 42 on a part of the first layer 41.
[0055] The process of providing the design layer 30 on the substrate 20 will be described. A colored layer 31 is provided on the substrate 20 by printing. A design layer 32 is provided on a portion of the colored layer 31 by printing. The design layer 32 is provided in a predetermined pattern so as to form a design to be displayed on the second surface 12 of the laminate 10. The colored layer 31 and the design layer 32 are provided by any printing method such as offset printing, inkjet printing, gravure printing, screen printing, etc. The printing method may be appropriately selected depending on the colorants contained in the colored layer 31 and the design layer 32, etc.
[0056] The process of providing the first layer 41 of the surface layer 40 on the design layer 30 will be described. A mixture of particles 41b and a resin composition that will become the binder resin 41a of the first layer 41 is placed on the design layer 30. The mixture may be placed by applying it to the design layer 30 by, for example, gravure printing, bar coating, roll coating, reverse roll coating, comma coating, or the like. The mixture may be placed by being formed into a sheet and attached to the design layer 30.
[0057] The resin composition is irradiated with light having a wavelength of more than 380 nm, preferably light having a wavelength of 385 nm or more and 400 nm or less, to pre-cure the entire resin composition. The pre-cure step may be omitted.
[0058] The surface of the resin composition is irradiated with light having a wavelength of 100 nm or more and 380 nm or less. A wrinkled structure is formed on the surface of the resin composition. The mechanism by which this wrinkled structure is formed is presumed to be as follows. When the surface of the resin composition is irradiated with light having a wavelength of 100 nm or more and 380 nm or less, the wavelength of the irradiated light is short, so that the energy of the light penetrates only the surface portion and does not reach the inside. Only the surface portion of the resin composition begins to harden. Only the surface undergoes hardening shrinkage, and the wrinkled structure is formed on the surface of the resin composition. It is considered that this occurs when only a portion of the resin composition within a certain thickness range from the surface is in a hardened state. It is considered that the particles 41b function like a nucleus that triggers the formation of the wrinkled structure. It is presumed that the resin on the surface portion of the resin composition gathers around the particles 41b, forming an uneven shape having a wrinkled structure. However, the present disclosure is not limited to this presumption.
[0059] As the light having a wavelength of 100 nm or more and 380 nm or less, for example, rare gases such as Ar, Kr, Xe, Ne, halogenated rare gases such as F, Cl, I, Br, or the like, or a dimer in an excited state formed by discharging a mixed gas of these gases, that is, "excimer light" including light in the ultraviolet wavelength region from an excimer may be used. The wavelength of the excimer light and the excimer serving as the light source may be, for example, light having a wavelength of 126 nm radiated from an excimer of Ar2 (hereinafter abbreviated as "126 nm (Ar2)"), 146 nm (Kr2), 157 nm (F2), 172 nm (Xe2), 193 nm (ArF), 222 nm (KrCl), 247 nm (KrF), 308 nm (XeCl), 351 nm (XeF), etc. The excimer light may be either spontaneous emission light or laser light with high coherence due to stimulated emission. Discharge lamps that emit excimer light are also called "excimer lamps." Excimer light has a single wavelength peak and a narrower half-width wavelength than normal ultraviolet light (e.g., ultraviolet light emitted from metal halide lamps, mercury lamps, etc.). By using such excimer light, a wrinkle structure can be stably formed in the resin composition.
[0060] The wavelength of the light irradiated to the surface of the resin composition may be 120 nm or more, 140 nm or more, 150 nm or more, or 155 nm or more. The wavelength of the light irradiated to the surface of the resin composition may be 320 nm or less, 300 nm or less, 250 nm or less, 200 nm or less, or 172 nm (Xe2).
[0061] When the light irradiated onto the surface of the resin composition has a wavelength of 172 nm, the integrated light quantity of the light is 0.1 mJ / cm 2 It may be 0.5 mJ / cm or more. 2 It may be more than 1 mJ / cm 2 The integrated light amount of the light irradiated onto the surface of the resin composition may be 300 mJ / cm or more. 2 It may be less than 100 mJ / cm 2 It may be less than 50 mJ / cm 2 When the light irradiated onto the surface of the resin composition has a wavelength of 172 nm, the power density of the light may be 0.001 W / cm or more, 0.01 W / cm or more, or 0.02 W / cm or more. The power density of the light irradiated onto the surface of the resin composition may be 1 W / cm or less, 0.5 W / cm or less, or 0.1 W / cm or less.
[0062] The oxygen concentration when the surface of the resin composition is irradiated with light may be 1000 ppm or less, 750 ppm or less, 500 ppm or less, or 300 ppm or less.
[0063] After irradiating the surface of the resin composition with light having a wavelength of 100 nm or more and 380 nm or less, the resin composition is irradiated with light having a wavelength longer than the wavelength of the light. Curing proceeds inside the resin composition, and the entire resin composition is cured. Due to the difference between the degree of curing proceeding on the surface of the resin composition and the degree of curing proceeding inside the resin composition, the formation of a wrinkle structure proceeds further. For example, ultraviolet light (UV) may be used as the light used when curing the entire resin composition. When curing the entire resin composition, other ionizing radiation, for example, an electron beam (EB), may be used instead of ultraviolet light.
[0064] A process of providing the second layer 42 on a part of the first layer 41 will be described. A mixture of particles and a composition that serves as a binder resin is arranged in a pattern corresponding to the pattern of the design layer 32 of the design layer 30. The mixture may be arranged by being applied to the first layer 41 by, for example, gravure printing, bar coating, roll coating, reverse roll coating, comma coating, or the like. The mixture may be arranged by being affixed to the first layer 41 in a sheet-like state.
[0065] The second layer 42, in which the binder resin forms part of the uneven shape 13 having a wrinkle structure on the second surface 12, is provided by the same process as the above-mentioned first layer 41. That is, the surface of the resin composition is irradiated with light having a wavelength of 100 nm or more and 380 nm or less, and then the resin composition is irradiated with light having a wavelength longer than the wavelength of the light or other ionizing radiation, thereby curing the entire resin composition.
[0066] The second layer 42, in which the particles form another part of the unevenness 13 on the second surface 12, is provided by irradiating the resin composition with ultraviolet light or other ionizing radiation to cure the resin composition.
[0067] In order to improve adhesion, a surface treatment such as a corona discharge surface treatment may be performed when each layer is provided.
[0068] When the second surface of the laminate is touched with a finger, the uneven surface increases the contact area between the second surface and the finger, so the finger's oils are likely to adhere to the second surface as fingerprints. Fingerprints are observed as stains. Fingerprints can ruin the design displayed on the second surface and can also reduce the gloss of the second surface.
[0069] In the laminate 10 of this embodiment, the second surface 12 is provided with an uneven shape 13. The uneven shape 13 can suppress the gloss on the second surface 12. The ratio of the total surface area of the portion having a height of 2.5 μm or less from the maximum height of the second surface 12 to the surface area of the second surface 12 is 10% or less. The ratio of the portion close to the maximum height of the uneven shape 13 to the entire second surface 12 is sufficiently small. When the second surface 12 of the laminate 10 is touched with a finger, sebum adheres to the portion close to the maximum height on the second surface 12. Since the ratio of the portion close to the maximum height on the second surface 12 is small, even if the second surface 12 of the laminate 10 is touched with a finger, the contact area between the second surface 12 and the finger is small, and sebum is unlikely to adhere. The uneven shape 13 on the second surface 12 of the laminate 10 can suppress the gloss while making it difficult for fingerprints to adhere to the second surface 12 of the laminate 10.
[0070] The maximum height roughness Rz of the second surface 12 as defined in JIS B0601:2013 is 12.5 μm or less. Because the maximum height roughness Rz is not too large, even if dirt such as sebum gets into the recesses 15 of the uneven shape 13 of the second surface 12, the dirt can be easily removed by wiping the second surface 12. Fingerprints can be easily removed from the second surface 12 of the laminate 10.
[0071] The uneven shape 13 has an irregular wrinkle structure. The uneven shape 13 is composed of linear convex portions 14 and concave portions 15 between the linear convex portions 14. Such an uneven shape 13 is formed by providing at least the first layer 41 using excimer light. By forming the uneven shape 13 using excimer light, it is possible to realize a structure that achieves the above-mentioned effects. Since at least the first layer 41 contains fewer particles 41b than the surface layer of a conventional laminate, the possibility that the particles are dragged on the second surface 12 and the second surface 12 is scratched is reduced. It is possible to suppress deterioration of the gloss of the second surface 12 due to scratches on the second surface 12.
[0072] The thickness of the first layer 41 is 1 μm or more and 20 μm or less. When the first layer 41 is sufficiently thick, the first layer 41 can form an appropriate uneven shape 13 on the second surface 12 of the laminate 10. The appropriate uneven shape 13 can suppress the gloss on the second surface 12 of the laminate 10. When the first layer 41 is not too thick, the laminate 10 can be prevented from becoming too thick.
[0073] The thickness of the second layer 42 is 0.1 μm or more and 5 μm or less. Since the second layer 42 is sufficiently thin, the concave and convex shape 13 can be formed in the second layer 42 without filling the concaves of the concave and convex shape formed by the first layer 41. The gloss of the second surface 12 of the laminate 10 can be suppressed also in the portion where the second layer 42 is provided.
[0074] Various modifications can be made to the above-described embodiment.
[0075] In the above-described embodiment, the decorative layer 30 may be omitted from the laminate 10. When the decorative layer 30 is omitted, the pattern in which the second layer 42 of the surface layer 40 is provided is a portion of the second surface 12 that reduces the gloss differently from the gloss reduced by the first layer 41. EXAMPLES
[0076] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples.
[0077] As examples and comparative examples, laminates having a substrate and a surface layer including a first layer and a second layer were produced. The production conditions of the laminates in each of the examples and comparative examples will be described.
[0078] <Example 1> A 60 μm thick substrate made of polypropylene resin that had been subjected to a corona discharge surface treatment was prepared. A first resin composition was applied to the substrate to a thickness of 15 μm, the first resin composition being prepared by adding 30 parts by mass of a multifunctional oligomer having an average number of functional groups of 3, 70 parts by mass of a bifunctional monomer, 3 parts by mass of silica particles having an average particle size of 8 μm, 3 parts by mass of alumina particles having an average particle size of 3 μm, and 0.5 parts by mass of a photopolymerization initiator. The first resin composition was pre-cured by irradiating it with ultraviolet light using a UV-LED light source, and then irradiated with excimer light having a wavelength of 172 nm at 1 W / cm by an excimer lamp. 2 The first resin composition was irradiated with an illuminance of 125 keV to cure the surface of the first resin composition. The first resin composition with the cured surface was irradiated with an electron beam at an acceleration voltage of 125 keV and an exposure dose of 5 Mrad in an environment with an oxygen concentration of 200 ppm or less to cure the entire first resin composition to form a first layer. The first layer was subjected to a corona discharge surface treatment. A second resin composition containing 60 parts by mass of polyfunctional oligomer, 3 parts by mass of silica particles with an average particle size of 8 μm, and 0.5 parts by mass of photopolymerization initiator was applied to the first layer in a natural wood duct-like pattern to a thickness of 2 μm so as to cover 80% of the first layer. The second resin composition was irradiated with an electron beam at an acceleration voltage of 110 keV and an exposure dose of 5 Mrad in an environment with an oxygen concentration of 200 ppm or less to cure the entire second resin composition to form a second layer.
[0079] <Example 2> A first layer was provided on a substrate and a second resin composition was applied to the first layer in the same manner as in Example 1. The second resin composition was pre-cured by irradiating it with ultraviolet light using a UV-LED light source, and then irradiated with excimer light having a wavelength of 172 nm at 1 W / cm2 using an excimer lamp. 2The second resin composition was irradiated with an electron beam at an accelerating voltage of 110 keV and an exposure dose of 5 Mrad in an environment with an oxygen concentration of 200 ppm or less to cure the entire second resin composition, thereby forming a second layer.
[0080] <Example 3> The procedure was the same as in Example 1, except that a third resin composition was used in which 30 parts by mass of a multifunctional oligomer having an average functionality of 3, 40 parts by mass of a bifunctional monomer, and 40 parts by mass of a monofunctional monomer were added to 3 parts by mass of silica particles having an average particle size of 8 μm, 3 parts by mass of alumina particles having an average particle size of 3 μm, and 0.5 parts by mass of a photopolymerization initiator, instead of the second resin composition.
[0081] <Example 4> A fourth resin composition, consisting of 75 parts by mass of a two-liquid acrylic urethane resin mainly composed of an acrylic polyol resin and hexamethylene diisocyanate, and 25 parts by mass of acrylic beads having an average particle size of 20 μm, was applied to the second layer of the laminate of Example 1 in a pattern resembling the ducts of natural wood so as to cover 25% of the second layer, to a thickness of 10 μm. Finally, the laminate was cured at 70° C. for 24 hours to form a raised portion (raised layer) made of the fourth resin composition. The raised portion raises the surface, imparting a tactile feel to the laminate.
[0082] <Example 5> A raised portion (raised layer) was formed on the second layer of the laminate of Example 2 using the fourth resin composition in the same manner as in Example 4.
[0083] <Example 6> The same procedure as in Example 1 was followed, except that the second resin composition was applied so as to cover 90% of the first layer.
[0084] <Example 7> The same procedure as in Example 1 was followed, except that the second resin composition was applied so as to cover 20% of the first layer.
[0085] <Example 8> The same procedure as in Example 1 was carried out except that alumina was not added to the first resin composition.
[0086] <Comparative Example 1> A two-component curing urethane resin was applied to a substrate similar to that of Example 1 to a thickness of 15 μm to form a first layer. An ionizing radiation curing resin was applied to the first layer to a thickness of 2 μm in a pattern resembling the conduit of natural wood so as to cover 80% of the first layer. The ionizing radiation curing resin was irradiated with an electron beam at an acceleration voltage of 110 keV and an exposure dose of 5 Mrad in an environment with an oxygen concentration of 200 ppm or less to cure the ionizing radiation curing resin, thereby forming a second layer.
[0087] <Comparative Example 2> The fourth resin composition was applied to the second layer of the laminate of Comparative Example 1 in the same manner as in Example 4.
[0088] <Comparative Example 3> A first resin composition was applied to a substrate similar to that of Example 1 in the same manner as in Example 1. Without curing the first resin composition, a second resin composition was applied to the first resin composition in the same manner as in Example 1. The first resin composition and the second resin composition were irradiated with an electron beam at an acceleration voltage of 110 keV and an exposure dose of 5 Mrad in an environment with an oxygen concentration of 200 ppm or less, and the first resin composition and the second resin composition were entirely cured to form a first layer and a second layer.
[0089] <Comparative Example 4> The same procedure as in Example 1 was followed, except that the second resin composition was applied so as to cover 100% of the first layer.
[0090] <Comparative Example 5> The procedure was the same as in Example 1, except that a fifth resin composition was used in which 30 parts by mass of a multifunctional oligomer having an average functionality of 3, 40 parts by mass of a bifunctional monomer, and 30 parts by mass of a monofunctional monomer were added to 3 parts by mass of silica particles having an average particle size of 8 μm, 3 parts by mass of alumina particles having an average particle size of 3 μm, and 0.5 parts by mass of a photopolymerization initiator, instead of the second resin composition.
[0091] For each of the laminates produced in the Examples and Comparative Examples, the ratio of the total surface area of the portion having a height within 2.5 μm from the maximum height of the second surface to the surface area of the second surface, the 60° specular gloss of the second surface as defined in JIS Z8741:1997, and the weight and removal rate of oleic acid adhered to the second surface were measured. The second surface is the surface of the laminate that forms the surface layer.
[0092] The ratio of the total surface area of the portion having a height within 2.5 μm from the maximum height of the second surface to the surface area of the second surface is calculated from the shape of the second surface measured using a shape analysis laser microscope (Keyence Corporation, VK-X150 (control unit) / VK-X160 (measurement unit)). The size of the measured second surface is 271 × 204 μm in plan view. 2 The resolution for measuring the second surface shall be 1024 x 768 pics. The ratio of the total surface area of the portion of the second surface that is 2.5 μm or less from the maximum height to the surface area of the second surface shall be the arithmetic mean of values calculated at any 10 points on the second surface.
[0093] The 60° specular gloss of the second surface as defined in JIS Z8741:1997 is measured at an incident angle of 60° using a micro-TRI-gloss Cat. No. 4563 manufactured by BYK-Gardner in accordance with Method 3 described in JIS Z8741:1997. The specular gloss is measured in a 1 cm square region of the second surface. The specular gloss of the second surface is measured in 10 randomly selected regions, and the average specular gloss is determined as the average value of the 10 regions.
[0094] The removal rate of oleic acid attached to the second surface is measured by the following method. The weight of the laminate used for measurement is measured. Oleic acid is attached to a finger. The finger with oleic acid attached is pressed against the second surface of the laminate 15 times to attach the oleic acid from the finger to the second surface. The weight of the laminate with oleic acid attached is measured. The weight of the oleic acid attached to the laminate is determined from the difference in weight from the laminate before the oleic acid is attached. The oleic acid attached to the second surface of the laminate is wiped off 10 times with a rag. The weight of the laminate is measured. The weight of the oleic acid wiped off from the laminate is determined from the difference in weight from the laminate before the oleic acid is wiped off. The ratio of the weight of the oleic acid wiped off from the laminate to the weight of the oleic acid attached to the laminate is taken as the removal rate of oleic acid.
[0095] A black plate was placed facing the first surface of each laminate of the examples and comparative examples, and the laminate was visually observed to see whether the gloss had been sufficiently reduced. Those in which the gloss had been sufficiently reduced were rated as A, and those in which the gloss reduction was insufficient were rated as B.
[0096] After measuring the removal rate of oleic acid for each of the laminates of the Examples and Comparative Examples, the laminates were visually observed to see whether the oleic acid attached to the second surface was noticeable. The laminates were rated as A when almost no oleic acid was observed, as B when oleic acid was not noticeable, as C when oleic acid was noticeable, and as D when oleic acid was significantly noticeable.
[0097] The second surface of each laminate of the Examples and Comparative Examples was rubbed five times with steel wool (Bonstar, #0000) with a weight of 1500 g placed thereon, and the second surface was observed to see if it was scratched. The laminates with almost no scratches were rated A, those with barely noticeable scratches were rated B, and those with noticeable scratches were rated C.
[0098] A line was drawn on the second surface of each laminate of the Examples and Comparative Examples with an oil-based black marker (Teranishi Chemical Industry Co., Ltd.'s marker ink), and then the line was wiped off 10 times with a cloth to check whether the line was noticeable. The laminate was rated as A if the line was barely noticeable, B if the line was barely noticeable, C if the line was noticeable, and D if the line was extremely noticeable.
[0099] The measurement results and evaluation results for the laminates of the respective Examples and Comparative Examples are summarized in Table 1 below.
[0100] [Table 1]
[0101] From a comparison between the Examples and Comparative Examples in Table 1, the following can be understood.
[0102] Even if the ratio of the total surface area of the portions of the second surface having a height within 2.5 μm of the maximum height thereof to the surface area of the second surface is 10% or less, the gloss of the second surface can be appropriately reduced.
[0103] By setting the ratio of the total surface area of the portions having a height within 2.5 μm of the maximum height of the second surface to the surface area of the second surface to 10% or less, the weight of oleic acid adhering to the second surface can be reduced. It is believed that sebum is less likely to adhere to the second surface as fingerprints. By setting the ratio of the total surface area of the portions having a height within 2.5 μm of the maximum height of the second surface to the surface area of the second surface to 10% or less, the removal rate of oleic acid adhering to the second surface is increased. It is believed that even if sebum adheres to the second surface as fingerprints, it can be easily removed. Similarly, by setting the ratio of the total surface area of the portions having a height within 2.5 μm of the maximum height of the second surface to the surface area of the second surface to 10% or less, oil-based marker lines can be easily wiped off on the second surface. This is thought to be because the ratio of the total surface area of the parts having a height within 2.5 μm of the maximum height of the second surface to the surface area of the second surface is 10% or less, which reduces the contact area of oleic acid and oil-based marker components with the second surface, making it difficult for the oleic acid and oil-based marker components to adhere to the second surface.
[0104] It is believed that the first layer is formed using excimer light, which adequately reduces gloss on the second side while making scratches less noticeable when tested with steel wool. [Explanation of symbols]
[0105] 10 Laminate 11 Page 1 12 Side 2 13 Uneven shape 14 Linear convex part 15 Recess 20 Base material 30 Design Layer 31 Colored layer 32 Picture layer 40 Surface layer 41 1st layer 42 2nd layer 50 Resin layer
Claims
1. A laminate having a first surface and a second surface opposite the first surface, A substrate and a surface layer are provided in this order from the first surface to the second surface, the surface layer includes a first layer and a second layer provided closer to the second surface than to the first surface with respect to the first layer, the second layer is provided in a predetermined pattern; The second surface has an uneven shape formed thereon, A laminate, wherein the ratio of the total surface area of portions of the second surface having a height within 2.5 μm of the maximum height thereof to the surface area of the second surface is 10% or less.
2. The laminate according to claim 1 , wherein the second surface has a maximum height roughness Rz defined in JIS B0601:2013 of 12.5 μm or less.
3. The laminate according to claim 1 , wherein the uneven shape has an irregular wrinkle structure.
4. The laminate according to claim 1 , wherein the uneven shape is formed by linear convex portions and concave portions between the linear convex portions.
5. The laminate according to claim 1 , wherein the first layer has a thickness of 1 μm or more and 20 μm or less.
6. The laminate according to claim 1 , wherein the second layer has a thickness of 0.1 μm or more and 5 μm or less.
7. 2. The laminate according to claim 1, wherein the second surface has a 60° specular gloss, as defined in JIS Z8741:1997, of 10.0 or less.
8. A design layer is disposed between the substrate and the surface layer, The design layer includes a colored layer and a pattern layer provided closer to the second surface than the first surface with respect to the colored layer, 2. The laminate of claim 1, wherein the design layer is provided in a pattern corresponding to the pattern of the second layer.
Citation Information
Patent Citations
Decorative sheet and decorative laminate
JP2017165030A