Method for manufacturing laminate

The method of forming oxide films and using hydrogen bonding for chip bonding addresses positioning and residue issues, enhancing manufacturing efficiency by facilitating easy detachment and reducing cleaning time.

JP2024165397APending Publication Date: 2024-11-28DISCO CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023081568
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The use of organic adhesives in chip bonding processes leads to positioning issues, adhesive residue, and prolonged manufacturing times due to cleaning requirements, especially in Co-D2W technology.

Method used

A method involving the formation of an oxide film on the surfaces of chips and temporary support substrates, followed by hydrophilic treatment and hydrogen bonding, allowing temporary bonding without adhesives, and subsequent vaporization of water to create separation points, facilitating easy detachment.

Benefits of technology

Enables precise chip positioning, reduces adhesive residue, and significantly shortens manufacturing time by eliminating the need for adhesive cleaning and simplifying the separation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165397000001_ABST
    Figure 2024165397000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a laminate, which includes temporarily bonding a tabular product and a temporary support substrate such as a carrier wafer without using an organic adhesive, and bonding the tabular product and a support substrate, so that the temporary support substrate can be easily separated from the tabular product after the bonding.SOLUTION: A method for manufacturing a laminate, including: a film-forming step of forming an oxide film on each of one surface of the tabular product and a surface to be temporarily bonded of the temporary support substrate, in a state in which a temperature of an atmosphere is maintained in a first temperature range; a hydrophilization step of subjecting an exposed surface of the oxide film to hydrophilization treatment; a temporary bonding step of temporarily bonding the tabular product and the temporary support substrate via the oxide film; a bonding-material forming step of forming a bonding material on a surface to be bonded of a support substrate; a bonding step of bonding the tabular product and the support substrate to each other via the bonding material; a vaporization step of vaporizing water included in the oxide film by maintaining a temperature of the atmosphere in a second temperature range higher than the first temperature range; and a separation step of separating the tabular product and the temporary support substrate.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminate comprising a plate-like object having one surface and another surface located on the reverse side of the one surface. [Background technology]

[0002] Three-dimensional packaging technologies such as CoC (Chip on Chip), CoW (Chip on Wafer), and WoW (Wafer on Wafer) are being developed for the purpose of achieving high integration of semiconductor device packages. For example, in CoW, a semiconductor device package is manufactured by bonding multiple chips to a wafer that serves as a supporting substrate, and then dividing the supporting substrate along the boundaries of the multiple chips (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-134231 A Summary of the Invention [Problem to be solved by the invention]

[0004] When multiple chips are bonded to a support substrate one by one, the time required is long. In light of this, a technology called Co-D2W (Collective Die to Wafer Bonding) has been proposed. Specifically, in Co-D2W, multiple chips are temporarily bonded to a wafer (temporary support substrate) separate from the wafer that will become the support substrate, and then bonded to the support substrate all at once. Once the multiple chips are bonded to the support substrate, the temporary support substrate is separated from the multiple chips.

[0005] The temporary bonding between the multiple chips and the temporary support substrate in Co-D2W is performed, for example, by using a relatively thick organic adhesive, for example, about 30 μm thick. Specifically, this temporary bonding is performed by placing each of the multiple chips at a desired position on the temporary support substrate via the organic adhesive and then curing the organic adhesive.

[0006] However, the organic adhesive shrinks as it hardens, so that each of the chips may be temporarily bonded to the temporary support substrate in a state shifted from the desired position on the temporary support substrate, which may make it difficult to bond each of the chips to the desired position on the support substrate.

[0007] Furthermore, when the chips are temporarily bonded to the temporary support substrate using a relatively thick organic adhesive, the heights of the chips temporarily bonded to the temporary support substrate may vary. In such a case, it is necessary to press the chips against each other strongly in order to bond them to the support substrate. As a result, each of the chips may move further during bonding, making it difficult to bond each chip to the support substrate at a desired position.

[0008] Furthermore, the organic adhesive has a strong adhesive force, and it is not necessarily easy to separate the chips from the temporary support substrate. Furthermore, at least a part of the organic adhesive remains on the chips after the temporary support substrate is separated from each of the chips. The remaining organic adhesive may become a contamination that deteriorates the performance of the semiconductor device.

[0009] Therefore, after the temporary support substrate is separated from the chips, the chips are generally washed to remove the organic adhesive. However, this washing process tends to take a long time. As a result, the time required to manufacture a laminate including a plate-like object such as a chip and a support substrate to which the plate-like object is bonded tends to be long.

[0010] In view of these points, the object of the present invention is to provide a method for manufacturing a laminate that temporarily bonds a plate-like object and a temporary support substrate without using an organic adhesive, and that enables the temporary support substrate to be easily separated from the plate-like object after the plate-like object and the support substrate are bonded. [Means for solving the problem]

[0011] According to the present invention, there is provided a method for producing a laminate including a plate-shaped object having one surface and another surface located on the reverse side of the one surface, the method including a film-forming step of forming an oxide film on at least one of the one surface of the plate-shaped object or a temporary bonding surface of a temporary support substrate while an ambient temperature is maintained within a first temperature range, a hydrophilization step of performing a hydrophilization treatment on the exposed surface of the oxide film after the film-forming step, a temporary bonding step of temporarily bonding the plate-shaped object and the temporary support substrate via the oxide film by bringing the one surface of the plate-shaped object and the temporary bonding surface of the temporary support substrate close to each other while the oxide film is interposed between the two surfaces, and a method for manufacturing a laminate including the plate-shaped object and the temporary support substrate. a bonding step, after the temporary bonding step and the bonding material forming step, of bonding the other surface of the plate-like object and the bonding surface of the support substrate via the bonding material by bringing the other surface of the plate-like object and the bonding surface of the support substrate close together while the two surfaces face each other via the bonding material; a vaporization step, after the bonding step, of vaporizing water contained in the oxide film by maintaining the temperature of the atmosphere in a second temperature range higher than the first temperature range; and a separation step, after the vaporization step, of separating the plate-like object and the temporary support substrate.

[0012] Preferably, the first temperature range is 80°C or more and 300°C or less. Also, preferably, the second temperature range is 200°C or more and 350°C or less. Furthermore, it is preferable that the manufacturing method of this laminate further comprises, after the film forming step and before the hydrophilization step, a preliminary vaporization step of vaporizing a part of the water contained in the oxide film by maintaining the temperature of the atmosphere in a third temperature range higher than the first temperature range and lower than the second temperature range. In addition, the thickness of the oxide film is preferably 1 μm or less. Effect of the Invention

[0013] In the present invention, the plate-like object and the temporary support substrate are temporarily bonded by utilizing the oxide film whose exposed surface is hydrophilized, that is, in the present invention, the plate-like object and the temporary support substrate are temporarily bonded by utilizing hydrogen bonds generated on the exposed surface of the oxide film without using an organic adhesive.

[0014] In addition, in the present invention, after the bonding of the plate-like object and the support substrate is completed, the temperature of the atmosphere is maintained at a temperature higher than the temperature of the atmosphere when the oxide film is formed, thereby vaporizing the water contained in the oxide film. This forms a large number of voids in the oxide film that act as separation starting points when the temporary support substrate is separated from the plate-like object. As a result, in the present invention, it becomes easy to separate the temporary support substrate from the plate-like object. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1(A) is a perspective view that shows a schematic example of a wafer, and FIG. 1(B) is a perspective view that shows a schematic example of a chip manufactured from the wafer shown in FIG. 1(A). [Diagram 2] FIG. 2 is a flow chart that illustrates an example of a method for manufacturing a stack including a chip. [Diagram 3] Figure 3(A) is a cross-sectional view showing typically multiple chips each having an oxide film formed on one surface thereof, and Figure 3(B) is a cross-sectional view showing typically a temporary support substrate having an oxide film formed on its temporary bonding surface. [Figure 4] Figure 4(A) is a cross-sectional view that shows a schematic diagram of a hydrophilic treatment being performed on an oxide film formed on one side of a chip, and Figure 4(B) is a cross-sectional view that shows a schematic diagram of a hydrophilic treatment being performed on an oxide film formed on a temporary bonding surface of a temporary support substrate. [Diagram 5] FIG. 5(A) is a cross-sectional view that shows a schematic diagram of a state in which a chip and a temporary supporting substrate are temporarily bonded together, and FIG. 5(B) is a cross-sectional view that shows a schematic diagram of the temporarily bonded chip and temporary supporting substrate. [Figure 6] FIG. 6 is a cross-sectional view that typically illustrates a support substrate having a bonding material formed on its bonding surface. [Figure 7] FIG. 7(A) is a cross-sectional view that shows a schematic diagram of a state in which a chip and a supporting substrate are bonded together, and FIG. 7(B) is a cross-sectional view that shows a schematic diagram of the bonded chip and supporting substrate. [Figure 8] FIG. 8 is a cross-sectional view that illustrates a stack including a plurality of chips, a temporary supporting substrate, and a supporting substrate after the water contained in the oxide film has evaporated. [Figure 9] FIG. 9 is a cross-sectional view that illustrates a state in which the temporary support substrate is separated from the chip. [Figure 10] FIG. 10 is a flow chart that illustrates an example of a method for producing a laminate, which is different from the method for producing a laminate shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An embodiment of the present invention will be described with reference to the accompanying drawings. Fig. 1(A) is a perspective view showing an example of a wafer, and Fig. 1(B) is a perspective view showing an example of a chip manufactured from the wafer shown in Fig. 1(A). The wafer 11 shown in Fig. 1(A) includes, for example, a front surface 11a and a back surface 11b that are substantially parallel to each other, and is made of a semiconductor material such as single crystal silicon.

[0017] The wafer 11 has a notch 11c formed on its outer edge to indicate a specific crystal orientation of the semiconductor material. A plurality of devices 13 are formed on the front surface 11a of the wafer 11. The devices 13 are arranged in a matrix. That is, the boundaries between the devices 13 extend in a lattice pattern. The wafer 11 is divided along the boundaries between the devices 13 to produce a plurality of chips 15.

[0018] 2 is a flow chart showing an example of a method for manufacturing a laminate including a plate-like object (specifically, a chip 15). In this method, first, an oxide film is formed on one surface of the chip 15 (e.g., the surface on which the device 13 is not formed) and a temporary bonding surface, which is the surface of a temporary supporting substrate that is temporarily bonded to the chip 15 (film formation step S1).

[0019] Fig. 3A is a cross-sectional view showing a plurality of chips 15 each having an oxide film formed on one surface thereof. The oxide film 17 shown in Fig. 3A is, for example, a silicon oxide film formed by using PECVD (Plasma Enhanced Chemical Vapor Deposition).

[0020] Such an oxide film 17 is formed, for example, by supplying a gas obtained by vaporizing a liquid raw material such as liquid TEOS (Tetraethyl orthosilicate) into a chamber in which one side of each of the multiple chips 15 is exposed in the internal space, and then converting the gas into plasma.

[0021] Here, the temperature of the atmosphere when the oxide film 17 is formed, i.e., the temperature inside the chamber, is set so as to increase the water content of the formed oxide film 17. For example, this temperature is set so as to be included in a first temperature range of 80°C or more and 300°C or less, preferably 100°C or more and 260°C or less, more preferably 120°C or more and 220°C or less, and most preferably 120°C or more and 180°C or less.

[0022] Moreover, the oxide film 17 has a thin thickness so as to suppress sinking of the chip 15 into the temporary support substrate when the chip 15 and the temporary support substrate are temporarily bonded to each other as described below. For example, the oxide film 17 has a thickness of 1 μm or less, preferably 500 nm or less, more preferably 250 nm or less, and most preferably 125 nm or less.

[0023] Also, in order to planarize the exposed surface of oxide film 17, i.e., the surface farther from device 13, this surface may be subjected to a planarization process such as chemical mechanical polishing (CMP). Furthermore, oxide film 17 may be formed to a thickness of more than 1 μm, and then subjected to a planarization process so that the thickness becomes 1 μm or less and the exposed surface is planarized. In addition, the planarization process may be performed on one surface of chip 15 before oxide film 17 is formed.

[0024] Fig. 3(B) is a cross-sectional view showing a temporary support substrate having an oxide film formed on the temporary bonding surface. The temporary support substrate 19 shown in Fig. 3(B) has the same structure as the wafer 11 shown in Fig. 1(A), except that the multiple devices 13 are not formed.

[0025] Alternatively, the temporary support substrate 19 may be a substrate made of an insulating material such as glass, etc. Also, the temporary support substrate 19 may be a substrate that is thicker and / or has a larger diameter than the wafer 11 shown in FIG.

[0026] 3B is, for example, a silicon oxide film formed in the same manner as the oxide film 17 shown in FIG 3A. Furthermore, a planarization process may be performed on the exposed surface of the oxide film 21 and / or on the temporary bonding surface of the temporary support substrate 19 before the oxide film 21 is formed.

[0027] After the film-forming step S1, the exposed surfaces of the oxide films 17 and 21 are subjected to a hydrophilic treatment (hydrophilic treatment step S2). Fig. 4(A) is a cross-sectional view that shows a schematic diagram of the hydrophilic treatment being performed on the exposed surface of the oxide film 17, and Fig. 4(B) is a cross-sectional view that shows a schematic diagram of the hydrophilic treatment being performed on the exposed surface of the oxide film 21.

[0028] This hydrophilic treatment is a treatment for forming and activating OH groups on the exposed surfaces of the oxide films 17 and 21. For example, the hydrophilic treatment is performed by irradiating the exposed surfaces of the oxide films 17 and 21 with nitrogen plasma or ultraviolet light from the irradiation unit 10 under atmospheric pressure.

[0029] In addition, when carrying out this hydrophilic treatment, it is preferable that the water contained in the oxide films 17 and 21 is not evaporated. Therefore, the temperature of the atmosphere when carrying out the hydrophilic treatment is set to a temperature lower than the temperature of the atmosphere when forming the oxide films 17 and 21, for example, room temperature.

[0030] After the hydrophilization step S2, the chip 15 and the temporary support substrate 19 are temporarily bonded via the oxide films 17 and 21 (temporary bonding step S3). Fig. 5(A) is a cross-sectional view showing the state in which the chip 15 and the temporary support substrate 19 are temporarily bonded, and Fig. 5(B) is a cross-sectional view showing the temporarily bonded chip 15 and temporary support substrate 19.

[0031] In this temporary bonding, first, one surface of each of the multiple chips 15 and the temporary bonding surface of the temporary support substrate 19 are placed opposite each other via the oxide films 17 and 21. Then, while maintaining this state, both surfaces of each of the multiple chips 15 and the temporary support substrate 19 are brought closer together until a load of, for example, about 10 kN is applied to each of the multiple chips 15 and the temporary support substrate 19. As a result, hydrogen bonds are generated between the oxide films 17 and 21, and the multiple chips 15 and the temporary support substrate 19 are temporarily bonded to each other.

[0032] This temporary bonding may be performed under atmospheric pressure or at 10 5The temporary bonding may be performed under a reduced pressure atmosphere of not more than Pa. In order to promote hydrogen bonding between the oxide films 17 and 21, water may be supplied to the exposed surfaces of the oxide films 17 and 21 immediately before the temporary bonding.

[0033] In addition, when performing this temporary bonding, it is preferable that the water contained in the oxide films 17 and 21 is not evaporated. Therefore, the temperature of the atmosphere when performing the temporary bonding is set to a temperature lower than the temperature of the atmosphere when the oxide films 17 and 21 are formed, for example, room temperature.

[0034] After the temporary bonding step S3, a bonding material is formed on the bonding surface of the support substrate, which is the surface to be bonded to the chip 15 (bonding material forming step S4). Fig. 6 is a cross-sectional view showing a schematic view of the support substrate with a bonding material formed on its bonding surface.

[0035] Support substrate 23 shown in Fig. 6 is a wafer made of a semiconductor material such as single crystal silicon and has a shape similar to that of wafer 11 shown in Fig. 1(A). A plurality of devices 25 are formed on the bonding surface side of support substrate 23, each of which is connected to device 13 included in chip 15. Note that the plurality of devices 25 are not essential components and may be omitted.

[0036] 6 is formed, for example, by forming a silicon oxide film in the same manner as the oxide film 17 shown in Fig. 3(A), and then performing a planarization process such as CMP on the exposed surface of the bonding material 27 so as to expose the multiple devices 25. However, in this case, the temperature of the atmosphere when forming the bonding material 27 is set to a temperature at which the water content of the formed silicon oxide film is reduced, for example, above 350°C.

[0037] Alternatively, the bonding material 27 may be an organic adhesive containing BCB (benzocyclobutene) etc. In this case, the bonding material 27 is formed, for example, by applying the bonding material 27 to the bonding surface of the support substrate 23 so that the plurality of devices 25 are exposed while maintaining the temperature of the atmosphere at, for example, room temperature, and then maintaining the temperature of the atmosphere at, for example, about 170° C. so that the organic adhesive is pre-baked (soft baked).

[0038] After the bonding material forming step S4, the chip 15 and the support substrate 23 are bonded via the bonding material 27 (bonding step S5). Fig. 7(A) is a cross-sectional view that shows a schematic diagram of the bonding of the chip 15 and the support substrate 23, and Fig. 7(B) is a cross-sectional view that shows a schematic diagram of the bonded chip 15 and the support substrate 23.

[0039] When the bonding material 27 is made of a silicon oxide film, after the bonding material forming step S4 and before the bonding step S5, it is necessary to perform the above-mentioned hydrophilization treatment on the exposed surface of the bonding material 27. Also, immediately before the bonding step S5, the other surface of each of the multiple chips 15 and / or the bonding surface of the support substrate 23 may be cleaned.

[0040] When bonding chips 15 and support substrate 23, first, the other surface of each of the multiple chips 15 is opposed to the bonding surface of support substrate 23 via bonding material 27. Then, while maintaining this state, both surfaces of each of the multiple chips 15 and support substrate 23 are brought closer together until a load of, for example, about 10 kN is applied to each of the multiple chips 15 and support substrate 23. As a result, the multiple chips 15 and support substrate 23 are bonded together.

[0041] This bonding may be performed under atmospheric pressure or at 10 5 The bonding may be performed under a reduced pressure atmosphere of less than or equal to Pa. When the bonding material 27 is made of a silicon oxide film, water may be supplied to the other surface of each of the chips 15 and / or the exposed surface of the bonding material 27 immediately before the bonding in order to promote hydrogen bonding between the chips 15 and the bonding material 27.

[0042] Furthermore, when the bonding material 27 is made of an organic adhesive, the temperature of the atmosphere when this bonding is performed is set to a temperature that can harden the bonding material 27, for example, about 300° C. Furthermore, when the wiring (for example, copper (Cu) wiring) included in the device 13 and the wiring (for example, copper (Cu) wiring) included in the device 25 are directly connected in the bonding step S5, that is, when hybrid bonding is formed, the temperature of the atmosphere when this bonding is performed may be set to, for example, 250° C. or higher and 350° C. or lower.

[0043] After the bonding step S5, the water contained in the oxide films 17 and 21 is evaporated (evaporation step S6). Fig. 8 is a cross-sectional view showing a schematic diagram of a stack including the multiple chips 15, the temporary support substrate 19, and the support substrate 23 after the water contained in the oxide films 17 and 21 has evaporated.

[0044] In this vaporization step S6, the laminate is heated in a nitrogen atmosphere using, for example, a heat treatment device equipped with an infrared lamp, which forms a large number of voids 29 in the oxide films 17 and 21, which act as separation starting points when the temporary support substrate 19 is separated from the multiple chips 15.

[0045] In order to vaporize the water contained in the oxide films 17 and 21, it is necessary to set the temperature of the atmosphere higher than that during the formation of the oxide films 17 and 21. On the other hand, if the temperature of the atmosphere during heating of the laminate is too high, siloxane bonds stronger than hydrogen bonds may be formed between the oxide films 17 and 21.

[0046] Therefore, the temperature of the atmosphere when heating the laminate is set to be within a second temperature range of 200°C or higher and 350°C or lower, preferably 215°C or higher and 320°C or lower, more preferably 230°C or higher and 290°C or lower, and most preferably 245°C or higher and 260°C or lower.

[0047] Furthermore, when the bonding material 27 is made of an organic adhesive, that is, when the temperature of the atmosphere in the bonding step S5 is set to, for example, about 300°C, the bonding step S5 and the vaporization step S6 may be performed successively without interruption.

[0048] After the vaporization step S6, the chip 15 and the temporary support substrate 19 are separated (separation step S7). Fig. 9 is a cross-sectional view that typically shows how the temporary support substrate 19 is separated from the chip 15.

[0049] In this separation step S7, an external force is applied to the temporary support substrate 19 and / or the support substrate 23 so as to separate the temporary support substrate 19 from the chip 15. As a result, the temporary support substrate 19 is separated from the chip 15, and a stacked body 31 including the chip 15 and the support substrate 23 is manufactured.

[0050] Furthermore, the laminate 31 may be etched so that the oxide film 17 remaining on one surface of the chip 15 is removed after the temporary support substrate 19 is separated from the chip 15. The laminate 31 may also be divided along the boundaries of the multiple chips 15 to be individualized.

[0051] 2, the chip 15 and the temporary support substrate 19 are temporarily bonded to each other by utilizing the oxide films 17 and 21 whose exposed surfaces have been made hydrophilic. That is, in this method, the chip 15 and the temporary support substrate 19 are temporarily bonded to each other by utilizing hydrogen bonds generated on the exposed surfaces of the oxide films 17 and 21 without using an organic adhesive.

[0052] In this method, after the bonding of the chips 15 and the support substrate 23 is completed, the temperature of the atmosphere is maintained at a temperature (second temperature range) higher than the temperature of the atmosphere (first temperature range) when the oxide films 17 and 21 are formed, thereby vaporizing the water contained in the oxide films 17 and 21. This forms a large number of voids 29 in the oxide films 17 and 21, which act as separation starting points when the temporary support substrate 19 is separated from the multiple chips 15. As a result, in this method, it becomes easy to separate the temporary support substrate 19 from the chips 15.

[0053] The above is one aspect of the present invention, and the present invention is not limited to the above. For example, in the film-forming step S1, the oxide films 17 and 21 may be formed on only one surface of each chip 15 or the temporary bonding surface of the temporary support substrate 19. That is, in the present invention, either the oxide film 17 or the oxide film 21 may be omitted.

[0054] In addition, in the film-forming step S1, an oxide film 17 may be formed on the surface of each chip 15 on which the device 13 is formed. That is, each chip 15 may be bonded to a temporary support substrate 19 on the side on which the device 13 is formed, and bonded to a support substrate 23 on the side on which the device 13 is not formed. In this case, the multiple devices 25 may not be formed on the bonding surface side of the support substrate 23.

[0055] In addition, in the film-forming step S1, an oxide film 17 may be formed on one surface (e.g., the back surface 11b) of the wafer 11 before it is divided into the plurality of chips 15. In this case, the plurality of chips 15 may be manufactured by dividing the wafer 11 along the boundaries of the plurality of devices 13 after the film-forming step S1 and before the hydrophilization step S2.

[0056] In the present invention, the timing of performing the bonding material forming step S4 is not limited as long as it is performed before the bonding step S5. For example, the bonding material forming step S4 may be performed before the film forming step S1.

[0057] Then, in a bonding material formation step S4 prior to the film formation step S1, a bonding material similar to the bonding material 27 made of the silicon oxide film described above may be formed on the other surface of the plate-like object (specifically, a plurality of chips 15 or a wafer 11 before being divided into a plurality of chips 15).

[0058] That is, in this case, the bonding material may be formed not only on the bonding surface of the support substrate 23 but also on the other surface of the plate-like object. Alternatively, in this case, the bonding material 27 may not be formed on the bonding surface of the support substrate 23, and the bonding material may be formed only on the other surface of the plate-like object.

[0059] Furthermore, the method for manufacturing a laminate of the present invention may include steps other than the steps shown in Fig. 2. Fig. 10 is a flow chart that illustrates an example of a method for manufacturing a laminate different from the method for manufacturing a laminate shown in Fig. 2. Specifically, in the method shown in Fig. 10, after the film-forming step S1 and before the hydrophilization step S2, a part of the water contained in the oxide films 17 and 21 is vaporized (pre-vaporization step S8).

[0060] In this preliminary vaporization step S8, for example, in order to reduce the amount of water contained in the oxide films 17 and 21, a heat treatment device equipped with an infrared lamp is used to heat a plate-like object having an oxide film 17 formed on one surface and / or a temporary support substrate 19 having an oxide film 21 formed on a temporary bonding surface under a nitrogen atmosphere.

[0061] In order to vaporize the water contained in the oxide films 17 and 21, the temperature of the atmosphere needs to be higher than that when the oxide films 17 and 21 are formed. On the other hand, if the temperature of the atmosphere when the laminate is heated is too high, all of the water contained in the oxide films 17 and 21 may be vaporized. Therefore, the temperature of the atmosphere when the plate-like object and / or the temporary support substrate 19 is heated is set to be included in a third temperature range that is higher than the above-mentioned first temperature range and lower than the above-mentioned second temperature range.

[0062] In addition, in the present invention, the plate-like object that is temporarily bonded to the temporary support substrate 19 and then bonded to the support substrate 23 may be the wafer 11. That is, in the present invention, the plurality of chips 15 manufactured from the wafer 11 are not bonded to the support substrate 23, but the wafer 11 itself may be bonded to the support substrate 23. Furthermore, in this case, the plurality of devices 13 do not need to be formed on the wafer 11.

[0063] In addition, the structures and methods according to the above-described embodiments can be modified as appropriate without departing from the scope of the present invention. [Explanation of symbols]

[0064] 10: Irradiation unit 11: wafer (11a: front surface, 11b: back surface, 11c: notch) 13: Device 15: Tip 17: Oxide film 19: Temporary support substrate 21: Oxide film 23: Support substrate 25: Device 27: Bonding material 29: Void 31: Laminate

Claims

1. A method for producing a laminate including a plate-shaped object having one surface and another surface located on the back side of the one surface, comprising: a film forming step of forming an oxide film on at least one of the one surface of the plate-like object or the temporary bonding surface of the temporary support substrate while maintaining the temperature of the atmosphere within a first temperature range; a hydrophilization step of subjecting an exposed surface of the oxide film to a hydrophilic treatment after the film-forming step; a temporary bonding step of temporarily bonding the plate-like object and the temporary bonding surface of the temporary support substrate via the oxide film by bringing the two surfaces of the plate-like object close to each other in a state where the two surfaces face each other via the oxide film after the hydrophilization step; a bonding material forming step of forming a bonding material on at least one of the other surface of the plate-like object or the bonding surface of a support substrate; a bonding step of bonding the plate-like object and the supporting substrate via the bonding material by bringing the other surface of the plate-like object and the bonding surface of the supporting substrate close to each other in a state in which the other surface and the bonding material are opposed to each other via the bonding material, after the temporary bonding step and the bonding material forming step; a vaporization step of vaporizing water contained in the oxide film by maintaining an atmosphere temperature in a second temperature range higher than the first temperature range after the bonding step; a separation step of separating the plate-like object from the temporary support substrate after the vaporization step; A method for manufacturing a laminate comprising the steps of:

2. The method for producing a laminate according to claim 1 , wherein the first temperature range is from 80° C. to 300° C.

3. The method for producing a laminate according to claim 1 , wherein the second temperature range is from 200° C. to 350° C.

4. 2. The method for manufacturing a laminate described in claim 1, further comprising a pre-vaporization step of vaporizing a portion of the water contained in the oxide film by maintaining an atmospheric temperature in a third temperature range that is higher than the first temperature range and lower than the second temperature range after the film-forming step and before the hydrophilization step.

5. 5. The method for producing a laminate according to claim 1, wherein the oxide film has a thickness of 1 [mu]m or less.

Citation Information

Patent Citations

  • Multilayer device manufacturing method and multi layer device

    JP2012134231A