Lithium-ion battery

A lithium ion battery design with a glass filler containing Group 2 elements addresses the resin deterioration issue by preventing hydrogen fluoride attack, ensuring durability and insulation performance even with a non-aqueous fluorine-containing electrolyte.

JP2024165512AActive Publication Date: 2024-11-28PRIME PLANET ENERGY & SOLUTIONS INC +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023081770
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

The deterioration of a filler-containing resin in lithium ion batteries is accelerated when a non-aqueous electrolyte containing fluorine is used, due to the generation of hydrogen fluoride from moisture, which dissolves the glass filler.

Method used

A lithium ion battery design that incorporates a resin member with a glass filler composed mainly of silicon oxide and added Group 2 elements, such as magnesium or calcium, to suppress the dissolution of the glass filler by hydrogen fluoride, maintaining the resin's properties and insulation performance.

Benefits of technology

The resin member's durability and insulation properties are maintained, even when exposed to a non-aqueous electrolyte containing fluorine, by using a glass filler with added Group 2 elements that preferentially react with hydrogen fluoride, preventing the glass from dissolving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165512000001_ABST
    Figure 2024165512000001_ABST
Patent Text Reader

Abstract

To provide a lithium-ion battery in which deterioration of a resin member is not accelerated even though a nonaqueous electrolyte containing fluorine is used.SOLUTION: A battery 1 according to the present disclosed technology is a lithium-ion battery including: a case 2; an electrode body 3 and an electrolyte contained which are inside the case 2; and a resin member 10 that is fixed to the case and has an inner exposed surface 11 which is exposed inside the case 2. The electrolytic solution is a nonaqueous electrolytic solution containing fluorine. The resin member 10 contains a glass filler formed of glass which contains silicon oxide as a main body and added with group 2 elements. A number of atoms ratio of the group 2 elements to silicon in component elements of the glass filler is 0.12% or more and 65% or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The disclosed technology relates to lithium-ion batteries. [Background technology]

[0002] In a lithium ion battery, an electrode body and an electrolyte are housed inside a case. A resin member is fixed to a part of the case of such a battery for the purpose of installing a terminal member or for other purposes. A part of the resin member is an internally exposed surface that is exposed inside the case. A resin member containing a glass filler can be used. For example, the resin containing the filler described in Patent Document 1 can be used. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-035950 A Summary of the Invention [Problem to be solved by the invention]

[0004] In some cases, a non-aqueous electrolyte containing fluorine is used as the electrolyte in this type of battery. In such cases, the filler-containing resin may deteriorate. The deterioration of the filler-containing resin occurs when moisture is mixed into the non-aqueous electrolyte. This is because hydrogen fluoride is generated by the reaction between the fluorine in the non-aqueous electrolyte and the mixed moisture. Hydrogen fluoride dissolves glass, so the glass filler dissolves and is lost.

[0005] An object of the present disclosure is to provide a lithium ion battery in which the deterioration of resin members is not accelerated even when a non-aqueous electrolyte solution containing fluorine is used. [Means for solving the problem]

[0006] A lithium ion battery in one embodiment of the disclosed technology is a battery having a case, an electrode body and an electrolyte contained inside the case, and a resin member that is fixed to the case and has an internal exposed surface exposed inside the case, wherein the electrolyte is a nonaqueous electrolyte containing fluorine, the resin member contains a glass filler formed of glass mainly composed of silicon oxide to which a Group 2 element has been added, and the atomic ratio of the Group 2 element to silicon in the component elements of the glass filler is 0.12% or more and 65% or less.

[0007] In the lithium ion battery according to the above embodiment, the linear expansion coefficient and elastic modulus of the resin member are adjusted by blending the glass filler in the resin member. Therefore, the linear expansion coefficient and elastic modulus of the resin member can be made close to those of the case. On the other hand, when moisture is mixed into the electrolyte, hydrogen fluoride produced by the reaction between fluorine in the electrolyte and water attempts to dissolve the glass filler. However, the Group 2 element added to the glass filler suppresses this dissolution. Therefore, the properties of the resin member are maintained even if moisture is mixed in.

[0008] In the lithium ion battery of the above embodiment, at least a part of the Group 2 element may be magnesium, and the mass ratio of magnesium to silicon in the component elements of the glass filler may be 0.1% to 25%. When magnesium is used as the Group 2 element, the effect of suppressing dissolution of the glass filler by hydrogen fluoride is higher.

[0009] In the lithium ion battery of the above aspect, at least a part of the Group 2 element may be calcium, and the mass ratio of calcium to silicon in the component elements of the glass filler may be 0.17% or more and 81% or less. Even if the Group 2 element is calcium, there is an effect of suppressing dissolution of the glass filler by hydrogen fluoride.

[0010] The lithium ion battery according to any of the above aspects may further include a terminal member connected to the electrode body inside the case, penetrating the case and partially exposed to the outside of the case, and the resin member may insulate the case from the terminal member, so that the insulating and sealing properties of the resin member between the case and the terminal member are maintained for a long period of time. Effect of the Invention

[0011] According to the disclosed technique, a lithium ion battery is provided in which the deterioration of resin members is not accelerated even when a non-aqueous electrolyte solution containing fluorine is used. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a cross-sectional view of a battery according to an embodiment. [Diagram 2] FIG. 2 is a partially enlarged view showing a part of FIG. [Diagram 3] 1 is a graph showing the maximum depth at which corrosion of a glass filler occurs due to immersion in an electrolyte. [Figure 4] 1 is a graph showing a change in elastic modulus of a resin member due to immersion in an electrolyte solution. [Diagram 5] 1 is a graph showing the relationship between the temperature and the penetration depth of fluorine due to immersion in an electrolyte. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] This embodiment embodies the disclosed technology as a battery 1 shown in Figs. 1 and 2. The battery 1 has an electrode body 3 housed in a case 2. The case 2 is an exterior member that defines the appearance of the battery 1. In this embodiment, the case 2 is made of metal (e.g., aluminum). The case 2 is composed of a box body 4 and a lid body 5. The electrode body 3 is made by stacking positive and negative electrode plates.

[0014] The case 2 contains not only the electrode body 3 but also an electrolyte 6. The electrolyte 6 is not only present in a liquid state in the internal space of the case 2, but also permeates the electrode body 3. The battery 1 further includes a terminal member 7. The terminal member 7 is provided so as to penetrate the case 2. The terminal member 7 is partially exposed to the outside of the case 2. The part of the terminal member 7 inside the case 2 is connected to the electrode body 3. The part of the terminal member 7 outside the case 2 is connected to an external terminal 8. The battery 1 has two terminal members 7 for the positive electrode and two external terminals 8 for the negative electrode. The terminal members 7 and the external terminals 8 are made of aluminum or copper.

[0015] The lid body 5 has a through hole 9 formed therein, through which the terminal member 7 passes. The battery 1 further has a resin member 10. The resin member 10 is fixed to the case 2. The position at which the resin member 10 is fixed in the case 2 is between the lid body 5 and the terminal member 7 at the through hole 9. The resin member 10 has two roles: to separate the internal space of the case 2 from the external space, and to insulate the case 2 from the terminal member 7. The resin member 10 has an internal exposed surface 11 exposed to the inside of the case 2.

[0016] The electrolyte 6 in the battery 1 of this embodiment will be described. In this embodiment, a non-aqueous electrolyte containing fluorine is used as the electrolyte 6. Examples of materials that can be used as the solvent and electrolyte in the electrolyte 6 of this embodiment include the following. Solvent: Polar organic solvents such as ethylene carbonate, propylene carbonate, and diethyl carbonate Electrolytes: Fluorine-containing salts such as lithium hexafluorophosphate and lithium tetrafluoroborate

[0017] The resin member 10 in the battery 1 of this embodiment will be described. The resin member 10 of this embodiment is a composite material in which a glass filler is blended with a base resin. The purpose of blending the glass filler is to adjust the linear expansion coefficient and elastic modulus of the resin member 10. Adjusting the linear expansion coefficient means lowering the linear expansion coefficient of the resin member 10. This is to bring it closer to the linear expansion coefficient of metal parts such as the lid body 5 and the terminal member 7. Adjusting the elastic modulus means increasing the elastic modulus of the resin member 10. Both of these contribute to improving the durability of the sealing performance of the resin member 10 in the battery 1.

[0018] The type of resin that can be used as the base resin of the resin member 10 of this embodiment is not particularly limited, but is preferably one that has excellent heat resistance and mechanical strength, such as polyphenylene sulfide resin (hereinafter, PPS resin), polyphenylene oxide resin, modified polyphenylene ether resin, etc.

[0019] The glass filler of the resin member 10 in this embodiment is a minute piece formed of glass. It is in the form of short fibers or particles. The glass used for the glass filler in this embodiment is mainly made of silicon oxide (silicon dioxide, etc.) to which a Group 2 element (particularly magnesium or calcium) has been added. The added Group 2 element is considered to be in an oxidized state in the glass. The glass may also contain small amounts of aluminum to improve productivity, and titanium and iron to improve acid resistance, all in an oxidized state.

[0020] The purpose of adding a Group 2 element to the glass filler in this embodiment is to improve the durability of the resin member 10. As described above, in this embodiment, a fluorine-containing salt is used as the electrolyte of the electrolytic solution 6. Therefore, the electrolytic solution 6 contains fluorine in the form of, for example, hexafluorophosphate ions.

[0021] On the other hand, during the manufacturing process of the battery 1, a certain amount of moisture may get into the inside of the case 2 due to water vapor in the environment. Even during the use of the battery 1, if the sealing of the case 2 is loose, moisture may get into the inside from the outside. For this reason, even if the electrolyte 6 is based on a non-aqueous solvent, it cannot be said that there is absolutely no moisture present.

[0022] When moisture is mixed into the electrolyte 6, fluorine in the electrolyte 6 takes hydrogen from water molecules to generate hydrogen fluoride. The generation of hydrogen fluoride is a factor that inhibits the durability performance originally expected of the resin member 10. This is because glass, which is generally a chemically stable compound, is decomposed into hydrogen fluoride. Therefore, when the hydrogen fluoride generated in the electrolyte 6 comes into contact with the inner exposed surface 11 of the resin member 10, the glass filler in the resin member 10 is attacked by the hydrogen fluoride. As the glass filler is eluted from the resin member 10, the linear expansion coefficient and elastic modulus of the resin member 10 approach the linear expansion coefficient and elastic modulus of the original base resin. In this way, the resin member 10 deteriorates earlier than expected.

[0023] However, in this embodiment, the Group 2 element added to the glass filler prevents the glass from being dissolved by hydrogen fluoride. This is because hydrogen fluoride attacks Group 2 elements preferentially over silicon oxide. In other words, the Group 2 element traps hydrogen fluoride and protects silicon oxide from attack by hydrogen fluoride. The Group 2 element itself becomes a fluoride by trapping hydrogen fluoride. Water is also produced at this time.

[0024] Therefore, the presence of the Group 2 element suppresses the dissolution of glass by hydrogen fluoride. This maintains the durability of the resin member 10 as originally expected. Therefore, in the battery 1 of this embodiment, even if moisture penetrates into the case 2, there is almost no decrease in the durability of the resin member 10. Therefore, in this embodiment, the insulation and sealing between the cover 5 and the terminal member 7 by the resin member 10 are maintained for a long period of time.

[0025] The amount of the Group 2 element in the glass filler is preferably such that the atomic ratio of the Group 2 element to silicon in the component elements is 0.12% or more and 65% or less. This is the total amount when multiple types of Group 2 elements (e.g. magnesium and calcium) are contained. If the amount of the Group 2 element is insufficient, the effect of improving durability performance becomes insufficient. If the amount of the Group 2 element is excessive, it becomes difficult to mold into short fibers, and there is a drawback in that the productivity of the glass decreases.

[0026] When at least a part of the Group 2 element is magnesium, the amount of magnesium blended is desirably 0.1% to 25% by mass relative to silicon, and when at least a part of the Group 2 element is calcium, the amount of calcium blended is desirably 0.17% to 81% by mass relative to silicon.

[0027] The inventors of the present invention conducted a test to evaluate the durability of the resin member 10 of this embodiment, and the results are described below. The evaluation results are described here for the following two types. -Erosion depth after durability test Change in elastic modulus before and after durability

[0028] The following two types of filled resins were each cut into 1 mm thick plate samples and subjected to these tests. (Example) Base resin: PPS resin Glass filler material: Magnesium blend (1.9% to 25% by mass relative to silicon) Glass filler shape: Short fiber (10μmφ x 0.3mm length) (Comparative Example) Base resin: Same as above Glass filler material: No Group 2 elements Glass filler shape: Same as above

[0029] In the test, samples of these resin members were immersed in an electrolyte solution under the following conditions. Solvent type of electrolyte: Mixture of ethylene carbonate and diethyl carbonate (mass ratio 1:1) Electrolyte type and concentration: Lithium hexafluorophosphate, 1 mol / L Moisture content: 1200ppm (equivalent to 25 years after the battery was first used) Electrolyte temperature during immersion: 3 levels: 25℃, 65℃, 80℃ Soaking time: 20 days

[0030] In the evaluation of the corrosion depth after durability testing, the corrosion state of the glass filler in the sample after immersion was evaluated. Specifically, the maximum depth from the surface at which the glass filler was completely lost in the cross section of the sample was evaluated. The surface of the sample corresponds to the internal exposed surface 11 of the resin member 10. This evaluation was performed by observing the cross section of the sample with a scanning electron microscope. The results are shown in FIG. 3. FIG. 3 shows the maximum corrosion depth (vertical axis) after immersion for each of the above three levels of immersion temperature, comparing the examples and comparative examples.

[0031] The following can be said from Figure 3: Overall, the higher the immersion temperature, the deeper the corrosion will progress. Under all temperature conditions, the corrosion depth was smaller in the Examples than in the Comparative Examples. Note that the corrosion depth in the Examples immersed at 25°C was zero.

[0032] 3, it can be seen that in the examples containing magnesium, corrosion of the glass filler is suppressed under all temperature conditions, compared to the comparative examples not containing magnesium. This is believed to be because the magnesium added to the examples suppresses dissolution of the glass by hydrogen fluoride.

[0033] In the evaluation of the change in elastic modulus before and after durability testing, the degree to which the elastic modulus of the sample after immersion had decreased compared to the elastic modulus of the sample before immersion was evaluated. Therefore, the elastic modulus of each sample before immersion and after immersion was measured, and the rate of decrease was calculated. The results are shown in FIG. 4. The vertical axis in FIG. 4 shows the ratio of the decrease in the elastic modulus of the sample after immersion from the reference elastic modulus of the sample before immersion as a negative value. The further down in FIG. 4, the more significant the decrease in the elastic modulus due to immersion. FIG. 4 also shows the results for each of the three levels of immersion temperature, comparing the examples and the comparative examples.

[0034] The following can be said from Figure 4: Overall, there is a tendency for the higher the immersion temperature, the greater the decrease in elastic modulus due to immersion. Under all temperature conditions, the degree of decrease in elastic modulus is smaller in the examples than in the comparative examples.

[0035] As shown in Fig. 4, in the examples containing magnesium, the decrease in elastic modulus due to immersion is suppressed under all temperature conditions, compared to the comparative examples not containing magnesium. This is believed to be because the magnesium added to the examples suppresses the dissolution of glass by hydrogen fluoride. In other words, while the comparative examples lose a significant amount of glass filler due to immersion, the examples retain a significant amount of glass filler even after immersion.

[0036] The present inventors also conducted further tests on the penetration of fluorine by immersing the resin member 10 of this embodiment in an electrolyte. For this test, resins containing glass fillers of the four compositions shown in Table 1 were used as samples. The shape of the samples was the same as that described above. Each value in the "mass %" column in Table 1 indicates the mass ratio of each element to the mass of the entire glass including oxygen, etc. Each value in the "mass ratio (%)" column indicates the relative mass ratio of only each element in the glass. Each value in the "atomic number ratio (%)" column is the mass ratio value converted to atomic number ratio based on the atomic weight of each element.

[0037] [Table 1]

[0038] Among the four types of samples in Table 1, sample A contains only calcium as a Group 2 element and does not contain magnesium. Samples B to D contain both magnesium and calcium as Group 2 elements. Among them, sample B has a calcium content close to the upper limit of the above-mentioned desirable range in terms of mass ratio, and a total content of magnesium and calcium close to the upper limit of the above-mentioned desirable range in terms of atomic ratio. Sample C has a magnesium content close to the upper limit of the above-mentioned desirable range in terms of mass ratio, and the magnesium content and calcium content are almost equal in terms of atomic ratio. Compared to sample C, sample D has a reduced magnesium content and an increased calcium content while keeping the total of the magnesium content and calcium content in terms of atomic ratio almost equal.

[0039] These four types of samples were immersed in an electrolyte, and the penetration depth of fluorine into the samples after immersion was measured. Multiple samples of each type were used for the measurement. The electrolyte used was the same as that described in the explanation of the test above. A scanning electron microscope equipped with an X-ray elemental analyzer was used to measure the penetration depth of fluorine. That is, while observing the cross section of the sample after immersion with the electron microscope, the distribution of fluorine was mapped with the X-ray elemental analyzer, and the maximum depth from the surface where the presence of fluorine was detected was measured. This is a different indicator from the "erosion depth" mentioned above, and is generally a larger value than the "erosion depth" under the same conditions.

[0040] Figure 5 is a graph showing the relationship between the measured fluorine penetration depth and the temperature of the electrolyte during immersion. The vertical axis in Figure 5 is penetration depth, and the lower the axis, the less penetration there is, meaning better resistance to the electrolyte. In the measurements in Figure 5, four temperatures were used during immersion: 25°C, 40°C, 60°C, and 80°C. The immersion time was 20 days. For each temperature level and sample type, five samples were immersed and then measured, and the maximum penetration depth for each sample was recorded.

[0041] It can be seen from Figure 5 that the higher the immersion temperature, the greater the penetration depth of fluorine. Furthermore, of the four types of samples, sample A, which does not contain magnesium, tends to have a greater penetration depth than samples B to D, which contain magnesium. This suggests that, among the Group 2 elements, magnesium is more effective than the other Group 2 elements. However, since fluorine penetrates so deeply into samples that do not contain any Group 2 elements at all that it does not fall within the range of the vertical axis of Figure 5, it can be said that fluorine penetration is suppressed even in Sample A by comparison.

[0042] As described above in detail, according to this embodiment, in the battery 1 in which the electrolyte 6 contains fluorine, a composite material containing a glass filler to which a Group 2 element is added is used as the resin member 10 that seals the through hole 9 through which the terminal member 7 passes. As a result, even if moisture gets mixed into the electrolyte 6, deterioration of the resin member 10 due to the mixing is suppressed. In other words, the durability of the resin member 10 is improved by adding a Group 2 element to the glass filler. Thus, a lithium ion battery 1 in which deterioration of the resin member 10 is not accelerated even when a nonaqueous electrolyte 6 containing fluorine is used is realized.

[0043] The present embodiment and examples are merely illustrative and do not limit the present disclosure in any way. Therefore, the present disclosure can be modified and improved in various ways without departing from the spirit of the present disclosure. For example, in the above embodiment, the battery 1 to which the present disclosure can be applied has a flat rectangular shape as shown in FIG. 1. However, the present disclosure can also be applied to batteries with other shapes, such as a cylindrical shape.

[0044] In the above embodiment, the resin member 10 to which the technology disclosed herein is applied is an insulating member between the terminal member 7 and the lid 5. However, the technology disclosed herein can be applied to resin materials in other locations in the battery. An example of a resin material in other locations is a sealing resin when a liquid injection port is sealed with a resin material. In addition, the box body 4 of the case 2 may be an insulating material, so that the box body 4 itself can be made of a resin member to which the technology disclosed herein is applied. In addition, the resin member of the technology disclosed herein can also be used as a sealing resin between a cylindrical case and a circular lid in the case of a cylindrical battery.

[0045] In the above embodiment, the terminal member 7 and the external terminal 8 are connected to the outside of the case 2. However, the terminal member 7 and the external terminal 8 may be configured as one unit. Inside the case 2, one end of the terminal member 7 is not limited to being directly connected to the electrode body 3, and may be indirectly connected via another current collecting member. [Explanation of symbols]

[0046] 1 battery 6 electrolyte 2 Case 7 Terminal material 3 Electrode body 10 Resin member 4 Box 11 Internal exposed surface 5 Lid

Claims

1. A lithium ion battery having a case, an electrode assembly and an electrolyte contained inside the case, and a resin member fixed to the case and having an inner exposed surface exposed to the inside of the case, The electrolyte is a non-aqueous electrolyte containing fluorine, the resin member includes a glass filler formed of glass mainly composed of silicon oxide and containing a Group II element added thereto; A lithium ion battery, wherein the atomic ratio of the Group 2 element to silicon in the component elements of the glass filler is 0.12% or more and 65% or less.

2. 2. The lithium ion battery of claim 1, At least a portion of the Group 2 element is magnesium; A lithium ion battery, wherein the mass ratio of magnesium to silicon in the component elements of the glass filler is 0.1% or more and 25% or less.

3. 2. The lithium ion battery of claim 1, At least a portion of the Group 2 element is calcium; A lithium ion battery, wherein the mass ratio of calcium to silicon in the component elements of the glass filler is 0.17% or more and 81% or less.

4. A lithium ion battery according to any one of claims 1 to 3, a terminal member connected to the electrode body inside the case and provided to pass through the case and be partially exposed to the outside of the case; The resin member insulates the case from the terminal members.

Citation Information

Patent Citations

  • Improved hole sealing structure of sealing terminal assembly

    JP1988088374A

  • Resin composition for gasket, production method therefor, and gasket for secondary battery

    WO2015030137A1

  • Inorganic particles for nonaqueous electrolyte battery

    WO2018101474A1

  • Polyarylene sulfide resin composition, and composite composed thereof

    JP2013035950A