Decorative coating material
A coating material using concrete and washed sand sludge with fine sand and additives addresses the issues of hiding base imperfections and waste utilization, achieving efficient texture replication and enhanced durability.
Patent Information
- Application Number
- JP2023082236
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Existing decorative finishing coating materials fail to effectively hide unevenness or cracks in the base and require multiple applications to cover the original color, while also not utilizing washed sand sludge, which is often discarded as waste.
A decorative finishing coating material composed of concrete sludge, washed sand sludge, synthetic resin emulsion paint, and fine sand with a particle size of less than 0.3 mm, along with additives like silica gel powder and ethylene-vinyl acetate copolymer resin, to achieve uniform application and texture replication.
The material allows for easy hiding of base irregularities and cracks with a single application, reproduces the texture of concrete, and utilizes waste materials, providing improved durability and fire resistance.
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative finishing coating material for making the appearance of building materials look like concrete or mortar. [Background technology]
[0002] The present inventors have developed a concrete decorative agent that is a conventional decorative finishing coating material that is composed of concrete sludge, synthetic resin emulsion paint, and water, reuses concrete sludge, and can reproduce the texture of exposed concrete. It is non-slip, resistant to cracking, lifting, and peeling, has great strength even when thin, and can produce the weightiness characteristic of concrete (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-109881 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the concrete decorative agent described in Patent Document 1 has a finished thickness of only about 0.1 mm, making it unable to hide irregularities or cracks in the base. In addition, it must be applied three or more times to completely remove the original color of the base, which results in a long construction time. Another unused waste material, similar to concrete sludge, is sand washing sludge discharged from sand washing plants. Currently, there is no effective way to utilize sand washing sludge, and almost all of it is discarded.
[0005] To provide a decorative finishing coating material which is made with a view to solving such problems, can easily erase the original color of the substrate by smoothing with a trowel, and can easily hide unevenness and cracks in the substrate, and can reproduce the texture of exposed concrete by reusing washed sand sludge in addition to concrete sludge. [Means for solving the problem]
[0006] In order to achieve the above object, the decorative finishing coating material of the present invention is characterized by including concrete sludge, washed sand sludge, synthetic resin emulsion paint, and sand with a particle size of less than 0.3 mm. The concrete sludge and the washed sand sludge are each preferably contained in an amount of 3% or more of the total mass. The moisture content is appropriately adjusted before use. The synthetic resin emulsion paint is preferably contained in an amount of 5% or more of the total mass. The sand having a particle size of less than 0.3 mm preferably accounts for 30% or more of the total mass. The decorative finishing coating material according to the present invention may contain silica gel powder. The decorative finishing coating material according to the present invention may also contain an ethylene-vinyl acetate copolymer resin. The decorative finishing coating material according to the present invention may also contain titanium oxide and sodium carboxymethylcellulose. The silica gel powder, ethylene-vinyl acetate copolymer resin, titanium oxide, and sodium carboxymethylcellulose are each preferably contained in an amount of 0.1% to 5.0% of the total mass.
[0007] The concrete sludge is preferably made of concrete sludge water. Concrete sludge water is recovered water generated during cleaning at factories that handle ready-mix concrete, and refers to water from which fine and coarse aggregates have been removed. Concrete sludge water contains a large amount of cement hydrate, and is also rich in potassium ions and calcium ions. In general, concrete and mortar tend to reduce in volume when dried. Cement hydrate, which is mainly formed by the hydration of cement and water, shrinks when dried. The texture of concrete is reproduced by adding concrete sludge.
[0008] It is desirable that the washed sand sludge is made from dehydrated washed sand sludge water. Washed sand sludge water means water that contains a lot of clay and silt that is generated when washing sand. Clay, which is used in pottery and earthen walls, reduces in volume and hardens as the moisture inside it is lost. Japan, a country with many volcanoes, often contains clays such as montmorillonite, which belong to the smectite group and have high ion exchange and water absorption properties, but the inside of the montmorillonite often has few ions due to the effects of rain over the long period of time before it is excavated. Therefore, by mixing it with concrete sludge, which contains a lot of calcium ions, the sand washing sludge starts to exchange ions with the concrete sludge, and they mix very strongly.
[0009] The particle size of concrete sludge is larger than that of washed sand sludge, so that the washed sand sludge sticks to the concrete sludge. This results in a state in which many calcium ions are present inside the washed sand sludge. Due to this sludge, the decorative finishing coating material of the present invention has a moderate viscosity like whipped cream before drying, so it is easy to apply like paint. In addition, as these two types of sludge dry, a large volume reduction occurs. In addition, calcium ions react with carbon dioxide in the air to produce calcium carbonate, which promotes densification and generates the same adhesive strength as plaster, and allows for continuous strength development. In addition, by using sand as the main material, just like mortar, the finished texture becomes closer to mortar, and building materials coated with the decorative finishing coating material of this invention can be expected to have improved fire resistance.
[0010] Sand with a particle size of less than 0.3 mm is preferably sieved after drying. By using only particles with a particle size of 0.3 mm or less, it is possible to apply a thin layer of sand at a consistent thickness when troweled. Generally, liquefaction is likely to occur in ground with a lot of sand that easily absorbs moisture. When moist sand is vibrated, the water floats out and the sand has the property of adhering to each other. By utilizing this property, even if the viscosity of the decorative finish coating material increases during troweling, the surface water in the sand is separated from the sand by vibration, so that it is essentially in a state where water has been added, and it is possible to temporarily reduce the viscosity. This makes it possible to level the surface with a trowel as many times as you like within the time it takes to dry. By smoothing the surface with a trowel, it is easy to erase the original color of the base and hide unevenness and cracks in the base. The decorative finishing coating material of the present invention can reproduce the texture of exposed concrete.
[0011] The synthetic resin emulsion paint is preferably white, as mixing it allows the color tone of the product to be consistent. The silica gel powder is preferably made of crushed silica scale or silica gel. Silica gel has an expansion force strong enough to destroy concrete from the inside, and this reaction is generally called the alkali-silica reaction of concrete. The silica gel powder is saturated with water inside the decorative finish coating material and expands in volume. When this powder dries, it generates a shrinkage force, which makes it possible to densify the decorative finish coating material. In addition, silica gel makes it possible to stabilize the amount of drying shrinkage of concrete sludge and washed sand sludge.
[0012] The ethylene vinyl acetate copolymer resin has the effect of wrapping the needle-like crystals of the sludge, compressing and adhering them. In other words, while concrete hardens by the growth of needle-like crystals due to hydration reaction within the material, the decorative finishing coating material of this invention has the needle-like crystals contained in the sludge and the substances surrounding them present from the beginning, and the synthetic resin emulsion paint connects them, and the ethylene vinyl acetate copolymer resin dries and shrinks, compressing the whole, achieving the same strength and durability as hardened concrete. Ethylene-vinyl acetate copolymer resin is preferably used for the first layer of a concrete floor that is subject to pressure, or when decorating a concrete surface that has a smooth feel.
[0013] Titanium dioxide is preferably white in color, and by mixing it it is possible to change the intensity of the white color of the product. By adding sodium carboxymethylcellulose, the degree of viscosity can be changed. Effect of the Invention
[0014] According to the present invention, it is possible to provide a decorative finishing coating material which can easily erase the original color of the base by smoothing with a trowel and hide unevenness and cracks in the base, and which can reproduce the texture of exposed concrete by reusing washed sand sludge in addition to concrete sludge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described. The decorative finishing coating material according to the embodiment of the present invention includes concrete sludge, washed sand sludge, synthetic resin emulsion paint, and sand with a particle size of less than 0.3 mm. The concrete sludge and washed sand sludge are preferably contained in an amount of 3% or more of the total mass. The moisture content is adjusted as appropriate. The synthetic resin emulsion paint is preferably contained in an amount of 5% or more of the total mass. The sand with a particle size of less than 0.3 mm is preferably contained in an amount of 30% or more. The decorative finishing coating material may include silica gel powder, ethylene-vinyl acetate copolymer resin, titanium oxide, and sodium carboxymethylcellulose. The silica gel powder, ethylene-vinyl acetate copolymer resin, titanium oxide, and sodium carboxymethylcellulose are preferably contained in an amount of 0.1% to 5.0% of the total mass, respectively.
[0016] Concrete sludge contains a large amount of cement hydrate. It is preferable that concrete sludge is made of concrete sludge water. Concrete sludge water discharged from a plant that handles ready-mix concrete is mainly cement hydrate that has not been mixed with water for a long time, so it needs to be managed to prevent precipitation and hardening for a certain period of time until the cement hydration reaction stabilizes. After stabilization, the concrete sludge water is used after removing excess water. Cement hydrate exists from the surface to the inside of concrete and mortar, and is the main cause of creating the texture of concrete, so by using it, it is possible to reproduce the texture of concrete.
[0017] Washed sand sludge is disposed of after being dewatered. Polymer coagulants are the mainstream chemicals used during dewatering, and are commonly used in water treatment facilities. In some cases, hydrated lime is used as the primary chemical and polymer coagulants as the secondary chemical to improve the dewatering effect, and the compatibility between hydrated lime and washed sand sludge has been demonstrated in sand washing plants. Concrete sludge is rich in calcium hydroxide, the main component of hydrated lime.
[0018] In a sand washing plant, the experience of the engineer in charge is very important for the dewatering process, and it is necessary to accurately grasp the ratio of water to sludge and the properties of the sludge before deciding the amount of chemicals to add. If this judgment is incorrect, the dewatering machine will break down or dewatering will fail, and the production of washed sand will stop. Therefore, the amount of chemicals contained in washed sand sludge that has been dewatered without any problems will be within a certain range and will be stable. Washed sand sludge that contains an appropriate amount of polymer coagulant will mix evenly with concrete sludge and will reduce in volume evenly after drying, making it possible to prevent drying shrinkage cracks in decorative finishing coating materials.
[0019] Sand with a particle size of less than 0.3 mm is preferably baked, dried, and then sieved and selected. Generally, sand used in ready-mix concrete, i.e. fine aggregate, is sand that passes through a 10 mm concrete sieve and 85% of the sand passes through a 5 mm mesh. Other meshes for determining particle size include 2.5 mm, 1.2 mm, 0.6 mm, 0.3 mm, and 0.15 mm. Generally, fine aggregates that are suitable for use in concrete are those that are a mixture of particles of various particle sizes, and the ratio of each is determined by JIS A 5308 Ready Mixed Concrete. Therefore, the sand currently sold in many stores is manufactured to meet this standard, but it is only sand for making concrete, and cannot be said to be suitable for mortar. Mortars using sand with a larger particle size, i.e. sand containing a large amount of 5.0 mm, 2.5 mm, and 1.2 mm sizes, have the problem that it is difficult to apply thinly due to the size of the particles, and the thicker the sand is applied, the more difficult it is to achieve a smooth finish. Sand with a particle size of less than 0.3 mm is easy to use as mortar. By using only sand with a particle size of less than 0.3 mm, it is possible to simplify thin application of decorative finishing coating materials.
[0020] Synthetic resin emulsion paint is mainly used for coloring sludge. Concrete sludge is gray, while washed sand sludge is brownish in color. Washed sand sludge in particular is a natural resource, so its color varies to some extent depending on the place of origin, stratum, and clay content. By changing the amount of synthetic resin emulsion paint added depending on the condition of the washed sand sludge, it is possible to maintain a consistent color for the decorative finish coating material. Ethylene-vinyl acetate copolymer resin is used primarily to stabilize the separation resistance of decorative finishing coating materials, and is used as an auxiliary agent to keep a certain amount of gas trapped inside the container to prevent the decorative finishing coating material from separating. Titanium dioxide is used as an auxiliary agent to stabilize the color tone in synthetic resin emulsion paints. Sodium carboxymethylcellulose is used as an auxiliary agent to stabilize the viscosity of decorative finishing coating materials.
[0021] <Application method> The decorative finishing coating material according to the embodiment of the present invention can be applied by a plasterer's trowel, roller, brush, rubber spatula, sponge, or by hand. If there is a possibility that the moisture in the decorative finishing coating material will cause scum to appear on the base, it is desirable to treat the base in advance, such as by preventing scum. The basic number of coats is one, but if durability is expected to be improved, the number of coats may be increased. The drying time is preferably 48 hours in summer and 72 hours or more in winter. Since the strength of the decorative finishing coating material stabilizes after application after more than two weeks, it is preferable to wait more than two weeks after application before cleaning the applied surface and wiping it with water.
[0022] <Effects after applying decorative finishing coating material> The areas where the decorative finishing coating material of the embodiment of the present invention is applied can reproduce the texture of natural concrete or mortar, or the texture of exposed concrete. This is because the main ingredient of the decorative finishing coating material is sand, and it also contains concrete sludge. The marks left by the sand being pulled by the trowel are characteristic patterns that appear when a plasterer finishes mortar. By reproducing this with the decorative finishing coating material, it is possible to more accurately reproduce the texture of mortar. Trowel smoothing can easily erase the original color of the base and hide unevenness and cracks in the base.
[0023] There are many types of concrete or mortar-like decorative finishing coating materials currently available, but few of them fit the definition of mortar, which is a mixture of cement, sand, and water. The decorative finishing coating material of the embodiment of the present invention is a one-material type decorative finishing coating material that contains all the substances contained in mortar, including cement hydrate, sand, and water. Since the decorative finishing coating material is mainly made of sand, it is expected to have the effect of delaying the time until ignition when applied to materials that may burn, such as wood. EXAMPLES
[0024] A decorative coating material was manufactured with the following composition: (Composition) Concrete sludge 0.05 kg Washed sand sludge 0.05 kg 0.60kg of sand with grain size less than 0.3mm White synthetic resin emulsion paint 0.20kg Dilution water 0.10kg (Manufacturing method) For the concrete sludge, concrete sludge water discharged from a ready mixed concrete plant and settled in a concrete sludge tank was used. For the washed sand sludge, sand discharged from a sand washing plant and dehydrated was used. A commercially available water-based white type synthetic resin emulsion paint was used. For sand with a particle size of less than 0.3 mm, fine aggregate for ready mixed concrete was baked and dried at a sand baking plant, and then sieved and selected using a 0.3 mm mesh, and all that passed through the mesh was used. For dilution water, the supernatant water of the concrete sludge water was used. All the above materials were mixed together to produce 1 kg of decorative finish coating material. The decorative finish coating material produced was applied to plywood (conpane) for concrete formwork. As a result, the texture of mortar plastering was reproduced.
[0025] <Test 1> In order to confirm the effect of Example 1, a comparative test was conducted with other decorative finishing coating materials. A comparative decorative finishing coating material (Comparative Example 1) was manufactured using the following formulation. (Composition) Concrete sludge 0.05kg Water-based paint 0.25kg Ethylene-vinyl acetate copolymer resin 0.20kg Silica gel 0.002kg Dilution water 0.50kg The decorative finishing coating material of Example 1 and the decorative finishing coating material of Comparative Example 1 were applied to plywood (conpane) for concrete formwork, and the finishes were compared.
[0026] As a result, the decorative finishing coating material of Example 1 contained sand less than 0.3 mm in size, so the finished thickness was at least 0.3 mm. This made it possible to flatten relatively small unevenness of the base with one application. In addition, because the finished thickness was increased, it became possible to erase the original color of the base in one application. In contrast, the decorative finish coating material of Comparative Example 1 was a low-viscosity liquid, and application with a trowel was impossible, so application was limited to rollers and brushes. In addition, the finished thickness was only about 0.1 mm, so it was not possible to hide the unevenness or cracks of the base, and it was only possible to give it a concrete-like color. It was necessary to apply it three or more times to completely erase the original color of the base, which took a long time to apply.
[0027] <Test 2> In order to confirm the effect of Example 1, a comparative test was carried out with general mortar. A comparative 1:3 mortar (Comparative Example 2) was produced with the following composition. (Composition) Portland cement 1.0kg Sand 3.0kg water 0.5kg The decorative finishing coating material of Example 1 and the mortar of Comparative Example 2 were applied to plywood for concrete formwork (conpane), and the finishes were compared.
[0028] As a result, the decorative finishing coating material of Example 1 becomes whipped cream-like due to the inclusion of washed sand sludge, so it maintains moderate viscosity until it dries, and can be spread thinly and applied, so the amount used per unit area can be reduced. In addition, due to the influence of the sludge with moderate adhesiveness, it does not peel off during application like mortar. Even if the viscosity decreases, it can be restored by mixing again. Mortar hardens by hydration reaction, but this decorative finishing coating material begins to harden when water evaporates, so it can be stored in a sealed container, eliminating the time constraints of mortar.
[0029] In contrast, the mortar of Comparative Example 2 contains sand with a maximum particle size of about 5 mm because it uses fine aggregate used in making ready-mix concrete, and the thickness of each application cannot be made thinner than 5 mm, and it is impossible to spread it thinner than 5 mm, so a large amount of mortar was required for application. Also, the thicker the application, the more likely it was to peel off during application.
[0030] Also, if the mortar was made too viscous and mixed to make it stick to the base, it was impossible to spread and apply. Conversely, if the viscosity was low, it became very difficult to finish the surface evenly. If the viscosity became too high and water was added, the water-cement ratio would change, which could lead to a loss of strength and make the mortar more susceptible to cracking. To make mortar with the right viscosity and that would not crack, it was necessary to thoroughly understand the relationship between sand, cement, and the amount of water. Also, because the hydration reaction continued to progress when cement was mixed with water, the entire process had to be completed within about an hour, and mortar once made could not be stored.
[0031] (result) (1) Thickness: Example 1: Approximately 0.3 mm (thin coating is possible) Comparative Example 2: 5mm or more (2) Amount used: Example 1: Small Comparative Example 2: Many (3) Viscosity: Example 1 Stable Comparative Example 2 Unstable (The viscosity of the mortar depends on the properties of the sand and the amount of water.) (4) Viscosity recovery: Example 1 Just mix Comparative Example 2: Water is required (Adding extra water to the mortar increases the chance of cracking.) (5) Preservation: Possible in Example 1 Comparative Example 2: Not possible (The hardening of the mortar is irreversible. It is necessary to use it up within the time limit.) EXAMPLES
[0032] A decorative coating material was manufactured with the following composition: (Composition) Concrete sludge 0.05 kg Washed sand sludge 0.05 kg 0.50kg of sand with a grain size of less than 0.3mm White synthetic resin emulsion paint 0.20kg Mixed water 0.18 kg (mixture of 0.02 kg silica gel powder, 0.001 kg ethylene vinyl acetate copolymer resin, 0.02 kg sodium carboxymethylcellulose, and 0.139 kg dilution water)
[0033] (Manufacturing method) The concrete sludge used was concrete sludge water discharged from a ready mixed concrete plant and settled in a concrete sludge tank. The washed sand sludge used was sand discharged from a sand washing plant and dehydrated. A commercially available water-based white synthetic resin emulsion paint was used. For sand with a particle size of less than 0.3 mm, fine aggregate for ready mixed concrete was baked and dried at a sand baking plant, and then sieved and selected using a 0.3 mm mesh. All sand that passed through the mesh was used. The silica gel powder used was powdered silica gel for drying. A commercially available viscosity modifier was used for sodium carboxymethylcellulose. The supernatant water of the concrete sludge water was used for dilution water. All the above materials were mixed together to produce 1 kg of decorative finish coating material. The decorative finish coating material produced was applied to plywood. As a result, the decorative finish coating material had excellent viscosity, adhesion, strength, storage properties, and application performance.
Claims
1. The decorative finishing coating material is characterized by containing concrete sludge, washed sand sludge, synthetic resin emulsion paint, and sand having a particle size of less than 0.3 mm.
2. 2. The decorative finishing coating material according to claim 1, further comprising silica gel powder.
3. 3. The decorative finishing coating material according to claim 1, further comprising an ethylene-vinyl acetate copolymer resin.
4. 3. The decorative finishing coating material according to claim 1, further comprising titanium oxide and sodium carboxymethylcellulose.
5. 4. The decorative finishing coating material according to claim 3, comprising titanium oxide and sodium carboxymethylcellulose.
Citation Information
Patent Citations
Concrete decorative agent, concrete decorative member, and method for producing concrete decorative agent
JP2021109881A