Silane-terminated resin for low viscosity sealant and method for producing the same
A silane-terminated resin with intramolecularly introduced short chain segments addresses high viscosity issues, enhancing sealant extrudability and mechanical performance.
Patent Information
- Application Number
- JP2023126346
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2023-08-02
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2043-08-02
AI Technical Summary
Existing silane-terminated resins have high viscosity, making it difficult to reduce sealant cost by increasing the amount of calcium carbonate without compromising mechanical performance.
Introduce short chain segments intramolecularly to soften and make molecular chains more mobile by synthesizing a silane-terminated resin with a specific structural formula and production method involving alkylene oxides and organotin catalysts.
The method reduces viscosity, improving extrudability and mechanical performance of sealants while maintaining flexibility and adhesion properties.
Smart Images

Figure 2024166013000001 
Figure 2024166013000002 
Figure 2024166013000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of sealants, and more particularly to silane-terminated resins for low viscosity sealants and methods for their preparation. [Background technology]
[0002] Sealants are now indispensable materials in many fields such as construction and transportation. With the vigorous development of prefabricated construction, people are increasingly interested in sealants and the demand for their performance is also increasing. Existing sealant products on the market are mainly silicone-based, polyurethane-based and silane-modified sealants. Here, silane-terminated resins not only have the flexibility and low-temperature resistance of polyether, but also have the good moisture curing and adhesive properties of siloxane groups, and combine the advantages and merits of silicone sealants and polyurethane sealants, and show excellent weather resistance, adhesiveness, paintability, and deformation and displacement resistance, which makes them prominent among them. However, since the viscosity characteristics of silane-terminated resins in the prior art are relatively large, when adjusting the compounding components of sealants containing these silane-terminated resins, it is not possible to reduce the cost of the sealant by increasing the amount of calcium carbonate added.
[0003] To solve the problem that the viscosity of the silane-terminated resin is too high, the viscosity of the sealant is generally reduced by adding a plasticizer. In the prior art, the viscosity of the silane-based sealing resin is also modified to reduce the viscosity of the silane-terminated resin. For example, Chinese patent CN104212046A provides a method for producing a low-viscosity silane-modified polymer resin, which includes the steps of taking two or more materials and polymerizing them at a temperature of 10-100 degrees Celsius to produce raw materials, and mixing the two or more raw materials in accordance with the ratio to obtain silane-modified polymer resins with different properties, that is, the mechanical properties and temperature resistance of the resin are effectively adjusted by obtaining the silane-modified resin by the combined method of polymerization and mixing. Chinese patents CN103080175A and CN1037041A both achieve the purpose of reducing the viscosity by adding a composition of a substance with a relatively small molecular weight. In all of the above methods, a certain amount of small molecule substances are mixed into the polymer. The addition of inactive small molecules reduces the strength of the sealant product itself, while the addition of active molecules reduces the tensile performance of the sealant product.
[0004] Therefore, there is a great need to develop a silane-terminated resin for sealants that can reduce the viscosity from the internal structure of the molecule, and a method for producing the same. Summary of the Invention [Problem to be solved by the invention]
[0005] In order to overcome the shortcomings of the prior art, the object of the present invention is to provide a silane-terminated resin for low viscosity sealants, which achieves the objective of lowering the viscosity by introducing short chain segments to plasticize the resin intramolecularly, making the molecular chains softer and more mobile. [Means for solving the problem]
[0006] In order to solve the above problems, the technical solutions used in the present invention are as follows:
[0007] A silane-terminated resin for low viscosity sealants, the structural formula of which is: [ka] where "-----" is [ka] The number of repeating units is ≧172, and R is C n H 2n where n=1 to 5, and R1 is a linear alkyl group C m H 2m+1 m≧1, the mass ratio of R1 in the repeating units being a methyl group is 50 to 90%, R2 is CH3 or CH2CH3, and R3 is OR2 or R2.
[0008] In a preferred embodiment of the present invention, the silane terminated resin has a number average molecular weight of about 15,000-3,000.
[0009] The second object of the present invention is to provide a method for producing the above-mentioned silane-terminated resin for low viscosity sealants, which comprises:
[0010] Step S1: add 1 part of an alcohol-based initiator and an alkaline earth metal to a reaction vessel, replace with nitrogen, and then heat to 75 to 150 ° C., add 7.5 to 14.5 parts of an alkylene oxide, control the pressure to 0.0 to 0.4 MPa, mature until the pressure does not decrease, cool to 90 to 115 ° C., degas and purify to obtain a low molecular weight polymer;
[0011] Step S2: add 1 part of the low molecular weight polymer obtained in step S1 to the reactor, add 5-15 ppm of the total mass of a multimetal cyanide catalyst, replace with nitrogen, heat to 120-130°C, dehydrate, heat to 130-140°C, add 250-355 parts of alkylene oxide, control the pressure to 0.0-0.4Mpa, mature until the pressure does not decrease, cool, degas and discharge to obtain a high molecular weight polymer resin;
[0012] The method includes step S3 of adding an organotin catalyst and an isocyanate silane to the polymer resin produced in step S2 to carry out a reaction, sampling the reaction mixture during the reaction and performing an infrared characteristic peak test, and terminating the reaction when the reaction mixture no longer has an isocyanate infrared characteristic peak, thereby obtaining the silane-terminated resin.
[0013] In a preferred embodiment of the present invention, the alcohol initiator in step S1 is a short-chain diol, preferably propylene glycol, isobutylene glycol or dex-1,3-butylene glycol, and the alkaline earth metal is K or Na.
[0014] In a preferred embodiment of the present invention, the alkylene oxide in steps S1 and S2 is a mixture of propylene oxide and one of butylene oxide, hexylene oxide, pentylene oxide, and heptalene oxide. Preferably, the molar ratio of propylene oxide to other alkylene oxide in the alkylene oxide mixture is 1:1 to 10:1, and more preferably, the molar ratio of propylene oxide to other alkylene oxide in the alkylene oxide mixture is 5:1 to 10:1.
[0015] In a preferred embodiment of the present invention, the number average molecular weight of the low molecular weight polymer prepared in step S1 is 400-800.
[0016] In a preferred embodiment of the present invention, the metal ions contained in the multimetal cyanide catalyst in step S2 are at least two of Co, Zn, and Pb.
[0017] In a preferred embodiment of the present invention, the dehydration time in step S2 is 30-90 min, the aging temperature is 130-150° C., and after the temperature is lowered to 90-110° C., the mixture is degassed and discharged.
[0018] In a preferred embodiment of the present invention, in step S2, first, 10 to 30 g of alkylene oxide is added, the pressure is controlled to 0.2 to 0.9 MPa, and the remaining alkylene oxide is added after the pressure has clearly dropped.
[0019] In a preferred embodiment of the present invention, the high molecular weight polymer resin has a number average molecular weight of 15,000 to 30,000.
[0020] In a preferred embodiment of the present invention, the number of nitrogen replacements in steps S1 and S2 is three or more.
[0021] In a preferred embodiment of the present invention, the amount of the organotin catalyst added in step S3 is 0.05 to 0.15% of the total input amount, and the organotin catalyst is dibutyltin dilaurate or dioctyltin dilaurate.
[0022] In a preferred embodiment of the present invention, the mass ratio of the hydroxyl value of the high molecular weight polymer resin to the NCO of the isocyanate silane in step S3 is OH:NCO=0.98 to 1.02:1.
[0023] In a preferred embodiment of the present invention, the reaction temperature in step S3 is 40 to 100° C., and the reaction time is 2 to 10 hours. Effect of the Invention
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0025] The present invention firstly synthesizes a low molecular weight polymer by using an alcohol-based initiator, an alkaline earth metal and an alkylene oxide, then adds a multimetal cyanide catalyst and an alkylene oxide to synthesize a high molecular weight polymer, and finally adds an organotin catalyst and an isocyanate silane to react to obtain a silane-terminated resin, thereby successfully introducing a short chain segment into the molecule, destroying the original molecular crystal, and plasticizing the molecule, softening the molecular chain and making it easier to move, thereby achieving the purpose of reducing the viscosity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be further described below in connection with specific embodiments.
[0027] A silane-terminated resin for low viscosity sealants, the number average molecular weight of which is about 15,000-30,000 and the structural formula of which is: [ka] and However, "-----" is [ka] and the number of said repeating units is ≧172; R is C n H 2n where n=1 to 5, and R1 is a linear alkyl group C m H 2m+1 m≧1, the mass ratio of R1 in the repeating units being a methyl group is 50 to 90%, R2 is CH3 or CH2CH3, and R3 is OR2 or R2.
[0028] The method for producing the silane-terminated resin for low viscosity sealants includes the steps of:
[0029] Step S1: add 1 part of alcohol-based initiator and alkaline earth metal to the reactor, replace with nitrogen three times or more, then heat to 75-150°C, add 7.5-14.5 parts of alkylene oxide, control the pressure to 0.0-0.4Mpa, mature until the pressure does not decrease, cool to 90-115°C, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of 400-800;
[0030] Step S2: add 1 part of the low molecular weight polymer obtained in step S1 to the reactor, add 5-15 ppm of the total mass of multimetal cyanide catalyst, replace with nitrogen three times, then heat to 120-130°C, dehydrate for 30-90 min, heat to 130-140°C, add 250-355 parts of alkylene oxide (first add 10-30 g of alkylene oxide, control the pressure to 0.2-0.9 MPa, add the remaining alkylene oxide after the pressure has dropped significantly), control the pressure to 0.0-0.4 MPa, mature at 130-150°C until the pressure does not drop, cool to 90-110°C, degas and discharge, obtain a high molecular weight polymer resin with a number average molecular weight of 15,000-30,000;
[0031] The method includes step S3 of adding 0.05-0.15% of the total amount of an organotin catalyst and isocyanate silane (OH:NCO=0.98-1.02:1) to the high molecular weight polymer resin produced in step S2, carrying out a reaction at a temperature of 40-100°C for 2-10 hours, sampling the reaction mixture during the reaction and conducting an infrared characteristic peak test, and terminating the reaction when the isocyanate infrared characteristic peak is no longer present in the reaction mixture, thereby obtaining the silane-terminated resin.
[0032] In the above method, the alcohol initiator in step S1 is one of propylene glycol, isobutylene glycol, and dex-1,3-butylene glycol, the alkaline earth metal is K or Na, and the alkylene oxide in steps S1 and S2 is a mixture of propylene oxide and one of butylene oxide, hexylene oxide, pentylene oxide, and heptalene oxide. The metal ions contained in the multimetal cyanide catalyst in step S2 are at least two of Co, Zn, and Pb. The organotin catalyst is dibutyltin dilaurate or dioctyltin dilaurate. Example 1:
[0033] 1. A method for producing a silane-terminated resin for a low viscosity sealant, comprising:
[0034] Step S1: add 100g of propylene glycol and 0.2% Na in the total amount of the input to the reactor, replace with nitrogen three times, then heat to 100±5°C, add 952g of alkylene oxide obtained by mixing propylene oxide and butylene oxide in a mass ratio of 9:1, control the pressure to less than 0.4Mpa, and after completion, mature until the pressure does not decrease, cool to 90°C, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of 796;
[0035] Add 100g of the low molecular weight polymer obtained in step S1 and a multimetal cyanide catalyst with a mass fraction of 0.002% of the total amount of the catalyst to the reactor, replace with nitrogen three times, then heat to 125±5°C, dehydrate for 40 minutes, further heat to 130-140°C, add 2135g of alkylene oxide obtained by mixing propylene oxide and butylene oxide in a mass ratio of 9:1 (first add 10-30g of alkylene oxide, control the pressure to less than 0.9Mpa, add the remaining alkylene oxide after the pressure has obviously dropped), control the pressure to less than 0.4Mpa, mature at a temperature of 140±5°C until the pressure does not drop, maintain for 20 minutes, cool to 110°C±5°C, degas and discharge, obtain a polymer resin with a number average molecular weight of about 15638; step S2.
[0036] Step S3 includes adding 0.1% of the total amount of dibutyltin dilaurate and 3-isocyanatopropyltrimethoxysilane (OH:NCO=0.98:1) to the high molecular weight polymer resin produced in step S2, and carrying out a reaction at a temperature of 100°C for 3 hours. During the reaction, the reaction mixture is sampled for an infrared characteristic peak test. When the reaction mixture no longer has an isocyanate infrared characteristic peak, the reaction is terminated to obtain a silane-terminated resin. Example 2:
[0037] 1. A method for producing a silane-terminated resin for a low viscosity sealant, comprising:
[0038] Step S1: add 100g of propylene glycol and 0.2% Na in the total amount of the input to the reactor, replace with nitrogen three times, then heat to 100±5°C, add 952g of alkylene oxide obtained by mixing propylene oxide and pentylene oxide in a mass ratio of 9:1, control the pressure to less than 0.4Mpa, and after completion, mature until the pressure does not decrease, cool, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of about 780;
[0039] Add 100g of the low molecular weight polymer obtained in step S1 and a multimetal cyanide catalyst with a mass fraction of 0.002% of the total amount of the catalyst to the reactor, replace with nitrogen three times, then heat to 120±5°C, dehydrate for 40 minutes, further heat to 130-140°C, add 2229g of alkylene oxide obtained by mixing propylene oxide and pentylene oxide in a mass ratio of 9:1 (first add 10-30g, control the pressure to less than 0.6Mpa, add the remaining alkylene oxide after the pressure has clearly decreased), control the pressure to less than 0.4Mpa, mature at a temperature of 130±5°C until the pressure does not decrease, maintain for 20 minutes, cool to 110°C±5°C, degas and discharge, obtain a polymer resin with a number average molecular weight of 15486; step S2.
[0040] Step S3 includes adding 0.1% of the total amount of dibutyltin dilaurate and 3-isocyanatopropyltrimethoxysilane (OH:NCO=0.98:1) to the high molecular weight polymer resin produced in step S2, and carrying out a reaction at a temperature of 100°C for 5 hours. During the reaction, the reaction mixture is sampled for an infrared characteristic peak test. When the reaction mixture no longer has an isocyanate infrared characteristic peak, the reaction is terminated to obtain a silane-terminated resin. Example 3:
[0041] 1. A method for producing a silane-terminated resin for a low viscosity sealant, comprising:
[0042] Step S1: add 100g of propylene glycol and 0.2% Na in the total amount of the input to the reactor, replace with nitrogen three times, then heat to 100±5°C, add 1052g of alkylene oxide obtained by mixing propylene oxide and hexylene oxide in a mass ratio of 9:1, control the pressure to less than 0.4Mpa, and after completion, mature until the pressure does not decrease, cool, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of 785;
[0043] Add 100g of the low molecular weight polymer obtained in step S1 and a multimetal cyanide catalyst with a mass fraction of 0.002% of the total amount of the catalyst to the reactor, replace with nitrogen three times, then heat to 120-130°C, dehydrate for 40 minutes, further heat to 130-140°C, add 2216g of alkylene oxide obtained by mixing propylene oxide and hexylene oxide in a mass ratio of 9:1 (first add 10-30g, control the pressure to less than 0.6Mpa, add the remaining alkylene oxide after the pressure has clearly decreased), control the pressure to less than 0.4Mpa, mature at a temperature of 145±5°C until the pressure does not decrease, maintain for 20 minutes, cool to 110°C±5°C, degas and discharge, obtain a polymer resin with a number average molecular weight of 15758; step S2.
[0044] Step S3 includes adding 0.10% of the total amount of dibutyltin dilaurate and 3-isocyanatopropyltrimethoxysilane (OH:NCO=0.98:1) to the high molecular weight polymer resin produced in step S2, and carrying out a reaction at a temperature of 100°C for 5 hours. During the reaction, the reaction mixture is sampled for an infrared characteristic peak test. When the reaction mixture no longer has an isocyanate infrared characteristic peak, the reaction is terminated to obtain a silane-terminated resin. Example 4:
[0045] 1. A method for producing a silane-terminated resin for a low viscosity sealant, comprising:
[0046] Step S1: add 100g of propylene glycol and 0.2% of Na in the total amount of the reaction vessel, replace with nitrogen three times, then heat to 100±5°C, add 952g of alkylene oxide obtained by mixing propylene oxide and heptalene oxide in a mass ratio of 9:1, control the pressure to less than 0.4Mpa, and after completion, mature until the pressure does not decrease, cool, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of 805;
[0047] Add 100g of the low molecular weight polymer obtained in step S1 and a multimetal cyanide catalyst with a mass fraction of 0.002% of the total amount of the catalyst to the reactor, replace with nitrogen three times, then heat to 120-130°C, dehydrate for 40 minutes, further heat to 130-140°C, add 2162g of alkylene oxide obtained by mixing propylene oxide and heptalene oxide in a mass ratio of 9:1 (first add 10-30g, control the pressure to less than 0.6Mpa, add the remaining alkylene oxide after the pressure has clearly dropped), control the pressure to less than 0.4Mpa, mature at a temperature of 140±5°C until the pressure does not drop, maintain for 20 minutes, cool to 105°C±5°C, degas and discharge, obtain a polymer resin with a number average molecular weight of about 15907; step S2.
[0048] Step S3 includes adding 0.1% of the total amount of dibutyltin dilaurate and 3-isocyanatopropyltrimethoxysilane (OH:NCO=0.98:1) to the high molecular weight polymer resin produced in step S2, and carrying out a reaction at a temperature of 100°C for 6 hours. During the reaction, the reaction mixture is sampled for an infrared characteristic peak test. When the reaction mixture no longer has an isocyanate infrared characteristic peak, the reaction is terminated to obtain a silane-terminated resin. Comparative Example 1
[0049] A method for producing a silane-terminated resin, comprising:
[0050] Step S1: add 100g of propylene glycol and 0.2% Na in the total amount of the reaction vessel, replace with nitrogen three times, then heat to 100±5°C, add 1052g of propylene oxide, control the pressure to less than 0.4Mpa, and after completion, mature until the pressure does not decrease, cool, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of 790;
[0051] Add 100g of the low molecular weight polymer obtained in step S1 and a multimetal cyanide catalyst with a mass fraction of 0.002% of the total amount of the catalyst to the reactor, replace with nitrogen three times, then heat to 125±5°C, dehydrate for 40 minutes, heat to 130-140°C, add 2178g of propylene oxide (first add 10-30g of propylene oxide, control the pressure to less than 0.6Mpa, add the remaining propylene oxide after the pressure has dropped significantly), control the pressure to less than 0.4Mpa, mature at a temperature of 145±5°C until the pressure does not drop, maintain for 20 minutes, cool to 110°C±5°C, degas and discharge, obtain a high molecular weight polymer resin with a number average molecular weight of 15796; step S2.
[0052] Step S3 includes adding 0.10% of the total amount of dibutyltin dilaurate and 3-isocyanatopropyltrimethoxysilane (OH:NCO=0.98:1) to the high molecular weight polymer resin produced in step S2, and carrying out a reaction at a temperature of 100°C for 5 hours. During the reaction, the reaction mixture is sampled for an infrared characteristic peak test. When the reaction mixture no longer has an isocyanate infrared characteristic peak, the reaction is terminated to obtain a silane-terminated resin.
[0053] The products obtained in Examples 1 to 4 and Comparative Example 1 were subjected to liquid phase analysis, and the results are shown in Table 1.
[0054] [Table 1]
[0055] As can be seen from Table 1, in Comparative Example 1, the main chain is a polyoxypropylene ether chain, and the kinetic viscosity is 32600 mpa.s at 25°C, which is much higher than the kinetic viscosity in Examples 1 to 4. This shows that in the present invention, the longer the alkyl group chain of R1 in the added segment, the lower the viscosity of the product, and the softer the molecular chain becomes, making it easier to move. Example 5
[0056] 1. A method for producing a silane-terminated resin for a low viscosity sealant, comprising:
[0057] Step S1: add 100g of isobutylene glycol and 0.3% Na in the total amount of the input to the reactor, replace with nitrogen three times, then heat to 100±5°C, add 345g of alkylene oxide mixture obtained by mixing propylene oxide and pentylene oxide according to a certain mass ratio, control the pressure to less than 0.4Mpa, and after completion, mature until the pressure does not decrease, cool, degas and purify to obtain a low molecular weight polymer with a number average molecular weight of about 400;
[0058] Add 100g of the low molecular weight polymer obtained in step S1 and a multimetal cyanide catalyst with a mass fraction of 0.005% of the total amount of the catalyst to the reactor, replace with nitrogen three times, then heat to 120-130°C, dehydrate for 40 minutes, further heat to 130-140°C, add 3680g of the alkylene oxide mixture obtained by mixing propylene oxide and pentylene oxide in a mass ratio of 5:1 (first add 10-30g, control the pressure to less than 0.6Mpa, add the remaining alkylene oxide after the pressure has clearly decreased), control the pressure to less than 0.4Mpa, mature at a temperature of 145±5°C until the pressure does not decrease, maintain for 20 minutes, cool to 110°C±5°C, degas and discharge, and obtain a polymer resin with a number average molecular weight of 15000; step S2.
[0059] Step S3 includes adding 0.10% of the total amount of dibutyltin dilaurate and 3-isocyanatopropyltrimethoxysilane (OH:NCO=1:1) to the high molecular weight polymer resin produced in step S2, and carrying out a reaction at a temperature of 100°C for 3 hours. During the reaction, the reaction mixture is sampled for an infrared characteristic peak test. When the reaction mixture no longer has an isocyanate infrared characteristic peak, the reaction is terminated to obtain a silane-terminated resin. Example 6
[0060] The only difference between this embodiment and embodiment 5 is that 3680 g of an alkylene oxide mixture obtained after mixing propylene oxide and pentylene oxide according to a mass ratio of 6:1 is added. Example 7
[0061] The only difference between this embodiment and embodiment 5 is that 3680 g of an alkylene oxide mixture obtained after mixing propylene oxide and pentylene oxide according to a mass ratio of 7:1 is added. Example 8
[0062] The only difference between this embodiment and embodiment 5 is that 3680 g of an alkylene oxide mixture obtained after mixing propylene oxide and pentylene oxide according to a mass ratio of 8:1 is added. Comparative Example 2
[0063] The only difference between this example and Example 5 is that 3680 g of propylene oxide was added.
[0064] The products obtained in Examples 5 to 8 and Comparative Example 2 were subjected to liquid phase analysis, and the results are shown in Table 2.
[0065] [Table 2]
[0066] As can be seen from Table 2, the viscosity of the product decreases with an increase in the soft segment. When the ratio of propylene oxide to pentylene oxide is 5:1, the viscosity of the product decreases slightly, which is because with an increase in pentylene oxide, the addition reaction becomes difficult, the molecular distribution coefficient reaches 1.101, and the molecular distribution becomes wider, which increases the viscosity of the resin. Application Example 1
[0067] The silane-terminated resins prepared in Examples 1 to 4, Comparative Example 1, Examples 5 to 8, and Comparative Example 2 were used to prepare sealants in the same manner. The components of the sealant were composed of the following mass percentages. Silane-terminated resin 18% Feeler 50.2% Plasticizer 25% Thixotropic agent 1.2% Stabilizer: 0.6% Silane Auxiliary Agent 4.5% Catalyst 0.5%.
[0068] In the above blended components, the filler is a mixture of nano calcium carbonate and heavy calcium carbonate in a mass ratio of 2:1, the plasticizer is DINP, the thixotropic agent is polyamide wax, the stabilizer is a mixture of antioxidant 1076 and light stabilizer in a mass ratio of 1:1, which is a commercially available common light stabilizer, the silane auxiliary is a mixture of vinyltrimethoxysilane (used amount is 2%) and KH792 (used amount is 2.5%), and the catalyst is dibutylene dilaurate.
[0069] The results of the measurements of the sealant's properties, such as extrudability, tensile properties, and tear strength, are shown in Tables 3 and 4.
[0070] [Table 3]
[0071] As can be seen from Table 3, the extrudability of Examples 1 to 4 is significantly improved compared to Comparative Example 1. The fluidity during application of the silane-terminated resin products prepared in Examples 1 to 4 is improved, and both the tensile modulus and tear strength are improved. This indicates that the internal flexibility of the silane-terminated resin molecule is improved, and the tensile property during application is improved, thereby improving the adhesive mechanical performance of the silane-terminated resin during application.
[0072] [Table 4]
[0073] As can be seen from Table 4, the extrudability of the silane-terminated resins of Examples 5 to 8 improved with increasing amounts of pentylene oxide used. In Comparative Example 2, the extrudability of the silane-terminated resin made with pure propylene oxide was only 302 g / 15 s, the breaking strength was 0.60 MPa, the elongation dropped to 308%, and the tear strength was 14.8 kN / m, which are significantly lower than the silane-terminated resins of Examples 5 to 8 with higher branching of the polyether segment.
[0074] The above embodiments are only preferred embodiments of the present invention, which cannot limit the scope of protection of the present invention, and any insubstantial modifications and replacements made by those skilled in the art based on the present invention belong to the scope of the claims of the present invention.
Claims
1. A silane-terminated resin for low viscosity sealants, the structural formula of which is: 【Chemistry 1】 where "----" means 【Chemistry 2】 The number of repeating units is ≧172, and R is C n H 2n where n=1 to 5, and R 1 is a linear alkyl group C m H 2m+1 m≧1, and in the repeating unit, R 1 The mass ratio of R being a methyl group is 50 to 90%, 2 is CH 3 or CH 2 CH 3 and R 3 is OR 2 Or R 2 1. A silane-terminated resin for low viscosity sealants, comprising:
2. The number average molecular weight of the silane-terminated resin is about 15,000-30,000. The silane-terminated resin for low viscosity sealants according to claim 1.
3. A method for producing the silane-terminated resin for low viscosity sealants according to claim 1 or 2, comprising the steps of: Step S1: add 1 part of an alcohol-based initiator and an alkaline earth metal to a reaction vessel, replace with nitrogen, and then heat to 75-150°C, add 7.5-14.5 parts of an alkylene oxide, control the pressure to 0.0-0.4 MPa, and mature until the pressure does not decrease, and then reduce the temperature, degas and purify to obtain a low molecular weight polymer; Step S2: add 1 part of the low molecular weight polymer obtained in step S1 to the reaction vessel, add 5-15 ppm of a multimetal cyanide catalyst based on the total mass, replace with nitrogen, heat to 120-130°C, dehydrate, heat to 130-140°C, add 250-355 parts of alkylene oxide, control the pressure to 0.0-0.4 MPa, and mature until the pressure does not decrease, cool, degas and discharge to obtain a high molecular weight polymer resin; The method includes the steps of: adding an organotin catalyst and an isocyanate silane to the polymer resin produced in step S2 to carry out a reaction; sampling the reaction mixture during the reaction to carry out an infrared characteristic peak test; and terminating the reaction when the reaction mixture no longer has an isocyanate infrared characteristic peak, thereby obtaining the silane-terminated resin.
4. The alcohol-based initiator in step S1 is one of propylene glycol, isobutylene glycol, and dex-1,3-butylene glycol, the alkaline earth metal is K or Na, and the alkylene oxide in steps S1 and S2 is a mixture of propylene oxide and one of butylene oxide, hexylene oxide, pentylene oxide, and heptalene oxide. A method for producing the silane-terminated resin for low viscosity sealants according to claim 3.
5. The alkylene oxide mixture has a molar ratio of propylene oxide to other alkylene oxides of 1:1 to 10:
1. A method for producing the silane-terminated resin for low viscosity sealants according to claim 4.
6. The number average molecular weight of the low molecular weight polymer produced in step S1 is 400-800. A method for producing the silane-terminated resin for low viscosity sealants according to claim 3.
7. The metal ions contained in the multimetal cyanide catalyst in step S2 are at least two of Co, Zn, and Pb. A method for producing the silane-terminated resin for low viscosity sealants according to claim 3.
8. The dehydration time in step S2 is 30-90 min, the aging temperature is 130-150° C., and the temperature is lowered to 90-110° C., after which the mixture is degassed and discharged. A method for producing the silane-terminated resin for low viscosity sealants according to claim 3.
9. The amount of the organotin catalyst added in step S3 is 0.05 to 0.15% of the total amount added, the organotin catalyst is dibutyltin dilaurate or dioctyltin dilaurate, and the mass ratio of the hydroxyl value of the polymer resin to the NCO of the isocyanate silane in step S3 is OH:NCO=0.98 to 1.02:
1. A method for producing the silane-terminated resin for low viscosity sealants according to claim 3.
10. The reaction temperature in step S3 is 40 to 100° C., and the reaction time is 2 to 10 hours. A method for producing the silane-terminated resin for low viscosity sealants according to claim 3.
Citation Information
Patent Citations
Reactive plasticizer and curable composition containing the same
JP2012229398A
Curable composition
JP2013076094A
Low viscosity silyl-modified polymer
JP2013531723A
Method for preparing mixed silane-terminated polymers
JP2021507051A
Method for preparing reactive sealant resin
JP2022509658A