Polyamide resin composition

The polyamide resin composition with crystalline polyamide, black pigment, and fatty acid metal salt addresses the issues of jet black appearance, scratch resistance, and bleed-out resistance, ensuring high mechanical properties and reduced gas evolution during molding.

JP2024167049AInactive Publication Date: 2024-11-29UNITIKA LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2024046306
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-03-22
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resin compositions for automobile interior parts fail to achieve high-quality jet black appearance, sufficient scratch resistance, and bleed-out resistance, while also experiencing gas evolution during molding.

Method used

A polyamide resin composition comprising 100 parts by mass of crystalline polyamide resin, 0.1 to 1 part by mass of black pigment or dye, and 0.05 to 0.5 parts by mass of a fatty acid metal salt with 23 or more carbon atoms, specifically calcium montanate, is used to enhance mechanical properties, scratch resistance, and jet blackness, while suppressing gas generation during molding.

Benefits of technology

The composition achieves excellent mechanical properties, scratch resistance, and jet blackness, with minimal bleed-out and reduced gas generation, maintaining gloss and color stability under high temperature and humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167049000001
    Figure 2024167049000001
Patent Text Reader

Abstract

To provide a polyamide resin composition with which it is possible to obtain a molded body sufficiently excellent in mechanical characteristics, scratch resistance, and jet blackness.SOLUTION: A polyamide resin composition includes: 100 pts.mass of crystalline polyamide resin (A); 0.1-1 pt.mass of a black pigment and / or a black dye (B); and 0.05-0.5 pt.mass of fatty acid metal salt having a carbon number of 23 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide resin composition. [Background technology]

[0002] Molded articles made of thermoplastic resins such as ABS resins are commonly used for automotive interior parts. Such resin molded articles are required to have excellent mechanical properties, and their appearance is highly required to have a designability, and in some cases, a jet black (piano black) appearance is required.

[0003] In order to meet such requirements, a method of painting a black paint on the surface of a resin molded body (so-called piano black painting) has been used in the past. However, this painting method uses organic solvents, which causes problems in terms of the working environment, and also causes problems of poor productivity and high costs. For this reason, unpainted molded products have been desired in recent years, and replacement with base resins has been actively considered. Base resins are resins that are colored by kneading pigments or dyes into the resin itself. However, there is a problem that unpainted molded products made of base resins are significantly inferior in scratch resistance compared to painted products. To solve this problem, for example, Patent Documents 1 to 3 disclose resin compositions in which an organic modified siloxane compound or the like is blended with a thermoplastic resin. Patent Documents 4 and 5 disclose resin compositions in which a fatty acid metal salt is blended with a thermoplastic resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-158630 A [Patent Document 2] JP 2014-196483 A [Patent Document 3] JP 2018-123277 A [Patent Document 4] JP 2014-234508 A [Patent Document 5] JP 2016-199633 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the resin compositions described in Patent Documents 1 to 3 improve the scratch resistance of the resulting molded product, but do not provide a high-quality jet black color that can be called piano black. In addition, the resin compositions described in Patent Documents 4 and 5 do not provide sufficient scratch resistance in the resulting molded product. Furthermore, conventional resin compositions such as those described in Patent Documents 1 to 5 have problems such as impaired jet black color due to the bleeding out of additives in high-temperature and high-humidity environments and / or generation of gas due to thermal decomposition during molding.

[0006] The present invention has been made to solve the above problems, and has an object to provide a polyamide resin composition which can give a molded article having sufficiently excellent mechanical properties, scratch resistance and jet black color.

[0007] Another object of the present invention is to provide a polyamide resin composition which can give a molded article having sufficiently excellent mechanical properties, scratch resistance, jet blackness and bleed-out resistance, and which can sufficiently suppress gas generation during molding. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above object can be achieved, thereby completing the present invention.

[0009] The gist of the present invention is as follows. <1> A polyamide resin composition comprising: 100 parts by mass of a crystalline polyamide resin (A); 0.1 to 1 part by mass of a black pigment and / or black dye (B); and 0.05 to 0.5 parts by mass of a fatty acid metal salt having 23 or more carbon atoms (C). <2> The fatty acid metal salt (C) is calcium montanate. <1> The polyamide resin composition according to claim 1. <3> The crystalline polyamide resin (A) is polyamide 6 alone or a mixture of polyamide 6 and a polyamide mainly composed of a diamine having 6 or more carbon atoms and a dicarboxylic acid having 10 or more carbon atoms, and the content of the polyamide mainly composed of a diamine having 6 or more carbon atoms and a dicarboxylic acid having 10 or more carbon atoms in the crystalline polyamide resin (A) is 30 mass% or less. <1> or <2> The polyamide resin composition according to claim 1. <4> A wearer having a square test surface with one side of 20 mm of glass beads corresponding to a particle size F54 specified in JIS R 6001-1 attached thereto is placed on a plate-shaped molded product obtained by injection molding the polyamide resin composition, and after applying a load of 21.6 N and reciprocating 50 times, the gloss retention based on the following formula at an incidence angle of 20° is 85% or more. <1> ~ <3> 2. The polyamide resin composition according to claim 1 . Gloss retention rate (%) = (surface gloss after abrasion test) / (surface gloss before abrasion test) x 100 <5> The L* value of a plate-shaped molded product obtained by injection molding the polyamide resin composition according to the SCE method defined in JIS Z 8781-4 is 3 or less. <1> ~ <4> 2. The polyamide resin composition according to claim 1 . <6> The content of the fatty acid metal salt (C) is 0.2 to 0.5 parts by mass. <1> ~ <5> 2. The polyamide resin composition according to claim 1 . <7> the crystalline polyamide resin (A) is polyamide 6 alone or a mixture of polyamide 6 and polyamide 610, and the content of polyamide 610 in the crystalline polyamide resin (A) is 30 mass% or less; the black pigment and / or black dye (B) is a black pigment, and the content of the black pigment is 0.3 to 0.8 parts by mass; The fatty acid metal salt (C) is calcium montanate, and the content of calcium montanate is 0.1 to 0.45 parts by mass. <1> ~ <6> 2. The polyamide resin composition according to claim 1 . <8> <1> ~ <7> A molded article comprising the polyamide resin composition according to any one of claims 1 to 5. Effect of the Invention

[0010] According to the present invention, it is possible to provide a polyamide resin composition which gives a molded article having sufficiently excellent mechanical properties, as well as sufficiently excellent scratch resistance and jet blackness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The polyamide resin composition of the present invention contains a crystalline polyamide resin (A), a black pigment and / or a black dye (B), and a fatty acid metal salt (C).

[0012] Crystallinity means that the heat of fusion measured using a differential scanning calorimeter (DSC) at a heating rate of 20°C / min under a nitrogen atmosphere is greater than 1 J / g (particularly 10 J / g or more, preferably 30 J / g or more, more preferably 50 J / g or more, and more preferably 70 J / g or more). The term "amorphous" means that the value of the heat of fusion measured by a differential scanning calorimeter (DSC) at a heating rate of 20° C. / min in a nitrogen atmosphere is 1 J / g or less. When the polyamide resin composition of the present invention contains an amorphous polyamide resin instead of a crystalline polyamide resin, the scratch resistance decreases.

[0013] The crystalline polyamide resin (A) used in the present invention is not particularly limited as long as it has crystallinity, and examples thereof include polycaproamide (polyamide 6), polytetramethylene adipamide (polyamide 46), polypentamethylene adipamide (polyamide 56), polyhexamethylene adipamide (polyamide 66), polypentamethylene sebamide (polyamide 510), polyhexamethylene sebamide (polyamide 610), polyhexamethylene Examples of the polymers include decamide (polyamide 612), polycaproamide / polyhexamethylene adipamide copolymer (polyamide 6 / 66), polyundecamide (polyamide 11), polycaproamide / polyundecamide copolymer (polyamide 6 / 11), polydodecamide (polyamide 12), polycaproamide / polydodecamide copolymer (polyamide 6 / 12), and mixtures thereof, or copolymers thereof. Among them, from the viewpoint of further improving scratch resistance and improving bleed-out resistance, it is preferable that the polyamide resin (A) is polyamide 6 alone or a mixture of polyamide 6 and a polyamide (hereinafter sometimes referred to as "polyamide a1") mainly composed of a diamine having 6 or more carbon atoms and a dicarboxylic acid having 10 or more carbon atoms. The mixture is more preferably a mixture of polyamide 6 and polyamide 610.

[0014] In this specification, the mechanical properties refer to properties that enable a molded article produced from the polyamide resin composition of the present invention to exhibit greater tensile strength. The scratch resistance refers to the property that the surface of a molded article produced from the polyamide resin composition of the present invention is less susceptible to scratching, and more specifically, refers to the property that the surface gloss of the molded article surface is maintained to a higher degree even after abrasion treatment compared to before the abrasion treatment. The jet blackness refers to the property that a molded article produced from the polyamide resin composition of the present invention has a darker color, and more specifically, refers to the property that the surface of the molded article has a smaller L* value. Bleed-out resistance refers to the property of a molded article produced from the polyamide resin composition of the present invention that suppresses bleed-out even in a high-temperature, high-humidity environment and exhibits better jet-black color; more specifically, it refers to the property that the surface of the molded article exhibits a smaller L* value even after exposure to a high-temperature, high-humidity environment. The molding gas suppression property refers to the property of suppressing gas generation when a molded article is produced from the polyamide resin composition of the present invention, and more specifically, refers to the property of generating less gas during injection molding. Among these properties, the mechanical properties, scratch resistance and jet blackness are properties that the polyamide resin composition of the present invention has. The bleed-out resistance and molding gas suppression properties are not necessarily properties that the polyamide resin composition of the present invention must have, but are properties that it is preferable for the composition to have.

[0015] Polyamide a1 is a polyamide containing a diamine component and a dicarboxylic acid component as monomer components, and contains the diamine having 6 or more carbon atoms in an amount of 60 mol % or more based on the total amount of the diamine components, and contains the dicarboxylic acid having 10 or more carbon atoms in an amount of 60 mol % or more based on the total amount of the dicarboxylic acid components.

[0016] Examples of diamines having 6 or more carbon atoms include hexamethylenediamine, octamethylenediamine, decamethylenediamine, and dodecamethylenediamine. Among these diamines, the carbon number of the diamine is preferably 6 to 10, more preferably 6 to 8, and even more preferably 6. The diamine may be an aliphatic diamine, an aromatic diamine, or an alicyclic diamine, and from the viewpoint of further improving scratch resistance, an aliphatic diamine is preferred. From the viewpoint of further improving scratch resistance, the content of the diamine having 6 or more carbon atoms in the polyamide a1 is preferably 70 mol % or more, more preferably 90 mol % or more, and even more preferably 100 mol % based on the total amount of the diamine components. The polyamide a1 may contain a diamine having 5 or less carbon atoms (e.g., pentamethylenediamine, tetramethylenediamine, etc.) as a diamine component. The content of diamines having 5 or less carbon atoms in polyamide a1 is usually 40 mol % or less based on the total amount of diamine components, and from the viewpoint of further improving scratch resistance, it is preferably 30 mol % or less, more preferably 10 mol % or less, and even more preferably 0 mol %. The carbon number of the diamine is the number of all carbon atoms constituting the diamine.

[0017] Examples of dicarboxylic acids having 10 or more carbon atoms include sebacic acid, undecanedioic acid, and dodecanedioic acid. Among these dicarboxylic acids, the carbon number of the dicarboxylic acid is preferably 10 to 14, more preferably 10 to 12, and even more preferably 10. The dicarboxylic acid may be an aliphatic dicarboxylic acid, an aromatic dicarboxylic acid, or an alicyclic dicarboxylic acid, and from the viewpoint of further improving scratch resistance, an aliphatic dicarboxylic acid is preferred. From the viewpoint of further improving scratch resistance, the content of the dicarboxylic acid having 10 or more carbon atoms in the polyamide a1 is preferably 70 mol % or more, more preferably 90 mol % or more, and even more preferably 100 mol % based on the total amount of the dicarboxylic acid component. The polyamide a1 may contain a dicarboxylic acid having 9 or less carbon atoms (e.g., azelaic acid, suberic acid, pimelic acid, etc.) as a dicarboxylic acid component. The content of dicarboxylic acid having 9 or less carbon atoms in polyamide a1 is usually 40 mol % or less based on the total amount of dicarboxylic acid components, and from the viewpoint of further improving scratch resistance, it is preferably 30 mol % or less, more preferably 10 mol % or less, and even more preferably 0 mol %. The carbon number of the dicarboxylic acid is the number of all carbon atoms constituting the dicarboxylic acid, and includes, for example, the number of carbon atoms constituting the carboxyl group.

[0018] From the viewpoint of further improving scratch resistance, polyamide a1 is preferably polyamide 610.

[0019] When a mixture of polyamide 6 and polyamide a1 is used as the crystalline polyamide resin (A), the content of polyamide a1 in the crystalline polyamide resin (A) is preferably more than 0% by mass and not more than 30% by mass (particularly 5 to 30% by mass), more preferably 10 to 30% by mass, from the viewpoint of further improving mechanical properties and scratch resistance. By using the above polyamide mixture, scratch resistance can be further improved.

[0020] When the crystalline polyamide resin (A) is polyamide 6 alone or a mixture of polyamide 6 and polyamide a1, the content of polyamide a1 in the crystalline polyamide resin (A) is preferably 30 mass% or less (particularly 0 to 30 mass%), more preferably 20 mass% or less (particularly 0 to 20 mass%), even more preferably 15 mass% or less (particularly 0 to 15 mass%), and particularly preferably 8 to 15 mass%, from the viewpoint of the balance between scratch resistance and jet blackness.

[0021] The relative viscosity, which is an index of the molecular weight of the crystalline polyamide resin (A), is not particularly limited, but from the viewpoint of further improving mechanical properties and scratch resistance, as well as improving bleed-out resistance and molding gas suppression properties, the relative viscosity measured using 96% by mass concentrated sulfuric acid as a solvent under conditions of a temperature of 25°C and a concentration of 1 g / dl is preferably 2.0 to 4.0, more preferably 2.5 to 3.5. When the crystalline polyamide resin (A) contains two or more kinds of crystalline polyamide resins, it is preferable that the relative viscosity of each crystalline polyamide resin is within the above range.

[0022] The proportion of the crystalline polyamide resin (A) relative to the total amount of the polyamide resin composition of the present invention is usually 60% by mass or more, and from the viewpoints of further improving the mechanical properties, scratch resistance and jet blackness, as well as improving the bleed-out resistance and molding gas suppression properties, it is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0023] The present invention does not preclude the polyamide resin composition from containing an amorphous polyamide resin. The content of the amorphous polyamide resin is usually 10 parts by mass or less relative to 100 parts by mass of the crystalline polyamide resin (A), and from the viewpoint of further improving mechanical properties, scratch resistance and jet blackness, and improving bleed-out resistance and molding gas suppression properties, it is preferably 5 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0 part by mass.

[0024] The polyamide resin composition of the present invention must contain a black pigment and / or a black dye (B). If the polyamide resin composition does not contain a black pigment and / or a black dye (B), the jet blackness and bleed-out resistance are reduced. The polyamide resin composition of the present invention preferably contains a black pigment from the viewpoint of further improving the mechanical properties, scratch resistance, and jet blackness, as well as improving the bleed-out resistance and molding gas suppression properties. The black pigment is not particularly limited, but examples thereof include carbon black, acetylene black, lamp black, bone black, graphite, iron black, aniline black, cyanine black, and titanium black. Among these, carbon black is preferred because it can easily achieve the effects of the present invention. The black dye is not particularly limited, but examples thereof include azine dyes containing nigrosine and polycyclic condensation dyes containing anthraquinone. Among these, azine dyes are preferred because they are easy to handle. Examples of commercially available azine dyes include NYB27620B (manufactured by Sanyo Kako Co., Ltd.), Orient Spirit Black SB (manufactured by Orient Chemical Industries Co., Ltd.), Spirit Black No. 850 (manufactured by Sumitomo Chemical Co., Ltd.), and Nigrosine Base LK (manufactured by BASF). The black pigment or black dye (B) may be used alone or in combination.

[0025] Among the azine dyes, nigrosine is more preferred. Examples of nigrosine include black azine condensation mixtures such as those described in COLOR INDEX as CISOLVENT BLACK 5 and CISOLVENT BLACK 7. Such nigrosine can be synthesized, for example, by oxidizing and dehydrating condensation of aniline, aniline hydrochloride, and nitrobenzene in the presence of iron chloride at a reaction temperature of 160 to 180°C. As the azine dye, purified nigrosine obtained by purifying the nigrosine thus obtained to have aniline and diphenylamine content of less than 0.1% is more preferred. Examples of commercially available nigrosine include Cramity 81 and NUBIAN BLACK series manufactured by Orient Chemical Industry Co., Ltd.

[0026] The content of the black pigment and / or black dye (B) is required to be 0.1 to 1 part by mass, preferably 0.3 to 0.8 parts by mass, and more preferably 0.3 to 0.6 parts by mass, relative to 100 parts by mass of the crystalline polyamide resin (A). If the content of the black pigment and / or black dye (B) is less than 0.1 part by mass, the jet blackness of the resulting molded product is insufficient, which is not preferable. In addition, the bleed-out resistance decreases. On the other hand, if the content exceeds 1 part by mass, a large amount of decomposition gas is generated during molding, which is not preferable because the jet blackness and tensile strength decrease. When two or more kinds of black pigments and / or black dyes (B) are contained, the total content thereof may be within the above range.

[0027] The polyamide resin composition of the present invention must contain a fatty acid metal salt (C) having 23 or more carbon atoms. In the case of an aliphatic metal salt having 22 or less carbon atoms, scratch resistance is not sufficiently expressed in the obtained molded product, and therefore it is not preferred. Examples of fatty acids in the fatty acid metal salt having 23 or more carbon atoms include tricosyl acid (having 23 carbon atoms), lignoceric acid (having 24 carbon atoms), cerotic acid (having 26 carbon atoms), and montanic acid (having 28 carbon atoms). Among these fatty acids, the carbon number of the fatty acid is preferably 23 to 40, more preferably 25 to 30, and even more preferably 27 to 29. Among these, montanic acid is preferred from the viewpoints of further improving mechanical properties, scratch resistance, and jet blackness, as well as bleed-out resistance, molding gas suppression properties, and thermal stability. Examples of metals in the fatty acid metal salt include sodium, magnesium, aluminum, calcium, and zinc. Among these, calcium is preferred from the viewpoint of further improving bleed-out resistance. The carbon number of a fatty acid metal salt is the number of carbon atoms of the fatty acid constituting the fatty acid metal salt, and includes, for example, the number of carbon atoms constituting the carboxyl group.

[0028] The content of the fatty acid metal salt (C) is required to be 0.05 to 0.5 parts by mass, preferably 0.1 to 0.5 parts by mass, more preferably 0.1 to 0.45 parts by mass, and even more preferably 0.2 to 0.5 parts by mass, relative to 100 parts by mass of the crystalline polyamide resin (A). If the content of the fatty acid metal salt (C) is less than 0.05 parts by mass, the scratch resistance of the obtained molded product is not sufficiently expressed, which is not preferable. On the other hand, if the content exceeds 0.5 parts by mass, the scratch resistance is not improved, and a large amount of decomposition gas is generated during molding, which reduces the L* value and tensile strength, which is not preferable. When two or more kinds of fatty acid metal salts (C) are contained, the total content thereof may be within the above range.

[0029] Additives such as heat stabilizers, plasticizers, lubricants, release agents, and antistatic agents can be added to the polyamide resin composition of the present invention, so long as they do not significantly impair its properties. The total content of such additives in the polyamide resin composition of the present invention is not particularly limited, and may be, for example, 20 parts by mass or less (i.e., 0 to 20 parts by mass) relative to 100 parts by mass of the crystalline polyamide resin (A), and may be particularly 10 parts by mass or less (i.e., 0 to 10 parts by mass). The method of mixing these additives in the polyamide resin composition of the present invention is not particularly limited. For example, these additives may be mixed with the amorphous polyamide resin (A), the black pigment and / or black dye (B), and the fatty acid metal salt (C) by blending, or may be mixed with the components (A) to (C) by melt kneading.

[0030] In the present invention, the polyamide resin composition can be produced by melt-kneading a crystalline polyamide resin (A), a black pigment and / or a black dye (B), and a fatty acid metal salt (C). Therefore, the polyamide resin composition of the present invention may be in the form of pellets obtained by melt-kneading a blend mixture containing those components (A) to (C).

[0031] When producing a molded article using the polyamide resin composition of the present invention, the production method (molding method) is not particularly limited, and examples thereof include injection molding and extrusion molding. As an example, when the injection molding method is adopted, the injection molding conditions suitable for the polyamide resin composition of the present invention include a cylinder temperature of the melting point or flow start temperature of the resin composition or higher, preferably 220 to 270°C, and a mold temperature of "melting point of the resin composition - 20"°C or lower. If the molding temperature is too low, the moldability may become unstable, such as short circuits occurring in the molded article, or the gloss of the surface of the obtained molded article may be lost. On the other hand, if the molding temperature is too high, the polyamide resin composition may decompose, which may cause the strength of the obtained molded article to decrease or the gloss to decrease.

[0032] The melting point of the resin composition means the melting point of the polyamide resin composition, and a value measured by the following method is used. Using a differential scanning calorimeter, 5 mg of the sample was heated to 350° C. at a heating rate of 20° C. / min in a nitrogen atmosphere, and the melting peak was measured, and this temperature was taken as the melting point.

[0033] The molded article of the polyamide resin composition of the present invention usually has a gloss retention rate of 85% or more, preferably 87% or more, and more preferably 90% or more after an abrasion test. The abrasion test is a test in which an abrasive having glass beads corresponding to the particle size F54 specified in JIS R 6001-1 attached to a square test surface with a side length of 20 mm is placed on the molded article, and a load of 21.6 N is applied and the abrasive is run back and forth 50 times. The gloss retention rate is the gloss retention rate based on the following formula for the surface gloss at an incidence angle of 20°. Gloss retention rate (%) = (surface gloss after abrasion test) / (surface gloss before abrasion test) x 100

[0034] The molded article of the polyamide resin composition of the present invention also has an L* value, as determined by the SCE method defined in JIS Z 8781-4, of usually 3 or less, preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.7 or less.

[0035] The molded article of the polyamide resin composition of the present invention, after being left to stand for 1000 hours in a high-temperature and high-humidity environment of 70°C and 62% RH, usually has an L* value of 3 or less, preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.7 or less, as measured by the SCE method specified in JIS Z 8781-4.

[0036] The polyamide resin composition of the present invention has excellent mechanical properties, as well as excellent scratch resistance and jet-black color in the obtained molded article, and can therefore be suitably used for automobile interiors, home appliances, and parts of electric and electronic products, etc. EXAMPLES

[0037] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0038] 1. Evaluation method (1) Heat of fusion of crystalline polyamide resin (A) Using a Hitachi High-Tech Science DSC7020 differential scanning calorimeter, 5 mg of the sample was heated to 350° C. at a heating rate of 20° C. / min in a nitrogen atmosphere, and the heat of fusion was calculated from the area of ​​the melting peak.

[0039] (2) Preparation of test specimens <Test piece 1> The obtained polyamide resin composition was subjected to injection molding in an injection molding machine (Toshiba Machine Co., Ltd., EC-100II type) under the conditions of resin temperature 260°C, mold temperature 80°C, holding pressure 30 MPa, injection speed 50 mm / s, injection pressure 100 MPa, and cooling time 10 seconds to obtain a plate-shaped molded body (test piece 1) having a length of 90 mm, a width of 50 mm, and a thickness of 2 mm. The mold used was polished with a polishing grit of 8000.

[0040] <Test piece 2> The obtained polyamide resin composition was subjected to injection molding in an injection molding machine (Toshiba Machine Co., Ltd., EC-100II type) under the conditions of a resin temperature of 260°C, a mold temperature of 80°C, a holding pressure of 30 MPa, an injection speed of 50 mm / s, an injection pressure of 100 MPa, and a cooling time of 10 seconds to obtain an ISO multipurpose test piece (test piece 2).

[0041] (3) Scratch resistance Based on JIS Z8741, the surface gloss of the test piece 1 was measured at an incidence angle of 20° using a gloss meter (Nippon Denshoku Industries Co., Ltd., Model PG-IIM gloss meter). Next, using a Gakushin abrasion tester (manufactured by Yasuda Seiki Seisakusho), an abrasive with a Potters Ballotini glass bead J-54 attached was applied with a load of 21.6 N and made 50 passes back and forth on test piece 1 (abrasion test). The surface gloss at an incidence angle of 20° was measured after the test in the same manner as before the test. The gloss retention was calculated based on the following formula: Gloss retention rate (%) = (surface gloss after abrasion test) / (surface gloss before abrasion test) x 100 The gloss retention, which is an index of scratch resistance, was evaluated according to the following criteria. ◎: 90% or more (good); ○: 85% or more but less than 90% (no problem in practical use); ×: Less than 85% (problems in practical use)

[0042] (4) Jet black Based on JIS Z 8781-4, the L* value of the test piece 1 was measured using a spectrophotometer (Konica Minolta CM-3700A type) by the SCE method (10° visual field, D65 light source). The L* value, which is an index of jet blackness, was evaluated according to the following criteria. ◎: 2 or less (good); ○: More than 2 and 3 or less (no problem in practical use); ×: More than 3 (problems in practical use)

[0043] (5) Mechanical properties The tensile strength was measured using test piece 2 based on ISO178. The tensile strength, which is an index of mechanical properties, was evaluated according to the following criteria. ◎: 75MPa or more (good); ×: Less than 75MPa (problems in practical use)

[0044] (6) Amount of gas generated during molding The amount of gas generated during molding of Test Piece 1 and Test Piece 2 was visually observed and evaluated according to the following criteria. ◎: The amount of generation is extremely small (good); ○: The amount of generation is small (no practical problem); ×: Large amount of generation (problems in practical use)

[0045] (7) Bleed-out resistance in high temperature and humidity environments Test piece 2 was placed in a thermo-hygrostat at 70°C x 62%RH, and after 1000 hours, the L* value of test piece 1 was measured using a spectrophotometer (Konica Minolta CM-3700A) according to JIS Z 8781-4, using the SCE method (10° field of view, D65 light source). The L* value, which is an index of jet blackness, was evaluated according to the following criteria. ◎: 2 or less (good); ○: More than 2 and 3 or less (no problem in practical use); ×: More than 3 (problems in practical use)

[0046] (8) Overall rating Among the evaluation results of the above-mentioned scratch resistance, mechanical properties, jet blackness, mechanical properties, amount of gas generated during molding, and bleed-out resistance in a high-temperature, high-humidity environment, the lower evaluation result was used as the overall judgment result.

[0047] 2.Raw materials (1) Polyamide resin A1: Polyamide 6 resin (Unitika "A1030BRF-BA"), melting point 225°C, relative viscosity 3.1, heat of fusion 70J / g A2: Polyamide 610 resin (Arkema "SMVO F"), melting point 229°C, relative viscosity 2.6, heat of fusion 72 J / g A3: Polyamide 510 resin (CATHAY "E-3100"), melting point 221°C, relative viscosity 2.6, heat of fusion 68J / g A4: Polyamide 6T / 6I resin (EMS "G21"), no melting point, relative viscosity 2.0, heat of fusion less than 1 J / g

[0048] (2) Black pigment B1: Carbon black (Columbia "Raven5000")

[0049] (3) Black dye B2: Nigrosine (Orient Chemical Industries "Cramity81")

[0050] (4) Metal salts of fatty acids C1: Calcium montanate (carbon number 28) ("CS-8CP" manufactured by Nitto Kasei Kogyo Co., Ltd.) C2: Sodium montanate (carbon number 28) ("NS-8" manufactured by Nitto Kasei Kogyo Co., Ltd.) C3: Sodium behenate (carbon number 22) ("NS-7" manufactured by Nitto Kasei Kogyo Co., Ltd.) C4: Magnesium stearate (carbon number 18) ("Mg-St" manufactured by Nitto Kasei Kogyo Co., Ltd.)

[0051] (5) Other additives D1: Organic modified siloxane compound (Evonik Industries "TEGOMER AntiScratch 100") D2: Silicone compound (Toray Dow Corning "BY27-219")

[0052] Example 1 100 parts by mass of crystalline polyamide resin (A1), 0.1 parts by mass of black pigment (B1), and 0.2 parts by mass of fatty acid metal salt (C1) were mixed together, fed into the main hopper of a twin-screw extruder, melt-kneaded, extruded into strands from a die, cooled, and pelletized to obtain polyamide resin composition pellets. The melt-kneading was performed at a resin temperature of 260°C, a screw rotation of 300 rpm, and a discharge rate of 30 kg / h. The obtained polyamide resin composition was used to prepare test pieces, which were then subjected to various evaluations. The results are shown in Table 1.

[0053] Examples 2 to 14, Comparative Examples 1 to 9 Polyamide resin composition pellets were obtained in the same manner as in Example 1, except that the components were blended in the amounts shown in Table 1, and further injection molding was carried out.

[0054] The resin composition of the resulting polyamide resin composition and its evaluation results are shown in Table 1.

[0055] [Table 1]

[0056] The polyamide resin compositions of Examples 1 to 14 satisfied all of the requirements of the present invention, and therefore were excellent in mechanical properties, scratch resistance and jet black color.

[0057] In the polyamide resin composition of Comparative Example 1, the polyamide resin (A) was an amorphous resin having a heat of fusion of less than 1 J / g, and therefore the gloss retention after the scratch test was less than 85%. The polyamide resin composition of Comparative Example 2 contained neither a black pigment nor a black dye, and therefore had an L* value of more than 3.0. The polyamide resin composition of Comparative Example 3 had an excessive black pigment content, so that a large amount of gas was generated during molding, the L* value exceeded 3.0, and the tensile strength fell below 75 MPa. The polyamide resin composition of Comparative Example 4 did not contain a fatty acid metal salt, and therefore the gloss retention after the scratch test was less than 85%. The polyamide resin composition of Comparative Example 5 had an excessive fatty acid metal salt content, and therefore generated a large amount of gas during molding, resulting in an L* value exceeding 3.0 and a tensile strength below 75 MPa. The polyamide resin compositions of Comparative Examples 6 and 7 did not contain a fatty acid metal salt having 23 or more carbon atoms, and therefore had a gloss retention rate of less than 85% after the scratch test. The polyamide resin compositions of Comparative Examples 8 and 9 contained a siloxane-based sliding agent, and therefore had an L* value of more than 3.0. [Industrial Applicability]

[0058] The polyamide resin composition of the present invention is useful for producing automobile interior parts, home appliances, electric and electronic products, or parts thereof.

Claims

1. A polyamide resin composition comprising: 100 parts by mass of a crystalline polyamide resin (A); 0.1 to 1 part by mass of a black pigment and / or black dye (B); and 0.05 to 0.5 parts by mass of a fatty acid metal salt having 23 or more carbon atoms (C).

2. The polyamide resin composition according to claim 1, wherein the fatty acid metal salt (C) is calcium montanate.

3. 3. The polyamide resin composition according to claim 1 or 2, wherein the crystalline polyamide resin (A) is polyamide 6 alone or a mixture of polyamide 6 and a polyamide mainly composed of a diamine having 6 or more carbon atoms and a dicarboxylic acid having 10 or more carbon atoms, and the content of the polyamide mainly composed of a diamine having 6 or more carbon atoms and a dicarboxylic acid having 10 or more carbon atoms in the crystalline polyamide resin (A) is 30 mass% or less.

4. 3. The polyamide resin composition according to claim 1, wherein an abrasive having glass beads corresponding to a particle size F54 specified in JIS R 6001-1 attached to a square test surface with one side of 20 mm is placed on a plate-shaped molded product obtained by injection molding the polyamide resin composition, and the abrasive is subjected to a load of 21.6 N and then reciprocated 50 times, and the gloss retention based on the following formula at an incident angle of 20° is 85% or more. Gloss retention (%)=(surface gloss after abrasion test) / (surface gloss before abrasion test)×100

5. 3. The polyamide resin composition according to claim 1, wherein the L* value of a plate-shaped molded article obtained by injection molding the polyamide resin composition is 3 or less according to the SCE method defined in JIS Z 8781-4.

6. 3. The polyamide resin composition according to claim 1, wherein the content of the fatty acid metal salt (C) is 0.2 to 0.5 parts by mass.

7. the crystalline polyamide resin (A) is polyamide 6 alone or a mixture of polyamide 6 and polyamide 610, and the content of polyamide 610 in the crystalline polyamide resin (A) is 30 mass% or less; The black pigment and / or black dye (B) is a black pigment, and the content of the black pigment is 0.3 to 0.8 parts by mass; 2. The polyamide resin composition according to claim 1, wherein the fatty acid metal salt (C) is calcium montanate, and the content of calcium montanate is 0.1 to 0.45 parts by mass.

8. A molded article comprising the polyamide resin composition according to claim 1.

Citation Information

Patent Citations

  • Polyamide resin composition

    JP2005162821A

  • Polyamide resin composition and molded body

    JP2017014388A

  • Polyamide resin composition, molding and article

    JP2018203964A

  • Resin composition, kit, method for producing molded product and molded product

    JP2019006839A

  • Polyamide resin composition and molded body

    JP2020041163A