Semiconductor device
A semiconductor device with a controlled layered structure and impurity-minimized manufacturing process addresses carrier concentration issues, enhancing electrical performance and reliability for high-power applications.
Patent Information
- Application Number
- JP2024152000
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing semiconductor devices using oxide semiconductors face challenges in achieving good electrical characteristics, reliability, and suitability for high-power applications due to issues with carrier concentration and impurity incorporation.
A semiconductor device is designed with a specific layered structure involving conductors, insulators, and metal oxides, where the carrier concentration is carefully controlled to enhance electrical performance, and impurities like hydrogen and nitrogen are minimized through controlled film formation and heat treatment in a multi-chamber apparatus to maintain high purity and crystallinity.
The solution provides a semiconductor device with improved electrical characteristics, high reliability, and suitability for high-power applications by optimizing carrier concentration and reducing impurities, resulting in stable and efficient transistor operation.
Smart Images

Figure 2024167385000001_ABST
Abstract
Description
[Technical field]
[0001] 1. Field of the Invention An embodiment of the present invention relates to a transistor, a semiconductor device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device. Another embodiment of the present invention relates to a semiconductor wafer and a module.
[0002] In this specification and the like, a semiconductor device refers to any device that can function by utilizing semiconductor characteristics. Semiconductor elements such as transistors, semiconductor circuits, arithmetic devices, and memory devices are all embodiments of semiconductor devices. Display devices (such as liquid crystal display devices and light-emitting display devices), projection devices, lighting devices, electro-optical devices, power storage devices, memory devices, semiconductor circuits, imaging devices, electronic devices, and the like may be considered to include semiconductor devices.
[0003] Note that one aspect of the present invention is not limited to the above technical field. One aspect of the invention disclosed in the present specification etc. relates to an object, a method, or a manufacturing method. Another aspect of the present invention relates to a process, a machine, a manufacture, or a composition of matter. [Background technology]
[0004] Technology that uses semiconductor thin films formed on substrates to construct transistors has been attracting attention. Such transistors are widely used in electronic devices such as integrated circuits (ICs) and image display devices (also simply referred to as display devices). There are also so-called power transistors that are used in power circuits for power applications. Silicon-based semiconductor materials are widely known as semiconductor thin films that can be used in transistors, but oxide semiconductors are also attracting attention as other materials.
[0005] In oxide semiconductors, c-axis aligned crystalline (CAAC) structures and nanocrystalline (nc) structures, which are neither single crystal nor amorphous, have been found (see Non-Patent Documents 1 and 2).
[0006] Non-Patent Documents 1 and 2 disclose techniques for manufacturing a transistor using an oxide semiconductor having a CAAC structure. [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] S. Yamazaki et al., “SID Symposium Digest of Technical Papers”, 2012, volume 43, issue 1, p.183-186 [Non-Patent Document 2] S. Yamazaki et al., “Japanese Journal of Applied Physics”, 2014, volume 53, Number 4S, p.04ED18-1-04ED18-10 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of one embodiment of the present invention is to provide a semiconductor device having favorable electrical characteristics. Another object of one embodiment of the present invention is to provide a semiconductor device for high power applications. Another object of one embodiment of the present invention is to provide a semiconductor device with favorable reliability.
[0009] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these will become apparent from the description of the specification, drawings, claims, etc., and it is possible to extract problems other than these from the description of the specification, drawings, claims, etc. [Means for solving the problem]
[0010] One aspect of the present invention includes a substrate, a first conductor on the substrate, a first metal oxide on the first conductor, a first oxide on the first metal oxide, a second oxide on the first oxide, a first insulator on the second oxide, a second conductor on the first insulator, a second insulator on the second conductor, a third insulator in contact with a side of the second conductor, a side of the first insulator, and a side of the second insulator, a second metal oxide on the second oxide, on the second insulator, and on the third insulator, and a second metal oxide on the second oxide, on the second insulator, and on the third insulator. and a third conductor on the metal oxide, wherein the second conductor has a region overlapping with the second oxide, the third conductor has a region in contact with the second metal oxide, the second metal oxide has a region in contact with the second oxide, the carrier concentration of the second oxide is lower than the carrier concentration of the first oxide, the carrier concentration of the first metal oxide is higher than the carrier concentration of the first oxide, and the carrier concentration of the second metal oxide is higher than the carrier concentration of the first oxide.
[0011] Also, one embodiment of the present invention has a substrate, a first conductor on the substrate, a first metal oxide on the first conductor, a first oxide on the first metal oxide, a second oxide on the first oxide, a second metal oxide on the second oxide, a first insulator on the second oxide, a second conductor on the first insulator, a second insulator on the second metal oxide, on the first insulator, and on the second conductor, and a third conductor on the second metal oxide and on the second insulator, wherein the second oxide and the second metal oxide are The semiconductor device has an opening, a first insulator contacts the sides and bottom of the opening, a second conductor has a region overlapping with a second oxide, a third conductor has a region in contact with a second metal oxide, the second metal oxide has a region in contact with the second oxide, a carrier concentration of the second oxide is lower than a carrier concentration of the first oxide, a carrier concentration of the first metal oxide is higher than a carrier concentration of the first oxide, and a carrier concentration of the second metal oxide is higher than a carrier concentration of the first oxide.
[0012] In the above, the first oxide and the second oxide preferably contain In, an element M (M is Al, Ga, Y, or Sn), and Zn.
[0013] In the above, the first metal oxide and the second metal oxide preferably contain one or more of Sn, W, Ti, and Si, and In.
[0014] Another embodiment of the present invention is a method for manufacturing a semiconductor device, comprising the steps of forming a first conductor over a substrate, forming a first metal oxide over the first conductor, forming the first oxide over the first metal oxide, forming a second oxide over the first oxide, forming a second metal oxide over the second oxide, forming openings in the second metal oxide and the second oxide by lithography, forming a first insulating film over the second metal oxide and in the openings, forming a first conductive film over the first insulating film, and polishing the first insulating film and the first conductive film by CMP until they reach a surface of the second metal oxide to form a first insulator and a second conductor buried in the openings, forming a second insulator in contact with the second metal oxide, the first insulator, and the second conductor, and forming a third conductor over the second metal oxide and the second insulator.
[0015] In the above, it is preferable that the first conductive film, the first metal oxide, the first oxide, and the second oxide are successively formed under reduced pressure using an apparatus having a plurality of treatment chambers. Effect of the Invention
[0016] According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. According to another embodiment of the present invention, a semiconductor device for high power applications can be provided. According to another embodiment of the present invention, a semiconductor device with favorable reliability can be provided.
[0017] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not need to have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract effects other than these from the description in the specification, drawings, claims, etc. [Brief description of the drawings]
[0018] [Figure 1] 1A and 1B are cross-sectional views of a semiconductor device according to an embodiment of the present invention. [Diagram 2] Fig. 2A is a top view of a semiconductor device according to one embodiment of the present invention, and Fig. 2B and Fig. 2C are cross-sectional views of the semiconductor device according to one embodiment of the present invention. [Diagram 3] Fig. 3A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and Fig. 3B and Fig. 3C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 4] Fig. 4A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and Fig. 4B and Fig. 4C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Diagram 5] Fig. 5A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and Fig. 5B and Fig. 5C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 6] Fig. 6A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and Fig. 6B and Fig. 6C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 7] Fig. 7A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and Fig. 7B and Fig. 7C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 8] 8A is a top view illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention, and FIGS. 8B and 8C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 9] Fig. 9A is a diagram for explaining the classification of the crystal structure of IGZO, which is one embodiment of the present invention. Fig. 9B is a diagram for explaining the XRD spectrum of a CAAC-IGZO film, which is one embodiment of the present invention. Fig. 9C is a diagram for explaining the ultrafine electron beam diffraction pattern of a CAAC-IGZO film, which is one embodiment of the present invention. [Figure 10] FIG. 10 is a top view illustrating an example of an apparatus for manufacturing a semiconductor device of one embodiment of the present invention. [Figure 11] Fig. 11A is a flow chart showing a manufacturing process of a semiconductor device according to one embodiment of the present invention, and Fig. 11B is a perspective view showing a semiconductor device according to one embodiment of the present invention. [Figure 12] Fig. 12A is a diagram showing an electronic device using the semiconductor device, and Fig. 12B is a diagram showing an electronic device using the semiconductor device. [Figure 13] Fig. 13A is a diagram showing the structure of a sample for cross-section observation, and Fig. 13B and Fig. 13C are diagrams showing selected area diffraction patterns of the sample for cross-section observation. [Figure 14] FIG. 14 is a diagram showing a bright-field image of a sample for cross-section observation. [Figure 15] Fig. 15A is a diagram showing a selected area diffraction pattern of a sample for cross-section observation, and Figs. 15B to 15D are diagrams showing dark-field images of the vicinity of the surface of a metal oxide film using spots of diffracted waves (009). [Figure 16] Fig. 16A is a diagram showing a selected area diffraction pattern of a sample for cross-section observation, and Fig. 16B to Fig. 16D are diagrams showing dark-field images in the vicinity of a silicon oxide film using a spot of a diffracted wave (009). [Figure 17] Fig. 17A is a diagram showing a selected area diffraction pattern of a sample for cross-section observation, and Fig. 17B to Fig. 17D are diagrams showing dark-field images of the vicinity of the surface of a metal oxide film using the spot of the diffracted wave (009). [Figure 18] Fig. 18A is a diagram showing a selected area diffraction pattern of a sample for cross-section observation, and Figs. 18B to 18D are diagrams showing dark-field images in the vicinity of a silicon oxide film using the spot of a diffracted wave (009). [Figure 19] Fig. 19A is a diagram showing a selected area diffraction pattern of a sample for planar observation, and Fig. 19B to Fig. 19D are diagrams showing dark field images of a metal oxide film using spots of a diffracted wave (100). [Figure 20] Fig. 20A is a diagram showing a bright-field image of the sample for plane observation, Fig. 20B is a diagram showing a dark-field image of the sample for plane observation, and Fig. 20C and Fig. 20D are diagrams showing high-resolution images of the sample for plane observation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the embodiments will be described with reference to the drawings. However, it will be easily understood by those skilled in the art that the embodiments can be implemented in many different ways, and that the modes and details can be changed in various ways without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the following embodiments.
[0020] In addition, in the drawings, the size, thickness of layers, or areas may be exaggerated for clarity. Therefore, the drawings are not necessarily limited to the scale. The drawings are schematic illustrations of ideal examples, and are not limited to the shapes or values shown in the drawings. For example, in an actual manufacturing process, layers, resist masks, etc. may be unintentionally thinned by etching or other processes, but this may not be reflected in the drawings to facilitate understanding. In addition, in the drawings, the same reference numerals are used in common between different drawings for the same parts or parts having similar functions, and repeated explanations may be omitted. In addition, when referring to similar functions, the same hatch pattern may be used and no particular reference numeral may be attached.
[0021] In order to facilitate understanding of the invention, particularly in top views (also called "plan views") and perspective views, some components may be omitted from the drawings. Also, some hidden lines may be omitted from the drawings.
[0022] In addition, in this specification, ordinal numbers such as first, second, etc. are used for convenience and do not indicate the order of steps or stacking. Therefore, for example, "first" can be appropriately replaced with "second" or "third" for explanation. In addition, the ordinal numbers described in this specification and the like may not match the ordinal numbers used to specify one embodiment of the present invention.
[0023] In addition, in this specification, the terms "above" and "below" indicating the arrangement are used for convenience in order to explain the positional relationship between the components with reference to the drawings. In addition, the positional relationship between the components changes as appropriate depending on the direction in which each component is depicted. Therefore, the terms are not limited to those described in the specification, and can be rephrased appropriately depending on the situation.
[0024] For example, when it is explicitly stated in this specification that X and Y are connected, the case where X and Y are electrically connected, the case where X and Y are functionally connected, and the case where X and Y are directly connected are considered to be disclosed in this specification. Therefore, it is not limited to a specific connection relationship, for example, a connection relationship shown in a figure or text, and a connection relationship other than that shown in a figure or text is also considered to be disclosed in the figure or text. Here, X and Y are objects (for example, a device, an element, a circuit, wiring, an electrode, a terminal, a conductive film, a layer, etc.).
[0025] In this specification, a transistor is an element having at least three terminals including a gate, a drain, and a source. A region where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode) (hereinafter, also referred to as a channel formation region) is provided, and a current can flow between the source and the drain through the channel formation region. In this specification, a channel formation region refers to a region through which a current mainly flows.
[0026] Furthermore, the functions of the source and drain may be interchanged when transistors of different polarities are used, when the direction of current changes during circuit operation, etc. For this reason, in this specification and the like, the terms source and drain may be used interchangeably.
[0027] Note that impurities in a semiconductor refer to, for example, anything other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity. The inclusion of impurities can, for example, increase the density of defect states in the semiconductor or reduce the crystallinity. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor, such as hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water can also function as an impurity. For example, the inclusion of impurities can cause oxygen deficiencies (V O :oxygen vacancy) may be formed.
[0028] In this specification and the like, silicon oxynitride refers to a material having a composition that contains more oxygen than nitrogen, and silicon nitride oxide refers to a material having a composition that contains more nitrogen than oxygen.
[0029] In this specification and the like, the term "insulator" can be replaced with an insulating film or an insulating layer, the term "conductor" can be replaced with a conductive film or a conductive layer, and the term "semiconductor" can be replaced with a semiconductor film or a semiconductor layer.
[0030] In addition, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes the case of -5 degrees or more and 5 degrees or less. "Approximately parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. "Perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes the case of 85 degrees or more and 95 degrees or less. "Approximately perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.
[0031] In this specification and the like, the term "metal oxide" refers to an oxide of a metal in a broad sense. Metal oxides are classified into oxide insulators, oxide conductors (including transparent oxide conductors), oxide semiconductors (also referred to as oxide semiconductors or simply OS), and the like. For example, when a metal oxide is used for a semiconductor layer of a transistor, the metal oxide may be referred to as an oxide semiconductor. In other words, an OS transistor can be rephrased as a transistor having a metal oxide or an oxide semiconductor.
[0032] In this specification and the like, normally-off means that when no potential is applied to the gate or when a ground potential is applied to the gate, the drain current flowing through the transistor per 1 μm of channel width is 1×10 -20 A or less, 1×10 at 85℃ -18 A or less, or 1×10 at 125°C -16 This means that it is A or lower.
[0033] (Embodiment 1) In this embodiment, an example of a semiconductor device including a transistor 200 according to one embodiment of the present invention and a manufacturing method thereof will be described with reference to FIGS.
[0034] <Configuration Example 1 of Semiconductor Device> 1A, a structure of a semiconductor device including a transistor 200 will be described. FIG 1A is a cross-sectional view of a semiconductor device including a transistor 200.
[0035] As shown in Figure 1A, a semiconductor device having a transistor 200 of one embodiment of the present invention includes a substrate 210, a conductor 242 on the substrate 210, a metal oxide 243 on the conductor 242, an oxide 230a on the metal oxide 243, an oxide 230b on the oxide 230a, an insulator 250 on the oxide 230b, a conductor 260 on the insulator 250, an insulator 272 on the conductor 260, an insulator 271 in contact with a side of the insulator 250, a side of the conductor 260, and a side of the insulator 272, a metal oxide 245 covering the oxide 230b, the insulator 271, the insulator 272, and the conductor 260, and a conductor 246 on the metal oxide 245. Conductor 260 has an area that overlaps with oxide 230b, conductor 246 has an area that contacts metal oxide 245, and metal oxide 245 has an area that contacts oxide 230b.
[0036] The carrier concentration of the oxide 230b is preferably lower than that of the oxide 230a. The carrier concentration of the metal oxide 243 is preferably higher than that of the oxide 230a, and the carrier concentration of the metal oxide 245 is preferably higher than that of the oxide 230a.
[0037] Here, the conductor 260 functions as the gate of the transistor 200, and the substrate 210 and the conductor 242 function as the drain. The conductor 246 functions as the source. The insulator 250 functions as a gate insulator. A part of the oxide 230a and a part of the oxide 230b become a channel formation region. That is, the transistor 200 is a vertical channel transistor.
[0038] In the transistor 200, a metal oxide that functions as a semiconductor (hereinafter also referred to as an oxide semiconductor) is preferably used for the oxide 230a including a channel formation region and the oxide 230b. Note that in this specification, the oxide 230a and the oxide 230b are collectively referred to as the oxide 230.
[0039] In addition, the metal oxide functioning as a semiconductor preferably has a band gap of 2 eV or more, more preferably 2.5 eV or more. By using a metal oxide having a wide band gap in this way, the off-state current of a transistor can be reduced.
[0040] The transistor 200 using an oxide semiconductor for a channel formation region has an extremely small leakage current (off-state current) in an off-state; therefore, a low-power semiconductor device can be provided.
[0041] For example, metal oxides such as In-M-Zn oxide (wherein element M is one or more selected from aluminum, gallium, yttrium, tin, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, etc.) may be used as the oxide 230a and the oxide 230b. In particular, element M may be aluminum, gallium, yttrium, or tin. Also, In-Ga oxide or In-Zn oxide may be used as the oxide 230a and the oxide 230b. Also, Ga-Zn oxide, tin oxide, copper oxide, nickel oxide, or RbCd oxide may be used as the oxide 230a and the oxide 230b.
[0042] Moreover, it is preferable to use a conductive oxide for the metal oxide 243 in contact with the conductor 242 and the metal oxide 245 in contact with the conductor 246. In particular, it is preferable to use a conductive oxide in which carrier generation does not depend only on oxygen vacancies but generates carriers by substitutional impurity donors. As a result, even if the oxygen vacancies in the metal oxide 243 and the metal oxide 245 are repaired by excess oxygen, carriers due to the impurity donors are present, so that it is possible to suppress a decrease in carrier density in the metal oxide 243 and the metal oxide 245. Therefore, it is considered that carriers are generated in the conductive oxide even in a state where there are few oxygen vacancies. In this way, the metal oxide 243 and the conductor 245 have high carrier concentrations, so that the conductor 242 and the metal oxide 243 can be in ohmic contact. Similarly, the conductor 246 and the metal oxide 245 can be in ohmic contact.
[0043] The metal oxide 243 and the metal oxide 245 preferably contain indium and one or more of tin, tungsten, titanium, and silicon. For example, indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may be used.
[0044] Alternatively, zinc oxide doped with gallium, titanium oxide doped with niobium, or ruthenium oxide may be used.
[0045] As shown in FIG. 1A, the transistor 200 is a vertical channel transistor. First, a suitable positive potential is applied to the conductor 260 functioning as a gate, and a channel is formed in the oxide 230b through the insulator 250 functioning as a gate insulator. Next, carriers flow from the conductor 246 functioning as a source through the metal oxide 245, the channel forming region of the oxide 230b, the channel forming region of the oxide 230a, and the metal oxide 243 to the conductor 242 functioning as a drain and the substrate 210. In other words, when the bottom surfaces of the films constituting the transistor 200 are taken as the reference, the carriers flow in the vertical direction of the bottom surfaces. In other words, a channel is formed in the vertical direction. In this embodiment, since the transistor 200 is an n-type transistor, the carriers are electrons.
[0046] Here, the conductor 242 and the metal oxide 243 are in ohmic contact, and the conductor 246 and the metal oxide 245 are in ohmic contact, so that the energy barrier is small in the path through which electrons flow, and therefore a large current can be obtained. Furthermore, by configuring the transistor 200 in this way, the cross-sectional area of the path through which electrons flow, i.e., the current path, can be made wider than that of a planar type transistor, and therefore a large on-current can be obtained. Therefore, a semiconductor device having the transistor 200 is suitable for use as a semiconductor device for high power applications, for example, a semiconductor device having a power transistor.
[0047] In addition, since the transistor 200 can be formed mainly by stacking thin films, the number of lithography steps can be minimized, and therefore a semiconductor device including the transistor 200 can be manufactured at low production costs.
[0048] In addition, in the manufacturing process of the transistor 200, it is preferable to perform heat treatment while the surface of the oxide 230b is exposed. The heat treatment may be performed, for example, at a temperature of 100° C. or higher and 600° C. or lower, more preferably 350° C. or higher and 400° C. or lower. Note that the heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing an oxidizing gas at 10 ppm or higher, 1% or higher, or 10% or higher. For example, the heat treatment is preferably performed in an oxygen atmosphere. This supplies oxygen to the oxide 230 to reduce oxygen deficiencies (V O ) can be reduced. The heat treatment may be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas in order to compensate for the desorbed oxygen after the heat treatment in a nitrogen gas or inert gas atmosphere. Alternatively, the heat treatment may be performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas in succession to a nitrogen gas or inert gas atmosphere.
[0049] In addition, by subjecting the oxide 230 to an oxygen addition treatment, the oxygen vacancies in the oxide 230 are repaired by the supplied oxygen. In other words, O In addition, the reaction of the hydrogen remaining in the oxide 230 with the oxygen supplied can be promoted, and the hydrogen can be removed as H2O (dehydrated). As a result, the hydrogen remaining in the oxide 230 recombines with the oxygen vacancies to form V O The formation of H can be suppressed.
[0050] It is preferable that the conductor 242, the metal oxide 243, the oxide 230a, and the oxide 230b are successively formed without exposure to the air environment. By forming the films without exposure to the air, it is possible to prevent impurities or moisture from the air environment from adhering to the conductor 242, the metal oxide 243, the oxide 230a, and the oxide 230b, and it is possible to keep the interface and the vicinity of the interface between the conductor 242 and the metal oxide 243, the interface and the vicinity of the interface between the metal oxide 243 and the oxide 230a, and the interface and the vicinity of the interface between the oxide 230a and the oxide 230b clean. An apparatus capable of successively forming the films will be described later.
[0051] As the conductor 242 and the conductor 246, for example, a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing tantalum and aluminum, a nitride containing titanium and aluminum, or the like is preferably used. In one embodiment of the present invention, a nitride containing tantalum is particularly preferable. In addition, for example, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, an oxide containing lanthanum and nickel, or the like may be used. These materials are preferable because they are conductive materials that are difficult to oxidize, or materials that maintain conductivity even when they absorb oxygen.
[0052] The insulator 250 functions as a gate insulator. The insulator 250 is preferably disposed in contact with the upper surface of the oxide 230b. The insulator 250 can be made of silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide doped with fluorine, silicon oxide doped with carbon, silicon oxide doped with carbon and nitrogen, silicon oxide having vacancies, or the like. In particular, silicon oxide and silicon oxynitride are preferable because they are stable against heat.
[0053] The insulator 250 is preferably made of an oxide material from which some oxygen is released by heating, in other words, an insulator material having an excess oxygen region. An oxide material from which oxygen is released by heating is an oxide material from which the amount of released oxygen molecules is 1.0×10 18 molecules / cm 3 More than 1.0×10 19 molecules / cm 3 More preferably, 2.0×10 19 molecules / cm 3 or more, or 3.0×10 20 molecules / cm 3 The oxide film is as described above. Note that the surface temperature of the film during the TDS analysis is preferably in the range of 100°C to 700°C, or 100°C to 400°C. By providing an insulator that releases oxygen when heated as the insulator 250 in contact with the upper surface of the oxide 230b, oxygen can be effectively supplied to the channel formation region of the oxide 230b, and oxygen vacancies in the channel formation region of the oxide 230b can be reduced. Therefore, it is possible to provide a transistor that suppresses fluctuations in electrical characteristics, has stable electrical characteristics, and has improved reliability. It is also preferable that the concentration of impurities such as water and hydrogen in the insulator 250 is reduced.
[0054] In FIG. 1A, the insulator 250 is illustrated as a single layer, but may have a laminated structure of two or more layers. When the insulator 250 has a laminated structure of two layers, it is preferable that the lower layer of the insulator 250 is formed using an insulator that releases oxygen when heated, and the upper layer of the insulator 250 is formed using an insulator that has a function of suppressing the diffusion of oxygen. With such a configuration, it is possible to suppress the diffusion of oxygen contained in the lower layer of the insulator 250 into the conductor 260. In other words, it is possible to suppress a decrease in the amount of oxygen supplied to the oxide 230. In addition, it is possible to suppress the oxidation of the conductor 260 due to the oxygen contained in the lower layer of the insulator 250.
[0055] When silicon oxide or silicon oxynitride is used for the lower layer of the insulator 250, the upper layer of the insulator 250 may be made of an insulating material that is a high-k material with a high dielectric constant. By forming the gate insulator into a laminated structure of the lower layer of the insulator 250 and the upper layer of the insulator 250, it is possible to obtain a laminated structure that is stable against heat and has a high dielectric constant. Therefore, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical film thickness of the gate insulator. In addition, it is possible to reduce the equivalent oxide thickness (EOT) of the insulator that functions as the gate insulator.
[0056] Specifically, the upper layer of the insulator 250 may be a metal oxide containing one or more of hafnium, aluminum, gallium, yttrium, zirconium, tungsten, titanium, tantalum, nickel, germanium, magnesium, etc., or a metal oxide that can be used as the oxide 230. In particular, it is preferable to use an insulator containing an oxide of one or both of aluminum and hafnium.
[0057] The conductor 260 functions as a gate of the transistor 200. Note that although the conductor 260 is shown as having a single-layer structure in Fig. 1A, it may have a two-layer structure or a stacked structure of three or more layers.
[0058] When the conductor 260 has a laminated structure, the lower layer of the conductor 260 is preferably made of a conductive material having a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, copper atoms, etc. Alternatively, it is preferable to use a conductive material having a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms, oxygen molecules, etc.).
[0059] Furthermore, since the lower layer of the conductor 260 has a function of suppressing oxygen diffusion, it is possible to suppress a decrease in conductivity due to oxidation of the upper layer of the conductor 260 caused by oxygen contained in the insulator 250. As a conductive material having a function of suppressing oxygen diffusion, it is preferable to use, for example, tantalum, tantalum nitride, ruthenium, ruthenium oxide, or the like.
[0060] In addition, since the conductor 260 also functions as wiring, it is preferable to use a conductor with high conductivity. For example, the upper layer of the conductor 260 can be made of a conductive material mainly composed of tungsten, copper, or aluminum. The upper layer of the conductor 260 may also have a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above-mentioned conductive material.
[0061] The insulator 271 is disposed so as to be in contact with a side surface of the conductor 260, and the insulator 272 is disposed so as to be in contact with an upper surface of the conductor 260. Therefore, it is preferable that the insulators 271 and 272 function as barrier insulating films at least against oxygen. For example, it is preferable that the insulators 271 and 272 have a function of suppressing oxygen diffusion more than the insulator 250. As the insulators 271 and 272, for example, it is preferable to form a film of an insulator containing an oxide of one or both of aluminum and hafnium.
[0062] <Materials for semiconductor devices> The following describes constituent materials that can be used in the semiconductor device.
[0063] <<Substrate>> The substrate on which the transistor 200 is formed may be, for example, a semiconductor substrate or a conductor substrate. The semiconductor substrate may be, for example, a semiconductor substrate made of silicon or germanium, or a compound semiconductor substrate made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, or gallium oxide. The conductor substrate may be, for example, a graphite substrate, a metal substrate, an alloy substrate, or a conductive resin substrate. Alternatively, the substrate may be a substrate having a metal nitride or a substrate having a metal oxide. The substrate may be a semiconductor substrate having a conductor, or a conductor substrate having a semiconductor. Alternatively, the substrate may be one on which an element is provided. The substrate may be a capacitance element, a resistance element, a switch element, a light-emitting element, a memory element, or the like.
[0064] <<Insulators>> Examples of the insulator include oxides, nitrides, oxynitrides, nitride oxides, metal oxides, metal oxynitrides, and metal nitride oxides, each of which has insulating properties.
[0065] For example, as transistors become smaller and more highly integrated, problems such as leakage current can occur due to thinner gate insulators. By using a high-k material for the insulator that functions as the gate insulator, it is possible to reduce the voltage required for transistor operation while maintaining the physical film thickness. On the other hand, by using a material with a low dielectric constant for the insulator that functions as the interlayer film, it is possible to reduce the parasitic capacitance that occurs between wiring. Therefore, it is best to select materials according to the function of the insulator.
[0066] Furthermore, examples of insulators with a high relative dielectric constant include gallium oxide, hafnium oxide, zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium.
[0067] Examples of insulators with a low dielectric constant include silicon oxide, silicon oxynitride, silicon oxide doped with fluorine, silicon oxide doped with carbon, silicon oxide doped with carbon and nitrogen, silicon oxide having voids, and resin.
[0068] In addition, the transistor using metal oxide can have stable electrical characteristics by being surrounded by an insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen. As the insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen, for example, an insulator containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, or tantalum may be used in a single layer or a stacked layer. Specifically, as the insulator having a function of suppressing the permeation of impurities such as hydrogen and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and metal nitrides such as aluminum nitride, silicon nitride oxide, and silicon nitride can be used.
[0069] The insulator that functions as the gate insulator is preferably an insulator having a region containing oxygen that is released by heating. For example, by using a structure in which silicon oxide or silicon oxynitride having a region containing oxygen that is released by heating is in contact with the oxide 230, oxygen vacancies in the oxide 230 can be compensated for.
[0070] <<Conductors>> As the conductor, it is preferable to use a metal element selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the above-mentioned metal elements as a component, or an alloy combining the above-mentioned metal elements. For example, it is preferable to use tantalum nitride, titanium nitride, tungsten, nitride containing titanium and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel, etc. In addition, tantalum nitride, titanium nitride, nitride containing titanium and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel are conductive materials that are difficult to oxidize, or materials that maintain conductivity even when oxygen is absorbed, so they are preferable. Furthermore, a semiconductor having high electrical conductivity, typified by polycrystalline silicon containing an impurity element such as phosphorus, or a silicide such as nickel silicide may be used.
[0071] A plurality of conductive layers formed of the above-mentioned materials may be stacked. For example, a stacked structure may be formed by combining the above-mentioned material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-mentioned material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-mentioned material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.
[0072] In addition, when an oxide is used for the channel formation region of a transistor, a conductor functioning as a gate electrode preferably has a stacked structure in which a material containing a metal element and a conductive material containing oxygen are combined. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen released from the conductive material is easily supplied to the channel formation region.
[0073] In particular, it is preferable to use a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed as a conductor functioning as a gate electrode. The conductive material containing the metal element and nitrogen described above may also be used. For example, a conductive material containing nitrogen, such as titanium nitride or tantalum nitride, may also be used. Indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, or indium tin oxide to which silicon is added may also be used. Indium gallium zinc oxide containing nitrogen may also be used. By using such a material, hydrogen contained in the metal oxide in which the channel is formed may be captured. Alternatively, hydrogen mixed in from an external insulator may be captured.
[0074] It is preferable to use a metal oxide that functions as a semiconductor (oxide semiconductor) as the oxide 230. Hereinafter, metal oxides that can be applied to the oxide 230 according to the present invention will be described.
[0075] <Metal oxide> In this embodiment, a metal oxide (hereinafter also referred to as an oxide semiconductor) functioning as a semiconductor which can be used for the OS transistor described in the above embodiment will be described.
[0076] The metal oxide preferably contains at least indium or zinc. In particular, it is preferable that the metal oxide contains indium and zinc. In addition to these, it is preferable that the metal oxide contains aluminum, gallium, yttrium, tin, etc. In addition, it may contain one or more elements selected from boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, cobalt, etc.
[0077] <Classification of crystal structures> First, classification of crystal structures in oxide semiconductors will be described with reference to Fig. 9A. Fig. 9A is a diagram for explaining classification of crystal structures of oxide semiconductors, typically IGZO (metal oxide containing In, Ga, and Zn).
[0078] As shown in FIG. 9A, oxide semiconductors are broadly classified into "Amorphous", "Crystalline", and "Crystal". "Amorphous" includes completely amorphous. "Crystalline" includes c-axis-aligned crystalline (CAAC), nanocrystalline (nc), and cloud-aligned composite (CAC) (excluding single crystal and poly crystal). "Crystalline" excludes single crystal, poly crystal, and completely amorphous. "Crystal" includes single crystal and poly crystal.
[0079] The structure in the bold frame shown in Fig. 9A is an intermediate state between "Amorphous" and "Crystal" and belongs to a new boundary region (New crystalline phase). In other words, this structure is completely different from the energetically unstable "Amorphous" and "Crystal".
[0080] The crystal structure of the film or substrate can be evaluated using an X-ray diffraction (XRD) spectrum. Figure 9B shows an XRD spectrum obtained by GIXD (Grazing-Incidence XRD) measurement of the CAAC-IGZO film classified as "Crystalline". The GIXD method is also called the thin film method or the Seemann-Bohlin method. Hereinafter, the XRD spectrum obtained by the GIXD measurement shown in Figure 9B will be simply referred to as the XRD spectrum. The composition of the CAAC-IGZO film shown in Figure 9B is in the vicinity of In:Ga:Zn=4:2:3 [atomic ratio]. The thickness of the CAAC-IGZO film shown in Figure 9B is 500 nm.
[0081] As shown in Figure 9B, a peak indicating clear crystallinity is detected in the XRD spectrum of the CAAC-IGZO film. Specifically, a peak indicating c-axis orientation is detected near 2θ=31° in the XRD spectrum of the CAAC-IGZO film. Note that, as shown in Figure 9B, the peak near 2θ=31° is asymmetric with respect to the angle at which the peak intensity is detected.
[0082] The crystal structure of the film or substrate can be evaluated by a diffraction pattern (also called a nanobeam electron diffraction pattern) observed by nanobeam electron diffraction (NBED). The diffraction pattern of the CAAC-IGZO film is shown in Figure 9C. Figure 9C shows a diffraction pattern observed by NBED, which causes an electron beam to be incident parallel to the substrate. The composition of the CAAC-IGZO film shown in Figure 9C is approximately In:Ga:Zn=4:2:3 [atomic ratio]. In the nanobeam electron diffraction method, electron diffraction is performed with a probe diameter of 1 nm.
[0083] As shown in FIG. 9C, multiple spots indicating c-axis orientation are observed in the diffraction pattern of the CAAC-IGZO film.
[0084] <<Structure of oxide semiconductor>> In addition, when focusing on the crystal structure, oxide semiconductors may be classified differently from that shown in FIG. 9A. For example, oxide semiconductors are divided into single-crystal oxide semiconductors and other non-single-crystal oxide semiconductors. Examples of non-single-crystal oxide semiconductors include the above-mentioned CAAC-OS and nc-OS. In addition, non-single-crystal oxide semiconductors include polycrystalline oxide semiconductors, pseudo-amorphous-like oxide semiconductors (a-like OS), amorphous oxide semiconductors, and the like.
[0085] Here, the above-mentioned CAAC-OS, nc-OS, and a-like OS will be described in detail.
[0086] [CAAC-OS] CAAC-OS is an oxide semiconductor having a plurality of crystalline regions, each of which has a c-axis aligned in a specific direction. The specific direction is the thickness direction of the CAAC-OS film, the normal direction of the surface on which the CAAC-OS film is formed, or the normal direction of the surface of the CAAC-OS film. The crystalline region is a region having periodic atomic arrangement. If the atomic arrangement is considered as a lattice arrangement, the crystalline region is also a region with a uniform lattice arrangement. CAAC-OS has a region in which a plurality of crystalline regions are connected in the ab-plane direction, and the region may have distortion. The distortion refers to a portion in which the direction of the lattice arrangement changes between a region with a uniform lattice arrangement and another region with a uniform lattice arrangement in the region in which the plurality of crystalline regions are connected. In other words, CAAC-OS is an oxide semiconductor having a c-axis aligned and no clear orientation in the ab-plane direction.
[0087] Each of the multiple crystalline regions is composed of one or more minute crystals (crystals with a maximum diameter of less than 10 nm). When a crystalline region is composed of one minute crystal, the maximum diameter of the crystalline region is less than 10 nm. When a crystalline region is composed of many minute crystals, the size of the crystalline region may be about several tens of nm.
[0088] In addition, in an In-M-Zn oxide (wherein element M is one or more elements selected from aluminum, gallium, yttrium, tin, titanium, etc.), the CAAC-OS tends to have a layered crystal structure (also referred to as a layered structure) in which a layer containing indium (In) and oxygen (hereinafter, In layer) and a layer containing element M, zinc (Zn), and oxygen (hereinafter, (M, Zn) layer) are stacked. Note that indium and element M are mutually substituted. Thus, the (M, Zn) layer may contain indium. Also, the In layer may contain element M. Note that the In layer may contain Zn. The layered structure is observed as a lattice image in a high-resolution TEM image, for example.
[0089] When the CAAC-OS film is subjected to structural analysis using, for example, an XRD device, a peak indicating c-axis orientation is detected at or near 2θ=31° in out-of-plane XRD measurement using θ / 2θ scan. Note that the position of the peak indicating c-axis orientation (2θ value) may vary depending on the type and composition of the metal elements constituting the CAAC-OS.
[0090] For example, a plurality of bright points (spots) are observed in the electron diffraction pattern of the CAAC-OS film, and the two spots are observed at positions symmetrical to each other with respect to the spot of the incident electron beam that has passed through the sample (also called the direct spot).
[0091] When the crystal region is observed from the specific direction, the lattice arrangement in the crystal region is based on a hexagonal lattice, but the unit cell is not necessarily a regular hexagon and may be a non-regular hexagon. The above distortion may have a pentagonal or heptagonal lattice arrangement. In addition, no clear grain boundary can be confirmed in the CAAC-OS even in the vicinity of the distortion. That is, it is found that the formation of grain boundaries is suppressed by the distortion of the lattice arrangement. This is considered to be because the CAAC-OS can tolerate distortion due to the fact that the arrangement of oxygen atoms is not dense in the ab-plane direction and the bond distance between atoms changes due to the substitution of metal atoms.
[0092] A crystal structure in which clear grain boundaries are observed is called a polycrystal. The grain boundaries are likely to become recombination centers and capture carriers, causing a decrease in the on-current of a transistor and a decrease in field effect mobility. Therefore, CAAC-OS in which clear grain boundaries are not observed is one of the crystalline oxides having a crystal structure suitable for a semiconductor layer of a transistor. In order to form a CAAC-OS, a structure containing Zn is preferable. For example, In-Zn oxide and In-Ga-Zn oxide are suitable because they can suppress the occurrence of grain boundaries more than In oxide.
[0093] The CAAC-OS is an oxide semiconductor with high crystallinity and no clear crystal grain boundaries. Therefore, it can be said that the CAAC-OS is less susceptible to a decrease in electron mobility due to crystal grain boundaries. In addition, since the crystallinity of an oxide semiconductor can be decreased by the inclusion of impurities or the generation of defects, the CAAC-OS can be said to be an oxide semiconductor with few impurities and defects (such as oxygen vacancies). Therefore, the physical properties of an oxide semiconductor having the CAAC-OS are stable. Therefore, an oxide semiconductor having the CAAC-OS is resistant to heat and has high reliability. In addition, the CAAC-OS is stable against high temperatures (so-called thermal budget) in the manufacturing process. Therefore, the use of the CAAC-OS in an OS transistor can increase the degree of freedom in the manufacturing process.
[0094] [nc-OS] The nc-OS has periodic atomic arrangement in a minute region (for example, a region of 1 nm to 10 nm, particularly a region of 1 nm to 3 nm). In other words, the nc-OS has minute crystals. Note that the size of the minute crystals is, for example, 1 nm to 10 nm, particularly 1 nm to 3 nm, and therefore the minute crystals are also called nanocrystals. In addition, the nc-OS does not show regularity in the crystal orientation between different nanocrystals. Therefore, no orientation is seen in the entire film. Therefore, depending on the analysis method, the nc-OS may be indistinguishable from an a-like OS or an amorphous oxide semiconductor. For example, when a structure analysis is performed on an nc-OS film using an XRD device, no peak indicating crystallinity is detected in out-of-plane XRD measurement using θ / 2θ scan. In addition, when an nc-OS film is subjected to electron diffraction (also called selected area electron diffraction) using an electron beam with a probe diameter larger than that of nanocrystals (for example, 50 nm or more), a diffraction pattern like a halo pattern is observed. On the other hand, when electron diffraction (also called nanobeam electron diffraction) is performed on an nc-OS film using an electron beam with a probe diameter (e.g., 1 nm to 30 nm) that is close to the size of a nanocrystal or smaller than the nanocrystal, an electron diffraction pattern in which multiple spots are observed within a ring-shaped region centered on the direct spot may be obtained.
[0095] [a-like OS] The a-like OS is an oxide semiconductor having a structure between the nc-OS and an amorphous oxide semiconductor. The a-like OS has a void or low-density region. That is, the a-like OS has lower crystallinity than the nc-OS and CAAC-OS. Moreover, the a-like OS has a higher hydrogen concentration in the film than the nc-OS and CAAC-OS.
[0096] <<Oxide semiconductor structure>> Next, the above-mentioned CAC-OS will be described in detail, with reference to its material composition.
[0097] [CAC-OS] CAC-OS is, for example, a material configuration in which elements constituting a metal oxide are unevenly distributed in a size range of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or in the vicinity thereof. In the following, a state in which one or more metal elements are unevenly distributed in a metal oxide and the regions having the metal elements are mixed in a size range of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or in the vicinity thereof, is also referred to as a mosaic or patch state.
[0098] Furthermore, CAC-OS is a composite metal oxide in which the material is separated into a first region and a second region, forming a mosaic structure, and the first region is distributed throughout the film (hereinafter, also referred to as a cloud structure). In other words, CAC-OS is a composite metal oxide in which the first region and the second region are mixed together.
[0099] Here, the atomic ratios of In, Ga, and Zn to the metal elements constituting the CAC-OS in the In-Ga-Zn oxide are represented as [In], [Ga], and [Zn], respectively. For example, in the CAC-OS in the In-Ga-Zn oxide, the first region is a region where [In] is larger than [In] in the composition of the CAC-OS film. Also, the second region is a region where [Ga] is larger than [Ga] in the composition of the CAC-OS film. Alternatively, for example, the first region is a region where [In] is larger than [In] in the second region and [Ga] is smaller than [Ga] in the second region. Also, the second region is a region where [Ga] is larger than [Ga] in the first region and [In] is smaller than [In] in the first region.
[0100] Specifically, the first region is a region mainly composed of indium oxide, indium zinc oxide, etc., and the second region is a region mainly composed of gallium oxide, gallium zinc oxide, etc. In other words, the first region can be rephrased as a region mainly composed of In, and the second region can be rephrased as a region mainly composed of Ga.
[0101] In addition, there are cases where a clear boundary between the first region and the second region cannot be observed.
[0102] For example, in the case of a CAC-OS of an In-Ga-Zn oxide, EDX mapping obtained using EDX (Energy Dispersive X-ray spectroscopy) has confirmed that the CAC-OS has a structure in which a region mainly composed of In (first region) and a region mainly composed of Ga (second region) are unevenly distributed and mixed.
[0103] When CAC-OS is used in a transistor, the conductivity due to the first region and the insulating property due to the second region act in a complementary manner, giving the CAC-OS a switching function (On / Off function). In other words, CAC-OS has a conductive function in part of the material and an insulating function in other parts of the material, and the material as a whole functions as a semiconductor. By separating the conductive function from the insulating function, it is possible to maximize both functions. Therefore, by using CAC-OS in a transistor, it is possible to achieve a high on-current (I on ), high field effect mobility (μ), and good switching behavior can be achieved.
[0104] Oxide semiconductors have a variety of structures and have different characteristics. The oxide semiconductor of one embodiment of the present invention may include two or more of an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, an a-like OS, a CAC-OS, an nc-OS, and a CAAC-OS.
[0105] <Transistor Having Oxide Semiconductor> Next, the case where the oxide semiconductor is used for a transistor will be described.
[0106] By using the oxide semiconductor for a transistor, a transistor with high field-effect mobility and high reliability can be realized.
[0107] For the transistor, an oxide semiconductor having a low carrier concentration is preferably used. For example, the carrier concentration of the oxide semiconductor is 1×10 17 cm -3 Less than or equal to 1×10 15 cm -3 Less than 1×10, more preferably 13 cm -3 Less than or equal to 1×10 11 cm -3 Less than 1×10, more preferably 10 cm -3 Less than 1 x 10 -9 cm -3 The above is the case. Note that in order to reduce the carrier concentration of an oxide semiconductor film, the impurity concentration in the oxide semiconductor film may be reduced to reduce the density of defect states. In this specification and the like, an oxide semiconductor having a low impurity concentration and a low density of defect states is referred to as a high-purity intrinsic or substantially high-purity intrinsic oxide semiconductor. Note that an oxide semiconductor having a low carrier concentration may be referred to as a high-purity intrinsic or substantially high-purity intrinsic oxide semiconductor.
[0108] Furthermore, a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor film has a low density of defect states, and therefore the density of trap states might also be low.
[0109] In addition, charges trapped in the trap states of an oxide semiconductor take a long time to disappear and may behave as if they are fixed charges. Therefore, a transistor in which a channel formation region is formed in an oxide semiconductor with a high density of trap states may have unstable electrical characteristics.
[0110] Therefore, in order to stabilize the electrical characteristics of a transistor, it is effective to reduce the impurity concentration in the oxide semiconductor. In order to reduce the impurity concentration in the oxide semiconductor, it is preferable to also reduce the impurity concentration in a nearby film. Examples of impurities include hydrogen, nitrogen, alkali metals, alkaline earth metals, iron, nickel, silicon, and the like.
[0111] <Impurities> Here, the influence of each impurity in an oxide semiconductor will be described.
[0112] When an oxide semiconductor contains silicon or carbon, which is one of the group 14 elements, defect levels are formed in the oxide semiconductor. For this reason, the concentrations of silicon or carbon in the oxide semiconductor and those near the interface with the oxide semiconductor (concentrations obtained by secondary ion mass spectrometry (SIMS)) are calculated as 2×10 18 atoms / cm 3 Less than or equal to 2 x 10 17 atoms / cm 3 The following applies.
[0113] In addition, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, defect states may be formed and carriers may be generated. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal is likely to have normally-on characteristics. For this reason, when the concentration of an alkali metal or an alkaline earth metal in an oxide semiconductor obtained by SIMS is 1×10 18 atoms / cm 3 Less than or equal to 2 x 10 16 atoms / cm 3 To the following:
[0114] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor is likely to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen as a semiconductor is likely to have normally-on characteristics. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. For this reason, the nitrogen concentration in an oxide semiconductor obtained by SIMS is set to 5×10 19 atoms / cm 3 Less than 5 x 10 18 atoms / cm 3 Less than or equal to 1×10 18 atoms / cm3 Less than 5×10, more preferably 17 atoms / cm 3 To the following:
[0115] Furthermore, hydrogen contained in an oxide semiconductor reacts with oxygen bonded to a metal atom to form water, which may form an oxygen vacancy. When hydrogen enters the oxygen vacancy, electrons serving as carriers may be generated. In addition, some of the hydrogen may bond with oxygen bonded to a metal atom to generate electrons serving as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to have normally-on characteristics. For this reason, it is preferable to reduce hydrogen in the oxide semiconductor as much as possible. Specifically, when the hydrogen concentration in an oxide semiconductor measured by SIMS is 1×10 20 atoms / cm 3 Less than 1 x 10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 Make it less than.
[0116] When an oxide semiconductor in which impurities are sufficiently reduced is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.
[0117] <<Other semiconductor materials>> The semiconductor material that can be used for the oxide 230 is not limited to the above-mentioned metal oxides. A semiconductor material having a band gap (a semiconductor material that is not a zero-gap semiconductor) may be used for the oxide 230. For example, a semiconductor of a single element such as silicon, a compound semiconductor such as gallium arsenide, or a layered material (also called an atomic layer material, a two-dimensional material, etc.) that functions as a semiconductor is preferably used for the semiconductor material. In particular, it is preferable to use a layered material that functions as a semiconductor for the semiconductor material.
[0118] Here, in this specification and the like, the layered material is a general term for a group of materials having a layered crystal structure. The layered crystal structure is a structure in which layers formed by covalent bonds or ionic bonds are stacked via bonds weaker than covalent bonds or ionic bonds, such as van der Waals forces. The layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-current can be provided.
[0119] Layered materials include graphene, silicene, and chalcogenides. Chalcogenides are compounds that contain chalcogen. Chalcogen is a general term for elements in group 16, including oxygen, sulfur, selenium, tellurium, polonium, and livermorium. Chalcogenides include transition metal chalcogenides and group 13 chalcogenides.
[0120] It is preferable to use, for example, a transition metal chalcogenide that functions as a semiconductor as the oxide 230. Specific examples of transition metal chalcogenides that can be used as the oxide 230 include molybdenum sulfide (representatively MoS2), molybdenum selenide (representatively MoSe2), molybdenum tellurium (representatively MoTe2), tungsten sulfide (representatively WS2), tungsten selenide (representatively WSe2), tungsten tellurium (representatively WTe2), hafnium sulfide (representatively HfS2), hafnium selenide (representatively HfSe2), zirconium sulfide (representatively ZrS2), and zirconium selenide (representatively ZrSe2).
[0121] <Configuration Example 2 of Semiconductor Device> 1B, a configuration of a semiconductor device including a transistor 200, which is different from the configuration shown in FIG 1A, will be described below. FIG 1B is a cross-sectional view of a semiconductor device including a transistor 200.
[0122] 1B, structures having the same functions as those of the structures constituting the semiconductor device shown in <Configuration Example 1 of Semiconductor Device> are denoted by the same reference numerals. Note that, in this section, the materials described in detail in <Configuration Example 1 of Semiconductor Device> can be used as the materials constituting the semiconductor device.
[0123] 1B, a semiconductor device including a transistor 200 according to one embodiment of the present invention includes a substrate 210, a conductor 242 on the substrate 210, a metal oxide 243 on the conductor 242, an oxide 230a on the metal oxide 243, an oxide 230b on the oxide 230a, an insulator 250 on the oxide 230b, a conductor 260 on the insulator 250, a metal oxide 245 on the oxide 230b, an insulator 272 on the metal oxide 245, and a conductor 246 on the metal oxide 245 and on the insulator 272. The oxide 230b and the metal oxide 245 have an opening, and the insulator 250 is arranged so as to be in contact with the side and bottom of the opening. The conductor 260 is arranged so that the bottom and the side of the conductor 260 are in contact with the insulator 250. Furthermore, the conductor 260 has a region that overlaps with the oxide 230b, the conductor 246 has a region that is in contact with the metal oxide 245, and the metal oxide 245 has a region that is in contact with the oxide 230b.
[0124] The carrier concentration of the oxide 230b is preferably lower than that of the oxide 230a. The carrier concentration of the metal oxide 243 is preferably higher than that of the oxide 230a, and the carrier concentration of the metal oxide 245 is preferably higher than that of the oxide 230a.
[0125] Here, the conductor 260 functions as the gate of the transistor 200, and the substrate 210 and the conductor 242 function as the drain. The conductor 246 functions as the source. The insulator 250 functions as a gate insulator. A part of the oxide 230a and a part of the oxide 230b become a channel formation region. That is, the transistor 200 is a vertical channel transistor.
[0126] The semiconductor device shown in FIG. 1B differs from the semiconductor device shown in FIG. 1A in that the oxide 230b and the metal oxide 245 have openings, and the insulator 250 and the conductor 260 are arranged so as to be embedded in the openings.
[0127] For other functions and effects, the description of <Configuration Example 1 of Semiconductor Device> can be referred to.
[0128] <Applications of semiconductor devices> The semiconductor device shown in Figures 2A to 2C is an application example of the semiconductor device shown in Figure 1B. Figure 2A shows a top view. Figure 2B is a cross-sectional view corresponding to the portion indicated by the dashed line A1-A2 in Figure 2A. Figure 2C is a cross-sectional view corresponding to the portion indicated by the dashed line A3-A4 in Figure 2A. Note that some elements are omitted from the top view of Figure 2A for clarity.
[0129] 2A to 2C has a configuration in which a plurality of transistors 200 included in the semiconductor device illustrated in FIG. 1B are arranged in parallel. As illustrated in FIG. 2A to 2C, the semiconductor device including a plurality of transistors 200 includes a conductor 242 on a substrate 210, a metal oxide 243 on the conductor 242, an oxide 230a on the metal oxide 243, an oxide 230b on the oxide 230a, an insulator 250 (insulators 250_1 to 250_4) on the oxide 230b, a conductor 260 (conductors 260_1 to 260_4) on the insulator 250, a metal oxide 245 on the oxide 230b, an insulator 272 on the metal oxide 245, and a conductor 246 on the metal oxide 245 and on the insulator 272. Moreover, the oxide 230b and the metal oxide 245 have openings, and the insulator 250 is arranged so as to contact the side and bottom of the opening. Moreover, the conductor 260 is arranged so that the bottom of the conductor 260 and the side of the conductor 260 are in contact with the insulator 250. Moreover, the conductor 260 has a region overlapping with the oxide 230b, the conductor 246 has a region in contact with the metal oxide 245, and the metal oxide 245 has a region in contact with the oxide 230b. Moreover, as shown in FIG. 2A and FIG. 2C, the insulator 272 has openings 240 (openings 240_1 to 240_4), and has a conductor 248 in contact with the conductor 260 in the opening 240. Note that the conductor 248 can be formed in the same layer as the conductor 246 at the same time, and therefore the conductor 248 and the conductor 246 can use the same conductor material. In this case, the conductor 248 can be made of the same conductor material that can be used for the conductor 246 .
[0130] The semiconductor device shown in FIG. 2A to FIG. 2C has conductors 260_1 to 260_4 functioning as gates and insulators 250_1 to 250_4 functioning as gate insulators. Thus, in this semiconductor device, four transistors 200 described in <Configuration Example 2 of Semiconductor Device> are arranged in parallel. Furthermore, the conductor 248 is electrically connected to each of the conductors 260_1 to 260_4 functioning as gates through an opening in the insulator 272. Thus, by applying a potential to the conductor 248, the same potential can be simultaneously applied to the conductors 260_1 to 260_4, so that all the transistors can be turned on. That is, a path through which a channel flows is formed in each of the four transistors, so that this semiconductor device can pass a large on-current.
[0131] Although the present semiconductor device has been described as having four transistors arranged in parallel, the number of transistors arranged in parallel is not limited to this example. Therefore, the number of transistors arranged can be increased or decreased as appropriate according to the specifications required for the semiconductor device.
[0132] <Method for manufacturing semiconductor device> Next, a manufacturing method of the semiconductor device of one embodiment of the present invention shown in FIGS. 2A to 2C will be described with reference to FIGS. 3A to 8C.
[0133] A in each figure shows a top view. B in each figure shows a cross-sectional view corresponding to the portion indicated by the dashed line A1-A2 in A in each figure. C in each figure shows a cross-sectional view corresponding to the portion indicated by the dashed line A3-A4 in A in each figure. Note that in the top view of A in each figure, some elements are omitted for clarity.
[0134] First, the substrate 210 is prepared, and the conductor 242 is formed on the substrate (see FIGS. 3A to 3C). The conductor 242 can be formed by, for example, a sputtering method, a CVD method, a molecular beam epitaxy (MBE) method, a pulsed laser deposition (PLD) method, an atomic layer deposition (ALD) method, or the like.
[0135] The CVD method can be classified into, for example, the plasma enhanced CVD (PECVD) method, which uses plasma, the thermal CVD (TCVD) method, which uses heat, the photo CVD (Photo CVD) method, etc. Furthermore, depending on the source gas used, the CVD method can be classified into the metal CVD (MCVD) method and the metal organic CVD (MOCVD) method.
[0136] The plasma CVD method can obtain a high-quality film at a relatively low temperature. Moreover, the thermal CVD method is a film formation method that can reduce plasma damage to the object to be processed because it does not use plasma. For example, wiring, electrodes, elements (transistors, capacitive elements, etc.) included in a semiconductor device may be charged up by receiving electric charge from plasma. At this time, the wiring, electrodes, elements, etc. included in the semiconductor device may be destroyed by the accumulated electric charge. On the other hand, in the case of the thermal CVD method that does not use plasma, such plasma damage does not occur, so the yield of the semiconductor device can be increased. Furthermore, in the thermal CVD method, plasma damage does not occur during film formation, so a film with few defects can be obtained.
[0137] As the ALD method, for example, a thermal ALD method in which a reaction between a precursor and a reactant is carried out using only thermal energy, a plasma enhanced ALD method in which a plasma excited reactant is used, or the like can be used.
[0138] In addition, the ALD method utilizes the self-regulating nature of atoms and can deposit atoms one layer at a time, which has the following advantages: extremely thin films can be formed; films can be formed on structures with high aspect ratios; films can be formed with fewer defects such as pinholes; films can be formed with excellent coverage; and films can be formed at low temperatures. In the PEALD (Plasma Enhanced ALD) method, the use of plasma can enable film formation at lower temperatures, which may be preferable. Note that some precursors used in the ALD method contain impurities such as carbon. For this reason, films formed by the ALD method may contain more impurities such as carbon than films formed by other film formation methods. Note that the amount of impurities can be quantified using X-ray photoelectron spectroscopy (XPS).
[0139] The CVD method and the ALD method are different from the film formation method in which particles emitted from a target or the like are deposited, and are film formation methods in which a film is formed by a reaction on the surface of a workpiece. Therefore, they are film formation methods that are not easily affected by the shape of the workpiece and have good step coverage. In particular, the ALD method has excellent step coverage and excellent thickness uniformity, so it is suitable for coating the surface of an opening with a high aspect ratio. However, since the ALD method has a relatively slow film formation speed, it may be preferable to use it in combination with other film formation methods such as the CVD method, which has a fast film formation speed.
[0140] In the CVD method and the ALD method, the composition of the film obtained can be controlled by the flow rate ratio of the raw material gases. For example, in the CVD method and the ALD method, a film of any composition can be formed by changing the flow rate ratio of the raw material gases. In addition, for example, in the CVD method and the ALD method, a film whose composition changes continuously can be formed by changing the flow rate ratio of the raw material gases while forming the film. When forming a film while changing the flow rate ratio of the raw material gases, the time required for film formation can be shortened compared to the case of forming a film using multiple film formation chambers because no time is required for transportation and pressure adjustment. Therefore, the productivity of semiconductor devices can be increased in some cases.
[0141] In this embodiment, the conductor 242 is formed as a film of tantalum nitride or tungsten by sputtering.
[0142] Next, a metal oxide 243 is formed over the conductor 242 (see FIGS. 3A to 3C). The metal oxide 243 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, indium tin oxide is formed as the metal oxide 243 by a sputtering method.
[0143] Next, an oxide 230a and an oxide 230b are formed in this order on the metal oxide 243 (see FIGS. 3A to 3C).
[0144] The oxide 230a and the oxide 230b can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.
[0145] When the oxide 230a and the oxide 230b are formed by sputtering, oxygen or a mixture of oxygen and a rare gas is used as the sputtering gas. By increasing the ratio of oxygen contained in the sputtering gas, the amount of excess oxygen in the oxide film to be formed can be increased. When the oxide film is formed by sputtering, the In-M-Zn oxide target can be used.
[0146] When the oxide 230a and the oxide 230b are formed by a sputtering method, an oxygen-excess oxide semiconductor is formed by setting the ratio of oxygen contained in the sputtering gas to more than 30% and less than or equal to 100%, preferably greater than or equal to 70% and less than or equal to 100%. A transistor using an oxygen-excess oxide semiconductor for a channel formation region can have relatively high reliability. However, one embodiment of the present invention is not limited to this. The crystallinity of the oxide film can be improved by forming the oxide film while heating the substrate. The carrier concentration of the oxide 230b is preferably lower than that of the oxide 230a.
[0147] In this embodiment, the oxide 230a is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn=4:2:4.1. The oxide 230b is formed by sputtering using an oxide target with an atomic ratio of In:Ga:Zn=1:3:4. Each oxide film may be formed according to the desired characteristics of the oxide 230a and the oxide 230b by appropriately selecting the film formation conditions and atomic ratio.
[0148] It is preferable that the conductor 242, the metal oxide 243, the oxide 230a, and the oxide 230b are successively formed under reduced pressure without exposure to the air environment. By forming the films without exposing to the air, it is possible to prevent impurities or moisture from the air environment from adhering to the conductor 242, the metal oxide 243, the oxide 230a, and the oxide 230b, and it is preferable that the interface and the vicinity of the interface between the conductor 242 and the metal oxide 243, the interface and the vicinity of the interface between the metal oxide 243 and the oxide 230a, and the interface and the vicinity of the interface between the oxide 230a and the oxide 230b can be kept clean. For example, a multi-chamber type film forming apparatus may be used for the successive film formation. By forming the films successively, it is preferable that the manufacturing process time of the semiconductor device can be shortened.
[0149] Next, after the oxide 230a and the oxide 230b are formed, it is preferable to perform a heat treatment. The heat treatment may be performed in a temperature range in which the oxide 230a and the oxide 230b are not polycrystallized, and may be performed at 250°C to 650°C, preferably 400°C to 600°C. The heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas may be about 20%. The heat treatment may be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere of nitrogen gas or an inert gas, and then in an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more to compensate for the oxygen that has been desorbed.
[0150] In addition, the gas used in the heat treatment is preferably highly purified. For example, the amount of moisture contained in the gas used in the heat treatment may be 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By using a highly purified gas to perform the heat treatment, it is possible to prevent moisture and the like from being taken into the oxide 230a and the oxide 230b as much as possible.
[0151] In this embodiment, the heat treatment is performed in a nitrogen atmosphere at 550° C. for 1 hour, followed by another heat treatment in an oxygen atmosphere at 550° C. for 1 hour. This heat treatment can remove impurities such as water and hydrogen in the oxide 230a and the oxide 230b. Furthermore, this heat treatment can improve the crystallinity of the oxide 230b, resulting in a denser and more compact structure. This can reduce the diffusion of oxygen or impurities in the oxide 230b.
[0152] Next, the metal oxide 245 is formed over the oxide 230b (see FIGS. 4A to 4C). The metal oxide 245 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In this embodiment, indium tin oxide is formed as the metal oxide 245 by a sputtering method.
[0153] Next, a part of the metal oxide 245 and a part of the oxide 230b are etched by lithography. It is preferable that the oxide 230b is etched by 50% to 80% of the thickness of the oxide 230b. As a result, openings are formed in the metal oxide 245 and the oxide 230b (see FIGS. 5A to 5C).
[0154] In the lithography method, first, the resist is exposed through a mask. Next, the exposed area is removed or left using a developer to form a resist mask. Next, a conductor, a semiconductor, an insulator, or the like can be processed into a desired shape by etching through the resist mask. For example, a resist mask may be formed by exposing the resist using KrF excimer laser light, ArF excimer laser light, EUV (Extreme Ultraviolet) light, or the like. Also, a liquid immersion technique may be used in which a liquid (e.g., water) is filled between the substrate and the projection lens and exposure is performed. Also, an electron beam or an ion beam may be used instead of the light described above. When an electron beam or an ion beam is used, a mask is not required. The resist mask can be removed by performing a dry etching process such as ashing, a wet etching process, a wet etching process after a dry etching process, or a dry etching process after a wet etching process.
[0155] Furthermore, a hard mask made of an insulator or a conductor may be used under the resist mask. When using a hard mask, an insulating film or a conductive film that will be the hard mask material is formed on the metal oxide 245, a resist mask is formed thereon, and the hard mask material is etched to form a hard mask of a desired shape. The etching of the metal oxide 245 and the oxide 230b may be performed after removing the resist mask, or may be performed while leaving the resist mask. In the latter case, the resist mask may disappear during etching. The hard mask may be removed by etching after etching the metal oxide 245 and the oxide 230b. On the other hand, if the material of the hard mask does not affect the subsequent process or can be used in the subsequent process, it is not necessary to remove the hard mask.
[0156] Next, the insulating film 250A is formed (see FIGS. 6A to 6C). A heat treatment may be performed before the formation of the insulating film 250A, and the heat treatment may be performed under reduced pressure, and the insulating film 250A may be formed continuously without exposure to the air. The heat treatment is preferably performed in an atmosphere containing oxygen. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the metal oxide 245 and the surface of the oxide 230b can be removed, and the moisture concentration and hydrogen concentration in the oxide 230a and the oxide 230b can be further reduced. The temperature of the heat treatment is preferably 100° C. or higher and 400° C. or lower.
[0157] The insulating film 250A can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. In addition, the insulating film 250A is preferably formed by a film formation method using a gas in which hydrogen atoms are reduced or removed. This can reduce the hydrogen concentration in the insulating film 250A.
[0158] When the insulator 250 has a two-layer laminated structure, it is preferable to continuously deposit the insulating film that will be the lower layer of the insulator 250 and the insulating film that will be the upper layer of the insulator 250 without exposing them to the atmospheric environment. By depositing the films without exposing them to the atmosphere, it is possible to prevent impurities or moisture from the atmospheric environment from adhering to the insulating film that will be the lower layer of the insulator 250 and the insulating film that will be the upper layer of the insulator 250, and it is possible to keep the vicinity of the interface between the insulating film that will be the lower layer of the insulator 250 and the insulating film that will be the upper layer of the insulator 250 clean.
[0159] Here, after the insulating film 250A is formed, a microwave treatment may be performed under an oxygen-containing atmosphere and reduced pressure. By performing the microwave treatment, an electric field due to microwaves is applied to the insulating film 250A, the oxide 230b, and the oxide 230a, etc., and V in the oxide 230b and the oxide 230a is increased. O H to V Oand hydrogen. At this time, some of the hydrogen separated may combine with oxygen to become H2O, which may be removed from the insulating film 250A, the oxide 230b, and the oxide 230a. In this way, by performing microwave treatment, the hydrogen concentrations in the insulating film 250A, the oxide 230b, and the oxide 230a can be reduced. In addition, the V in the oxide 230a and the oxide 230b can be reduced. O H to V O V that can exist after splitting into and hydrogen O Oxygen is supplied to V O can be repaired or compensated for.
[0160] Moreover, a heat treatment may be performed while maintaining the reduced pressure state after the microwave treatment. By performing such a treatment, hydrogen in the insulating film 250A, the oxide 230b, and the oxide 230a can be efficiently removed. Alternatively, a step of performing a heat treatment may be repeated multiple times while maintaining the reduced pressure state after the microwave treatment. By repeatedly performing the heat treatment, hydrogen in the insulating film 250A, the oxide 230b, and the oxide 230a can be more efficiently removed. Note that the heat treatment temperature is preferably 300° C. or more and 500° C. or less.
[0161] Furthermore, by performing microwave processing to modify the film quality of the insulating film 250A, it is possible to suppress the diffusion of hydrogen, water, impurities, etc. Therefore, it is possible to suppress the diffusion of hydrogen, water, impurities, etc. into the oxide 230b, the oxide 230a, etc. through the insulator 250 by a post-process such as film formation of a conductive film that becomes the conductor 260, or a post-treatment such as heat treatment.
[0162] Next, the conductive film 260A is formed (see FIGS. 6A to 6C). The conductive film 260A can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.
[0163] Next, the insulating film 250A and the conductive film 260A are polished by CMP until the metal oxide 245 is exposed, thereby forming the insulators 250 (insulators 250_1, 250_2, 250_3, and 250_4) and the conductors 260 (conductors 260_1, 260_2, 260_3, and 260_4) (see FIGS. 7A to 7C). As a result, the insulators 250 are disposed so as to cover the inner walls (side walls and bottom surface) of the opening. The conductors 260 are disposed so as to fill the opening through the insulators 250.
[0164] Next, an insulating film that becomes the insulator 272 is formed on the metal oxide 245, the insulator 250, and the conductor 260. The insulating film that becomes the insulator 272 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.
[0165] Next, the insulating film that becomes the insulator 272 is processed by lithography to form the insulator 272. The insulator 272 has openings 240 (opening 240_1, opening 240_2, opening 240_3, and opening 240_4) that reach the conductor 260 (see FIGS. 8A to 8C). The insulating film that becomes the insulator 272 can be processed by dry etching or wet etching.
[0166] Next, a conductive film is formed to become the conductor 246 and the conductor 248. The conductive film to become the conductor 246 and the conductor 248 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.
[0167] Next, the conductive film to be the conductor 246 and the conductor 248 is processed by lithography to form the conductor 246 and the conductor 248 (see FIGS. 2A to 2C). The conductive film to be the conductor 246 and the conductor 248 can be processed by dry etching or wet etching.
[0168] 2A and 2B, conductor 246 is formed to have a region in contact with metal oxide 245, and conductor 246 and metal oxide 245 are electrically connected. Also, as shown in Figures 2A and 2C, conductor 248 is formed to have a region in contact with conductor 260 through opening 240, and conductor 248 and conductor 260 are electrically connected.
[0169] Through the above steps, a semiconductor device including the transistor 200 illustrated in FIGS. 2A to 2C can be manufactured.
[0170] The structures, methods, and the like described in the above-described embodiment modes can be used in appropriate combination with structures, methods, and the like described in other embodiment modes and examples.
[0171] (Embodiment 2) In this embodiment, an apparatus that can be used for manufacturing a semiconductor device of one embodiment of the present invention will be described with reference to FIGS.
[0172] When manufacturing a semiconductor device according to one embodiment of the present invention, it is preferable to use a so-called multi-chamber apparatus having a plurality of treatment chambers in which different types of films can be successively formed. In each treatment chamber, a film formation process such as sputtering, CVD, or ALD can be performed. For example, when one treatment chamber is a sputtering chamber, a gas supply device, a gas purification device connected to the gas supply device, a vacuum pump, a target, and the like can be connected to the sputtering chamber.
[0173] In each treatment chamber, a cleaning treatment, a plasma treatment, a reverse sputtering treatment, an etching treatment, an ashing treatment, a heating treatment, etc. may be performed. By appropriately performing different treatments in each treatment chamber, an insulator, a conductor, and a semiconductor film can be formed without exposure to the atmosphere.
[0174] A typical example of a semiconductor film used in one embodiment of the present invention is an oxide semiconductor film. In particular, an oxide semiconductor film having a low impurity concentration and a low density of defect states (few oxygen vacancies) can be used to manufacture a transistor with excellent electrical characteristics. Here, a semiconductor film having a low impurity concentration and a low density of defect states is referred to as a highly pure intrinsic film or a substantially highly pure intrinsic film.
[0175] A highly-purified intrinsic or substantially highly-purified intrinsic oxide semiconductor film can have a low carrier density because there are few carrier generation sources. Therefore, a transistor in which a channel formation region is formed in the oxide semiconductor film rarely has electrical characteristics in which the threshold voltage is negative (also referred to as normally-on). In addition, a highly-purified intrinsic or substantially highly-purified intrinsic oxide semiconductor film has a low density of defect states, and therefore the density of trap states may also be low. In addition, a highly-purified intrinsic or substantially highly-purified intrinsic oxide semiconductor film has an extremely small off-state current and a channel width of 1×10 6 Even if the device has a channel length L of 10 μm and a width of 1 μm, the off-current is below the measurement limit of the semiconductor parameter analyzer, that is, 1×10 -13 It is possible to obtain a characteristic of A or less.
[0176] Typical examples of impurities in an oxide semiconductor film include water and hydrogen. In this specification and the like, reducing or removing water and hydrogen from an oxide semiconductor film may be referred to as dehydration or dehydrogenation. Adding oxygen to an oxide semiconductor film may be referred to as oxygen addition, and a state in which oxygen is added and the oxide semiconductor film has more oxygen than the stoichiometric composition may be referred to as an excess oxygen state.
[0177] Here, by successively depositing different types of films, that is, an oxide semiconductor film, an insulator or conductor located below the oxide semiconductor film, and an insulator or conductor located above the oxide semiconductor film, without exposure to the air, it is possible to form a substantially high-purity intrinsic oxide semiconductor film in which the concentration of impurities (particularly, hydrogen and water) is reduced.
[0178] First, a detailed configuration example of an apparatus that can be used to manufacture a semiconductor device of one embodiment of the present invention will be described with reference to Fig. 10. By using the apparatus shown in Fig. 10, a semiconductor film, an insulator or conductor located under the semiconductor film, and an insulator or conductor located over the semiconductor film can be successively formed. Therefore, impurities (particularly hydrogen and water) that may enter the semiconductor film can be suppressed.
[0179] FIG. 10 is a schematic top view of a single-wafer type multi-chamber apparatus 4000.
[0180] The apparatus 4000 has an atmosphere-side substrate supply chamber 4010, an atmosphere-side substrate transfer chamber 4012 for transferring substrates from the atmosphere-side substrate supply chamber 4010, a load lock chamber 4020a for transferring substrates and switching the pressure inside the chamber from atmospheric pressure to reduced pressure or from reduced pressure to atmospheric pressure, an unload lock chamber 4020b for transferring substrates and switching the pressure inside the chamber from reduced pressure to atmospheric pressure or from atmospheric pressure to reduced pressure, a transfer chamber 4029 and a transfer chamber 4039 for transferring substrates in a vacuum, a transfer chamber 4030a and a transfer chamber 4030b connecting the transfer chamber 4029 and the transfer chamber 4039, and treatment chambers 4024a, 4024b, 4034a, 4034b, 4034c, 4034d, and 4034e for performing film formation or heating.
[0181] The multiple processing chambers can each perform different processes in parallel. Therefore, a stacked structure of different film types can be easily fabricated. Parallel processing can be performed up to the number of processing chambers. For example, the apparatus 4000 shown in FIG. 10 has seven processing chambers. Therefore, seven film formation processes can be performed consecutively using one apparatus (also referred to as in-situ in this specification) without being exposed to the atmosphere.
[0182] On the other hand, in a laminated structure, the number of layers that can be produced without exposing to the atmosphere is not necessarily the same as the number of processing chambers. For example, if the desired laminated structure has multiple layers of the same material, the layers can be provided in one processing chamber, so that a laminated structure with a greater number of layers than the number of processing chambers installed can be produced.
[0183] The atmosphere side substrate supply chamber 4010 also includes a cassette port 4014 for accommodating substrates, and an alignment port 4016 for aligning the substrates. Note that the configuration may include a plurality of cassette ports 4014 (for example, three in FIG. 10).
[0184] The atmosphere side substrate transfer chamber 4012 is connected to the load lock chamber 4020a and the unload lock chamber 4020b. The transfer chamber 4029 is connected to the load lock chamber 4020a, the unload lock chamber 4020b, the transfer chamber 4030a, the transfer chamber 4030b, the processing chamber 4024a, and the processing chamber 4024b. The transfer chamber 4030a and the transfer chamber 4030b are connected to the transfer chamber 4029 and the transfer chamber 4039. The transfer chamber 4039 is connected to the transfer chamber 4030a, the transfer chamber 4030b, the processing chamber 4034a, the processing chamber 4034b, the processing chamber 4034c, the processing chamber 4034d, and the processing chamber 4034e.
[0185] A gate valve 4028 or a gate valve 4038 is provided at the connection between the chambers, and each chamber can be independently maintained in a vacuum state, except for the atmosphere side substrate supply chamber 4010 and the atmosphere side substrate transfer chamber 4012. The atmosphere side substrate transfer chamber 4012 has a transfer robot 4018. The transfer chamber 4029 has a transfer robot 4026, and the transfer chamber 4039 has a transfer robot 4036. The transfer robot 4018, the transfer robot 4026, and the transfer robot 4036 each have a plurality of movable parts and an arm that holds a substrate, and can transfer a substrate to each chamber.
[0186] The number of transfer chambers, processing chambers, load lock chambers, unload lock chambers and transport chambers is not limited to the above, and an optimum number can be provided depending on the installation space and process conditions.
[0187] In particular, when there are multiple transfer chambers, it is preferable to have two or more transfer chambers between one transfer chamber and another transfer chamber. For example, as shown in Fig. 10, when there are transfer chambers 4029 and 4039, it is preferable to arrange transfer chambers 4030a and 4030b in parallel between transfer chambers 4029 and 4039.
[0188] By arranging the transfer chamber 4030a and the transfer chamber 4030b in parallel, for example, a step in which the transfer robot 4026 carries a substrate into the transfer chamber 4030a and a step in which the transfer robot 4036 carries a substrate into the transfer chamber 4030b can be performed simultaneously. Also, a step in which the transfer robot 4026 carries a substrate out of the transfer chamber 4030b and a step in which the transfer robot 4036 carries a substrate out of the transfer chamber 4030a can be performed simultaneously. In other words, by driving multiple transfer robots simultaneously, production efficiency is improved.
[0189] 10 shows an example in which one transfer chamber has one transfer robot and is connected to multiple processing chambers, but the present invention is not limited to this structure. One transfer chamber may have multiple transfer robots.
[0190] In addition, one or both of the transfer chamber 4029 and the transfer chamber 4039 are connected to a vacuum pump and a cryopump via valves. Therefore, the transfer chamber 4029 and the transfer chamber 4039 are evacuated from atmospheric pressure to a low or medium vacuum (several hundred Pa to about 0.1 Pa) using a vacuum pump, and then the valve is switched and the cryopump is used to evacuate from the medium vacuum to a high or ultra-high vacuum (0.1 Pa to 1×10 -7 It is possible to evacuate to a pressure of approximately 10 Pa.
[0191] Also, for example, two or more cryopumps may be connected in parallel to one transfer chamber. By having multiple cryopumps, even if one cryopump is in regeneration, it is possible to use the other cryopumps to pump air. Note that regeneration is the process of releasing molecules (or atoms) that have accumulated in the cryopump. If a cryopump accumulates too many molecules (or atoms), its pumping capacity will decrease, so it is a good idea to regenerate it periodically.
[0192] The processing chambers 4024a, 4024b, 4034a, 4034b, 4034c, 4034d, and 4034e can each perform different processes in parallel. That is, in each processing chamber, a film formation process using, for example, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like, a heat treatment, or a plasma treatment can be performed on a substrate placed therein. In addition, a film formation process may be performed in the processing chamber after a heat treatment or a plasma treatment is performed.
[0193] The apparatus 4000 has multiple processing chambers, and thus can transport the substrate between processing steps without exposing it to the atmosphere, thereby preventing impurities from being adsorbed on the substrate. In addition, since each processing chamber can perform a film formation process for different types of films, a heat treatment process, or a plasma treatment process, the order of film formation, heat treatment, etc. can be freely determined.
[0194] Each processing chamber may be connected to a vacuum pump via a valve. As the vacuum pump, for example, a dry pump, a mechanical booster pump, or the like can be used.
[0195] Each processing chamber may be connected to a power source capable of generating plasma. The power source may be a DC power source, an AC power source, or a high-frequency (RF, microwave, etc.) power source. A pulse generator may be connected to the DC power source.
[0196] The processing chamber may be connected to a gas purification device via a gas supply device. The gas supply devices and gas purification devices may be provided in the same number as the number of gas types.
[0197] For example, when a film formation process by sputtering is performed in a process chamber, the process chamber may include a target, a backing plate connected to the target, a cathode arranged facing the target via the backing plate, an adhesion prevention plate, a substrate stage, etc. Also, for example, the substrate stage may include a substrate holding mechanism for holding a substrate, a back surface heater for heating the substrate from the back surface, etc.
[0198] The substrate stage is held in a generally vertical position relative to the floor during film formation, and is held in a generally horizontal position relative to the floor during substrate transfer. By holding the substrate stage generally vertical to the floor, the probability that dust or particles that may be mixed in during film formation will adhere to the substrate can be reduced more than if the substrate stage were held horizontal. However, if the substrate stage is held vertical (90°) relative to the floor, there is a risk that the substrate will fall, so the angle of the substrate stage relative to the floor is preferably 80° or more and less than 90°.
[0199] The configuration of the substrate stage is not limited to the above. For example, the substrate stage may be configured to be approximately horizontal with respect to the floor surface. In this configuration, the target may be placed below the substrate stage, and the substrate may be placed between the target and the substrate stage. The substrate stage may also include a jig for fixing the substrate so that the substrate does not fall, or a mechanism for fixing the substrate.
[0200] Furthermore, by providing an adhesion prevention plate in the processing chamber, it is possible to prevent the particles sputtered from the target from accumulating in unnecessary areas. It is also desirable to process the adhesion prevention plate so that the accumulated sputtered particles do not peel off. For example, a blasting process may be performed to increase the surface roughness, or the surface of the adhesion prevention plate may be provided with irregularities.
[0201] The backing plate has a function of holding the target, and the cathode has a function of applying a voltage (for example, a negative voltage) to the target.
[0202] Note that the target may be a conductor, an insulator, or a semiconductor. For example, when the target is an oxide semiconductor such as a metal oxide, an oxide semiconductor film can be formed in the treatment chamber. Even when the target is a metal oxide, an oxynitride semiconductor film can be formed by using nitrogen gas as a film formation gas.
[0203] Each processing chamber may be connected to a gas supply device via a gas heating mechanism. The gas heating mechanism is connected to a gas purification device via a gas supply device. The gas introduced into the processing chamber may have a dew point of -80°C or less, preferably -100°C or less, more preferably -120°C or less, and may be, for example, oxygen gas, nitrogen gas, or a rare gas (such as argon gas). The gas introduced into the processing chamber may be heated to 40°C or more and 400°C or less by the gas heating mechanism. The gas heating mechanism, gas supply device, and gas purification device may be provided in the same number as the number of gas types.
[0204] Each processing chamber may be connected to a turbo molecular pump and a vacuum pump via a valve, and each processing chamber may be provided with a cryotrap.
[0205] A cryotrap is a mechanism capable of adsorbing molecules (or atoms) with a relatively high melting point, such as water. A turbomolecular pump is excellent in productivity because it stably pumps large-sized molecules (or atoms) and requires little maintenance, but has a low pumping capacity for hydrogen and water. Therefore, a cryotrap can be used to improve the pumping capacity for water and the like. The temperature of the cryotrap refrigerator is 100K or less, preferably 80K or less. In addition, when a cryotrap has multiple refrigerators, it is preferable to change the temperature of each refrigerator, since this allows for efficient pumping. For example, the temperature of the first-stage refrigerator may be 100K or less, and the temperature of the second-stage refrigerator may be 20K or less.
[0206] The exhaust method of the processing chamber is not limited to this, and may be the same as the exhaust method of the connected transfer chamber (exhaust method of a cryopump and a vacuum pump). The exhaust method of the transfer chamber may be the same as the exhaust method of the processing chamber (exhaust method of a turbo molecular pump and a vacuum pump).
[0207] In particular, a combination of a vacuum pump and a cryotrap may be used as an exhaust means for the treatment chamber in which the oxide semiconductor film is formed. It is preferable that an exhaust means provided in the treatment chamber in which the oxide semiconductor film is formed has a function of adsorbing at least water molecules.
[0208] In addition, the partial pressure of hydrogen molecules in the treatment chamber for forming the oxide semiconductor film was 1×10 -2 Pa or less, and the partial pressure of water molecules is 1×10 -4 In addition, the pressure in the treatment chamber in which the oxide semiconductor film is formed in a standby state is preferably 8.0×10 Pa or less. -5 Pa or less, preferably 5.0×10 -5 Pa or less, more preferably 1.0×10 -5 The partial pressure of hydrogen molecules and the partial pressure of water molecules are values when the processing chamber in which sputtering is performed is in a standby state and in a film forming state (plasma is in a discharging state) as described above.
[0209] The total pressure and partial pressure of the process chamber can be measured using a mass spectrometer, for example, a quadrupole mass spectrometer (also called Q-mass) Qulee CGM-051 manufactured by ULVAC, Inc.
[0210] When the partial pressure of hydrogen molecules, the partial pressure of water molecules, and the pressure in the standby state in the treatment chamber are set to the above ranges, the impurity concentration in the oxide semiconductor film to be formed can be low.
[0211] In particular, by using each treatment chamber for a film formation process by sputtering, part of the configuration of the transistor 200 described in the above embodiment can be manufactured to have a stacked structure in which films are successively formed in situ.
[0212] In a method for manufacturing the transistor 200, the conductor 242, the metal oxide 243, the oxide 230a, and the oxide 230b are successively formed using an apparatus 4000.
[0213] In other words, the conductor 242, the metal oxide 243, the oxide 230a, and the oxide 230b can be formed in succession without exposure to the atmosphere.
[0214] With the above-mentioned configuration, it is possible to form a laminated film from which impurities (typically, water, hydrogen, etc.) are thoroughly eliminated. In addition, since each interface of the laminated film is not exposed to the atmosphere, the impurity concentration is reduced.
[0215] Furthermore, for example, when heat treatment is performed in a treatment chamber, the treatment chamber may include a plurality of heating stages capable of storing substrates. The heating stages may be configured in multiple stages. By increasing the number of heating stages, a plurality of substrates can be simultaneously heat-treated, thereby improving productivity.
[0216] The heating mechanism that can be used in the processing chamber may be, for example, a heating mechanism that uses a resistance heating element for heating. Alternatively, it may be a heating mechanism that uses heat conduction or heat radiation from a medium such as a heated gas for heating. For example, RTAs (Rapid Thermal Anneals) such as GRTA (Gas Rapid Thermal Anneal) and LRTA (Lamp Rapid Thermal Anneal) can be used. LRTAs heat the workpiece by radiation of light (electromagnetic waves) emitted from lamps such as halogen lamps, metal halide lamps, xenon arc lamps, carbon arc lamps, high pressure sodium lamps, and high pressure mercury lamps. GRTAs perform heat treatment using high-temperature gas. An inert gas is used as the gas.
[0217] The load lock chamber 4020a may include a substrate transfer stage, a backside heater for heating the substrate from the backside, etc. The load lock chamber 4020a increases the pressure from a reduced pressure state to the atmosphere, and when the pressure in the load lock chamber 4020a reaches atmospheric pressure, the substrate transfer stage receives the substrate from the transfer robot 4018 provided in the atmosphere side substrate transfer chamber 4012. Thereafter, the load lock chamber 4020a is evacuated to a reduced pressure state, and then the transfer robot 4026 provided in the transfer chamber 4029 receives the substrate from the substrate transfer stage.
[0218] The load lock chamber 4020a is connected to a vacuum pump and a cryopump via valves. The unload lock chamber 4020b may have the same configuration as the load lock chamber 4020a.
[0219] The atmosphere side substrate transfer chamber 4012 has a transfer robot 4018, so that the transfer robot 4018 can transfer substrates between the cassette port 4014 and the load lock chamber 4020a. A mechanism for suppressing the intrusion of dust or particles, such as a HEPA filter (High Efficiency Particulate Air Filter), may be provided above the atmosphere side substrate transfer chamber 4012 and the atmosphere side substrate supply chamber 4010. The cassette port 4014 can store a plurality of substrates.
[0220] By using the above-described apparatus 4000 to successively form an insulating film, a semiconductor film, and a conductive film without exposure to the atmosphere, it is possible to suitably suppress the intrusion of impurities into the semiconductor film.
[0221] As described above, by using the apparatus according to one embodiment of the present invention, a stacked structure including a semiconductor film can be manufactured by successive film formation. Therefore, impurities such as hydrogen and water that are taken into the semiconductor film can be suppressed, and a semiconductor film with a low density of defect states can be manufactured.
[0222] The structures, methods, and the like described in this embodiment mode can be used in appropriate combination with structures, methods, and the like described in other embodiment modes and examples.
[0223] (Embodiment 3) In this embodiment mode, an example in which the semiconductor device described in the above embodiment mode is applied to an electronic component and an example in which the semiconductor device is applied to an electronic device including the electronic component will be described with reference to FIGS.
[0224] 11A illustrates an example in which the semiconductor device described in the above embodiment is applied to an electronic component. The electronic component is also called a semiconductor package or an IC package. There are multiple standards and names for this electronic component depending on the terminal extraction direction and terminal shape. Therefore, in this embodiment, an example of this will be described.
[0225] A semiconductor device constituted by transistors as shown in FIGS. 2A, 2B, and 2C in the above-mentioned first embodiment is completed by assembling a plurality of detachable parts to a printed circuit board through an assembly process (post-process).
[0226] The back-end process can be completed through the steps shown in Fig. 11A. Specifically, after the element substrate obtained in the front-end process is completed (step S1), the back surface of the substrate is ground (step S2). By thinning the substrate at this stage, warping of the substrate in the front-end process can be reduced, and the component can be made smaller.
[0227] A dicing process is performed in which the back surface of the substrate is ground to separate the substrate into multiple chips. Then, a die bonding process is performed in which the separated chips are individually picked up and mounted and bonded onto a lead frame (step S3). The bonding between the chip and the lead frame in this die bonding process is performed by selecting a method appropriate for the product, such as bonding with resin or tape. Note that the die bonding process may also be performed by mounting and bonding on an interposer.
[0228] Next, wire bonding is performed to electrically connect the leads of the lead frame and the electrodes on the chip with thin metal wires (step S4). Silver wires or gold wires can be used as the thin metal wires. The wire bonding can be ball bonding or wedge bonding.
[0229] The wire-bonded chip is subjected to a molding process in which it is sealed with epoxy resin or the like (step S5). By carrying out the molding process, the inside of the electronic component is filled with resin, which reduces damage to the built-in circuitry and wires caused by external mechanical forces, and also reduces deterioration of characteristics caused by moisture and dust.
[0230] Next, the leads of the lead frame are plated, and then cut and shaped (step S6). This plating process prevents the leads from rusting, and allows for more reliable soldering when mounting the leads on a printed circuit board later.
[0231] Next, a printing process (marking) is applied to the surface of the package (step S7), and the electronic component is completed after a final inspection process (step S8) (step S9).
[0232] The electronic component described above can be configured to include the semiconductor device described in the above embodiment. Therefore, it is possible to realize an electronic component having a semiconductor device that reduces malfunctions in high-temperature environments and reduces manufacturing costs. Since the electronic component includes a semiconductor device that reduces malfunctions in high-temperature environments and reduces manufacturing costs, it is an electronic component that is miniaturized and has relaxed restrictions on the usage environment.
[0233] 11B shows a schematic perspective view of a completed electronic component. FIG. 11B shows a schematic perspective view of a QFP (Quad Flat Package) as an example of an electronic component. An electronic component 700 shown in FIG. 11B has leads 701 and a semiconductor device 703. The electronic component 700 shown in FIG. 11B is mounted on, for example, a printed circuit board 702. A plurality of such electronic components 700 are combined and electrically connected on the printed circuit board 702 to complete a board (mounted board 704) on which electronic components are mounted. The completed mounted board 704 is provided inside an electronic device or the like.
[0234] Next, referring to Figures 12A and 12B, an application example in which the above-mentioned electronic components are applied to a drive circuit that drives an inverter, a motor, etc., provided in a vehicle (such as a bicycle) that is powered by electric power from a fixed power source will be described.
[0235] Fig. 12A shows an electric bicycle 1010 as an application example. The electric bicycle 1010 obtains power by passing a current through a motor unit 1011. The electric bicycle 1010 also has a battery 1012 for supplying the current to the motor unit 1011, and a drive circuit 1013 for driving the motor unit. Note that although pedals are shown in Fig. 12A, they may be omitted.
[0236] A mounting board provided with an electronic component having the semiconductor device described in the above embodiment is mounted on the driver circuit 1013. Therefore, restrictions on the usage environment can be alleviated, and an electric bicycle provided with miniaturized electronic components can be realized.
[0237] 12B shows an electric vehicle 1020 as another application example. The electric vehicle 1020 obtains power by passing a current through a motor unit 1021. The electric vehicle 1020 also has a battery 1022 for supplying the current to the motor unit 1021, and a drive circuit 1023 for driving the motor unit.
[0238] A mounting board provided with an electronic component having the semiconductor device described in the above embodiment is mounted on the driver circuit 1023. Therefore, restrictions on the usage environment are alleviated, and an electric vehicle including miniaturized electronic components can be realized.
[0239] As described above, the electronic device shown in this embodiment is equipped with a mounting board provided with an electronic component having the semiconductor device according to the previous embodiment, which alleviates restrictions on the usage environment and realizes an electronic device equipped with a miniaturized electronic component.
[0240] The structures, methods, and the like described in the above-described embodiment modes can be used in appropriate combination with structures, methods, and the like described in other embodiment modes and examples. EXAMPLES
[0241] In this example, the aggregation morphology of the metal oxide film was analyzed. Specifically, a sample having a metal oxide film was subjected to selected area electron diffraction (SAED: Selected Area Electron Diffraction). In addition, the sample was observed using a dark-field observation method and a bright-field observation method.
[0242] First, the samples used in this embodiment will be described.
[0243] First, a sample is prepared. As shown in FIG. 13A, the sample includes a substrate 800, an oxide film 801 on the substrate 800, and a metal oxide film 802 on the oxide film 801. The substrate 800 is a substrate containing silicon. The oxide film 801 is a silicon oxide film having a thickness of 100 nm, which is formed by heat-treating the surface of the substrate 800 in a hydrogen chloride (HCl) atmosphere. The metal oxide film 802 is an IGZO film having a thickness of 3 μm, which is formed by a sputtering method. The metal oxide film 802 is formed using an oxide target with an atomic ratio of In:Ga:Zn=4:2:4.1, argon gas of 30 sccm and oxygen gas of 15 sccm as film-forming gases, with a film-forming pressure of 0.4 Pa, a film-forming power of 500 W, a substrate temperature of 200° C., and a distance between the target and the substrate of 60 cm.
[0244] Next, the above sample was processed using a focused ion beam (FIB) to prepare a sample for cross-sectional observation and a sample for planar observation.
[0245] The above is a description of the samples used in this embodiment.
[0246] In order to examine the crystal structure of the metal oxide film 802, SAED was performed on a cross-sectional observation sample. For SAED, a transmission electron microscope "H-9500" manufactured by Hitachi High-Technologies Corporation was used. The diameter of the SAED measurement area (sometimes called a limited-view area) was about 3 μm.
[0247] Since the metal oxide film 802 is thick, the intensity of the electron beam spot can be increased in a selected area diffraction pattern obtained by performing SAED.
[0248] The selected-area diffraction patterns of the cross-section observation sample obtained by performing SAED are shown in Fig. 13B and Fig. 13C. The selected-area regions of the selected-area diffraction patterns shown in Fig. 13B and Fig. 13C are regions 810 and 811 shown by dotted circles in Fig. 13A, respectively. That is, Fig. 13B is a selected-area diffraction pattern in the case where the selected-area region is located in the metal oxide film 802. Fig. 13C is a selected-area diffraction pattern in the case where the selected-area region extends over the metal oxide film 802, the oxide film 801, and the substrate 800.
[0249] In the selected area diffraction patterns shown in Figures 13B and 13C, the spot observed in the center is a spot of transmitted wave (000). The bow-shaped spot observed above the center, shown in the area surrounded by a dotted line in Figure 13B, is a spot of diffracted wave (009). Figure 13B shows that the metal oxide film 802 is a CAAC-IGZO film.
[0250] Next, a bright-field electron microscope image (also called a bright-field image) of the cross-sectional observation sample was observed using bright-field observation, a technique for extracting and imaging transmitted waves. The transmitted waves used for imaging are extracted by positioning the objective aperture so that the transmitted waves are transmitted and diffracted waves are blocked. A Hitachi High-Technologies transmission electron microscope "H-9500" was used to observe the bright-field image.
[0251] A bright-field image of the sample for cross-sectional observation is shown in Fig. 14. Fig. 14 is a bright-field image of a metal oxide film 802 and an oxide film 801.
[0252] As shown in Fig. 14, a unique contrast was observed in the metal oxide film 802 in the bright-field image of the cross-section observation sample. This contrast is presumed to contain information due to different crystal orientations. This suggests that there are regions with different orientation orders, several tens of nanometers in size, in the metal oxide film 802.
[0253] Next, in order to capture the partial orientation state of the metal oxide film 802, a dark-field electron microscope image (also called a dark-field image) of the cross-sectional observation sample was observed using a dark-field observation method, which is a method of extracting and imaging specific diffracted waves. The diffracted waves used for imaging are extracted by positioning the objective aperture so that the diffracted waves are transmitted and the transmitted waves are blocked. Since the diffracted waves are observed as spots in a selected-area diffraction pattern, the dark-field image may be referred to as a dark-field image obtained by extracting the spots of the diffracted waves observed in the selected-area diffraction pattern with the objective aperture. A transmission electron microscope "H-9500" manufactured by Hitachi High-Technologies was used to observe the dark-field image.
[0254] The selected area electron diffraction pattern of the cross-sectional observation sample is shown in Fig. 15A. Fig. 15A is a selected area diffraction pattern of the cross-sectional observation sample near the surface of the metal oxide film 802.
[0255] Dark-field images of the cross-sectional observation sample are shown in Figs. 15B to 15D. Figs. 15B to 15D are dark-field images of the vicinity of the surface of the metal oxide film 802, using the spot of the diffracted wave (009) observed in the selected area diffraction pattern shown in Fig. 15A. Fig. 15B is a dark-field image obtained when the region 820 (left side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 15A is extracted by the objective aperture. Fig. 15C is a dark-field image obtained when the region 821 (center and periphery of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 15A is extracted by the objective aperture. Fig. 15D is a dark-field image obtained when the region 822 (right side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 15A is extracted by the objective aperture. The dark-field images shown in FIGS. 15B to 15D are formed near the surface, which is the uppermost part of the metal oxide film 802, and all have the same field of view.
[0256] In the dark-field image when region 820 is extracted (see FIG. 15B) and the dark-field image when region 822 is extracted (see FIG. 15D), string-like contrast was observed slightly tilted from the normal direction of the substrate surface. On the other hand, in the dark-field image when region 821 is extracted (see FIG. 15C), a region with a peculiar orientation state was not clearly observed compared to the dark-field image when region 820 is extracted and the dark-field image when region 822 is extracted. In addition, in this cross-sectional observation, the information on the thickness of the sample prepared by FIB processing is included as information in the depth direction, so there is a possibility that the orientation order of the CAAC structure forms a crystal layer while tilting also in the normal direction of the substrate surface.
[0257] 16A shows a selected area electron diffraction pattern of the sample for cross-sectional observation, which is near the surface of the oxide film 801.
[0258] Also, dark-field images of the cross-sectional observation sample are shown in Figs. 16B to 16D. Figs. 16B to 16D are dark-field images of the oxide film 801 using the spot of the diffracted wave (009) observed in the selected area diffraction pattern shown in Fig. 16A. Fig. 16B is a dark-field image obtained when the region 825 (left side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 16A is extracted by the objective aperture. Fig. 16C is a dark-field image obtained when the region 826 (center and periphery of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 16A is extracted by the objective aperture. Fig. 16D is a dark-field image obtained when the region 827 (right side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 16A is extracted by the objective aperture. The dark-field images shown in Figs. 16B to 16D are formed near the oxide film 801, and all have the same field of view.
[0259] Next, in order to minimize information in the depth direction, a sample for cross-sectional observation was prepared by processing it as thin as possible in the depth direction (thinning it), and the selected area diffraction pattern and dark-field image of the sample for cross-sectional observation were observed.
[0260] The selected area diffraction pattern of the sliced sample for cross-sectional observation is shown in Fig. 17A. Fig. 17A shows the selected area diffraction pattern of the sliced sample for cross-sectional observation near the surface of the metal oxide film 802.
[0261] Dark-field images of the sliced sample for cross-section observation are shown in Figs. 17B to 17D. Figs. 17B to 17D are dark-field images of the surface of the metal oxide film 802 using the spot of the diffracted wave (009) observed in the selected area diffraction pattern shown in Fig. 17A. Fig. 17B is a dark-field image obtained when the region 830 (left side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 17A is extracted by the objective aperture. Fig. 17C is a dark-field image obtained when the region 831 (center and periphery of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 17A is extracted by the objective aperture. Fig. 17D is a dark-field image obtained when the region 832 (right side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 17A is extracted by the objective aperture. The dark-field images shown in FIGS. 17B to 17D are formed near the surface, which is the uppermost part of the metal oxide film 802, and all have the same field of view.
[0262] In the dark-field image when the region 830 is extracted (see FIG. 17B) and the dark-field image when the region 832 is extracted (see FIG. 17D), a bundle of contrasts that is slightly tilted from the direction perpendicular to the substrate surface is observed. On the other hand, in the dark-field image when the region 831 is extracted (see FIG. 17C), crystal groups having a unique orientation state as a whole are hardly observed, compared with the dark-field image when the region 830 is extracted and the dark-field image when the region 832 is extracted. Therefore, it is presumed that the metal oxide film 802 is composed of crystal groups having a very long oriented structure in the direction perpendicular to the substrate surface. Furthermore, contrasts in different orientation regions were observed in the dark-field image when the region 830 is extracted and the dark-field image when the region 832 is extracted. Therefore, if these contrasts are connected via the dark-field image when the region 831 is extracted, it is presumed that the continuity of the crystal groups in the metal oxide film 802 is maintained even if string-like contrasts are observed.
[0263] It is presumed that in the dark-field image (see FIG. 17C) obtained by extracting the region 831, information oriented in all directions is concentrated and imaged. This is presumed to be because, due to the thinning of the cross-sectional observation sample, information on the crystal group oriented at an angle in the depth direction of the cross-sectional observation sample is lost, and the diffraction intensity of the crystal group having an orientation vector close to the depth direction of the cross-sectional observation sample cannot be obtained sufficiently. Therefore, it is presumed that the information on the crystal group having an orientation vector close to the depth direction of the cross-sectional observation sample is not observed brightly in the dark-field image obtained by extracting the regions (regions 830 and 832) that are out of the center of the spot of the diffracted wave (009).
[0264] 18A shows a selected area diffraction pattern of a sliced sample for cross-sectional observation in the vicinity of oxide film 801.
[0265] Also, dark-field images of the sliced sample for cross-section observation are shown in Figs. 18B to 18D. Figs. 18B to 18D are dark-field images of the oxide film 801 using the spot of the diffracted wave (009) observed in the selected area diffraction pattern shown in Fig. 18A. Fig. 18B is a dark-field image of the region 835 (left side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 18A extracted by the objective aperture. Fig. 18C is a dark-field image of the region 836 (center and periphery of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 18A extracted by the objective aperture. Fig. 18D is a dark-field image of the region 837 (right side of the spot of the diffracted wave (009)) shown by the dotted line in Fig. 18A extracted by the objective aperture. The dark-field images shown in Figs. 18B to 18D are formed near the oxide film 801, and all have the same field of view.
[0266] 18B to 18D, string-like contrasts were obtained that indicated oriented regions with a width of about 10 nm and extending in the normal direction to the substrate surface. Furthermore, it was confirmed that the growth of a crystal layer of the metal oxide film 802 started from a point less than 1 nm away from the interface with the oxide film 801, and that the crystal layer was oriented at an angle of about 2 to 3 degrees to the normal direction to the substrate surface.
[0267] In order to evaluate the distribution of crystalline layers with long-range order observed as string-like contrast in the sliced samples for cross-sectional observation, we observed dark-field images of the samples for planar observation, in which the spots of the diffracted waves (100) were extracted using the objective aperture. Note that an atomic resolution analytical electron microscope "JEM-ARM200F" manufactured by JEOL Ltd. was used to observe the selected-area electron diffraction patterns, dark-field images, bright-field images, and high-resolution images of the samples for planar observation.
[0268] The selected area electron diffraction pattern of the sample for planar observation is shown in Fig. 19A. Fig. 19A is a selected area diffraction pattern of the metal oxide film 802 sample for planar observation.
[0269] Also, dark-field images of the sample for planar observation are shown in Figs. 19B to 19D. Figs. 19B to 19D are dark-field images of the metal oxide film 802 using the spots of the diffracted waves (100) observed in the selected area diffraction pattern shown in Fig. 19A. Fig. 19B is a dark-field image when the region 840 (left side of the spot of one diffracted wave (100)) shown by the dotted line in Fig. 19A is extracted by the objective aperture. Fig. 19C is a dark-field image when the region 841 (center and periphery of the spot of one diffracted wave (100)) shown by the dotted line in Fig. 19A is extracted by the objective aperture. Fig. 19D is a dark-field image when the region 842 (right side of the spot of one diffracted wave (100)) shown by the dotted line in Fig. 19A is extracted by the objective aperture. All the dark-field images shown in Figs. 19B to 19D are of the same field of view.
[0270] 19B to 19D, in the metal oxide film 802, the orientation order represented by the spots of the diffracted wave (100) was distributed with a size of about 100 nm, and it was observed as a contrast in the dark-field image that the orientation region tilted by several degrees was connected to this vertical orientation region.
[0271] FIG. 20A shows a bright-field image of the sample for planar observation. FIG. 20B shows a dark-field image of the sample for planar observation. FIG. 20C and FIG. 20D show high-resolution images of the sample for planar observation. Note that the region of the bright-field image shown in FIG. 20A is the same as the region of the dark-field image shown in FIG. 20B. The high-resolution image shown in FIG. 20C is an image acquired for the region shown by the dotted line in FIG. 20B. The high-resolution image shown in FIG. 20D is an image acquired for the region shown by the dotted line in FIG. 20C.
[0272] 20B to 20D, the long-range orientational order that cannot be confirmed in the high-resolution image can be confirmed in the dark-field image.
[0273] From the above, it was found that the crystal orientation of the CAAC-IGZO film is continuous even in the nano region, which is larger than the atomic level, and the intermediate region between the bulk (the so-called mesoscopic region).
[0274] At least a part of the configurations, methods, and the like shown in this embodiment can be appropriately combined with other embodiment modes described in this specification. [Explanation of symbols]
[0275] 200 transistor, 210 substrate, 230 oxide, 230a oxide, 230b oxide, 240 opening, 240_1 opening, 240_2 opening, 240_3 opening, 240_4 opening, 242 conductor, 243 metal oxide, 245 metal oxide, 246 conductor, 248 conductor, 250 insulator, 250_1 insulator, 250_2 insulator, 250_3 insulator, 250_4 insulator, 250A insulating film, 260 conductor, 260_1 conductor, 260_2 conductor, 260_3 conductor, 260_4 conductor, 260A conductive film, 271 insulator, 272 insulator, 700 electronic component, 701 lead, 702 printed circuit board, 703 Semiconductor device, 704 mounting substrate, 800 substrate, 801 oxide film, 802 metal oxide film, 810 region, 811 region, 820 region, 821 region, 822 region, 825 region, 826 region, 827 region, 830 region, 831 region, 832 region, 835 region, 836 region, 837 region, 840 region, 841 region, 842 region, 1010 electric bicycle, 1011 motor unit, 1012 battery, 1013 drive circuit, 1020 electric vehicle, 1021 motor unit, 1022 battery, 1023 drive circuit, 4000 device, 4010 atmospheric side substrate supply chamber, 4012 atmospheric side substrate transfer chamber, 4014 cassette port, 4016 alignment port, 4018 Transfer robot, 4020a load lock chamber, 4020b unload lock chamber, 4024a processing chamber, 4024b processing chamber, 4026 transfer robot, 4028 gate valve, 4029 transfer chamber, 4030a transfer chamber, 4030b transfer chamber, 4034a processing chamber, 4034b processing chamber, 4034c processing chamber, 4034d processing chamber, 4034e processing chamber, 4036 transfer robot, 4038 gate valve, 4039 transfer chamber
Claims
[Claim 1] A substrate; a first conductor on the substrate; a first metal oxide on the first conductor; a first oxide on the first metal oxide; a second oxide on the first oxide; and a first insulator on the second oxide; and a second conductor on the first insulator; and a second insulator on the second conductor; and a third insulator having a region in contact with a side surface of the second conductor, a region in contact with a side surface of the first insulator, and a region in contact with a side surface of the second insulator; a second metal oxide having a region in contact with an upper surface of the second oxide, a region in contact with an upper surface of the second insulator, and a region in contact with an upper surface of the third insulator; a third conductor on the second metal oxide; the first oxide comprises at least indium or zinc; the second oxide comprises at least indium or zinc; the second conductor has a region overlapping the second oxide, the third conductor has a region in contact with the second metal oxide, the second metal oxide has a region in contact with the second oxide, The carrier concentration of the second oxide is lower than the carrier concentration of the first oxide; a carrier concentration of the first metal oxide is higher than a carrier concentration of the first oxide; A semiconductor device, wherein the second metal oxide has a higher carrier concentration than the first metal oxide.
Citation Information
Patent Citations
Metallic oxide thin film transistor and preparation method thereof
CN107452810A
Field effect transistor
JP2006041127A
Power insulated-gate field-effect transistor
JP2013062461A
Semiconductor element and diode
JP2015076540A
Semiconductor device and method for manufacturing semiconductor device
JP2018129503A