Piezoelectric fiber and method for manufacturing the same
By optimizing the molecular weight and crystallinity of poly(3-hydroxyalkanoate) resin in piezoelectric fibers, the fibers achieve improved piezoelectric performance while maintaining antibacterial and biodegradable properties.
Patent Information
- Application Number
- JP2023083958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Piezoelectric fibers containing poly(3-hydroxyalkanoate) resin with a weight average molecular weight of 50,000 to 500,000 exhibit insufficient piezoelectricity.
Incorporating a poly(3-hydroxyalkanoate) resin with a weight average molecular weight of 50,000 to 500,000 and achieving a crystallinity of 52% or more in the piezoelectric fibers through a heat treatment process, including melt spinning and drawing steps.
The resulting piezoelectric fibers demonstrate enhanced piezoelectricity, maintaining antibacterial properties without the use of harmful antibacterial agents and being biodegradable.
Smart Images

Figure 2024167706000002 
Figure 2024167706000003 
Figure 2024167706000004
Abstract
Description
[Technical field]
[0001] The present invention relates to piezoelectric fibers and methods for their manufacture. [Background technology]
[0002] Because piezoelectric fibers exhibit antibacterial properties, they are used as textile materials for clothing (socks, shoes, compression wear, underwear, etc.) and hygiene products (disposable diapers, masks). Other fibers that exhibit antibacterial properties are known to be fibers that contain antibacterial agents. However, unlike fibers that contain antibacterial agents, piezoelectric fibers have the advantage that their antibacterial properties do not decrease with post-processing such as washing, and can maintain their antibacterial properties semi-permanently. Furthermore, antibacterial agents can be harmful, and piezoelectric fibers have the advantage that they can exhibit antibacterial properties without containing such antibacterial agents.
[0003] In addition, because piezoelectric fibers exhibit sensing functions, they are also used as textile materials to make smart fabrics (clothing incorporating digital components (sensors, LEDs, batteries, microchips, etc.)) and are used in a variety of fields, including information and communications, medicine, nursing care, and sports.
[0004] Polyhydroxyalkanoates are known as resins with excellent biodegradability. As piezoelectric fibers containing polyhydroxyalkanoate, electrospun fibers of polyhydroxyalkanoate-based copolymers are known (Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2022-501480 Summary of the Invention [Problem to be solved by the invention]
[0006] Here, when a piezoelectric fiber containing a poly(3-hydroxyalkanoate) resin having a weight-average molecular weight of 50,000 to 500,000 was produced, the piezoelectricity of the piezoelectric fiber was not sufficient.
[0007] Therefore, an object of the present invention is to provide a piezoelectric fiber containing a poly(3-hydroxyalkanoate) resin having a weight-average molecular weight of 50,000 to 500,000, which has excellent piezoelectric properties. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that in piezoelectric fibers containing a poly(3-hydroxyalkanoate) resin having a weight average molecular weight of 50,000 to 500,000, the piezoelectricity of the piezoelectric fibers is enhanced when the crystallinity of the piezoelectric fibers is equal to or higher than a predetermined level.
[0009] That is, the first aspect of the present invention is a composition containing a poly(3-hydroxyalkanoate) resin, The weight average molecular weight of the poly(3-hydroxyalkanoate) resin is 50,000 to 500,000; The present invention relates to a piezoelectric fiber having a crystallinity of 52% or more.
[0010] A second aspect of the present invention is a method for producing the piezoelectric fiber, comprising the steps of: The present invention relates to a method for producing a piezoelectric fiber, the method comprising a heat treatment step of heat treating a filament to obtain the piezoelectric fiber. Effect of the Invention
[0011] According to the present invention, a piezoelectric fiber containing a poly(3-hydroxyalkanoate) resin having a weight average molecular weight of 50,000 to 500,000 can be provided, which has excellent piezoelectric properties. [Brief description of the drawings]
[0012] [Figure 1]Optical layout diagram for X-ray diffraction analysis (XRD analysis). [Diagram 2] FIG. 2 is a schematic diagram of an apparatus used in the melt spinning process of the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus used in the stretching step of the present embodiment. [Figure 4] FIG. 4 is a schematic diagram of an apparatus for use in the melt spinning and drawing steps of another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, one embodiment of the present invention will be described.
[0014] <Piezoelectric fiber> First, the piezoelectric fiber according to this embodiment will be described. The piezoelectric fiber according to this embodiment contains a poly(3-hydroxyalkanoate) resin. The poly(3-hydroxyalkanoate) resin has a weight average molecular weight of 50,000 to 500,000. The crystallinity of the piezoelectric fiber according to this embodiment is 52% or more.
[0015] The piezoelectric fiber according to this embodiment has a crystallinity of 52% or more, and therefore has excellent piezoelectric properties. The crystallinity is preferably 52.2% or more, more preferably 52.5% or more. The crystallinity is saturated at about 60%. If the crystallinity is too high, it may adversely affect the fiber quality due to whitening, etc., so the crystallinity is preferably 59% or less, more preferably 57% or less.
[0016] The crystallinity can be determined by X-ray diffraction analysis (XRD). The measurement conditions are, for example, as follows. Equipment: PANalytical X'Pert PRO MPD Analysis conditions: X-rays used: CuKα rays (whitening: focusing mirror) X-ray intensity 45kV, 40mA Detector: X' Celerator (semiconductor one-dimensional detector) Optical system arrangement Transmission (Debye-Scherrer optical system) Divergence slit 1 / 2deg Anti-scatter slit 1 / 2deg Measurement range 2θ=3~48deg (φ direction rotates at 1rps) Scanning speed: 0.02 deg / sec (step: 0.017 deg) For example, 60 fiber bundles are obtained as a sample from piezoelectric fibers, and the sample is fixed to a sample holder as shown in Figure 1. In order to eliminate the influence of orientation, the sample is rotated in the φ direction and 2θ scan is performed. Peak separation analysis is performed on the obtained 2θ scan profile to determine the area of the crystalline peak and the area of the amorphous halo peak (area of the amorphous peak), and the crystallinity is calculated using the following formula. Crystallinity [%] = crystalline peak area / (crystalline peak area + amorphous peak area) × 100
[0017] The piezoelectric fiber includes one or more single yarns. The piezoelectric fiber may be a multifilament or a monofilament. From the viewpoint of versatile use including general clothing, the piezoelectric fiber is preferably a multifilament. When the piezoelectric fiber is a multifilament, it preferably has 30 or more single yarns, more preferably 30 to 500,000 single yarns, and further preferably 50 to 300,000 single yarns.
[0018] The single yarn may be any yarn having a circular cross section (a concept including a perfect circle, an approximately circular shape, an ellipse, and an approximately ellipse) or a single yarn having a modified cross section.
[0019] The average fineness of the single yarn is preferably 0.5 detx or more, more preferably 1 to 1000 dtex, and further preferably 1.5 to 500 dtex. Since the average fineness of the single yarn is 0.5 dtex or more, the piezoelectric fiber according to this embodiment has an advantage that it can be used in general clothing, including underwear, which requires thinness and flexibility. The fineness of each single yarn can be measured using an autoblow type fineness measuring device "DENIER COMPUTER Type DC-11" (Search). When the piezoelectric fiber contains one single yarn, the fineness of the single yarn means the average fineness of the single yarn. Moreover, the average value means an arithmetic average value. When the number of single yarns contained in the piezoelectric fiber exceeds 20, the finenesses of 20 or more randomly selected single yarns are measured, and the arithmetic average value is calculated from the fineness values of all the measured single yarns.
[0020] The piezoelectric fiber according to the present embodiment is formed from a polymer composition that contains a polymer component. The polymer component contains a poly(3-hydroxyalkanoate) resin. The polymer component may contain other polymers in addition to the poly(3-hydroxyalkanoate) resin. The polymer composition may contain additives.
[0021] The poly(3-hydroxyalkanoate) resin is a polyester having 3-hydroxyalkanoic acid as a monomer. That is, the poly(3-hydroxyalkanoate) resin is a resin containing 3-hydroxyalkanoic acid as a constituent unit. Moreover, the poly(3-hydroxyalkanoate) resin is a biodegradable polymer. In this embodiment, "biodegradability" refers to a property that can be decomposed into low molecular weight compounds by microorganisms in nature. Specifically, the presence or absence of biodegradability can be determined based on tests suitable for each environment, such as ISO 14855 (compost) and ISO 14851 (activated sludge) under aerobic conditions, and ISO 14853 (aqueous phase) and ISO 15985 (solid phase) under anaerobic conditions. In addition, the decomposition by microorganisms in seawater can be evaluated by measuring biochemical oxygen demand. The poly(3-hydroxyalkanoate) resin may be a homopolymer or a copolymer.
[0022] The poly(3-hydroxyalkanoate) resin preferably contains a structural unit represented by the following formula (1). [-CHR-CH2-CO-O-] (1) (In the above formula (1), R is C p H 2p+1 and p represents an integer of 1 to 15.
[0023] The poly(3-hydroxyalkanoate) resin preferably includes a poly(3-hydroxybutyrate) resin. The poly(3-hydroxybutyrate)-based resin is a resin that contains a 3-hydroxybutyrate unit. The poly(3-hydroxybutyrate)-based resin may be a homopolymer or a copolymer.
[0024] Examples of the poly(3-hydroxyalkanoate) resin include P3HB, P3HB3HH, P3HB3HV, P3HB4HB, poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate), and the like. Here, P3HB means the homopolymer poly(3-hydroxybutyrate). P3HB3HH means poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). P3HB3HV means poly(3-hydroxybutyrate-co-3-hydroxyvalerate). P3HB4HB means poly(3-hydroxybutyrate-co-4-hydroxybutyrate).
[0025] Since P3HB has the function of promoting crystallization of P3HB itself and poly(3-hydroxyalkanoate) resins other than P3HB, it is preferable that the poly(3-hydroxyalkanoate) resin contains P3HB.
[0026] As the poly(3-hydroxyalkanoate) resin, from the viewpoint of achieving both excellent biodegradability and moldability, P3HB, P3HB3HH, P3HB3HV, P3HB4HB, and the like are preferred, but are not particularly limited. Moreover, as the poly(3-hydroxyalkanoate)-based resin, P3HB3HH is preferable from the viewpoint of increasing the strength and moldability of the piezoelectric fiber according to this embodiment.
[0027] The poly(3-hydroxyalkanoate) resin contains a copolymer having 3-hydroxybutyrate units, and the content of the 3-hydroxybutyrate units in the poly(3-hydroxyalkanoate) resin is preferably 85.5 mol % or more and 99.5 mol % or less. The content of the 3-hydroxybutyrate unit in the poly(3-hydroxyalkanoate) resin is more preferably 85.5 mol % or more and 97.0 mol % or less. When the content of the 3-hydroxybutyrate unit in the poly(3-hydroxyalkanoate) resin is 85.5 mol % or more, the rigidity of the piezoelectric fiber according to this embodiment is increased. In addition, since the content of the 3-hydroxybutyrate unit in the poly(3-hydroxyalkanoate) resin is 99.5 mol % or less, the piezoelectric fiber according to this embodiment has excellent flexibility.
[0028] The polymer component may contain only one type of the poly(3-hydroxyalkanoate) resin, or may contain two or more types of the poly(3-hydroxyalkanoate) resin. When the poly(3-hydroxyalkanoate) resin contains a copolymer (such as P3HB3HH), it may contain two or more types of copolymers having different average composition ratios of structural units. The poly(3-hydroxyalkanoate) resin contains two or more types of copolymers having different average composition ratios of structural units, which makes it easier to adjust the melting point and rigidity.
[0029] The weight average molecular weight of the poly(3-hydroxyalkanoate) resin is 50,000 to 500,000, and preferably 100,000 to 450,000. When the weight average molecular weight of the poly(3-hydroxyalkanoate) resin is 500,000 or less, the piezoelectric fiber according to this embodiment can be easily molded. When the weight average molecular weight of the poly(3-hydroxyalkanoate) resin is 50,000 or more, the strength of the piezoelectric fiber according to this embodiment can be increased. In the present embodiment, the weight average molecular weight is measured from the polystyrene equivalent molecular weight distribution by gel permeation chromatography (GPC) using chloroform as an eluent. As the column for the GPC, a column suitable for measuring the molecular weight may be used. For example, the weight average molecular weight (Mw) can be determined by setting the column temperature at 40°C, injecting 10 μl of 3 mg of the target substance dissolved in 2 ml of chloroform, and setting the flow rate of the chloroform eluent (mobile phase) to 1.0 ml / min. The GPC device used is an LC-10A system (manufactured by Shimadzu Corporation), and the column used is a GPCK-806M (manufactured by Showa Denko Corporation).
[0030] The other polymer is preferably biodegradable.
[0031] Other biodegradable polymers include, for example, polycaprolactone, polylactic acid, polybutylene succinate, polybutylene succinate adipate, polybutylene adipate terephthalate, polyethylene succinate, polyvinyl alcohol, polyglycolic acid, unmodified starch, modified starch, cellulose acetate, and chitosan. The polycaprolactone is a polymer obtained by ring-opening polymerization of ε-caprolactone. The polymer composition may contain one type of other polymer, or may contain two or more types of other polymers.
[0032] The piezoelectric fiber according to this embodiment contains a poly(3-hydroxyalkanoate)-based resin in an amount of preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0033] Since the piezoelectric fiber according to this embodiment contains a biodegradable polymer, even if the piezoelectric fiber is discarded in the environment, it is easily decomposed in the environment, and therefore the burden on the environment can be reduced.
[0034] Examples of additives include crystal nucleating agents, lubricants, stabilizers (antioxidants, ultraviolet absorbers, etc.), colorants (dyes, pigments, etc.), plasticizers, flame retardants, inorganic fillers, organic fillers, and antistatic agents.
[0035] The polymer composition preferably contains a crystal nucleating agent. The crystal nucleating agent is a compound capable of promoting the crystallization of the poly(3-hydroxyalkanoate) resin, and has a melting point higher than that of the poly(3-hydroxyalkanoate) resin. Examples of the crystal nucleating agent include inorganic substances (boron nitride, titanium oxide, talc, layered silicates, calcium carbonate, sodium chloride, metal phosphates, etc.); sugar alcohol compounds derived from natural products (pentaerythritol, erythritol, galactitol, mannitol, arabitol, etc.); polyvinyl alcohol; chitin; chitosan; polyethylene oxide; aliphatic carboxylates; aliphatic alcohols; aliphatic carboxylate esters; dicarboxylic acid derivatives (dimethyl adipate, dibutyl adipate, diisodecyl adipate, dibutyl selenite, etc.); Examples include cyclic compounds having C=O and a functional group selected from NH, S and O in the molecule (indigo, quinacridone, quinacridone magenta, etc.); sorbitol derivatives (bisbenzylidene sorbitol, bis(p-methylbenzylidene)sorbitol, etc.); compounds containing a nitrogen-containing heteroaromatic nucleus (pyridine ring, triazine ring, imidazole ring, etc.) (pyridine, triazine, imidazole, etc.); phosphate ester compounds; bisamides of higher fatty acids; metal salts of higher fatty acids; and branched polylactic acid. The poly(3-hydroxyalkanoate) resin P3HB can also be used as a crystal nucleating agent. These may be used alone or in combination of two or more.
[0036] As the crystal nucleating agent, from the viewpoint of the effect of improving the crystallization rate of the poly(3-hydroxyalkanoate)-based resin and from the viewpoint of compatibility and affinity with the poly(3-hydroxyalkanoate)-based resin, sugar alcohol compounds, polyvinyl alcohol, chitin, and chitosan are preferred. Among the sugar alcohol compounds, pentaerythritol is preferred.
[0037] The crystal nucleating agent preferably has a crystal structure at room temperature (25° C.). The crystal nucleating agent has a crystalline structure at room temperature (25° C.), which has the advantage of further promoting the crystallization of the poly(3-hydroxyalkanoate) resin. Moreover, the crystal nucleating agent having a crystal structure at room temperature (25° C.) is preferably in a powder form at room temperature (25° C.). Furthermore, the average particle size of the crystal nucleating agent in powder form at room temperature (25° C.) is preferably 10 μm or less.
[0038] The content of the crystal nucleating agent in the polymer composition is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin. By having the content of the crystal nucleating agent in the polymer composition be 0.05 parts by mass or more relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin, there is an advantage that the crystallization of the poly(3-hydroxyalkanoate)-based resin can be further promoted. The content of the crystal nucleating agent in the polymer composition is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin. By having the content of the crystal nucleating agent in the polymer composition be 10 parts by mass or less relative to 100 parts by mass of the poly(3-hydroxyalkanoate)-based resin, the viscosity of the melt can be reduced when producing piezoelectric fibers from the melt by melt spinning, which has the advantage of facilitating the production of piezoelectric fibers. In addition, since P3HB is a poly(3-hydroxyalkanoate) resin and can also function as a crystal nucleating agent, when the polymer composition contains P3HB, the amount of P3HB is included in both the amount of poly(3-hydroxyalkanoate) resin and the amount of crystal nucleating agent.
[0039] In the case where the piezoelectric fiber according to the present embodiment is a multifilament, the polymer composition preferably contains the lubricant. When the single yarn contains the lubricant, the lubricating property of the single yarn is improved, and the fusion of the single yarns can be suppressed. The lubricant may, for example, be a compound having an amide bond. The compound having an amide bond preferably includes at least one selected from lauric amide, myristic amide, stearic amide, behenic amide, and erucic amide.
[0040] The content of the lubricant in the polymer composition is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.5 parts by mass or more, based on 100 parts by mass of the polymer component. By having the content of the lubricant in the polymer composition be 0.05 parts by mass or more based on 100 parts by mass of the polymer component, there is an advantage in that the lubricating property of the single yarn is excellent. The content of the lubricant in the polymer composition is preferably 12 parts by mass or less, more preferably 10 parts by mass or less, further preferably 8 parts by mass or less, and most preferably 5 parts by mass or less, relative to 100 parts by mass of the polymer component. By having the content of the lubricant in the polymer composition be 12 parts by mass or less relative to 100 parts by mass of the polymer component, there is an advantage in that the lubricant can be prevented from bleeding out onto the surface of the piezoelectric fiber.
[0041] When the piezoelectric fiber according to this embodiment is a multifilament, it is preferable that the fiber further has a spinning oil on the surface of the single yarn, from the viewpoint of suppressing fusion between adjacent single yarns and suppressing separation of adjacent single yarns due to static electricity. Examples of the spinning oil include cationic surfactants, anionic surfactants, nonionic surfactants, refined esterified oils, mineral oils, poly(oxyethylene) alkyl ethers, silicone oils, paraffin waxes, etc. These may be used alone or in combination of two or more. From the viewpoint of suppressing fusion between adjacent filaments, the spinning oil is preferably silicone oil. From the viewpoint of preventing adjacent single yarns from being separated from each other due to static electricity, the spinning oil is preferably an anionic surfactant or a nonionic surfactant. As the spinning oil, for example, a spinning oil containing silicone oil and an anionic surfactant (for example, "Polymax FKY" manufactured by Marubishi Chemical Co., Ltd.) can be used.
[0042] The piezoelectric fiber according to this embodiment may be used as it is. Furthermore, a textile product (fibrous body) may be produced using the piezoelectric fiber according to this embodiment. The textile product can be in various forms (eg, in the form of a nonwoven fabric, etc.). The piezoelectric fiber and the textile product according to this embodiment can be suitably used for conventionally known applications. The piezoelectric fiber and textile product according to this embodiment can be used in various fields, such as information and communications, medicine, nursing care, and sports. In addition, the piezoelectric fiber according to this embodiment can be used as a fiber material for making smart fabrics (clothing incorporating digital components (sensors, LEDs, batteries, microchips, etc.)), clothing (socks, shoes, compression wear, underwear, etc.), hygiene products (disposable diapers, masks), etc.
[0043] <Method of manufacturing piezoelectric fiber> The piezoelectric fiber according to this embodiment is configured as described above. Next, a method for producing the piezoelectric fiber according to this embodiment will be described.
[0044] The method for producing a piezoelectric fiber according to this embodiment includes a heat treatment step of heat treating a filament to obtain the piezoelectric fiber. In the method for producing a piezoelectric fiber according to this embodiment, by carrying out the heat treatment step, a piezoelectric fiber having a high degree of crystallinity and excellent piezoelectric performance can be obtained.
[0045] Hereinafter, the method for producing a piezoelectric fiber will be described with reference to FIGS. 2 and 3 by taking as an example a method for producing a piezoelectric fiber which further includes a melt spinning step of obtaining a filament for drawing by discharging a molten material by a melt spinning method, and a drawing step of obtaining the filament as a drawn filament by drawing the filament for drawing, the melt spinning step and the drawing step being performed by a sequential drawing method, and the obtained piezoelectric fiber is a multifilament.
[0046] In the method for producing a piezoelectric fiber according to the present embodiment, the piezoelectric fiber is produced by a melt spinning method. In this case, by setting the weight average molecular weight of the poly(3-hydroxyalkanoate) resin to 50,000 to 500,000, it is possible to relatively easily and economically produce a piezoelectric fiber having an average single yarn fineness of 0.5 dtex or more.
[0047] (Melt spinning process) As shown in FIG. 2, in the melt spinning process, first, the molten material is charged into a material charging section 101 . Next, the material fed from the material feed section 101 is kneaded while being heated in a kneading extruder 102 to obtain the melt. The melt is the polymer composition in a molten state. A screw extruder is preferably used as the kneading extruder 102. The kneading extruder 102 may be a single screw extruder or a twin screw extruder.
[0048] Then, using a spinning nozzle 104 having a plurality of discharge holes, the molten material obtained in the kneading extruder 102 is discharged from the plurality of discharge holes to obtain a plurality of molten raw yarns 100A. The flow rate of the molten material discharged from the multiple discharge holes of the spinning nozzle 104 is adjusted by a gear pump 103 .
[0049] The temperature of the spinning nozzle 104 is, for example, 140 to 180°C.
[0050] The spinning nozzle 104 has two or more discharge holes, preferably 30 or more discharge holes, more preferably 30 to 10,000 discharge holes, and further preferably 30 to 5,000 discharge holes. The shape and size of each discharge hole are selected according to the characteristics required for the piezoelectric fiber (e.g., appearance, fineness, strength, cross-sectional shape, etc.). The shape of the discharge hole is, for example, circular (a concept including a perfect circle, an approximately circular shape, an ellipse, and an approximately ellipse). The area of each discharge hole is determined so as to be, for example, 10 to 5000 times the cross-sectional area of a single yarn in the filament to be drawn. In this embodiment, the ejection holes have substantially the same shape and substantially the same area. The area of each outlet hole is preferably 1.0×10 -3 ~20mm 2 , more preferably 5.0×10 -3 ~10mm 2 It is.
[0051] The speed at which the molten material is discharged from the spinning nozzle 104 (hereinafter also referred to as "spinning nozzle flow speed") is preferably 0.02 m / min to 20 m / min, more preferably 0.05 m / min to 10 m / min, and even more preferably 0.1 m / min to 5.0 m / min.
[0052] In this embodiment, the spinning oil may be applied to the surface of each of the cooled raw yarns 100A.
[0053] In the melt spinning step, gas is blown onto the obtained molten raw yarns to cool 30 or more raw yarns, thereby obtaining filaments to be drawn. In this embodiment, the raw yarn 100A is cooled by gas in a first cooling box 105. In this embodiment, the yarn 100A cooled in the first cooling box 105 may be further cooled with gas in a second cooling box .
[0054] In the melt spinning step, the temperature of the gas blown onto the obtained plurality of raw yarns 100A in a molten state is preferably 0 to 50°C, more preferably 0 to 40°C, and further preferably 15 to 40°C. Moreover, by setting the temperature of the gas to 0° C. or higher, fusion between the single yarns of the drawing filament can be suppressed. By setting the temperature of the gas to 50° C. or less, unevenness in the fineness of the single yarn of the drawing filament is suppressed. In addition, by setting the temperature of the gas to 50° C. or less, breakage of some of the raw yarns 100A can be suppressed. In the melt spinning step, the temperature of the gas is preferably equal to or higher than the glass transition temperature of the polymer composition, which makes the polymer composition more susceptible to plastic deformation and makes the yarn 100A less likely to break. The "temperature of the gas blown onto the obtained plurality of raw yarns 100A in a molten state" means the temperature of the gas when the gas comes into contact with the raw yarns 100A.
[0055] In the melt spinning process, the speed of the gas blown onto the multiple raw yarns is preferably 0.10 m / s or more, more preferably 0.20 to 5.0 m / s, even more preferably 0.20 to 3.0 m / s, even more preferably 0.30 to 3.0 m / s, and particularly preferably 0.32 to 3.0 m / s. When the velocity of the gas is 0.10 m / s or more, the cooling effect of the gas is easily exerted. By setting the gas velocity to 5.0 m / s or less, the molten yarn 100A discharged from the spinning nozzle 104 is prevented from being shaken by the gas. As a result, the molten yarns 100A are prevented from fusing together and / or breaking, thereby improving spinning stability. The term "speed of the gas blown onto the obtained plurality of raw yarns 100A in a molten state" refers to the relative speed of the gas with respect to the raw yarns 100A when the gas comes into contact with the raw yarns 100A.
[0056] Examples of the gas include air, inert gases (nitrogen gas, argon gas, etc.), and water vapor.
[0057] Examples of the gas blowing method include the circular method and the back method. The back surface method is a method in which the gas is blown onto multiple raw yarns 100A from one direction inside a cooling box when viewed in the longitudinal direction of the multiple raw yarns 100A (a cross-sectional view of the raw yarns A perpendicular to the longitudinal direction of the raw yarns A). The circular method uses a cooling box having a cylindrical side wall, and blows gas into the cylindrical box in a spiral shape along the inner circumferential surface of the cylindrical side wall, thereby blowing the gas onto the multiple raw yarns 100A. The flow direction of the multiple raw yarns 100A is approximately parallel to the virtual axis of the cylindrical side wall. The cooling box may have a cylindrical punched metal on the inside of the cylindrical side wall, and may further have a cylindrical mesh (e.g., 80 mesh) on the inside of the cylindrical punched metal. The outer diameter of the cylindrical punched metal is smaller than the inner diameter of the cylindrical side wall. The outer diameter of the cylindrical mesh is smaller than the inner diameter of the cylindrical punched metal. In this case, in the circular method, a plurality of raw yarns 100A pass through the inside of a cylindrical net. The gas blowing method is preferably the circular method, which can blow gas relatively uniformly onto the multiple raw yarns 100A, thereby cooling the multiple raw yarns 100A more uniformly and suppressing the variation in fineness of the multiple raw yarns 100A.
[0058] In the melt spinning process, a plurality of the raw yarns 100A cooled by gas are taken up by a first take-up roll section 107. The first take-up roll section 107 is composed of two rolls. The first take-up roll section 107 may be composed of one roll, or may be composed of three or more rolls. In this embodiment, the multiple raw yarns 100A taken up by the first take-up roll unit 107 are transported using a first transport roll unit 108, a second transport roll unit 109, a third transport roll unit 110, and a fourth transport roll unit 111, and the multiple raw yarns 100A transported by the transport roll units 108, 109, 110, and 111 are wound up by a first winding roll unit 112 to obtain a filament for drawing. The first winding roll unit 112 has a bobbin. The bobbin is a concept that includes a paper tube. The bobbin may or may not have a flange. Specifically, in the drawing step, the raw yarn 100A is wound around a bobbin of the first winding roll unit 112 to obtain a filament to be drawn. Although each transport roll section is configured with two rolls in FIG. 2, it may be configured with one roll, or may be configured with three or more rolls.
[0059] In the melt spinning step, the multiple raw yarns 100A are cooled to preferably 70° C. or less, more preferably 60° C. or less, even more preferably 50° C. or less, and particularly preferably 40° C. or less. In the melt spinning step, the multiple raw yarns 100A are cooled to, for example, 0° C. or more, preferably 10° C. or more. In the melt spinning step, the plurality of raw yarns 100A are cooled, preferably to a temperature equal to or higher than the glass transition temperature of the polymer composition. In the melt spinning process, 30 or more of the raw yarns may be cooled to 70° C. or less by blowing a gas at 0° C. or more and 50° C. or less. In the melt spinning process, the raw yarns 100A may be cooled to a certain degree by blowing a gas at 0° C. or more and 50° C. or less, and then cooled by ambient air while transporting the raw yarns 100A from the first take-up roll unit 107 to the first wind-up roll unit 112, thereby cooling the raw yarns 100A to 70° C. or less.
[0060] (Stretching process) As shown in FIG. 3, in the drawing step, the filament to be drawn 100B is heated and drawn by a drawing roll section 114.
[0061] In the drawing step, the filament to be drawn is taken up from the first winding roll section 112 by a second take-up roll section 113 . Next, in the drawing step, the filament to be drawn 100B taken up by the second take-up roll section 113 is drawn by the drawing roll section 114. In the drawing step, the filament to be drawn 100B drawn by the drawing roll section 114 is wound by a second winding roll section 116 to obtain a drawn filament. The second winding roll unit 116 has a bobbin. The bobbin is a concept that includes a paper tube. The bobbin may or may not have a flange. Specifically, in the drawing step, the drawn filament to be drawn 100B is wound around a bobbin of the second winding roll unit 116 to obtain a drawn filament. In the drawing process in FIG. 3, the draw filament 100B drawn in the drawing roll section 114 is wound up by the second winding roll section 116 to obtain a drawn filament, but the draw filament 100B drawn in the drawing roll section 114 may be obtained without being wound up by the second winding roll section 116. In the drawing step, the filament 100B to be drawn in the drawing roll section 114 may be transported in a take-off roll section 115.
[0062] The second take-off roll section 113 is composed of two rolls. Note that the second take-off roll section 113 may be composed of one roll, or may be composed of three or more rolls. In the drawing step, it is preferable that the filament to be drawn 100B is heated by the second take-up roll section 113. In the drawing process, by heating the drawing filament 100B in the second take-up roll section 113, it becomes easier to adjust the temperature of the single yarn so that it is within a temperature range suitable for increasing the orientation of the polymer component contained in the single yarn in the drawing filament 100B, and as a result, it becomes easier to increase the orientation of the polymer component of the single yarn. The temperature of the second take-up roll section 113 is preferably 15°C or higher and lower than 60°C, and more preferably 20 to 55°C. When the temperature of the environment in which the drawing step is carried out is 15° C. or higher, the filament to be drawn 100B does not need to be heated by the second take-up roll section 113.
[0063] The stretching roll section 114 is composed of two rolls. Note that the stretching roll section 114 may be composed of one roll, or may be composed of three or more rolls. In the drawing step, the filament 100B to be drawn may or may not be heated by the drawing roll section 114. That is, in this embodiment, the drawing roll section 114 may also serve as a heat treatment roll section. In the drawing process, the drawing filament 100B can be heated in the drawing roll section 114 to promote crystallization of the polymer component contained in the single yarn in the drawing filament 100B, or to improve the heat resistance of the polymer component contained in the single yarn. The temperature of the stretching roll section (heat treatment roll section) 114 is preferably 30 to 100°C, and more preferably 40 to 90°C.
[0064] In this embodiment, it is preferable that the take-off roll section 115 also serves as the heat treatment roll section. The take-off roll section 115 (heat treatment roll section 115) is composed of two rolls. The take-off roll section 115 (heat treatment roll section 115) may be composed of one roll, or may be composed of three or more rolls. In the drawing process, the drawing filament 100B is heated by the heat treatment roll section 115, thereby promoting crystallization of the polymer component contained in the single yarn in the drawing filament 100B, or improving the heat resistance of the polymer component contained in the single yarn. The temperature of the take-off roll section (heat treatment roll section) 115 is preferably 30 to 100°C, and more preferably 40 to 90°C. In addition, both or only one of the stretching roll section 114 and the take-off roll section 115 may be a heat treatment roll section.
[0065] In the drawing process of this embodiment, the single yarn is heated in the take-up roll section 113, the drawing roll section 114, and the take-off roll section 115. The single yarn may be heated appropriately to achieve the purpose of controlling the orientation, crystallization, and heat resistance of the polymer component of the single yarn. For example, the single yarn may be heated in the first winding roll unit 112 . The single yarn may also be heated in the second winding roll section 116 to obtain a drawn filament. The single yarn may be heated at all of the roll sections from the first winding roll section 112 to the second winding roll section 116. Alternatively, the single yarn may be heated at only some of the roll sections from the first winding roll section 112 to the second winding roll section 116, and not heated at the other roll sections. Incidentally, it is preferable that the heating of the single yarn in the roll section is controlled in each roll section.
[0066] In addition, the method of heating the polymer component of the single yarn in the drawing process of this embodiment (hereinafter also simply referred to as the "heating method") may be a method of heating the polymer component of the single yarn by heating the roll of the roll section. In addition, the roll section may have a container for accommodating rolls and a liquid (such as water) that is accommodated in the container together with the rolls, and the heating method may be a method for heating the liquid to heat the polymer component of the single yarn. In the drawing step, for example, drawing in a bath may be performed. Furthermore, the heating method may be a method in which a heated gas (for example, air, etc.) is blown onto the roll portion or near the roll portion to heat the polymer component of the single yarn. These heating methods may also be used in combination.
[0067] The stretching ratio in the stretching step is preferably 1.5 times or more, more preferably 1.7 times or more, and is, for example, 20 times or less. By setting the draw ratio in the drawing step to 1.5 times or more, the orientation of the polymer components of the single yarns in the filament for drawing 100B is further increased. The stretching ratio in the stretching step can be calculated by the following formula. Stretching ratio in the stretching step=speed of stretching roll section (m / min) / speed of take-up roll section (in this embodiment, “second take-up roll section 113”) used in the stretching step (m / min)
[0068] In the stretching step, the relaxation rate calculated by the following formula is preferably from 1 to 30%, and more preferably from 1 to 15%. Relaxation rate (%)=((speed of the drawing roll unit 114−speed of the take-up roll unit that takes up the filament for drawing (in this embodiment, the “second take-up roll unit 116”)) / speed of the take-up roll unit that takes up the filament for drawing)×100
[0069] The speed (m / min) of the stretching roll section is the length of the filament to be stretched transported by the stretching roll section per unit time. In this embodiment, only one stretching roll section is used, but multiple stretching roll sections may be used. When multiple stretching roll sections are used, the highest speed among the multiple stretching roll sections is defined as the "speed of the stretching roll section." The speed (m / min) of the take-up roll section used in the drawing step is the length per unit time of the filament to be drawn transported by the take-up roll section. The speed (m / min) of the winding roll section for winding the filament to be drawn is the length of the filament to be drawn that is wound on the winding roll section per unit time.
[0070] In the drawing step, the drawn filament may be obtained by drawing only one draw filament, or a plurality of draw filaments may be combined together and the combined plurality of draw filaments may be drawn to obtain the drawn filament.
[0071] (Heat treatment process) In the heat treatment step (hereinafter also referred to as the "annealing step"), the filaments, which are drawn filaments, are heat treated to obtain the piezoelectric fibers.
[0072] In the annealing process, the filament can be heat-treated by holding the filament in a medium whose temperature is kept constant at a specific temperature for a predetermined time. Examples of the medium include air, water, and oil. In the annealing process, an oven, a constant temperature bath, and the like can be used. When holding the filament in the constant temperature medium, it is preferable to fix both ends of the filament. Also, when holding the filament in the constant temperature medium, the filament may be wound around a bobbin or the like. Alternatively, the filaments may be heat-treated by contacting them with a heated roll for a predetermined period of time. For example, the annealing step can be performed by adjusting the number of turns of the filament around the heated godet roll and the rotation time of the roll. In the annealing step, it is preferable to use an oven for ease of handling.
[0073] In the annealing step, the temperature of the heat treatment (hereinafter also referred to as "annealing temperature") is preferably 40°C or higher, from the viewpoint of being able to shorten the heat treatment time while increasing the crystallinity of the filament. In the annealing step, the annealing temperature is preferably 140° C. or less, from the viewpoint of being able to increase the crystallinity of the filaments while suppressing melting of the filaments. The annealing temperature is more preferably 50°C to 130°C. The preferred annealing time varies depending on the temperature. For example, if the annealing temperature is 60° C., the annealing time is preferably 10 minutes or more. If the annealing temperature is 120° C., the annealing time is preferably 5 minutes or less.
[0074] The present invention is not limited to the above-described embodiment. The present invention is also not limited to the above-described effects. Furthermore, the present invention can be modified in various ways without departing from the gist of the present invention.
[0075] For example, in the method for producing a piezoelectric fiber according to the present embodiment, a multifilament is produced, but in the method for producing a piezoelectric fiber according to other embodiments, a monofilament may be produced.
[0076] In addition, in the method for producing a piezoelectric fiber according to this embodiment, the melt spinning step and the drawing step are performed by a sequential drawing method, but in the method for producing a piezoelectric fiber according to other embodiments, the melt spinning step and the drawing step may be performed by a spin draw method. The spin-draw method is a method in which the process of obtaining multiple molten yarns by discharging the molten material from multiple nozzles and the process of drawing the filaments to be drawn with a drawing roll are carried out in a single process. The spin-draw method is also called the "SDY method" or "direct spinning drawing method."
[0077] In another embodiment of the spin-draw method, as shown in FIG. 4, gas is blown onto multiple molten raw yarns 100A in the melt spinning process to cool 30 or more raw yarns 100A, thereby obtaining a filament for drawing 200B, and the filament for drawing 200B is taken up by a take-up roll section 207. Next, in the drawing step, the filament to be drawn 200B taken up by the take-up roll section 207 is drawn by three drawing roll sections (a first drawing roll section 208, a second drawing roll section 209, and a third drawing roll section 210). In the drawing step, the drawn filament 200B to be drawn is wound around a winding roll section 212 to obtain a drawn filament. The winding roll unit 212 has a bobbin. The bobbin is a concept that includes a paper tube. The bobbin may or may not have a flange. Specifically, in the drawing step, the drawn filament 200B to be drawn is wound around a bobbin of the winding roll unit 212 to obtain a drawn filament. In the drawing process in FIG. 4, the draw filament 200B drawn in the drawing roll section is wound up in the winding roll section 212 to obtain a drawn filament, but the draw filament 200B drawn in the drawing roll section may be obtained without being wound up in the winding roll section 212. In the drawing step, the filament 200B to be drawn in the drawing roll section may be transported by a take-off roll section 211.
[0078] In the melt spinning step, a plurality of the raw yarns 100A are cooled in a first cooling box 105 to obtain a filament to be drawn 200B, and in the drawing step, the filament to be drawn 200B is taken up by a take-up roll section 207. The plurality of raw yarns 100A cooled in the first cooling box 105 may be cooled in a second cooling box 106 to obtain the filament to be drawn 200B. Although the take-off roll section 207 is configured with two rolls in FIG. 1, it may be configured with one roll, or may be configured with three or more rolls.
[0079] In other embodiments where the spin-draw process is carried out, each of the drawing roll sections may also serve as a heat treatment roll section. Each of the stretching roll sections 208, 209, 210 (each of the heat treatment roll sections 208, 209, 210) is configured with two rolls in FIG. 1, but may be configured with one roll or with three or more rolls. From the viewpoint of promoting crystallization of the polymer component contained in the single yarn in the drawing filament 200B, or from the viewpoint of improving the heat resistance of the polymer component contained in the single yarn, the temperature of the heat treatment roll section is preferably 30 to 100°C, more preferably 40 to 90°C. When the temperature of the environment in which the drawing step is carried out is 30° C. or higher, the crystallization of the polymer component contained in the single yarn can be promoted even without using a heat treatment roll section.
[0080] [Disclosure items] Each of the following sections is a disclosure of a preferred embodiment.
[0081] [Item 1] Contains poly(3-hydroxyalkanoate) resin, The weight average molecular weight of the poly(3-hydroxyalkanoate) resin is 50,000 to 500,000; A piezoelectric fiber having a crystallinity of 52% or more. [Item 2] the poly(3-hydroxyalkanoate)-based resin comprises a copolymer having a 3-hydroxybutyrate unit; 2. The piezoelectric fiber according to item 1, wherein the content of the 3-hydroxybutyrate unit in the poly(3-hydroxyalkanoate) resin is 85.5 mol % or more and 99.5 mol % or less. [Item 3] the piezoelectric fiber comprises one or more single yarns; 3. The piezoelectric fiber according to item 1 or 2, wherein the average fineness of the single yarn is 0.5 dtex or more. [Item 4] 4. The piezoelectric fiber according to any one of items 1 to 3, wherein the piezoelectric fiber is a multifilament. [Item 5] A method for producing a piezoelectric fiber according to any one of items 1 to 4, A method for producing a piezoelectric fiber, comprising a heat treatment step of heat treating a filament to obtain the piezoelectric fiber. [Item 6] 6. The method for producing a piezoelectric fiber according to item 5, further comprising a drawing step of drawing the filament to obtain a drawn filament. [Item 7] 7. The method for producing a piezoelectric fiber according to item 6, further comprising a melt spinning step of discharging a molten material by a melt spinning method to obtain the filament for drawing. [Item 8] 8. The method for producing a piezoelectric fiber according to any one of items 5 to 7, wherein the heat treatment temperature in the heat treatment step is 40° C. to 140° C. EXAMPLES
[0082] The present invention will now be described in more detail with reference to examples and comparative examples, although the present invention is not limited to these examples in any way.
[0083] <Example 1> The filaments were produced by a sequential drawing method.
[0084] (Melt spinning process) First, the following materials were dry-blended in the following mixing ratio, and the dry-blended materials were melt-kneaded at 150° C. in an extruder to obtain pellets. As a poly(3-hydroxyalkanoate) resin, (3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin (ratio of 3-hydroxyhexanoate: 6 mol%, Mw: 350,000, melt flow rate (MFR) (165°C, 5 kg): 12 g / 10 min) (P3HB3HH): 100 parts by mass Pentaerythritol as a crystal nucleating agent (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., NeuRizer P): 1.0 part by mass Lubricant: erucic acid amide: 0.5 parts by mass Behenic acid amide as a lubricant: 0.5 parts by mass The glass transition temperature of the pellets was 2°C. The crystallization temperature of the pellets was 100°C. The melting point of the pellets was 146°C. The thermal decomposition temperature of the pellets was 180°C.
[0085] Then, as shown in FIG. 2, the pellets were melted in a kneading extruder 102 (single-screw extruder, screw diameter: 25 mm) to obtain a melt. The molten material was then extruded from the spinning nozzle 104 (temperature: 175° C., number of nozzle holes: 368, shape of nozzle holes: circular, diameter of nozzle holes: 0.3 mm) to obtain 368 original yarns 100A. The flow rate of the molten material was adjusted to 5.6 kg / h by the gear pump 103. Next, air at 20° C. was blown onto the 368 original yarns 100A at a speed of 0.7 m / s by a circular method in the cooling box 105. Note that no gas was blown onto the cooling box 106. Next, the 368 raw yarns 100A cooled in the cooling boxes 105 and 106 were taken up by the first take-up roll section 107 (563 m / min), and the 368 raw yarns 100A passed through the first conveying roll section 108 (563 m / min), the second conveying roll section 109 (563 m / min), the third conveying roll section 110 (563 mm / min), and the fourth conveying roll section 111 (471 m / min) in that order, after which the 368 raw yarns 100A were taken up by the first winding roll section (552 m / min) and stored at room temperature (5 to 35°C) for 18 hours to obtain a filament for drawing.
[0086] (Stretching process) As shown in FIG. 3, the filament to be drawn was taken up from the first winding roll section 112 by the second take-up roll section 113 (55.5 m / min, 30° C.), drawn by the drawing roll section 114 (110 m / min, 90° C.), transported by the take-off roll section (heat treatment roll section) 115 (100 m / min, 100° C.), and taken up by the second winding roll section 116 (100 m / min) to obtain a drawn filament. The stretching ratio was 1.8 times.
[0087] The take-up roll section and the transport roll section each used a roll section made up of two rolls with the same speed and temperature.
[0088] (Heat treatment process (annealing process)) The filament was wound around the second winding roll unit 116 and then heat-treated in an oven at 60° C. for 10 minutes to obtain a piezoelectric fiber.
[0089] <Examples 2 to 5> A piezoelectric fiber was obtained in the same manner as in Example 1, except that the heating conditions in the annealing treatment step were as shown in Table 1 below.
[0090] <Comparative Example 1> The drawn filament obtained in Example 1 was used as the piezoelectric fiber of Comparative Example 1. In other words, the piezoelectric fiber was obtained in the same manner as in Example 1, except that the annealing treatment step was not performed.
[0091] (Degree of crystallinity, weight average molecular weight, and average fineness) The degree of crystallinity of the piezoelectric fiber, the weight average molecular weight of the poly(3-hydroxyalkanoate) resin in the piezoelectric fiber, and the average fineness of a single yarn in the piezoelectric fiber were measured by the methods described above. The measured values are shown in Table 1 below.
[0092] (output piezoelectric difference) The output piezoelectric difference of the piezoelectric fiber was measured. The output piezoelectric difference was measured by the Berlincourt method. Measurements were performed with an applied stress of 0.1 N. The charge meter was adjusted so that the output voltage was 100 mV and the piezoelectric constant was 0.1 pC / N. The measured values are shown in Table 1 below. A larger output piezoelectric difference means a higher piezoelectricity.
[0093] [Table 1]
[0094] As shown in Table 1, in Examples 1 to 4 within the scope of the present invention, the output piezoelectric difference was larger than that in Comparative Example 1, in which the crystallinity was 51.0%. Therefore, it is clear that the present invention can provide a piezoelectric fiber having excellent piezoelectric properties, which contains a poly(3-hydroxyalkanoate) resin having a weight average molecular weight of 50,000 to 500,000. Moreover, the crystallinity of Example 5 was 53.5%, which was as high as the other Examples. From this, it is believed that the piezoelectric fiber of Example 5 also has excellent piezoelectric properties. [Explanation of symbols]
[0095] 100A: raw yarn, 100B: filament for drawing, 101: material input section, 102: kneading extruder, 103: gear pump, 104: spinning nozzle, 105: first cooling box, 106: second cooling box, 107: first take-up roll section, 108: first conveying roll section, 109: second conveying roll section, 110: third conveying roll section, 111: fourth conveying roll section, 112: first winding roll section, 113: second take-up roll section, 114: drawing roll section (heat treatment roll section), 115: take-off roll section (heat treatment roll section), 116: second winding roll section, 200B: filament for drawing, 207: take-up roll section, 208: first drawing roll section (heat treatment roll section), 209: second drawing roll section (heat treatment roll section), 210: third drawing roll section (heat treatment roll section), 211: take-off roll section, 212: winding roll section
Claims
1. Contains poly(3-hydroxyalkanoate) resin, The weight average molecular weight of the poly(3-hydroxyalkanoate) resin is 50,000 to 500,000; A piezoelectric fiber having a crystallinity of 52% or more.
2. the poly(3-hydroxyalkanoate)-based resin comprises a copolymer having a 3-hydroxybutyrate unit, 2. The piezoelectric fiber according to claim 1, wherein the content of the 3-hydroxybutyrate units in the poly(3-hydroxyalkanoate) resin is 85.5 mol % or more and 99.5 mol % or less.
3. the piezoelectric fiber comprises one or more single yarns; The piezoelectric fiber according to claim 1 or 2, wherein the average fineness of the single yarn is 0.5 dtex or more.
4. The piezoelectric fiber of claim 1 or 2, wherein the piezoelectric fiber is a multifilament.
5. A method for producing the piezoelectric fiber according to claim 1 or 2, comprising the steps of: A method for producing a piezoelectric fiber, comprising a heat treatment step of heat treating a filament to obtain the piezoelectric fiber.
6. The method for producing a piezoelectric fiber according to claim 5 , further comprising a drawing step of drawing a filament to obtain the filament as a drawn filament.
7. The method for producing a piezoelectric fiber according to claim 6, further comprising a melt spinning step of discharging a molten material by a melt spinning method to obtain the filament for drawing.
8. The method for producing a piezoelectric fiber according to claim 5, wherein the heat treatment temperature in the heat treatment step is 40°C to 140°C.
Citation Information
Patent Citations
Piezoelectric sensors containing electrospun poly[(R)-3-hydroxybutyrate-co-(R)-3-hydroxyhexanoate] (PHBHX) nanofibers
JP2022501480A