Powder containing rare earth oxide and group ii element oxide, and method for producing ceramic powder

By setting the CV value of rare earth oxides to Group 2 element oxides to 35% or less and using a bead mill process, the powders are uniformly dispersed in ceramic materials, improving their effectiveness as additives.

JP2024167824APending Publication Date: 2024-12-04NIPPON YTTRIUM
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084172
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Rare earth oxides and Group 2 element oxides tend to agglomerate and aggregate, making it difficult to uniformly mix them with ceramic powders, which affects their performance in applications such as sintering aids and dielectrics.

Method used

The CV value of the mass concentration ratio of rare earth oxides to Group 2 element oxides is set to 35% or less, and the powders are produced by wet-mixing in a bead mill with subsequent solvent removal, ensuring uniform dispersion.

Benefits of technology

The resulting powder achieves uniform mixing with ceramic powders, enhancing their dispersibility and performance as ceramic additives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167824000001_ABST
    Figure 2024167824000001_ABST
Patent Text Reader

Abstract

To provide powder containing a rare earth oxide and a group II element oxide, capable of being mixed uniformly with a ceramic powder, and useful as a ceramic additive.SOLUTION: The present invention provides powder containing a rare earth oxide and a group II element oxide, in which a CV value of a ratio (group II element oxide / rare earth oxide) of mass concentrations of the rare earth oxide and the group II element oxide, which is measured by SEM-EDX and converted to oxides, is 35% or less. It is preferable that the powder have a total content of the group II element oxide and the rare earth oxide of 90 mass% or more. It is preferable that the powder have a content ratio of the group II element oxide of 0.1 mass% or more and 50 mass% or less, when the total content of the rare earth oxide and the group II element oxide is 100 mass% as measured by ICP emission spectroscopy.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder containing a rare earth oxide and a Group II element oxide, and a method for producing a ceramic powder using the powder. [Background technology]

[0002] Both rare earth oxides and Group II element oxides are used as additives. Applications of rare earth oxides and Group II element oxides as additives include sintering aids for ceramics, dielectrics or internal electrodes for capacitors, phosphors, refractive index adjusters for optical glass, oxygen sensors, catalysts, refractories, etc. They are used in a variety of forms, including coatings (paint films), trace additions, and molded bodies (including sintered bodies).

[0003] In general, rare earth oxide powders tend to aggregate, and Group II element oxide powders also have the property of being aggregated, making it difficult to uniformly mix the rare earth oxide powder and the Group II element oxide powder with the ceramic powder. For these reasons, in the above-mentioned applications, when adding the rare earth oxide powder and the Group II element oxide powder to a base material such as a ceramic powder, the rare earth oxide powder and the Group II element oxide powder are usually first mixed using a medium or the like, and then mixed with the base material (for example, Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-251699 A Summary of the Invention [Problem to be solved by the invention]

[0005] There is a demand for a technology that can more finely and uniformly disperse the powdered ceramic base material and the powdered rare earth oxide and Group II element oxide.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a powder of a rare earth oxide and an oxide of a Group II element which is highly dispersible in ceramic powders and the like. [Means for solving the problem]

[0007] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by setting the CV value of the abundance ratio of rare earth oxide and Group II element oxide to a specific value or less.

[0008] The present invention is based on the above-mentioned findings and provides a powder containing a rare earth oxide and a Group II element oxide, in which the CV value of the ratio of the mass concentrations of the rare earth oxide and the Group II element oxide (Group II element oxide / rare earth oxide), measured by SEM-EDX and converted into oxides, is 35% or less.

[0009] The present invention also provides a method for producing a ceramic powder, which comprises wet-mixing the above powder and a ceramic powder in a solvent using a bead mill, and then removing the solvent. Effect of the Invention

[0010] According to the present invention, there is provided a powder containing a rare earth oxide and a Group II element oxide which can be uniformly mixed with a ceramic powder and is useful as a ceramic additive. Furthermore, according to the present invention, by using the powder of the present invention, it is possible to produce a ceramic powder in which the rare earth oxide and the Group II element oxide are well dispersed in the ceramic powder. [Brief description of the drawings]

[0011] [Figure 1] 1 is an SEM image showing the appearance of the powder of the mixture of Y2O3 and MgO obtained in Example 1. It also shows nine points measured by SEM (scanning electron microscope)-EDX (energy dispersive X-ray analyzer). [Diagram 2] 1 is a SEM image showing the appearance of the powder of barium titanate and the mixture of Y2O3 and MgO obtained in Example 1 after being crushed in a bead mill and dried. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below based on preferred embodiments thereof.

[0013] <Powder> One of the features of the present invention is that the concentration ratio of rare earth oxide and Group II element oxide in a powder containing rare earth oxide and Group II element oxide, measured by SEM (scanning electron microscope)-EDX (energy dispersive X-ray analyzer), is uniform in the powder. Specifically, the CV value (Coefficient of Variation) of the concentration ratio of rare earth oxide and Group II element oxide (Group II element oxide / rare earth oxide) measured by SEM-EDX in a powder containing rare earth oxide and Group II element oxide, that is, the ratio of the average value Av to the standard deviation Sd (CV=Sd / Av) is 35% or less. The CV value is an index showing the variation in the concentration ratio, and it can be determined that the smaller the value, the less the variation in the concentration ratio and the higher the uniformity.

[0014] The present inventors have intensively studied a method for uniformly mixing rare earth oxide and Group II element oxide in a base material such as ceramic. As a result, they have found that the problem can be solved by setting the CV value of the concentration ratio of rare earth oxide and Group II element oxide to 35% or less. According to the present disclosure, the reason for this is believed to be that the rare earth oxide and Group II element oxide coexist in the primary particles to form a dispersed state, and that the surface charge of the primary particles in which both oxides are dispersed is different from the surface charge of the primary particles consisting of only either the rare earth oxide or the Group II element oxide. Such a low CV value indicates that the rare earth oxide and Group II element oxide are uniformly distributed in the particles or powder.

[0015] In the present invention, the CV value is preferably 32% or less. The lower limit of the CV value is not particularly limited. The lower limit of the CV value is not limited, and may be 0% or more, 3% or more, or 5% or more.

[0016] The standard deviation Sd and average value Av in SEM-EDX can be obtained by dividing three fields of view of a 5000x SEM image into thirds vertically (Y direction in Fig. 1) and horizontally (X direction in Fig. 1) to obtain a total of nine partial images, calculating the abundance of Group II elements and rare earth elements relative to the total mass on a mass basis at each center point C, converting the data into oxides to obtain mass-based concentration ratio (Group II element oxide / rare earth oxide) data for a total of 27 items for the three fields of view, and calculating the average value Av and standard deviation Sd. The center point C is the intersection point of a center line extending in the vertical direction Y and bisecting the horizontal direction X in the partial images, and a center line extending in the horizontal direction X and bisecting the vertical direction Y in the partial images.

[0017] A powder having the above CV value can be produced by a suitable production method described later.

[0018] The powder is more preferably measured by ICP emission spectroscopy for the content of rare earth oxide and Group II element oxide relative to the total mass, and the content of Group II element oxide is 0.05% by mass or more and 50% by mass or less when the total mass of the rare earth oxide and Group II element oxide is 100% by mass. This range has the advantage that the ratio of the rare earth oxide and Group II element oxide can be arbitrarily adjusted in a highly dispersible state. Also, 0.1% by mass or more and 50% by mass or less is more preferable, and 2% by mass or more and 50% by mass or less is even more preferable. The content of rare earth oxide and Group II element oxide measured by ICP emission spectroscopy can be obtained by measuring the amount of rare earth metal and Group II metal in a liquid obtained by dissolving the powder in nitric acid, hydrochloric acid or sulfuric acid by ICP emission spectroscopy, and dividing the value converted into oxide by the total mass of the powder. The ICP emission spectroscopy was performed according to JIS1688:2010.

[0019] The powder may be composed of a rare earth oxide and a Group II element oxide, or may contain other components in addition to the rare earth oxide and the Group II element oxide. Whether or not the powder contains other components in addition to the rare earth oxide and the Group II element oxide can be confirmed by fluorescent X-ray analysis.

[0020] In addition, the powder preferably has a total content of Group II element oxide and rare earth oxide measured by ICP atomic emission spectroscopy of 90 mass% or more, more preferably 95 mass% or more, and even more preferably 99 mass% or more. The mass ratio of the Group II element oxide content to the rare earth oxide content (rare earth oxide:Group II element oxide) measured by ICP emission spectroscopy is preferably 1:0.9-1000.

[0021] In the present invention, the rare earth oxide includes at least one oxide selected from Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Examples of the oxides of these elements include Sc2O3, Y2O3, La2O3, CeO, Pr6O 11 , Nd2O3, Sm2O3, Eu2O3, Gd2O3, Tb4O7, Dy2O3, Ho2O3, Er2O3, Tm2O3, Yb2O3 and Lu2O3.

[0022] From the viewpoint of superior significance of the effect of the present invention due to the conventional difficulty in suppressing agglomeration, as the oxide of a rare earth element, an oxide other than Ce is particularly preferred, and among them, an oxide of an element selected from Y, La, Pr, Nd, Eu, Gd, Dy, Ho, Er and Yb is preferred, and in particular, an oxide of an element selected from Y, Gd, Dy, Ho and Yb, that is, at least one selected from yttrium oxide, gadolinium oxide, dysprosium oxide, holmium oxide and ytterbium oxide is preferred.

[0023] In the present invention, examples of Group II metals include beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba), with magnesium being preferred in terms of suppressing solid solution at high temperatures. The formula of the oxide of Group II metal element M is MO. Since magnesium oxide does not form a solid solution even when mixed with rare earth oxides, each can exist in the oxide state even at high temperatures, and no change occurs in the other chemical substances (crystal structure).

[0024] It is preferable that the primary particle diameter of the powder is in a certain small range. In the present invention, it is of great technical significance that the powder has such a small primary particle diameter and a small CV value under conditions where aggregation is likely to occur. From this viewpoint, the primary particle diameter of the powder is preferably 10 to 100 nm, more preferably 15 to 80 nm, and even more preferably 20 to 50 nm.

[0025] In the present invention, the primary particle size of the powder is the primary particle size converted into a specific surface area, specifically, the specific surface area S (m 2 / g). For example, the primary particle diameter d (nm) is d = 6000 / (ρs). (ρ is the true density (g / cm 3 The true density ρ of a powder in which rare earth oxide and Group II element oxide are mixed is defined as 1 / ((rare earth oxide mass concentration / true density of rare earth oxide)+(Group II element oxide concentration / true density of Group II element oxide)).

[0026] The specific surface area of ​​the powder is 30 m2 or less because of the high technical significance of having a large specific surface area and a small CV value under conditions that tend to cause agglomeration. 2 / g or more 45m 2 / g or less is preferable, and 31m 2 / g or more 43m 2 / g or less is particularly preferred.

[0027] The powder of the present invention preferably has an aggregate particle size in a specific range in a specific crushing treatment. Specifically, the powder of the present invention is more preferably mixed with pure water to prepare a water slurry containing 10% by mass of the powder, and then the operation (A) is repeated until the average particle size becomes larger than the previous measured value, so that the average particle size falls within a specific range. As a method for preparing a water slurry containing 10% by mass of the powder, a method of mixing 4.6 g of water with 42 g of the powder to prepare a slurry can be mentioned. In this case, 0.15 times the mass of the powder (specifically 0.69 g) of Floren GW-1500 (Kyoeisha Chemical Co., Ltd.) is added to the slurry as a dispersant (to be specific, 0.69 g). (A): The slurry is subjected to a bead mill treatment for 10 minutes using zirconia beads with a diameter of 0.05 mm, and then the average particle size is measured by dynamic light scattering. Specifically, the operation (A) is as follows: (a): Using zirconia beads with a diameter of 0.05 mm, the slurry:beads mass ratio was set to 45:230, and the bead mill processing was carried out for 10 minutes in a bead mill having an effective volume of a vessel of 80 cc at a peripheral speed of 4 m / s to 6 m / s, after which the average particle size was measured by dynamic light scattering. (However, if the average particle size becomes larger than the previous measurement, the bead mill processing is terminated at that point, and even if the process (A) is repeated 20 times and the average particle size does not become larger than the previous measurement in any of the 2nd to 20th times, the process is terminated when the process (A) has been repeated 20 times.) Here, the minimum average particle size (Dd) means the minimum value of the average particle size measured by dynamic light scattering method by sampling every 10 minutes during the bead mill treatment. Note that the average particle size is expressed in nm units, and if there is a decimal value, the value is rounded off to the first decimal place to the nearest integer, and the size is determined based on the value.

[0028] The minimum average particle diameter (Dd) obtained by the above measurement indicates the minimum agglomeration diameter by bead crushing, which is a common crushing process in the technical field related to metal oxide fine powder slurries. The minimum average particle diameter (Dd) is preferably 110 nm or less. By setting the minimum average particle diameter (Dd) to 110 nm or less, the dispersibility in the main material such as ceramic powder is further improved. From this perspective, the minimum average particle diameter (Dd) is more preferably 105 nm or less. In addition, the minimum average particle diameter (Dd) is preferably 40 nm or more, and more preferably 55 nm or more. By setting this lower limit to a predetermined value or more, the dispersion stability of the slurry can be improved.

[0029] In addition, the polydispersity index (PI) at the time of measuring the minimum average particle size (Dd) is preferably 0.250 or less in terms of a sharp particle size distribution and easier maintenance of high dispersibility when made into a slurry, and more preferably 0.210 or less. The polydispersity index (PI) is a dimensionless index that indicates the spread of the particle size distribution.

[0030] The powder having the above-mentioned minimum average particle size (Dd) and polydispersity index can be produced by a suitable production method described below.

[0031] The effective volume of the vessel refers to the internal volume of the container (vessel) in which the beads and slurry are accommodated. The peripheral speed of the bead mill may be any speed between 4 m / s and 6 m / s, more preferably between 4 m / s and 5 m / s, and even more preferably 4 m / s.

[0032] The measurement of the average particle size and polydispersity index (PI) by the dynamic light scattering method (photon correlation method) is performed by filling a measurement sample into a dynamic light scattering photometer. The measurement sample is a sample that is not subjected to ultrasonic treatment, with a part of the above-mentioned slurry taken out and the solvent used in the wet disintegration as a dispersion medium. The concentration of the measurement sample is a dilution ratio within the range of 1000 to 10000 times by volume that the dynamic light scattering photometer judges to be an appropriate concentration. As the dynamic light scattering photometer, a device that employs a method of determining the average particle size and polydispersity index (PI) by cumulant analysis from the autocorrelation function obtained by the photon correlation method can be used, and for example, the ELSZ-2000ZS manufactured by Otsuka Electronics can be used. The cumulant method is described in "9.2.1 Cumulant method" of JIS Z 8828:2019 "Particle size analysis -- Dynamic light scattering method" and in "A.1.2 Cumulant method" of Appendix A of the same JIS.

[0033] Furthermore, the powder of the present invention preferably has a ratio Ds / Dd of the average particle size (Dd) to the primary particle size Ds calculated as a specific surface area of ​​0.3 or more. The ratio Ds / Dd indicates the degree of aggregation. The larger the ratio Ds / Dd, the smaller the difference between the primary particle size and the secondary particle size, indicating that aggregation is suppressed. From this point of view, it is particularly preferable that the ratio Ds / Dd is 0.34 or more. On the other hand, the upper limit of the above ratio is preferably 0.7 or less in terms of suppressing the activity of the particle surface, and more preferably 0.6 or less. When Ds>Dd, the particles are pulverized. When pulverized, the particle surface is activated, and a mechanochemical reaction occurs, causing the particle surface to react with the solvent, which may change the composition of the surface.

[0034] A powder having the above ratio of the minimum average particle size (Dd) to the primary particle size (Ds) can be produced by a suitable production method described later.

[0035] The powder of the present invention preferably has an aggregate particle size of a specific value or less in another crushing process. Specifically, the powder of the present invention is mixed with water to prepare a water slurry containing 10% by mass of the powder, and then the slurry is subjected to a bead mill process using zirconia beads having a diameter of 0.05 mm for 60 minutes, and then the average particle size is measured by a dynamic light scattering method, and the average particle size Dd1 is preferably 150 nm or less. The method of preparing a water slurry containing 10% by mass of the powder can be the same as that described for the minimum average particle size (Dd). The bead mill treatment is carried out for 60 minutes using zirconia beads with a diameter of 0.05 mm, with a mass ratio of slurry:beads of 45:230, in a bead mill having an effective volume of a vessel of 80 cc, at a peripheral speed of 4 m / s, and then the average particle size is measured by dynamic light scattering. In this way, a powder that can suppress aggregation even with a relatively short time of crushing is preferable because it is easier to mix with ceramic powder. For this reason, the average particle size Dd1 is more preferably 100 nm or less. It is preferable that the lower limit of the above average particle size Dd1 is 10 nm or more because crushing is less likely to occur and the active surface is reduced.

[0036] The powder having the average particle diameter Dd1 in the above ratio can be produced by a suitable production method described later.

[0037] The powder of the present invention is preferably one having a certain aggregate size before disintegration, since it has a specific CV value, which is technically significant. From this point of view, the volume-based D measured by a laser diffraction scattering type particle size distribution measurement method after ultrasonic irradiation is 50 The volume cumulative particle size at 50% by volume of the cumulative volume is preferably 1 μm or more, and more preferably 2 μm or more. 50 is preferably 25 μm or less, and more preferably 21 μm or less.

[0038] D 50 is measured after ultrasonic irradiation. More specifically, the ultrasonic irradiation is a process of dispersing the sample for 5 minutes with ultrasonic waves of 300 W and a frequency of 19.5 kHz. The irradiation device may be an attachment to a laser diffraction scattering type particle size measuring device, and may be irradiated to a sample in which a powder is added to a 0.2% by mass aqueous solution of sodium hexametaphosphate. The concentration of the powder in the dispersion liquid during ultrasonic irradiation is preferably a concentration that the particle size measuring device judges to be an appropriate concentration for particle size measurement, and is usually within the range of 0.002 to 0.2% by mass. The ultrasonic irradiation is specifically performed according to the method described in the Examples, but irradiation may be performed using a device other than that attached to the laser diffraction scattering type particle size measuring device used for measurement as long as it is an equivalent irradiation device. However, when irradiation is performed using a device other than that attached to the laser diffraction scattering type particle size measuring device used for measurement, 0.2 g of the sample is placed in about 100 ml of a 0.2% by mass aqueous solution of sodium hexametaphosphate, and after ultrasonic irradiation, the slurry after ultrasonic irradiation is added to a sample circulation device until the particle size measuring device judges it to be an appropriate concentration for particle size measurement, and then the measurement is performed.

[0039] Furthermore, in terms of the excellent technical significance of having a specific CV value, the powder of the present invention has a volume-based D measured by a laser diffraction scattering type particle size distribution measurement method after ultrasonic irradiation. 90The volume cumulative particle size at 90% by volume of the cumulative volume is preferably 3 μm or more and 90 μm or less, and even more preferably 4 μm or more and 85 μm or less.

[0040] The dispersion index D is the technical significance of having a specific CV value. 90 / D 50 may be in a specific range. Specifically, D 90 / D 50 is preferably 1.0 or more and 5.0 or less, and more preferably 1.5 or more and 4.0 or less.

[0041] The above mentioned D 50 and D. 90 In order to obtain the dispersion index, a suitable method for producing a powder, which will be described later, may be adopted.

[0042] Next, a preferred method for producing the powder of the present invention will be described. This manufacturing method includes a reaction / solid-liquid separation step in which an aqueous solution of an alkaline agent (hereinafter also referred to as "Liquid A") and an aqueous solution containing a water-soluble salt of a rare earth element and a water-soluble salt of a Group II element (hereinafter also referred to as "Liquid B") are simultaneously charged into a reaction vessel and mixed under high speed stirring so that the pH of the mixed solution becomes 6 to 10, causing a reaction between the alkaline agent and the water-soluble salt of the rare earth element and the water-soluble salt of the Group II element, and initiating solid-liquid separation within 5 minutes from the start of mixing of Liquids A and B; a washing step in which the residue obtained in the reaction / solid-liquid separation step is washed with water; and a calcination step in which the washed residue is calcined.

[0043] In order to successfully obtain the powder of the present invention, the water-soluble salt concentration in the water-soluble salt solution as Solution B is preferably 10 to 400 g / L, more preferably 25 to 350 g / L, and particularly preferably 30 to 300 g / L, calculated as the oxide. The water-soluble salt in oxide form referred to here means the concentration of the water-soluble metal salt in oxide form, and includes the amount of the water-soluble salt of the rare earth element in oxide form and the amount of the water-soluble salt of the Group II element in oxide form.

[0044] (Reaction / solid-liquid separation process) In the A solution, which is an aqueous alkaline agent solution, examples of the alkaline agent include carbonates such as ammonium hydrogen carbonate, ammonium carbonate, sodium carbonate, and sodium hydrogen carbonate, and hydroxides such as sodium hydroxide and potassium hydroxide, and carbonates are preferred from the viewpoint of ease of solid-liquid separation during production. The carbonates referred to in this specification include not only normal salts but also hydrogen carbonates, which are acidic salts. In particular, ammonium hydrogen carbonate or ammonium carbonate is preferred from the viewpoint of ease of adjusting the pH of the mixed solution and reducing impurities. In particular, hydrogen carbonates such as ammonium hydrogen carbonate are preferred when producing a powder having a Group II element oxide content of less than 1.0% by mass as determined by ICP emission spectral analysis. Furthermore, carbonates as normal salts such as ammonium carbonate are preferred when producing a powder having a Group II element oxide content of 1.0% by mass or more.

[0045] In the solution B, which is an aqueous solution of water-soluble salts of rare earth elements and Group II elements, the water-soluble salts of rare earth elements and Group II elements include nitrates, acetates, ammine complexes, and chlorides, with nitrates being preferred from the viewpoints of ease of adjusting the pH of the mixed solution and productivity. The anions of the water-soluble salts of the rare earth elements and Group II elements may be the same or different.

[0046] In this manufacturing method, liquid A, which is an aqueous carbonate solution, and liquid B, which is an aqueous solution of a water-soluble salt of a rare earth element and a group II element, are simultaneously charged into a reaction tank so that the pH of the mixture of the two is 6 to 10. The pH here is the pH at the temperature of the mixture of the two. The pH of the mixture is below a certain level, which is advantageous in that the primary particles can be prevented from becoming large. The pH is above a certain level, which is advantageous in that most of the rare earth ions and group II ions in liquid B can be precipitated. In particular, when producing a powder having a group II element oxide content of less than 1.0 mass% by ICP atomic emission spectrometry, the pH of the mixture of liquid A and liquid B is preferably 6 to 9, more preferably 6.5 to 7. On the other hand, when producing a powder having a group II element oxide content of 1.0 mass% or more by ICP atomic emission spectrometry, the pH of the mixture of liquid A and liquid B is preferably 7 to 10, more preferably 7 to 8.

[0047] Liquid A and liquid B may or may not be heated at the time of introduction. Liquid A and liquid B are preferably at 5 to 50°C at the time of introduction into the reaction vessel. In order to keep the CV value within a suitable range, it is preferable to carry out the reaction in an extremely short time and filter immediately. For this reason, it is preferable to adjust the timing and rate of introduction of both liquids so that the pH of the mixed liquid is within the above range from the start of introduction of liquid A and liquid B into the reaction vessel (the start of mixing liquid A and liquid B) to the time when the reaction product is generated (more specifically, the start of solid-liquid separation), and to maintain the pH constant within the above range. The reaction proceeds smoothly when the pH is within the above range.

[0048] The simultaneous addition of liquid A and liquid B means that the time when liquid A is added to the reaction vessel and the time when liquid B is added are at least partially simultaneous. As described above, in order for the pH of the mixed liquid to be within the above range from the time when liquid A and liquid B start to be added to the reaction vessel (the time when liquid A and liquid B start to be mixed) to the time when the reaction product is generated (more specifically, the time when solid-liquid separation starts), it is preferable that the start of each addition is almost simultaneous and the addition speed is constant. In addition, it is preferable to adjust the addition speed of liquid A and liquid B so that solid-liquid separation can start within 5 minutes, more preferably within 3 minutes, from the start of mixing liquid A and liquid B. Liquid A containing an alkaline agent and liquid B containing water-soluble salts of rare earth and Group II elements are simultaneously charged into a reaction tank, and the reaction is completed in a short time under conditions of maintaining a predetermined pH, so that the rare earth elements and Group II elements begin to precipitate simultaneously, and the ratio of the rare earth elements and Group II elements precipitated can be kept constant from the start to the end of the reaction. Furthermore, by keeping the reaction time short, aggregation of the rare earth elements and Group II elements can be prevented, making it possible to obtain a powder that is easy to disintegrate and has excellent dispersibility in ceramic powder.

[0049] In the present production method, it is preferable that the mixed solution of the A liquid and the B liquid is simultaneously introduced into the reaction tank as described above and stirred at high speed under a predetermined pH condition. This embodiment makes it easy to obtain powders having the CV value, average particle size Dd, Dd1, Ds / Dd, etc., within the above-mentioned predetermined ranges. Examples of high-speed stirring include stirring at a rotation speed of 10,000 to 25,000 rpm, and more preferably 18,000 to 21,000 rpm. In these stirring methods, when the stirrer in the reaction tank of the mixed solution rotates as described above, the capacity of the reaction tank is preferably 50 ml to 1 L, and more preferably 100 ml to 500 ml. Such high-speed stirring can complete the reaction in a short time.

[0050] From the viewpoint of making it easier to obtain the above CV value, average particle diameters Dd, Dd1, and Ds / Dd, the concentration of the alkaline agent in solution A is preferably 5 to 25% by mass, and more preferably 10 to 15% by mass.

[0051] (Cleaning process) The residue (also referred to as "solid material") obtained in the solid-liquid separation step is washed with water. The amount of water used for washing is preferably 0.1 L to 10 L, more preferably 0.5 L to 5 L, and even more preferably 1 L to 3 L, per 1 g of rare earth oxide used. The amount referred to here is the total amount when pure water is passed through the residue several times for washing. Pure water or ultrapure water is preferably used as the water used for washing.

[0052] (Firing process) The firing temperature is preferably 1000°C or less in terms of suppressing aggregation and suppressing crystal growth, and more preferably 800°C or less. The firing temperature is preferably 500°C or more in terms of reducing the carbon content. From this viewpoint, the firing temperature is more preferably 500°C or more and 1000°C or less, and even more preferably 500°C or more and 800°C or less. The firing can be performed in an oxygen gas-containing atmosphere such as air atmosphere, or in an inert atmosphere such as argon or nitrogen, but it is preferable to perform the firing in an oxygen gas-containing atmosphere, particularly air atmosphere, in terms of reducing the carbon content and costs.

[0053] (Crushing process) It is preferable to crush the powder obtained by firing into coarse particles. For crushing, a dry crusher can be used, for example, a crusher (product name: Force Mill, manufactured by Osaka Chemical Co., Ltd.).

[0054] The powder obtained as described above can be used for various applications by taking advantage of its dispersibility. Examples of such applications include sintering aids for ceramics, dielectrics or internal electrodes for capacitors, phosphors, refractive index adjusters for optical glass, oxygen sensors, additives for alloys, catalysts, refractories, laser crystal raw materials, and corrosion-resistant materials for semiconductor manufacturing equipment. There are various ways of using the powder, and the powder can be applied to various forms such as coating (film formation), trace addition, and molded bodies (including sintered bodies). In particular, the powder of the present invention has good dispersibility in ceramic powder, so it can be suitably used as an additive to be mixed with a ceramic main material, and can be suitably used as a sintering aid for ceramic powder, since it can be uniformly dispersed in the ceramic main material to obtain high-quality ceramics. The ceramic main material refers to a main material made of ceramic powder. The main material refers to a material that occupies 51% by mass or more of the total, more preferably 75% by mass or more, and even more preferably 90% by mass or more. The powder of the present invention has high dispersibility in ceramics, so that it is possible to disperse ceramic particles without using a large amount of energy, and the original performance of the ceramic particles can be reduced by being crushed or worn down.

[0055] <Method of manufacturing ceramic powder> The method for producing the ceramic powder of the present invention will be described below. The method for producing the ceramic powder of the present invention comprises wet mixing the powder of the present invention and a ceramic powder as a main material in a solvent using a bead mill, and then removing the solvent.

[0056] When the powder of the present invention and a ceramic powder are wet mixed in a solvent using a bead mill, the solvent, powder, and ceramic powder may be simultaneously placed in a container and mixed, or the solvent and powder may be mixed to obtain a powder dispersion, and this dispersion may be mixed with the ceramic powder. In the latter case, the solvent and powder may be mixed to obtain a powder dispersion, and the ceramic powder and solvent may be mixed to obtain a ceramic powder dispersion, and the two dispersions may be mixed.

[0057] Examples of the solvent include water and monohydric alcohols, and water is particularly preferred. When a dispersion of a powder and a dispersion of a ceramic powder are separately prepared, the solvents for both dispersions may be the same or different.

[0058] The ceramic powder preferably has a primary particle diameter of 0.05 μm or more and 5 μm or less. A primary particle diameter of 0.05 μm or more has the advantage that aggregation of the ceramic powder is suppressed and the powder can be easily dispersed in the ceramic powder. In addition, a primary particle diameter of the ceramic powder of 5 μm or less has the advantage that the technical significance of the present invention, which improves the dispersibility of the powder in the ceramic powder, becomes significant. From this viewpoint, it is more preferable that the ceramic powder has a primary particle diameter of 0.1 μm or more and 1 μm or less. The primary particle diameter is determined by the specific surface area s (m2) measured by the BET method. 2 / g) The primary particle diameter d (μm) is d = 6 / (ρs) (ρ is the true density (cm 3 The method for measuring the BET specific surface area of ​​the ceramic powder is the same as the method for measuring the specific surface area of ​​the powder described later in the Examples.

[0059] The material of the ceramic powder is not limited, but examples thereof include barium titanate, silicon nitride, aluminum nitride, and zirconium oxide.

[0060] Furthermore, the amount of the solvent used is preferably such that the solids concentration in the mixture of the solvent, ceramic powder, and powder is 1% by mass or more and 80% by mass or less, in order to uniformly adhere the powder to the ceramic powder and to reduce the viscosity and improve operability, and more preferably is 5% by mass or more and 50% by mass or less.

[0061] The powder of the present invention is preferably mixed in an amount of 0.01 to 20 parts by mass per 100 parts by mass of the main ceramic powder, in order to achieve a balance between the quality and physical properties of the resulting ceramic, and more preferably mixed in an amount of 1 to 15 parts by mass.

[0062] When a dispersion medium is used to mix the ceramic powder, the powder of the present invention, and a solvent, the material of the dispersion medium is not particularly limited, but from the viewpoint of suppressing the inclusion of metal impurities, preferred examples of the dispersion medium include ceramic media such as alumina, zirconia, silicon carbide, and silicon nitride. Zirconia here includes stabilized zirconia such as YSZ and PSZ.

[0063] From the viewpoint of shortening the dispersion time and improving the dispersibility, the particle size of the dispersion media is preferably 0.015 mm or more and 5 mm or less, and more preferably 0.05 mm or more and 1 mm or less.

[0064] The solvent is removed from the mixture of the obtained powder, ceramic powder, and water to obtain a powder. Drying is convenient for removing the solvent. Drying may be performed by a spray drying method such as spray drying, and granulation may be performed in this process. Drying can be performed at, for example, 50°C to 200°C. Examples of the drying atmosphere include an oxygen gas-containing atmosphere such as air atmosphere, an inert atmosphere such as argon or nitrogen, and a vacuum atmosphere. Drying under these conditions makes it possible to cover the surface of the ceramic particles with powder. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0066] Example 1 10 kg of an aqueous solution of ammonium hydrogen carbonate (liquid A, 25° C.) in which 13% by mass of ammonium hydrogen carbonate was dissolved was prepared. In addition, 40 L of a mixed aqueous solution of yttrium nitrate and magnesium nitrate (liquid B, 25°C) was prepared so that the total concentration of Y2O3 and MgO, calculated as oxides, was 50 g / L. The ratio of yttrium nitrate and magnesium nitrate in the nitrate aqueous solution was 100:18 in terms of mass when converted to Y2O3 and MgO, respectively. The flow rate of the B liquid was 220 mL / min, and the A and B liquids were simultaneously added to the same reaction vessel (inner volume 100 mL) and mixed at such a flow rate that the pH of the mixture was 6.5. When the liquid was added, the mixture in the vessel was stirred at 20,000 rpm. After the suspension overflowing from the vessel was filtered for 20 seconds, the addition of both liquids and stirring were stopped, and the residue, which was the filtrate, was washed with 5 L of ultrapure water. This washing process was repeated 15 times. The washed residue was fired at 700°C in an air atmosphere to obtain 10 g of a mixture of Y2O3 and MgO. The obtained mixture of Y2O3 and MgO was crushed for 30 seconds in a force mill (manufactured by Osaka Chemical Co., Ltd.) to obtain a powder.

[0067] Example 2 10 kg of an aqueous solution of ammonium carbonate (liquid A, 25° C.) in which 13% by mass of ammonium carbonate was dissolved was prepared. In addition, 40 L of a mixed aqueous solution of yttrium nitrate and magnesium nitrate (liquid B, 25°C) was prepared so that the total concentration of Y2O3 and MgO, calculated as oxides, was 50 g / L. The ratio of yttrium nitrate and magnesium nitrate in the nitrate aqueous solution was 100:18 in terms of mass when converted to Y2O3 and MgO, respectively. The flow rate of the B solution was 200 mL / min, and the A and B solutions were simultaneously charged into the same reaction tank (inner volume 100 mL) and mixed at flow rates such that the pH of the mixture was 7.5. Other than these points, the contents were the same as those described in Example 1.

[0068] Example 3 The ratio of yttrium nitrate and magnesium nitrate in the nitrate aqueous solution, which was solution B, was the same as that described in Example 2, except that the ratio was 1:9 in terms of mass of Y2O3 and MgO, respectively.

[0069] The following Comparative Examples 1 to 3 are examples in which ammonium hydrogen carbonate and yttrium nitrate were reacted to obtain Y2O3, which was then mixed with MgO powder. (Comparative Examples 1 to 3) 10 kg of an aqueous solution of ammonium hydrogen carbonate (liquid A, 25° C.) in which 13% by mass of ammonium hydrogen carbonate was dissolved was prepared. Also, 40 L of an aqueous solution (liquid B, 25° C.) containing yttrium nitrate at a concentration of 50 g / L calculated as the oxide was prepared. The flow rate of liquid B was 200 mL / min, and liquids A and B were simultaneously poured into the same reaction vessel (inner volume 100 mL) and mixed at a flow rate such that the pH of the mixture was 6.5. When pouring, the mixed liquid in the vessel was stirred at 20,000 rpm. The suspension that overflowed from the vessel was successively filtered for 20 seconds, after which the pouring of both liquids and the stirring were stopped, and the residue that was the filtrate was washed with 5 L of ultrapure water. This washing process was repeated 15 times. The washed residue was calcined at 700°C in an air atmosphere to obtain Y2O3 powder. The obtained Y2O3 powder was mixed with MgO in the ratio shown in Table 1, and crushed for 30 seconds in a force mill (manufactured by Osaka Chemical Co., Ltd.) to obtain a powder. Here, the MgO used was product number 4810NH manufactured by Skyspring Nanomaterials. The obtained powder was measured for MgO content, 40L, and specific surface area S (m 2 / g), primary particle diameter Ds (nm), volume cumulative particle diameter (D 50 , D 90 The average particle size was calculated under the specified crushing conditions, and the dispersibility with barium titanate powder was evaluated. The results are shown in Table 1.

[0070] (MgO content) The obtained powder was dissolved in nitric acid, and the amount of Mg was measured by ICP emission spectrometry and calculated as MgO.

[0071] (CV value) A scanning electron microscope (SEM, JEOL JST-IT500) and an energy dispersive X-ray analyzer (EDX, JEOL JST-IT500) were used. The SEM was measured in high current mode, with a magnification of 5000 times, an acceleration voltage of 20 kV, and a working distance of 10.0 mm. The aspect ratio of the image was 3:4. Under the above observation conditions, an image was captured using EDX, and the image was divided into 3 equal parts vertically and horizontally, and 9 central points were observed to calculate the total Mg element content and the total Y element content relative to the total mass of the powder. Analysis software: SMILE VIEW Lab CPS: 10,000 or more The total Mg element content and the total Y element content relative to the total mass were measured at nine points on each of the three images, i.e., 27 points. The MgO / Y2O3 mass ratio was calculated in terms of oxides for the 27 points, and the average value Av and standard deviation Sd were calculated, and CV = Sd / Av × 100 (%) was calculated.

[0072] (Specific surface area S) Measurement was performed using the BET single point method with a Mountec fully automatic specific surface area analyzer Macsorb model-1201. The gas used was a nitrogen-helium mixed gas (nitrogen 30 vol%). As a pretreatment for the measurement, the powder was placed in a glass cell and set in the device, and nitrogen gas was passed through the set glass cell to degas it at 300°C for 60 minutes.

[0073] (Calculation method for primary particle diameter Ds) Specific surface area S (m 2 The particle size was calculated from the particle diameter (nm) of the sample by the following formula: Ds = 6000 / (ρs) (ρ is the true density (g / cm 3 The true density of Y2O3 is 5.01 (g / cm 3 ), MgO is 3.58 (g / cm 3The true density of the mixed state was defined as 1 / ((Y2O3 concentration / ρY2O3)+(MgO concentration / ρMgO)).

[0074] (Volume cumulative particle size (D 50 , D 90 )) Place approximately 0.4 g of powdered sample in a 100 mL glass beaker, then pour 0.2 mass % sodium hexametaphosphate aqueous solution as a dispersion medium up to the 100 mL line of the beaker. Place the beaker containing the particles and dispersion medium in an ultrasonic homogenizer US-300T (output 300 W) manufactured by Nippon Seiki Seisakusho Co., Ltd., and ultrasonicate for 5 minutes to obtain a slurry for measurement. Drop this slurry for measurement into the chamber of the sample circulator of a Nikkiso Microtrac MT3300EXII, which contains a 0.2 mass % sodium hexametaphosphate aqueous solution, until the device determines that the concentration is appropriate, and then drop it into the D 50 , D 90 was measured.

[0075] (Physical properties after dispersion in a bead mill) Using each of the powders of the examples and comparative examples obtained above, 45 g of slurry (dispersion medium: pure water) with a powder concentration of 10% by mass was prepared, and 0.15 mass times the amount of the powder was added as a dispersant, FLOWLEN GW-1500 (Kyoeisha Chemical Co., Ltd.). 230 g of zirconia beads with a diameter of 0.05 mm were crushed for 60 minutes at a peripheral speed of 4 m / s using a bead mill (Apex LABO / A-LABO, manufactured by Hiroshima Metal & Machinery Co., Ltd., effective capacity 80 cc). The average particle diameter Dd1 and PI after crushing were measured by the following method.

[0076] -Method of measuring average particle size and polydispersity index- The average particle size was measured using Otsuka Electronics' ELSZ-2000ZS after the device determined that the concentration was appropriate. The slurry was diluted with pure water as the solvent at a dilution ratio determined to be in the appropriate range of 1000 to 10000 times. The average particle size and polydispersity index obtained by dynamic light scattering (photon correlation method) measured in accordance with JIS Z 8828:2019 were adopted. The same sample was measured three times, and the average of the three measurements was used as the average particle size. However, if the absolute value of the difference between the measured value of each measurement and the average of the three measurements exceeded 2% for even one of the three average measurements, the measurement result was not adopted and three new measurements were performed. The measurements were performed at 25°C.

[0077] (Disintegration evaluation: measurement of average particle size) Using the powder obtained above, 45 g of slurry (dispersion medium: water) with a powder concentration of 10% by mass was prepared, and 0.15 times the mass of Floren GW-1500 (Kyoeisha Chemical Co., Ltd.) was added as a dispersant. 230 g of zirconia beads with a diameter of 0.05 mm were crushed using a bead mill (Apex LABO / A-LABO manufactured by Hiroshima Metal & Machinery Co., Ltd., effective capacity 80 cc) at a peripheral speed of 4 m / s. Crushing was stopped at 10-minute intervals and the average particle size was measured using the following method. However, if the average particle size becomes larger than the previous measurement value, the bead mill treatment was terminated at that point, and even if the average particle size does not become larger than the previous measurement value in each of the 20 times (A) of repeating 20 times, the treatment was terminated at the point when the 20 times (A) were repeated. The particle size that was the smallest in the maximum 20 times of repetition was taken as the minimum average particle size (Dd).

[0078] (Dispersibility test with ceramic powder) 4.6 g of barium titanate powder (primary particle diameter 0.1 μm, Kyoritsu Material Co., Ltd. BTHP-100), 0.2 g of the above powder (powders of Examples 1 to 3 and Comparative Examples 1 to 3), and pure water were mixed to obtain a slurry with a solid concentration of 9.6 mass%. 0.92 g of Flowlen GW-1500 (Kyoeisha Chemical Co., Ltd.) was added as a dispersing agent. 236 g of zirconia beads (manufactured by) with a diameter of 0.05 mm were added and crushed for 60 minutes with a bead mill (Apex LABO / A-LABO manufactured by Hiroshima Metal & Machinery Co., Ltd., effective capacity 80 cc). (CV value) After disintegration, the mixture was dried at 120° C. for 10 hours in an air atmosphere (FIG. 2 is an SEM image of Example 1, magnification: 5000 times). Next, the barium titanate powder obtained as described above and the powders of each Example and Comparative Example were crushed and dried, and the SEM images were subjected to measurement of MgO / Y2O3 at nine points to measure the CV value in the same manner as described above in "(CV value)".

[0079] [Table 1]

[0080] The powders of the examples, which contain rare earth oxides and Group II element oxides and have a CV value of the ratio of the mass concentrations of the rare earth oxides and Group II element oxides (Y2O3 / MgO mass ratio), measured by SEM-EDX and converted into oxides, of 35% or less, had good dispersibility with the ceramic powder. On the other hand, in Comparative Examples 1 to 3 in which the CV was more than 35%, it was shown that the dispersibility with the ceramic powder was poor. From the above, it is clear that the powder of the present invention is useful as a sintering aid that is required to be mixed uniformly with ceramic powder.

Claims

1. The powder contains a rare earth oxide and a Group II element oxide, and the CV value of the ratio of the mass concentrations of the rare earth oxide and the Group II element oxide (Group II element oxide / rare earth oxide), measured by SEM-EDX and converted into oxides, is 35% or less.

2. 2. The powder according to claim 1, wherein the total amount of the Group II element oxide content and the rare earth oxide content is 90 mass % or more based on the total mass of the powder.

3. 2. The powder according to claim 1, wherein the content of the Group II element oxide is 0.05% by mass or more and 50% by mass or less when the total amount of the rare earth oxide and the Group II element oxide is taken as 100% by mass, as measured by ICP atomic emission spectroscopy.

4. 3. The powder of claim 1 or 2, wherein the Group II element is magnesium.

5. 3. The powder according to claim 1, wherein the rare earth oxide is at least one selected from the group consisting of yttrium oxide, gadolinium oxide, dysprosium oxide, holmium oxide and ytterbium oxide.

6. The specific surface area measured by the BET single point method is 30 m 2 / g or more 45m 2 The powder according to claim 1 or 2, wherein the molecular weight is 1 / g or less.

7. 3. The powder according to claim 1 or 2, wherein when the powder is mixed with water to form a water slurry containing 10% by mass of the powder, and the following operation (A) is repeatedly performed until the average particle diameter becomes larger than the previous measurement value, the minimum average particle diameter Dd is 40 nm or more and 110 nm or less. (A): The slurry is subjected to a bead mill treatment for 10 minutes using zirconia beads having a diameter of 0.05 mm, and then the average particle size is measured by a dynamic light scattering method. (However, if the average particle size becomes larger than the previous measurement value, the bead mill treatment is terminated at that point. Also, if the process (A) is repeated 20 times and the average particle size does not become larger than the previous measurement value in each of the second to twentieth times, the process (A) is terminated after 20 repetitions. The minimum average particle diameter Dd herein means the minimum value of the average particle diameter measured by the dynamic light scattering method by sampling after each treatment of (A).

8. The powder was mixed with water to prepare a water slurry containing 10% by mass of the powder, and the following operation (A) was repeated until the average particle diameter became larger than the previous measurement value. The smallest average particle diameter Dd was measured, and the primary particle diameter Ds calculated as the specific surface area was measured.

3. The powder according to claim 1, wherein the ratio Ds / Dd is 0.3 or more. (A): The slurry is subjected to a bead mill treatment for 10 minutes using zirconia beads having a diameter of 0.05 mm, and then the average particle size is measured by a dynamic light scattering method. (However, if the average particle size becomes larger than the previous measurement value, the bead mill treatment is terminated at that point. Also, if the process (A) is repeated 20 times and the average particle size does not become larger than the previous measurement value in each of the second to twentieth times, the process (A) is terminated after 20 repetitions. The minimum average particle diameter Dd herein means the minimum value of the average particle diameter measured by the dynamic light scattering method by sampling after each treatment of (A).

9. 3. The powder according to claim 1 or 2, wherein when the powder is mixed with water to form a water slurry containing 10% by mass of the powder, and the slurry is then subjected to a bead mill treatment for 60 minutes using zirconia beads having a diameter of 0.05 mm, the average particle size measured by a dynamic light scattering method is 150 nm or less.

10. Volume cumulative particle size D at 50% cumulative volume measured by laser diffraction scattering particle size distribution measurement method 50 The powder according to claim 1 or 2, wherein the particle size is 1 μm or more and 25 μm or less.

11. Volume cumulative particle size D at 90% cumulative volume measured by laser diffraction scattering particle size distribution measurement method 90 The powder according to claim 1 or 2, wherein the particle size is 3 μm or more and 90 μm or less.

12. 3. The powder according to claim 1, which is a ceramic additive used by mixing with a ceramic base material.

13. 13. The powder according to claim 12, which is a sintering aid for ceramic base materials.

14. A method for producing a ceramic powder containing a powder including a rare earth oxide and a Group II element oxide, comprising: A method for producing a ceramic powder, comprising wet-mixing the powder according to claim 1 or 2 with a ceramic powder in a solvent using a bead mill, and then removing the solvent.

Citation Information

Patent Citations

  • Manufacturing method of multilayer electronic part

    JP2008251699A