Polyester fiber product and polyester fiber product dyeing method

Laser pre-treatment of polyester fibers to adjust crystallinity, combined with disperse dye printing and moist heat treatment, addresses the issues of uneven dyeing and high energy consumption in conventional methods, ensuring efficient and strong dyeing results.

JP2024167888APending Publication Date: 2024-12-04KOMATSU SEIREN CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024076764
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-09
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Conventional dyeing methods for polyester fibers require high temperatures and large amounts of water, leading to uneven dyeing and increased energy consumption, while chemically modified fibers suffer from reduced strength and higher production costs.

Method used

A method involving laser pre-treatment to reduce the surface crystallinity of polyester fibers by 4% to 20% less than the center crystallinity, followed by a printing process using disperse dyes and a moist heat treatment, which includes a carbon dioxide laser with a fluence of 25J/cm² to 150J/cm² for efficient dyeing.

Benefits of technology

This approach reduces water and energy usage while preventing uneven dyeing and maintaining sufficient strength for practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167888000001
    Figure 2024167888000001
  • Figure 2024167888000002
    Figure 2024167888000002
Patent Text Reader

Abstract

To provide a polyester fiber product, which can reduce water and energy amount used in dyeing while suppressing uneven dyeing and has sufficient strength for practical use, and also to provide a method to dye the polyester fiber product.SOLUTION: A polyester fiber product to be provided includes: a polyester yarn having high surface crystallinity lower by 4% or more and 20% or less than a central part crystallinity; and a disperse dye. A polyester fiber product dyeing method to be provided includes: a laser pretreatment step to make the surface crystallinity lower by 4% or more and 20% or less than the central part crystallinity by irradiating laser to the polyester fiber product; and a printing step to print the disperse dye after the laser pretreatment step.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester fiber product and a method for dyeing a polyester fiber product. [Background technology]

[0002] For example, polyester resins having repeating carboxylic acid ester groups in the main chain, such as polyethylene terephthalate obtained by condensation polymerization of terephthalic acid and ethylene glycol, are processed into textile products such as threads, strings, woven fabrics, knitted fabrics, and nonwoven fabrics, and are widely used as polyester textile products.

[0003] Polyester fibers have excellent strength and elongation, and among general-purpose synthetic fibers, they have high heat resistance and are particularly versatile. For this reason, polyester fiber products are used in a wide variety of products, including underwear such as shirts and pants, innerwear such as blouses and sweaters, outerwear such as coats and anoraks, furniture such as curtains and upholstery, and daily necessities such as bags and sheets.

[0004] Conventionally, a dyeing method for coloring such polyester fiber products has been known in which a fiber product such as a yarn is immersed in an aqueous dispersion containing a disperse dye, and the aqueous dispersion is heated and treated at a high temperature of 130°C to 135°C, thereby causing the disperse dye to be absorbed (adsorbed) between the molecular chains constituting the polyester fiber.

[0005] However, conventional dyeing methods are prone to uneven dyeing when the amount of water used is reduced or the processing temperature is lowered. Therefore, conventional methods require a large amount of water during dyeing and a high-temperature, high-pressure heat treatment at 130°C or higher, which poses the problem of requiring a large amount of energy and time.

[0006] Therefore, a technique has been proposed to lower the temperature during dyeing by modifying polyester resin.For example, polyester fibers using sulfoisophthalic acid or the like as a polymerization component of polyester and introducing a sulfo group into polyester to enable dyeing with cationic dyes at a temperature (normal pressure) below the boiling point of water, or polyester fibers having a polyoxyalkylene group introduced into polyester to enable dyeing with disperse dyes at low temperatures, or a combination of these, are known (Patent Document 1). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 5-9807 Summary of the Invention [Problem to be solved by the invention]

[0008] However, polyester fibers that have been chemically modified, such as by introducing a sulfo group, have a problem in that the strength of the yarn is weaker than that of yarn made of general polyester fibers that are not chemically modified.In addition, the chemically modified polyester fibers have a problem in that the production cost of the polyester resin is higher than that of general polyester fibers, making them difficult to use for general purposes.

[0009] Therefore, an object of the present invention is to provide a polyester fiber product that can reduce the amount of water and energy used during dyeing while suppressing uneven dyeing, and has sufficient strength for practical use, and a method for dyeing a polyester fiber product. [Means for solving the problem]

[0010] In order to solve the above problems, the polyester fiber product according to the present invention has the following configuration.

[0011] (1) A polyester fiber product comprising a polyester yarn having a crystallinity on the surface that is 4% to 20% lower than the crystallinity in the center, and a disperse dye.

[0012] The method for dyeing polyester fiber products according to the present invention has the following configuration.

[0013] (2) A method for dyeing a polyester fiber product, comprising: a laser pretreatment step of irradiating a polyester fiber product with a laser to reduce the crystallinity of the surface by 4% to 20% lower than the crystallinity of the central portion; and a printing step of printing a disperse dye after the laser pretreatment step.

[0014] (3) The method for dyeing a polyester fiber product according to (2), wherein the printing is performed by an inkjet method.

[0015] (4) The method for dyeing a polyester fiber product according to (2) or (3), further comprising a wet heat treatment step after the printing step.

[0016] (5) The laser is a carbon dioxide laser, and the fluence of the laser is 25 J / cm 2 More than 150J / cm 2 The method for dyeing a polyester fiber product according to any one of (2) to (4) below. Effect of the Invention

[0017] According to the present invention, it is possible to provide a polyester fiber product and a dyeing method for a polyester fiber product which can reduce the amount of water and energy used during dyeing while suppressing uneven dyeing and have sufficient strength for practical use. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present invention will be described. Note that each of the embodiments described below shows one specific example of the present invention. Furthermore, the present invention is not limited to only the following aspects, and many modifications are possible within the spirit and scope of the present invention.

[0019] <Polyester fiber products> The polyester fiber product according to the present embodiment is a polyester fiber product containing a polyester yarn having a crystallinity at the surface that is 4% to 20% lower than the crystallinity at the center, and a disperse dye.

[0020] The material of the polyester fiber according to the present embodiment is not particularly limited as long as it is a polymer (polyester resin) having repeated carboxylate groups in the main chain, and examples thereof include polyethylene terephthalate (PET), polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene succinate, and polylactic acid. From the viewpoints of ease of processing by heat, high versatility, and ease of recycling, PET is preferable as the material of the polyester fiber. Note that chemical modification for improving dyeability by introducing sulfo groups or oxyalkylene groups into the molecule may be performed, but this may result in a decrease in the strength, washing fastness, sublimation fastness, and the like of the yarn. Since even polyester resins that are not particularly chemically modified can be sufficiently applied as the material of the polyester fiber according to the present embodiment, it is preferable to use polyester resins that are not particularly chemically modified.

[0021] The polyester fiber products according to the present embodiment include threads (polyester threads) made of the polyester fiber material, strings made of the threads, fabrics such as woven fabrics, knitted fabrics, and nonwoven fabrics, and sewn products such as clothing, bags, curtains, and duvet covers made using the fabrics, as well as seamless knit products made by knitting the threads into specific three-dimensional shapes such as clothing.

[0022] The polyester yarn constituting the polyester fiber product according to the present embodiment may be either a long fiber or a short fiber, and may be either a monofilament or a multifilament. From the viewpoint of versatility, the polyester yarn is preferably a long fiber multifilament.

[0023] The polyester yarn is not particularly limited, but has a fineness of 10 dtex to 200 dtex and a filament count of 1 to 300.

[0024] The polyester fiber product according to the present embodiment includes polyester yarn having a crystallinity at the surface that is 4% to 20% lower than the crystallinity at the center.

[0025] When dyeing polyester fiber products with disperse dyes, if the disperse dye is present in a form in which it is sandwiched and held between the molecular chains of the polyester resin (exhaustion) rather than in a form in which it is attached to the surface of the polyester yarn, the fastness properties of the polyester fiber products can be improved. In order for the disperse dye to be efficiently exhausted by the polyester yarn, it is preferable that the crystalline state of the polyester resin is loose, that is, the degree of crystallization is low. On the other hand, the degree of crystallization of the polyester resin is related to the mechanical strength of the fiber, so the degree of crystallization must be high to a certain degree.

[0026] Generally, polyester yarns are made by processing polyester resin into a thread shape in a melt spinning process, and then improving the mechanical strength through subsequent stretching and false twisting processes. The obtained polyester yarns are in a nearly uniform crystalline state, and the degree of crystallinity is often controlled to match the required mechanical strength, for example, about 25% to 45% for yarns made of PET fibers.

[0027] In order to improve the exhaust efficiency of disperse dyes while maintaining sufficient strength for practical use, the crystallinity of the polyester yarn may be reduced on the surface while maintaining the crystallinity of the center of the polyester yarn. From the above viewpoints, the polyester yarn contained in the polyester fiber product according to the present embodiment has a surface crystallinity that is 4% to 20% lower than the crystallinity of the center. The lower limit of the difference in crystallinity is preferably 6% or more, more preferably 8% or more. The upper limit of the difference in crystallinity is preferably 18% or less, more preferably 16% or less. In this application, the "center" refers to a cylindrical portion within a region of 1 / 2 the radius from the center of the polyester yarn when the polyester yarn is regarded as a cylinder, and the "surface" refers to a region other than the center of the polyester yarn.

[0028] The method for reducing the crystallinity of the surface of a polyester yarn is not particularly limited as long as it can be performed by heating the polyester yarn to a temperature above the glass transition temperature and below the melting point or crystallization temperature of the polyester resin and then rapidly cooling it. However, a laser irradiation treatment is preferred, which concentrates thermal energy only on the surface of the polyester yarn, makes it easy to create a difference in crystallinity between the surface and the center, and does not require any special rapid cooling means.

[0029] The crystallinity of the entire polyester yarn can be determined by the XRD method, which is determined from the integrated value of the scattering profile obtained by wide-angle X-ray scattering measurement, the DSC method, which is determined from the heat of fusion obtained by differential scanning calorimetry, and the IR method, which is determined from the absorbance ratio of a specific wavelength in the infrared spectrum. For example, in the case of PET fibers, the DSC method is used to determine the heat of fusion generated at 240°C to 260°C (after subtracting the heat of crystallization in the case where cold crystallization occurs) by dividing it by 140 J / g, the heat of fusion of a perfect crystal. In addition, the crystallinity of the surface of a polyester yarn made of PET fibers is determined by IR measurement using the ATR method, and the absorption at 973 cm, which is due to the trans isomer that constitutes the crystal, is obtained. -1 The peak absorbance at 793 cm -1 Intensity ratio A 973 / A 793and then multiplying it by 0.3. From the above, the crystallinity at the center of the polyester yarn can be calculated using the following (Equation 1), and the difference between the crystallinity at the center of the polyester yarn and the crystallinity at the surface of the polyester yarn can be calculated using the following (Equation 2). In (Equation 1) and (Equation 2), "yarn" refers to polyester yarn.

[0030] (Crystallization degree at the center of the yarn) = 4 × (Crystallization degree of the entire yarn) - 3 × (Crystallization degree of the surface of the yarn) (Equation 1) (Difference between crystallinity at the center of the yarn and crystallinity at the surface of the yarn) = 4 × {(crystallinity of the entire yarn) - (crystallinity at the surface of the yarn)} (Equation 2)

[0031] In addition, the polyester fiber product according to the present embodiment may be combined with natural fibers such as cotton, hemp, and wool, synthetic fibers such as nylon and acrylic, regenerated fibers such as rayon, and semi-synthetic fibers such as acetate, without departing from the object of the present invention. In other words, the yarn constituting the polyester fiber product according to the present embodiment may contain yarns other than polyester yarns. In addition, if the polyester fiber product is a part of a normal polyester fiber product and a part of a crystalline state, it is possible to intentionally impart color shading or to impart designs such as patterns and letters. However, from the viewpoint of easily achieving the effect of the present invention, which can reduce the amount of water and energy used while suppressing uneven dyeing, it is preferable that the fiber product used in the present embodiment uses polyester fiber products in the crystalline state for the entire yarn constituting the fiber product.

[0032] The polyester fiber product according to the present embodiment is a polyester fiber product containing the polyester yarn and a disperse dye. A typical polyester fiber product is dyed by immersing the product in an aqueous dispersion containing a disperse dye and heating the aqueous dispersion at a high temperature of 130°C to 135°C. On the other hand, in the polyester fiber product according to the present embodiment, the disperse dye is efficiently absorbed into the crystalline polyester yarn, so that uneven dyeing is suppressed even when dyed by a printing method, and the amount of water and energy used during dyeing can be reduced. Furthermore, a polyester fiber product having sufficient strength for practical use can be obtained.

[0033] <Dyeing method for polyester fiber products> Next, the method for dyeing polyester fiber products according to the present embodiment will be described.

[0034] The dyeing method for polyester fiber products according to the present embodiment is a dyeing method for polyester fiber products, including a laser pretreatment step of irradiating a polyester fiber product made of polyester yarn with a laser to reduce the crystallinity of the surface of the polyester yarn by 4% to 20% lower than the crystallinity of the center portion, and a printing step of printing a disperse dye on the polyester fiber product after the laser pretreatment step.

[0035] The dyeing method for polyester fiber products according to the present embodiment includes a laser pretreatment step of irradiating a polyester fiber product made of polyester yarn with a laser. By irradiating a polyester fiber product with a laser, heat energy is intensively applied only to the surface of the polyester yarn at least for the polyester yarn, and only the polyester molecules present on the surface of the polyester yarn are amorphized by micro-Brownian motion, and are rapidly cooled and solidified as a supercooled liquid simply by stopping the laser irradiation. The above action allows the crystallinity of the polyester yarn to be differentiated from that of the surface.

[0036] The laser used in the laser pretreatment step is not particularly limited in terms of the medium and oscillation method used, as long as it can heat only the surface of the polyester yarn in a concentrated manner. The wavelength of the laser used is preferably an infrared laser that is less attenuated in the atmosphere and can efficiently heat the polyester resin, and among them, it is preferable to use a carbon dioxide gas laser that is relatively inexpensive, has a large output, and can oscillate far-infrared rays with a wavelength of about 9.2 to 10.8 μm.

[0037] When using a carbon dioxide laser, the laser fluence is 25 J / cm 2 More than 150J / cm 2 It is preferable that the fluence of the carbon dioxide gas laser irradiated on the polyester fiber product is 25 J / cm or less. 2 More than 150J / cm 2 By setting the fluence of the carbon dioxide gas laser at 35 J / cm or less, it is easy to modify the crystallinity of the surface of the polyester yarn to a crystallinity state that is 4% to 20% lower than the crystallinity of the center portion. 2 More than 45 J / cm is preferable. 2 More preferably, the upper limit of the fluence of the carbon dioxide gas laser is 100 J / cm. 2 Less than 75 J / cm is preferable. 2 The following is more preferred:

[0038] In the laser pretreatment step, the polyester yarn is irradiated with a laser, and the treated polyester yarn may be further organized into a specific three-dimensional shape such as a string, a cloth such as a woven fabric, or a garment, or the laser irradiation treatment may be performed after the polyester yarn is previously organized into a string, a cloth, or a specific three-dimensional shape. In addition, a polyester yarn that has been laser pretreated may be combined with a polyester yarn that has not been laser pretreated, or the laser pretreatment may be performed only on a part of the organized polyester fiber product. If the polyester fiber product contains a polyester yarn that has been laser pretreated only in a part, it is possible to intentionally impart a shading of color or to impart a design such as a pattern or letter. However, from the viewpoint that the effect of the present invention, which can reduce the amount of water and energy used while suppressing dyeing unevenness, is easily obtained, it is preferable that the dyeing method of the polyester fiber product used in this embodiment performs laser pretreatment on the entire constituting yarn. When the entire constituting yarn is laser pretreated, from the viewpoint that the laser pretreatment can be performed simply and uniformly, it is preferable to perform laser pretreatment on a linear polyester fiber product such as a thread or string, or a planar polyester fiber product such as a woven fabric or knitted fabric, and then organize it into a specific three-dimensional shape such as a garment by sewing or knitting.

[0039] The dyeing method for polyester fiber products according to the present embodiment includes a step of printing a disperse dye on a polyester fiber product after the laser pretreatment step. Generally, polyester fiber products are dyed by immersing them in an aqueous dispersion containing a disperse dye and heating the aqueous dispersion at a high temperature of 130° C. to 135° C., but the polyester fiber product according to the present embodiment can be dyed by a printing method that applies a disperse dye to the surface of the polyester fiber product, thereby obtaining a polyester fiber product with reduced dyeing unevenness, and thus reducing the amount of water and energy used during dyeing.

[0040] The disperse dye colorant used in printing is not particularly limited, and for example, a color having the color index name "Disperse" may be used.

[0041] The dye is used as a disperse dye by mixing it with a medium such as water and appropriate auxiliaries such as a dispersant for dispersing the dye in the medium, a penetrant for facilitating the dye's penetration into polyester yarn, a glue for fixing the dye to polyester yarn, etc. When printing is performed using the inkjet method described below, in order to prevent the occurrence of problems such as the dye clogging the ejection nozzle, the pH of the disperse dye should be 5.5 or more and 9.5 or less, the electrical conductivity of the disperse dye should be 60 S / m or less, and the average particle size (D50) of the dye should be 350 nm or less.

[0042] The specific printing method for printing the disperse dye on the polyester fiber product that has been subjected to the laser pretreatment is not particularly limited, and examples thereof include a screen method, a rotary method, a flexographic method, a gravure method, an offset method, a thermal transfer method, an inkjet method, etc. Among them, the inkjet method is preferably used as the printing method, from the viewpoint that a polyester fiber product in which dye unevenness is suppressed is easily obtained even with a disperse dye that is mixed with a high pigment ratio and a low amount of an auxiliary, by discharging only the necessary amount of disperse dye on the target without leaving any residual dye.

[0043] From the viewpoint that the crystalline state of the polyester yarn is unlikely to change due to heat treatment or the like between the laser pretreatment step and the next printing step, it is preferable not to include another step between the laser pretreatment step and the printing step.

[0044] In the dyeing method for polyester fiber products according to the present embodiment, it is preferable to carry out a wet heat treatment step after the printing step. In this wet heat treatment step, the polyester fiber product to which the disperse dye has been applied by printing is subjected to a wet heat treatment. By carrying out the wet heat treatment step, the disperse dye is more firmly absorbed and the dyeing efficiency of the disperse dye and various fastnesses can be improved. The specific wet heat treatment method is not particularly limited, but examples include a method of introducing the material into a chamber filled with steam at 105°C to 150°C, and a method of spraying live steam or dry steam at 160°C to 190°C. The method of spraying dry steam is preferable because it can be treated at high temperatures even in an open system and the amount of moisture given to the polyester fiber product can be easily controlled.

[0045] Furthermore, in order to improve the fastness of the polyester fiber product, a washing step may be included in which unadsorbed coloring matter and auxiliaries in the disperse dye are washed away. The washing step is not particularly limited as long as it is possible to remove excess chemicals from the polyester fiber, and for example, the polyester fiber product printed with the disperse dye may be treated in a bath containing cold water, hot water, or a soaping agent made of an appropriate surfactant, reducing agent, etc.

[0046] As described above, according to the dyeing method of the polyester fiber product of the present embodiment, even if the polyester fiber product is dyed by a printing method in which a disperse dye is applied to the surface of the polyester fiber product, a polyester fiber product with suppressed dyeing unevenness can be obtained, and therefore the amount of water and energy used during dyeing can be reduced.

[0047] The dyed polyester fiber product may be subjected to functional treatments such as drying, finishing set, water repellency, water absorption, flame retardancy, antibacterial and deodorizing, bacteriostatic, SR, deodorizing, ultraviolet shielding, and infrared shielding by known methods.

[0048] The dyed polyester fiber product may be subjected to a process for imparting design, such as calendaring, embossing, or printing with a special pattern or letters.

[0049] Furthermore, in the case of a cloth-like polyester fiber product, it may be laminated with the same or a different fabric to change the thickness or the appearance of the front and back, or a resin film made of a urethane resin, acrylic resin, or the like may be laminated on the dyed cloth-like polyester fiber product by a known method to make a waterproof fabric. EXAMPLES

[0050] The polyester fiber product and the dyeing method of the polyester fiber product according to the present embodiment will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. Note that various physical properties in the following examples and comparative examples were measured by the following methods.

[0051] (1) Crystallinity of polyester yarn First, the crystallinity of the entire polyester yarn was determined by the DSC method. A DSC8500 (PerkinElmer) was used as the DSC measurement device, and measurements were performed under conditions of a temperature rise rate of 5°C / min from room temperature to 280°C to obtain a DSC profile. From the obtained profile, the heat of fusion (J / g) generated at 240°C to 260°C and the heat of crystallization when cold crystallization occurred were obtained, and the value obtained by subtracting the heat of crystallization from the heat of fusion was divided by 140 J / g to obtain the crystallinity of the entire polyester yarn.

[0052] Next, the crystallinity of the surface of the polyester yarn was measured by the IR method. The IR spectrometer used was IRPrestige-21 (manufactured by Shimadzu Corporation), and the prism was germanium. The ATR method was performed with an incident angle of 45° and a wavelength of 4000 to 700 cm. -1 The IR spectrum was obtained by integrating the range 32 times. -1 Peak absorbance at 793 cm -1 The intensity ratio of the peak absorbance at each point was calculated and then multiplied by 0.3 to determine the crystallinity of the surface of the polyester yarn.

[0053] From the crystallinity of the entire polyester yarn obtained above and the crystallinity of the surface of the polyester yarn, the difference between the crystallinity of the center part of the polyester yarn and the crystallinity of the surface of the polyester yarn was calculated by the following (Equation 3). In (Equation 3), "yarn" refers to polyester yarn.

[0054] (Difference between crystallinity at the center of the yarn and crystallinity at the surface of the yarn) = 4 × {(crystallinity of the entire yarn) - (crystallinity at the surface of the yarn)} (Equation 3)

[0055] (2) Ease of dyeing The dyeability of the dyed fabric was evaluated based on the K / S value. A KURABO COLOR-7x (Kurabo Industries, Ltd.) was used as a colorimeter, and a reflectance spectrum was obtained using a D65 light source at 380 nm to 720 nm and a viewing angle of 2°. The reflectance at the maximum absorption wavelength in the obtained spectrum was taken as R, and the K / S value was calculated using the following formula 4. A larger K / S value indicates a darker dye.

[0056] K / S=(1-R) 2 / 2R...(Formula 4)

[0057] (3) Washing fastness The dyed fabric was tested according to JIS L0844 (2011) Color fastness test for washing, Method A, No. A-2. The attached white cloth was made of polyester and cotton, and the staining was evaluated by the grade of the attached white cloth with the most severe staining.

[0058] (4) Tear strength Tear strength according to JIS L1096 (2020) Method D (pendulum method) was tested three times in each warp and weft directions of the fabric, and the average value was taken as the tear strength.

[0059] Example 1 <Polyester fabric> In Example 1, a polyester fabric was prepared as a polyester fiber product. Specifically, a polyester fabric was prepared that was woven using polyester yarns made of polyethylene terephthalate and false-twisted, with a warp and weft fineness of 22 dtex / 20 filaments.

[0060] <Laser pretreatment> Using a galvano-type carbon dioxide gas laser processing machine, SEI INFINITY 3350 (manufactured by Comnet Co., Ltd.), the entire surface of the polyester fabric was laser-cut with a fluence of 25 J / cm. 2 The carbon dioxide gas laser was irradiated under the following conditions. The difference in crystallinity between the center of the polyester yarn and the surface of the polyester yarn immediately after the laser pretreatment is shown in Table 1.

[0061] <Ink> The ground red anthraquinone disperse dye was classified to an average particle size (D50) of 300 nm, and the pigment was dispersed in water using a dispersant to prepare a red ink containing 7 wt% pigment. Similarly, a yellow ink was prepared using a yellow anthraquinone disperse dye, and a blue ink was prepared using a blue anthraquinone disperse dye. The pH of each ink was 7.0 to 7.6, and the electrical conductivity of each ink was 45 to 54 S / m.

[0062] <Inkjet printing> The ink was discharged onto the laser-pretreated polyester fabric at a discharge rate of 10 pL from one nozzle with a resolution of 600 x 600 dpi, and then dried at 120°C.

[0063] <Post-processing> The inkjet-printed polyester fabric was washed in a soaping bath containing a soaping agent, then in a water bath, and then dried to obtain a polyester fabric whose entire surface was inkjet-printed (dyed) in a plain khaki color with a disperse dye. The various evaluation results of the obtained polyester fabric are shown in Table 1.

[0064] Example 2 <Moisture heat treatment> In Example 2, a dyed polyester fabric was obtained in the same manner as in Example 1, except that a wet heat treatment was performed by spraying dry steam at 170° C. between the inkjet printing step and the post-treatment step. The evaluation results of the obtained polyester fabric are shown in Table 1.

[0065] (Examples 3 and 4) In Examples 3 and 4, the fluence of the carbon dioxide laser was 50 J / cm 2 Except for the above, two dyed polyester fabrics were obtained in the same manner as in Examples 1 and 2. The two obtained polyester fabrics are designated as Examples 3 and 4, and the results of various evaluations are shown in Table 1.

[0066] (Examples 5 and 6) In Examples 5 and 6, the fluence of the carbon dioxide laser was 150 J / cm 2 Except for the above, two dyed polyester fabrics were obtained in the same manner as in Examples 1 and 2. The obtained two polyester fabrics are designated as Examples 5 and 6, and the results of various evaluations are shown in Table 1.

[0067] Comparative Example 1 In Comparative Example 1, except that the laser pretreatment step was omitted, a dyed polyester fabric was obtained in the same manner as in Example 2. The various evaluation results of the obtained polyester fabric are shown in Table 1.

[0068] Comparative Example 2 In Comparative Example 2, the fluence of the carbon dioxide laser was 200 J / cm 2 A dyed polyester fabric was obtained in the same manner as in Example 2, except that the above-mentioned was used. The evaluation results of the obtained polyester fabric are shown in Table 1.

[0069] [Table 1]

[0070] (Examples 7 and 8) In Examples 7 and 8, two polyester fabrics were obtained by dyeing in the same manner as in Examples 1 and 2, except that a polyester fabric woven using false-twisted polyethylene terephthalate yarns with a warp and weft fineness of 83 dtex / 36 filaments was used as the polyester fiber product. The two obtained polyester fabrics are referred to as Examples 7 and 8, and the various evaluation results are shown in Table 2.

[0071] (Examples 9 and 10) In Examples 9 and 10, the fluence of the carbon dioxide laser was 75 J / cm 2 Except for the above, two dyed polyester fabrics were obtained in the same manner as in Examples 7 and 8. The obtained two polyester fabrics are designated as Examples 9 and 10, and the results of various evaluations are shown in Table 2.

[0072] (Examples 11 and 12) In Examples 11 and 12, the fluence of the carbon dioxide laser was 150 J / cm 2 Except for the above, two dyed polyester fabrics were obtained in the same manner as in Examples 7 and 8. The obtained two polyester fabrics are designated as Examples 11 and 12, and the results of various evaluations are shown in Table 2.

[0073] Comparative Example 3 In Comparative Example 3, except that the laser pretreatment step was omitted, a dyed polyester fabric was obtained in the same manner as in Example 8. The various evaluation results of the obtained polyester fabric are shown in Table 2.

[0074] Comparative Example 4 In Comparative Example 4, the fluence of the carbon dioxide laser was 200 J / cm 2 Except for the above, a dyed polyester fabric was obtained in the same manner as in Example 8. The evaluation results of the obtained polyester fabric are shown in Table 2.

[0075] [Table 2]

Claims

1. The polyester fiber product comprises a polyester yarn having a crystallinity at the surface that is 4% to 20% lower than the crystallinity at the center, and a disperse dye.

2. A method for dyeing a polyester fiber product, comprising: a laser pretreatment step of irradiating a polyester fiber product made of polyester yarn with a laser to reduce the crystallinity of the surface of the polyester yarn by 4% to 20% lower than the crystallinity of the central portion; and a printing step of printing a disperse dye on the polyester fiber product after the laser pretreatment step.

3. The method for dyeing a polyester fiber product according to claim 2, wherein the printing is performed by an inkjet method.

4. The method for dyeing a polyester fiber product according to claim 2 or 3, further comprising a wet heat treatment step after the printing step.

5. The laser is a carbon dioxide laser, and the fluence of the laser is 25 J / cm 2 More than 150J / cm 2 The method for dyeing a polyester fiber product according to claim 2 or 3, wherein:

Citation Information