Binder for lithium ion electrode, lithium ion electrode, lithium ion battery, and method for producing binder for lithium ion electrode
A solvent-free binder system for lithium ion batteries, composed of a copolymer of (meth)acrylate and vinyl carboxylic acid with a polyolefin macromonomer, addresses the issues of solvent-based and water-based binders by providing strong adhesion and electrode strength without affecting battery performance, thus being environmentally friendly.
Patent Information
- Application Number
- JP2023084843
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing solvent-based binders for lithium ion batteries are harmful to human health and the environment, while water-based binders like SBR-based and ethylene-(meth)acrylic acid copolymers have issues with processability and can affect battery performance, such as increased internal resistance and deteriorated cycle characteristics.
A solvent-free binder system using a copolymer of (meth)acrylate and vinyl carboxylic acid with a polyolefin macromonomer having a hydroxyl group, specifically a binder composed of an ester of a copolymer of (meth)acrylate and vinyl carboxylic acid with a polyolefin macromonomer having a weight average molecular weight of 5,000 to 10,000 and an acid value of 15 to 25 mgKOH/g, which provides good adhesion and electrode strength without adverse effects on battery performance.
The proposed binder achieves good adhesion with the current collector, maintains sufficient electrode strength, and does not negatively impact battery performance, while being environmentally friendly due to the absence of solvents.
Smart Images

Figure 2024168295000001 
Figure 2024168295000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder for a lithium ion electrode, a lithium ion electrode, a lithium ion battery, and a method for producing the binder for a lithium ion electrode. [Background technology]
[0002] Non-aqueous secondary batteries such as lithium ion batteries are characterized by high voltage and high energy density, and are therefore widely used in the field of portable information devices, including mobile phones and laptop computers. In addition, as portable devices become more sophisticated and diversified, there is a demand for even higher performance (higher capacity, higher energy density, etc.) for the non-aqueous secondary batteries that serve as their power sources.
[0003] There are two types of electrode binders known for lithium-ion batteries: solvent-based and water-based. Of these, solvent-based electrode binders have tended to be avoided in recent years due to their toxicity to the human body and their large environmental impact, and research into water-based electrode binders is underway. Conventionally, SBR-based binders have been widely used as aqueous electrode binders, and other binders that have been investigated include ethylene-(meth)acrylic acid copolymers (Patent Document 1) and neutralized ethylene-(meth)acrylic acid copolymers (Patent Document 2).
[0004] However, the binder described in Patent Document 1 has poor processability and requires a thickener when preparing an electrode. In addition, the binder described in Patent Document 2 has issues such as the possibility that residues of non-volatile alkaline compounds and the like may affect battery performance (specifically, for example, an increase in internal resistance and a deterioration in cycle characteristics). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-051678 A [Patent Document 2] International Publication No. 2015 / 083358 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems, and has an object to provide a lithium ion electrode binder that can be used to produce, in a solvent-free system, a lithium ion electrode that has good adhesion to a current collector, sufficient electrode strength, and does not adversely affect battery performance (internal resistance, cycle characteristics), and a method for producing the lithium ion electrode binder in a solvent-free system. [Means for solving the problem]
[0007] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. The present invention relates to a lithium ion electrode binder (X) comprising a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms, and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, wherein the polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000, and the ester (C) has an acid value of 15 to 25 mgKOH / g; a lithium ion electrode comprising the lithium ion electrode binder; a lithium ion battery comprising the lithium ion electrode; and a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end. The method for producing a lithium ion electrode binder (X) contains a copolymer (A) of a vinyl carboxylic acid (a2) having 4 or more carbon atoms and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, the method comprising the step of polymerizing the (meth)acrylate (a1) and the vinyl carboxylic acid (a2) having 4 or more carbon atoms in the presence of the polyolefin macromonomer (B) to obtain the copolymer (A), wherein the polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000 and the ester (C) has an acid value of 15 to 25 mgKOH / g. Effect of the Invention
[0008] According to the present invention, it is possible to provide a binder for lithium ion electrodes that can be used to produce, in a solvent-free system, a lithium ion electrode that has good adhesion to a current collector, sufficient electrode strength, and does not adversely affect battery performance (internal resistance, cycle characteristics), and a method for producing the binder for lithium ion electrodes in a solvent-free system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Lithium ion electrode binder (X)> The lithium ion electrode binder (X) of the present invention comprises a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms, and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, wherein the polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000, and the ester (C) has an acid value of 15 to 25 mgKOH / g.
[0010] The copolymer (A) is a copolymer of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms.
[0011] [(Meth)acrylate (a1)] In this specification, "(meth)acrylate" refers to an alkyl ester of (meth)acrylic acid. Also, "(meth)acrylate" refers to "acrylate and / or methacrylate".
[0012] The alkyl group constituting the (meth)acrylate (a1) is preferably an alkyl group having 1 to 4 carbon atoms, and more preferably an alkyl group having 1 to 2 carbon atoms. Examples of the (meth)acrylate (a1) include methyl (meth)acrylate and ethyl (meth)acrylate. Two or more kinds of (meth)acrylates (a1) may be used in combination. Of these, methyl methacrylate is preferred.
[0013] [Vinyl carboxylic acid (a2)] The vinyl carboxylic acid (a2) has 4 or more carbon atoms.
[0014] Examples of the vinyl carboxylic acid (a2) having 4 or more carbon atoms include aliphatic vinyl carboxylic acids such as methacrylic acid, 3-butenoic acid, 4-pentenoic acid, 5-hexenoic acid, 6-heptenoic acid, 7-octenoic acid, 8-nonenoic acid, 9-decenoic acid, 10-undecenoic acid, 11-dodecenoic acid, 12-tridecenoic acid, 13-tetradecenoic acid, 14-pentadecenoic acid, 15-hexadecenoic acid, 16-heptadecenoic acid, 17-octadecenoic acid, 18-nonadecenoic acid, and 19-icosenoic acid; and aromatic vinyl carboxylic acids such as 4-vinylbenzoic acid and 4-allylbenzoic acid. Two or more kinds of vinyl carboxylic acids (a2) may be used in combination.
[0015] The vinyl carboxylic acid (a2) preferably has 5 or more carbon atoms. The vinyl carboxylic acid (a2) preferably has 11 or less carbon atoms.
[0016] The vinyl carboxylic acid (a2) is preferably an aliphatic vinyl carboxylic acid, more preferably an aliphatic vinyl carboxylic acid having 5 or more carbon atoms. By using an aliphatic vinyl carboxylic acid having 5 or more carbon atoms, the cycle characteristics can be improved.
[0017] The weight proportion of the (meth)acrylate (a1) in the copolymer (A) is preferably 10% by weight or more, more preferably 20% by weight or more, further preferably 30% by weight or more, and particularly preferably 40% by weight or more. The weight proportion of the (meth)acrylate (a1) in the copolymer (A) is preferably 80% by weight or less, more preferably 70% by weight or less, even more preferably 60% by weight or less, and particularly preferably 50% by weight or less.
[0018] [Polyolefin macromonomer (B)] The polyolefin macromonomer (B) has a hydroxyl group at least at one end. The polyolefin macromonomer (B) may have hydroxyl groups at both ends.
[0019] As the polyolefin macromonomer (B), for example, hydrogenated polybutadiene alcohol, hydroxyl group-modified polypropylene, etc. can be used.
[0020] The weight average molecular weight (Mw) of the polyolefin macromonomer (B) is 5,000 to 10,000. The Mw of the polyolefin macromonomer (B) is preferably 6,000 or more. The Mw of the polyolefin macromonomer (B) is preferably 8,000 or less.
[0021] [Ester (C)] The ester (C) is an ester of the copolymer (A) and the polyolefin macromonomer (B).
[0022] From the viewpoint of electrode strength, the weight proportion of the structural unit derived from the polyolefin macromonomer (B) is preferably 50 to 70% based on the weight of the ester (C). If the weight ratio of the structural unit derived from the polyolefin macromonomer (B) exceeds 70% based on the weight of the ester (C), the breaking strength of the ester (C) may decrease, and if the weight ratio of the structural unit derived from the polyolefin macromonomer (B) is less than 50% based on the weight of the ester (C), the flexibility of the ester (C) may decrease.
[0023] The weight proportion of the structural units derived from the polyolefin macromonomer (B) in the ester (C) can be determined from the hydroxyl value of the ester (C).
[0024] The glass transition temperature (Tg) of the ester (C) is preferably −20° C. or higher, more preferably 0° C. or higher, and even more preferably 5° C. or higher, from the viewpoint of moldability. The glass transition temperature (Tg) of the ester (C) is preferably 40° C. or lower, more preferably 20° C. or lower, and even more preferably 10° C. or lower.
[0025] The glass transition temperature (Tg) of the ester (C) can be determined by differential scanning calorimetry (DSC). Specifically, the glass transition temperature (Tg) is determined from the intersection of the baseline of a heat flux curve obtained using a differential scanning calorimeter and the tangent at the inflection point. The heat flux curve is obtained under the following conditions: about 10 mg of a sample is cooled to -50°C, held for 5 minutes, heated to 120°C at 10°C / min, cooled to -50°C, held for 5 minutes, and then heated to 120°C at 10°C / min. The glass transition temperature (Tg) is determined using the second heat flux curve. As the differential scanning calorimeter, for example, DSC Q2000 manufactured by TA Instruments can be used.
[0026] The acid value of the ester (C) is 15 to 25 mg KOH / g. The acid value of the ester (C) is preferably 17 to 23 mgKOH / g. The acid value of the ester (C) can be measured by the method specified in JIS K0070 (1992).
[0027] The weight average molecular weight (Mw) of the ester (C) is preferably 5,000 or more, more preferably 30,000 or more, even more preferably 50,000 or more, particularly preferably 100,000 or more, and most preferably 140,000 or more, from the viewpoints of electrode strength and battery performance. The weight average molecular weight (Mw) of the ester (C) is preferably 1,000,000 or less, more preferably 500,000 or less, further preferably 300,000 or less, particularly preferably 200,000 or less, and most preferably 150,000 or less, from the viewpoints of electrode strength and battery performance.
[0028] The weight average molecular weight (Mw) of the copolymer (A), the polyolefin macromonomer (B) and the ester (C) can be determined by gel permeation chromatography (hereinafter abbreviated as GPC) measurement under the following conditions. The sample polymer is dissolved in tetrahydrofuran (THF) to prepare a 0.25 wt % THF solution, and the insoluble matter is filtered through a PTFE filter having an aperture of 1 μm to prepare the sample solution. Equipment: HLC-8320 [Tosoh Corporation] Column: 2 TSK GEL GMH6 [Tosoh Corporation] Measurement temperature: 40℃ Sample solution: 0.25% by weight tetrahydrofuran (THF) solution Mobile phase: THF (containing no polymerization inhibitor) Solution injection volume: 100μL Detector: Refractive index detector Reference material: Standard polystyrene (TSKstandard POLYSTYRENE)
[0029] The breaking strength of the ester (C) is preferably 0.2 MPa or more, more preferably 0.3 MPa or more, and even more preferably 0.4 MPa or more.
[0030] The breaking strength of ester (C) is 20kgf / cm at 100℃. 2 The specimen is pressed under a pressure of 100 MPa for 30 seconds to form into a 1 mm thick sheet, which is then punched out into a shape conforming to JIS K 7127 (1999) and subjected to an autograph tensile test to measure the strength. The measurement conditions are a temperature of 25°C and a tensile speed of the test piece of 200 mm / min.
[0031] The peel strength of the ester (C) is preferably 0.8 N / mm or more, and more preferably 1.0 N / mm or more.
[0032] The peel strength of ester (C) was measured by stacking ester (C) on a 25 μm thick polypropylene film at 100°C and 20 kgf / cm 2 The strength is measured by performing a 90° peel strength test on an adhesive film made by bonding a 1 mm thick ester (C) sheet to a 25 μm thick polypropylene film, pressing the film under a pressure of 1000 psi for 30 seconds. The measurement conditions are a temperature of 25°C and a pulling speed of 20 mm / min.
[0033] The lithium ion electrode binder (X) of the present invention may contain only the ester (C) or may contain components other than the ester (C). When the lithium ion electrode binder (X) contains a component other than the ester (C), the weight ratio of the components other than the ester (C) in the lithium ion electrode binder (X) is preferably 10% by weight or less.
[0034] <Lithium ion electrode> The lithium ion electrode of the present invention comprises the binder for a lithium ion electrode of the present invention. It should be noted that the lithium ion electrode refers to an electrode for a lithium ion battery.
[0035] Since the lithium ion electrode of the present invention contains the binder for lithium ion electrodes of the present invention, it has good adhesion to the current collector, has sufficient electrode strength, and does not adversely affect battery performance (internal resistance, cycle characteristics).
[0036] Since the lithium ion electrode binder of the present invention is used, the lithium ion electrode of the present invention is produced by a method that does not use a solvent (organic solvent or aqueous solvent), and therefore is less harmful to the human body and has a small environmental impact.
[0037] For the components constituting the lithium ion electrode of the present invention, other than the binder for the lithium ion electrode, known materials can be used. That is, known materials can be used as the positive electrode active material, the negative electrode active material, the conductive assistant, and the like. The lithium ion electrode of the present invention may be a positive electrode or a negative electrode for a lithium ion battery.
[0038] <Lithium-ion battery> The lithium ion battery of the present invention comprises the lithium ion electrode of the present invention.
[0039] The lithium ion battery of the present invention has excellent battery performance (internal resistance, cycle characteristics) because it includes the lithium ion electrode of the present invention.
[0040] For the components constituting the lithium ion battery of the present invention, other than the lithium ion electrodes, known materials can be used. That is, known materials can be used as the materials for the current collector, the electrolyte, the separator, and the like.
[0041] In the lithium ion battery of the present invention, only the positive electrode may be composed of the lithium ion electrode of the present invention, only the negative electrode may be composed of the lithium ion electrode of the present invention, or both the positive electrode and the negative electrode may be composed of the lithium ion electrode of the present invention.
[0042] <Method of manufacturing binder for lithium ion electrodes> The method for producing a lithium ion electrode binder of the present invention is a method for producing a lithium ion electrode binder (X) containing a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms, and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, the method comprising the step of polymerizing the (meth)acrylate (a1) and the vinyl carboxylic acid (a2) having 4 or more carbon atoms in the presence of the polyolefin macromonomer (B) to obtain the copolymer (A), wherein the polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000, and the ester (C) has an acid value of 15 to 25 mgKOH / g.
[0043] The method for producing a binder for a lithium ion electrode of the present invention includes a step of polymerizing a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms in the presence of a polyolefin macromonomer (B) to obtain a copolymer (A) (hereinafter also referred to as a first polymerization step).
[0044] In the method for producing a binder for a lithium ion electrode of the present invention, the polyolefin macromonomer (B) functions as a solvent when the (meth)acrylate (a1) and the vinyl carboxylic acid (a2) are polymerized in the first polymerization step, so there is no need to use a solvent in the first polymerization step.
[0045] In the method for producing a lithium ion electrode binder of the present invention, the first polymerization step is followed by a step of polymerizing the polyolefin macromonomer (B) and the copolymer (A) to obtain an ester (C) of the polyolefin macromonomer (B) [hereinafter also referred to as the second polymerization step].
[0046] In the second polymerization step, since the unreacted polyolefin macromonomer (B) and the water generated by the esterification reaction function as a solvent, there is no need to add a separate solvent.
[0047] As described above, the method for producing a lithium ion electrode binder of the present invention can produce the lithium ion electrode binder of the present invention in a solvent-free system without using an organic solvent.
[0048] In the method for producing a binder for a lithium ion electrode of the present invention, it is preferable not to use an organic solvent in the first polymerization step, and it is more preferable to mix only the polyolefin macromonomer (B), the (meth)acrylate (a1), the vinyl carboxylic acid (a2), and the polymerization initiator.
[0049] The amount of polyolefin macromonomer (B) used in the first polymerization step may be the same as the amount used for polymerization with copolymer (A) in the second polymerization step, or may be less than the amount used for polymerization with copolymer (A) in the second polymerization step. When the amount of polyolefin macromonomer (B) used in the first polymerization step is less than the amount used for polymerization with copolymer (A) in the second polymerization step, it is preferable to adjust the amount of polyolefin macromonomer (B) after the first polymerization step and before the start of the second polymerization step.
[0050] The amount of the polyolefin macromonomer (B) used in the polymerization with the copolymer (A) in the second polymerization step is preferably 50 to 70% by weight based on the total weight of the copolymer (A) and the polyolefin macromonomer (B).
[0051] The present specification discloses the following:
[0052] The present disclosure (1) relates to a lithium ion electrode binder (X) comprising a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms, and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, wherein the polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000, and the ester (C) has an acid value of 15 to 25 mgKOH / g.
[0053] The present disclosure (2) is the binder for a lithium ion electrode according to the present disclosure (1), in which the weight ratio of the structural unit derived from the polyolefin macromonomer (B) is 50 to 70% based on the weight of the ester (C).
[0054] The present disclosure (3) is a lithium ion electrode comprising the binder for a lithium ion electrode according to the present disclosure (1) or (2).
[0055] The present disclosure (4) is a lithium ion battery including the lithium ion electrode according to the present disclosure (3).
[0056] The present disclosure (5) is a method for producing a lithium ion electrode binder (X) containing a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms, and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, the method comprising the step of polymerizing the (meth)acrylate (a1) and the vinyl carboxylic acid (a2) having 4 or more carbon atoms in the presence of the polyolefin macromonomer (B) to obtain the copolymer (A), wherein the polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000, and the ester (C) has an acid value of 15 to 25 mgKOH / g. EXAMPLES
[0057] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the present invention. In addition, unless otherwise specified, parts means parts by weight and % means % by weight.
[0058] Example 1 <Preparation of Lithium-ion Electrode Binder (X)> An autoclave was charged with 658 parts of hydrogenated butadiene alcohol (Mw: 7,000) as the polyolefin macromonomer (B), and the inside was replaced with nitrogen, and then the temperature was raised to 70° C. in a stirred, sealed state. While controlling the temperature inside the autoclave at 70° C., a mixed solution of 164 parts of methyl methacrylate as the (meth)acrylate (a1), 164 parts of methacrylic acid as the vinyl carboxylic acid (a2) having 4 or more carbon atoms, and 3.5 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) as a polymerization initiator was dropped over 3 hours to carry out polymerization. After the dropping, the dropping line was washed with 12 parts of hydrogenated butadiene alcohol. After keeping the mixture at the same temperature for another hour, the mixture was heated to 80°C and reacted for 2 hours. Then, an esterification reaction was carried out at 120°C to obtain a binder for lithium ion electrodes (X-1) consisting of the copolymer (A) and the ester (C-1) of the polyolefin macromonomer (B). The acid value, weight average molecular weight (Mw), glass transition temperature (Tg), breaking strength and peel strength of the lithium ion electrode binder (X-1) [ester (C-1)] were measured by the above-mentioned methods, and the results were acid value: 20 mg KOH / g, Mw: 145,000, Tg: 1.5°C, peel strength: 1.0 N / mm and breaking strength: 0.4 MPa, respectively.
[0059] (Examples 2 to 4, Comparative Examples 1 to 3) The amount of (a1), the type and amount of (a2), and the amount of (B) were changed as shown in Table 1, and the same procedure as in Example 1 was used to prepare lithium ion electrode binders (X-2) to (X-4) and (X-1) to (X-3) made of esters (C-2) to (C-4) and (C-1) to (C-3), and the acid value, weight average molecular weight (Mw), glass transition temperature (Tg), breaking strength, and peel strength were measured. The results are shown in Table 1.
[0060] [Table 1]
[0061] The results in Table 1 show that the lithium ion electrode binder of the present invention has high peel strength and breaking strength.
[0062] Example 5 (Preparation of positive electrodes for lithium-ion batteries) A slurry was prepared by mixing 85 parts of lithium nickel oxide (NCA) powder (manufactured by Sumitomo Metal Mining Co., Ltd.) as a positive electrode active material and 10 parts of acetylene black (Denka Black (registered trademark) manufactured by Denka Co., Ltd.) with an N-methylpyrrolidone (NMP) solution containing 5 parts of polyvinylidene fluoride (PVdF) (manufactured by Sigma-Aldrich Co., Ltd.). The above slurry was applied to one side of an aluminum electrolytic foil having a thickness of 20 μm using a coater in the atmosphere, and dried at 100° C. for 15 minutes to prepare a positive electrode for a lithium ion battery. The weight of the positive electrode active material layer formed on the aluminum electrolytic foil was 18.0 mg / cm 2 It was.
[0063] (Preparation of negative electrodes for lithium-ion batteries) 92 parts of graphite as a negative electrode active material, 2 parts of carbon fiber as a conductive material, 4 parts of the binder (X-1) prepared in Example 1, and 2 parts of acetylene black as a conductive assistant were blended in a Henschel mixer for 3 minutes, and then the temperature was adjusted to 80°C and pressed in a hot press for 30 seconds at a pressure of 15 MPa to obtain an electrode sheet, which was punched out to a diameter of 16 mm to prepare a negative electrode for a lithium ion battery. The weight of the negative electrode for a lithium ion battery was 20 mg / cm. 2 It was.
[0064] (Preparation of batteries for performance evaluation) The fabricated lithium-ion battery negative electrode was placed on both ends of a 2032-type coin cell together with a lithium-ion battery positive electrode punched to a diameter of 15 mm. A copper foil having a thickness of 20 μm was used as the current collector on the negative electrode side. Two separators (Celgard 3501) were inserted between the electrodes to create a battery cell for evaluation. The above electrolyte was injected into an evaluation battery cell and sealed, to prepare an evaluation battery (Y-1) according to Example 5.
[0065] (Examples 6 to 8, Comparative Examples 4 to 8) Except for changing the lithium ion electrode binder (X-1) to the binder shown in Table 2, the same procedure as in Example 5 was used to obtain evaluation batteries (Y-2) to (Y-4) according to Examples 6 to 8 and comparative batteries (comparison Y-1) to (comparison Y-5) according to Comparative Examples 4 to 8. In Comparative Example 8, polyvinylidene fluoride (PVdF) was used as the binder for the lithium ion electrode (Comparative Example X-4).
[0066] [Electrode strength evaluation] The yield stress of the obtained negative electrode (Φ16 mm) was measured using an autograph (manufactured by Shimadzu Corporation) in accordance with ISO178 (Plastics - Determination of bending properties) by the following method, and the electrode strength was evaluated according to the following criteria. The negative electrode (Φ16 mm) was set in the center of a jig with a support distance of 5 mm, and a load cell (rated load: 20 N) set in an autograph was lowered toward the electrode at a speed of 1 mm / min, and the yield stress was calculated from the yield point. The results are shown in Table 2. [Evaluation Criteria] 〇: Yield stress is 1kPa or more △: Yield stress is 0.8 kPa or more but less than 1 kPa ×: Yield stress is less than 0.8 kPa
[0067] [Measurement of direct current resistance (DCR)] At room temperature, using a charge / discharge measuring device [HJ0501SM8A] [manufactured by Hokuto Denko Corporation], the battery was charged at 1C up to 4.2C with CC-CV (cutoff current 0.01C) and then after one hour of rest, discharged to 2.5V at 0.1C. The voltage immediately before discharging was V0, the voltage 10 seconds after discharging was V1, and the current during discharging was I1, and (V1-V0) / I1 was calculated as the direct current resistance (DCR). The results are shown in Table 2.
[0068] [Cycle characteristic evaluation] At room temperature, the battery was charged at 0.1C up to 4.2C with CC-CV (cutoff current 0.01C) using a charge / discharge measuring device [HJ0501SM8A] [manufactured by Hokuto Denko Corporation], and after resting for 1 hour, it was discharged at 0.01C down to 2.5V. The discharge capacity at this time was defined as the initial capacity X0. After that, the charge / discharge was repeated to obtain the discharge capacity X1 at the 50th cycle. The X1 / X0 was defined as the 50 cycle discharge capacity retention rate, and the cycle characteristics were evaluated according to the following criteria. The results are shown in Table 2. [Evaluation Criteria] ◎: Discharge capacity retention rate is 93% or more ○: Discharge capacity retention rate is 89% or more but less than 93% ×: Discharge capacity retention rate is less than 89%
[0069] [Table 2]
[0070] The results in Table 2 show that the lithium ion electrode of the present invention produced using the lithium ion electrode binder of the present invention has sufficient electrode strength. Furthermore, it was found that the lithium ion battery equipped with the lithium ion electrode of the present invention had a low DCR and excellent cycle characteristics. In particular, the evaluation batteries (Y-2) and (Y-3) using the lithium ion electrode binders (X-2) and (X-3) according to Examples 2 and 3, in which 5-hexenoic acid or 10-undecenoic acid, which is an aliphatic vinyl carboxylic acid having 5 or more carbon atoms, was used as the vinyl carboxylic acid (a2) having 4 or more carbon atoms, had a particularly low DCR and excellent cycle characteristics. [Industrial Applicability]
[0071] The lithium ion electrode binder and the method for producing the lithium ion electrode binder of the present invention are particularly useful for producing lithium ion electrodes constituting lithium ion batteries used in mobile phones, personal computers, hybrid automobiles, electric automobiles, etc. The lithium ion electrode of the present invention is particularly useful as a lithium ion electrode for lithium ion batteries used in mobile phones, personal computers, hybrid automobiles, electric automobiles, etc. The lithium ion battery of the present invention is particularly useful as a lithium ion battery for mobile phones, personal computers, hybrid automobiles, and electric automobiles.
Claims
1. A binder (X) for a lithium ion electrode, comprising: a copolymer (A) of a (meth)acrylate (a1) and a vinyl carboxylic acid (a2) having 4 or more carbon atoms; and an ester (C) of a polyolefin macromonomer (B) having a hydroxyl group at least at one end, The weight average molecular weight of the polyolefin macromonomer (B) is 5,000 to 10,000; The binder for a lithium ion electrode, wherein the acid value of the ester (C) is 15 to 25 mgKOH / g.
2. 2. The binder for lithium ion electrodes according to claim 1, wherein the weight ratio of the structural unit derived from the polyolefin macromonomer (B) is 50 to 70% based on the weight of the ester (C).
3. A lithium ion electrode comprising the lithium ion electrode binder according to claim 1 or 2.
4. A lithium ion battery comprising the lithium ion electrode according to claim 3.
5. A method for producing a lithium ion electrode binder (X) comprising: (A) a copolymer of (meth)acrylate (a1) and (a2) a vinyl carboxylic acid having 4 or more carbon atoms; and (C) an ester of (B) a polyolefin macromonomer having a hydroxyl group at least at one end, the method comprising the steps of: a step of polymerizing the (meth)acrylate (a1) and the vinyl carboxylic acid (a2) having 4 or more carbon atoms in the presence of the polyolefin macromonomer (B) to obtain the copolymer (A), The polyolefin macromonomer (B) has a weight average molecular weight of 5,000 to 10,000, and the ester (C) has an acid value of 15 to 25 mgKOH / g.
Citation Information
Patent Citations
Binder composition for power storage device positive electrode, slurry for power storage device positive electrode, power storage device positive electrode, and power storage device
JP2016051678A
Binder for electrochemical cells, paste for electrochemical cells, and method for producing electrode for electrochemical cells
WO2015083358A1