Oxidation neutralization treatment method
By monitoring and adjusting conditions based on oxygen generation in the oxidative neutralization process, the method effectively reduces side reactions and minimizes agent consumption, addressing the inefficiencies in existing oxidative neutralization treatments.
Patent Information
- Application Number
- JP2023085089
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
In oxidative neutralization treatments using chlorine as an oxidizing agent for removing impurities from nickel chloride solutions, side reactions consume oxidizing and neutralizing agents, leading to increased costs due to drug loss, and there is a lack of methods to monitor and control these side reactions effectively.
Monitor the extent of side reactions by measuring oxygen and nitrogen concentrations in the reaction gas, estimate oxygen generation, and adjust conditions such as nickel concentration, chlorine gas flow, and temperature to reduce side reactions and minimize agent consumption.
Reduces the consumption of oxidizing and neutralizing agents by controlling side reactions, thereby lowering chemical costs and optimizing the oxidative neutralization process.
Smart Images

Figure 2024168415000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an oxidation neutralization method, and more particularly to a method for removing impurities contained in water to be treated, such as an aqueous solution of nickel chloride, by an oxidation neutralization method. [Background technology]
[0002] In the nickel hydrometallurgical process, nickel sulfide is leached with chlorine, impurities are removed from the resulting nickel chloride aqueous solution, and electrolytic nickel is recovered by electrowinning. The oxidation neutralization method is known as a method for removing impurities from nickel chloride aqueous solution. For example, Patent Document 1 describes the removal of impurities such as lead contained in nickel chloride aqueous solution by the oxidation neutralization method. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-171972 A Summary of the Invention [Problem to be solved by the invention]
[0004] When chlorine gas is blown into an aqueous solution of nickel chloride as an oxidizing agent and basic nickel carbonate is added as a neutralizing agent, nickel precipitates are produced by the following main reaction. At the same time, impurities such as lead and manganese contained in the aqueous solution of nickel chloride are precipitated as hydroxides or oxides. If these neutralized precipitates are removed by solid-liquid separation, a clear aqueous solution of nickel chloride is obtained. (Main reaction) 3NiCl2+Cl2+(4 / 3)Ni3(CO3)(OH)4·4H2O →Ni3O2(OH)4+4NiCl2+(4 / 3)CO2+6H2O
[0005] However, in the oxidation neutralization treatment using chlorine as an oxidizing agent, in addition to the above-mentioned main reaction, the following side reaction may also occur in which chlorine oxidizes water to generate hydrochloric acid and oxygen. (Side reactions) Cl2+H2O→2HCl+(1 / 2)O2
[0006] The side reaction consumes the oxidizing agent chlorine, and the hydrochloric acid produced by the side reaction consumes the neutralizing agent. In other words, some of the oxidizing agent and neutralizing agent do not contribute to the production of neutralized precipitate, resulting in a loss of chemicals. Therefore, the side reaction causes an increase in the consumption of the oxidizing agent and neutralizing agent, leading to an increase in chemical costs.
[0007] Therefore, it is conceivable to select operating conditions that suppress side reactions and reduce the consumption of oxidizing agents and neutralizing agents. To do so, it is necessary to monitor the extent to which side reactions are occurring, but a method for doing so is not known.
[0008] In view of the above circumstances, an object of the present invention is to provide an oxidation / neutralization treatment method that makes it possible to monitor the extent to which a side reaction occurs in which chlorine oxidizes water to generate hydrochloric acid and oxygen. [Means for solving the problem]
[0009] The oxidation neutralization treatment method of the first embodiment is characterized by comprising an oxidation neutralization process in which chlorine gas as an oxidizing agent is blown into impurity-containing water to be treated in a reaction tank, a neutralizing agent is added, and a neutralization precipitate containing the impurities is produced by an oxidation neutralization reaction; a measurement process in which the oxygen concentration and nitrogen concentration of the annular gas in the reaction tank are measured; and an oxygen generation amount estimation process in which the reaction-derived oxygen concentration is obtained by subtracting the atmospheric oxygen concentration obtained from the nitrogen concentration of the annular gas from the oxygen concentration of the annular gas, and the reaction-derived oxygen concentration is multiplied by the mass of the annular gas to obtain the amount of oxygen generated. The second aspect of the oxidation neutralization treatment method is characterized in that, in the first aspect, the neutralizing agent is a carbonate, and in the measurement process, the nitrogen concentration of the annular collected gas is determined from the oxygen concentration and carbon dioxide concentration of the annular collected gas. The oxidation neutralization treatment method of a third aspect is the method of the first or second aspect, further comprising an adjustment step of adjusting conditions for the oxidation neutralization step using the amount of oxygen generated as an index. The oxidation neutralization treatment method of a fourth aspect is the method of the third aspect, characterized in that the water to be treated is an aqueous nickel chloride solution, and the nickel concentration of the aqueous nickel chloride solution is adjusted in the adjusting step. The oxidation neutralization treatment method of a fifth aspect is the third or fourth aspect, characterized in that in the adjusting step, the blowing amount of the chlorine gas is adjusted. The oxidation neutralization treatment method of a sixth aspect is characterized in that in any one of the first to third and fifth aspects, the water to be treated is an aqueous nickel chloride solution. Effect of the Invention
[0010] According to the present invention, it is possible to monitor the degree to which the side reaction of chlorine oxidizing water to generate hydrochloric acid and oxygen occurs based on the amount of oxygen generated. In addition, by adjusting the conditions of the oxidation / neutralization step so as to reduce the amount of oxygen generated, it is possible to reduce the consumption of the oxidizing agent and neutralizing agent, thereby suppressing chemical costs. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is an overall flow diagram of a nickel hydrometallurgical process. [Diagram 2] FIG. 2 is a detailed process diagram of the lead removal process. [Diagram 3] FIG. [Figure 4] 1 is a graph showing the relationship between the nickel concentration in an aqueous crude nickel chloride solution and the amount of oxygen generated. [Diagram 5] 1 is a graph showing the relationship between the amount of chlorine and the amount of oxygen generated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, an embodiment of the present invention will be described with reference to the drawings. The oxidation neutralization treatment method according to one embodiment of the present invention is a method for removing impurities contained in water to be treated by oxidation neutralization.
[0013] The water to be treated is an aqueous solution containing impurities. Examples of the water to be treated include an aqueous nickel chloride solution and an aqueous cobalt chloride solution. Examples of impurities contained in the aqueous nickel chloride solution include iron, lead, manganese, and cobalt. Examples of impurities contained in the aqueous cobalt chloride solution include iron, lead, and manganese. The water to be treated is subjected to an oxidation neutralization treatment to remove impurities. However, impurities that cannot be completely removed may remain in the water to be treated after the treatment.
[0014] The oxidation neutralization treatment method of this embodiment is preferably applied to the de-iron step and the de-leading step, particularly the de-leading step, of the nickel hydrometallurgical smelting process described below. Therefore, the following description will be given taking the treatment of an aqueous nickel chloride solution in the de-leading step as an example. However, the oxidation neutralization treatment method of this embodiment is not limited to the de-leading step, and may be applied to any process step. Furthermore, the water to be treated is not limited to an aqueous nickel chloride solution.
[0015] As shown in Figure 1, in the nickel hydrometallurgy process, the raw material nickel sulfide is first treated in the leaching process to obtain leachate. Nickel matte and nickel-cobalt mixed sulfide can be used as nickel sulfide.
[0016] The leaching process includes a chlorine leaching process and a cementation process. In the chlorine leaching process, the metals contained in the solid matter in the raw slurry are substantially all leached into the liquid by the oxidizing power of the chlorine gas blown into the leaching tank. In the cementation process, the chlorine leaching solution is brought into contact with nickel sulfide, preferably nickel matte, to carry out a substitution reaction between copper and nickel. As a result, for example, nickel in the nickel matte is leached into the liquid, and copper ions in the liquid are precipitated in the form of copper sulfide or metallic copper. The leaching solution obtained in the leaching process is mainly composed of an aqueous nickel chloride solution, and contains impurities such as copper, iron, and lead in addition to cobalt.
[0017] In the iron removal process, impurities such as iron and arsenic are removed from the leachate (nickel chloride aqueous solution) by oxidation neutralization. In the iron removal process, an oxidizing agent is applied to the leachate to adjust the oxidation-reduction potential (based on Ag / AgCl electrode, the same applies below) to 400-1,100 mV, while a neutralizing agent is added to adjust the pH to 1.5-3. Chlorine gas, for example, is used as the oxidizing agent. Nickel carbonate, for example, is used as the neutralizing agent. Impurities such as iron and arsenic contained in the leachate are precipitated as hydroxides or oxides by the oxidation neutralization reaction. The precipitate is removed by solid-liquid separation to obtain a deironized final solution from which impurities have been removed.
[0018] In the solvent extraction step, the cobalt contained in the iron-removal final solution is separated by solvent extraction to obtain an aqueous nickel chloride solution and an aqueous cobalt chloride solution. Hereinafter, for the sake of convenience, the aqueous nickel chloride solution and the aqueous cobalt chloride solution obtained in the solvent extraction step are referred to as an aqueous crude nickel chloride solution and an aqueous crude cobalt chloride solution, respectively. The nickel concentration in the aqueous crude nickel chloride solution is 160 to 200 g / L. The aqueous crude nickel chloride solution contains impurities such as lead, manganese, cobalt, and zinc. The cobalt contained in the aqueous crude nickel chloride solution is extracted into an organic solvent and selectively separated from the nickel chloride in the aqueous crude nickel chloride solution, but a very small amount of cobalt still remains in the extraction residue (aqueous crude nickel chloride solution).
[0019] The crude cobalt chloride aqueous solution is purified in a purification process to remove impurities, and the resulting high-purity cobalt chloride aqueous solution is sent to the cobalt electrolysis process, where electrolytic cobalt is produced by electrowinning.
[0020] The crude nickel chloride aqueous solution is subjected to a deleading process to remove impurities, resulting in a high-purity nickel chloride aqueous solution. The deleading process will be described in detail later. After the deleading process, other solution purification treatments may be performed as necessary. For example, trace amounts of zinc remaining in the nickel chloride aqueous solution may be removed by adsorbing them onto an anion exchange resin. The high-purity nickel chloride aqueous solution is sent to a nickel electrolysis process. In the nickel electrolysis process, electrolytic nickel is produced by electrowinning.
[0021] As shown in Fig. 2, the deleading process has three sub-processes: a dilution process, an oxidation / neutralization process, and a solid-liquid separation process. In the following description, the term "crude nickel chloride aqueous solution" is used to mean not only the starting liquid of the deleading process, but also the water to be treated in the dilution process and the oxidation / neutralization process.
[0022] In the dilution step, the crude nickel chloride aqueous solution is diluted with a diluent to reduce the nickel concentration. For example, the crude nickel chloride aqueous solution (nickel concentration 160 to 200 g / L) obtained in the solvent extraction step is diluted so that the nickel concentration becomes 90 to 130 g / L. Since the main component of the crude nickel chloride aqueous solution is nickel chloride, the nickel concentration can be used as an index showing the chloride ion concentration of the crude nickel chloride aqueous solution.
[0023] If the nickel concentration of the crude nickel chloride aqueous solution is 130g / L or less, the chloride ion concentration is low, which makes the chloro complex unstable and makes it easier for impurities, especially cobalt, to precipitate in the oxidation neutralization process. Also, if the nickel concentration of the crude nickel chloride aqueous solution is 130g / L or less, the nucleus growth of the precipitate particles is promoted and the particle size increases, improving the filterability in the solid-liquid separation process. If the nickel concentration of the crude nickel chloride aqueous solution is 90g / L or more, the amount of diluent added can be reduced and a significant increase in the volume of the crude nickel chloride aqueous solution can be suppressed, making it unnecessary to increase the facility capacity.
[0024] It is preferable to use nickel electrolysis waste liquid as the diluent. Nickel electrolysis waste liquid is obtained as waste liquid after using a high-purity nickel chloride aqueous solution as an electrolyte in the nickel electrolysis process. By using nickel electrolysis waste liquid as a diluent, it is possible to prevent an increase in the total amount of liquid in the system of the hydrometallurgical process. Industrial water may be used as the diluent instead of nickel electrolysis waste liquid. If industrial water is used, the crude nickel chloride aqueous solution can be diluted to the target nickel concentration with a smaller amount of liquid than if nickel electrolysis waste liquid is used.
[0025] The diluted crude nickel chloride aqueous solution is sent to the oxidation neutralization step. In the oxidation neutralization step, an oxidizing agent is applied to the crude nickel chloride aqueous solution to adjust the redox potential to 600 to 1,200 mV, while a neutralizing agent is added to adjust the pH to 4 to 6. Impurities such as lead, manganese, and cobalt contained in the crude nickel chloride aqueous solution are coprecipitated with nickel precipitate by the oxidation neutralization reaction. Hereinafter, the nickel precipitate containing impurities is referred to as neutralized precipitate.
[0026] Chlorine gas is used as the oxidizing agent. Nickel carbonate, sodium carbonate, calcium carbonate, nickel hydroxide, sodium hydroxide, calcium hydroxide, etc. can be used as the neutralizing agent. Of these, nickel carbonate and nickel hydroxide do not increase the impurities in the nickel chloride aqueous solution, so they are preferably used for the oxidation neutralization treatment of the nickel chloride aqueous solution.
[0027] The slurry containing the neutralized precipitate is separated into a high-purity nickel chloride aqueous solution and the neutralized precipitate in the solid-liquid separation process. The main components of the neutralized precipitate are nickel hydroxide and oxide. Therefore, the neutralized precipitate is used as a raw material for nickel sulfate.
[0028] In the oxidation neutralization step, a reaction tank shown in FIG. 3 is used. A crude nickel chloride aqueous solution is continuously supplied to the reaction tank. The flow rate of the crude nickel chloride aqueous solution is, for example, 2,200 to 3,000 L / min. An oxidizing agent (chlorine gas) and a neutralizing agent are continuously supplied to the reaction tank. Chlorine gas is blown as an oxidizing agent into the water to be treated (crude nickel chloride aqueous solution) in the reaction tank, and a neutralizing agent is added to generate a neutralized precipitate by an oxidation neutralization reaction. The reaction tank is equipped with an agitator for stirring the crude nickel chloride aqueous solution, the oxidizing agent (chlorine gas), and the neutralizing agent. A slurry containing the neutralized precipitate is continuously discharged from the reaction tank.
[0029] In addition, a plurality of reaction tanks may be connected in series to carry out the oxidation neutralization treatment stepwise. In this case, the crude nickel chloride aqueous solution is continuously supplied to the most upstream reaction tank and flows in sequence to the downstream reaction tanks. The dilution step may be carried out in a concentration adjustment tank, or the dilution step and the oxidation neutralization step may be carried out in the same reaction tank. In the latter case, both the crude nickel chloride aqueous solution before dilution and the diluent may be supplied to the reaction tank. In this case, the dilution rate of the crude nickel chloride aqueous solution may be adjusted using the nickel concentration of the crude nickel chloride aqueous solution in the slurry continuously discharged from the reaction tank, or the nickel concentration of the crude nickel chloride aqueous solution before dilution and the nickel concentration of the diluent as an index.
[0030] Chlorine gas supplied as an oxidant is absorbed into the crude nickel chloride aqueous solution, and almost the entire amount contributes to the oxidation neutralization reaction. Nevertheless, to prevent chlorine gas, which is a toxic gas, from leaking outside the reaction tank, a circulating collection pipe is connected to the gas phase of the reaction tank, and the inside of the reaction tank is kept at negative pressure by an induced draft fan. The gas drawn by the induced draft fan (hereinafter referred to as "circulating collection gas") is sent to the detoxification tower through the circulating collection pipe. The circulating collection gas includes the gas generated in the reaction tank as well as the atmosphere (free air) that flows in through the gaps in the reaction tank.
[0031] When chlorine gas is blown into an aqueous solution of crude nickel chloride as an oxidizing agent and basic nickel carbonate is added as a neutralizing agent, nickel precipitate is produced by the following main reaction: At the same time, impurities such as lead and manganese contained in the aqueous solution of crude nickel chloride are precipitated as hydroxides or oxides. (Main reaction) 3NiCl2+Cl2+(4 / 3)Ni3(CO3)(OH)4·4H2O →Ni3O2(OH)4+4NiCl2+(4 / 3)CO2+6H2O
[0032] When a carbonate such as nickel carbonate, sodium carbonate, or calcium carbonate is used as a neutralizing agent, carbon dioxide is generated, which is discharged as reflux gas.
[0033] In addition to the main reaction, the oxidation neutralization treatment using chlorine as an oxidizing agent may also cause the following side reaction in which chlorine oxidizes water to generate hydrochloric acid and oxygen. The oxygen generated by the side reaction is discharged as reflux gas. (Side reactions) Cl2+H2O→2HCl+(1 / 2)O2
[0034] The side reaction consumes the oxidizing agent chlorine, and the hydrochloric acid produced by the side reaction consumes the neutralizing agent. In other words, some of the oxidizing agent and neutralizing agent do not contribute to the production of neutralized precipitate, resulting in a loss of chemicals. Therefore, the side reaction causes an increase in the consumption of the oxidizing agent and neutralizing agent, leading to an increase in chemical costs.
[0035] Therefore, it is conceivable to select operating conditions that suppress the side reactions and reduce the consumption of the oxidizing agent and neutralizing agent. To do this, it is necessary to monitor the extent to which the side reactions are occurring. However, it is difficult to directly measure the extent to which the side reactions are occurring. Therefore, in this embodiment, the extent to which the side reactions are occurring is monitored by the following measurement process and oxygen generation amount estimation process.
[0036] In the measurement step, the oxygen concentration and nitrogen concentration of the annular gas in the reaction tank are measured. A gas analyzer can be used for the concentration measurement. The oxygen concentration and nitrogen concentration of the annular gas may be directly measured by a gas analyzer or the like, or may be indirectly determined from the concentration of other components. For example, when a carbonate is used as a neutralizing agent, the annular gas also contains carbon dioxide generated by the main reaction. In this case, the oxygen concentration and carbon dioxide concentration of the annular gas may be directly measured by a gas analyzer, and the nitrogen concentration of the annular gas may be determined from these measured values. Assuming that the remainder of the oxygen and carbon dioxide contained in the annular gas is nitrogen, the nitrogen concentration may be determined by subtracting the oxygen concentration and carbon dioxide concentration from 100%.
[0037] It is known that the components of the atmosphere are 78.1% nitrogen, 20.9% oxygen, 0.9% argon, and 0.1% other trace components. The value obtained by subtracting the oxygen concentration and carbon dioxide concentration from 100% is, precisely, the total concentration of nitrogen, argon, and other trace components (excluding carbon dioxide).
[0038] Next, in the oxygen generation amount estimation process, the amount of oxygen generated by a side reaction (hereinafter referred to as the "oxygen generation amount") is calculated from the oxygen concentration and nitrogen concentration of the collected gas. Specifically, first, the oxygen concentration originating from the atmosphere (hereinafter referred to as the "atmospheric oxygen concentration") is calculated from the nitrogen concentration of the collected gas. Since nitrogen is not generated in the reaction tank, all of the nitrogen contained in the collected gas is originating from the atmosphere. In addition, the ratio of nitrogen and oxygen contained in the atmosphere is known. Therefore, the atmospheric oxygen concentration can be obtained by multiplying the nitrogen concentration of the collected gas by the ratio of nitrogen and oxygen in the atmosphere. The ratio by which the nitrogen concentration of the collected gas is multiplied is 0.268 (= 20.9% / 78.1%) when the nitrogen concentration is measured directly, and 0.264 (= 20.9% / 79.1%) when the nitrogen concentration is calculated by subtracting the oxygen concentration and carbon dioxide concentration from 100%.
[0039] Next, the oxygen concentration derived from the reaction (hereinafter referred to as "generated oxygen concentration") is calculated by subtracting the atmospheric oxygen concentration from the oxygen concentration in the collected gas. The generated oxygen concentration is then multiplied by the mass of the collected gas to calculate the amount of generated oxygen. As the mass of the collected gas, for example, the flow rate of the collected gas flowing through the collected gas pipe can be used.
[0040] For example, suppose the oxygen concentration in the collected gas is 16.9% and the carbon dioxide concentration is 34.7%. In this case, the nitrogen concentration (including argon, etc.) is calculated to be 48.4%. The atmospheric oxygen concentration is calculated to be 12.8% by multiplying the nitrogen concentration (including argon, etc.) of 48.4% by 0.264. Then, the generated oxygen concentration is calculated to be 4.1% by subtracting the atmospheric oxygen concentration of 12.8% from the oxygen concentration in the collected gas of 16.9%.
[0041] The amount of oxygen generated is the amount of oxygen generated by a side reaction. Therefore, the amount of oxygen generated is an index of the extent to which a side reaction is occurring. In other words, the amount of side reaction occurring can be monitored based on the amount of oxygen generated.
[0042] In addition, by adjusting the conditions of the oxidation / neutralization step using the amount of oxygen generated as an index, it is possible to suppress side reactions (adjustment step). For example, the conditions of the oxidation / neutralization step may be adjusted so that the amount of oxygen generated is equal to or less than a control value.
[0043] When the water to be treated is an aqueous nickel chloride solution, the occurrence of side reactions can be suppressed by adjusting the nickel concentration of the aqueous nickel chloride solution. The horizontal axis of the graph shown in Figure 4 is the nickel concentration of the aqueous crude nickel chloride solution in the deleading process, and the vertical axis is the amount of oxygen generated determined by the method described above. As can be seen from the graph in Figure 4, the higher the nickel concentration of the aqueous crude nickel chloride solution, the lower the amount of oxygen generated. It is known that the higher the nickel chloride concentration of the aqueous solution, the lower the water activity. It is presumed that when the nickel concentration of the aqueous crude nickel chloride solution is high, the water activity decreases and the equilibrium potential of the water oxidation reaction increases, suppressing the oxidation of water, i.e., the side reaction.
[0044] For example, when the amount of oxygen generated exceeds the control value, the nickel concentration of the aqueous solution of crude nickel chloride may be increased. The nickel concentration of the aqueous solution of crude nickel chloride may be adjusted by the amount of diluent added in the dilution step.
[0045] The side reaction can also be suppressed by adjusting the amount of chlorine gas blown into the reaction tank. The horizontal axis of the graph shown in FIG. 5 is the amount of chlorine (the value obtained by dividing the flow rate of chlorine gas into the reaction tank by the flow rate of the crude nickel chloride aqueous solution into the reaction tank), and the vertical axis is the amount of oxygen generated obtained by the above-mentioned method. As can be seen from the graph in FIG. 5, when the nickel concentration of the crude nickel chloride aqueous solution is low, particularly when it is 111 g / L or less, the smaller the amount of chlorine, the smaller the amount of oxygen generated. Therefore, for example, when the amount of oxygen generated exceeds the control value, the amount of chlorine gas blown into the reaction tank may be reduced. However, the amount of chlorine gas blown into the reaction tank affects the redox potential of the crude nickel chloride aqueous solution. It is preferable to adjust the amount of chlorine so that the redox potential of the crude nickel chloride aqueous solution is in a range suitable for oxidation neutralization treatment, 600 to 1,200 mV in the deleading process.
[0046] In addition, it is believed that side reactions can also be suppressed by adjusting the temperature of the water to be treated.
[0047] As described above, by adjusting the conditions of the oxidation / neutralization step so as to reduce the amount of oxygen generated, it is possible to suppress side reactions, which in turn reduces the consumption of the oxidizing agent and neutralizing agent, thereby reducing chemical costs.
Claims
1. an oxidation / neutralization step in which chlorine gas as an oxidizing agent is blown into the impurity-containing water to be treated in the reaction tank, and a neutralizing agent is added to generate a neutralized precipitate containing the impurities by an oxidation / neutralization reaction; a measuring step of measuring an oxygen concentration and a nitrogen concentration in the collected gas of the reaction tank; and an oxygen generation amount estimation step of determining a reaction-derived oxygen concentration by subtracting an atmospheric oxygen concentration calculated from the nitrogen concentration in the collected gas from the oxygen concentration in the collected gas, and determining an oxygen generation amount by multiplying the reaction-derived oxygen concentration by the mass amount of the collected gas. The oxidation and neutralization treatment method according to the present invention is characterized in that
2. The neutralizing agent is a carbonate, In the measuring step, the nitrogen concentration of the collected gas is determined from the oxygen concentration and the carbon dioxide concentration of the collected gas.
2. The method for oxidation and neutralization treatment according to claim 1.
3. The method further includes an adjustment step of adjusting the conditions of the oxidation / neutralization step using the amount of oxygen generated as an index.
2. The method for oxidation and neutralization treatment according to claim 1.
4. The water to be treated is an aqueous nickel chloride solution, In the adjusting step, the nickel concentration of the nickel chloride aqueous solution is adjusted.
4. The method for oxidation and neutralization treatment according to claim 3.
5. In the adjusting step, the amount of chlorine gas blown in is adjusted.
4. The method for oxidation and neutralization treatment according to claim 3.
6. The water to be treated is an aqueous solution of nickel chloride.
6. The method for oxidation and neutralization treatment according to claim 1, wherein the oxidation and neutralization treatment is carried out in a manner similar to that described above.
Citation Information
Patent Citations
Lead removal method for nickel chloride solution
CN114107697A
Preparation of alkali chlorate
JP1985046384A
Method for removing lead in chloride solution
JP1994306503A
Method for decomposing away ammonia nitrogen and apparatus for the same
JP2010099542A
Apparatus and method for producing perchlorate