Structure and processing device
A CFRP structure with ceramic moisture-proof layers addresses thermal expansion and rigidity issues in processing devices, enhancing accuracy and productivity by reducing vibrations and deformations.
Patent Information
- Application Number
- JP2023085437
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Existing processing devices face issues with thermal expansion, low rigidity, and weight, leading to decreased processing accuracy and productivity due to frame vibrations and thermal deformations.
A structure comprising a carbon fiber reinforced plastic (CFRP) main body with ceramic moisture-proof layers on both main surfaces and optional side surfaces, designed to minimize thermal expansion and enhance rigidity while reducing moisture absorption.
The structure achieves high processing accuracy, reduced weight, and improved productivity by minimizing thermal deformations and vibrations, allowing for faster and more precise operations.
Smart Images

Figure 2024168611000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a structure including carbon fibers and a processing device in which the structure is used. [Background technology]
[0002] Conventionally, various processing devices such as exposure devices and laser processing devices have been used. In many of these processing devices, a design is adopted in which components constituting the device are supported by a frame. For example, in the case of an exposure device, components such as a light emitting unit, a mask stage, a projection optical system, and a work stage are supported by a frame. In the case of a laser processing device, components such as a laser emitting unit and a work stage are supported by a frame. Examples of the work include a substrate.
[0003] In such a processing device, if the frame expands or shrinks due to thermal expansion caused by changes in the ambient temperature or heat generated by the device itself, the positions of the components supported by the frame may change, and the processing accuracy may decrease. Therefore, it is desirable to use a material with as low a thermal expansion coefficient as possible for the material of the processing device frame.
[0004] In addition, the frame of the processing equipment must also have high rigidity (elastic modulus). For example, consider the case where a work stage is supported by a frame. The work stage frequently repeats sequential movements, for example, in step-and-repeat, which divides and exposes areas of a board, or in drilling, which forms many through-holes in a board. For this reason, the time spent moving the stage is often longer than the time spent actually performing the exposure process.
[0005] Therefore, if the work stage is supported by a frame with low rigidity, the frame will vibrate significantly due to the incremental movement of the work stage, and the time it takes for the frame to stop vibrating, i.e., the time it takes to perform the next exposure or processing, will be long. As a result, the processing time for the work will be long, and the productivity of the device will decrease. Furthermore, if the frame has low rigidity, it will be vulnerable to external vibrations and will be prone to shaking. This can also cause the processing accuracy to deteriorate.
[0006] Another important condition for the frame components is that they have a low density so that even large equipment is relatively lightweight. In order to shorten the stage movement time and increase speed, the stage needs to be accelerated and decelerated at a high acceleration rate, but if the stage is heavy, there is a limit to how much it can be accelerated and decelerated. For this reason, it is desirable for the moving parts to be as light as possible. Another method is to use a large drive motor, but this increases the weight, and the floor of the factory where the equipment is installed must be reinforced, which increases the cost of the equipment.
[0007] Thus, it is desirable for the frame of the processing equipment to have characteristics such as high rigidity (elastic modulus) and low thermal expansion coefficient (coefficient of thermal expansion) and density. Note that the conditions of high rigidity and low density can also be said to be the conditions of high specific rigidity (rigidity / specific gravity).
[0008] The characteristics that satisfy these conditions are often effective not only for the frame, but also for the components that make up the processing equipment. For example, the work stage on which the substrate or the like is placed requires high flatness in order to perform high-precision positioning. Also, in order to perform high-precision positioning in a short time, it is required to be highly rigid and lightweight, i.e., to have a high specific rigidity. Furthermore, it is necessary that the dimensions do not deform due to temperature changes, and a small coefficient of thermal expansion is required. Of course, the characteristics that satisfy these conditions are often effective for components other than the work stage as well.
[0009] It has high rigidity, a small coefficient of thermal expansion, and a small density. An example of a material that satisfies these conditions is carbon fiber reinforced plastic (CFRP).
[0010] CFRP is a composite material made by reinforcing resin with carbon fiber. In terms of reinforced concrete, which is also made of composite materials, the resin corresponds to the concrete and the carbon fiber to the reinforcing bars. CFRP is made by impregnating carbon fiber with resin and making it into a plate-shaped (sheet-shaped) component called prepreg. Several sheets of this prepreg are stacked in a mold while taking into consideration the direction of the fibers, and then molded by heating and pressing them in an autoclave to harden them.
[0011] Thermosetting resins such as epoxy resins are often used for the matrix (base material). CFRP is lightweight and has high strength, so it is used in a variety of applications, including golf clubs, fishing rods, aircraft, and automobiles.
[0012] CFRP has the characteristic of absorbing moisture from the environment in which it is used, expanding and causing dimensional deformation. In addition, since the penetration and diffusion of moisture into CFRP proceeds slowly, the distribution of moisture concentration inside CFRP is non-uniform and the condition changes gradually. This causes problems such as deterioration of surface roughness and twisting deformation, which can lead to various complex deformations.
[0013] The following Patent Documents 1 and 2 describe measures to prevent moisture absorption by CFRP. Patent Document 1 describes a structure in which ceramic members are sandwiched and bonded to both sides of a CFRP member, in particular, the CFRP member being coated with an inorganic material such as metal or ceramic.
[0014] Patent Document 2 describes bonding aluminum or ceramics to the end faces of a CFRP-laminated member. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] JP 2009-248398 A [Patent Document 2] JP 2017-80899 A Summary of the Invention [Problem to be solved by the invention]
[0016] In exposure devices, laser processing devices, and the like, improving exposure accuracy and laser processing accuracy are important issues. Of course, improving processing accuracy is also important in other processing devices. As described above, in order to achieve high accuracy in processing devices, it is effective to improve the characteristics of the frame, components, and the like.
[0017] In view of the above circumstances, an object of the present invention is to provide a structure that exhibits effective characteristics in improving processing accuracy when used in the frame, components, etc. of a processing device, and a processing device in which said structure is used. [Means for solving the problem]
[0018] In order to achieve the above object, a structure according to one embodiment of the present invention includes a main body, a first moisture barrier layer, and a second moisture barrier layer. The main body is formed by stacking a plurality of sheet-like members whose main component is carbon fiber, and has a first main surface and a second main surface that face each other in the stacking direction of the plurality of sheet-like members. The first moisture proof layer is laminated on the first main surface, and at least a portion of a surface opposite to the side laminated on the first main surface is made of a ceramic material. The second moisture proof layer is laminated on the second main surface and is made of a material different from a ceramic material.
[0019] In this structure, a first moisture-proof layer, at least a part of whose surface is made of a ceramic material, is laminated on a first main surface of a main body constituted by laminating a plurality of sheet-like members whose main component is carbon fiber. In addition, a second moisture-proof layer, made of a material different from the ceramic material, is laminated on a second main surface of the main body. As a result, by applying this structure to the frame or components of a processing device, it is possible to exhibit characteristics that are effective in improving processing accuracy.
[0020] The first moisture proof layer may have an entire surface made of a ceramic material.
[0021] Each of the plurality of sheet-like members may be a prepreg made of carbon fiber impregnated with a resin, and in this case, the main body may be a carbon fiber reinforced plastic member formed by laminating the prepregs.
[0022] The first moisture proof layer may be made of low thermal expansion glass.
[0023] The first moisture-proof layer has a thermal expansion coefficient of −1×10 at temperatures of 20° C. to 130° C. in a direction parallel to the surface of the first moisture-proof layer that is laminated on the first main surface. -6 / ℃ greater than 1×10 -6 / °C.
[0024] The first moisture proof layer may include a low thermal expansion glass that constitutes the surface, and an intermediate member that is disposed between the low thermal expansion glass and the first main surface.
[0025] The intermediate member may be made of a metal foil.
[0026] The second moisture-proof layer may be made of any one of a metal foil, a rubber tape on which the metal foil is formed, and a resin film on which a moisture-proof coating is formed.
[0027] At least one of the first moisture barrier layer and the second moisture barrier layer may be joined to the main body portion via an adhesive that hardens at a low temperature or an adhesive layer that exerts adhesive strength at a low temperature.
[0028] The second moisture proof layer may be configured by adhering the metal foil to the second main surface with an adhesive that hardens at a low temperature.
[0029] The first moisture-proof layer may be made of a material that causes a thermal residual stress resulting from a step of bonding the first moisture-proof layer to the main body portion to be 6 MPa or less.
[0030] The thermal expansion coefficient of the first moisture-proof layer in a direction parallel to the surface of the first main surface at temperatures of 20° C. to 130° C. is −1×10 -6 / ℃ greater than 1×10 -6 / °C.
[0031] The difference in thermal expansion coefficient between the first moisture-proof layer and the main body is 1×10 -6 / °C.
[0032] The first moisture proof layer may be laminated on the entire surface of the first main surface, and in this case, the second moisture proof layer may be laminated on the entire surface of the second main surface.
[0033] The first moisture proof layer may be configured such that the surface made of a ceramic material serves as a processing surface that is to be processed.
[0034] The surface to be machined may be a surface to be machined into a flat surface.
[0035] The body may have a side surface between the first main surface and the second main surface. In this case, the structure may further include a third moisture barrier layer laminated on the side surface.
[0036] The third moisture-proof layer may be made of any one of a metal foil, a metal sheet, and a rubber tape having the metal foil formed thereon.
[0037] The third moisture proof layer may be bonded to the side surface via an adhesive that hardens at a low temperature or an adhesive layer that exerts adhesive strength at a low temperature.
[0038] The third moisture-proof layer may be configured by adhering the metal foil or the metal sheet to the side surface with an adhesive that hardens at a low temperature.
[0039] A structure according to another aspect of the present invention includes a main body, a first moisture barrier layer, a second moisture barrier layer, and a third moisture barrier layer. The main body portion is formed by stacking a plurality of sheet-like members whose main component is carbon fiber, and has a first main surface and a second main surface that face each other in the stacking direction of the plurality of sheet-like members, and a side surface between the first main surface and the second main surface. The first moisture barrier layer is laminated on the first main surface. The second moisture barrier layer is laminated onto the second main surface. The third moisture barrier layer is laminated to the side surface. At least one of the first moisture barrier layer and the second moisture barrier layer is made of a material other than a ceramic material.
[0040] In this structure, a first moisture-proof layer is laminated on a first main surface of a main body formed by laminating a plurality of sheet-like members whose main component is carbon fiber, and a second moisture-proof layer is laminated on a second main surface. In addition, a third moisture-proof layer is laminated on a side surface of the main body. At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material. This makes it possible to exert properties that are effective in improving processing accuracy by applying it to the frame or components of a processing device.
[0041] A structure according to another aspect of the present invention includes a main body, a first moisture barrier layer, and a second moisture barrier layer. The main body is made up of a plurality of sheet-like members whose main component is carbon fiber, and has a first main surface and a second main surface opposed to each other. The first moisture proof layer is laminated on the first main surface, and at least a portion of a surface opposite to the side laminated on the first main surface is made of a ceramic material. The second moisture proof layer is laminated on the second main surface and is made of a material different from a ceramic material. The configuration of this structure can also exert properties that are effective in improving processing accuracy by applying it to the frame or components of a processing device.
[0042] A structure according to another aspect of the present invention includes a main body, a first moisture barrier layer, a second moisture barrier layer, and a third moisture barrier layer. The main body portion is composed of a plurality of sheet-like members whose main component is carbon fiber, and has a first main surface and a second main surface facing each other, and a side surface between the first main surface and the second main surface. The first moisture barrier layer is laminated on the first main surface. The second moisture barrier layer is laminated onto the second main surface. The third moisture barrier layer is laminated to the side surface. At least one of the first moisture barrier layer and the second moisture barrier layer is made of a material other than a ceramic material. The configuration of this structure can also exert properties that are effective in improving processing accuracy by applying it to the frame or components of a processing device.
[0043] A method for manufacturing a structure according to one embodiment of the present invention includes the following steps. A lamination process in which multiple sheet-like members whose main component is carbon fiber are laminated. A bonding process for bonding the plurality of sheet-like members to each other: a first moisture-proof layer laminated on a first main surface, which is one main surface in the stacking direction of the plurality of sheet-like members; and a second moisture-proof layer laminated on a second main surface opposite the first main surface. At least a part of the surface of the first moisture-proof layer opposite to the side laminated on the first main surface is made of a ceramic material, and the second moisture-proof layer is made of a material different from the ceramic material.
[0044] The joining process may include a process of integrally joining the multiple sheet-like members, the first moisture-proof layer, and the second moisture-proof layer by heat-pressing, or a process of joining each of the first moisture-proof layer and the second moisture-proof layer to a main body portion in which the multiple sheet-like members are joined to each other by heat-pressing.
[0045] A method for manufacturing a structure according to another aspect of the present invention includes the following steps. A lamination process in which multiple sheet-like members whose main component is carbon fiber are laminated. a first joining step for joining together the plurality of sheet-like members, a first moisture-proof layer laminated on a first main surface which is one main surface in the stacking direction of the plurality of sheet-like members, and a second moisture-proof layer laminated on a second main surface opposite the first main surface. a second bonding step of bonding a third moisture-proof layer to a side surface between the first main surface and the second main surface of the plurality of sheet-like members; At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material.
[0046] A method for manufacturing a structure according to another aspect of the present invention includes the following steps. A molding process for forming a main body portion having a first main surface and the second main surface from a plurality of sheet-like members whose main component is carbon fiber. a first bonding step of bonding a first moisture proof layer to the first main surface; A second bonding step of bonding a second moisture proof layer to the second main surface. At least a part of the surface of the first moisture-proof layer opposite to the side laminated on the first main surface is made of a ceramic material, and the second moisture-proof layer is made of a material different from the ceramic material.
[0047] A method for manufacturing a structure according to another aspect of the present invention includes the following steps. A molding process for molding a main body having a first main surface, a second main surface, and a side surface between the first main surface and the second main surface, using a plurality of sheet-like members whose main component is carbon fiber. a first bonding step of bonding a first moisture proof layer to the first main surface; A second bonding step of bonding a second moisture proof layer to the second main surface. a third bonding step of bonding a third moisture proof layer to the third main surface; At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material.
[0048] A processing device according to one embodiment of the present invention is a processing device for processing a workpiece, and is configured using the structure described above.
[0049] The structure may be used as a work stage that holds the workpiece.
[0050] The processing apparatus may be configured as an exposure apparatus. Effect of the Invention
[0051] As described above, according to the present invention, it is possible to provide a structure that exhibits characteristics effective for improving processing accuracy by adopting it for the frame or components of a processing device, a manufacturing method for the structure, and a processing device using the structure. Note that the effects described here are not necessarily limited, and may be any of the effects described in this disclosure. [Brief description of the drawings]
[0052] [Figure 1] FIG. 1 is a schematic diagram showing an example of a basic configuration of a structure according to a first embodiment (side view). [Diagram 2] FIG. 1 is a schematic diagram (perspective view) showing a basic configuration example of a structure according to a first embodiment. [Diagram 3]FIG. 1 is a schematic diagram (exploded perspective view) showing a basic configuration example of a structure according to a first embodiment. [Figure 4] 1 is a graph showing the results of an accelerated moisture absorption test verifying the presence or absence of a moisture proof layer on the first and second principal surfaces of a CFRP member and the change over time in the amount of change in moisture absorption expansion strain. [Diagram 5] 1 is a graph showing the change over time in the amount of change in moisture expansion strain in Examples 1 to 8. [Figure 6] 1 is a table showing the moisture expansion strain and reference ratio in Examples 1 to 8. [Figure 7] FIG. 11 is a schematic view (perspective view) showing a basic configuration example of a structure according to a second embodiment. [Figure 8] 1 is a graph showing the change over time in the amount of change in moisture absorption expansion strain in Examples 9 to 20. [Figure 9] 1 is a table showing the moisture expansion strain and reference ratio in Examples 9 to 20. [Figure 10] 1 is a graph showing the change over time in the rate of weight increase of each sample due to immersion in water. [Figure 11] FIG. 1 is a schematic diagram showing a schematic configuration of an exposure apparatus which is an example of a processing apparatus. [Figure 12] 1 is a schematic diagram showing a schematic configuration of a laser processing device which is an example of a processing device; [Figure 13] 11A and 11B are schematic diagrams illustrating an example of the configuration of a structure according to another embodiment. [Figure 14] FIG. 11 is a schematic diagram showing an example of the configuration of a CFRP member according to another embodiment. [Figure 15] FIG. 15 is a schematic diagram showing an internal structure of the CFRP member shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0053] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0054] <First embodiment> 1 to 3 are schematic diagrams showing a basic configuration example of a structure according to a first embodiment of the present invention. Fig. 1 is a side view of the structure 1 as viewed from the side. Fig. 2 is a perspective view of the structure 1 as viewed obliquely. Fig. 3 is an exploded perspective view showing components of the structure 1 in an exploded state.
[0055] In this embodiment, the structure 1 is a CFRP structure including carbon fiber reinforced plastic (CFRP).
[0056] In the following, for ease of understanding, the left-right direction, front-rear direction, and up-down direction are defined for the sake of convenience with respect to the structure 1. Specifically, the X direction in the drawing is the left-right direction (the positive side of the X axis is the right side, and the negative side is the left side), the Y direction in the drawing is the front-rear direction (the positive side of the Y axis is the rear side, and the negative side is the front side), and the Z direction in the drawing is the up-down direction (the positive side of the Z axis is the upper side, and the negative side is the lower side).
[0057] Of course, the application of this technology is not limited to the direction in which the structure 1 is arranged, nor is it limited to which part of the structure 1 is the front part and which part is the side part.
[0058] The exploded perspective view shown in Fig. 3 is a diagram created to facilitate understanding of the configuration of the structure 1. It does not necessarily mean that the structure 1 has a configuration in which each component can be clearly disassembled as shown in Fig. 3 (although of course such a configuration is also included).
[0059] As shown in FIGS. 1 to 3, a structure 1 has a CFRP member 2, a first moisture-proof layer 3, and a second moisture-proof layer 4.
[0060] The CFRP member 2 is formed by laminating a plurality of prepregs 5. The prepregs 5 are sheet-like members whose main component is carbon fiber. Specifically, the prepregs 5 are sheet-like members in which carbon fibers are impregnated with resin while maintaining fiber directionality.
[0061] In this embodiment, a plurality of prepregs 5 are stacked in the vertical direction (Z direction) and integrated by heat and pressure bonding. Specifically, the CFRP member 2 is formed by heating to about 120°C to 130°C under reduced pressure and hardening by pressure (pressure bonding).
[0062] 1 to 3, the vertical direction (Z direction) is the stacking direction of the multiple prepregs 5. In other words, Fig. 1 to Fig. 3 can be said to be drawings in which the stacking direction of the multiple prepregs 5 is defined as the vertical direction (Z direction) with respect to the structure 1.
[0063] The matrix resin constituting the prepreg 5 is, for example, a thermosetting epoxy resin. In addition, other thermosetting resins such as unsaturated polyester, vinyl ester, phenol, cyanate ester, polyimide, etc. may also be used as the matrix resin.
[0064] The CFRP member 2 is a high-strength material while having a lower density (i.e., lighter) than metal materials such as iron and aluminum. It is also possible to use standard CFRP plates (for example, 5 mm UD (Uni-Directional) material) of standard dimensions (standard dimensions) that can be stocked inexpensively as multiple sheet-like members mainly composed of carbon fiber.
[0065] In the structure 1 according to this embodiment, it is also possible to integrally mold the first moisture barrier layer 3 and the second moisture barrier layer 4 when molding the CFRP member 2. Of course, it is also possible to join the first moisture barrier layer 3 and the second moisture barrier layer 4 to the molded CFRP member 2. In other words, in application of the present technology, any method can be adopted as a method for joining the first moisture barrier layer 3 and the second moisture barrier layer 4 to the CFRP member 2.
[0066] The method of integrally molding the first moisture barrier layer 3 and the second moisture barrier layer 4 when molding the CFRP member 2 is advantageous in shortening the time and reducing the cost required to manufacture the structure 1. On the other hand, when the first moisture barrier layer 3 and the second moisture barrier layer 4 are adhesively bonded to the molded CFRP member 2, the thermal residual stress can be reduced, which is advantageous in reducing the risk of deformation due to the relaxation of the thermal residual stress over the long term. Thermal residual stress will be explained in detail later.
[0067] As shown in Fig. 3, the CFRP member 2 has an approximate outer shape of a rectangular parallelepiped. The CFRP member 2 has a first main surface 6 and a second main surface 7 that face each other in the stacking direction of the multiple prepregs 5, i.e., the vertical direction (Z direction). In this embodiment, the upper surface of the CFRP member 2 on the upper side serves as the first main surface 6, and the lower surface of the CFRP member 2 on the lower side serves as the second main surface 7. This is not limiting, and the present technology can also be implemented with the lower surface of the CFRP member 2 as the first main surface and the upper surface as the second main surface.
[0068] In addition, the CFRP member 2 has side surfaces 8 between the first main surface 6 and the second main surface 7. In this embodiment, the side surfaces 8 include four surfaces: a left side surface 8a, a right side surface 8b, a front side surface 8c, and a rear side surface 8d.
[0069] Both the first principal surface 6 and the second principal surface 7 of the CFRP member 2 are also called flatwise surfaces of the CFRP member 2. In addition, the side surface 8 of the CFRP member 2 is also called edgewise surfaces of the CFRP member 2.
[0070] In this embodiment, the CFRP member 2 corresponds to one embodiment of a main body portion according to the present invention.
[0071] The first moisture barrier layer 3 is laminated on the first main surface 6 of the CFRP member 2. As shown in Figs. 1 to 3, the first moisture barrier layer 3 is laminated on the entire surface of the first main surface 6. Furthermore, at least a part of a surface 9 of the first moisture barrier layer 3 opposite to the side to be laminated on the first main surface 6 is made of a ceramic material. In this embodiment, the surface 9 corresponds to the upper surface of the upper side of the first moisture barrier layer 3. Furthermore, in this embodiment, the entire surface 9 of the first moisture barrier layer 3 is made of a ceramic material.
[0072] The second moisture-proof layer 4 is laminated on the second main surface 7. As shown in Fig. 1 to Fig. 3, the second moisture-proof layer 4 is laminated on the entire second main surface 7. In addition, the second moisture-proof layer 4 is made of a material different from the ceramic material.
[0073] A method for manufacturing the structure 1 of this embodiment may include a method (including integral molding) of joining a CFRP member 2 having a desired size in terms of left-right width (size in the left-right direction) and front-to-back width (size in the front-to-back direction) when viewed from above to a moisture barrier layer (first moisture barrier layer 3 / second moisture barrier layer 4).
[0074] Without being limited to this, one example is a method in which the CFRP member 2 and the moisture barrier layer (first moisture barrier layer 3 / second moisture barrier layer 4) are joined (including integral molding) in a state in which the left-right width and top-bottom width when viewed from above are larger than the desired size, and then cutting is performed so that the left-right width and top-bottom width are the desired size.
[0075] The CFRP is molded in a state in which the left-right width and the up-down width when viewed from above are larger than the desired size. The CFRP member 2 is then produced by cutting out the left-right width and the up-down width to the desired size. The first moisture barrier layer 3 and the second moisture barrier layer 4 are bonded to the first main surface 6 and the second main surface 7 of the produced CFRP member 2. Such a method can also be adopted.
[0076] In the following description, the process of cutting out the desired left-right and up-down widths may be omitted. That is, the structure 1 will be described mainly in terms of the mode in which the CFRP members 2 (plurality of prepregs 5) whose left-right and up-down widths are aligned to the desired sizes, the first moisture barrier layer 3, and the second moisture barrier layer 4 are bonded to each other.
[0077] Of course, the various technical matters described below can be implemented in appropriate combination with the process of cutting out the CFRP member 2 so that the left-right width and the top-bottom width are the desired sizes. For example, the content of the following description of creating a CFRP member 2 by heat-pressing a plurality of prepregs 5 can be applied not only to a state in which the left-right width and the front-back width are uniform to the desired sizes, but also to a state in which the left-right width and the front-back width are larger than the desired sizes.
[0078] In addition, in the following explanation, the content of manufacturing the structure 1 by integral molding by heat-pressing multiple prepregs 5 and moisture-proof layers (first moisture-proof layer 3 / second moisture-proof layer 4) can be applied not only to a state in which the left-right width and front-to-back width are uniform to the desired size, but also to a state in which the left-right width and front-to-back width are larger than the desired size.
[0079] Of course, if integral molding or joining of parts is performed when the left-right width and front-to-back width are larger than the desired size, a cutting process can be performed at an appropriate time thereafter so that the left-right width and top-to-bottom width are the desired size.
[0080] [CFRP components] The CFRP member 2 is integrally molded by applying pressure and heating to harden a plurality of prepregs 5. Examples of prepregs 5 include pitch-based prepregs that are characterized by high elasticity and high vibration damping, and PAN-based prepregs that are characterized by high strength.
[0081] The pitch-based CF (Carbon Fiber) that constitutes the pitch-based prepreg has a high elastic modulus. Therefore, even if the matrix resin expands due to heat, the change can be suppressed, making it possible to reduce the thermal expansion coefficient (linear expansion coefficient). In addition, even if the matrix resin (e.g., epoxy resin) tries to expand due to moisture absorption, the pitch-based CF can suppress the change.
[0082] Therefore, the pitch-based prepreg can be made smaller in terms of moisture-absorption expansion (deformation) than the PAN-based prepreg. Whether the cause of the expansion (deformation) is thermal expansion or moisture-absorption expansion, the basic behavior (expansion mode) is the same. Furthermore, in the application of the present invention, the pitch-based prepreg has a great advantage in terms of its high vibration damping properties.
[0083] [Moisture-proof layer] The first moisture barrier layer 3 and the second moisture barrier layer 4 have moisture barrier performance for suppressing moisture absorption (adsorption of moisture) of the CFRP member 2. The moisture barrier performance can be evaluated using, for example, the water vapor transmission rate (WVTR).
[0084] In this embodiment, the moisture-proof performance of the first moisture-proof layer 3 and the second moisture-proof layer 4 is such that the water vapor transmission rate at 40° C. and 90% RH is 1.0 g / (m 2 ·day) or less. The water vapor permeability is 1×10 -1 g / (m 2 The moisture-proof performance of the first moisture-proof layer 3 and the second moisture-proof layer 4 is preferably 1×10 -2 g / (m 2 It is preferable that the moisture-proof performance is less than or equal to 1.0 m / s. The lower the water vapor transmission rate, the higher the moisture-proof performance.
[0085] [First moisture-proof layer] The first moisture proof layer 3 having a surface 9 made of a ceramic material can be realized, for example, by laminating a ceramic member made of a ceramic material on the first main surface 6 of the CFRP member 2.
[0086] As the ceramic member, for example, low thermal expansion glass can be used. Low thermal expansion glass is glass with a small linear expansion coefficient, and includes crystallized glass, synthetic quartz glass, borosilicate glass, and the like. Among these, crystallized glass is glass that has both crystallinity and transparency, and for example, heat-resistant crystallized glass "Neoceram" manufactured by Nippon Electric Glass Co., Ltd. (NEG) can be used. Of course, ceramic members other than low thermal expansion glass may also be used.
[0087] In this disclosure, "low thermal expansion glass" refers to a glass having a thermal expansion coefficient (linear expansion coefficient) of ±1×10 at temperatures of 20°C to 130°C in a direction parallel to the joining surface. -6 This refers to glass that satisfies the following criteria: / °C. Note that the " / °C" notation may be omitted in some cases.
[0088] The coefficient of thermal expansion (CTE) is the rate of change in the length and volume of an object caused by an increase in temperature, expressed as the rate of change per 1K (1℃). For example, it can be measured and evaluated using a method that uses optical interference in accordance with JISR3251 (1995). It can also be evaluated by measuring the displacement of the surface or inside the CFRP using a strain gauge.
[0089] When measuring the thermal expansion coefficients of the CFRP member 2 (multiple prepregs 5), the first moisture barrier layer 3, and the second moisture barrier layer 4, it is preferable to measure them before joining with other members. In this case, the thermal expansion coefficients of each member are measured in a direction parallel to a surface that can become a joining surface. Of course, this is not limited to this. In this embodiment, the directions parallel to the joining surfaces are the left-right direction (X direction) and the front-back direction (Y direction).
[0090] Furthermore, for a non-isotropic member such as the CFRP member 2, the thermal expansion coefficient at 20°C to 130°C in a direction parallel to the joint surface may not be uniform in the thickness direction of the member when viewed microscopically. In this case, the average value of the thermal expansion coefficients measured as different values in the thickness direction can be used as the thermal expansion coefficient parallel to the joint surface of the member, and the present technology can be applied.
[0091] In the following description, when indicating the coefficient of thermal expansion, the condition "at a temperature of 20° C. to 130° C. in a direction parallel to the joining surfaces" may be omitted.
[0092] The first moisture-proof layer 3 may be configured to include a ceramic member disposed on the front surface 9 and an intermediate member disposed between the ceramic member and the first main surface 6. The ceramic member may be, for example, low-thermal expansion glass. The intermediate member may be, for example, a metal foil containing metal as a main component. For example, a metal foil made of copper (Cu), aluminum (Al), titanium (Ti), stainless steel (SUS), Super Invar, or the like may be used.
[0093] In this way, a moisture-proof layer having a multi-layer structure made of low thermal expansion glass and metal foil can be used as the first moisture-proof layer 3. By disposing the low thermal expansion glass on the surface 9 side, the first moisture-proof layer 3 having the surface 9 made of a ceramic member is realized. Of course, a ceramic member other than low thermal expansion glass may be used. Furthermore, a member other than metal foil may be used as the intermediate member. Furthermore, the intermediate member itself may be formed of a multi-layer structure.
[0094] [Second moisture barrier layer] Any member having moisture-proof properties and a configuration other than that of a ceramic material can be used as the second moisture-proof layer 4. That is, the second moisture-proof layer 4 can be realized by laminating a member having moisture-proof properties and a configuration other than that of a ceramic material on the second main surface 7 of the CFRP member 2.
[0095] For example, as the second moisture-proof layer 4, it is possible to use a metal foil, a rubber tape on which a metal foil is formed (laminated), or a resin film on which a moisture-proof film is formed.
[0096] The metal foil may be made of, for example, copper (Cu), aluminum (Al), titanium (Ti), stainless steel (SUS), super invar, etc. The rubber tape on which the metal foil is formed may be, for example, a butyl tape with an Al foil.
[0097] As the resin film on which the moisture-proof coating is formed, for example, a high-barrier film in which a moisture-proof coating of alumina, silica, etc. is coated on a PET (polyethylene terephthalate) film, etc. by PVD, CVD, etc. can be used. The resin film on which the moisture-proof coating is formed can also be called a moisture-proof coating film.
[0098] When using a resin film with a moisture-proof membrane formed thereon as the second moisture-proof layer 4, it is effective to laminate it so that the moisture-proof membrane side faces the CFRP member 2. This is because it is possible to eliminate the influence of water vapor transmission through the base film itself, such as PET, and because the base film acts as a protective layer, improvements in performance and reliability can be expected.
[0099] In particular, metal foil does not transmit water vapor, so the water vapor transmission rate is zero, making it possible to demonstrate extremely high moisture-proofing performance.
[0100] [Method of manufacturing structure 1] As a method for manufacturing the structure 1, a manufacturing method including the following steps can be adopted. A lamination process in which a plurality of sheet-like members (a plurality of prepregs 5) whose main component is carbon fiber are laminated. A bonding process for bonding together a plurality of sheet-like members, a first moisture-proof layer 3 laminated on a first main surface 6, which is one main surface in the stacking direction of the plurality of sheet-like members, and a second moisture-proof layer 4 laminated on a second main surface 7 opposite the first main surface 6. As described above, the first moisture-proof layer 3 is made of a ceramic material on at least a part of the surface 9 (in this embodiment, the entire surface 9) opposite to the side laminated on the first main surface 6. The second moisture-proof layer 4 is made of a material different from the ceramic material.
[0101] [Method of joining the first moisture-proof layer 3 and the second moisture-proof layer 4] In the joining step, any method can be adopted as a method for joining the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) to the CFRP member 2. For example, as a method for joining the moisture barrier layers, a method can be adopted in which the moisture barrier layers are directly and integrally molded when the CFRP member 2 is molded (hereinafter, this may be referred to as an integral molding method).
[0102] As a method for joining the moisture-proof layer, a method of bonding the moisture-proof layer to the molded CFRP member 2 using an adhesive can also be adopted (hereinafter, this may be referred to as an adhesive bonding method).
[0103] As a method for joining the moisture-proof layer, it is also possible to adopt a method in which an adhesive tape such as double-sided tape with excellent moisture-proof performance is used to bond the moisture-proof layer together (hereinafter, this may be referred to as the tape bonding method).
[0104] Furthermore, when a rubber tape or the like on which a metal foil is formed is used as the moisture-proof layer, an adhesive layer is formed on the moisture-proof layer, and this adhesive layer bonds the moisture-proof layer to the CFRP component 2. In this way, a method in which the moisture-proof layer is bonded to the CFRP component 2 by an adhesive layer in the moisture-proof layer can also be employed (hereinafter, this may be referred to as an adhesive layer bonding method).
[0105] It is also possible to employ a method that combines the integral molding method and the adhesive lamination method by using a sheet-like adhesive. For example, a plurality of prepregs 5 are laminated, and moisture-proof layers (first moisture-proof layer 3 / second moisture-proof layer 4) are placed on both end faces in the lamination direction (faces that will become the first main face 6 and second main face 7 of the CFRP member 2) with a sheet-like adhesive sandwiched between them. Then, when the CFRP member 2 is molded, the moisture-proof layers are integrally bonded (hereinafter, this bonding method may be referred to as an adhesive integral molding method).
[0106] Note that sheet-like adhesives are available in thermoplastic and thermosetting types, and a type (model) that can adhere at the curing temperature (e.g., 120°C to 130°C) during molding of the CFRP member 2 is selected. This makes it possible to bond the moisture-proof layer to the CFRP member 2 by sandwiching the sheet-like adhesive between the moisture-proof layer and the prepreg 5 and laminating and curing it.
[0107] For example, as a sheet-like adhesive, it is possible to use a thermoplastic adhesive film, so-called a hot melt adhesive film (sheet). When the film is heated, it melts and generates adhesive force, and when it is returned to room temperature, it hardens again and maintains a stable adhesive force. Film-like adhesives with a constant thickness are available, and they are easy to work with and can easily suppress unevenness in thickness within the surface. In addition, since there are many types, it is possible to select an appropriate type and grade depending on the material to be bonded and the heating and bonding temperature. For example, olefin-based and polyester-based hot melt adhesives have good heat resistance and thermal stability, and are therefore one of the suitable materials for manufacturing the structure 1 according to the present technology.
[0108] In addition, a thermosetting adhesive film can be used as a sheet-like adhesive, and epoxy-based thermosetting resin adhesive films also exist. When epoxy resin is used as the matrix resin, the prepreg 5 and the film are made of the same material, so the properties, including the thermal expansion coefficient, are similar and the affinity is high, which is effective. In addition, a thermosetting resin adhesive film provides stable adhesive strength even at relatively high temperatures, which is advantageous in terms of long-term reliability.
[0109] Furthermore, because it is in film form, it is as easy to work with as a thermoplastic adhesive film, and by appropriately selecting the type and grade, it is also possible to mold prepreg laminates, adhesive films, and various moisture-proof layers in the same process.
[0110] The adhesive integral molding method using a sheet-like adhesive can improve the adhesive strength between the prepreg 5 and the moisture-proof layer compared to the integral molding method. On the other hand, the integral molding method not using a sheet-like adhesive can reduce the cost of parts.
[0111] In addition, in each of the adhesive bonding method, tape bonding method, adhesive layer bonding method, and adhesive integral molding method, the state (bonding mode) after bonding of the moisture proof layer to the CFRP component 2 does not necessarily have clearly different characteristics. Depending on the materials and configurations of the adhesive, tape, and adhesive layer, the states after bonding may be very similar.
[0112] The above-mentioned integral molding method and adhesive integral molding method correspond to an embodiment of a process of integrally bonding a plurality of sheet-like members, a first moisture barrier layer, and a second moisture barrier layer by heat and pressure bonding according to the present invention. The adhesive bonding method, tape bonding method, and adhesive layer bonding method correspond to an embodiment of a process of bonding each of the first moisture barrier layer and the second moisture barrier layer to a main body portion formed by bonding a plurality of sheet-like members to each other by heat and pressure bonding according to the present invention.
[0113] [Specific examples of integral molding methods] A specific example of the integral molding method will be described. First, a plurality of prepregs 5 are prepared. The prepregs 5 are laminated, and low thermal expansion glass that will become the first moisture proof layer 3 is laminated on the upper surfaces in the lamination direction (the surface that will become the first main surface 6 of the CFRP member 2). In addition, metal foil is laminated on the lower surfaces of the plurality of prepregs 5 (the surface that will become the second main surface 7 of the CFRP member 2).
[0114] The laminate, which is made by stacking the metal foil, the prepregs 5, and the low-thermal expansion glass in that order, is sandwiched between two bagging films in the vertical direction (Z direction), and the edges of the two bagging films are sealed with sealing tape, so that the laminate is contained in a sealed space.
[0115] The inside of the sealed space is depressurized by drawing a vacuum, and then pressurized by the external atmospheric pressure, and the temperature is raised to 120°C to 130°C over 1 to 2 hours. This causes the prepreg 5 to harden, while bonding the low thermal expansion glass to the first main surface 6 and bonding the metal foil to the second main surface 7.
[0116] Hereinafter, the method of housing the structure in a sealed space, depressurizing the inside and pressurizing it with atmospheric pressure will be referred to as “bagging adsorption pressurization.” Note that conditions such as temperature and time can be set appropriately.
[0117] After the bagging and pressure application, in order to improve the degree of hardening and eliminate distortion during molding, a post-bake (PB) is performed at a higher temperature (for example, 145°C) for 2 hours. Note that this PB process is not essential.
[0118] By such heat and pressure bonding, it is possible to manufacture the structure 1 by integral molding. In addition to the above-mentioned bagging adsorption and pressure method, it is of course possible to use the autoclave method in which the temperature is raised and cured under pressure. When the autoclave method is adopted, the cost is expensive in terms of equipment, etc., but stable production is possible.
[0119] When a metal foil is used as the second moisture-proof layer 4, a protective layer can be formed to prevent oxidation and dirt on the surface of the metal foil opposite to the joint surface with the CFRP member 2, and to prevent the generation of wear powder. As the protective layer, for example, a plastic film such as PET, PEN (polyethylene naphthalate), or PI (polyimide) can be used. Nickel plating or tin plating can also be used as the protective layer.
[0120] [Thermal residual stress on CFRP member 2] For example, when the CFRP member 2 and the moisture barrier layer (first moisture barrier layer 3 / second moisture barrier layer 4) are integrally molded by the above-mentioned integral molding method, the interface between the CFRP member 2 and the moisture barrier layer is in a stress-free state at a temperature of, for example, 120°C to 130°C. When the structure 1 is subsequently returned to room temperature (usage temperature), high thermal residual stress is applied between the CFRP member 2 and the moisture barrier layer, causing deformation such as warping. Furthermore, if the thermal residual stress is gradually alleviated over a long period of time at the usage temperature, there is a risk that the deformation of the structure 1 will gradually progress.
[0121] There is concern that long-term changes and deformations will be a major problem in achieving a high-precision CFRP structure 1. Therefore, in order to achieve a high-precision structure 1, it is important to reduce the thermal residual stress caused by the process of joining the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) to the CFRP member 2. This also applies when a joining method other than the integral molding method is adopted.
[0122] In addition, when the matrix resin of the CFRP member 2 itself is an epoxy resin, for example, the stress relaxation is not zero, but it is possible to reduce the effect by using a highly elastic CF.
[0123] The thermal residual stress can be evaluated, for example, by multiplying the difference in the thermal expansion coefficients of both components by the temperature difference (the temperature difference ΔT from the stress-free temperature to the usage temperature). When using the value obtained by such a calculation, it is effective to construct the moisture barrier layer from a material that causes a thermal residual stress resulting from the process of bonding the moisture barrier layer to the CFRP component 2 of 6 MPa or less.
[0124] Furthermore, the following two measures can be cited as effective measures for reducing thermal residual stress.
[0125] (1) The moisture-proof layers (first moisture-proof layer 3 / second moisture-proof layer 4) are made of a material whose thermal expansion coefficient differs little from that of the CFRP member 2. (2) The process of bonding the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) to the CFRP member 2 is performed at a low temperature (for example, at the usage temperature such as room temperature or at a temperature close to the usage temperature). This reduces the temperature difference ΔT.
[0126] Regarding countermeasure (1), for example, the thermal expansion coefficient of pitch-based prepreg cross-ply laminates (CP (Cross-Ply) material) and quasi-isotropic plates (QI (Quasi-Isotropic) material) is -5×10 -7 On the other hand, low thermal expansion glass, especially "Neoceram", has a thermal expansion coefficient of -2×10 over a wide temperature range above room temperature. -7 Since the two materials have roughly the same thermal expansion coefficient in the temperature range of the CFRP hardening and molding process, it is possible to greatly reduce the thermal residual stress between the two materials.
[0127] For example, the first moisture-proof layer 3 has a thermal expansion coefficient of −1×10 at temperatures of 20° C. to 130° C. in a direction parallel to the surface on the side laminated to the first main surface 6. -6 / ℃ greater than 1×10 -6 / °C. This makes it possible to maintain small differences in the thermal expansion coefficient during the molding process from when the CFRP hardens at high temperatures until it is returned to room temperature, thereby suppressing thermal residual stress.
[0128] More specifically, the thermal expansion coefficient of the first moisture-proof layer 3 in a direction parallel to the surface on the side laminated to the first main surface 6 at temperatures of 20° C. to 130° C. is −1×10 -6 / ℃ greater than 1×10 -7 / ° C. This further reduces the difference in thermal expansion coefficient, making it possible to further suppress thermal residual stress.
[0129] The thermal expansion coefficient of NEG's "Neoceram" in the direction parallel to the surface laminated on the first main surface 6 at temperatures between 20°C and 130°C is -1×10 -6 / ℃ greater than 1×10 -7This corresponds to low thermal expansion glass having a thermal expansion coefficient in the range smaller than 1 / °C.
[0130] Of course, even when a ceramic material other than low thermal expansion glass is used, the thermal expansion coefficient at temperatures of 20°C to 130°C in a direction parallel to the surface laminated on the first main surface 6 of the first moisture-proof layer 3 is set to be less than -1×10 -6 / ℃ greater than 1×10 -6 / °C, it is possible to suppress thermal residual stress. In particular, the thermal expansion coefficient of the first moisture-proof layer 3 at temperatures of 20°C to 130°C in a direction parallel to the surface laminated on the first main surface 6 is in the range of -1×10 -6 / ℃ greater than 1×10 -7 / °C, it is possible to further suppress the thermal residual stress.
[0131] The difference in thermal expansion coefficient between the first moisture-proof layer 3 and the CFRP member 2 is 1×10 -6 The ceramic material should be made of a material with a thermal expansion coefficient smaller than 1 / ℃ (such as low thermal expansion glass). This makes it possible to suppress thermal residual stress.
[0132] For example, a pitch-based CFRP structure in which pitch-based prepregs are laminated and integrated is adopted as the CFRP member 2. The first moisture-proof layer 3 is made of a material such as "Neoceram" manufactured by NEG, which has a thermal expansion coefficient of -1×10 at temperatures of 20° C. to 130° C. in a direction parallel to the surface laminated on the first main surface 6. -6 / ℃ greater than 1×10 -7 / ° C. is bonded to the first main surface 6 of the CFRP member 2.
[0133] The difference in thermal expansion coefficient between such low thermal expansion glass and the CFRP member 2 having a pitch-based CFRP structure is 1×10 -6 / ° C. Furthermore, the thermal residual stress caused by the step of bonding the first moisture proof layer 3 to the CFRP member 2 is 6 MPa or less, and the effect of suppressing the thermal residual stress is extremely high.
[0134] Furthermore, when a material with a very small thickness (size in the vertical direction (Z direction)) such as metal foil is used as the moisture barrier layer, the metal foil itself undergoes elastic and plastic deformation, making it possible to design the residual stress on the CFRP member 2 to be significantly small. Therefore, even if a multilayer structure of a ceramic member (low thermal expansion glass) and metal foil is adopted as the first moisture barrier layer 3, the suppression of thermal residual stress is maintained.
[0135] For example, the first moisture-proof layer 3 may be a material such as "Neoceram" manufactured by NEG, which has a thermal expansion coefficient of -1×10 -6 / ℃ greater than 1×10 -7 A multi-layer structure of low thermal expansion glass, the range of which is smaller than 100 / °C, and metal foil is adopted. A pitch-based CFRP configuration is adopted as the CFRP member 2. In this case, metal foil is disposed between the CFRP member 2 having the pitch-based CFRP configuration and the low thermal expansion glass. As a result, it is possible to shift the thermal expansion coefficient of the CFRP member 2 to the positive side, and it is possible to further reduce the difference in thermal expansion coefficient with the low thermal expansion glass. It is expected that the effect of reducing the difference in thermal expansion coefficient can be improved by appropriately adjusting the thickness of the metal foil.
[0136] The second moisture barrier layer 4 is also made of a material with a small difference in thermal expansion coefficient from the CFRP member 2. This makes it possible to reduce the thermal residual stress applied to the CFRP member 2. It is also effective to use a metal foil as the second moisture barrier layer 4, which can suppress the thermal residual stress by elastic deformation and plastic deformation.
[0137] In addition, a rubber tape with a metal foil formed thereon, such as an Al foil-attached butyl tape, is used as the second moisture-proof layer. The adhesive layer of the rubber tape is made of rubber such as butyl rubber and has a small elastic modulus, so it is possible to further reduce the thermal residual stress. In addition, the thermal residual stress can also be suppressed by using a resin film with a moisture-proof film such as a high-barrier film formed thereon as the second moisture-proof layer 4.
[0138] Even when an adhesive lamination method is used in which a moisture-proof layer is bonded to the CFRP component 2 via an adhesive, if there is a difference in the thermal expansion coefficient between the two components, thermal residual stress will occur due to the difference in the amount of shrinkage when returned to the operating temperature.
[0139] Furthermore, the state of this thermal residual stress changes over time. Adhesives are typically resins, and therefore have viscoelastic properties, and creep deformation occurs over time if stress remains applied. Therefore, the change (deformation) in the direction of relieving the thermal residual stress progresses very slowly.
[0140] Regarding countermeasure (2), the moisture-proof layer (first moisture-proof layer 3 / second moisture-proof layer 4) is bonded to the CFRP member 2 via an adhesive that hardens at low temperatures (low-temperature adhesive) or an adhesive layer that exerts adhesive strength at low temperatures. This makes it possible to reduce the temperature difference ΔT and suppress thermal residual stress.
[0141] In the adhesive lamination method, by using a low-temperature adhesive, it is possible to reduce the temperature difference ΔT, and it is possible to suppress thermal residual stress. Also, in the tape lamination method and the adhesive layer bonding method, by forming an adhesive layer that hardens at a low temperature, it is possible to reduce the temperature difference ΔT, and it is possible to suppress thermal residual stress.
[0142] In this disclosure, "low temperature" refers to a range of temperatures equal to or lower than the higher of room temperature (the temperature at which the structure 1 is used) and 70° C. Typically, temperatures equal to or lower than 70° C. are considered to fall under the "low temperature" in this disclosure.
[0143] Epoxy resin (epoxy adhesive) can be used as a low-temperature adhesive. In addition to the two-liquid mixture type that uses a hardener that can initiate a hardening reaction with the epoxy base at low temperatures, it is also possible to use a "latent hardener" that initiates hardening when triggered by an external stimulus such as heat or light.
[0144] As a stimulus trigger for hardening low-temperature adhesives, there are methods (types) that use light, pressure, etc., in addition to heat. For example, there are types that decompose when exposed to light to generate cations, and types that undergo structural changes when exposed to light to generate anions. There is also a method in which the hardener is microencapsulated and dispersed in the epoxy resin. These methods can initiate and progress the reaction between the epoxy base agent and the hardener without using heat, making it possible to harden at low temperatures.
[0145] Of course, countermeasure (2) can also be achieved by appropriately using a tape or film that has an adhesive layer (a layer made of adhesive) that uses a "latent hardener," making it possible to suppress thermal residual stress.
[0146] The effect of suppressing thermal residual stress is also achieved when only one of the first moisture barrier layer 3 and the second moisture barrier layer 4 is joined via an adhesive that hardens at low temperatures or an adhesive layer that exerts its adhesive strength at low temperatures.
[0147] The following method can also be used to bond the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) to the CFRP member 2. First, metal foil is bonded to each of the first main surface 6 and the second main surface 7. Then, thermal expansion glass is bonded to the metal foil bonded to the first main surface 6 via an adhesive or the like. In this configuration, the first moisture barrier layer 3 has a multi-layer structure of metal foil and low thermal expansion glass.
[0148] By first laminating metal foil on the first main surface 6 and the second main surface 7, a moisture-proof function for the first main surface 6 and the second main surface 7 is realized. Therefore, there is a high degree of freedom in the selection of materials for the adhesive used when laminating low thermal expansion glass on the metal foil in the next process. For example, a low-temperature adhesive can be used. It is also possible to use an adhesive that does not have high rigidity. It is also possible to use a material that functions as a stress relaxation layer. Furthermore, there is a high degree of freedom in the selection of the thickness of the adhesive, etc.
[0149] In other words, even if there is a difference in thermal expansion coefficient between the multiple prepregs 5 and the low-thermal expansion glass, the adhesive that bonds the metal foil and the low-thermal expansion glass can provide a stress relief function. As a result, it is possible to sufficiently prevent deformation such as warping from occurring at the top and bottom of the completed structure 1.
[0150] [Study on improving the properties of CFRP structures] The inventors have conducted extensive research into CFRP structures that can exhibit characteristics that are effective in improving the processing accuracy of processing equipment, and in particular, have conducted extensive research into CFRP structures that can be applied to components that require high flatness accuracy, such as suction plates on which workpieces are placed in work stages of exposure equipment and the like.
[0151] For example, suppose an adsorption plate or the like is constructed using a single CFRP member 2. In this case, it is difficult to process the first main surface 6 and the second main surface 7 of the CFRP member 2 with high precision, and high flatness precision cannot be ensured (hereinafter, this may be referred to as a flatness problem). Furthermore, with the CFRP member 2 alone, problems arise such as deformation due to expansion caused by moisture absorption and changes in shape over time (hereinafter, this may be referred to as a moisture absorption deformation problem).
[0152] Fig. 4 is a graph showing the results of an accelerated moisture absorption test verifying the presence or absence of a moisture-proof layer on the first principal surface 6 and the second principal surface 7 of the CFRP member 2, and the change over time in the amount of change in moisture absorption expansion strain. The horizontal axis of Fig. 4 is the elapsed time (Hr), and the vertical axis is the amount of change in moisture absorption expansion strain (με). Furthermore, "both sides" in Fig. 4 correspond to the first principal surface 6 and the second principal surface 7, which are the flatwise surfaces of the CFRP member 2. Note that the change in strain was measured by placing a strain gauge in the center layer during CFRP laminate molding and embedding it inside by hardening molding.
[0153] Fig. 4 shows the change over time in moisture absorption expansion strain for a reference sample, which is a CFRP member 2 alone that does not have a moisture barrier layer formed on either the first main surface 6 or the second main surface 7. Fig. 4 also shows a graph of a sample in which glass is bonded as a moisture barrier layer to the entire surface of either the first main surface 6 or the second main surface 7 of the CFRP member 2. Fig. 4 also shows a graph of a sample in which low thermal expansion glass is bonded to the first main surface 6 of the CFRP member 2 and Al foil is bonded to the second main surface 7 (corresponding to an embodiment of this structure 1).
[0154] As shown in Figure 4, it was confirmed that the reference sample (without a moisture-proof layer) had a very large moisture absorption expansion in the accelerated moisture absorption test. It was also confirmed that the sample in which a glass layer was integrally formed on one of the flatwise faces of the CFRP member 2 had a large moisture absorption expansion in the accelerated moisture absorption test.
[0155] On the other hand, it was confirmed that a sample in which low thermal expansion glass was laminated on the first main surface 6 of the CFRP member 2 and Al foil was laminated on the second main surface 7 hardly expanded due to moisture absorption. In other words, it was found that for the moisture absorption of the CFRP member 2, it is very important to use a moisture proof layer on both flatwise surfaces, i.e., on both the first main surface 6 and the second main surface 7.
[0156] In the structure 1 according to this embodiment shown in Figures 1 to 3, a first moisture barrier layer 3 is laminated on a first main surface 6 of a CFRP member 2, and a second moisture barrier layer 4 is laminated on a second main surface 7. This provides a very effective configuration against the problem of deformation due to moisture absorption.
[0157] Furthermore, in the structure 1 according to this embodiment, a first moisture proof layer 3 having a surface 9 made of a ceramic material is laminated on the first main surface 6 of the CFRP member 2. This allows highly accurate processing of the surface 9 made of a ceramic material, making it possible to achieve high flatness accuracy. In other words, the structure 1 according to this embodiment has a configuration that is extremely effective in dealing with flatness issues.
[0158] The layer made of a ceramic material on the surface 9 side of the first moisture-proof layer 3 can also be considered as a processing-sacrificial layer. When the first moisture-proof layer 3 is made of low-thermal expansion glass, the entire first moisture-proof layer 3 can be considered as a processing-sacrificial layer.
[0159] In addition, in the structure 1 according to this embodiment, a second moisture proof layer 4 made of a material other than the ceramic material is laminated on the second main surface 7 of the CFRP member 2. This is extremely advantageous in reducing the weight of the structure 1.
[0160] For example, suppose that moisture-proof layers made of a ceramic material (e.g., low-thermal expansion glass) are laminated on both the first main surface 6 and the second main surface 7 of the CFRP member 2. In this case, taking into account the density and thickness of the ceramic material, the weight increases considerably, greatly compromising the benefit of reducing the weight of the CFRP structure 1.
[0161] For example, the second moisture-proof layer 4 may have a density of 2.5 g / cm 3 When low thermal expansion glass with a thickness of 3 mm and a size of 600 mm square is used, the weight increases by about 2.7 kg. In contrast, when a glass with a density of 2.7 g / cm is used as the second moisture-proof layer 4, 3 When an aluminum foil with a thickness of 20 μm and a size of 600 mm square is used, the weight will be 19 g, which is approximately 1 / 140 of the weight.
[0162] The first moisture-proof layer 3, which is the target of planar processing, needs to function both as a processing sacrificial layer and as a moisture-proof layer. On the other hand, the second moisture-proof layer 4, which is bonded to the opposite second main surface 7, only needs to function as a moisture-proof layer. Therefore, the second moisture-proof layer 4 is made of a material that can reduce weight, such as a very thin metal foil. Note that grinding is the main method for processing ceramic materials thin, which increases processing costs. To begin with, ceramic materials themselves are expensive materials, and material costs are also an issue.
[0163] The present inventors have devised a new configuration for a structure 1, as exemplified in Figures 1 to 3. This configuration makes it possible to realize a structure 1 that can exhibit characteristics effective in improving the processing accuracy of a processing device.
[0164] When the structure 1 according to the present technology is applied to a work stage (adsorption plate), high-precision positioning can be achieved due to high flatness accuracy. In addition, high-precision positioning can be performed in a short time. In addition, dimensional deformation due to temperature change and moisture absorption can be sufficiently suppressed.
[0165] For example, in the case of an apparatus that performs high-precision exposure by frequently moving the stage position, such as a step-and-repeat exposure apparatus (division projection exposure apparatus), there are significant benefits to applying the structure 1 of the present technology to a work stage (adsorption plate).
[0166] This structure 1 can be made lightweight while retaining high rigidity and high dimensional stability, making it possible to shorten the time it takes to move the stage. This is because, according to the relationship F=ma, the smaller the mass m, the higher the acceleration a that can be obtained with the same driving force F. Being able to accelerate and decelerate at high acceleration shortens the time required to move a given distance, making it possible to shorten the tact time of the device.
[0167] Furthermore, when moving with the same acceleration a, a smaller driving force F is required, making it possible to use a smaller driving motor and making the entire device smaller and lighter. It is also possible to reduce the reaction force, making it possible to reduce vibrations in the entire device.
[0168] It is also possible to achieve high vibration damping characteristics, so that even if the device accelerates or decelerates at high acceleration, the vibrations converge in a short time, allowing the device to proceed to the exposure process. Usually, the settling time required for the vibrations to converge accounts for a large proportion of the overall takt time. Therefore, by shortening the settling time, it is possible to significantly improve the processing speed performance of the exposure device.
[0169] Of course, the present structure 1 can be applied to a work stage or the like of other processing devices such as laser processing devices, without being limited to exposure devices. Also, the present structure 1 can be applied to components other than the work stage, or to a frame supporting the components.
[0170] In particular, the present structure 1 can be configured such that the first moisture barrier layer 3 has a surface 9 made of a ceramic material that serves as a processing target surface. Therefore, the present structure 1 is effective for components or frames that have a surface to be processed.
[0171] In an example where the present structure 1 is applied to a work stage (adsorption surface), the surface 9 of the first moisture-proof layer 3 is configured as a surface to be processed into a flat surface. Of course, this is not limited to this, and the surface 9 of the first moisture-proof layer 3 may be configured as a surface to be processed for various other processes, such as processes to form a surface of a predetermined shape such as a tapered surface, or a concave / convex portion, etc.
[0172] [Evaluation of each example] The inventors have created a number of examples of the configuration and manufacturing method of the structure 1 according to the present technology, and evaluated the moisture-proof performance by an accelerated moisture absorption test, which will be described in detail below.
[0173] (Reference sample) For CFRP member 2 used as the reference sample, a mirror symmetrical 8-ply structure made of PAN-based CP material was adopted. In practice, pitch-based prepregs with a high elastic modulus are often used, but in order to make it easier to measure changes in moisture absorption and expansion, PAN-based prepregs, which have a lower elastic modulus than pitch-based prepregs, were used for the evaluation. Note that when epoxy resin is used as the matrix resin, both pitch-based and PAN-based prepregs show similar moisture-proofing properties, so the evaluation results are the same.
[0174] When creating the CFRP member 2 of the reference sample, curing molding was performed at 120°C for 2 hours, which is the recommended curing condition for PAN-based prepreg (curing under bagging adsorption pressure). After that, PB was performed at 145°C for 2 hours.
[0175] (Moisture absorption test conditions) The evaluation was carried out at high temperatures and high humidity of 80°C and 95% or higher relative humidity. In terms of the water vapor diffusion coefficient, a temperature of 80°C is an accelerated condition that is approximately 32 times faster than a room temperature of 20°C. Since the moisture absorption of the CFRP member 2 increases in proportion to the difference between the internal moisture concentration and the relative humidity of the environment, a moisture absorption test at a relative humidity of 95% can be said to be a stricter accelerated condition compared to an evaluation in a normal environment (for example, a relative humidity of 50%).
[0176] (Evaluation and measurement method) The strain gauge was placed in the center of the central layer of the prepreg laminate and molded as a single unit. After the prepreg was cured and PB was performed, the strain change was measured based on the strain level at the point where the constant conditions of 80°C and 95% relative humidity were reached.
[0177] FIG. 5 is a graph showing the change over time in the amount of change in moisture expansion strain in each of the examples described below. FIG. 6 is a table showing the moisture absorption expansion strain and the reference ratio in each example at the time when the moisture absorption expansion of the reference sample was saturated after 60 hours.
[0178] Example 1 First moisture-proof layer (low thermal expansion glass integrally molded) / Second moisture-proof layer (Aluminum foil integrally molded) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: Aluminum foil (thickness 20 μm) The laminate is made of low thermal expansion glass, 8 layers of PAN-based prepreg CP arrangement, and aluminum foil, and then molded into a single piece by heating and pressing using bagging adsorption pressure. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 1 was 0.8 με, which was suppressed to 0.9% compared to the reference.
[0179] Example 2 First moisture-proof layer (integrally molded low-thermal expansion glass) / Second moisture-proof layer (integrally molded electrolytic copper foil) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: copper foil (thickness 20 μm) The laminate is made of low thermal expansion glass, 8 layers of PAN-based prepreg CP arrangement, and copper foil, and then molded into a single piece by heat and pressure bonding using bagging suction pressure. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 2 was 0.8 με, which was suppressed to 0.9% compared to the reference.
[0180] Example 3 First moisture-proof layer (low thermal expansion glass integrally molded) / Second moisture-proof layer (electrolytic copper foil bonded with low-temperature adhesive) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: copper foil (thickness 20 μm) Low thermal expansion glass / PAN-based prepreg CP arrangement 8 layers are laminated and molded into one piece by heat compression bonding using bagging adsorption pressure. After carrying out PB, copper foil is laminated to the second main surface 7 of the roughened CFRP member 2 using a low-temperature adhesive. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 3 was 4.5 με, which was suppressed to 4.8% compared to the reference.
[0181] In all of the structures 1 of Examples 1 to 3, the second moisture proof layer 4 was made of a thin (small thickness) metal foil, and it was possible to sufficiently suppress the thermal residual stress in the CFRP member 2.
[0182] Example 4 First moisture-proof layer (low thermal expansion glass integrally molded with adhesive film) / Second moisture-proof layer (Aluminum foil integrally molded) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: Aluminum foil (thickness 20 μm) The laminate is made up of low thermal expansion glass / adhesive film / 8 layers of PAN-based prepreg CP arrangement / Aluminum foil, and is molded into a single piece by heat and pressure bonding using bagging adsorption pressure. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 4 was 1.5 με, which was suppressed to 1.6% compared to the reference.
[0183] Example 5 First moisture-proof layer (low thermal expansion glass bonded with low-temperature adhesive) / Second moisture-proof layer (integrally molded aluminum foil) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: Aluminum foil (thickness 20 μm) Laminated in a configuration of 8 layers of PAN-based prepreg CP arrangement / Al foil, and molded into a single piece by heat compression bonding using bagging adsorption pressure. After carrying out PB, low thermal expansion glass is bonded to the first main surface 6 of the CFRP component 2 using a low-temperature adhesive. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 5 was 3.5 με, which was suppressed to 3.7% compared to the reference.
[0184] Example 6 First moisture-proof layer (multi-layer structure of low thermal expansion glass and copper foil) / Second moisture-proof layer (copper foil integrally molded) First moisture-proof layer: NEG's "Neoceram" (thickness 3 mm) / copper foil (thickness 20 μm) Second moisture-proof layer: copper foil (thickness 20 μm) Copper foil / PAN-based prepreg CP arrangement 8 layers / copper foil are laminated, and molded into one piece by heat pressing with bagging suction pressure. After carrying out PB, low-thermal expansion glass is bonded to the copper foil formed on the first main surface 6 of the CFRP member 2 using a low-temperature adhesive. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 6 was 2.5 με, which was suppressed to 2.7% compared to the reference.
[0185] In Example 6, copper foil is first bonded to both flatwise surfaces (first main surface 6 and second main surface 7) of the CFRP member 2 by integral molding. For example, with the basic configuration in which copper foil is bonded to both surfaces, when a surface to be processed is required, low thermal expansion glass is bonded to the copper foil bonded to the first main surface 6. By employing such a manufacturing method, it is possible to improve the workability in manufacturing the structure 1 and to increase efficiency.
[0186] Example 7 First moisture-proof layer (low thermal expansion glass integrally molded) / Second moisture-proof layer (resin film with moisture-proof coating formed integrally) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: High barrier film (multi-layer moisture-proof layer laminated on film using CVD) (Thickness 38μm) The structure is low thermal expansion glass / 8 layers of PAN-based prepreg CP arrangement / high barrier film, and then molded into a single piece by heat pressing using bagging adsorption pressure, followed by PB. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 7 was 3.7 με, which was suppressed to 3.9% compared to the reference.
[0187] In Example 7, the high barrier film is based on a resin film such as a PET film, so that the elastic modulus is low, and even if laminated, almost no thermal residual stress is applied to the CFRP member 2. In addition, the barrier layer formed by CVD is SiO X Thin films such as SiON are often used, which have excellent flexibility and a multi-layer structure that provides high water vapor barrier properties.
[0188] Also usable is a barrier film having a barrier layer of alumina or the like formed by PVD (sputtering). As mentioned above, when a resin film having a moisture-proof film formed thereon is used as the second moisture-proof layer 4, the water vapor permeability is preferably 1×10 -1 g / (m 2 ·day) or less, so-called high barrier properties are desirable.-2 g / (m 2 Moisture-proof performance of less than 1.5 sq. days is preferable.
[0189] Example 8 First moisture-proof layer (low thermal expansion glass integrally molded) / Second moisture-proof layer (rubber tape with metal foil attached) First moisture-proof layer: NEG's "Neoceram" (thickness 3mm) Second moisture-proof layer: Butyl tape with aluminum foil (thickness of aluminum foil is 7 μm) The low thermal expansion glass / PAN-based prepreg is laminated in a CP arrangement of 8 layers, and then molded into a single piece by heat pressing using bagging adsorption pressure, followed by PB. After 60 hours, when the moisture absorption expansion of the reference sample was saturated, the moisture absorption expansion strain of Structure 1 of Example 8 was 5.5 με, which was suppressed to 5.9% compared to the reference. In Example 8, the metal foil is very thin and the thick rubber layer functions as a buffer material, making it possible to keep the thermal residual stress very small.
[0190] Thus, each Example exhibited high moisture-proofing performance, and it was possible to greatly reduce moisture-absorption expansion. If the Examples are listed in order of high moisture-proofing performance, i.e., low moisture-absorption expansion, the order is (Example 1), (Example 2), (Example 4), (Example 6), (Example 5), (Example 7), (Example 3), and (Example 8).
[0191] As shown in Figures 5 and 6, when the CFRP member 2, the first moisture barrier layer 3, and the second moisture barrier layer 4 were all integrally molded, the moisture barrier performance was slightly higher than when the first moisture barrier layer 3 and the second moisture barrier layer 4 were bonded to the molded CFRP member 2 using an adhesive or the like. However, the difference was very small, and considering measurement errors, it is thought that there is no significant difference. It is also thought that the moisture barrier performance can be further improved by devising the bonding conditions.
[0192] As described above, in the structure 1 according to this embodiment, a first moisture barrier layer 3 having at least a part of a surface 9 (in this embodiment, the entire surface 9) made of a ceramic material is laminated on a first main surface 6 of a CFRP member 2 formed by laminating a plurality of prepregs 5 whose main component is carbon fiber. In addition, a second moisture barrier layer 4 made of a material different from the ceramic material is laminated on a second main surface 7 of the CFRP member 2. As a result, by applying this structure 1 to the frame or components of a processing device, it becomes possible to exhibit characteristics that are effective in improving processing accuracy.
[0193] By implementing this technology, it is possible to realize a structure 1 that exhibits less dimensional deformation due to changes in humidity than CFRP alone, is more rigid than metal, has a low density and high specific rigidity, and is capable of achieving surface precision.
[0194] <Second embodiment> A structure according to a second embodiment of the present invention will be described below. In the following description, the description of the same configurations and functions as those of the structure 1 described in the above embodiment will be omitted or simplified.
[0195] [Forming a moisture-proof layer on the sides] Fig. 7 is a schematic diagram showing a basic configuration example of a structure according to the second embodiment. In the structure 12 according to this embodiment, a moisture-proof layer is further laminated on the side surfaces 8 (left side surface 8a, right side surface 8b, front side surface 8c, rear side surface 8d) which are edgewise surfaces of the CFRP member 2. Please also refer to Figs. 1 to 3 for illustrations of each part such as the side surface 8 (left side surface 8a, right side surface 8b, front side surface 8c, rear side surface 8d).
[0196] Hereinafter, the moisture-proof layer laminated on the side surface 8 will be referred to as the third moisture-proof layer 13. In the structure 12 shown in Fig. 7, the third moisture-proof layer 13a (not shown) is laminated on the entire surface of the left side surface 8a, and the third moisture-proof layer 13b is laminated on the entire surface of the right side surface 8b. In the structure 12, the third moisture-proof layer 13c is laminated on the entire surface of the front side surface 8c, and the third moisture-proof layer 13d (not shown) is laminated on the entire surface of the rear side surface 8d.
[0197] As explained in the first embodiment, the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) are bonded to the flatwise surfaces of the CFRP member 2, i.e., the first main surface 6 and the second main surface 7. This makes it possible to exhibit high moisture barrier performance and solve the problem of moisture absorption deformation of the CFRP structure.
[0198] The inventors have conducted extensive research into the formation of a third moisture-proof layer 13 on the side surface 8 as shown in FIG. 7 in order to further improve the moisture-proof performance.
[0199] In order to fully prevent the moisture absorption deformation problem and to achieve high dimensional accuracy and long-term stability, it is important to improve moisture proof performance. In the structure 1 as shown in Figures 1 to 3, preventing moisture absorption from the side surface 8 of the CFRP member 2 is considered to be effective in further improving the moisture proof performance.
[0200] It is considered that the diffusion speed of moisture is slow inside the CFRP member 2, and the effect of moisture absorption on the center is small. Therefore, it is considered that the effect of moisture absorption is large on the flatwise surfaces (first principal surface 6 / second principal surface 7) which have a large area and a small thickness dimension (dimension in the Z direction).
[0201] On the other hand, the edgewise surface (side surface 8) is considered to be less affected by moisture absorption than the flatwise surface, and therefore the required moisture barrier performance may be slightly lower, but the formation of the third moisture barrier layer 13 is considered to improve the moisture barrier performance.
[0202] The CFRP member 2 is formed by laminating a plurality of prepregs 5 and bonding them under heat and pressure. As described above, when molding the CFRP member 2, it is possible to integrally mold the first moisture barrier layer 3 and the second moisture barrier layer 4 on the first main surface 6 and the second main surface 7 of the CFRP member 2. However, when molding the CFRP member 2, excess matrix resin is pushed out from the side surface 8, making it difficult to simultaneously integrally mold the third moisture barrier layer 13 on the side surface 8 of the CFRP member 2.
[0203] The third moisture barrier layer 13 must be laminated after a precise edgewise surface is produced by cutting and edge trimming the molded CFRP member 2. Therefore, the joining of the third moisture barrier layer 13 to the side surface 8 of the CFRP member 2 must be performed in a separate process from the process of joining the first moisture barrier layer 3 and the second moisture barrier layer 4 to the flatwise surface (first main surface 6 / second main surface 7).
[0204] The thermal expansion coefficient in the stacking direction (Z direction) of the multiple prepregs 5 on the edgewise surface (side surface 8) is large because there is no constraint by the CF that constitutes the prepreg 5. Although it depends on the type of prepreg 5 and molding conditions, for example, at room temperature, -6 / °C or more, and in higher temperature regions the thermal expansion coefficient is even greater.
[0205] Therefore, the third moisture barrier layer 13 is bonded and integrated to the edgewise surface (side surface 8) with a thermosetting adhesive or the like at high temperatures. In this case, there is a possibility that a large thermal residual stress will occur in the edgewise surface (side surface 8) due to a large difference in thermal expansion coefficient during the process of returning to room temperature (operating temperature) after bonding at high temperatures. This may result in deformation around the edgewise surface (side surface 8) or peeling of the third moisture barrier layer 13. As a result, problems such as a decrease in moisture barrier performance will occur, increasing the risk that high dimensional accuracy cannot be ensured.
[0206] The inventors have studied the selection of a material for the third moisture barrier layer 13 to be laminated on the side surface 8 of the CFRP member 2 that can suppress the thermal residual stress caused by the temperature difference between the temperature at the time of joining and the temperature at which the third moisture barrier layer 13 is used, and the reduction of the temperature difference between the time of joining and the time of normal use. As a result, the following effective countermeasures have been newly discovered.
[0207] (1) By using metal foil as the base for the third moisture-proof layer 13, it is possible to achieve both high (or complete) moisture-proof performance and suppression of stress on the CFRP member 2. Because the metal foil is very thin, it is possible to suppress thermal residual stress even if a temperature difference occurs when bonding to the side surface 8. In addition, the adhesive layer or bonding layer for bonding the metal foil to the side surface 8 functions as a buffer material, making it possible to further suppress thermal residual stress.
[0208] (2) The temperature at which the third moisture barrier layer 13 is bonded to the side surface 8 of the CFRP member 2 is low (a temperature equal to or lower than the higher of the operating temperature of the structure 12 and 70°C), thereby reducing thermal residual stress during bonding. If bonding of the third moisture barrier layer 13 is possible at the operating temperature, it is possible to reduce thermal residual stress to almost zero. For example, it is very effective to bond the third moisture barrier layer 13 to the side surface 8 via an adhesive that hardens at low temperature or an adhesive layer that exerts adhesive strength at low temperature.
[0209] The inventors have newly discovered the following effective embodiment regarding the configuration and bonding method of the third moisture proof layer 13 that satisfies these conditions. Metal foil is attached with low temperature adhesive. The metal foil is attached with a UV-curable adhesive. The adhesive layer of a butyl tape laminated with metal foil (such as butyl tape with Al foil) is attached at room temperature. Double-sided butyl tape is used to attach thin metals or metal foils at room temperature. Attach the substrate at room temperature using the adhesive layer of Al tape.
[0210] [Evaluation of each example] The inventors evaluated the moisture barrier performance of each example of the third moisture barrier layer 13 made based on metal foil by an accelerated moisture absorption test.
[0211] Furthermore, if an attempt is made to measure the change in moisture absorption expansion strain by placing a strain gauge between the edgewise surface (side surface 8) and the third moisture barrier layer 13, it is thought that the measurement accuracy will be questionable due to the effects of moisture absorption by the strain gauge itself and the effects of stress generated at the interface between the third moisture barrier layer 13 and the edgewise surface (side surface 8).
[0212] Therefore, first, in order to measure the basic moisture-proof performance of the material and joining method used for the third moisture-proof layer 13, a moisture-proof layer was formed on the flatwise surfaces (first main surface 6 and second main surface 7) of the CFRP member 2 using the material and joining method to be used for the third moisture-proof layer 13, and the moisture-proof performance was evaluated by an accelerated moisture absorption test.
[0213] (Reference sample) A 10-ply structure with mirror symmetry between the top and bottom of pitch-based UD material was used as the CFRP member 2 used as the reference sample. When creating the CFRP member 2 reference sample, the curing molding was performed at 120°C for 2 hours, which is the recommended curing condition for pitch-based prepreg (curing under bagging adsorption pressure). After that, PB was performed at 145°C for 2 hours.
[0214] (Moisture absorption test conditions) The evaluation was carried out under conditions of a temperature of 45°C and a relative humidity of 95% or more. Evaluation of UD material in the 90° direction to the CF fiber is mainly due to the moisture absorption expansion of the matrix resin (epoxy resin), so the change in moisture absorption expansion strain is large. Therefore, the evaluation was performed at a temperature condition of 45°C, which has a low acceleration factor. In terms of the diffusion coefficient of water vapor, the temperature condition of 45°C is about four times the acceleration condition of room temperature of 25°C.
[0215] (Evaluation and measurement method) The strain gauge was placed in the center of the central layer of the prepreg laminate and molded as a single unit. After the prepreg was cured and PB was performed, the strain change was measured based on the strain level at the time when the temperature reached 45°C and the relative humidity reached 95%.
[0216] FIG. 8 is a graph showing the change over time in the amount of change in moisture expansion strain in each of the examples described below. FIG. 9 is a table showing the moisture expansion strain and the reference ratio for each example after 135 hours at 45° C. and a relative humidity of 95%.
[0217] Example 9 Al foil is bonded to the first main surface 6 and the second main surface 7 with a low-temperature adhesive (Al foil thickness: 20 μm). A low-temperature adhesive was applied to each of the roughened first principal surface 6 and second principal surface 7, and cured at a temperature of 40° C. to 60° C. for 2 to 8 hours (curing under bagging adsorption pressure). After 135 hours at 45° C. and a relative humidity of 95%, the moisture absorption expansion strain was 18 με, and the reference ratio was 2.8%, confirming that the moisture barrier performance of the third moisture barrier layer 13 was sufficient.
[0218] Example 10 Electrolytic copper foil is bonded to the first main surface 6 and the second main surface 7 with a low-temperature adhesive (electrolytic copper foil thickness: 20 μm). A low-temperature adhesive was applied to each of the roughened first principal surface 6 and second principal surface 7, and cured at a temperature of 40° C. to 60° C. for 2 to 8 hours (curing under bagging adsorption pressure). After 135 hours at 45° C. and a relative humidity of 95%, the moisture absorption expansion strain was 15 με and the reference ratio was 2.2%, confirming that the moisture barrier performance of the third moisture barrier layer 13 was sufficient.
[0219] In Examples 9 and 10, even when the curing temperature was changed in the range of 40°C to 60°C, there was no effect on moisture proofing by ensuring sufficient curing time corresponding to each temperature. For example, low-temperature adhesives can be cured at room temperature over time. In addition, there was no effect on moisture proofing performance even when pressure was applied by weight instead of bagging adsorption pressure, with respect to the pressure conditions. There was almost no difference in moisture proofing performance between Al foil and electrolytic copper foil, and high moisture proofing performance was confirmed.
[0220] Example 11 Al foil is bonded with a UV-curable adhesive (Al foil thickness: 20 μm) to the first main surface 6 and the second main surface 7. The UV-curable adhesive used is an epoxy-type tape adhesive that begins to harden rapidly when exposed to UV light. Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. A tape-like adhesive is applied to the Al foil in advance, and after UV irradiation, it is attached to the CFRP component 2 by applying pressure under weight. After 135 hours at 45° C. and a relative humidity of 95%, the moisture absorption expansion strain was 64 με and the reference ratio was 9.5%, confirming that the moisture barrier performance of the third moisture barrier layer 13 was sufficient.
[0221] Example 12 Electrolytic copper foil (electrolytic copper foil thickness: 20 μm) is bonded with a UV-curable adhesive to the first main surface 6 and the second main surface 7. The UV-curable adhesive used is an epoxy-type tape adhesive that begins to cure rapidly when exposed to UV light. Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. A tape-like adhesive is applied to the electrolytic copper foil in advance, and after UV irradiation, it is attached to the CFRP component 2 by applying pressure under weight. After 135 hours at 45° C. and a relative humidity of 95%, the moisture absorption expansion strain was 54 με and the reference ratio was 8.0%, confirming that the moisture barrier performance of the third moisture barrier layer 13 was sufficient.
[0222] In Examples 11 and 12, there was almost no difference in moisture-proofing performance between the Al foil and the electrolytic copper foil, and high moisture-proofing performance was confirmed.
[0223] (Example 13) to (Example 15) Butyl tape with Al foil was pressed at room temperature (usage temperature) and bonded to the first principal surface 6 and the second principal surface 7. As Examples 13 to 15, three different products of butyl tape with Al foil were used. Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. After 135 hours at 45°C and a relative humidity of 95%, Example 13 had a moisture expansion strain of 47 με, a ratio to the reference of 7.0%, Example 14 had a moisture expansion strain of 71 με, a ratio to the reference of 10.6%, and Example 15 had a moisture expansion strain of 62 με, a ratio to the reference of 9.2%. Although there were slight differences between products, all of them exhibited high moisture-proofing performance as the third moisture-proof layer 13. In addition, good results were obtained, showing that the moisture absorption expansion tended to saturate over time.
[0224] (Example 16) An Al foil (thickness of Al foil: 20 μm) was adhered to the first principal surface 6 and the second principal surface 7 by pressure at room temperature (usage temperature) using double-sided butyl tape. Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. After 135 hours at 45° C. and a relative humidity of 95%, the moisture absorption expansion strain was 76 με and the reference ratio was 11.3%, confirming that the moisture barrier performance of the third moisture barrier layer 13 was sufficient. The use of double-sided butyl tape allows for greater freedom in the selection of metal foils. In other words, various metal foils can be used as the third moisture-proof layer 13. In addition, since thin metal plates can be used in addition to metal foils, it is also possible to provide a function as a protective guard member for the CFRP structure 12 by attaching an Al channel (with a U-shaped cross section) to the side surface.
[0225] (Example 17) An Al tape is bonded to the first main surface 6 and the second main surface 7 at room temperature (operating temperature). The Al tape used has an adhesive layer made of synthetic resin. Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. After 135 hours at 45° C. and a relative humidity of 95%, the moisture absorption expansion strain was 98 με and the reference ratio was 14.6%, confirming that the moisture barrier performance of the third moisture barrier layer 13 was sufficient.
[0226] (Example 18) An Al tape is bonded to the first main surface 6 and the second main surface 7 at room temperature (operating temperature). The Al tape used is an airtight, waterproof type Al tape with an acrylic adhesive layer. Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. After 135 hours at 45°C and a relative humidity of 95%, the moisture absorption expansion strain was 288 με, which was 42.6% compared to the reference sample. This is a slightly low characteristic for the moisture barrier performance of the third moisture barrier layer 13, but the moisture barrier effect is recognized when compared to the reference sample not forming the third moisture barrier layer 13.
[0227] When the Al tapes of Examples 17 and 18 were used, the moisture-proof performance and reproducibility were slightly lower. This is presumably due to differences in the condition of the substrate (unevenness) and the finish at the time of application. The butyl tapes of Examples 13 to 16 have a thick adhesive layer, and butyl rubber has very low water vapor permeability, so they are less susceptible to the condition of the substrate and provide stable results.
[0228] In contrast, it was recognized that the moisture-proofing performance of the Al tape may be reduced depending on the conditions of the substrate and the bonding conditions.However, it is believed that a considerable moisture-proofing performance can be obtained under appropriate conditions, and the effect is demonstrated when compared with the untreated edgewise product (reference sample).
[0229] (Example 19) Butyl tape without metal foil was attached to the first main surface 6 and the second main surface 7 by applying pressure at room temperature (usage temperature). Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. After 135 hours at 45°C and 95% relative humidity, the moisture absorption expansion strain was 550με, 81.8% compared to the reference.
[0230] (Example 20) An airtight waterproof tape is adhered to the first principal surface 6 and the second principal surface 7 under pressure at room temperature (operating temperature). Each of the first main surface 6 and the second main surface 7 is subjected to a roughening treatment. After 135 hours at 45°C and a relative humidity of 95%, the moisture absorption expansion strain was 603με, 89.7% compared to the reference.
[0231] High moisture-proof performance was not obtained in the third moisture-proof layer 13 not using a metal foil in Examples 19 and 20. However, compared with the reference sample not forming the third moisture-proof layer 13, a moisture-proof effect was exhibited.
[0232] The examples are listed in order of decreasing moisture-proofing performance, i.e., decreasing moisture absorption expansion, as follows: (Example 10), (Example 9), (Example 13), (Example 12), (Example 15), (Example 11), (Example 14), (Example 16), (Example 17), (Example 18), (Example 19), and (Example 20).
[0233] In order to confirm whether the moisture-proofing performance results of Examples 9 to 20 from the above-mentioned accelerated moisture absorption test were consistent with actual moisture absorption conditions, the inventors measured the long-term change in weight gain due to immersion in water using the moisture-proof layers of Examples 14, 15, and 20 as representative samples.
[0234] (Reference sample) As a reference sample, a configuration was adopted in which the butyl tape with Al foil used in Example 15 was bonded to the flatwise surfaces (first main surface 6 / second main surface 7) of a CFRP member 2 made of eight mirror-symmetric layers of PAN-based CP material. As shown in Figures 8 and 9, the butyl tape with Al foil used in Example 15 has been confirmed to have a high moisture-proof effect.
[0235] (Representative samples 1-3) Representative samples 1 to 3 were prepared by bonding a third moisture-proof layer 13 to the edgewise surface (side surface 8) of the reference sample using the materials and bonding methods of Examples 14, 15 and 20.
[0236] (Measurement of weight increase by water immersion) Each sample was immersed in a water tank, removed at the designated time, and weighed after 45 minutes of natural drying.
[0237] FIG. 10 is a graph showing the change over time in the weight gain rate of each sample due to immersion in water.
[0238] As shown in Figure 10, it was confirmed that by joining a third moisture-proof layer 13 to the edgewise surface (side surface 8) of the CFRP member 2, it is possible to suppress weight increase due to moisture absorption and to exhibit a moisture-proof effect.
[0239] The effect of suppressing weight increase was found to have a similar tendency to the effect of suppressing moisture absorption expansion strain in the moisture absorption accelerated test shown in Figures 8 and 9. That is, the order of representative sample 2 (Example 15), representative sample 1 (Example 14), and representative sample 3 (Example 20), which is the order of the effect of suppressing moisture absorption expansion strain in the moisture absorption accelerated test shown in Figures 8 and 9, is the same order of the effect of suppressing weight increase due to water immersion. From these results, it is recognized that the results of moisture proof performance in the moisture absorption accelerated test shown in Figures 8 and 9 are consistent with the actual moisture absorption state.
[0240] Furthermore, by improving the moisture barrier performance of each of the first moisture barrier layer 3 laminated on the first main surface 6 and the second moisture barrier layer 4 laminated on the second main surface 7, the weight increase due to water immersion shown in Figure 10 is further suppressed.
[0241] [Further considerations regarding the formation of a third moisture barrier on the sides] 8 to 10, it was confirmed that the moisture barrier performance was improved by bonding the third moisture barrier layer 13 to the side surface 8 of the CFRP member 2. It was also found that this effect was widely exhibited without limiting the material or bonding method of the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) bonded to the flatwise surfaces (first main surface 6 and second main surface 7) of the CFRP member 2.
[0242] That is, assume that any material and any joining method are adopted as the material and joining method of the moisture barrier layers (first moisture barrier layer 3 / second moisture barrier layer 4) joined to the flatwise surfaces (first main surface 6 and second main surface 7) of the CFRP member 2. No matter what material and what joining method are selected, when comparing a configuration in which the third moisture barrier layer 13 is not formed on the edgewise surfaces (side surfaces 8) of the CFRP member 2 with a configuration in which the third moisture barrier layer 13 is formed on the edgewise surfaces (side surfaces 8), the configuration in which the third moisture barrier layer 13 is formed exhibits higher moisture barrier performance.
[0243] The present inventor has newly discovered the following configuration for a structure in which the first moisture-proof layer 3, the second moisture-proof layer 4, and the third moisture-proof layer 13 are formed, which can exhibit characteristics effective in improving the processing accuracy of a processing apparatus.
[0244] (Configuration 1) A main body portion is formed by stacking a plurality of sheet-like members mainly composed of carbon fiber, and has a first main surface and a second main surface opposed to each other in a stacking direction of the plurality of sheet-like members, and a side surface between the first main surface and the second main surface; a first moisture proof layer laminated on the first main surface; a second moisture proof layer laminated on the second main surface; A third moisture-proof layer laminated on the side surface; Equipped with At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material. structure.
[0245] In a structure having this configuration, a first moisture barrier layer 3 is laminated on a first main surface 6 of a CFRP member 2 formed by laminating a plurality of prepregs 5 whose main component is carbon fiber, and a second moisture barrier layer 4 is laminated on a second main surface 7. In addition, a third moisture barrier layer 13 is laminated on a side surface 8 of the CFRP member 2. This provides high moisture barrier performance.
[0246] In the structure having (Configuration 1), at least one of the first moisture-proof layer 3 and the second moisture-proof layer 4 is made of a material other than a ceramic material, which makes it possible to reduce the weight of the structure and the processing costs and material costs.
[0247] As a result, by applying the structure having (Configuration 1) to the frame or components of a processing device, it becomes possible to exert properties that are effective in improving processing accuracy.
[0248] For example, a structure in which the first moisture barrier layer 3, at least a part of whose surface 9 is made of a ceramic material as described in the first embodiment, and the second moisture barrier layer 4, made of a material other than the ceramic material, are joined to the flatwise surfaces (first main surface 6 / second main surface 7) and a third moisture barrier layer 13 is joined to the side surface 8, is included in the structure having the above-mentioned (Configuration 1). This structure corresponds to the configuration of the structure 12 shown in FIG.
[0249] Without being limited thereto, a configuration in which both the first moisture barrier layer 3 and the second moisture barrier layer 4 are made of a material other than a ceramic material, and a third moisture barrier layer 13 is joined to the side surface 8, is also included in the structure having the above-mentioned (Configuration 1). For example, a configuration in which various moisture barrier layers given as examples of the second moisture barrier layer 4 in the first embodiment are joined to both flatwise surfaces (first main surface 6 / second main surface 7) of the CFRP member 2, and a third moisture barrier layer 13 is joined to the side surface 8 is included in the structure having the above-mentioned (Configuration 1).
[0250] For example, a structure having the above-mentioned (Configuration 1) includes a structure in which metal foil is bonded to both flatwise surfaces (first main surface 6 / second main surface 7) of the CFRP member 2 and a third moisture-proof layer 13 is bonded to the side surface 8. A structure having the above-mentioned (Configuration 1) includes a structure in which a rubber tape having metal foil formed thereon is bonded to both flatwise surfaces (first main surface 6 / second main surface 7) of the CFRP member 2 and a third moisture-proof layer 13 is bonded to the side surface 8. A structure having the above-mentioned (Configuration 1) includes a structure in which a resin film having a moisture-proof membrane formed thereon is bonded to both flatwise surfaces (first main surface 6 / second main surface 7) of the CFRP member 2 and a third moisture-proof layer 13 is bonded to the side surface 8.
[0251] Furthermore, the inventors have newly devised a structure having the following configuration, which is a further ingenious addition to the structure having the configuration of (Configuration 1).
[0252] (Configuration 2) The structure according to (Configuration 1), The third moisture-proof layer is made of a material other than a ceramic material. structure. This (configuration 2) makes it possible to realize a reduction in the weight of the structure 1.
[0253] (Configuration 3) The structure according to (Configuration 1), The third moisture-proof layer is composed of any one of a metal foil, a metal thin plate, and a rubber tape on which the metal foil is formed. structure.
[0254] (Configuration 4) The structure according to (Configuration 1), The third moisture-proof layer is bonded to the side surface via an adhesive that hardens at low temperatures or an adhesive layer that exerts adhesive strength at low temperatures. structure.
[0255] (Configuration 5) (Configuration 3) The structure according to The third moisture-proof layer is formed by adhering the metal foil or the metal sheet to the side surface with an adhesive that hardens at a low temperature. structure.
[0256] (Configuration 6) The structure according to (Configuration 1), the first moisture proof layer has at least a portion of a surface opposite to a side laminated on the first main surface, the surface being made of a ceramic material; The second moisture-proof layer is made of a material other than a ceramic material. structure. This (Configuration 6) makes it possible to exert the effects related to the structure 1 described in the first embodiment.
[0257] (Configuration 7) The structure according to (Configuration 6), The first moisture-proof layer has an entire surface made of a ceramic material. structure.
[0258] (Configuration 8) The structure according to (Configuration 1), Each of the first moisture barrier layer and the second moisture barrier layer is made of a material different from a ceramic material. structure.
[0259] (Configuration 9) (Configuration 1) The structure according to the present invention, The first moisture-proof layer is composed of any one of a metal foil, a rubber tape on which the metal foil is formed, and a resin film on which a moisture-proof film is formed. The second moisture-proof layer is composed of any one of a metal foil, a rubber tape on which the metal foil is formed, and a resin film on which a moisture-proof film is formed. structure.
[0260] [Method for producing a structure having (Configuration 1)] As a method for producing a structure having (Configuration 1), it is possible to employ a production method including the following steps. A lamination process in which a plurality of sheet-like members (a plurality of prepregs 5) whose main component is carbon fiber are laminated. A first bonding process bonds together a plurality of sheet-like members, a first moisture-proof layer 3 laminated on a first main surface 6 which is one main surface in the stacking direction of the plurality of sheet-like members, and a second moisture-proof layer 4 laminated on a second main surface 7 opposite the first main surface 6. a second bonding step of bonding a third moisture-proof layer 13 to the side surface 8 between the first main surface 6 and the second main surface 7 of the plurality of sheet-like members; As described above, at least one of the first moisture barrier layer 3 and the second moisture barrier layer 4 is made of a material other than a ceramic material.
[0261] In the second bonding step, the third moisture-proof layer 13 is bonded to the side surface 8 with an adhesive that hardens at a low temperature, so that residual thermal stress can be suppressed.
[0262] [Processing equipment] An example of a processing device to which the structure according to the present technology can be applied will be described. The structure according to the present technology can be used in any processing device that processes a workpiece such as a substrate.
[0263] 11 is a schematic diagram showing a schematic configuration of an exposure apparatus, which is an example of a processing apparatus. The exposure apparatus 15 is a projection exposure apparatus that exposes a workpiece W. Here, the workpiece W is a silicon workpiece, a printed circuit board, a glass substrate for a liquid crystal panel, or the like, and is a workpiece with a resist film applied to its surface.
[0264] The exposure apparatus 15 has a light emitting unit 16 , a mask stage 17 , a projection optical system 18 , a work stage 19 , and a frame 20 .
[0265] The light emitting unit 16 emits the exposure light EL. For example, a short arc type mercury lamp is used as the light emitting unit 16. The mercury lamp emits ultraviolet light having wavelengths of, for example, 365 nm (i-line), 405 nm (h-line), 436 nm (g-line), etc. Of course, the configuration is not limited to this, and a lamp that emits light in a wavelength band other than ultraviolet light may be used. Alternatively, a solid-state light source such as an LED (Light Emitting Diode) or an LD (Laser Diode) may be used.
[0266] The mask stage 17 is disposed below the light emitting unit 16. The mask stage 17 holds a mask M for exposure. A predetermined mask pattern is formed on the mask M. Furthermore, an alignment mark (mask mark) is formed on the mask M.
[0267] The projection optical system 18 irradiates the exposure light EL emitted from the light emitting unit 16 and transmitted through the mask M onto the workpiece W held on the workpiece stage 19. As a result, an image of the mask pattern formed on the mask M is projected onto the workpiece W. The projection optical system 18 is configured as an imaging optical system having a projection lens.
[0268] The workpiece stage 19 holds the workpiece W. The workpiece stage 19 has an adsorption plate to which the workpiece W is adsorbed. A plurality of vacuum adsorption holes are formed in the adsorption plate, and the workpiece W is held by vacuum adsorption.
[0269] The frame 20 supports components that make up the exposure apparatus 15, such as the light emitting unit 16, the mask stage 17, the projection optical system 18, and the workpiece stage 19. These components are held in predetermined positions by the frame 20.
[0270] Components such as the mask stage 17 and the work stage 19 may be movably supported by the frame 20. For example, the components may be supported by the frame 20 so as to be capable of linear movement in two mutually perpendicular directions along the horizontal direction, linear movement along the optical axis direction of the exposure light EL (up and down direction), and rotational movement with the optical axis direction of the exposure light EL (up and down direction) as the rotation axis direction. Of course, a portion of the frame 20 supporting the components may be configured to be movable.
[0271] For example, a moving mechanism for moving components or a frame can be realized using any moving mechanism such as a linear stage using a stepping motor, or any rotating mechanism using a gear mechanism.
[0272] In the exposure device 15, when the alignment of the mask M and the workpiece W and the focus control are completed, the exposure process for the workpiece W is started, and the exposure light EL is emitted from the light emitting unit 16. The exposure light EL emitted from the light emitting unit 16 is irradiated onto the workpiece W via the mask M on which a mask pattern is formed and the projection optical system 18. As a result, the mask pattern is projected onto the workpiece W and exposed.
[0273] 11, the structure according to the present technology is applied to components such as a frame 20 and a work stage (adsorption plate) 19. This makes it possible to exert characteristics effective for improving exposure accuracy, and high exposure accuracy is realized.
[0274] 12 is a schematic diagram showing a schematic configuration of a laser processing apparatus, which is an example of a processing apparatus. The laser processing apparatus 22 has a laser emission unit 23, a workpiece stage 24, and a frame 25.
[0275] The laser emission unit 23 emits a laser beam L. The laser beam L emitted from the laser emission unit 23 is irradiated onto a workpiece W held on a workpiece stage 24, and processing such as cutting and drilling the workpiece W is performed.
[0276] The frame 25 supports components that configure the laser processing apparatus 22, such as the laser emission unit 23 and the work stage 24. These components are held in predetermined positions by the frame 25. Note that the components, such as the work stage 24, may be supported movably by the frame 25. Of course, a portion of the frame 25 that supports the components may be configured to be movable.
[0277] 12, the structure according to the present technology is applied to components such as a frame 25 and a work stage 24. This makes it possible to exert characteristics effective for improving the laser processing accuracy, and high laser processing accuracy is realized.
[0278] In addition, the structure according to the present technology can be applied to various processing devices. For example, the structure according to the present technology can be used as a member for a semiconductor element manufacturing device. The structure according to the present technology is also suitable as a stage member used for precision positioning in a stepper, an inspection device, etc. In addition, the structure according to the present technology can be applied to a position measurement mirror, a wafer chuck, a position adjustment member, a precision measurement jig, etc., making it possible to improve processing accuracy.
[0279] <Other embodiments> The present invention is not limited to the above-described embodiment, and various other embodiments can be realized.
[0280] Fig. 13 is a schematic diagram showing a configuration example of a structure according to another embodiment. A structure 27 shown in Fig. 13 is an embodiment in which the first moisture-proof layer 3 has a multi-layer structure including a ceramic member 28 and an intermediate member 29 as described in (Example 6).
[0281] 13, a metal foil is bonded to the entire first main surface 6 of the CFRP member 2 as an intermediate member 29. A ceramic member 28 is bonded to the surface (upper surface) of the intermediate member 29. As the second moisture proof layer 4, for example, the same metal foil as the intermediate member 29 is bonded.
[0282] The shape and size of the ceramic member 28 to be joined to the intermediate member 29 when viewed from above can be designed arbitrarily. That is, the ceramic member 28 can be designed to have a size smaller than the size of the entire first main surface 6 (the entire surface of the intermediate member 29) when viewed from above.
[0283] A metal foil is bonded to the entire surface of the first main surface 6 as an intermediate member 29. This provides a moisture-proof function for the first main surface 6. This allows the ceramic member 28 bonded to the metal foil to be configured to be smaller in size than the entire surface of the metal foil. This allows the structure 1 to be made smaller and lighter. It also makes it possible to reduce the material cost of the ceramic member 28.
[0284] 13, the surface 9 of the first moisture-proof layer 3 opposite the side to be laminated on the first main surface 6 includes an upper surface 30 of the ceramic member 28 and an upper surface 31 of a portion of the intermediate member 29 on which the ceramic member 28 is not laminated. Thus, the first moisture-proof layer 3 of the structure 27 is laminated over the entire first main surface 6, and a portion of the surface 9 opposite the side to be laminated on the first main surface 6 is made of a ceramic material. Even with this configuration, the effects unique to the present invention described above can be achieved.
[0285] For example, when the structure 27 is applied to a work stage (adsorption plate), the ceramic member 28 can be designed in a shape and size required to hold the work. Of course, even when various processing other than flat processing is performed, the ceramic member 28 can be designed in a required shape and size.
[0286] The second moisture-proof layer 4 laminated on the second main surface 7 of the CFRP member 2 and the third moisture-proof layer 13 bonded to the side surface 5 may have a multi-layer structure.
[0287] [Other configuration examples of CFRP components] Fig. 14 is a schematic diagram showing an example of the configuration of a CFRP member according to another embodiment, and Fig. 15 is a schematic diagram showing the internal structure of the CFRP member shown in Fig. 14.
[0288] In the above embodiment, a plurality of prepregs, which are sheet-like members mainly composed of carbon fiber, are laminated to form the CFRP member 2. The bonding of the first moisture barrier layer 3, the second moisture barrier layer 4, and the third moisture barrier layer 13 according to the present invention described above can also be applied to CFRP members having other configurations.
[0289] 14 has an approximate rectangular parallelepiped outer shape, and has a first main surface 6 and a second main surface 7 which are flatwise surfaces with large areas. In addition, the CFRP member 32 has side surfaces 8 (left side surface 8a, right side surface 8b, front side surface 8c, and rear side surface 8d) which are edgewise surfaces with small areas.
[0290] The structure 33 also has an upper skin member 34, a lower skin member 35, side skin members 36 (left skin member 36a, right skin member 36b, front skin member 36c, rear skin member 36d), and an internal structure 37.
[0291] The upper skin member 34 is joined to the upper side of the internal structure 37 and constitutes the first main surface 6. The lower skin member 35 is joined to the lower side of the internal structure 37 and constitutes the second main surface 7.
[0292] The side skin portions 36 are joined to the sides of the internal structure 37 to form the side surfaces 8. As shown in Figs. 14 and 15, a left side surface 8a is formed by a left skin member 36a joined to the left side of the internal structure 37. A right side surface 8b is formed by a right skin member 36b joined to the right side of the internal structure 37. A front side surface 8c is formed by a front skin member 36c joined to the front side of the internal structure 37. A rear side surface 8d is formed by a rear skin member 36d joined to the rear side of the internal structure 37.
[0293] The upper skin member 34, the lower skin member 35, and the side skin member 36 are made of carbon fiber reinforced plastic members formed by laminating prepregs made of carbon fibers impregnated with resin. The upper skin member 34, the lower skin member 35, and the side skin member 36 may each be made of a single sheet of prepreg. The specific material of the prepreg is not limited.
[0294] 15, the internal structure 37 is configured by assembling a plurality of plate-like members 39. The plate-like members 39 are configured from carbon fiber reinforced plastic members molded by laminating prepregs made of carbon fibers impregnated with resin. Note that the plate-like members 39 may be configured from one sheet of prepreg. The specific material of the prepreg is not limited.
[0295] In this embodiment, four plate-like members 39a having the same rectangular shape are arranged at equal intervals in the front-rear direction (Y direction) so as to extend in the left-right direction (X direction). Four plate-like members 39b having the same shape as the plate-like members 39a are arranged so as to intersect with the four plate-like members 39a.
[0296] 15, the four plate-like members 39b are arranged at equal intervals in the left-right direction (X direction) so as to extend in the front-rear direction (Y direction). Note that slits (not shown) are formed at the intersections of the plate-like members 39a and 39b, and the slits fit together.
[0297] As shown in FIG. 15, plate-like members 39a and 39b are assembled such that both ends of each member are located at the periphery of a predetermined rectangle when viewed from above.
[0298] In addition to the plate members 39a and 39b, six plate members 39c, whose short-side sizes are equal to those of the plate members 39a and 39b and whose long-side sizes are appropriately adjusted, are arranged so as to intersect with the plate members 39a and 39b.
[0299] The six plate-like members 39c are arranged at equal intervals along a direction perpendicular to the left-right direction (X direction) and the front-rear direction (Y direction) (left-right direction in FIG. 15) so as to extend along the direction intersecting at 45 degrees with each of the left-right direction (X direction) and the front-rear direction (Y direction). The six plate-like members 39c are also arranged so as to intersect at the midpoint between adjacent plate-like members 39a and at the midpoint between adjacent plate-like members 39b. Slits (not shown) are formed at the intersecting portions, and the slits fit together.
[0300] The size of the six plate-like members 39c in the longitudinal direction is appropriately adjusted so that the positions of both ends are located on the periphery of a predetermined rectangle where both ends of the plate-like members 39a and 39b are located.
[0301] As shown in FIG. 15, when the internal structure 37 is viewed from above, it has a configuration in which hexagonal gaps 40 and triangular gaps 41 are arranged periodically.
[0302] When viewed from above, an upper skin member 34 having a rectangular shape that fits along both ends of the plate-like members 39a to 39c is joined to the upper side of the internal structure 37 to form a first main surface 6. A lower skin member 35 having approximately the same shape as the upper skin member 34 is joined to the lower side of the internal structure 37 to form a second main surface 7. Side skin members 36 (36a to 36d) are joined to the sides of the internal structure 37 to form side surfaces 8 (8a to 8d).
[0303] It is possible to apply the bonding of the first moisture barrier layer 3, the second moisture barrier layer 4, and the third moisture barrier layer 13 according to the present invention described above to such a CFRP member 37, and it is possible to achieve the effects unique to the present invention described above.
[0304] Of course, the present invention can be applied to a CFRP member having a different configuration from the structure 37 shown in Figures 14 and 15. That is, in application of the present invention, various configurations can be adopted for the internal structure 37 that constitutes the CFRP member.
[0305] For example, an internal structure may be adopted in which gaps of a predetermined shape, such as a triangle, a rectangle, a regular hexagon, or another polygon, are regularly arranged when viewed from above. For example, an internal structure having a honeycomb structure may be adopted. In addition, the configurations shown in Figures 14 and 15 can also be said to be internal structures having a honeycomb structure in a broad sense.
[0306] The inner structure may be formed using corrugated members made of carbon fiber reinforced plastic members, or may be formed by randomly assembling members made of carbon fiber reinforced plastic members.
[0307] The first moisture barrier layer 3 and the second moisture barrier layer 4 described in the first embodiment are bonded to a CFRP member 2 of any configuration having a first main surface 6, a second main surface 7, and a side surface 8. A structure thus constructed is included in the following (Structure A).
[0308] (Structure A) A main body portion is formed of a plurality of sheet-like members mainly composed of carbon fiber and has a first main surface and a second main surface opposed to each other; a first moisture-proof layer that is laminated on the first main surface, and at least a part of a surface opposite to the side laminated on the first main surface is made of a ceramic material; a second moisture-proof layer laminated on the second main surface and made of a material different from the ceramic material; A structure comprising:
[0309] Of course, the structure 1 shown in FIG. 1 and the structure 33 shown in FIG. 14 are also included in (structure A).
[0310] As a method for producing such a (Structure A), a production method including the following steps can be adopted.
[0311] A molding process for forming a main body portion having a first main surface and the second main surface from a plurality of sheet-like members whose main component is carbon fiber. a first bonding step of bonding a first moisture proof layer to the first main surface; A second bonding step of bonding a second moisture proof layer to the second main surface. At least a part of the surface of the first moisture-proof layer opposite to the side laminated on the first main surface is made of a ceramic material, and the second moisture-proof layer is made of a material different from the ceramic material.
[0312] The molding step, the first bonding step, and the second bonding step may be performed in separate steps, or may be performed integrally in the same step. Also, any combination of the molding step, the first bonding step, and the second bonding step may be performed integrally in the same step.
[0313] The first bonding step includes a step of bonding the first moisture-proof layer to a sheet-like member (which can be called a first sheet-like member) constituting the first main surface before the molding step, and the second bonding step includes a step of bonding a second moisture-proof layer to a sheet-like member (which can be called a second sheet-like member) constituting the second main surface before the molding step.
[0314] 14 and 15, the molding step of the inner structure 37 and the step of joining the skin members to the inner structure 37 may be performed in separate steps, or may be performed integrally in the same step. Also, the molding step of the CFRP member 33 and the step of joining each moisture proof layer may be performed in separate steps, or may be performed integrally in the same step.
[0315] Furthermore, after the first moisture proof layer 3 is joined to the upper skin member 34, a joining step between the upper skin member 34 and the inner structure 37 (i.e., a molding step of the CFRP member 33) may be performed. Furthermore, after the second moisture proof layer 4 is joined to the lower skin member 35, a joining step between the lower skin member 35 and the inner structure 37 (i.e., a molding step of the CFRP member 33) may be performed.
[0316] Moreover, the above-described (Configuration 1) is applied to a CFRP member 2 having an arbitrary configuration, which has a first main surface 6, a second main surface 7, and a side surface 8. A structure thus configured is included in the following (Structure B).
[0317] (Structure B) A main body portion is formed of a plurality of sheet-like members mainly composed of carbon fiber, and has a first main surface and a second main surface opposed to each other, and a side surface between the first main surface and the second main surface; a first moisture proof layer laminated on the first main surface; a second moisture proof layer laminated on the second main surface; A third moisture-proof layer laminated on the side surface; Equipped with At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material. structure.
[0318] As a method for producing such a (Structure B), a production method including the following steps can be adopted.
[0319] A molding process for molding a main body having a first main surface, a second main surface, and a side surface between the first main surface and the second main surface, using a plurality of sheet-like members whose main component is carbon fiber. a first bonding step of bonding a first moisture proof layer to the first main surface; A second bonding step of bonding a second moisture proof layer to the second main surface. a third bonding step of bonding a third moisture proof layer to the third main surface; At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material.
[0320] The molding step, the first bonding step, the second bonding step, and the third bonding step may be performed in separate steps, or may be performed integrally in the same step. Also, any combination of the molding step, the first bonding step, the second bonding step, and the third bonding step may be performed integrally in the same step.
[0321] The first joining step includes a step of joining the first moisture-proof layer to a sheet-like member (which can be called a first sheet-like member) constituting the first main surface before the molding step. The second joining step includes a step of joining a second moisture-proof layer to a sheet-like member (which can be called a second sheet-like member) constituting the second main surface before the molding step. The third joining step includes a step of joining a third moisture-proof layer to a sheet-like member (which can be called a third sheet-like member) constituting the side surface before the molding step.
[0322] 14 and 15, the molding step of the inner structure 37 and the step of joining the skin members to the inner structure 37 may be performed in separate steps, or may be performed integrally in the same step. Also, the molding step of the CFRP member 33 and the step of joining each moisture proof layer may be performed in separate steps, or may be performed integrally in the same step.
[0323] Furthermore, after the first moisture proof layer 3 is joined to the upper skin member 34, a joining step between the upper skin member 34 and the inner structure 37 (i.e., a molding step of the CFRP member 33) may be performed. Moreover, after the second moisture proof layer 4 is joined to the lower skin member 35, a joining step between the lower skin member 35 and the inner structure 37 (i.e., a molding step of the CFRP member 33) may be performed. Moreover, after the third moisture proof layer 13 is joined to the side skin member 36, a joining step between the side skin member 36 and the inner structure 37 (i.e., a molding step of the CFRP member 33) may be performed.
[0324] In the above embodiment, the first moisture barrier layer 3 having at least a part of the surface 9 made of a ceramic material, the second moisture barrier layer 4 made of a material other than a ceramic material, and the third moisture barrier layer 13 basically made of metal foil have been described. For example, the third moisture barrier layer 13 can be realized using the configuration and bonding method described for the second moisture barrier layer 4 made of a material other than a ceramic material. Also, the second moisture barrier layer 13 can be realized using the configuration and bonding method described for the third moisture barrier layer 13 basically made of metal foil.
[0325] Furthermore, an intermediate member for the first moisture barrier layer 3 constituting a multi-layer structure with a ceramic member may be realized using the configuration and bonding method described for the second moisture barrier layer 4 made of a material different from a ceramic material. Also, an intermediate member for the first moisture barrier layer 3 constituting a multi-layer structure with a ceramic member may be realized using the configuration and bonding method described for the third moisture barrier layer 13 basically made of metal foil.
[0326] In the present disclosure, the metal foil is configured to have a thickness of 200 μm or less. For example, the metal foil according to the present invention can be formed so as to have a thickness of 1 μm or more and 200 μm or less.
[0327] If the thickness of the metal foil is too small, through holes may be formed, which may reduce the function of the moisture-proof layer. Therefore, in order to achieve a high moisture-proof function, it is preferable to use a metal foil having a thickness of 5 μm or more.
[0328] As described above, the metal foil undergoes elastic and plastic deformation, thereby making it possible to reduce the thermal residual stress applied to the CFRP member 2. The smaller the thickness of the metal foil, the greater the effect of suppressing the thermal residual stress due to elastic and plastic deformation.
[0329] Therefore, by reducing the upper limit of the thickness condition of the metal foil, for example, to 200 μm or less, 175 μm or less, 150 μm or less, 125 μm or less, 100 μm or less, 75 μm or less, 50 μm or less, or 25 μm or less, it is possible to realize a metal foil that has a high effect of suppressing thermal residual stress due to elastic deformation and plastic deformation.
[0330] Considering both the moisture-proof function and the effect of suppressing thermal residual stress, the thinner the metal foil is, within the range of 5 μm or more, the more preferable the configuration. Of course, even if a metal foil with a thickness of 200 μm is used, the moisture-proof function and the effect of suppressing thermal residual stress are exhibited.
[0331] For example, in the structure 1 of the above-mentioned (Example 6), the copper foil serving as the intermediate member of the first moisture-proof layer 3 and the copper foil serving as the second moisture-proof layer 4 were both changed to Al foils with a thickness of 20 μm. In this case, no deformation due to thermal residual stress was observed. Furthermore, the verification results of the accelerated moisture absorption test showed that when the moisture absorption expansion of the reference sample was saturated after 60 hours, the moisture absorption expansion strain was 2.5 με, which was suppressed to 2.7% compared to the reference. This result is equivalent to the result when the 20 μm thick copper foil of (Example 6) was used.
[0332] Also, in the structure 1 of Example 6, the copper foil serving as the intermediate member of the first moisture-proof layer 3 and the copper foil serving as the second moisture-proof layer 4 were both changed to Al foils with a thickness of 50 μm. In this configuration, no deformation or the like caused by thermal residual stress was observed. The results of the accelerated moisture absorption test also showed that when the moisture absorption expansion of the reference sample was saturated after 60 hours, the moisture absorption expansion strain was 2.0 με, which was suppressed to 2.1% compared to the reference.
[0333] That is, in the structure 1 of Example 6, three types of samples, namely, copper foil having a thickness of 20 μm, Al foil having a thickness of 20 μm, and Al foil having a thickness of 50 μm, were tested as the metal foil that serves as the intermediate member of the first moisture-proof layer 3 and the metal foil that serves as the second moisture-proof layer 4. As a result, no deformation due to thermal residual stress was observed in any of the structures 1, and the verification results of the accelerated moisture absorption test were also at almost the same level and gave good results.
[0334] It is possible to manufacture various parts using the processing apparatus according to the present invention. For example, by performing exposure using the exposure apparatus according to the present invention, it is possible to manufacture various substrates on which a predetermined pattern is formed as parts. For example, it is possible to manufacture electric circuit elements, optical elements, MEMS, recording elements, sensors, or molds as parts. Examples of the electric circuit element include volatile or non-volatile semiconductor memories such as DRAM, SRAM, flash memory, and MRAM, and semiconductor elements such as LSI, CCD, image sensor, and FPGA. Examples of the mold include a mold for imprinting.
[0335] The configurations of the structure, CFRP member, first moisture-proof layer, second moisture-proof layer, third moisture-proof layer, processing device, exposure device, laser processing device, etc., the manufacturing method of the structure, the bonding method of the first moisture-proof layer, the bonding method of the second moisture-proof layer, the bonding method of the third moisture-proof layer, the integral molding method of a plurality of prepregs, the exposure method, the laser processing method, etc., explained with reference to the drawings are merely one embodiment and can be arbitrarily modified without departing from the spirit of the present invention. In other words, any other configuration, process flow, algorithm, etc. for carrying out the present invention may be adopted.
[0336] In this disclosure, in order to facilitate understanding of the explanation, the words "approximately", "almost", "approximately", etc. are used as appropriate. However, there is no clear difference between using these words "approximately", "almost", "approximately", etc. and not using them. In other words, in the present disclosure, concepts that define shape, size, positional relationship, state, and the like, such as "center," "central," "uniform," "equal," "same," "orthogonal," "parallel," "symmetric," "extending," "axial direction," "cylindrical," "cylindrical," "ring-shaped," and "annular," are concepts that include "substantially central," "substantially central," "substantially uniform," "substantially equal," "substantially the same," "substantially orthogonal," "substantially parallel," "substantially symmetric," "substantially extending," "substantially axial direction," "substantially cylindrical," "substantially cylindrical," "substantially ring-shaped," "substantially annular," and the like. For example, this includes states that are included within a specified range (e.g., a range of ±10%) based on standards such as "perfectly centered," "perfectly central," "perfectly uniform," "perfectly equal," "perfectly the same," "perfectly orthogonal," "perfectly parallel," "perfectly symmetrical," "perfectly extended," "perfectly axial," "perfectly cylindrical," "perfectly cylindrical," "perfectly ring-shaped," "perfectly toric," etc. Therefore, even if the words "approximately", "almost", "roughly", etc. are not added, the concept expressed by adding "approximately", "almost", "approximately", etc. may be included. Conversely, a state expressed by adding "approximately", "almost", "approximately", etc. does not necessarily exclude a perfect state.
[0337] In this disclosure, expressions using "more than", such as "greater than A" and "smaller than A", are expressions that comprehensively include both concepts that include equivalent to A and concepts that do not include equivalent to A. For example, "greater than A" is not limited to cases that do not include equivalent to A, but also includes "A or greater." Furthermore, "smaller than A" is not limited to "less than A" but also includes "A or less." When implementing the present technology, specific settings and the like may be appropriately adopted from the concepts included in "greater than A" and "smaller than A" so as to achieve the effects described above.
[0338] It is also possible to combine at least two of the characteristic parts of the present technology described above. That is, the various characteristic parts described in each embodiment may be arbitrarily combined without distinction between the embodiments. In addition, the various effects described above are merely examples and are not limited thereto, and other effects may be exhibited. [Explanation of symbols]
[0339] 1, 12...Structure (CFRP structure) 2…CFRP member 3...First moisture barrier layer 4...Second moisture barrier 5…Prepreg 6...First main surface 7...Second main surface 8(8a~8d)...Side 9...Surface of the first moisture-proof layer 13 (13a to 13d)...Third moisture-proof layer 15...Exposure equipment 19, 24…Work Stage 20, 25…frame 22...Laser processing equipment
Claims
1. A main body portion is formed by stacking a plurality of sheet-like members mainly composed of carbon fiber, and has a first main surface and a second main surface opposed to each other in a stacking direction of the plurality of sheet-like members; a first moisture-proof layer that is laminated on the first main surface, and at least a part of a surface opposite to the side laminated on the first main surface is made of a ceramic material; a second moisture-proof layer laminated on the second main surface and made of a material different from the ceramic material; A structure comprising:
2. 2. The structure of claim 1, The first moisture-proof layer has an entire surface made of a ceramic material. structure.
3. 2. The structure of claim 1, Each of the plurality of sheet-like members is a prepreg made of carbon fiber impregnated with resin, The main body is a carbon fiber reinforced plastic member formed by laminating the prepreg. structure.
4. 2. The structure of claim 1, The first moisture-proof layer is made of low thermal expansion glass. structure.
5. 2. The structure of claim 1, The first moisture-proof layer has a thermal expansion coefficient of −1×10 at temperatures of 20° C. to 130° C. in a direction parallel to the surface of the first moisture-proof layer that is laminated on the first main surface. -6 / °C or more than 1×10 -6 / °C. structure.
6. 2. The structure of claim 1, The first moisture proof layer includes a low thermal expansion glass that constitutes the surface, and an intermediate member that is disposed between the low thermal expansion glass and the first main surface. structure.
7. 7. The structure of claim 6, The intermediate member is made of a metal foil. structure.
8. 2. The structure of claim 1, The second moisture-proof layer is composed of any one of a metal foil, a rubber tape on which the metal foil is formed, and a resin film on which a moisture-proof film is formed. structure.
9. 2. The structure of claim 1, At least one of the first moisture-proof layer and the second moisture-proof layer is bonded to the main body via an adhesive that hardens at a low temperature or an adhesive layer that exerts adhesive strength at a low temperature. structure.
10. 2. The structure of claim 1, The second moisture-proof layer is configured by adhering the metal foil to the second main surface with an adhesive that hardens at a low temperature. structure.
11. 2. The structure of claim 1, The first moisture-proof layer is made of a material that has a thermal residual stress of 6 MPa or less caused by a step of bonding the first moisture-proof layer to the main body. structure.
12. 2. The structure of claim 1, The thermal expansion coefficient of the first moisture-proof layer in a direction parallel to the surface of the first main surface at temperatures of 20° C. to 130° C. is −1×10 -6 / °C or more than 1×10 -6 / ℃ structure.
13. 2. The structure of claim 1, The difference in thermal expansion coefficient between the first moisture-proof layer and the main body is 1×10 -6 / °C. structure.
14. 2. The structure of claim 1, the first moisture proof layer is laminated on the entire first main surface, The second moisture-proof layer is laminated on the entire second main surface. structure.
15. 2. The structure of claim 1, The first moisture-proof layer is configured such that the surface made of a ceramic material is a processing target surface that is to be processed. structure.
16. 16. The structure of claim 15, The surface to be machined is a surface to be machined into a flat surface. structure.
17. 2. The structure of claim 1, the body portion has a side surface between the first main surface and the second main surface, The structure further includes a third moisture-proof layer laminated to the side surface. A structure comprising:
18. 20. The structure of claim 17, The third moisture-proof layer is formed of any one of a metal foil, a metal thin plate, and a rubber tape on which the metal foil is formed. structure.
19. 20. The structure of claim 17, The third moisture-proof layer is bonded to the side surface via an adhesive that hardens at a low temperature or an adhesive layer that exerts adhesive strength at a low temperature. structure.
20. 20. The structure of claim 17, The third moisture-proof layer is formed by adhering the metal foil or the metal sheet to the side surface with an adhesive that hardens at a low temperature. structure.
21. A main body portion is formed by stacking a plurality of sheet-like members mainly composed of carbon fiber, and has a first main surface and a second main surface that face each other in a stacking direction of the plurality of sheet-like members, and a side surface between the first main surface and the second main surface; a first moisture proof layer laminated on the first main surface; a second moisture proof layer laminated on the second main surface; A third moisture-proof layer laminated on the side surface; Equipped with At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material. structure.
22. A main body portion is formed of a plurality of sheet-like members mainly composed of carbon fiber and has a first main surface and a second main surface opposed to each other; a first moisture-proof layer that is laminated on the first main surface, and at least a part of a surface opposite to the side laminated on the first main surface is made of a ceramic material; a second moisture-proof layer laminated on the second main surface and made of a material different from the ceramic material; A structure comprising:
23. A main body portion is formed of a plurality of sheet-like members mainly composed of carbon fiber, and has a first main surface and a second main surface opposed to each other, and a side surface between the first main surface and the second main surface; a first moisture proof layer laminated on the first main surface; a second moisture proof layer laminated on the second main surface; A third moisture-proof layer laminated on the side surface; Equipped with At least one of the first moisture-proof layer and the second moisture-proof layer is made of a material other than a ceramic material. structure.
24. A processing device for processing a workpiece, comprising the structure according to claim 1, 21, 22 or 23. Processing equipment.
25. 25. The processing device according to claim 24, The structure is used for a work stage for holding the work. Processing equipment.
26. 25. The processing device according to claim 24, Configured as an exposure device Processing equipment.
Citation Information
Patent Citations
High flatness structure
JP2017080899A
Structure containing ceramic and carbon fiber reinforced plastic
JP2009248398A