Method for manufacturing electrode composition for non-aqueous electrolyte secondary battery, method for manufacturing electrode for non-aqueous electrolyte secondary battery, and method for manufacturing non-aqueous electrolyte secondary battery
By employing carboxymethylcellulose and a saturated carboxylic acid lithium salt or borate to form a crosslinked structure, the method addresses the issue of weak film strength and variability in battery characteristics, enhancing electrode stability and performance.
Patent Information
- Application Number
- JP2023085894
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing non-aqueous electrolyte secondary batteries result in weak film strength and poor durability due to undissolved carboxymethylcellulose remaining in the slurry, leading to variations in battery characteristics.
The use of carboxymethylcellulose and/or its salt with a specific degree of carboxymethyl substitution, combined with a saturated carboxylic acid lithium salt or borate, to form a crosslinked structure that enhances the stability and uniformity of the electrode composition, reducing variations in battery characteristics.
The method produces electrodes with improved film strength and reduced variations in battery characteristics, resulting in enhanced battery performance and stability.
Smart Images

Figure 2024168872000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an electrode composition for a non-aqueous electrolyte secondary battery, a method for producing an electrode for a non-aqueous electrolyte secondary battery, and a method for producing a non-aqueous electrolyte secondary battery. [Background technology]
[0002] In recent years, electronic devices, particularly mobile devices such as mobile phones such as smartphones, tablets, and notebook computers, have become smaller, lighter, thinner, and more powerful, and the use of mobile devices is becoming more widespread. As the range of use of such mobile devices becomes more diverse, batteries that drive them have become very important components. Among such batteries, non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, which have high energy density and high capacity, are widely used.
[0003] Usually, a non-aqueous electrolyte secondary battery is manufactured as follows. That is, a negative electrode containing a negative electrode active material made of a carbon material capable of absorbing and releasing lithium ions and a positive electrode containing a positive electrode active material made of a lithium-containing transition metal composite oxide (e.g., LiCoO2, LiNiO2, LiMn2O4, etc.) are formed in a sheet shape on the surface of a metal foil as a current collector substrate (current collector), respectively, to obtain a sheet-shaped positive electrode and a sheet-shaped negative electrode. Then, the sheet-shaped positive electrode and the sheet-shaped negative electrode are wound or stacked with a separator also formed in a sheet shape interposed therebetween, and are stored in a case. The sheet-shaped positive electrode and the sheet-shaped negative electrode have a structure including a metal foil as a current collector substrate (current collector) and a mixture layer containing an active material formed on the surface thereof, and are formed by applying a negative electrode active material slurry (or paste) or a positive electrode active material slurry (or paste) to a current collector and drying it.
[0004] The negative electrode active material slurry (paste) contains a binder in addition to a negative electrode active material made of a carbon material capable of absorbing and releasing lithium ions. Patent Document 1 discloses a binder for negative electrodes containing styrene / butadiene latex (SBR) as a main component.
[0005] According to Patent Document 1, carboxymethyl cellulose as a water-soluble thickener is dissolved in water to prepare an aqueous solution, and SBR and a negative electrode active material are mixed with this to produce a slurry. The slurry is applied as a coating liquid onto a substrate and dried to form a sheet-shaped negative electrode.
[0006] On the other hand, in the manufacture of positive electrodes for non-aqueous electrolyte secondary batteries, organic solvents such as N-methyl-2-pyrrolidone (NMP) have traditionally been used as the solvent, but in recent years, water has come to be used as the solvent in order to reduce the cost of handling and to reduce the impact on the environment when it is discharged.
[0007] The positive electrode active material slurry (paste) contains a lithium-containing transition metal composite oxide (e.g., LiCoO2, LiNiO2, LiMn2O4, etc.) as a positive electrode active material, carbon as a conductive material, and a binder. Patent Document 2 describes a binder such as cellulose, such as carboxymethylcellulose, which has a viscosity of 4000 mPa·s or more in a 1% aqueous solution. Patent Document 2 describes the preparation of an active material paste by adding carboxymethylcellulose, together with a conductive material, polytetrafluoroethylene (PTFE), and the like, to pure water.
[0008] However, in both Patent Document 1 and Patent Document 2, undissolved carboxymethyl cellulose used as a binder remains in the slurry, which can cause line-like defects (streaks) on the current collecting substrate to which the slurry is applied, or the film strength when the slurry is applied to the current collecting substrate is weak, raising concerns about poor durability. As a result, it tends not to be possible to obtain good battery characteristics. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 5-74461 [Patent Document 2] JP 2003-157847 A Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, the present inventors conducted an investigation to improve the battery characteristics, and found that although the battery characteristics were improved by adding a specific substance, the battery characteristics (particularly the capacity retention rate) varied greatly.
[0011] An object of the present invention is to provide a method for producing an electrode composition for a non-aqueous electrolyte secondary battery, which enables the production of batteries with less variation in battery characteristics, a method for producing an electrode for a non-aqueous electrolyte secondary battery using the electrode composition for a non-aqueous electrolyte secondary battery obtained by the method for producing an electrode composition for a non-aqueous electrolyte secondary battery, and a method for producing a non-aqueous electrolyte secondary battery. [Means for solving the problem]
[0012] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the following (1) to (12). That is, according to the present invention, (1) A method for producing an electrode composition for a non-aqueous electrolyte secondary battery, comprising a first mixing step of mixing carboxymethylcellulose and / or a salt thereof having a carboxymethyl substitution degree of 0.45 or more per anhydrous glucose unit with an electrode active material, and a second mixing step of mixing a lithium salt of a saturated carboxylate or a borate having 6 or less carbon atoms with the mixture obtained in the first mixing step; (2) The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1), wherein the lithium salt of a saturated carboxylic acid having 6 or less carbon atoms includes at least a lithium salt of citrate. (3) A method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1) or (2), which satisfies the following condition (I): Condition (I): When the degree of carboxymethyl substitution of the carboxymethyl cellulose and / or a salt thereof is 0.45 or more and 1.0 or less, the saturated lithium carboxylate having 6 or less carbon atoms is contained in an amount of 1 to 100 parts by weight per 100 parts by weight of the carboxymethyl cellulose and / or a salt thereof, (4) A method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to claim 1 or 2, which satisfies the following condition (II): Condition (II): When the degree of carboxymethyl substitution of the carboxymethyl cellulose and / or a salt thereof is more than 1.0, the saturated carboxylic acid lithium salt having 6 or less carbon atoms is contained in an amount of 1 to 200 parts by weight per 100 parts by weight of the carboxymethyl cellulose and / or a salt thereof; (5) The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1), wherein the borate comprises at least one selected from sodium borate and lithium borate. (6) The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1) or (5), wherein the borate is contained in an amount of 0.1 to 20 parts by weight per 100 parts by weight of a solid content of the carboxymethyl cellulose and / or a salt thereof. (7) The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1) or (2), wherein the carboxymethyl cellulose and / or a salt thereof has a degree of dispersion of 20 to 60% as measured using a powder tester. (8) The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1) or (2), wherein, when 2 L of a 0.3 mass % aqueous solution of the carboxymethyl cellulose or a salt thereof having a dry mass B is prepared, the whole solution is filtered through a 250 mesh filter under reduced pressure conditions of -200 mmHg, and the dry mass A of the residue on the filter after filtration is measured, the ratio of the dry mass A to the dry mass B is less than 50 ppm. (9) The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to (1) or (2), wherein the carboxymethyl cellulose and / or the salt thereof is a mechanically pulverized product. (10) The method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to (1) or (2), wherein the electrode active material contains a silicon-based compound. (11) A method for producing an electrode for a non-aqueous electrolyte secondary battery, the method comprising the step of forming an electrode using the electrode composition for a non-aqueous electrolyte secondary battery produced by the method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to (1) or (2). (12) A method for producing a non-aqueous electrolyte secondary battery, comprising the step of producing a non-aqueous electrolyte secondary battery using the electrode composition for a non-aqueous electrolyte secondary battery produced by the method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to (1) or (2). is provided. Effect of the Invention
[0013] According to the present invention, there are provided a method for producing an electrode composition for a non-aqueous electrolyte secondary battery, which enables production of batteries with less variation in battery characteristics, a method for producing an electrode for a non-aqueous electrolyte secondary battery using the electrode composition for a non-aqueous electrolyte secondary battery obtained by the method for producing an electrode composition for a non-aqueous electrolyte secondary battery, and a method for producing a non-aqueous electrolyte secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The method for producing the electrode composition for non-aqueous electrolyte secondary batteries of the present invention will be described below. The method for producing the electrode composition for non-aqueous electrolyte secondary batteries of the present invention (hereinafter sometimes referred to as "electrode composition") includes a first mixing step of mixing carboxymethylcellulose and / or a salt thereof having a carboxymethyl substitution degree of 0.45 or more per anhydrous glucose unit with an electrode active material, and a second mixing step of mixing the mixture obtained in the first mixing step with a saturated lithium carboxylate or borate having 6 or less carbon atoms.
[0015] (1st mixing step) In the first mixing step of the method for producing an electrode composition of the present invention, carboxymethylcellulose and / or its salt having a carboxymethyl substitution degree of 0.45 or more per anhydrous glucose unit is mixed with an electrode active material. The mixing method is not particularly limited, and known devices and known techniques can be used.
[0016] <Carboxymethylcellulose and / or its salt> The carboxymethylcellulose and / or its salt used in the present invention has a structure in which the hydroxyl group in the glucose residue constituting cellulose is replaced with a carboxymethyl ether group. The carboxymethylcellulose may be in the form of a salt. Examples of the salt of carboxymethylcellulose include metal salts such as sodium carboxymethylcellulose.
[0017] In the present invention, cellulose refers to a polysaccharide having a structure in which D-glucopyranose (also simply called "glucose residue" or "anhydroglucose") is linked by β,1-4 bonds. Cellulose is generally classified into natural cellulose, regenerated cellulose, fine cellulose, microcrystalline cellulose excluding the amorphous region, etc., based on the origin, manufacturing method, etc.
[0018] Examples of natural cellulose include bleached pulp or unbleached pulp (bleached wood pulp or unbleached wood pulp); linters, refined linters; cellulose produced by microorganisms such as acetic acid bacteria, and the like. The raw material for bleached pulp or unbleached pulp is not particularly limited, and examples thereof include wood, cotton, straw, bamboo, and the like. The manufacturing method for bleached pulp or unbleached pulp is also not particularly limited, and may be a mechanical method, a chemical method, or a method that combines the two in between. Examples of bleached pulp or unbleached pulp classified according to the manufacturing method include mechanical pulp, chemical pulp, groundwood pulp, sulfite pulp, and kraft pulp. Furthermore, dissolving pulp may be used in addition to paper pulp. Dissolving pulp is chemically refined pulp, and is mainly used by dissolving it in chemicals, and is the main raw material for artificial fibers, cellophane, and the like.
[0019] Examples of regenerated cellulose include cellulose dissolved in some solvent such as cuprammonium solution, cellulose xanthate solution, or morpholine derivative, and then spun again.
[0020] Examples of fine cellulose include those obtained by subjecting cellulosic materials, including the above-mentioned natural cellulose and regenerated cellulose, to depolymerization treatment (e.g., acid hydrolysis, alkaline hydrolysis, enzymatic decomposition, explosive crushing treatment, vibrating ball mill treatment, etc.), and those obtained by mechanically treating the above-mentioned cellulosic materials.
[0021] It is important that the carboxymethyl cellulose and / or salt thereof of the present invention has a degree of carboxymethyl substitution per anhydroglucose unit of 0.45 or more, and more preferably 0.5 or more. If the degree of carboxymethyl substitution is less than 0.45, there is a risk that the solubility in water will be insufficient.
[0022] The upper limit of the degree of carboxymethyl substitution per anhydrous glucose unit of carboxymethyl cellulose and / or a salt thereof is preferably 2.0 or less, more preferably 1.5 or less.
[0023] In the present invention, the anhydroglucose unit means each anhydroglucose (glucose residue) constituting cellulose. The degree of carboxymethyl substitution (also called the degree of etherification) indicates the ratio of hydroxyl groups (-OH) in the glucose residues constituting cellulose that are substituted with carboxymethyl ether groups (-OCH2COOH). The degree of carboxymethyl substitution may be abbreviated as DS or CM-DS.
[0024] The degree of carboxymethyl substitution can be confirmed by measuring the amount of base such as sodium hydroxide required to neutralize the carboxymethyl cellulose in the sample. In this case, when the carboxymethyl ether group of the carboxymethyl cellulose and / or its salt is in the form of a salt, it is converted to carboxymethyl cellulose in advance before the measurement. In the measurement, a base, back titration using an acid, and an indicator such as phenolphthalein can be appropriately combined.
[0025] The degree of substitution of the carboxymethyl group is measured as follows: Weigh out approximately 2.0 g of sample and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of a solution of 100 mL of concentrated nitric acid in 1000 mL of methanol, and shake for 3 hours to convert carboxymethylcellulose salt (CMC) to H-CMC (hydrogen-type carboxymethylcellulose). Weigh out 1.5 to 2.0 g of the bone-dry H-CMC and place it in a 300 mL Erlenmeyer flask with a stopper. Moisten the H-CMC with 15 mL of 80% methanol, add 100 mL of 0.1 N-NaOH, and shake for 3 hours at room temperature. Using phenolphthalein as an indicator, back-titrate the excess NaOH with 0.1 N-H2SO4, and calculate the degree of carboxymethyl substitution (DS value) using the following formula. A = [(100 × F'-0.1N-H2SO4 (mL) × F) × 0.1] / (bone dry mass of H-CMC (g)) Degree of carboxymethyl substitution = 0.162 x A / (1-0.058 x A) F': Factor of 0.1N-H2SO4 F: Factor of 0.1N-NaOH
[0026] In the present invention, the carboxymethyl cellulose and / or salt thereof preferably has a viscosity of 1,000 to 20,000 mPa·s, more preferably 1,500 to 15,000 mPa·s, and even more preferably 2,000 to 10,000 mPa·s, of a 1% by mass aqueous solution measured with a Brookfield viscometer (30 rpm) at 25° C. When the viscosity is within the above range, it is difficult to settle and an electrode slurry having good coatability can be prepared, which is suitable for nonaqueous electrolyte secondary batteries.
[0027] The viscosity was measured as follows: Carboxymethylcellulose and / or its salt is weighed into a 1000 mL glass beaker and dispersed in 900 mL of distilled water to prepare an aqueous dispersion with a solid content of 1% (w / v). The aqueous dispersion is stirred at 600 rpm for 3 hours at 25°C using a stirrer. The viscosity is then measured after 3 minutes at a rotation speed of 30 rpm using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.) according to the method of JIS-Z-8803.
[0028] In addition, the carboxymethylcellulose and / or its salt is preferably such that the ratio of mass M to mass m is less than 50 ppm, where M is the dry mass of the residue on the filter when 2 liters of an aqueous solution of 0.3% by mass of the carboxymethylcellulose and / or its salt is filtered through a 250 mesh filter under reduced pressure conditions of -200 mmHg, and m is the mass of the carboxymethylcellulose and / or its salt dissolved in the aqueous solution. If the ratio is 50 ppm or more, when an electrode is formed using the carboxymethylcellulose and / or its salt, the electrode may have poor appearance such as streaks or pinholes, which may reduce the quality of the battery. There is no particular lower limit to the ratio of mass M to mass m, and the lower the ratio, the better.
[0029] (Dispersion degree) The carboxymethyl cellulose and / or salt thereof of the present invention has a degree of dispersion measured using a powder tester of 20 to 60%, preferably 25 to 55%, and more preferably 30 to 50%. When the degree of dispersion is within the above range, CMC exhibits good dispersibility when used as a binder or dispersant in a negative electrode composition, and therefore the electrical resistance value is improved.
[0030] On the other hand, if the degree of dispersion is too high, there will be a lot of dusting, and it will be impossible to dissolve a specified amount of carboxymethyl cellulose, which will reduce its function as a binder and dispersant in the negative electrode, resulting in a problem of high electrical resistance. Conversely, if the degree of dispersion is too low, it will not mix well with other materials, resulting in a problem of high electrical resistance.
[0031] The degree of dispersion was measured using a powder tester (Powder Tester PT-X (manufactured by Hosokawa Micron Corporation)). A 10 g sample was placed in the dispersion unit of the PT-X and dropped. The degree of dispersion was calculated from the amount of powder that fell onto a watch glass using the following formula. Dispersion degree (%) = (10 (g) - amount of powder dropped onto the watch glass (g)) / 10 (g)
[0032] In the present invention, the method for producing carboxymethyl cellulose and / or a salt thereof is not limited, and any known method for producing carboxymethyl cellulose and / or a salt thereof can be applied. That is, the carboxymethyl cellulose and / or a salt thereof in the present invention can be produced by treating the raw material cellulose with a mercerizing agent (alkali) to prepare mercerized cellulose (alkali cellulose), and then adding an etherifying agent to carry out an etherification reaction.
[0033] The cellulose raw material can be any of the above-mentioned celluloses without any particular limitations, but those with high cellulose purity are preferred, and dissolving pulp and linters are particularly preferred. By using these, carboxymethyl cellulose and / or a salt thereof with high purity can be obtained.
[0034] As the mercerizing agent, an alkali metal hydroxide such as sodium hydroxide, potassium hydroxide, etc. can be used. As the etherifying agent, monochloroacetic acid, sodium monochloroacetate, etc. can be used.
[0035] In the case of a general method for producing water-soluble carboxymethylcellulose, the molar ratio of the mercerizing agent to the etherifying agent is generally set to 2.00 to 2.45 when monochloroacetic acid is used as the etherifying agent. The reason is that if the molar ratio is less than 2.00, the etherification reaction may not proceed sufficiently, resulting in unreacted monochloroacetic acid remaining and generating waste, and if the molar ratio exceeds 2.45, a side reaction between the excess mercerizing agent and monochloroacetic acid may proceed, resulting in the production of an alkali metal glycolate, which may be uneconomical.
[0036] In the present invention, the carboxymethylcellulose and / or its salt may be a commercially available product, which may be used as is or after being treated as necessary. An example of a commercially available product is "Sunrose" (sodium salt of carboxymethylcellulose) manufactured by Nippon Paper Industries Co., Ltd.
[0037] [Crushing process] In the present invention, the carboxymethylcellulose and / or its salt may be the above-mentioned carboxymethylcellulose and / or its salt as it is, or may be a product that has been subjected to a pulverization treatment (a pulverized product). The pulverization treatment is usually a mechanical pulverization treatment performed using a machine. Examples of the pulverization method of carboxymethylcellulose and / or its salt include a dry pulverization method in which the cellulose is treated in a powder state, and a wet pulverization method in which the cellulose is treated in a state dispersed or dissolved in a liquid. Either of these methods may be selected in the present invention.
[0038] When an aqueous solution of carboxymethylcellulose and / or its salt is prepared, gel particles derived from carboxymethylcellulose and / or its salt remain in the aqueous solution as undissolved matter. By mechanically dry- or wet-grinding carboxymethylcellulose and / or its salt, the gel particles are made fine in the aqueous solution of the mechanically pulverized carboxymethylcellulose and / or its salt. As a result, when an electrode is formed using an aqueous solution of the mechanically pulverized carboxymethylcellulose and / or its salt, it is considered that the occurrence of streaky defects (streaks), peeling, pinholes, etc. on the surface of the electrode can be further suppressed. The grinding apparatus usable for the mechanical grinding treatment in the present invention includes the following dry grinders and wet grinders.
[0039] Dry grinding machines include cutting mills, impact mills, airflow mills, and media mills. These can be used alone or in combination, and can be used in several stages with the same model, but airflow mills are preferred.
[0040] Examples of cutting type mills include Mesh Mill (manufactured by Horai Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Seisakusho Co., Ltd.), Knife Mill (manufactured by Parman Co., Ltd.), Granulator (manufactured by Herbolt Co., Ltd.), Rotary Cutter Mill (manufactured by Nara Machinery Co., Ltd.), and the like.
[0041] Examples of impact mills include Pulperizer (manufactured by Hosokawa Micron Corporation), Fine Impact Mill (manufactured by Hosokawa Micron Corporation), Super Micron Mill (manufactured by Hosokawa Micron Corporation), Sample Mill (manufactured by Seishin Corporation), Bantam Mill (manufactured by Seishin Corporation), Atomizer (manufactured by Seishin Corporation), Tornado Mill (Nikkiso Co., Ltd.), Turbo Mill (Turbo Kogyo Co., Ltd.), and Bevel Impactor (Aikawa Iron Works Co., Ltd.).
[0042] Examples of airflow mills include a CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), a jet mill (manufactured by Sansho Industry Co., Ltd.), an Ebara jet micronizer (manufactured by Ebara Corporation), a selenium mirror (manufactured by Masuko Sangyo Co., Ltd.), and a supersonic jet mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.). An example of the media mill is a vibrating ball mill.
[0043] Examples of the wet grinding machine include a Masscolloider (manufactured by Masuko Sangyo Co., Ltd.), a high pressure homogenizer (manufactured by Sanmaru Kikai Kogyo Co., Ltd.), and a media mill. Examples of the media mill include a bead mill (manufactured by Imex Co., Ltd.).
[0044] [Particle size of carboxymethyl cellulose] In the present invention, the particle size of carboxymethylcellulose and / or its salt is preferably small. That is, the value of the volume cumulative 100% particle size measured by a laser diffraction / scattering type particle size distribution analyzer using methanol as a dispersion medium (hereinafter, sometimes referred to as "maximum particle size") is preferably less than 100 μm, more preferably less than 50 μm, and even more preferably less than 45 μm. If the maximum particle size of carboxymethylcellulose and / or its salt is too large, the amount of undissolved matter in the aqueous solution of carboxymethylcellulose and / or its salt tends to increase.
[0045] In the present invention, the carboxymethylcellulose and / or salt thereof may be granulated. This makes it easier to handle. Although the maximum particle size of the carboxymethylcellulose and / or salt thereof may be greater than or equal to the above-mentioned value by granulation, the maximum particle size of the carboxymethylcellulose and / or salt thereof before granulation is preferably less than the above-mentioned value. The lower limit of the maximum particle size is not particularly limited. The smaller the value, the better, and it is sufficient if it exceeds 0.
[0046] The particle size of carboxymethylcellulose and / or its salt at 50% cumulative volume (hereinafter referred to as the average particle size) measured by a laser diffraction / scattering type particle size distribution analyzer using methanol as a dispersion medium is usually 30 μm or less, preferably 20 μm or less, and more preferably 15 μm or less. The lower limit of the average particle size is not particularly limited, but is usually 5 μm or more, preferably 10 μm or more, and more preferably 12 μm or more.
[0047] In the present invention, carboxymethylcellulose and / or a salt thereof can be classified based on the particle size (preferably the maximum particle size). Classification refers to a process of sieving particles to be classified into those having a particle size equal to or larger than a certain size and those having a particle size smaller than the certain size.
[0048] The classification is preferably carried out based on whether the maximum particle size is less than the above value or equal to or greater than the above value, thereby making it possible to selectively collect carboxymethylcellulose and / or a salt thereof having a maximum particle size less than the above value.
[0049] When a ground product of carboxymethyl cellulose and / or a salt thereof is used as the carboxymethyl cellulose and / or a salt thereof, the timing of the above-mentioned classification is not particularly limited, and the classification may be carried out during the grinding process or after the completion of the grinding process.
[0050] The classification method may be a known method, such as a method using a dry classifier or a wet classifier. Examples of dry classifiers include a cyclone classifier, a DS separator, a turbo classifier, a microseparator, and an air separator. On the other hand, examples of wet classifiers include a liquid cyclone type classifier, a centrifugal settler, and a hydrosilator. Among these, a dry classifier is preferred, and a cyclone classifier is more preferred.
[0051] <Electrode active material> Examples of the electrode active material include a negative electrode active material and a positive electrode active material. Examples of the negative electrode active material include graphite materials such as graphite (natural graphite, artificial graphite), coke, and carbon fiber; compounds containing elements capable of forming an alloy with lithium, i.e., elements such as Al, Si, Sn, Ag, Bi, Mg, Zn, In, Ge, Pb, and Ti; composites of the elements and compounds capable of forming an alloy with lithium, and carbon and / or the graphite materials; and nitrides containing lithium. Among these, graphite materials and / or silicon-based compounds are preferred, more preferably graphite and / or silicon-based compounds are included, and it is preferred to include at least a silicon-based compound.
[0052] The positive electrode active material is LiMe x O y (Me means a transition metal including at least one of Ni, Co, and Mn. x and y are arbitrary numbers.)-based positive electrode active materials are preferred. x O yThe positive electrode active material of the LiMn2O4 system is not particularly limited, but LiMn2O4 system, LiCoO2 system, LiNiO2 system positive electrode active material is preferable. For example, LiMn2O4 system, LiCoO2 system, LiNiO2 system positive electrode active material is a compound in which various metal elements are substituted with LiMnO2, LiMn2O4, LiCoO2, LiNiO2 as a main skeleton. Since LiMn2O4 system, LiCoO2 system, LiNiO2 system positive electrode active material has excellent performance as a positive electrode active material such as excellent diffusion performance of electrons and lithium ions, a lithium ion secondary battery having high charge and discharge efficiency and good cycle characteristics can be obtained. Among them, LiCoO2 system positive electrode active material is preferable, and LiCoO2 is more preferable. On the other hand, it is preferable to use LiMn2O4 system positive electrode active material from the viewpoint of low material cost.
[0053] Furthermore, it is preferable to use a conductive material in addition to the electrode active material. When the electrode composition contains a conductive material, the properties of the electrode to be manufactured are improved. In addition, the conductive material can ensure the electrical conductivity of the electrode. Examples of the conductive material include a mixture of one or more carbon materials such as carbon black, acetylene black, and graphite. Of these, carbon black is preferable. The timing of adding the conductive material is not particularly limited, but it is preferable to mix it in the first mixing step.
[0054] (Second mixing process) In the second mixing step of the method for producing an electrode composition of the present invention, a saturated lithium carboxylate or borate having 6 or less carbon atoms is mixed with the mixture obtained in the first mixing step. By mixing the saturated lithium carboxylate or borate having 6 or less carbon atoms in this order, it is possible to suppress variation in battery characteristics such as the capacity retention rate of the obtained nonaqueous electrolyte secondary battery. The mixing method in the second mixing step is not particularly limited, and known devices and known techniques can be used.
[0055] <Lithium salts of saturated carboxylic acids or borates having 6 or less carbon atoms> In the present invention, it is important to mix a lithium salt of a saturated carboxylate or a borate having 6 or less carbon atoms in the second mixing step.
[0056] In the present invention, the lithium salt of a saturated carboxylate having 6 or less carbon atoms refers to a lithium salt of an aliphatic hydroxy acid, aromatic hydroxy acid, saturated fatty acid, dicarboxylic acid, tricarboxylic acid, or the like having 6 or less carbon atoms, and more preferably a lithium salt of an aliphatic hydroxy acid having 6 or less carbon atoms. Examples of such an aliphatic hydroxy acid include lithium salts of citric acid, malic acid, gluconic acid, succinic acid, and the like, and among these, lithium citrate is more preferable.
[0057] When such a lithium salt of a saturated carboxylic acid having 6 or less carbon atoms is used as an electrode binder together with carboxymethyl cellulose, the hydroxyl or carboxyl group in the saturated carboxylic acid having 6 or less carbon atoms forms a crosslinked structure through hydrogen bonds with the carboxyl group of carboxymethyl cellulose. This crosslinked structure contains more hydroxyl and carboxyl groups in the molecule than carboxymethyl cellulose alone, so it is highly reactive with the negative electrode material such as SiOx dispersed in the negative electrode slurry through hydrogen bonds. As a result, a stable oxide film can be formed on the surface of the negative electrode material such as SiOx, decomposition of the electrolyte is suppressed, and the SEI film (Solid Electrolyte Interface) on the electrode surface does not become excessively thick, which is presumably linked to improved battery characteristics.
[0058] Here, by using a saturated carboxylic acid having 6 or less carbon atoms as a lithium salt, the saturated carboxylic acid can exhibit neutrality or weak alkalinity when added to the electrode composition. If the saturated carboxylic acid is not in the form of a lithium salt, the electrode composition in the form of an aqueous solution becomes strongly acidic, which is undesirable because it reduces the viscosity of the electrode composition and causes uneven polarity distribution, which can lead to unevenness when the electrode composition is applied to the current collector. Furthermore, by using a saturated carboxylic acid having 6 or less carbon atoms as a lithium salt, the amount of impurities mixed in is reduced when using a lithium-based active material, making it easier to exhibit electrical performance.
[0059] In addition, examples of the borate salt in the present invention include potassium borate salt, sodium borate salt, calcium borate salt, lithium borate salt, etc. Among these, sodium borate salt and lithium borate salt are preferred.
[0060] When such a borate is used as an electrode binder together with carboxymethylcellulose, the hydroxyl group in the borate forms a crosslinked structure with the carboxyl group of the carboxymethylcellulose via hydrogen bonding. This crosslinked structure has a stronger binder than carboxymethylcellulose alone, so it is believed that the structural destruction of the coating layer caused by the expansion and contraction of the active material during charging and discharging can be suppressed, leading to improved battery characteristics.
[0061] In addition, when a lithium borate salt is used, boric acid can exhibit neutrality or weak alkalinity when added to an electrode binder. If boric acid is not in the form of a lithium salt, the electrode composition in the form of an aqueous solution becomes strongly acidic, which is undesirable because it reduces the viscosity of the electrode composition and causes uneven polarity distribution, which can lead to unevenness when the electrode composition is applied to a current collector. Furthermore, since boric acid is a lithium salt, impurities are less likely to be mixed in when using a lithium-based active material, making it easier to demonstrate electrical performance. When using a saturated lithium carboxylate having 6 or less carbon atoms, it is preferable that the following condition (I) or (II) is satisfied.
[0062] Condition (I): When the degree of carboxymethyl substitution of carboxymethyl cellulose and / or a salt thereof is 0.45 or more and 1.0 or less, the saturated lithium carboxylate having 6 or less carbon atoms is contained in an amount of 1 to 100 parts by weight per 100 parts by weight of carboxymethyl cellulose and / or a salt thereof.
[0063] Condition (II): When the degree of carboxymethyl substitution of the carboxymethyl cellulose and / or a salt thereof exceeds 1.0, the saturated lithium carboxylate having 6 or less carbon atoms is contained in an amount of 1 to 200 parts by weight per 100 parts by weight of the carboxymethyl cellulose and / or a salt thereof.
[0064] When the degree of carboxymethyl substitution of carboxymethyl cellulose and / or its salt is high, the number of crosslinking points in the carboxymethyl cellulose increases, so that aggregation does not occur even if the amount of the saturated lithium carboxylate having 6 or less carbon atoms added is increased.
[0065] Therefore, when the carboxymethyl cellulose and / or a salt thereof is a carboxymethyl cellulose and / or a salt thereof having a degree of carboxymethyl substitution of 0.45 or more and 1.0 or less, the saturated lithium carboxylate having 6 or less carbon atoms is preferably contained in an amount of 1 to 100 parts by weight, more preferably 1 to 80 parts by weight, and even more preferably 10 to 50 parts by weight, relative to 100 parts by weight of the carboxymethyl cellulose and / or a salt thereof.
[0066] Furthermore, when the carboxymethyl cellulose and / or a salt thereof has a degree of carboxymethyl substitution of more than 1.0, the saturated carboxylic acid lithium salt having 6 or less carbon atoms is preferably contained in a range of 1 to 200 parts by weight, more preferably 1 to 180 parts by weight, even more preferably 10 to 150 parts by weight, and particularly preferably more than 100 parts by weight and up to 150 parts by weight of the saturated carboxylic acid lithium salt having 6 or less carbon atoms, relative to 100 parts by weight of the carboxymethyl cellulose and / or a salt thereof.
[0067] It is presumed that when the blending ratio is within the above range, the formation of a crosslinked structure between the carboxymethyl cellulose and / or a salt thereof and the lithium salt of a saturated carboxylate having 6 or less carbon atoms occurs more effectively.
[0068] When a borate is used, the borate is preferably contained in the range of 0.1 to 20% by mass, more preferably 0.5 to 15% by mass, and even more preferably 1 to 10% by mass, relative to the carboxymethylcellulose and / or its salt. When the blending ratio is within this range, it is presumed that the formation of the crosslinked structure between the carboxymethylcellulose and the borate occurs more effectively.
[0069] In the present invention, the content of carboxymethyl cellulose and / or a salt thereof in the electrode composition is preferably 0.1 to 4.0% by mass based on the total amount of the electrode composition.
[0070] The content of the active material in the electrode composition is usually 90 to 99 mass %, preferably 91 to 99 mass %, and more preferably 92 to 99 mass %.
[0071] The electrode composition may contain a binder other than the aqueous solution of carboxymethyl cellulose and / or its salt (hereinafter, sometimes referred to as "other binder"). In the case of the electrode composition for the negative electrode, an example of the binder is a synthetic rubber-based binder. As the synthetic rubber-based binder, one or more selected from the group consisting of styrene butadiene rubber (SBR), nitrile butadiene rubber, methyl methacrylate butadiene rubber, chloroprene rubber, carboxy-modified styrene butadiene rubber, and latexes of these synthetic rubbers can be used. Among these, styrene butadiene rubber (SBR) is preferred.
[0072] When SBR is used, the average particle size (D50) of SBR is preferably 50 to 300 nm, more preferably 50 to 200 nm. If the average particle size (D50) of SBR is too large, the SBR does not adhere uniformly to the active material, and the binder function is reduced, resulting in a problem of high electrical resistance. If the average particle size (D50) of SBR is too small, the SBR covers the active material, resulting in a problem of high electrical resistance.
[0073] The glass transition temperature (Tg) of SBR is preferably −50° C. to 50° C. When the SBR is within the above range, it mixes well with the carboxymethyl cellulose and / or a salt thereof of the present invention and has appropriate flexibility when used in the negative electrode layer, so that the electrical resistance is unlikely to become high.
[0074] In addition, examples of binders for the electrode composition for the positive electrode include the synthetic rubber binders listed as the binders for the negative electrode, as well as polytetrafluoroethylene (PTFE), of which polytetrafluoroethylene (PTFE) is preferred. The timing of adding the other binders is not particularly limited, but it is preferred to add them after the second mixing step.
[0075] The content of other binders in the electrode composition is usually 1 to 10 mass %, preferably 1 to 6 mass %, and more preferably 1 to 2 mass %.
[0076] The form of the electrode composition is not particularly limited, and may be any of a liquid, a paste, a slurry, and the like.
[0077] The electrode composition for non-aqueous electrolyte secondary batteries produced by the production method of the present invention can also contain other components constituting the electrode composition, as long as the effects of the present invention are not impaired. Examples of such additive components include inorganic salts that are cationized in an aqueous solution. The presence of cations reinforces the crosslinked structure of carboxymethyl cellulose, so that excellent effects can be exhibited in terms of electrical properties. As such cations, cations such as monovalent, divalent, and trivalent cations can be appropriately used, and specifically, those containing Fe ions and the like are preferred. The timing of adding other components constituting the electrode composition is not particularly limited as long as the effects of the present invention are not impaired.
[0078] The electrode composition is used in the manufacture of an electrode for a non-aqueous electrolyte secondary battery. The electrode for a non-aqueous electrolyte secondary battery may be manufactured by a method of laminating the electrode composition on a current collecting substrate (current collector). Examples of the lamination method include blade coating, bar coating, and die coating, and blade coating is preferred. For example, in the case of blade coating, a method of casting the electrode composition on a current collecting substrate using a coating device such as a doctor blade is exemplified. In addition, the lamination method is not limited to the above specific example, and a method of discharging the electrode composition from an extrusion type injector having a slot nozzle onto a current collecting substrate wound around a backup roll and running is also exemplified. In blade coating, after casting, drying by heating (for example, 80 to 120°C, heating time, for example, 4 to 12 hours) or pressurization by roll press or the like may be performed as necessary. The current collecting substrate may be any electrical conductor that will not undergo a detrimental chemical reaction in the assembled battery.
[0079] As the current collecting substrate for the negative electrode, stainless steel, nickel, copper, titanium, carbon, copper, or the above-mentioned stainless steel surface treated with carbon, nickel, titanium or silver can be used. Among these, copper or a copper alloy is preferable, and copper is most preferable.
[0080] Examples of materials for the current collecting substrate for the positive electrode include metals such as aluminum and stainless steel, with aluminum being preferred. The shape of the current collecting substrate may be a mesh, punched metal, foam metal, or foil processed into a plate shape, with foil processed into a plate shape being preferred.
[0081] The shape of the electrode for a non-aqueous electrolyte secondary battery formed from the electrode composition is not particularly limited, but is usually a sheet. The thickness of the sheet-shaped electrode plate (the thickness of the mixture layer formed from the electrode composition, excluding the current collecting substrate portion) is difficult to define uniquely because it is appropriately selected depending on the composition of the composition and the manufacturing conditions, but is usually 30 to 150 μm.
[0082] The electrode formed from the composition is used as an electrode for a non-aqueous electrolyte secondary battery. That is, the present invention includes an electrode formed from the composition, and a non-aqueous electrolyte secondary battery can be manufactured using the electrode. The non-aqueous electrolyte secondary battery can have a structure in which positive electrodes and negative electrodes are alternately stacked with separators interposed therebetween and wound many times. The separator is usually impregnated with a non-aqueous electrolyte.
[0083] The negative electrode and / or positive electrode may be formed from the electrode composition described above. Such a nonaqueous electrolyte secondary battery uses carboxymethyl cellulose and / or a salt thereof, which has excellent solubility, and can omit a process such as filtration using a filter, so that it is excellent in productivity, has a significantly improved initial irreversible capacity, and exhibits high battery characteristics. EXAMPLES
[0084] Hereinafter, the present invention will be described in detail with reference to examples, but the present invention is not limited thereto.
[0085] In the present examples and comparative examples, the indices of carboxymethylcellulose and / or its salts are measured by the following methods.
[0086] <Method for measuring the degree of carboxymethyl substitution (CM-DS)> Approximately 2.0 g of the carboxymethylcellulose crushed sample was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 100 mL of methanol (1000 mL of methanol plus 100 mL of concentrated nitric acid) was added and shaken for 3 hours to convert the carboxymethylcellulose salt (CMC salt) to H-CMC (carboxymethylcellulose). 1.5 to 2.0 g of bone-dried H-CMC was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. The H-CMC was moistened with 15 mL of 80% methanol, 100 mL of 0.1 N NaOH was added, and the mixture was shaken at room temperature for 3 hours. Excess NaOH was back-titrated with 0.1 N H2SO4 using phenolphthalein as an indicator. CM-DS was calculated using the following formula 1. (Formula 1) A = [(100 x F - (0.1N H2SO4 (mL)) x F') x 0.1] / (bone dry weight of H-CMC (g)) Carboxymethyl substitution degree (CM-DS) = 0.162 x A / (1-0.058 x A) A: The amount of 1N NaOH required to neutralize 1g of H-CMC (mL) F': Factor of 0.1N H2SO4 F: Factor of 0.1N NaOH
[0087] <Viscosity> Carboxymethylated cellulose or its salt was weighed into a 1000 mL glass beaker and dispersed in 900 mL of distilled water to prepare an aqueous dispersion with a solid content of 1% (w / v). The aqueous dispersion was stirred at 600 rpm for 3 hours at 25°C using a stirrer. The viscosity after 3 minutes was then measured using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.) with a No. 1 rotor at a rotation speed of 30 rpm in accordance with the method of JIS-Z-8803.
[0088] <Dispersion> The degree of dispersion of the carboxymethyl cellulose and / or its salt used in the examples and comparative examples was measured using a powder tester (Powder Tester PT-X, manufactured by Hosokawa Micron Corp.) Specifically, when 10 g of a sample was placed in the dispersion unit of the PT-X and dropped, the degree of dispersion was calculated from the amount of powder that fell onto a watch glass according to the following formula. Dispersion degree (%) = (10 (g) - amount of powder dropped onto the watch glass (g)) / 10 (g)
[0089] <Measurement of the mass ratio of the mass of the filtration residue to the dry mass of carboxymethyl cellulose dissolved in an aqueous solution> 2 liters of an aqueous solution of 0.3% by mass (mass % based on the dry mass of carboxymethyl cellulose or its salt) of carboxymethyl cellulose and / or its salt was prepared. 2 liters of this aqueous solution was filtered through a 250 mesh filter (stainless steel, 63 μm mesh) using a filter ("Separoth", Kiriyama Seisakusho) under reduced pressure conditions of -200 mmHg. The residue remaining on the 250 mesh filter was dried by blowing air at a temperature of 105°C for 16 hours, and the mass of the dried residue was measured and expressed as a mass percent (ppm) relative to the mass of carboxymethyl cellulose in the aqueous carboxymethyl cellulose solution. In the examples and comparative examples, the batteries were evaluated as follows.
[0090] <Battery evaluation> (Discharge capacity (charge / discharge rate test)) The charge and discharge rate test of the coin-type non-aqueous electrolyte secondary batteries obtained in the Examples and Comparative Examples was carried out using Nagano Corporation's BTS2004 in a thermostatic chamber at 25° C., with 52 cycles being performed, with one cycle being a charge and discharge cycle in that order, using the coin-type non-aqueous electrolyte secondary batteries. Note that the charging conditions were constant current constant voltage (CC-CV) (CC current 0.2C, CV voltage 4.2V, final current 0.02C) in all cycles.
[0091] As a condition for the discharge treatment, the final voltage was set to 3.0 V. In the first cycle, the discharge treatment was performed at a constant current of 0.2 C, and the discharge capacity (mAh / g) after one cycle was measured. After that, up to the 52nd cycle, the constant current for the discharge treatment was set as follows, and the discharge capacity (mAh / g) was measured after each cycle of discharge. [Constant current for discharge treatment in each cycle] 2 to 10 cycles: Discharge treatment at a constant current of 0.2C 11 to 20 cycles: constant current 1C for discharge treatment 21 cycles: Discharge treatment at constant current of 0.2C 22 to 31 cycles: constant current 2C for discharge treatment 32 cycles: Discharge treatment at constant current of 0.2C 33 - 42 cycles: Constant current 3C for discharge treatment 43 - 52 cycles: Constant current 0.2C for discharge treatment
[0092] (Capacity retention rate) The capacity retention rate is calculated from the discharge capacity (mAh / g) in each of the above - mentioned cycle tests as follows: "Capacity retention rate = Discharge capacity (mAh / g) after 1 cycle / Discharge capacity (mAh / g) after 52 cycles × 100" using the above formula. In addition, for the coin - type non - aqueous electrolyte secondary batteries manufactured in the examples and comparative examples, the average value, standard deviation, and coefficient of variation of the capacity retention rate were determined.
[0093] (Preparation of CMC) The CMC used in the examples and comparative examples was prepared according to the following Production Examples 1 and 2. (Production Example 1) To a twin - screw kneader with the rotation speed adjusted to 100 rpm, 2720 g of isopropyl alcohol, 170 g of sodium monochloroacetate, and a solution of 58 g of sodium hydroxide dissolved in 480 g of water were added, and 160 g of lint pulp was charged based on the dry weight when dried at 30 °C for 60 minutes. After stirring and mixing at 30 °C for 90 minutes to prepare mercerized cellulose, the temperature was raised to 70 °C and carboxymethylation reaction was carried out for 90 minutes. After the reaction was completed, it was neutralized with acetic acid to a pH of about 7, de - liquidified, dried, and pulverized to obtain sodium carboxymethyl cellulose with a degree of carboxymethyl substitution of 0.70, a viscosity of 7,900 mPa·s for a 1 mass% aqueous solution measured with a B - type viscometer at 25 °C, and a filtration residue of 48 ppm with respect to the dry mass of carboxymethyl cellulose dissolved in the aqueous solution (hereinafter sometimes referred to as "CMC1"). Also, the degree of dispersion of CMC1 was 36.1%.
[0094] (Production Example 2) In a twin-shaft kneader adjusted to 100 rpm, 1000 g of isopropyl alcohol, 240 g of sodium monochloroacetate, and 83 g of sodium hydroxide dissolved in 120 g of water were added, and 160 g of linter pulp was added based on the dry weight after drying at 30°C for 60 minutes. Mercerized cellulose was prepared by stirring and mixing for 90 minutes at 30°C, and then the temperature was raised to 70°C and carboxymethylation reaction was carried out for 90 minutes. After the reaction was completed, the mixture was neutralized with acetic acid to about pH 7, deliquored, dried, and pulverized to obtain a sodium salt of carboxymethylcellulose (hereinafter sometimes referred to as "CMC2") with a carboxymethyl substitution degree of 1.34, a viscosity of a 1% by mass aqueous solution measured with a B-type viscometer at 25°C of 4,220 mPa·s, and a filtration residue of 46 ppm relative to the dry mass of carboxymethylcellulose dissolved in the aqueous solution. The dispersion degree of CMC2 was 16.3%.
[0095] <Preparation of electrode composition> In the examples and comparative examples, electrode compositions were prepared by the following method 1 or method 2.
[0096] (Method 1) In method 1, an electrode composition was prepared by carrying out the following steps (1) to (4) in order. (1) An electrode binder 1 was prepared having a solid concentration of 1% trilithium citrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.; hereinafter, sometimes referred to as "Li citrate") and a solid concentration of 2% CMC. (2) 100 parts of SiOx as a negative electrode active material were mixed with 0.5 parts of acetylene black (manufactured by Stream Chemical Co.), 1 part of CMC in the electrode binder 1 prepared above in terms of solid content, and 0.5 parts of lithium citrate in terms of solid content, and the mixture was stirred. (3) Water was added to the mixture obtained in (2) so that the final slurry concentration was 45.6%, and the mixture was stirred. (4) To the slurry obtained in (3), 1.5 parts of SBR (manufactured by ENEOS Materials Corporation, product number TRD-104A) was added and stirred so as to be 100 parts of SiOx, thereby obtaining an electrode composition.
[0097] <Method 2> In method 2, an electrode composition was prepared by carrying out the following steps (1) to (4) in order. (1) Electrode binder 2 having a CMC solids concentration of 2% was prepared. (2) 100 parts of SiOx as a negative electrode active material were mixed with 0.5 parts of acetylene black (manufactured by Stream Chemical Co.) and 1 part of CMC in the electrode binder 2 prepared above in terms of solid content, and the mixture was stirred. (3) To the mixture obtained in (2), a 35 wt % aqueous solution of lithium citrate was further added and stirred so that the solid content of lithium citrate was 0.5 parts per 100 parts of SiOx and the final slurry concentration was 45.6%. (4) To the slurry obtained in (3), 1.5 parts of SBR (manufactured by ENEOS Materials Corp., product number TRD-104A) was added and stirred so as to be 100 parts of SiOx, thereby obtaining an electrode composition.
[0098] <Preparation of coin-type non-aqueous electrolyte secondary battery> The electrode composition obtained by method 1 or method 2 was applied to a copper foil (manufactured by Furukawa Electric Co., Ltd., NC-WS) measuring 320 mm in length, 170 mm in width, and 17 μm in thickness using an applicator, and then air-dried for 30 minutes, and then dried in a dryer at 60° C. for 30 minutes. The composition was then pressed using a small tabletop roll press (manufactured by Tester Sangyo Co., Ltd., SA-602) under conditions of 5 kN and a roll peripheral speed of 50 m / min to obtain a coating weight of 19.7 g / m 2 Thus, a negative electrode plate with an effective discharge capacity of 2100 mAh / g was obtained.
[0099] The negative electrode plate obtained above and a LiCoO2 positive electrode plate (manufactured by Hosensha, basis weight 110.2 g / m 2 The negative and positive electrode plates were then vacuum dried at 120° C. for 12 hours.
[0100] Similarly, a separator (manufactured by CS Tech, a polypropylene separator having a thickness of 20 μm) was punched out to have a diameter of 17 mm, and vacuum dried at 60° C. for 12 hours.
[0101] Then, the negative electrode plate 1 was placed in a stainless steel circular dish-shaped container with a diameter of 20.0 mm, and then a separator, a positive electrode plate, a spacer (diameter 15.5 mm, thickness 1 mm), and a stainless steel washer (manufactured by Hosen Co., Ltd.) were stacked in this order, and then 300 μL of electrolyte (1 mol / L LiPF6, ethylene carbonate and diethyl carbonate volume ratio 1:1) was added to the circular dish-shaped container. A stainless steel cap was placed over this via a polypropylene packing, and the container was sealed with a coin battery crimping machine (Hosen Co., Ltd.) to obtain a coin-shaped nonaqueous electrolyte secondary battery.
[0102] The electrode compositions and coin-type nonaqueous electrolyte secondary batteries in the examples and comparative examples were prepared as follows.
[0103] (Example 1: T4 to T7) An electrode composition was prepared by using CMC1 as the CMC and by method 2. In addition, a coin-type nonaqueous electrolyte secondary battery was prepared by using this electrode composition according to the above-mentioned procedure.
[0104] (Example 2: T12 to T15) An electrode composition was prepared by using CMC2 as the CMC and by method 2. In addition, a coin-type nonaqueous electrolyte secondary battery was prepared by using this electrode composition according to the above-mentioned procedure.
[0105] (Comparative example 1: T2~T3) An electrode composition was prepared by using CMC1 as the CMC and by method 1. In addition, a coin-type nonaqueous electrolyte secondary battery was prepared by using this electrode composition according to the above-mentioned procedure.
[0106] (Comparative Example 2: T8 to T11) An electrode composition was prepared using CMC2 as the CMC by method 1. In addition, a coin-type nonaqueous electrolyte secondary battery was prepared using this electrode composition according to the above-mentioned procedure.
[0107] (Example: T1) An electrode composition was prepared according to the procedure of Method 2, except that CMC1 was used as the CMC and water was added instead of the Li citrate aqueous solution in (3) of Method 2. In addition, a coin-type nonaqueous electrolyte secondary battery was prepared using this electrode composition according to the above procedure. The results of Examples 1 and 2, Comparative Examples 1 and 2, and the Reference Example are shown in Table 1 below.
[0108] [Table 1]
[0109] As shown in Table 1, in preparing the electrode composition, Example 1 (T4 to T7) and Example 2 (T12 to T15), in which Method 2 was used, had smaller standard deviations and coefficients of variation in the capacity retention rates, indicating less variation, compared to Comparative Example 1 (T2 to T3) and Comparative Example 2 (T12 to T15), in which Method 1 was used.
Claims
1. A first mixing step of mixing carboxymethylcellulose and / or a salt thereof having a carboxymethyl substitution degree per anhydrous glucose unit of 0.45 or more with an electrode active material; a second mixing step of mixing a lithium salt of a saturated carboxylic acid having 6 or less carbon atoms or a borate salt of the saturated carboxylic acid having 6 or less carbon atoms with the mixture obtained in the first mixing step; The method for producing an electrode composition for a non-aqueous electrolyte secondary battery comprises the steps of:
2. 2. The method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to claim 1, wherein the lithium salt of a saturated carboxylic acid having 6 or less carbon atoms includes at least a lithium citrate salt.
3. 3. The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to claim 1, wherein the following condition (I) is satisfied: Condition (I): When the degree of carboxymethyl substitution of the carboxymethyl cellulose and / or its salt is 0.45 or more and 1.0 or less, The saturated carboxylic acid lithium salt having 6 or less carbon atoms is contained in an amount in the range of 1 to 100 parts by weight per 100 parts by weight of the carboxymethyl cellulose and / or its salt.
4. 3. The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to claim 1, wherein the following condition (II) is satisfied: Condition (II): When the degree of carboxymethyl substitution of the carboxymethyl cellulose and / or its salt is more than 1.0, The saturated carboxylic acid lithium salt having 6 or less carbon atoms is contained in an amount of 1 to 200 parts by weight per 100 parts by weight of the carboxymethyl cellulose and / or its salt.
5. 2. The method for producing an electrode composition for a non-aqueous electrolyte secondary battery in accordance with claim 1, wherein the borate comprises at least one selected from the group consisting of sodium borate and lithium borate.
6. 6. The method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to claim 1, wherein the borate is contained in an amount of 0.1 to 20 parts by weight per 100 parts by weight of the solid content of the carboxymethyl cellulose and / or the salt thereof.
7. 3. The method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to claim 1, wherein the degree of dispersion of the carboxymethyl cellulose and / or the salt thereof as measured using a powder tester is 20 to 60%.
8. 3. The method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to claim 1, wherein when 2 L of a 0.3 mass % aqueous solution of the carboxymethyl cellulose or salt thereof having a dry mass B is prepared, the whole is filtered through a 250 mesh filter under a reduced pressure condition of -200 mmHg, and the dry mass A of the residue on the filter after filtration is measured, the ratio of the dry mass A to the dry mass B is less than 50 ppm.
9. The method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein the carboxymethyl cellulose and / or the salt thereof is a product that has been mechanically ground.
10. The method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein the electrode active material contains a silicon-based compound.
11. A method for producing an electrode for a non-aqueous electrolyte secondary battery, comprising the step of forming an electrode using the electrode composition for a non-aqueous electrolyte secondary battery produced by the method for producing an electrode composition for a non-aqueous electrolyte secondary battery according to claim 1 or 2.
12. A method for producing a nonaqueous electrolyte secondary battery, comprising the step of producing a nonaqueous electrolyte secondary battery using the electrode composition for a nonaqueous electrolyte secondary battery produced by the method for producing an electrode composition for a nonaqueous electrolyte secondary battery according to claim 1 or 2.
Citation Information
Patent Citations
Secondary battery negative electrode
JP1993074461A
Method of manufacturing electrode for lithium battery and electrode for lithium battery
JP2003157847A