Power storage device and exterior material for power storage device
The exterior material for all-solid-state batteries uses a colored adhesive to define adhesive-coated and uncoated areas, enabling precise opening formation and improving cooling performance by exposing the gas barrier layer, thus addressing gas leakage and cooling challenges.
Patent Information
- Application Number
- JP2023086465
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional all-solid-state batteries face challenges in accurately forming openings in the sealant layer with dimensional accuracy due to difficulties in determining the boundary between areas where the sealant layer is removed and where it remains, leading to potential gas leakage and inadequate cooling performance.
The exterior material for all-solid-state batteries is designed with a base material layer, a metal foil layer, a gas barrier layer, and a sealant layer, where the sealant layer has openings exposed to the gas barrier layer, and uses a colored adhesive in the adhesive layer to clearly distinguish adhesive-coated and uncoated areas, enabling precise opening formation.
This design allows for highly accurate opening formation in the sealant layer, preventing gas leakage and enhancing cooling performance by ensuring efficient heat dissipation and insulation, while also allowing for a thinner battery design.
Smart Images

Figure 2024169201000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electricity storage device such as an all-solid-state battery used as a high-power battery such as an in-vehicle battery, a battery for portable devices such as a mobile electronic device, or a battery for storing regenerative energy, and an exterior material for the electricity storage device. [Background technology]
[0002] All-solid-state batteries use solid electrolytes, so there is no risk of electrolyte leakage or dendrites, and the separator is not damaged. Therefore, there is no risk of fire caused by separator damage, and so they are attracting a lot of attention from the perspective of safety.
[0003] A typical all-solid-state battery is configured by sealing an all-solid-state battery body, such as an electrode active material and a solid electrolyte, inside an exterior material serving as a casing. As research into solid electrolytes in this all-solid-state battery progresses, it has gradually become apparent that the performance required of the exterior material differs from that of exterior materials for batteries using conventional liquid electrolytes, and various exterior materials have been proposed to satisfy the performance requirements for all-solid-state batteries.
[0004] The exterior material for an all-solid-state battery has a basic structure including a metal foil layer and a heat-sealing layer (sealant layer) laminated on the inside of the metal foil layer, and the all-solid-state battery body is encapsulated by heat-sealing the sealant layer.
[0005] For example, the all-solid-state battery packaging material shown in Patent Document 1 below has a protective film interposed between a metal foil layer and a sealant layer, and uses a sealant layer with high hydrogen sulfide gas permeability. Furthermore, the all-solid-state battery packaging material shown in Patent Document 2 uses a sealant layer with low hydrogen sulfide gas permeability. Furthermore, the all-solid-state battery packaging material shown in Patent Document 3 uses a sealant layer that absorbs gas. Furthermore, the all-solid-state battery packaging material shown in Patent Document 4 is configured by laminating a vapor deposition film layer on the inner surface of the sealant layer.
[0006] However, the conventional all-solid-state batteries have a problem in that gases such as hydrogen sulfide gas generated by a reaction between the solid electrolyte and moisture may leak.
[0007] On the other hand, in all-solid-state batteries, the exchange of electrons (ions) occurs through the solid electrolyte during charging and discharging, so the resistance value is higher and the amount of heat generated is greater than that of liquid electrolytes. However, it is believed that the performance of all-solid-state batteries is not affected even in high-temperature environments, and the current situation is that no consideration has been given to high-temperature countermeasures (cooling properties) including those in the above Patent Documents 1 to 4. However, as battery technology advances toward higher output and higher capacity, it is fully predicted that in the future, improved cooling properties will also be required for all-solid-state batteries.
[0008] Therefore, the applicant of the present application has proposed an all-solid-state battery capable of preventing leakage of hydrogen sulfide gas and the like while ensuring sufficient cooling performance, as disclosed in Patent Document 5 below.
[0009] In this all-solid-state battery, the exterior material is configured by sequentially laminating a metal foil layer, a gas barrier layer, and a sealant layer on the inner surface side of a base layer, and an opening is formed in the sealant layer to expose the gas barrier layer to the inside. In this all-solid-state battery, the gas barrier layer prevents leakage of hydrogen sulfide gas and the like, while the opening is formed to improve cooling performance.
[0010] In this all-solid-state battery, an opening is formed by removing a part (a portion to be opened) of the sealant layer in the packaging material sheet in which the sealant layer is laminated over the entire inner surface of the gas barrier layer. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Patent No. 6777276 [Patent Document 2] Patent No. 6747636 [Patent Document 3] Patent Publication No. 2020-187855 [Patent Document 4] Patent Publication No. 2020-187835 [Patent Document 5] International Publication No. 2023 / 022087 Summary of the Invention [Problem to be solved by the invention]
[0012] However, because the exterior material of an all-solid-state battery is composed of a film-like laminate (laminate sheet), it is difficult to accurately grasp the boundary between the part of the sealant layer to be removed (the part to be opened) and the part to be left, and this makes it difficult to properly remove the sealant layer corresponding to the opening, resulting in the problem that it is difficult to form an opening with excellent dimensional accuracy.
[0013] Although the issues in all-solid-state batteries have been described above, similar issues may arise in other power storage devices.
[0014] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide an electricity storage device and an exterior material for an electricity storage device that can reliably form an opening with excellent dimensional accuracy in a sealant layer. [Means for solving the problem]
[0015] In order to solve the above problems, the present invention comprises the following means.
[0016] [1] A power storage device comprising a power storage device main body and an exterior material for a power storage device that exteriorly covers the power storage device main body, The electrical storage device exterior material includes a resin base layer, a metal foil layer laminated on an inner surface side of the base layer, a gas barrier layer laminated on the inner surface side of the metal foil layer, and a resin sealant layer laminated on the inner surface side of the gas barrier layer via an adhesive layer, the sealant layer has an opening at a position corresponding to the electricity storage device main body, the opening being free of a sealant layer resin; The adhesive layer has an adhesive-uncoated portion that is provided in correspondence with the opening and in which no adhesive is present, and an adhesive-coated portion that is provided in correspondence with a portion other than the opening and in which adhesive is present, The electricity storage device, wherein the adhesive of the adhesive-coated portion is composed of a colored adhesive.
[0017] [2] A case body having an accommodation portion in which the power storage device body is accommodated, and a closing member attached to the case body in a state in which the closing member closes an open portion of the accommodation portion, 2. The electricity storage device according to item 1, wherein at least one of the case body and the closing member is made of the exterior material for an electricity storage device.
[0018] [3] An exterior material for an electricity storage device used in the electricity storage device according to the preceding item 1 or 2, the sealant layer has a sealant layer resin present therein and is provided with an intended opening portion that will become the opening; The adhesive layer has an adhesive-uncoated portion that is provided in correspondence with the intended opening portion and in which no adhesive is present, and an adhesive-coated portion that is provided in a portion other than the intended opening portion and in which adhesive is present, An exterior material for an electricity storage device, wherein the adhesive in the adhesive-coated portion is composed of a colored adhesive.
[0019] [4] The colored adhesive includes a two-component curing adhesive and a colorant, 4. The exterior material for an electricity storage device according to item 3 above, wherein the colorant contains a pigment or a dye.
[0020] [5] The coating amount of the colored adhesive is 1 g / m 2 ~6g / m 2 and 5. An exterior material for an electricity storage device according to item 3 or 4 above, wherein the content of the colorant is 0.1 wt % to 10 wt %.
[0021] [6] When the L value of the adhesive-coated part measured from the inner surface side of the sealant layer is "La" and the L value of the adhesive-uncoated part is "Lb", |La-Lb|≧0.5 6. The exterior packaging material for an electricity storage device according to any one of items 3 to 5 above, wherein the following relational expression is satisfied:
[0022] [7] An exterior material with an opening for an electricity storage device, which is formed by removing the sealant layer at the intended opening portion in the exterior material for an electricity storage device according to any one of items 3 to 6 above. Effect of the Invention
[0023] According to the energy storage device of the inventions [1] [2], in the adhesive layer between the heat-resistant gas barrier layer and the sealant layer in the exterior material, an adhesive-uncoated portion where no adhesive is applied is formed at the opening, and an adhesive-coated portion where a colored adhesive is applied is formed in the portion other than the opening. Therefore, when forming an opening by removing a portion of the sealant layer, the boundary position between the adhesive-coated portion and the adhesive-uncoated portion can be accurately grasped due to the color difference caused by the presence or absence of the colored adhesive, and the sealant layer can be partially cut accurately along the boundary position, thereby forming an opening with high precision.
[0024] According to the packaging material for an electricity storage device of the invention [3], similarly to the above, openings can be formed with high precision in the sealant layer.
[0025] According to the packaging materials for an electricity storage device of the inventions [4] to [6], the adhesive-coated portion and the adhesive-uncoated portion can be more clearly distinguished, and the above-mentioned effects can be more reliably obtained.
[0026] According to the exterior material with an opening for an electricity storage device of the invention [7], similarly to the above, an opening can be formed with high precision in the sealant layer. [Brief description of the drawings]
[0027] [Figure 1]FIG. 1 is a schematic cross-sectional view showing an all-solid-state battery as an electricity storage device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged schematic cross-sectional view showing a main part of FIG. [Diagram 3] FIG. 3 is an exploded perspective view illustrating a schematic diagram of the all-solid-state battery according to the embodiment. [Figure 4] FIG. 4 is a schematic cross-sectional view showing an exterior material for a case body in the all-solid-state battery according to the embodiment. [Diagram 5] FIG. 5 is a schematic inner surface view showing the exterior material of the embodiment. [Figure 6] FIG. 6 is a schematic cross-sectional view illustrating a method for forming an opening in the exterior material of the embodiment. [Figure 7] FIG. 7 is a schematic cross-sectional view showing a mold device for molding a case body using an exterior material with an opening according to an embodiment. [Figure 8] FIG. 8 is a schematic cross-sectional view showing an all-solid-state battery according to a first modified example of the present invention. [Figure 9] FIG. 9 is a schematic cross-sectional view showing an all-solid-state battery according to a second modified example of the present invention. [Figure 10] FIG. 10 is a schematic cross-sectional view showing an all-solid-state battery according to a third modified example of the present invention. [Figure 11] FIG. 11 is a schematic cross-sectional view showing an all-solid-state battery according to a fourth modified example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Fig. 1 is a schematic cross-sectional view showing an all-solid-state battery as an electricity storage device according to an embodiment of the present invention, Fig. 2 is a schematic cross-sectional view showing an enlarged view of a main part of Fig. 1, and Fig. 3 is an exploded perspective view showing a schematic view of the all-solid-state battery according to the embodiment. As shown in these figures, the all-solid-state battery according to this embodiment includes a case body 3 and a blocking member 4 as a casing, and an all-solid-state battery body 5 housed and sealed in the casing.
[0029] 4 is a schematic cross-sectional view showing an exterior material 1 constituting a case body 3 in an all-solid-state battery according to an embodiment. As shown in the figure, the exterior material 1 includes a base layer 11 disposed on the outermost side, a metal foil layer 12 laminated and bonded to the inner side of the base layer 11 via a first adhesive layer (not shown), a heat-resistant gas barrier layer 13 laminated and bonded to the inner side of the metal foil layer 12 via a second adhesive layer (not shown), and a sealant layer 15 laminated and bonded to the inner side of the heat-resistant gas barrier layer 13 via a third adhesive layer 14. In the present invention, when describing the positions of the layers constituting the exterior material 1 in terms of directions, the direction of the base layer 11 (upper side in FIG. 3) is referred to as the outer side, and the direction of the sealant layer 15 (lower side in FIG. 3) is referred to as the inner side.
[0030] The exterior material 1 constituting the blocking member 4 also has a similar structure to the exterior material 1 constituting the case body 3 described above.
[0031] The case body 3 is formed of a molded body of the exterior material 1, and integrally includes a top wall 31, a side wall (circumferential side wall) 32 extending downward from the outer periphery of the top wall 31, and a flange 33 provided on the outer periphery of the lower end of the side wall 32. A storage section 35 is formed inside the top wall 31 and the side wall 32. The blocking member 4 is formed of a sheet-like exterior material 1. The all-solid-state battery body 5 is accommodated in the accommodation section 35 of the case body 3, and the blocking member 4 is arranged so as to close the lower end open part of the accommodation section 35. The blocking member 4 is arranged so that its sealant layer 15 faces inward (upper side), and the sealant layer 15 of the flange 33 of the case body 3 and the sealant layer 15 of the outer periphery of the blocking member 4 are overlapped opposite each other. The overlapped sealant layers 15 are joined and integrated by thermal adhesion (heat sealing), thereby producing an all-solid-state battery in which the all-solid-state battery body 5 is accommodated in a sealed state in the casing (case body 3 and blocking member 4).
[0032] In addition, the case body 3 of the all-solid-state battery has an opening 2 in which the resin constituting the sealant layer 15 and the adhesive constituting the adhesive layer 14 are not present in a portion corresponding to the storage portion 35. Furthermore, the closing member 4 also has an opening 2 in which the resin for the sealant layer and the adhesive for the adhesive layer are not present in a portion corresponding to the storage portion 35. And through the opening 2 of the case body 3 and the closing member 4, the heat-resistant gas barrier layer 13 of the exterior material 1 is exposed inside the storage portion 35 and is disposed so as to face the all-solid-state battery body 5.
[0033] In addition, in the all-solid-state battery of this embodiment, a tab lead is provided for taking out electricity, although not shown in the drawings. One end (inner end) of this tab lead is adhesively fixed to the all-solid-state battery body 5, and the middle part is arranged so that it passes through the heat-sealed part between the flange 33 of the case body 3 and the outer circumferential edge part of the blocking member 4, and the other end side is drawn out to the outside.
[0034] Each part of the all-solid-state battery of this embodiment will be described in detail below.
[0035] The base material layer 11 of the exterior material 1 is composed of a heat-resistant resin film having a thickness of 5 μm to 50 μm. The resin that composes this base material layer 11 can be suitably selected from oriented polyamide film, oriented polyester (PET, PBT, PEN, etc.), oriented polyolefin (PE, PP, etc.), etc.
[0036] The metal foil layer 12 has a thickness set to 5 μm to 120 μm, and has a function of blocking the intrusion of oxygen and moisture from the surface (outer surface) side. Aluminum foil, SUS foil (stainless steel foil), copper foil, nickel foil, etc. can be suitably used as this metal foil layer 12. In this embodiment, the terms "aluminum", "copper", and "nickel" are used to include their alloys.
[0037] Furthermore, by subjecting the metal foil layer 12 to a plating process or the like, the risk of pinholes occurring can be reduced, and the function of blocking the intrusion of oxygen and moisture can be further improved.
[0038] Furthermore, if the metal foil layer 12 is subjected to a chemical conversion treatment such as chromate treatment, the corrosion resistance is further improved, making it possible to more reliably prevent defects such as chipping, and also to improve adhesion to the resin, thereby further improving durability.
[0039] The sealant layer (thermally adhesive resin layer) 15 has a thickness set to 20 μm to 100 μm and is made of a film of a thermally adhesive (thermally adhesive) resin. Suitable resins for the sealant layer 15 include polyethylene (LLDPE, LDPE, HDPE), polyolefins such as polypropylene, cyclic polyolefins, olefin copolymers, acid-modified products thereof, and ionomers, such as non-oriented polypropylene (CPP, IPP).
[0040] Considering that electricity is taken out using a tab lead, that is, in consideration of sealing properties and adhesiveness with the tab lead, it is preferable to use a polypropylene resin (non-oriented polypropylene film (CPP, IPP)) as the sealant layer 15.
[0041] The heat-resistant gas barrier layer 13 is made of a resin film having heat resistance and insulating properties. The resin for the heat-resistant gas barrier layer 13 may be selected from the group consisting of polyamide (6-nylon, 66-nylon, MXD nylon, etc.), polyester (PET, PBT, PEN), polyvinylidene chloride (PVDC), polyethylene (LLDPE, LDPE, HDPE), polypropylene (CPP, OPP), and other polyolefins, olefin copolymers, acid-modified products thereof, and ionomers.
[0042] In this embodiment, the thickness of the heat-resistant gas barrier layer 13 is preferably set to 3 μm to 50 μm, and more preferably to 10 μm to 40 μm. In other words, when the thickness of the heat-resistant gas barrier layer 13 is set in this range, the permeation suppression effect of hydrogen sulfide gas and water vapor gas can be reliably obtained, and even if the sealant layer 15 melts and flows out due to thermal adhesion, the heat-resistant gas barrier layer 13 can reliably ensure insulation. In other words, if the heat-resistant gas barrier layer 13 is too thin, there is a risk that the gas permeation suppression effect and insulation cannot be ensured, which is not preferable. Conversely, if the heat-resistant gas barrier layer 13 is too thick, not only cannot the exterior material 1 be thinned, but also the effect of making it thicker than necessary cannot be fully obtained, which is not preferable.
[0043] In this embodiment, it is preferable to use a resin film as the heat-resistant gas barrier layer 13. That is, the entire film becomes a barrier layer, and therefore, unlike a vapor-deposited film, no barrier cracks occur and the barrier properties can be improved.
[0044] Furthermore, a non-stretched film or a stretched film may be used as the resin film constituting the heat-resistant gas barrier layer 13, and it is particularly preferable to use a stretched film. That is, when a stretched film is used, it is possible to further improve the heat resistance, insulating properties, formability, and gas barrier properties.
[0045] The heat-resistant gas barrier layer 13 of this embodiment has good insulating properties, and maintains good insulating properties even after the all-solid-state battery body 5 is encapsulated (sealed) with the case body 3 and the blocking member 4 as the exterior material 1 of this embodiment.
[0046] In this embodiment, the resin constituting the heat-resistant gas barrier layer 13 has a water vapor transmission rate of 50 (g / m2) or more, measured in accordance with JIS K7129-1 (humidity sensor method at 40° C. and 90% Rh). 2 / day), i.e., the water vapor transmission rate is 50 (g / m 2 / day) or less, the gas permeation prevention effect of the heat-resistant gas barrier layer 13 can prevent the intrusion of moisture such as water vapor gas from the outside, thereby suppressing the generation of hydrogen sulfide gas due to the reaction between moisture and the solid electrolyte, and more reliably preventing the leakage of hydrogen sulfide gas and the like.
[0047] In this embodiment, it is preferable to use a resin having a thermal conductivity of 0.2 W / m·K or more as the resin constituting the heat-resistant gas barrier layer 13. That is, when this configuration is used, the heat conductivity of the heat-resistant gas barrier layer 13 can be sufficiently ensured, and the cooling performance of the all-solid-state battery body 5 can be further improved.
[0048] Furthermore, in this embodiment, it is preferable to adopt a resin constituting the heat-resistant gas barrier layer 13 having a melting point 10° C. or more higher than that of the resin constituting the sealant layer 15. In other words, when the heat-resistant gas barrier layer 13 has a high melting point, there is no change in thickness of the heat-resistant gas barrier layer 13 during heat sealing after the solid-state battery is housed, the water vapor permeation prevention effect of the heat-resistant gas barrier layer 13 can be well maintained, and the generation of hydrogen sulfide gas can be more reliably suppressed. In this embodiment, the melting point is measured by the DSC melting peak temperature measured in accordance with JIS K7121-1987.
[0049] In this embodiment, two-component curing adhesives for dry lamination, such as polyurethane adhesives, acrylic adhesives, polyacrylate adhesives, modified polypropylene adhesives, polyester adhesives, polyamide adhesives, and epoxy adhesives, can be suitably used as the first adhesive layer that bonds the base layer 11 and the metal foil layer 12, the second adhesive layer that bonds the metal foil layer 12 and the heat-resistant gas barrier layer 13, and the third adhesive layer 14 that bonds the heat-resistant gas barrier layer 13 and the sealant layer 15. The thicknesses of these first to third adhesive layers are preferably set to 1 μm to 6 μm.
[0050] In this embodiment, the adhesive constituting the third adhesive layer 14 between the heat-resistant gas barrier layer 13 and the sealant layer 15 is composed of a colored adhesive in which a colorant made of a pigment or dye is added to the above-mentioned adhesive. As a result, in the exterior material 1 before the opening 2 is formed, as described below, the adhesive-uncoated portion 14b (opening portion 2a) where no adhesive is present and the adhesive-coated portion 14a where the colored adhesive is present can be clearly distinguished from each other by the color difference due to the presence or absence of the colored adhesive.
[0051] A colored adhesive is a two-part curing adhesive containing a colorant. Colorants are generally classified into dyes that are soluble in solvents such as water and oil, and pigments that are not soluble in solvents such as water and oil.
[0052] Dyes classified according to their chemical structure include azo dyes having an azo group (-N=N-) in the molecule, anthraquinone dyes having an anthraquinone skeleton in the molecule, and indigoid dyes such as indigo, thioindigo, and derivatives thereof.
[0053] Pigments are classified into inorganic and organic pigments. Inorganic pigments include various oxides, sulfides, and ferrocyanide compounds, such as white pigments (titanium oxide, zinc oxide, zinc-containing calcined hydrotalcite), red pigments (iron oxide red), blue pigments (ferrocyanide Prussian blue), and black pigments (carbon black).
[0054] Furthermore, some pigments are not only used for coloring but also for special purposes. For example, aluminum oxide, which is a white pigment, may be used as a moisture absorbent, and when zinc-containing calcined hydrotalcite is added to an adhesive as a white pigment, it absorbs hydrogen sulfide gas generated by the reaction of the sulfide all-solid-state battery with moisture, suppressing the leakage of hydrogen sulfide gas to the outside of the battery, and also absorbs water vapor entering from the outside of the battery, suppressing the generation of hydrogen sulfide gas.
[0055] On the other hand, organic pigments include azo pigments, phthalocyanine pigments, perylene pigments, quinacridone pigments, etc. Azo pigments are yellow to red coloring materials and are widely used for plastics, while phthalocyanine pigments are blue and green coloring materials and are used for plastics and inks.
[0056] In this embodiment, between pigments and dyes, the use of pigments is advantageous in terms of weather resistance, solvent resistance, and heat resistance, and it is even more preferable to use pigments as the colorant.
[0057] In this embodiment, it is preferable to adjust the colorant content in the colored adhesive to 0.1wt% to 10wt%. That is, when this content is 0.1wt% or more, the boundary between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be clearly defined when the exterior material 1 is viewed from the inside, and the opening 2 can be formed with high precision. Note that even if the colorant content exceeds 10wt%, there is no particular effect commensurate with that content, and there is a risk of an increase in costs in some cases, so it is preferable to adjust it to 10wt% or less.
[0058] Furthermore, the coating amount of the colored adhesive in the adhesive coating portion 14a of the third adhesive layer 14 is set to 1 g / m 2 ~6g / m 2 It is preferable to adjust the coating weight to 1 g / m2. 2 In the above case, when the exterior packaging material 1 is viewed from the inside, the boundary between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be clearly defined, and the opening 2 can be formed with high accuracy. 2 Even if the amount exceeds 6g / m, the effect is not commensurate with the amount applied, and there is a risk of increased costs in some cases. 2 It is preferable to adjust as follows:
[0059] In this embodiment, the second adhesive layer that bonds the metal foil layer 12 and the heat-resistant gas barrier layer 13 can be formed by using an adhesive resin (polyolefin-based resins such as polyolefin, carboxylic acid-modified polyolefin, and metal-modified polyolefin, polyvinyl acetate-based resin, (meth)acrylic resin, amino resin, etc.) instead of an adhesive, and laminating the adhesive resin and the resin that forms the heat-resistant gas barrier layer 13 on the metal foil layer 12 by co-extruding (extrusion lamination method), or by forming a laminate in which the adhesive resin and the heat-resistant gas barrier layer 13 are laminated in advance, and laminating this laminate on the metal foil layer 12 by a thermal lamination method, or by pouring molten adhesive resin between the metal foil layer 12 and the heat-resistant gas barrier layer 13 while bonding the metal foil layer 12 and the heat-resistant gas barrier layer 13 together (sand lamination method), or the like.
[0060] In this embodiment, the opening 2 on the case body 3 side has its outer peripheral edge 21 provided on the flange 33 of the case body 3. Furthermore, the opening 2 on the closing member 4 side has its opening edge 21 formed to correspond to the opening edge 21 of the opening 2 of the case body 3.
[0061] In this embodiment, the opening 2 formed in the case body 3 and the blocking member 4 is not provided with a colored adhesive that constitutes the adhesive layer 14, and the heat-resistant gas barrier layer 13 is exposed (exposed) to the inside through the opening 2. In a state in which the all-solid-state battery is fabricated, the heat-resistant gas barrier layer 13 is disposed so as to face the upper surface, peripheral side surface and lower surface of the all-solid-state battery body 5.
[0062] Next, a method for manufacturing the exterior material 1 in this embodiment will be described. Needless to say, in the present invention, the method for manufacturing the exterior material 1 is not limited (the same applies to the method for manufacturing the case body 3 and the method for manufacturing the all-solid-state battery, which will be described later).
[0063] In this embodiment, first, a laminate without a sealant layer is produced, for example, by a dry lamination method. That is, a resin film for the base layer 11 is bonded via an adhesive to the outer surface of a metal foil for the metal foil layer 12, which has been subjected to a base treatment and a chemical conversion treatment as necessary, and a resin film for the heat-resistant gas barrier layer 13 is bonded via an adhesive to the inner surface of the metal foil, thereby producing a laminate without a sealant layer in which the metal foil layer 12 and the heat-resistant gas barrier layer 13 are laminated on the inner surface side of the base layer 11.
[0064] In addition, when producing a laminate without a sealant layer, it is possible to produce it by a method other than the dry lamination method, such as the extrusion lamination method, as described above. For example, the above laminate may be produced by extruding and laminating the resin composition for the base layer 11 and the resin composition for the heat-resistant gas barrier layer 13 onto the inner and outer surfaces of a metal foil, respectively.
[0065] Next, the adhesive (colored adhesive) that constitutes the adhesive layer 14 is applied to the inner surface of the laminate without the sealant layer (the inner surface of the heat-resistant gas barrier layer 13) using a gravure roll or the like. During this application, the adhesive is applied to the inner surface of the heat-resistant gas barrier layer 13 except for the portion (planned opening portion 2a) where the opening 2 in the sealant layer 15 is to be formed, forming an adhesive-coated portion 14a, while the adhesive is not applied to the portion corresponding to the planned opening portion 2a, forming an adhesive-uncoated portion 14b.
[0066] A resin film for a sealant layer is attached to the inner surface of the heat-resistant gas barrier layer 13 having the adhesive-uncoated portion 14b via the adhesive layer 14, and then dried. The resin film for a sealant layer is also provided in the portion corresponding to the adhesive-uncoated portion 14b.
[0067] As shown in Figure 5, the exterior material 1 obtained in this manner has adhesive-coated portion 14a (indicated by diagonal hatching in the figure) colored with a colored adhesive, and therefore the boundary between adhesive-coated portion 14a and adhesive-uncoated portion 14b (planned opening portion 2a) becomes clear due to the color difference (difference in brightness, etc.) between adhesive-coated portion 14a and adhesive-uncoated portion 14b.
[0068] 6, the area between the adhesive-coated portion 14a and the intended opening portion 2a is cut away, and the intended opening portion 2a, which is the sealant layer 15 of the adhesive-uncoated portion 14b, is cut away to form the opening 2. This cutting method is performed using a laser cutter, a roll blade, a punching blade (Thomson blade, etching blade, etc.), an ultrasonic cutter, etc. Among these, it is preferable to use a laser cutter, which can perform processing with high precision.
[0069] In this embodiment, as shown in FIG. 5, it is possible to automatically cut out the sealant layer 14 at the intended opening portion 2a to form the opening 2 using an opening position detection device and a laser cutting device 82.
[0070] That is, the opening position detection device 81 detects the boundary position between the adhesive coated portion 14a and the adhesive uncoated portion 14b, and is provided with a detection sensor that detects the amount of reflected light of light irradiated from a light source to the subject, and detects the boundary position between the adhesive coated portion 14a and the adhesive uncoated portion 14b based on the difference in the amount of light. The laser cutting device 82 is composed of a CO2 laser cutting device, etc., and cuts the boundary position between the adhesive coated portion 14a and the adhesive uncoated portion 14b, that is, the outer peripheral edge portion 21a of the opening portion 2a based on the position information from the opening position detection device 81, and cuts off the sealant layer 15 of the opening portion 2a to form the opening 2. In this way, the opening 2 is automatically formed in the exterior material 1 to produce an exterior material with an opening. Therefore, by using the opening position detection device 81 and the laser cutting device 82, the opening 2 can be automatically formed in the exterior material 1 to produce an exterior material with an opening.
[0071] In the exterior material 1 before the opening 2 of this embodiment is formed, when the L value, which is the lightness of the adhesive-coated portion 14a measured from the sealant layer 15 side (inner surface side), is "La" and the L value, which is the lightness of the adhesive-uncoated portion 14b, is "Lb", it is preferable to set the absolute position of ΔL (lightness difference) as the absolute value of the difference between La and Lb to 0.5 or more. In other words, it is preferable to configure so that the relational expression |La-Lb|=|ΔL|≧0.5 holds.
[0072] In other words, when the above relational expression is satisfied, the brightness difference ΔL between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b is large, so that the boundary position between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be properly captured, and the opening 2 can be formed with high precision.
[0073] However, in the present invention, the color difference (boundary position) between adhesive-coated portion 14a and adhesive-uncoated portion 14b may be detected by a color difference other than the brightness difference, such as a difference in hue or a difference in saturation.
[0074] Next, a method of molding the sheet-like exterior material with an opening obtained as described above to produce the case body 3 will be described. First, as shown in Fig. 6, the sheet-like exterior material 1 for the case body before molding includes a top wall planned portion 31a which is a portion intended to become the top wall 31, a side wall planned portion 32a which is a portion intended to become the side wall 32, and a flange planned portion 33a which is a portion intended to become the flange 33.
[0075] In this embodiment, the outer circumferential edge portion 21a of the intended opening portion 2a is set within the range of the intended flange portion 33a.
[0076] 7 is a schematic cross-sectional view showing a mold device for molding a case body 3 using an opening-equipped exterior material 1. As shown in the figure, this mold device includes a die 6 as an upper mold, and a punch 7 and a blank holder 70 as a lower mold.
[0077] The die 6 has a molding recess 65 formed on its lower surface for molding the accommodation portion 35 (the top wall 31 and the side wall 32) of the case body 3.
[0078] The punch 7 is disposed in correspondence with the molding recess 65 of the die 6 , and the blank holder die 70 is disposed on the outer periphery of the punch 7 and faces the outer periphery of the lower surface of the die 6 .
[0079] Then, the opening-equipped exterior material 1 as a molding material is placed so that its side wall planned portion 32a corresponds to the tip outer peripheral edge portion of the punch 7. In this state, the flange planned portion 33a of the exterior material 1 is sandwiched and supported by the outer peripheral portion of the die 6 and the blank holder die 70, and the punch 7 is driven into the molding recess 65 of the die 6, whereby the exterior material 1 is pressed. As a result, a case body molded body (molding material) having a storage portion 35 (top wall 31 and side wall 32) and a flange 33 on the outside of the storage portion 35 is molded. Next, the flange 33 of the molded body is cut to a predetermined size, thereby producing the case body 3 of this embodiment. In this case body 3, the opening 2 is arranged in the entire area of the storage portion 35, and the outer peripheral edge portion 21 of the opening 2 is arranged on the flange 33, as shown in Figures 1 to 3.
[0080] As shown in Figs. 1 to 3, in this embodiment, the solid-state battery body 5 is packaged using the case body 3 and the sheet-like blocking member 4 to produce an all-solid-state battery. That is, the all-solid-state battery body 5 is accommodated in the accommodation portion 35 of the case body 3, and the blocking member 4 is arranged so as to block the accommodation portion 35 from the lower side, and the sealant layer 15 of the flange 33 of the case body 3 and the sealant layer 15 of the outer peripheral edge of the blocking member 4 are arranged so as to face and overlap each other. In this state, the flange 33 of the case body 3 and the outer peripheral edge of the blocking member 4 are sandwiched between a pair of sealing dies and heated. As a result, the sealant layers 15 that overlap each other are heat-sealed and joined together, and an all-solid-state battery in which the all-solid-state battery body 5 is accommodated in an airtight state in the case body 3 and the blocking member 4 is produced.
[0081] According to the all-solid-state battery of this embodiment having the above-mentioned configuration, the heat-resistant gas barrier layer 13 is provided between the metal foil layer 12 and the sealant layer 15 in the case body 3 and the closing member 4, and the opening 2 is formed in the top wall 31 and the side wall 32 by removing a part of the sealant layer 15. Therefore, heat generated from the all-solid-state battery body 5 is efficiently transferred to the metal foil layer 12 via the opening 2 and the heat-resistant gas barrier layer 13 without being blocked by the sealant layer 15, and is dissipated, thereby ensuring sufficient heat dissipation and cooling properties.
[0082] In particular, in this embodiment, the outer peripheral edge 21 of the opening 2 in the case body 3 is set to the flange 33 of the case body 3, so that a large opening 2 corresponding to almost the entire area of the all-solid-state battery body 5 can be formed, and heat dissipation and cooling properties can be further improved.
[0083] Furthermore, in the adhesive layer 14 between the heat-resistant gas barrier layer 13 and the sealant layer 15 in the exterior material 1 of this embodiment, an adhesive-uncoated portion 14b where no adhesive is applied is formed in the intended opening portion 2a, and an adhesive-coated portion 14a is formed by applying a colored adhesive to portions other than the intended opening portion 2a. Therefore, the boundary position between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be accurately grasped due to the color difference caused by the presence or absence of the colored adhesive, and the sealant layer 15 can be accurately cut along the boundary position (the outer peripheral edge portion 21a of the intended opening portion 2a) using a laser cutter or the like, and the opening 2 can be formed with high precision.
[0084] In particular, in this embodiment, when the brightness difference |La-Lb| between the adhesive-coated portion 15a and the adhesive-uncoated portion 15b is adjusted to 0.5 or more, the boundary position between the two portions 14a, 14b can be captured more accurately, and an opening 2 with even higher dimensional accuracy can be formed.
[0085] Moreover, according to the all-solid-state battery of this embodiment, since the heat-resistant gas barrier layer 13 is disposed on the inner surface side of the metal foil layer 12, even if the solid electrolyte of the all-solid-state battery body 5 reacts with moisture in the outside air to generate hydrogen sulfide gas or the like, the gas can be reliably prevented from leaking by the heat-resistant gas barrier layer 13. Furthermore, the gas permeation prevention action of the heat-resistant gas barrier layer 13 can prevent the intrusion of moisture such as water vapor gas from the outside, so that the generation of hydrogen sulfide gas itself due to the reaction between the moisture and the solid electrolyte can be suppressed, and the leakage of hydrogen sulfide gas or the like can be more reliably prevented.
[0086] In the all-solid-state battery of this embodiment, in the portion where the opening 2 is formed, although there is no sealant layer 15 between the all-solid-state battery body 5 and the metal foil layer 12, the heat-resistant gas barrier layer 13 having insulating properties is disposed therebetween, and therefore, the heat-resistant gas barrier layer 13 can reliably ensure insulation.
[0087] Furthermore, when cutting the exterior material 1 with a laser cutter or the like to form the opening 2, a damaged portion caused by the laser is formed at the outer peripheral edge 21 of the opening, which may cause defects such as cracks and pinholes. However, in this embodiment, the outer peripheral edge 21 of the opening is formed at the flange 33 of the case body 3, so that the adverse effects of the damaged portion can be avoided. That is, the flange 33 of the molded body 3 is heat-sealed, so that a resin reservoir formed by the heat seal is formed at the damaged portion (the outer peripheral edge 21 of the opening). Therefore, the damaged portion can be covered and repaired by the resin reservoir, so that the adverse effects of the damaged portion caused by laser cutting can be reliably avoided.
[0088] Furthermore, in the all-solid-state battery of this embodiment, the sealant layer 15 is not formed in the portion of the exterior material 1 that corresponds to the all-solid-state battery body 5, and therefore the space for accommodating the all-solid-state battery body 5 can be made larger (thicker). Therefore, in the all-solid-state battery of this embodiment, compared to conventional all-solid-state batteries, a larger-sized all-solid-state battery body 5 can be accommodated without changing the external dimensions of the case body 3, and therefore high output and high capacity can be achieved while achieving a thin design.
[0089] In addition, in the all-solid-state battery of this embodiment, the sealant layer 15 is provided on the flange 33 provided around the entire periphery of the case body 3, and therefore the sealant layer 15 provided around the entire periphery can reliably seal the entire periphery of the all-solid-state battery, thereby ensuring good sealing performance.
[0090] In the above-described all-solid-state battery of this embodiment, the case where the opening 2 is formed in both the case body 3 and the blocking member 4 has been described as an example, but the present invention is not limited thereto. As shown in FIG. 8 , the opening 2 may be formed in the case body 3, and the opening 2 may not be formed in the blocking member 4.
[0091] In addition, the all-solid-state battery of this embodiment shown in FIG. 1 is arranged so that the case body 3 is disposed on the upper side and the blocking member 4 is disposed on the lower side, but the present invention is not limited to this. In other words, the all-solid-state battery shown in FIG. 1 may be inverted, that is, the case body 3 which is a molded body is disposed on the lower side and the sheet-like blocking member 4 is disposed on the upper side.
[0092] In the above embodiment, the edge 21 of the opening 2 is set within the flange 33, but the present invention is not limited to this. For example, in the present invention, the edge 21 of the opening 2 may be set on the side wall 32 of the case body 3 as shown in Fig. 9, or the edge 21 of the opening 2 may be set on the top wall (bottom wall) 33 of the case body 3 as shown in Fig. 10. In other words, the shape and size of the opening 2 are not particularly limited in the present invention.
[0093] Furthermore, in the present invention, a molded body may be used as the blocking member 4. For example, as shown in Fig. 11, a tray-shaped molded body having a shape obtained by inverting the case body 3 upside down may be used as the blocking member 4, and the casing of the all-solid-state battery may be formed by the case body 3 which is a molded body and the tray-shaped blocking member 4 which is a molded body. In this case, by using a similar configuration for the blocking member 4 as the case body 3, the same effect can be obtained with the blocking member 4.
[0094] In the above embodiment, a case has been described in which an all-solid-state battery is used as the power storage device of the present invention. However, the present invention is not limited to this, and can be applied to power storage devices other than all-solid-state batteries. EXAMPLES
[0095] [Table 1]
[0096] The abbreviations shown in Table 1 are as follows. TDI: Toluene diisocyanate TMP: Trimethylolpropane HDI: Hexamethylene diisocyanate HT: Zinc-containing calcined hydrotalcite [(Mg / Zn) 0.8. Al 0.2 (OH)2] 0.2 (CO3) 0.2 CB: Carbon black <Example 1> As shown in Table 1, in the inner configuration of the sample (exterior material), a 12 μm thick matte PET (polyethylene terephthalate) film was laminated as a heat-resistant gas barrier layer on the inner surface (matte side) of an aluminum foil made of A8021-O specified in JIS H4160 with a thickness of 40 μm as a metal foil layer, via a two-liquid curing polyester-urethane adhesive as a second adhesive layer. Furthermore, a 80 μm thick CPP (non-oriented polypropylene) film was laminated as a sealant layer on the inner surface of the heat-resistant gas barrier layer, using a colored adhesive as a third adhesive layer. At this time, the third adhesive layer was not applied to the intended opening portion. The size of this adhesive-uncoated portion (intended opening portion) was a rectangle of 100 mm x 200 mm (see Figures 4 and 5).
[0097] The colored adhesive as the third adhesive layer is obtained by adding 0.2 wt% of CB with a particle size of 0.4 μm as a colorant to an adhesive having a polyester polyol as the main resin and an adduct of TDI and TMP as the curing agent. The coating amount of the colored adhesive is 2 g / m 2 is.
[0098] Although not described in the table, in the configuration of the outside of the sample, a stretched nylon film (ONY) with a thickness of 25 μm is laminated on the outer surface (glossy surface) of the metal foil layer 12 via a two-component curable polyester-urethane-based adhesive (first adhesive layer) (the same applies to Examples 2 to 10 and Comparative Examples 1 and 2).
[0099] After laminating each layer of the laminated film thus obtained, it was cured at 40 °C for 5 days to produce 50 samples (exterior materials) of Example 1.
[0100] <Examples 2 to 7 and Comparative Examples 1 and 2> Using the materials shown in Table 1, in the same manner as in Example 1 above, 50 samples (exterior materials) without an adhesive-coated portion were produced for each of Examples 2 to 7 and Comparative Examples 1 and 2.
[0101] In the samples of Comparative Examples 1 and 2, no colorant was added to the adhesive constituting the third adhesive layer.
[0102] <Evaluation of L value and detectability>
[0103]
Table 2
[0104] As shown in Table 2, for 50 samples each of the above Examples and Comparative Examples, using a spectrophotometer (CM-2500c) manufactured by Konica Minolta, the L value (Lb) of the non-adhesive-coated portion (planned opening portion) and the L value (La) of the adhesive-coated portion were measured from the inner surface side, and the average value of the brightness difference (|ΔL| = |La - Lb|) between the non-adhesive-coated portion and the adhesive-coated portion was obtained. The results are shown in Table 2.
[0105] In addition, for 50 samples of each of the above examples and comparative examples, an opening forming device consisting of an opening position detection device and a laser cutting device was used to remove the sealant layer from the intended opening areas (areas where adhesive was not applied).
[0106] The opening position detection device used was an MR101 scanning head manufactured by Nireco Corporation. This detection device uses an LED as a light source, and detects the outer periphery of the colored adhesive uncoated area (area to be opened) based on a mechanism that receives the difference in the amount of light reflected between the colored adhesive uncoated area and the colored adhesive coated area with an SPD (silicon photodiode) and outputs a voltage proportional to the amount of light.
[0107] A CO2 laser cutting device was used as the laser cutting device. Based on the position information of the colored adhesive uncoated part (planned opening part) in the center of each sample detected by the opening position detection device, this cutting device cuts and removes only the sealant layer (CPP film) on the colored adhesive uncoated part, and creates an exposed part (opening) of the heat-resistant gas barrier layer (matte PET film) measuring 100 mm wide x 200 mm long.
[0108] In Table 2, with regard to the detectability of the uncoated areas, an "○" indicates that the outer circumferential position of the uncoated areas was accurately detected in all 50 samples, and an opening was formed with high precision, an "△" indicates that the uncoated areas could not be detected in only one of the 50 samples, and an opening could not be formed, and an "×" indicates that the outer circumferential position of the uncoated areas could not be detected sufficiently, and an opening could not be formed.
[0109] As is clear from Table 2, the samples of Examples 2 to 10 had large ΔL, the difference between the adhesive-uncoated area and the adhesive-coated area was clear, and the adhesive-uncoated area (the area to be opened) could be cut out with high precision. Note that, although the ΔL of the sample of Example 1 was somewhat small, it was basically possible to detect the adhesive-uncoated area, and it is believed that an opening can be formed without any problems in practical use.
[0110] In contrast, in the samples of Comparative Examples 1 and 2, ΔL was small, the difference between the uncoated and coated areas was unclear, and the opening position detection device was unable to accurately detect the outer circumferential position of the uncoated areas, and the intended opening portion could not be cut out. [Industrial Applicability]
[0111] The exterior packaging material for an electricity storage device of the present invention can be suitably used as a material for a battery case (casing) for housing an all-solid-state battery main body such as an all-solid-state battery. [Explanation of symbols]
[0112] 1: Exterior material 11: Base material layer 12: Metal foil layer 13: Heat-resistant gas barrier layer 14:Adhesive layer (3rd adhesive layer) 14a: Adhesive coating section 14b: Uncoated with adhesive 15: Sealant layer 2: Opening 2a: Opening area 3: Case body 35: Storage unit 4: Closure member 5: All-solid battery body La: L value of adhesive coating part Lb: L value of the adhesive uncoated area
Claims
1. An electricity storage device comprising an electricity storage device main body and an exterior material for an electricity storage device that exteriorly covers the electricity storage device main body, The electrical storage device exterior material includes a resin base layer, a metal foil layer laminated on an inner surface side of the base layer, a gas barrier layer laminated on the inner surface side of the metal foil layer, and a resin sealant layer laminated on the inner surface side of the gas barrier layer via an adhesive layer, the sealant layer has an opening at a position corresponding to the electricity storage device main body, the opening being free of a sealant layer resin; The adhesive layer has an adhesive-uncoated portion that is provided in correspondence with the opening and in which no adhesive is present, and an adhesive-coated portion that is provided in correspondence with a portion other than the opening and in which adhesive is present, The electricity storage device, wherein the adhesive of the adhesive-coated portion is composed of a colored adhesive.
2. a case body having a storage section for storing the power storage device body; and a closing member attached to the case body in a state where the closing member closes an open portion of the storage section, The electricity storage device according to claim 1 , wherein at least one of the case body and the closing member is made of the exterior material for an electricity storage device.
3. An exterior material for an electricity storage device used in the electricity storage device according to claim 1 or 2, the sealant layer has a sealant layer resin present therein and is provided with an intended opening portion that will become the opening; the adhesive layer is provided with an adhesive-uncoated portion that is provided in correspondence with the intended opening portion and in which no adhesive is present, and an adhesive-coated portion that is provided in a portion other than the intended opening portion and in which adhesive is present; An exterior material for an electricity storage device, wherein the adhesive in the adhesive-coated portion is composed of a colored adhesive.
4. The colored adhesive includes a two-component curing adhesive and a colorant, The packaging material for an electricity storage device according to claim 3 , wherein the colorant includes a pigment or a dye.
5. The coating amount of the colored adhesive is 1 g / m 2 ~6g / m 2 and 4. The exterior packaging material for an electricity storage device according to claim 3, wherein the content of the colorant is 0.1 wt % to 10 wt %.
6. When the L value of the adhesive-coated portion measured from the inner surface side of the sealant layer is "La" and the L value of the adhesive-uncoated portion is "Lb", |La-Lb|≧0.5 The electrical storage device packaging material according to claim 3 , wherein the above relational expression is satisfied.
7. An opening-equipped exterior material for an electricity storage device according to claim 3 , which is formed by removing the sealant layer at the intended opening portion in the exterior material for an electricity storage device according to claim 3 .
Citation Information
Patent Citations
Electrochemical device
JP2015228365A
Outer packaging body for power storage device
JP2016129091A
Method for working laminate material
JP2018069418A
Outer package material for all-solid-state batteries, and all-solid-state battery
WO2023017683A1
All-solid-state battery sheathing material and all-solid-state battery
WO2023022087A1