Optical adhesive sheet

The optical adhesive sheet addresses peeling and temperature-related issues in flexible display panels by maintaining low shear modulus and stress relaxation properties, ensuring reliable adhesion and handling across temperature changes.

JP2024169234APending Publication Date: 2024-12-05NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023086539
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Optical adhesive sheets used in flexible display panels, such as foldable and rollable devices, tend to peel off from adherends due to high tensile stress during deformation, leading to device malfunction, and have narrow cutting temperature margins due to significant elastic modulus changes with temperature.

Method used

An optical adhesive sheet with a shear storage modulus of 70 kPa or less at -20°C, a ratio of first shear loss modulus to second shear loss modulus of 14 or less, and specific adhesive properties to ensure stress relaxation and wide cutting temperature margins.

Benefits of technology

The adhesive sheet effectively suppresses peeling from adherends during deformation and maintains adhesion across varying temperatures, ensuring reliable performance and ease of handling in flexible devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169234000001_ABST
    Figure 2024169234000001_ABST
Patent Text Reader

Abstract

To provide an optical adhesive sheet suitable for flexible devices.SOLUTION: An adhesive sheet 10 is an optical adhesive sheet, exhibiting a shear storage modulus of at most 70 kPa at -20°C, wherein the ratio of a first shear loss modulus at -30°C to a second shear loss modulus at 60°C is at most 14.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an optical pressure-sensitive adhesive sheet. [Background technology]

[0002] A display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. In the manufacturing process of such a display panel, for example, an optically transparent adhesive sheet (optical adhesive sheet) is used to bond the elements included in the laminated structure.

[0003] Meanwhile, development of repeatedly foldable display panels for smartphones and tablet devices is progressing. Specifically, foldable display panels can be repeatedly deformed between a bent shape and a flat, unbent shape. In such foldable display panels, each element in the laminated structure is made to be repeatedly foldable, and a thin optical adhesive sheet is used to bond such elements. Optical adhesive sheets for flexible devices such as foldable display panels are described, for example, in Patent Document 1 listed below. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 2018-111754 Summary of the Invention [Problem to be solved by the invention]

[0005] Conventionally, optical adhesive sheets tend to peel off from elements serving as adherends at the bending points of foldable display panels. This is because, when a display panel is bent, relatively large tensile stress is generated locally at the bent portion of the optical adhesive sheet. At the bent portion of the optical adhesive sheet, the greater the tensile stress, for example in the shear direction, on the element (adherend), the more likely peeling occurs between the optical adhesive sheet and the element. The occurrence of such peeling is undesirable, as it can cause malfunctions of the device. Optical adhesive sheets for foldable display panels are highly required to resist peeling from elements (adherends) when the display is bent.

[0006] Meanwhile, development of rollable display panels as flexible devices is also progressing. Rollable display panels can be repeatedly deformed, for example, between a rolled shape after being completely or partially rolled up and a flat shape after being completely unrolled. In such rollable display panels, each element in the laminated structure is made to be repeatedly deformable, and a thin optical adhesive sheet is used to bond such elements. When the rollable display panel is in a rolled shape, the optical adhesive sheet bonded to the rolled element continues to receive tensile stress from the element. Such optical adhesive sheets are required to be highly resistant to peeling from the element (adherend) when the display is in a rolled shape.

[0007] Optical adhesive sheets for flexible devices are required to be highly flexible so as to have excellent stress relaxation properties. Conventionally, such optical adhesive sheets are cooled to a low temperature, for example, -20°C or lower, before being cut with a cutting blade. This is to prevent the optical adhesive sheet from adhering to the cutting blade (the lower the temperature, the higher the elasticity of the optical adhesive sheet, making it less likely to adhere to the cutting blade). However, during the cutting process, the temperature of the optical adhesive sheet gradually increases. In conventional optical adhesive sheets, the decrease in elastic modulus (softening) due to temperature increase in the optical adhesive sheet is relatively large, and the margin for cutting temperature is relatively narrow.

[0008] The present invention provides an optical pressure-sensitive adhesive sheet suitable for flexible device applications. [Means for solving the problem]

[0009] The present invention [1] includes an optical adhesive sheet having a shear storage modulus of 70 kPa or less at -20°C, and a ratio of a first shear loss modulus at -30°C to a second shear loss modulus at 60°C of 14 or less.

[0010] The present invention [2] includes the optical pressure-sensitive adhesive sheet according to the above [1], wherein the first shear loss modulus is 100 kPa or less.

[0011] The present invention [3] includes the optical adhesive sheet according to the above [1] or [2], in which the ratio of the first shear loss modulus to the third shear loss modulus at -20°C is 2.8 or less.

[0012] The present invention [4] includes the optical pressure-sensitive adhesive sheet according to the above [3], wherein the third shear loss modulus is 50 kPa or less.

[0013] The present invention [5] includes the optical pressure-sensitive adhesive sheet according to any one of the above [1] to [4], which has a maximum loss tangent tanδ of 1 or more and 3 or less at -50°C to 150°C.

[0014] The present invention [6] has a moisture permeability of 400 g / m2 measured under conditions of 40°C and 92% relative humidity. 2 The optical pressure-sensitive adhesive sheet according to any one of [1] to [5] above, wherein the durability is 24 hours or less.

[0015] The present invention [7] includes an optical adhesive sheet according to any one of [1] to [6] above, which has an adhesive strength of 2.0 N / 10 mm or more in a peel test under conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min. [Effects of the Invention]

[0016] As described above, the optical adhesive sheet of the present invention has a shear storage modulus of 70 kPa or less at -20°C. Such a soft optical adhesive sheet is suitable for alleviating stresses occurring in the optical adhesive sheet and the adherend when the adherend to which the optical adhesive sheet is bonded deforms (stress relaxation function). Stress relaxation in the optical adhesive sheet is suitable for preventing peeling of the optical adhesive sheet from the adherend. Stress relaxation in the adherend is suitable for preventing damage such as cracking of the adherend. In addition, as described above, the optical adhesive sheet of the present invention has a ratio (G1 / G2) of the first shear loss modulus at -30°C to the second shear loss modulus at 60°C of 14 or less. Such an optical adhesive sheet is suitable for preventing softening of the optical adhesive sheet due to temperature rise and ensuring a wide margin for cutting processing temperatures. Such optical adhesive sheets are suitable for flexible device applications. [Brief explanation of the drawings]

[0017] [Figure 1] 1 is a cross-sectional schematic view of one embodiment of the optical pressure-sensitive adhesive sheet of the present invention. [Figure 2] 2A shows an example of a method for using the optical pressure-sensitive adhesive sheet of the present invention, in which Fig. 2A shows a step of attaching the optical pressure-sensitive adhesive sheet to a first adherend, Fig. 2B shows a step of joining the first adherend and a second adherend via the optical pressure-sensitive adhesive sheet, and Fig. 2C shows an aging step. [Figure 3] FIG. 3A shows the test piece in a flat state during the repeated bending test, and FIG. 3B shows the test piece in a curved state during the repeated bending test. DETAILED DESCRIPTION OF THE INVENTION

[0018] As shown in Figure 1, a pressure-sensitive adhesive sheet 10 as one embodiment of the optical pressure-sensitive adhesive sheet of the present invention has a sheet shape of a predetermined thickness and extends in a direction (plane direction) perpendicular to the thickness direction H. The pressure-sensitive adhesive sheet 10 has a pressure-sensitive adhesive surface 11 on one side in the thickness direction H and a pressure-sensitive adhesive surface 12 on the other side in the thickness direction H. Figure 1 exemplarily shows a state in which release liners L1 and L2 are bonded to the pressure-sensitive adhesive surfaces 11 and 12 of the pressure-sensitive adhesive sheet 10. The release liner L1 is disposed on the pressure-sensitive adhesive surface 11. The release liner L2 is disposed on the pressure-sensitive adhesive surface 12. The release liners L1 and L2 are each peeled off at a predetermined timing when the pressure-sensitive adhesive sheet 10 is used.

[0019] The adhesive sheet 10 is an optically transparent adhesive sheet disposed at a light passage location in a flexible device. Examples of flexible devices include flexible display panels. Examples of flexible display panels include foldable display panels and rollable display panels. Flexible display panels have a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. The adhesive sheet 10 is used, for example, to bond elements included in the laminated structure during the manufacturing process of a flexible display panel.

[0020] The pressure-sensitive adhesive sheet 10 has a shear storage modulus of 70 kPa or less at -20°C, and the ratio of the first shear loss modulus at -30°C to the second shear loss modulus at 60°C is 14 or less. The shear storage modulus and shear loss modulus of the pressure-sensitive adhesive sheet 10 are determined by dynamic viscoelasticity measurement, which will be described later in the examples.

[0021] As described above, the adhesive sheet 10 has a shear storage modulus of 70 kPa or less at -20°C. Such a soft adhesive sheet 10 is suitable for alleviating stresses that occur in the adhesive sheet 10 and the adherend when the adherend to which the adhesive sheet 10 is attached deforms (stress relaxation function). The stress relaxation in the adhesive sheet 10 is suitable for preventing peeling of the adhesive sheet 10 from the adherend. The stress relaxation in the adherend is suitable for preventing damage such as cracking of the adherend.

[0022] Additionally, as described above, the ratio of the first shear loss modulus at -30°C to the second shear loss modulus at 60°C of the adhesive sheet 10 is equal to or less than 14. Such an adhesive sheet 10 is suitable for suppressing softening of the adhesive sheet 10 due to a rise in temperature, and for ensuring a wide margin for the temperature of the adhesive sheet 10 during cutting (cutting processing temperature).

[0023] The optical pressure-sensitive adhesive sheet described above is suitable for use in flexible devices.

[0024] The shear storage modulus of the pressure-sensitive adhesive sheet 10 at −20° C. is preferably 65 kPa or less, more preferably 55 kPa or less, and even more preferably 45 kPa or less, from the viewpoint of stress relaxation at the deformed portion when the pressure-sensitive adhesive sheet 10 is deformed (bent, curved, etc.). The shear storage modulus is preferably greater than 40 kPa, more preferably 45 kPa or more, from the viewpoint of ensuring good adhesiveness and handleability (ease of handling) of the pressure-sensitive adhesive sheet 10. Methods for adjusting the shear storage modulus of the pressure-sensitive adhesive sheet 10 include, for example, selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight and amount of the base polymer, and selecting the type of crosslinking agent and adjusting the amount of the crosslinking agent.

[0025] The ratio (ratio R1) of the first shear loss modulus (-30°C) to the second shear loss modulus (60°C) of the pressure-sensitive adhesive sheet 10 is preferably 13 or less, more preferably 12 or less, even more preferably 11 or less, and even more preferably 10 or less, from the viewpoint of suppressing softening of the pressure-sensitive adhesive sheet 10 due to a rise in temperature and ensuring a wide margin for the cutting processing temperature. Ratio R1 is, for example, 0 or more, 1 or more, 3 or more, 5 or more, or 7 or more.

[0026] The first shear loss modulus (-30°C) is preferably 100 kPa or less, more preferably 90 kPa or less, and even more preferably 85 kPa or less, from the viewpoint of suppressing changes in the physical properties of the pressure-sensitive adhesive sheet 10 in the low temperature range. The first shear loss modulus (-30°C) is preferably 30 kPa or more, more preferably 40 kPa or more, and even more preferably 50 kPa or more, from the viewpoint of ensuring good adhesiveness and handleability in the pressure-sensitive adhesive sheet 10. Methods for adjusting the shear storage modulus of the pressure-sensitive adhesive sheet 10 include, for example, selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight and amount of the base polymer, and selecting the type of crosslinking agent and adjusting the amount of the crosslinking agent.

[0027] The second shear loss modulus (60°C) is preferably 3 kPa or more, more preferably 5 kPa or more, even more preferably 6 kPa or more, and even more preferably 7 kPa or more, from the viewpoint of suppressing changes in the physical properties of the pressure-sensitive adhesive sheet 10 in high temperature regions. The second shear loss modulus (60°C) is preferably 15 kPa or less, more preferably 10 kPa or less, and even more preferably 8 kPa or less, from the viewpoint of ensuring the stress relaxation properties required in the pressure-sensitive adhesive sheet 10 for flexible device applications such as foldable display panels.

[0028] The third shear loss modulus of the pressure-sensitive adhesive sheet 10 at -20°C is preferably 50 kPa or less, more preferably 40 kPa or less, and even more preferably 35 kPa or less, from the viewpoint of suppressing changes in the physical properties of the pressure-sensitive adhesive sheet 10 in the low temperature range. The third shear loss modulus (-20°C) is preferably 10 kPa or more, more preferably 15 kPa or more, and even more preferably 20 kPa or more, from the viewpoint of ensuring good adhesiveness and handleability of the pressure-sensitive adhesive sheet 10.

[0029] The fourth shear loss modulus of the pressure-sensitive adhesive sheet 10 at 25°C is preferably 4 kPa or more, more preferably 6 kPa or more, and even more preferably 7 kPa or more, from the viewpoint of ensuring good handleability (ease of handling) of the pressure-sensitive adhesive sheet 10 in the room temperature region. The fourth shear loss modulus (25°C) is preferably 15 kPa or less, more preferably 12 kPa or less, and even more preferably 9 kPa or less, from the viewpoint of ensuring the stress relaxation properties required for flexible device applications in the pressure-sensitive adhesive sheet 10.

[0030] The ratio (ratio R2) of the first shear loss modulus (-30°C) to the third shear loss modulus (-20°C) of the pressure-sensitive adhesive sheet 10 is preferably 2.8 or less, more preferably 2.6 or less, and even more preferably 2.4 or less, from the viewpoint of suppressing softening of the pressure-sensitive adhesive sheet 10 due to a rise in temperature and ensuring a wide margin for the cutting processing temperature. Ratio R2 is, for example, 0 or more, 1 or more, or 2 or more.

[0031] The shear storage modulus of the pressure-sensitive adhesive sheet 10 at -30°C (first shear storage modulus) is preferably 120 kPa or less, more preferably 100 kPa or less, even more preferably 80 kPa or less, and even more preferably 70 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the pressure-sensitive adhesive sheet 10. The first shear storage modulus (-30°C) is preferably 45 kPa or more, more preferably 50 kPa or more, and even more preferably 55 kPa or more, from the viewpoint of ensuring good adhesiveness and handleability in the pressure-sensitive adhesive sheet 10.

[0032] The ratio (ratio R3) of the first shear storage modulus (-30°C) to the shear storage modulus (second shear storage modulus) of the pressure-sensitive adhesive sheet 10 at -20°C is preferably 1.8 or less, more preferably 1.7 or less, and even more preferably 1.6 or less, from the viewpoint of ensuring a stable stress relaxation function of the pressure-sensitive adhesive sheet 10 in the low temperature range. The ratio R3 is, for example, 0.9 or more, 1.0 or more, or 1.1 or more.

[0033] The shear storage modulus of the pressure-sensitive adhesive sheet 10 at 25°C (third shear storage modulus) is preferably 50 kPa or less, more preferably 40 kPa or less, even more preferably 30 kPa or less, and even more preferably 23 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good adhesiveness and handleability in the pressure-sensitive adhesive sheet 10, the third shear storage modulus (25°C) is preferably more than 18 kPa, more preferably 19 kPa or more, and even more preferably 20 kPa or more.

[0034] The shear storage modulus of the pressure-sensitive adhesive sheet 10 at 60°C (fourth shear storage modulus) is preferably 50 kPa or less, more preferably 40 kPa or less, even more preferably 30 kPa or less, and even more preferably 23 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the pressure-sensitive adhesive sheet 10. The fourth shear storage modulus (60°C) is preferably 13 kPa or more, more preferably 15 kPa or more, and even more preferably 17 kPa or more, from the viewpoint of ensuring good adhesiveness, cohesive strength, and handleability in the pressure-sensitive adhesive sheet 10.

[0035] The pressure-sensitive adhesive sheet 10 preferably has a maximum loss tangent tanδ (=shear loss modulus / shear storage modulus) between -50°C and 150°C, and more preferably has a maximum loss tangent tanδ in the low temperature range of -40°C or lower. From the viewpoint of ensuring the impact resistance of the pressure-sensitive adhesive sheet 10, this maximum value is preferably 1 or more, more preferably 1.2 or more, even more preferably 1.4 or more, and is preferably 3 or less, more preferably 2.5 or less, even more preferably 2 or less. The loss tangent tanδ of the pressure-sensitive adhesive sheet 10 is determined by dynamic viscoelasticity measurement, which will be described later in connection with the examples.

[0036] The thickness of the pressure-sensitive adhesive sheet 10 is preferably 45 μm or more, more preferably 48 μm or more, and even more preferably 50 μm or more, from the viewpoint of ensuring a good stress relaxation function in the pressure-sensitive adhesive sheet 10. The thickness of the pressure-sensitive adhesive sheet 10 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 70 μm or less, from the viewpoint of thinning the flexible device.

[0037] The moisture permeability of the pressure-sensitive adhesive sheet 10 measured under conditions of 40°C and a relative humidity of 92% is preferably 400 g / m from the viewpoint of suppressing swelling of the pressure-sensitive adhesive sheet 10 in a humid environment. 2 24h or less, preferably 395g / m 2 24 hours or less, preferably 390g / m 2 24 hours or less, more preferably 380 g / m 2 24 hours or less. The moisture permeability of the pressure-sensitive adhesive sheet 10 refers to the moisture permeability when the thickness of the pressure-sensitive adhesive sheet 10 is 50 μm. A low-moisture permeability pressure-sensitive adhesive sheet 10 is suitable for suppressing partial swelling of the edges of the pressure-sensitive adhesive sheet 10 when the pressure-sensitive adhesive sheet 10 is used to bond adherends (swelling occurs due to moisture penetration into the edges). Suppressing partial swelling at the edges of the pressure-sensitive adhesive sheet 10 is suitable for suppressing peeling of the edges from the adherend. Methods for adjusting the moisture permeability of the pressure-sensitive adhesive sheet 10 include, for example, selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight, and adjusting the amount of the base polymer. Selecting the type of base polymer includes selecting the type and amount of the side chain of the base polymer. Selecting the type of side chain of the base polymer includes adjusting the length of the alkyl moiety in the side chain and the type and amount of the functional group contained in the side chain. Methods for adjusting the moisture permeability of the pressure-sensitive adhesive sheet 10 also include selecting the type and amount of additives other than the base polymer. The method for measuring the moisture permeability of the pressure-sensitive adhesive sheet 10 is as described below in the examples.

[0038] The dielectric constant D1 of the PSA sheet 10 at 100 kHz (the dielectric constant before humidification, described below) is preferably 4.0 or less, more preferably 3.8 or less, and even more preferably 3.6 or less, from the viewpoint of achieving good sensing sensitivity in the touch sensor provided in the display panel. The dielectric constant D1 is, for example, 3.0 or more, 3.3 or more, or 3.5 or more. Methods for adjusting the dielectric constant D1 include, for example, selecting the type of base polymer in the PSA sheet 10, adjusting the molecular weight, and adjusting the blending amount. Selecting the type of base polymer includes selecting the type and adjusting the amount of the side chain of the base polymer. Selecting the type of side chain of the base polymer includes adjusting the length of the alkyl moiety in the side chain and selecting the type and adjusting the amount of the functional group contained in the side chain. Methods for adjusting the dielectric constant D1 also include selecting the type and adjusting the blending amount of additives other than the base polymer (the same applies to the dielectric constant D2, described below). Specific methods for measuring the dielectric constant are as described below in the Examples.

[0039] The dielectric constant D2 of the PSA sheet 10 after 24 hours in an environment of 40°C and 92% relative humidity (after humidification) is preferably 4.0 or less, preferably 3.8 or less, and more preferably 3.6 or less, from the viewpoint of realizing good sensing sensitivity in a humidified environment in a touch sensor provided in a display panel. The dielectric constant D2 is, for example, 2.8 or more, 3.0 or more, or 3.2 or more.

[0040] From the viewpoint of obtaining stable dielectric properties in the adhesive sheet 10, the ratio of the relative dielectric constant D2 to the relative dielectric constant D1 (D2 / D1) is preferably 0.80 or more, more preferably 0.85 or more, and is preferably 1.1 or less, more preferably 1.05 or less.

[0041] The adhesive strength F1 of the pressure-sensitive adhesive sheet 10 in a peel test (first peel test) under conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 2.0 N / 10 mm or more, more preferably 2.2 N / 10 mm or more, from the viewpoint of suppressing peeling of the pressure-sensitive adhesive sheet 10 from an adherend in the room temperature region. The adhesive strength F1 refers to the adhesive strength to a polyimide (PI) film at 25°C. Specific methods for measuring the adhesive strength F1 are as described below in the Examples. Methods for adjusting the adhesive strength F1 include, for example, selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight, and adjusting the blending amount. Selecting the type of base polymer includes adjusting the composition of the monomers that form the base polymer. Methods for adjusting the adhesive strength F1 also include selecting the type of components other than the base polymer in the pressure-sensitive adhesive sheet 10 and adjusting the blending amount of these components. Examples of such components include crosslinkers, silane coupling agents, and oligomers. The above-mentioned adhesive strength adjustment methods also apply to the adhesive strength F2 described below.

[0042] The adhesive strength F2 of the pressure-sensitive adhesive sheet 10 in a peel test (second peel test) under conditions of 65°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 1.3 N / 10 mm or more, preferably 1.5 N / 10 mm or more, and more preferably 1.7 N / 10 mm or more, from the viewpoint of suppressing peeling of the pressure-sensitive adhesive sheet 10 from the adherend in the high temperature range. The adhesive strength F2 refers to the adhesive strength to a PI film at 65°C. The specific method for measuring the adhesive strength F2 is as described below in the Examples.

[0043] The adhesive sheet 10 is a sheet-shaped pressure-sensitive adhesive formed from an adhesive composition. The adhesive sheet 10 (adhesive composition) contains at least a base polymer.

[0044] The base polymer is an adhesive component that imparts adhesiveness to the pressure-sensitive adhesive sheet 10. Examples of base polymers include acrylic polymers, silicone polymers, polyester polymers, polyurethane polymers, polyamide polymers, polyvinyl ether polymers, vinyl acetate / vinyl chloride copolymers, modified polyolefin polymers, epoxy polymers, fluoropolymers, and rubber polymers. The base polymers may be used alone or in combination of two or more. From the viewpoint of ensuring good transparency and adhesiveness in the pressure-sensitive adhesive sheet 10, acrylic polymers are preferred as the base polymer.

[0045] An acrylic polymer is a copolymer of monomer components containing 50% by mass or more of (meth)acrylic acid ester. "(Meth)acrylic" means acrylic and / or methacrylic.

[0046] As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid alkyl ester is used, and more preferably, a (meth)acrylic acid alkyl ester in which the number of carbon atoms in the alkyl group is 1 to 20. The (meth)acrylic acid alkyl ester may have a linear or branched alkyl group, or may have an alicyclic alkyl group.

[0047] Examples of (meth)acrylic acid alkyl esters having a linear or branched alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate. , nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (i.e., lauryl (meth)acrylate), isotridecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, and nonadecyl (meth)acrylate.

[0048] Examples of (meth)acrylic acid alkyl esters having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl esters, (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring, and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring. Examples of (meth)acrylic acid cycloalkyl esters include cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate. Examples of (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring include isobornyl (meth)acrylate. Examples of (meth)acrylic acid esters having three or more aliphatic hydrocarbon rings include dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0049] As the (meth)acrylic acid alkyl ester, from the viewpoint of achieving a balance between the flexibility and adhesive strength required of an adhesive sheet for flexible device applications and the low moisture permeability of the adhesive sheet, preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group of 6 to 14 carbon atoms is used, more preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group of 8 to 12 carbon atoms is used, and even more preferably at least two selected from (meth)acrylic acid alkyl esters having an alkyl group of 8 to 12 carbon atoms are used. Preferred (meth)acrylic acid alkyl esters having an alkyl group of 6 to 14 carbon atoms are 2-ethylhexyl acrylate (2EHA), n-octyl acrylate (NOAA), isononyl acrylate (INAA), and lauryl acrylate (LA).

[0050] The proportion of the (meth)acrylic acid alkyl ester in the monomer components is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more, from the viewpoint of appropriately achieving flexibility, adhesive strength, and low moisture permeability in the pressure-sensitive adhesive sheet 10. This proportion is, for example, 99.9% by mass or less, 99.5% by mass or less, or 99% by mass or less. When a first (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group containing 8 to 12 carbon atoms and a second (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group containing 8 to 12 carbon atoms are used in combination, the proportion of the first (meth)acrylic acid alkyl ester in the monomer components is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less. The proportion of the second (meth)acrylic acid alkyl ester in the monomer component is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 65% ​​by mass or less.

[0051] The monomer component may include a copolymerizable monomer copolymerizable with the (meth)acrylic acid alkyl ester. Examples of the copolymerizable monomer include a monomer having a polar group. Examples of the polar group-containing monomer include a hydroxy group-containing monomer, a monomer having a nitrogen atom-containing ring, and a carboxy group-containing monomer. The polar group-containing monomer is useful for modifying the acrylic polymer, such as by introducing crosslinking points into the acrylic polymer and ensuring the cohesive strength of the acrylic polymer.

[0052] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Preferably, the hydroxyl group-containing monomer is at least one selected from the group consisting of 2-hydroxyethyl acrylate (2HEA) and 4-hydroxybutyl acrylate (4HBA).

[0053] The proportion of the hydroxy group-containing monomer in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. From the viewpoint of adjusting the polarity of the acrylic polymer (which is related to the compatibility between the acrylic polymer and various additive components in the pressure-sensitive adhesive sheet 10), this proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0054] Examples of monomers having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, and N-vinylisothiazole.

[0055] When a monomer having a nitrogen atom-containing ring is used, the proportion of the monomer having a nitrogen atom-containing ring in the monomer components is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.5% by mass or more, from the viewpoints of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10 and ensuring the adhesive strength to the adherend of the pressure-sensitive adhesive sheet 10. This proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and adjusting the polarity of the acrylic polymer (which is related to the compatibility of the acrylic polymer with various additive components in the pressure-sensitive adhesive sheet 10).

[0056] Examples of carboxy group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.

[0057] When a carboxyl group-containing monomer is used, the proportion of the carboxyl group-containing monomer in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.8% by mass or more, from the viewpoints of introducing a crosslinked structure into the acrylic polymer, ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10, and ensuring the adhesive strength to the adherend in the pressure-sensitive adhesive sheet 10. The proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and avoiding the risk of corrosion of the adherend by acid.

[0058] The proportion of the polar group-containing monomer in the monomer component (when multiple polar group-containing monomers are included, the proportion of the total amount of the multiple polar group-containing monomers) is preferably 7% by mass or less, more preferably 5% by mass or less, even more preferably 3.5% by mass or less, and particularly preferably 3% by mass or less, from the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the flexibility of the pressure-sensitive adhesive sheet 10. This proportion is, for example, 0.1% by mass or more, 0.5% by mass or more, or 0.8% by mass or more.

[0059] The monomer component may contain other copolymerizable monomers. Examples of the other copolymerizable monomers include acid anhydride monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, alkoxy group-containing monomers, and aromatic vinyl compounds. These other copolymerizable monomers may be used alone or in combination of two or more.

[0060] The monomer components forming the base polymer preferably include a (meth)acrylic acid alkyl ester and a polar group-containing monomer, and more preferably include a (meth)acrylic acid alkyl ester having an alkyl group with 8 to 12 carbon atoms and a hydroxy group-containing monomer. In this case, the proportion of the hydroxy group-containing monomer in the total amount of the (meth)acrylic acid alkyl ester and the hydroxy group-containing monomer is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. From the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the flexibility of the pressure-sensitive adhesive sheet 10, this proportion is preferably 5 mass% or less, more preferably 3.5 mass% or less, even more preferably 3 mass% or less, still more preferably 2 mass% or less, and even more preferably 1.5 mass% or less.

[0061] The base polymer preferably has a crosslinked structure. Examples of methods for introducing a crosslinked structure into a base polymer include the following first and second methods. In the first method, a base polymer having functional groups reactive with the crosslinking agent and the crosslinking agent are blended into a pressure-sensitive adhesive composition, and the base polymer and the crosslinking agent are reacted in a pressure-sensitive adhesive sheet. In the second method, a polyfunctional compound is included as a crosslinking agent in the monomer components forming the base polymer, and a base polymer having a branched structure (crosslinked structure) introduced into the polymer chain is formed by polymerization of the monomer components. These methods may be used in combination.

[0062] Examples of the crosslinking agent used in the first method include compounds that react with functional groups (such as hydroxyl groups and carboxyl groups) contained in the base polymer. Examples of such crosslinking agents include isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, and carbodiimide crosslinking agents. The crosslinking agents used in the first method may be used alone or in combination of two or more. As the crosslinking agent in the first method, an isocyanate crosslinking agent is preferably used because it has high reactivity with the hydroxyl groups and carboxyl groups in the base polymer and facilitates the introduction of a crosslinked structure.

[0063] Examples of isocyanate crosslinking agents include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, tetramethylxylylene diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, and polymethylene polyphenylisocyanate. Also included as isocyanate crosslinking agents are derivatives of these isocyanates. Examples of the isocyanate derivatives include isocyanurate-modified products and polyol-modified products. Commercially available isocyanate crosslinking agents include, for example, Coronate L (a trimethylolpropane adduct of tolylene diisocyanate, manufactured by Tosoh), Coronate HL (a trimethylolpropane adduct of hexamethylene diisocyanate, manufactured by Tosoh), Coronate HX (an isocyanurate of hexamethylene diisocyanate, manufactured by Tosoh), Takenate D110N (a trimethylolpropane adduct of xylylene diisocyanate, manufactured by Mitsui Chemicals), and Takenate 600 (1,3-bis(isocyanatomethyl)cyclohexane, manufactured by Mitsui Chemicals).

[0064] Peroxide crosslinking agents include dibenzoyl peroxide, di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, and t-butylperoxypivalate.

[0065] Epoxy crosslinkers include bisphenol A, epichlorohydrin-type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0066] The amount of crosslinking agent in the first method is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of base polymer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10, the amount of crosslinking agent in ...

[0067] In the second method, the monomer components (including a polyfunctional compound and a monofunctional monomer for introducing a crosslinked structure) may be polymerized in one step or in multiple steps. In the multi-step polymerization method, first, a monofunctional monomer for forming a base polymer is polymerized (prepolymerization), thereby preparing a prepolymer composition containing a partial polymer (a mixture of a low-polymerization polymer and unreacted monofunctional monomer). Next, a polyfunctional compound is added as a crosslinking agent to the prepolymer composition, and then a polymerization reaction is allowed to proceed in a reaction system containing the partial polymer and the polyfunctional compound (main polymerization).

[0068] Examples of polyfunctional compounds include polyfunctional monomers and polyfunctional oligomers containing two or more ethylenically unsaturated double bonds in one molecule, and examples of polyfunctional monomers include polyfunctional (meth)acrylates.

[0069] Examples of the polyfunctional (meth)acrylate include difunctional (meth)acrylate, trifunctional (meth)acrylate, and tetrafunctional or higher polyfunctional (meth)acrylate.

[0070] Examples of difunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, glycerin di(meth)acrylate, ethoxylated bisphenol A diacrylate (BPAEODE), and neopentyl glycol di(meth)acrylate.

[0071] Examples of trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(acryloyloxyethyl)isocyanurate.

[0072] Examples of tetrafunctional or higher polyfunctional (meth)acrylates include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0073] Examples of polyfunctional oligomers include urethane (meth)acrylate oligomers, polyester (meth)acrylate oligomers, polyether (meth)acrylate oligomers, polyol (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate.

[0074] The polyfunctional compound as the crosslinking agent in the second method may be used alone or in combination of two or more kinds. As the polyfunctional compound, a polyfunctional monomer is preferably used, and more preferably at least one selected from the group consisting of dipentaerythritol hexaacrylate (DPHA), 1,6-hexanediol diacrylate (HDDA), and trimethylolpropane triacrylate (TMPTA) is used.

[0075] The amount of the polyfunctional compound as a crosslinking agent in the monomer components is preferably 0.02 parts by mass or more, more preferably 0.04 parts by mass or more, and even more preferably 0.06 parts by mass or more per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. The amount of the polyfunctional compound is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10.

[0076] The acrylic polymer (base polymer) can be formed by polymerizing the above-mentioned monomer components. Examples of polymerization methods include solution polymerization, emulsion polymerization, and solvent-free photopolymerization (e.g., ultraviolet polymerization). Examples of solvents used in solution polymerization include ethyl acetate and toluene. A chain transfer agent may be used in the polymerization. Examples of polymerization initiators include thermal polymerization initiators and photopolymerization initiators. The polymerization initiators may be used alone or in combination. The amount of the polymerization initiator used is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.07 parts by mass or more, per 100 parts by mass of the monomer components. It is also preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less.

[0077] Examples of thermal polymerization initiators include azo polymerization initiators and peroxide polymerization initiators. Examples of azo polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid) dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, and 2,2'-azobis(2-amidinopropane) dihydrochloride. Examples of peroxide polymerization initiators include dibenzoyl peroxide, t-butyl permaleate, and lauroyl peroxide.

[0078] Examples of the photopolymerization initiator include a radical photopolymerization initiator, a cationic photopolymerization initiator, and an anionic photopolymerization initiator.

[0079] Examples of the radical photopolymerization initiator include an acylphosphine oxide photopolymerization initiator, a benzoin ether photopolymerization initiator, and an acetophenone photopolymerization initiator.

[0080] Examples of acylphosphine oxide photopolymerization initiators include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Examples of benzoin ether photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone.

[0081] The weight average molecular weight of the base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more, from the viewpoint of ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. The weight average molecular weight of the base polymer is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0082] The glass transition temperature (Tg) of the base polymer is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower. The glass transition temperature is, for example, −80° C. or higher.

[0083] The glass transition temperature (Tg) of the base polymer can be determined using the theoretical glass transition temperature calculated based on the Fox equation below. The Fox equation is a relationship between the glass transition temperature Tg of a polymer and the glass transition temperature Tgi of a homopolymer of the monomers constituting the polymer. In the Fox equation below, Tg represents the glass transition temperature (°C) of the polymer, Wi represents the weight fraction of monomer i constituting the polymer, and Tgi represents the glass transition temperature (°C) of the homopolymer formed from monomer i. Literature values ​​can be used for the glass transition temperature of the homopolymer. For example, the "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999) lists the glass transition temperatures of various homopolymers. Meanwhile, the glass transition temperature of a homopolymer of a monomer can also be determined using the method specifically described in JP 2007-51271 A.

[0084] Fox formula 1 / (273+Tg)=Σ[Wi / (273+Tgi)]

[0085] The pressure-sensitive adhesive composition may contain a silane coupling agent. The content of the silane coupling agent in the pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, relative to 100 parts by mass of the base polymer. The content is preferably 5 parts by mass or less, more preferably 3 parts by mass or less.

[0086] The PSA composition may contain other components as needed. Examples of the other components include solvents, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, UV absorbers, surfactants, and antistatic agents. Examples of the solvent include polymerization solvents used as needed during polymerization of the acrylic polymer, and solvents added to the polymerization reaction solution after polymerization. Examples of the solvent include ethyl acetate and toluene.

[0087] The PSA sheet 10 can be produced, for example, by applying the above-mentioned PSA composition to a release liner L1 (first release liner) to form a coating film, and then drying the coating film. The PSA sheet 10 may also be produced by applying the above-mentioned PSA composition to a release liner L1 (first release liner) to form a coating film, laminating a release liner L2 (second release liner) on top of the coating film, and then drying the coating film between the release liners.

[0088] The release liner L1 may be, for example, a flexible plastic film. Examples of such plastic films include polyester films such as polyethylene terephthalate films, polyethylene films, and polypropylene films. The thickness of the release liner L1 is, for example, 3 μm or more and, for example, 200 μm or less. The surface of the release liner L1 is preferably release-treated.

[0089] Examples of methods for applying the pressure-sensitive adhesive composition include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating. The drying temperature for the coating film is, for example, 50°C to 200°C. The drying time is, for example, 5 seconds to 20 minutes.

[0090] The release liner L2 is preferably a flexible plastic film whose surface has been subjected to a release treatment. The plastic films described above for the release liner L1 can be used as the release liner L2.

[0091] In this manner, adhesive sheet 10 can be manufactured in which adhesive surfaces 11, 12 are covered and protected by release liners L1, L2.

[0092] The haze of the pressure-sensitive adhesive sheet 10 is preferably 3% or less, more preferably 2% or less, and more preferably 1% or less. The haze of the pressure-sensitive adhesive sheet 10 can be measured using a haze meter in accordance with JIS K7136 (2000). Examples of haze meters include the "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. and the "HM-150" manufactured by Murakami Color Research Laboratory Co., Ltd.

[0093] The total light transmittance of the pressure-sensitive adhesive sheet 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. The total light transmittance of the pressure-sensitive adhesive sheet 10 is, for example, 100% or less. The total light transmittance of the pressure-sensitive adhesive sheet 10 can be measured in accordance with JIS K 7375 (2008).

[0094] 2A to 2C show an example of how the adhesive sheet 10 can be used.

[0095] In this method, first, as shown in FIG. 2A, an adhesive sheet 10 is attached to one surface in the thickness direction H of a first member 21 (adherend). The first member 21 is, for example, one element in the laminated structure of a flexible display panel. Examples of such elements include a pixel panel, a polarizing film, a touch panel, and a cover film (the same applies to the second member 22 described below). This step provides the adhesive sheet 10, which will be used for bonding to other members, on the first member 21.

[0096] 2B, one surface of the first member 21 in the thickness direction H is bonded to the other surface of the second member 22 in the thickness direction H via the adhesive sheet 10 on the first member 21. The second member 22 is, for example, another element in the laminated structure of the flexible display panel.

[0097] Next, as shown in FIG. 2C, the adhesive sheet 10 between the first member 21 and the second member 22 is aged. Aging increases the bonding strength between the adhesive sheet 10 and the members 21 and 22. The aging temperature is, for example, 20°C to 160°C. The aging time is, for example, 1 minute to 21 days. When aging is performed by autoclave treatment (heat and pressure treatment), the temperature is, for example, 30°C to 80°C, the pressure is, for example, 0.1 to 0.8 MPa, and the treatment time is, for example, 15 minutes or more. [Example]

[0098] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to these examples. The specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be substituted for the upper limits (numerical values ​​defined as "equal to or less than") or lower limits (numerical values ​​defined as "equal to or more than") of the corresponding blending amounts (contents), physical property values, parameters, etc. described in the above-mentioned "Description of the Invention."

[0099] Example 1 Preparation of Prepolymer Composition In a flask, 0.05 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name "Omnirad651", manufactured by IGM Resins) as a first photopolymerization initiator and 0.05 parts by mass of 1-hydroxycyclohexyl phenyl ketone (trade name "Omnirad184", manufactured by IGM Resins) as a second photopolymerization initiator were added to a monomer mixture containing 60 parts by mass of 2-ethylhexyl acrylate (2EHA), 39 parts by mass of lauryl acrylate (LA), and 1 part by mass of 4-hydroxybutyl acrylate (4HBA). The mixture was then irradiated with ultraviolet light under a nitrogen atmosphere to polymerize some of the monomer components in the mixture, thereby obtaining a first prepolymer composition (containing monomer components that had not undergone a polymerization reaction) with a polymerization rate of approximately 10%.

[0100] <Preparation of Pressure-Sensitive Adhesive Composition> A first adhesive composition was obtained by mixing 100 parts by mass of the first prepolymer composition, 0.06 parts by mass of dipentaerythritol hexaacrylate (DPHA) as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.).

[0101] <Formation of adhesive layer> A first pressure-sensitive adhesive composition was applied to the release-treated surface of a first release liner (product name "Diafoil MRF#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side to form a coating film. Next, the release-treated surface of a second release liner (product name "Diafoil MRE#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side was attached to the coating film on the first release liner. Next, ultraviolet light was irradiated onto the coating film between the release liners to photocure the coating film and form a pressure-sensitive adhesive layer (thickness 50 μm). For ultraviolet irradiation, a black light was used as the irradiation light source, and the irradiation intensity was 5 mW / cm. 2 It was decided.

[0102] In this manner, a pressure-sensitive adhesive sheet (50 μm thick) with a double-sided release liner was prepared for Example 1. The composition of the pressure-sensitive adhesive sheet for Example 1 is shown in Table 1 in units of "parts by mass" (the same applies to the examples and comparative examples described below).

[0103] Example 2 An adhesive sheet of Example 2 with a double-sided release liner was produced in the same manner as the adhesive sheet of Example 1, except that in preparing the prepolymer composition, the amount of 2EHA was 51 parts by mass and the amount of LA was 48 parts by mass.

[0104] Example 3 An adhesive sheet of Example 3 with a double-sided release liner was produced in the same manner as the adhesive sheet of Example 1, except that in preparing the prepolymer composition, the amount of 2EHA was set to 58 parts by mass and the amount of 4HBA was set to 3 parts by mass.

[0105] Example 4 First, in a flask, 0.05 parts by mass of a first photopolymerization initiator (Omnirad651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad184) were added to a monomer mixture containing 29 parts by mass of n-octyl acrylate (NOAA), 70 parts by mass of 2EHA, and 1 part by mass of 4HBA. The mixture was then irradiated with ultraviolet light under a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a second prepolymer composition with a polymerization rate of approximately 10%.

[0106] Next, 100 parts by mass of the second prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a second pressure-sensitive adhesive composition.

[0107] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in Example 1, except that the second adhesive composition was used instead of the first adhesive composition.

[0108] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) of Example 4 with double-sided release liners was produced.

[0109] Example 5 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad184) were added to a monomer mixture containing 70 parts by mass of isononyl acrylate (INAA), 29 parts by mass of LA, and 1 part by mass of 4HBA in a flask. Then, the mixture was irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a third prepolymer composition with a polymerization rate of approximately 10%.

[0110] Next, 100 parts by mass of the third prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a third pressure-sensitive adhesive composition.

[0111] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in Example 1, except that the third adhesive composition was used instead of the first adhesive composition.

[0112] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners of Example 5 was prepared.

[0113] Example 6 The pressure-sensitive adhesive sheet of Example 6 with double-sided release liner was produced in the same manner as the pressure-sensitive adhesive sheet of Example 4, except that in preparing the prepolymer composition, the amount of 2EHA was 50 parts by mass and the amount of NOAA was 49 parts by mass.

[0114] Comparative Example 1 A pressure-sensitive adhesive sheet with a double-sided release liner of Comparative Example 1 was produced in the same manner as the pressure-sensitive adhesive sheet of Example 1, except for the following: In preparing the prepolymer composition, the blend amounts of 2EHA were 56 parts by mass, LA were 34 parts by mass, 4HBA were 7 parts by mass, and 2 parts by mass of N-vinyl-2-pyrrolidone (NVP) were blended. In preparing the pressure-sensitive adhesive composition, 1 part by mass of the following acrylic oligomer was further blended.

[0115] Preparation of Oligomers First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 60 parts by weight of dicyclopentanyl methacrylate (DCPMA), 40 parts by weight of methyl methacrylate (MMA), 3.5 parts by weight of α-thioglycerol as a chain transfer agent, and 100 parts by weight of toluene as a solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was then reacted under a nitrogen atmosphere at 70°C for 1 hour and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove the toluene, chain transfer agent, and unreacted monomer. This yielded an acrylic oligomer (solid) as a hydrophobic oligomer without polar groups. The weight-average molecular weight of this acrylic oligomer was 5100.

[0116] Comparative Example 2 An adhesive sheet of Comparative Example 2 with a double-sided release liner was produced in the same manner as the adhesive sheet of Example 5, except that in preparing the prepolymer composition, the amount of INAA blended was 50 parts by mass and the amount of LA blended was 49 parts by mass.

[0117] <Moisture permeability> The moisture permeability was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 6 and Comparative Examples 1 and 2. Specifically, the results are as follows.

[0118] First, the pressure-sensitive adhesive sheet with double-sided release liners was left to stand for 3 days in an atmosphere at a temperature of 23°C and a relative humidity of 55%. This adjusted the condition of the pressure-sensitive adhesive sheet. Next, one of the release liners was peeled off from the pressure-sensitive adhesive sheet, and the exposed surface was then covered with a 25 μm-thick triacetyl cellulose (TAC) film (moisture permeability: 1070 g / m 2 The adhesive sheet on the TCA film was then peeled off from the other release liner, yielding a sample film for measuring moisture permeability.

[0119] Next, the moisture permeability in the thickness direction of the PSA sheet was measured in accordance with the moisture permeability test (cup method) of JIS Z0208. Specifically, first, a predetermined amount of calcium chloride weighed in advance was placed in a test cup (an aluminum cup with a circular opening of 30 mm diameter, used in the cup method of JIS Z0208), and the opening of the cup was blocked with a sample film. The area of ​​the sample film blocking the opening of the cup was equivalent to the area of ​​a circle with a diameter of 30 mm. Next, the cup with the sample film was placed in a constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 90%, and left for 24 hours. Next, the calcium chloride removed from the cup was weighed. The increased mass (g) of calcium chloride was calculated by multiplying the area (m²) of the sample film blocking the opening of the cup. 2 The value was divided by the moisture permeability (g / m 2 The moisture permeability obtained in this manner is the moisture permeability of the adhesive sheet with TAC film, but since the moisture permeability of the TAC film is significantly greater than that of the adhesive sheet, the moisture permeability of the sample film was considered to be that of the adhesive sheet.

[0120] <Relative permittivity> The relative dielectric constant was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 6 and Comparative Examples 1 and 2. Specifically, the results are as follows.

[0121] First, a measurement sample was prepared by sandwiching the adhesive sheet between copper foil and an electrode. Next, the dielectric constant of the measurement sample was measured at a frequency of 100 kHz under the following conditions (first dielectric constant measurement) using an Agilent Technologies Precision Impedance Analyzer 4294A in accordance with JIS K6911. The measurement results are shown in Tables 1 and 2 as the dielectric constant D1 of the adhesive sheet at 100 kHz.

[0122] [Measurement conditions for relative permittivity] Electrode configuration: 12.1 mm diameter and 0.5 mm thick aluminum plate Counter electrode: 3oz copper plate Measurement environment: Temperature 25°C, relative humidity 50%

[0123] Furthermore, the adhesive sheet was subjected to a humidification treatment, and then the dielectric constant of the adhesive sheet was measured (second dielectric constant measurement). For the humidification treatment, the adhesive sheet was stored for 24 hours in an environment of 40°C and a relative humidity of 92%. The method for measuring the second dielectric constant was the same as the first dielectric constant measurement method described above. The measurement results are shown in Tables 1 and 2 as the dielectric constant D2 at 100 kHz after humidification of the adhesive sheet. The ratio of the dielectric constant D2 to the dielectric constant D1 described above (D2 / D1) is also shown in Tables 1 and 2.

[0124] <Shear storage modulus> For each of the pressure-sensitive adhesive sheets of Examples 1 to 6 and Comparative Examples 1 and 2, the dynamic viscoelasticity was measured.

[0125] For each adhesive sheet, the required number of measurement samples were prepared. Specifically, first, a plurality of adhesive sheet pieces cut from the adhesive sheet were bonded together to prepare a sample sheet with a thickness of approximately 1.5 mm. Next, this sheet was punched out to obtain cylindrical pellets (7.9 mm in diameter) as measurement samples.

[0126] The measurement sample was then fixed to a parallel plate jig with a diameter of 7.9 mm using a dynamic viscoelasticity measuring device (product name "Discovery Hybrid Reometer-2 (DHR-2)", manufactured by TA Instruments), and dynamic viscoelasticity measurement was performed. In this measurement, the measurement mode was shear mode, the measurement temperature range was -50°C to 150°C, the heating rate was 5°C / min, and the frequency was 1 Hz.

[0127] From the measurement results, the shear storage modulus G' and shear loss modulus G" were read at specified temperatures (-30°C, -20°C, 25°C, 60°C). The shear storage modulus G' and shear loss modulus G" at each temperature are shown in Tables 1 and 2. The ratio of the shear storage modulus G' (first shear storage modulus) at -30°C to the shear storage modulus G' (second shear storage modulus) at -20°C is also shown in Tables 1 and 2. The ratio of the shear loss modulus G" (first shear loss modulus) at -30°C to the shear loss modulus G" (second shear loss modulus) at 60°C, and the ratio of the shear loss modulus G" (first shear loss modulus) at -30°C to the shear loss modulus G" (third shear loss modulus) at -20°C are also shown in Tables 1 and 2. Furthermore, from the measurement results, the maximum value of the loss tangent tanδ (= shear loss modulus G" / shear storage modulus G') was read out from -50°C to 150°C. These values ​​are also shown in Tables 1 and 2.

[0128] <180° peel test> For each of the pressure-sensitive adhesive sheets of Examples 1 to 6 and Comparative Examples 1 and 2, the adhesive strength to the adherend was examined by a 180° peel test.

[0129] Specifically, the required number of measurement samples were prepared for each pressure-sensitive adhesive sheet. To prepare the measurement samples, the first release liner was first peeled from the pressure-sensitive adhesive sheet, and the resulting exposed surface was bonded to a plasma-treated polyethylene terephthalate (PET) film (product name "Lumirror S10", 50 μm thick, manufactured by Toray Industries, Inc.) to obtain a laminate. The plasma treatment was performed using a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) at a voltage of 160 V, a frequency of 10 kHz, and a treatment speed of 5000 mm / min. Next, a test piece (10 mm wide x 100 mm long) was cut from the laminate (PET film / pressure-sensitive adhesive sheet / second release liner). Next, the second release liner was peeled from the pressure-sensitive adhesive sheet of this test piece, and the resulting exposed surface was bonded to a plasma-treated polyimide (PI) film (product name "GV200", 80 μm thick, manufactured by Kolon Co., Ltd.). Next, the PI film with the adhesive sheet (test piece) was subjected to a heating and pressure treatment at a temperature of 50°C and a pressure of 0.5 MPa for 15 minutes. This resulted in the test piece being pressure-bonded to the PI film. In this way, a measurement sample was prepared.

[0130] Next, the test sample was left to stand at room temperature for 30 minutes, after which a 180° peel test was performed to peel the test piece from the PI film on the test sample, and the force required for peeling (peel strength) was measured (first peel test). This measurement was performed using a tensile tester (product name "Autograph AG-50NX plus" manufactured by Shimadzu Corporation). The measurement temperature was 25°C, the relative humidity was 55%, the test piece was peeled from the PI film at a 180° angle, the test piece was pulled at a speed of 60 mm / min, and the peel length was 50 mm. The average measured peel strength is shown in Tables 1 and 2 as adhesive strength F1 (N / 10 mm).

[0131] On the other hand, a peel test (second peel test) was conducted under the same conditions as the first peel test, except that the measurement temperature was changed to 65°C. The measurement results are shown in Tables 1 and 2 as adhesive strength F2 (N / 10 mm).

[0132] <Bending test> The pressure-sensitive adhesive sheets of Examples 1 to 6 and Comparative Examples 1 and 2 were subjected to a bending test as follows.

[0133] First, the second release liner was peeled off from the pressure-sensitive adhesive sheet with double-sided release liner, and the exposed surface was plasma-treated. Meanwhile, both sides (first and second sides) of a 51 μm-thick polarizing film were also plasma-treated. The surface of an 80 μm-thick transparent polyimide film and the surface of a 125 μm-thick polyethylene terephthalate (PET) film were also plasma-treated. For each plasma treatment, a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) was used, with a voltage of 160 V, a frequency of 10 kHz, and a treatment speed of 5000 mm / min. The exposed surface of the pressure-sensitive adhesive sheet was then bonded to the first side of the polarizing film. For this bonding, the pressure-sensitive adhesive sheet with the first release liner and the polarizing film were pressed together by moving a 2 kg roller back and forth once in an environment of 23°C. Next, after peeling the first release liner from the adhesive sheet with polarizing film, the transparent polyimide film was bonded to the exposed surface of the adhesive sheet. Next, the PET film was bonded to the second surface of the polarizing film via a 15 μm thick thin and strong adhesive sheet. In this bonding, the polarizing film and the PET film were pressure-bonded by moving a 2 kg roller back and forth once in an environment of 23°C. This resulted in a laminated film having a laminated structure of a PET film (thickness 125 μm), a thin and strong adhesive sheet (thickness 15 μm), a polarizing film (thickness 51 μm), an adhesive sheet (thickness 50 μm), and a transparent polyimide film (thickness 80 μm).

[0134] Next, a test piece for evaluation was cut out from the laminated film thus prepared. Specifically, a rectangular test piece measuring 35 mm × 100 mm was cut out from the laminated film so that the absorption axis direction of the polarizing film was parallel to the long side direction of the cut test piece. Next, the test piece was autoclaved for 15 minutes under conditions of 35°C and 0.50 MPa.

[0135] Next, a bending test was performed on the test specimen using a sheet-shaped unloaded U-shaped expansion / contraction testing machine (manufactured by Yuasa System Co., Ltd.) (first bending test). In this test, as shown in FIG. 3A, bending jigs 201 and 202 of the testing machine were attached to both ends of the long side of the test specimen 100, and the test specimen 100 was fixed to the testing machine. Each of the bending jigs 201 and 202 held the test specimen 100 within a 20 mm range from the edge. A central 60 mm region of the long side of the test specimen 100 was not fixed to the bending jigs 201 and 202. In this test, the test specimen 100 was repeatedly deformed (bent) 200,000 times at a bending speed of 60 rpm in a thermostatic chamber at a temperature of −20°C between a bent configuration (FIG. 3B) in which the PET film side was facing inward and an unbent configuration (FIG. 3A). Specifically, the bent shape in this test is a shape in which the axial direction of the bending moment acting on the test piece 100 is perpendicular to the absorption axis direction of the polarizing film. In this bent shape, the bend radius of the test piece 100 was 1.3 mm, and the bend angle was 180°. The bent portion 100a of the test piece 100 that had been repeatedly bent was observed, and the adhesion of the pressure-sensitive adhesive sheet to the adherend in the bending test was evaluated as "good" when no peeling occurred between the pressure-sensitive adhesive sheet and the adherend (transparent polyimide film, polarizing film), and as "poor" when peeling occurred. The evaluation results are shown in Tables 1 and 2.

[0136] On the other hand, a bending test (second bending test) was carried out on a test piece that had not undergone the first bending test under the same conditions as the first bending test, except that the temperature was changed to 25°C. The evaluation results are shown in Tables 1 and 2.

[0137] Each of the PSA sheets of Examples 1 to 6 had a shear storage modulus (-20°C) of 70 kPa or less, and a ratio (ratio R1) of the first shear loss modulus (-30°C) to the second shear loss modulus (60°C) of 14 or less. Each of these PSA sheets of Examples 1 to 6 exhibited good adhesion to the adherend in both the first flex test (-20°C) and the second flex test (25°C). In contrast, the PSA sheet of Comparative Example 1 did not have a shear storage modulus of 70 kPa or less, did not have a ratio R1 of 14 or less, and did not exhibit good adhesion to the adherend in the second flex test (25°C). The PSA sheet of Comparative Example 2 did not have a ratio R1 of 14 or less, and did not exhibit good adhesion to the adherend in the second flex test (25°C).

[0138] [Table 1]

[0139] [Table 2] [Explanation of symbols]

[0140] 10 Adhesive sheet (optical adhesive sheet) 11,12 Adhesive surface H thickness direction L1, L2 release liner 21 First member 22 Second member

Claims

1. An optical adhesive sheet, having a shear storage modulus of 70 kPa or less at −20° C.; An optical adhesive sheet having a ratio of a first shear loss modulus at -30°C to a second shear loss modulus at 60°C of 14 or less.

2. The optical adhesive sheet according to claim 1 , wherein the first shear loss modulus is 100 kPa or less.

3. The optical adhesive sheet according to claim 1, wherein the ratio of the first shear loss modulus to the third shear loss modulus at -20°C is 2.8 or less.

4. The optical adhesive sheet according to claim 3 , wherein the third shear loss modulus is 50 kPa or less.

5. The optical adhesive sheet according to claim 1, wherein the loss tangent tanδ has a maximum value of 1 or more and 3 or less at -50 ° C. to 150 ° C.

6. Moisture permeability measured at 40°C and 92% relative humidity is 400g / m 2 The optical adhesive sheet according to claim 1, wherein the durability is 24 hours or less.

7. 7. The optical adhesive sheet according to claim 1, which has an adhesive strength of 2.0 N / 10 mm or more in a peel test under conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min.