Manufacturing method of battery
The CO2 laser-based welding method addresses the challenge of carbonization in infrared welding, ensuring rapid and effective sealing in battery manufacturing.
Patent Information
- Application Number
- JP2023086697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-26
AI Technical Summary
In existing battery manufacturing methods, infrared irradiation for sealing member welding results in carbonization, making it difficult to ensure sufficient welding in a short time.
A battery manufacturing method using CO2 laser irradiation with specific power and scanning speed to thermally weld sealing members, employing polyolefin films and optimizing laser parameters to prevent carbonization.
Ensures sufficient welding in a short time while minimizing carbonization, enhancing sealing performance and efficiency.
Smart Images

Figure 2024169874000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a battery. [Background technology]
[0002] In the method for manufacturing an electricity storage device disclosed in Patent Document 1, a laminate is prepared that includes a plurality of current collectors provided with active material layers and a plurality of frame-shaped sealing members. In the laminate, the sealing members are disposed between the plurality of current collectors. Infrared rays are irradiated to melt the sealing members, thereby forming a side surface that is made up of the sealing members and includes a communication port. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2023-000059 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors have discovered the following problems. In such a method for manufacturing an electricity storage device, infrared rays are applied to melt the sealing member. In order to shorten the manufacturing time, the output of the infrared rays is increased. This causes the surface of the sealing member to be carbonized. As a result, it is difficult to ensure sufficient welding.
[0005] The present disclosure has been made in consideration of the above-mentioned problems, and provides a method for manufacturing a battery that can ensure sufficient welding in a short period of time. [Means for solving the problem]
[0006] A method for manufacturing a battery according to the present disclosure includes: The electrode assembly includes a plurality of electrode bodies and a sealing portion. The plurality of electrode bodies are stacked, The sealing portion includes a welding portion that seals between ends of the plurality of electrode bodies, The method includes a step of irradiating a CO2 laser onto a plurality of sealing members disposed between the ends of the plurality of electrode bodies, thereby heating and welding the plurality of sealing members to form the welded portions.
[0007] In the above-described battery manufacturing method, the CO2 laser may be irradiated using a galvano scanner in the step.
[0008] In the above-described battery manufacturing method, the output of the CO2 laser may be 100 W or more and 300 W or less, and the scanning speed of the CO2 laser may be 4000 mm / sec or more and 6000 mm / sec or less.
[0009] In the above-described method for manufacturing a battery, the plurality of sealing members may preferably contain polyolefin.
[0010] In addition, in the above-mentioned battery manufacturing method, the multiple sealing members are films having a thickness of 120 μm, and when light having a wavelength of 9.4 μm is irradiated onto the film and the optical axis of the light extends in the thickness direction of the film, the absorptance of the light by the film is preferably 10% or more and 30% or less. Effect of the Invention
[0011] According to the present disclosure, sufficient welding can be ensured in a short period of time. [Brief description of the drawings]
[0012] [Figure 1] 4 is a flowchart showing a method for manufacturing a battery according to the first embodiment. [Figure 2A] 1 is a schematic diagram showing a step of a method for producing a battery according to a first embodiment. [Figure 2B] 1 is a schematic diagram showing a step of a method for producing a battery according to a first embodiment. [Figure 2C]1 is a schematic diagram showing a step of a method for producing a battery according to a first embodiment. [Figure 2D] FIG. 2D is a view taken along the arrow AA in FIG. 2C. [Figure 2E] 1 is a schematic diagram showing a step of a method for producing a battery according to a first embodiment. [Figure 3A] 4 is a schematic diagram showing a step of a first modified example of the manufacturing method for the battery according to the first embodiment. FIG. [Figure 3B] 4 is a schematic diagram showing a step of a first modified example of the manufacturing method for the battery according to the first embodiment. FIG. [Figure 4A] 2 is a schematic diagram showing a step of an example in which the battery manufacturing method according to the first embodiment is applied. FIG. [Figure 4B] 3 is a schematic diagram showing details of one step in an example to which the battery manufacturing method according to the first embodiment is applied. FIG. [Figure 5A] 1 is a graph showing absorptance versus light wavelength. [Figure 5B] FIG. 13 is a schematic diagram showing a method for calculating an integrated absorption amount with respect to a depth from an incident surface. [Figure 5C] FIG. 13 is a schematic diagram showing a method for calculating an integrated absorption amount with respect to a depth from an incident surface. [Figure 5D] 1 is a graph showing the amount of absorption and the integrated amount of absorption versus the depth from the incident surface. [Figure 5E] 1 is a graph showing the amount of absorption and the integrated amount of absorption versus the depth from the incident surface. [Figure 5F] 1 is a graph showing the amount of absorption and the integrated amount of absorption versus the depth from the incident surface. [Figure 6] 4 is a schematic diagram showing a step of a second modified example of the method for producing a battery according to the first embodiment. FIG. [Figure 7A] 4 is a schematic diagram showing a step of a third modified example of the method for producing a battery according to the first embodiment. FIG. [Figure 7B] 1 is a schematic diagram showing a main part of a battery according to a first embodiment. [Figure 8A] 4 is a schematic diagram showing a step of Example 2 in which the battery manufacturing method according to the first embodiment was carried out. FIG. [Figure 8B]4 is a schematic diagram showing a step of Example 2 in which the battery manufacturing method according to the first embodiment was carried out. FIG. [Figure 9] 1 is a schematic diagram showing a main part of a battery according to a technique related to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (Related Technology) Prior to describing specific embodiments to which the present disclosure is applied, a battery according to a technique related to the present disclosure will be described with reference to Fig. 9. Fig. 9 is a schematic diagram showing a main part of a battery according to a technique related to the present disclosure.
[0014] As shown in FIG. 9, the battery 900 includes a plurality of electrode bodies 90. The plurality of electrode bodies 90 are stacked. Each electrode body 90 includes a negative electrode 92, a foil 94, a positive electrode 91, a separator 93, and a resin film 95. The negative electrode 92, the foil 94, the positive electrode 91, and the separator 93 are stacked in this order. The negative electrode 92, the foil 94, the positive electrode 91, and the separator 93 are, for example, a film-like body or a plate-like body extending in a substantially square or substantially rectangular shape. When the battery 900 is viewed from above (here, the positive direction of the Z axis), the foil 94 and the separator 93 may include the negative electrode 92 and the positive electrode 91. The resin film 95 may extend in a frame shape to cover the ends of the foil 94 and the separator 93. The resin film 95 may extend in a frame shape so as to include the ends of the negative electrode 92 and the positive electrode 91. The welded portion A9 of the resin film 95 is formed on one side of the stacked electrode bodies 90. The welded portion A9 is formed using infrared rays. Specifically, infrared rays are irradiated onto the entire side of the stacked resin films 95 to heat the entire side of the stacked resin films 95. As a result, the resin films 95 are welded together to form the welded portion A9. The welded portion A9 extends over the entire side of the stacked resin films 95. Therefore, infrared energy and the time for irradiating the infrared rays are required to form the welded portion A9.
[0015] Hereinafter, the best mode for carrying out the present invention will be described with reference to the accompanying drawings. However, the present invention is not limited to the following mode. In addition, the following description and drawings have been appropriately simplified for clarity of explanation.
[0016] <Embodiment 1> A method of manufacturing the battery according to the first embodiment will be described with reference to FIGS. 1 and 2A to 2D.
[0017] It should be noted that the right-handed XYZ coordinate system shown in Fig. 2A and other drawings is of course for the convenience of explaining the positional relationship of the components. Usually, the Z axis positive direction is vertically upward, which is the direction in which the electrode body 10 described later is stacked, and the XY plane is a horizontal plane, which is common to all drawings. Also, in Figs. 2A, 2B, 7B, 8A, etc., cross sections are shown, but hatching is omitted for ease of viewing.
[0018] As shown in FIG. 2A, electrode assemblies 10 are laminated to form a laminate 100 (step ST1).
[0019] The electrode assembly 10 includes a negative electrode 2, a foil 4, a positive electrode 1, a separator 3, and a resin film 5. The foil 4 is, for example, a current collector. The negative electrode 2, the foil 4, the positive electrode 1, and the separator 3 are laminated in this order. The negative electrode 2, the foil 4, the positive electrode 1, and the separator 3 are, for example, a film-like body or a plate-like body extending in a substantially square or rectangular shape.
[0020] 2C , when the laminate 100 is viewed from above (here, the positive direction of the Z axis), the foil 4 and the separator 3 may encompass the negative electrode 2 and the positive electrode 1. The resin film 5 may extend in a frame shape and cover the ends of the foil 4 and the separator 3.
[0021] The resin film 5 may extend in a frame shape so as to encompass the ends of the negative electrode 2 and the positive electrode 1. The end face of the end A1 of the resin film 5 is exposed on one side of the laminate 100. The resin film 5 may include a material that can be welded by irradiation with a CO2 laser. Such a material is, for example, polyolefin. Specifically, the polyolefin is polyethylene or polypropylene. The polyethylene may be, for example, modified polyethylene. The portion where the multiple resin films 5 are heat-welded to each other functions as a sealing portion in the battery. The resin film 5 functions as a sealing member.
[0022] 2B to 2D, a CO2 laser is irradiated onto the side surface of the laminate 100 using a galvano scanner GS (step ST2). The output of the CO2 laser is, for example, 100 W or more and 300 W or less, specifically, 200 W. The scanning speed of the CO2 laser is, for example, 4000 mm / sec or more and 6000 mm / sec or less, specifically, 5000 mm / sec.
[0023] Specifically, the pressure restraint part PRU is placed above the end part A1 of the resin film 5 of the laminate 100. The pressure restraint part PRD is placed below the end part A1 of the resin film 5 of the laminate 100. The end part A1 of the resin film 5 of the laminate 100 is sandwiched between the pressure restraint part PRU and the pressure restraint part PRD. The pressure restraint part PRU and the pressure restraint part PRD pressurize and restrain the end part A1 of the resin film 5 of the laminate 100.
[0024] Also, a CO2 laser is irradiated onto one side of the laminate 100. That is, the end face of the end A1 of the resin film 5 exposed on one side of the laminate 100 is irradiated with the CO2 laser. The CO2 laser is irradiated while scanning one side of the laminate 100 with a laser light spot of the CO2 laser using a galvano scanner GS. In this scanning, the laser light spot reciprocates at a predetermined pitch on one side of the laminate 100. The CO2 laser may be irradiated onto the entire one side of the laminate 100 by this scanning.
[0025] Specifically, as shown in Figures 2C and 2D, a laser light spot repeatedly moves back and forth at a predetermined pitch on one side of the laminate 100 in a direction along the interface between the multiple laminated resin films 5 (here, the Y-axis direction).
[0026] 2D, a CO2 laser is applied so that a laser light spot moves along paths P1 to P10. The paths P1 to P10 may extend in a direction along the interfaces between the ends A1 of the multiple resin films 5 (here, the Y-axis direction).
[0027] In path P1, a laser light spot of a CO2 laser moves from one end to the other end of the resin film 5 laminated on the uppermost side of the laminate 100. Note that path P1 extends in the negative direction of the Y axis.
[0028] In pass P2, the laser light spot of the CO2 laser moves in the opposite direction to pass P1 (here, the positive direction of the Y axis) from a position that is a predetermined distance below the end point of pass P1. The predetermined distance is the size of the pitch described above.
[0029] In passes P3 to P10, similar to pass P2, the laser light spot of the CO2 laser moves in the opposite direction to the previous pass from a position that is a predetermined distance below the end point of the previous pass. The predetermined distance is the above-mentioned pitch. End A1 of the resin film 5 is irradiated with the CO2 laser and heated. As a result, multiple resin films 5 are welded together at end A1 of the resin film 5. This welding may be repeated to form a welded portion on the entire one side surface of the laminate 100.
[0030] Similarly, the CO2 laser is irradiated to the other side of the laminate 100. The ends A1 of the resin films 5 are welded on all sides of the laminate 100, forming welded parts A2 shown in FIG. 2E. At the welded parts A2, the resin films 5 are welded together, and the spaces between the resin films 5 are sealed. This makes it difficult for liquids or foreign matter to pass through the welded parts A2. In other words, the spaces between the resin films 5 are blocked, ensuring the hermeticity of the laminate 100.
[0031] In this manner, the battery 200 can be manufactured. The battery 200 is, for example, a bipolar battery. According to the battery manufacturing method according to the first embodiment, a CO2 laser is irradiated onto the side surface of the laminate 100, and the end A1 of the resin film 5 is welded to the side surface of the laminate 100. As a result, a welded portion A2 is formed. Therefore, energy is concentrated on the resin film 5, and the end A1 of the resin film 5 is sufficiently welded in a short time.
[0032] According to the battery manufacturing method of the first embodiment, the CO2 laser is irradiated using the galvano scanner GS. That is, the CO2 laser is irradiated while scanning the side surface of the laminate 100 with a laser light spot of the CO2 laser. This allows the end A1 of the resin film 5 to be uniformly welded on the side surface of the laminate 100.
[0033] In the battery manufacturing method according to the first embodiment, the resin film 5 contains polyolefin. The output of the CO2 laser is 100 W or more and 300 W or less. The scanning speed of the CO2 laser is 4000 mm / sec or more and 6000 mm / sec or less. This makes it possible to reduce the time required to weld the end A1 of the resin film 5 while suppressing carbonization of the end A1 of the resin film 5.
[0034] <Variation 1> Next, a step of Variation 1 of the manufacturing method for the battery according to Embodiment 1 will be described with reference to FIGS. 3A and 3B.
[0035] The electrode bodies 10 are stacked to form a laminate 100A (step ST21). The laminate 100A shown in FIG. 3A has the same configuration as the laminate 100 shown in FIG. 2D, except for the presence of an opening 5a and a component 6. The opening 5a opens on one side of the laminate 100A. The opening 5a has a size that allows a liquid such as an electrolyte to pass through. The liquid passes through the opening 5a and is supplied to the inside of the laminate 100A. The component 6 protrudes from one side of the laminate 100A. The component 6 is, for example, a charging terminal.
[0036] 3B, a CO2 laser is irradiated onto the side surface of the laminate 100A using a galvano scanner GS (not shown) (step ST22). Step ST22 is the same as step ST2, except that the laser light spot of the CO2 laser travels back and forth at a predetermined pitch while avoiding the opening 5a and the component 6 on one side surface of the laminate 100A.
[0037] In the example shown in FIG. 3B, the CO2 laser is irradiated so that the laser light spot produced by the CO2 laser moves along paths P21 to P28.
[0038] In pass P21, the laser light spot of the CO2 laser moves from one end to the other end of the resin film 5 laminated on the uppermost side of the laminate 100A.
[0039] In pass P22, the laser light spot of the CO2 laser moves in the opposite direction to pass P1 from a position spaced a predetermined distance below the end point of pass P1.
[0040] In passes P23 to P28, similarly to pass P22, in principle, the laser light spot of the CO2 laser moves in the opposite direction to the previous pass from a position spaced a predetermined distance below the end point of the previous pass.
[0041] However, in paths P24 and P25, when the CO2 laser light spot starts to move and reaches the vicinity of one end or the other end of the opening 5a, the CO2 laser irradiation is stopped. Then, the CO2 laser irradiation is resumed at the other end or the one end of the opening 5a. Furthermore, the CO2 laser light spot resumes moving from the vicinity of the other end or the one end of the opening 5a.
[0042] Similarly, in path P27, after the laser light spot of the CO2 laser starts to move, when it reaches the vicinity of the other end of the component 6, the CO2 laser irradiation is stopped. Then, the CO2 laser irradiation is resumed near one end of the component 6. Furthermore, the laser light spot of the CO2 laser resumes moving from the vicinity of one end of the opening 5a.
[0043] Next, the CO2 laser is irradiated to the other side of the laminate 100A, and the end A1 of the resin film 5 is welded on all sides of the laminate 100A. As a result, a welded portion (not shown) is formed. From the above, a battery can be manufactured. In this manufacturing method, energy is concentrated on the resin film 5, and the end A1 of the resin film 5 is sufficiently welded in a short time. In addition, the opening 5a and the component 6 are not irradiated with the CO2 laser. That is, the CO2 laser is irradiated while scanning with a laser light spot by the CO2 laser following the shape of the side of the laminate 100A. In addition, the depth of the welded portion near the opening 5a and near the component 6 is approximately the same as the depth of the welded portion in other parts of the side of the laminate 100A. Therefore, the design freedom can be improved.
[0044] <Example 1> Next, Example 1 to which the battery manufacturing method according to the first embodiment is applied will be described with reference to FIGS. 4A and 4B.
[0045] As shown in Fig. 4A, in this embodiment, the thickness of the laminate 100 is 10 mm, and the width of the laminate 100 is 200 mm. The processing conditions are a CO2 laser output of 200 W, a CO2 laser scanning speed of 5000 mm / sec, and an irradiation time of 4 sec. Specifically, the irradiation time per pass is 0.04 sec, the number of passes per scan is 10 passes, and the number of scans is 10.
[0046] Steps ST1 and ST2 are performed. Here, the thermal conduction to the unit area AU1 of the resin film 5 in step ST2 will be described. As shown in Fig. 4B, a CO2 laser L1 is irradiated to the unit area AU1 of the resin film 5 on the side surface of the laminate 100 using a galvano scanner GS (step ST2a). As a result, the unit area AU1 of the resin film 5 is heated.
[0047] Next, the side surface of the laminate 100 is scanned with a laser light spot by the CO2 laser L1 (step ST2b). After 0.1 seconds from step ST2a, for example, the CO2 laser is irradiated to a portion of the resin film 5 other than the unit area AU1 using the galvano scanner GS.
[0048] Subsequently, the side surface of the laminate 100 is scanned with a laser light spot by the CO2 laser L1 (step ST2c). For example, 0.3 seconds after step ST2a, the surface AU3 of the unit area AU1 dissipates heat and the temperature drops. The deep area AU2 of the unit area AU1 rises in temperature due to thermal conduction from the surface AU3.
[0049] Next, the CO2 laser L1 is again irradiated to the unit area AU1 of the resin film 5 on the side surface of the laminate 100 (step ST2d). For example, 0.4 seconds after step ST2a, the unit area AU1 of the resin film 5 is reheated. Then, the surface AU3 of the unit area AU1, whose temperature was lowered in step ST2c, rises in temperature. Also, the deep area AU2, whose temperature was raised in step ST2c, has a higher temperature than the surrounding area of the deep area AU2.
[0050] As described above, when the CO2 laser L1 is repeatedly scanned with a laser light spot, the surface AU3 and deep portion AU2 of the unit portion AU1 are heated. This causes the resin film 5 at the surface AU3 and deep portion AU2 to weld together. Furthermore, the surface AU3 of the unit portion AU1 is not easily carbonized because its temperature repeatedly rises and falls. Furthermore, the deep portion AU2 of the unit portion AU1 is gradually heated by heat conduction from the surface AU3. Therefore, it is possible to further form a welded portion while suppressing carbonization of the surface AU3.
[0051] <Electromagnetic wave absorption characteristics of resin film> Next, the electromagnetic wave absorption characteristics of the resin film will be described with reference to FIG. 5A.
[0052] First, the resin film was irradiated with electromagnetic waves, and the absorptance for each wavelength of the electromagnetic waves was measured. In this measurement, the irradiation axis of the electromagnetic waves extends in the thickness direction of the resin film. The resin film is one example of the resin film 5, and is made of modified polyethylene. An absorptance curve C1 representing the measured absorptance is shown in FIG. 5A. The thickness of the resin film is 120 μm. The wavelength range of the electromagnetic waves is 0.5 μm or more and 10.7 μm or less. The wavelength range of the electromagnetic waves includes the wavelength λ1, which is the fundamental wavelength of the infrared laser (IR (Infrared) laser), the wavelength λ2, which is the same as the wavelength of the energy ray that an infrared carbon heater can irradiate, and the wavelengths λ3 and λ4, which are the same as the wavelengths of the CO2 laser. The wavelength λ1 is 1.06 μm, the wavelength λ2 is 2.00 μm, the wavelength λ3 is 9.4 μm, and the wavelength λ4 is 1.06 μm.
[0053] As shown in FIG. 5A, the absorptance of electromagnetic waves having wavelength λ1, which is the fundamental wavelength of an infrared laser, is about 4.7%. The absorptance of electromagnetic waves having wavelength λ2 by an infrared carbon heater is about 8.0%. On the other hand, the absorptance of electromagnetic waves having wavelength λ3 is about 23.1%. The absorptance of electromagnetic waves having wavelength λ4 is about 15.7%. The absorptance of electromagnetic waves having wavelengths λ3 and λ4 by a CO2 laser is both higher than the absorptance of electromagnetic waves having wavelengths λ1 and λ2.
[0054] <Integrated absorption amount versus depth from the incident surface of the resin film> Next, referring to Fig. 5B to Fig. 5F, the results of irradiating each laser to the resin film made of the modified polyethylene and calculating the integrated absorption amount with respect to the depth from the incidence surface of the resin film will be described. The lasers are a CO2 laser having a wavelength λ3 or λ4, and an infrared laser having a wavelength λ1. Here, as shown in Fig. 5B, the resin film 5 made of the modified polyethylene is replaced with a resin film group 50 arranged in close contact with each other in the laser irradiation direction, and the above calculation is performed. That is, the resin film group 50 is irradiated with a laser L1, and the integrated absorption amount by the resin film group 50 is calculated to obtain the integrated absorption amount by the resin film 5.
[0055] Resin film group 50 includes resin films 51, 52, ..., 51+N, in other words, N resin films. N is a natural number. Resin films 51, 52, ..., 51+N all have the same configuration, are made of the same material as resin film 5, and have the same thickness. The thickness direction of resin films 51, 52, ..., 51+N and the main surface direction of resin film 5 are the same as the irradiation direction of laser L1 (here, the X-axis direction).
[0056] The resin films 51, 52, ..., 51+N are arranged in the thickness direction (here, the X-axis direction) of the resin films 51, 52, ..., 51+N while being in close contact with each other. The resin film 51 has a main surface 51a and a main surface 51b. The main surface 51a faces the outside of the resin film group 50, and the main surface 51b faces the opposite side to the main surface 51a and faces and is in close contact with the main surface 52a of the resin film 52. Since the resin films 52, ..., 51+N are located inside the resin film group 50, the main surfaces 51b, ..., 51+Nb of the resin films 51, ..., 51+N are in close contact with the main surfaces 52a, ..., 51+N+1a of the other adjacent resin films 52, ..., 51+N+1, respectively. Therefore, no reflected light is generated on the main surfaces 52a, ..., 51+Na of the resin films 52, ..., 51+N.
[0057] As shown in FIG. 5C, the resin film group 50 is irradiated with a laser L1. Then, the laser L1 is divided into a transmitted light L1a that passes through the resin film 51, an absorbed light L1b that is absorbed by the resin film 51, and a reflected light L1c that is reflected by the resin film 51. Then, the transmitted light L1a is incident on the resin film 52. The transmitted light L1a is divided into a transmitted light L2a that passes through the resin film 52, and an absorbed light L1b that is absorbed by the resin film 52. Similarly, the transmitted light LNa is divided into a transmitted light L1+Na that passes through the resin film 51+N, and an absorbed light L1+Nb that is absorbed by the resin film 51+N. In the resin films 53, ..., 51+N, the branching of the transmitted light and the absorbed light is repeated, as in the resin film 52. A plurality of the resin films are stacked in close contact with each other. The laser L1 is irradiated in the thickness direction of the resin film and enters the main surface of the resin film.
[0058] A calculation method for calculating the absorption amount and the integrated absorption amount of a laser having a wavelength λ3 relative to the depth from the incident surface of the resin film group 50 will be described. First, a laser having a wavelength λ3 was irradiated onto the resin film 51, and the reflectance, absorptance, and transmittance were measured. When the amount of incident light of the laser was 100%, the reflectance was 8%, the absorptance was 23.1%, and the transmittance was 68.9%. In addition, the absorptance and transmittance were calculated when a laser having a wavelength λ3 was incident on the resin film 52. When the amount of incident light of the laser was 100, the absorptance was 25.1%, and the transmittance was 74.9%. As a result, when the light transmitted through the resin film 51 is incident on the resin film 52, the absorptance can be calculated to be 17.3% and the transmittance to be 51.6%. Using a similar calculation method, when the amount of incident light of the laser is 100 and the light transmitted through the resin film 51+k is incident on the resin film 51+k+1, the absorptance and transmittance are calculated. k is a natural number. The integrated absorption amount of the laser having the wavelength λ3 with respect to the depth from the incident surface of the resin film group 50 was calculated, and the calculation results are shown in FIG. 5D.
[0059] Similarly, the integrated absorption amount of the laser having a wavelength λ4 with respect to the depth from the incident surface of the resin film group 50 was calculated, and the calculation result is shown in FIG. 5E. The integrated absorption amount of the laser having a wavelength λ1 with respect to the depth from the incident surface of the resin film group 50 was calculated, and the calculation result is shown in FIG. 5F. The resin film 51 was irradiated with a laser having a wavelength λ4, and the reflectance, absorptance, and transmittance were measured. When the amount of incident laser light was 100%, the reflectance was 8.6%, the absorptance was 15.7%, and the transmittance was 75.7%. The resin film 51 was irradiated with a laser having a wavelength λ1, and the reflectance, absorptance, and transmittance were measured. When the amount of incident laser light was 100%, the reflectance was 7.9%, the absorptance was 4.7%, and the transmittance was 87.4%.
[0060] As shown in Figures 5D and 5E, when a laser having a wavelength of λ3 or λ4 is irradiated, as the depth from the incident surface increases, the amount of absorption decreases and approaches 0 (zero), and the integrated amount of absorption increases and approaches 100.
[0061] As shown in FIG. 5D, the cumulative absorption exceeds 90 at a depth of 1.00 mm to 2.00 mm from the incident surface. In other words, the resin film 5 can absorb most of the laser light at a depth of 1.00 mm to 2.00 mm from the incident surface of the resin film 5. Therefore, when a laser having a wavelength λ3 is irradiated, the welded portion A2 can be sufficiently formed at a depth of 1.00 mm to 2.00 mm from the incident surface. As a result, the welded portion A2 is formed up to a portion 1.00 mm or deeper from the side surface of the laminate 100, and functions as a sealing portion.
[0062] 5E, the cumulative absorption exceeds 80 at a depth of 1.00 mm to 2.00 mm from the incident surface. In other words, most of the laser light can be absorbed at a depth of 1.00 mm to 2.00 mm from the incident surface in resin film 5. Therefore, when a laser having a wavelength λ4 is irradiated, it is possible to form welded portion A2 at a depth of 1.00 mm to 2.00 mm from the incident surface.
[0063] As shown in Fig. 5F, the cumulative absorption is 70 or less at a depth of 1.00 mm to 2.00 mm from the incident surface. The cumulative absorption of the laser light at a depth of 1.00 mm to 2.00 mm from the incident surface when irradiating with a laser having a wavelength λ1 is smaller than that when irradiating with a laser having a wavelength λ3 or λ4. Therefore, when irradiating with a laser having a wavelength λ1, the welded portion A2 is formed gradually at a depth of 1.00 mm to 2.00 mm from the incident surface.
[0064] From the above, among the lasers having wavelengths λ3, λ4, and λ1, the laser having wavelength λ3 has the highest cumulative absorption relative to the depth from the main surface of the resin film group 50, and therefore the welded portion A2 can be stably formed. As described above, when a resin film 5 having a thickness of 120 μm is irradiated with light having wavelength λ3 (9.4 μm), the absorptance of the resin film 5 is 23.1%. When a resin film 5 having a thickness of 120 μm is irradiated with light having wavelength λ3 (9.4 μm) and the optical axis of the light extends in the thickness direction of the resin film 5, the absorptance of the resin film 5 is 10% or more and 30% or less, so that the welded portion A2 can be stably formed.
[0065] <Variation 2> Next, a second variation of the method for producing a battery according to the first embodiment will be described with reference to Fig. 6. The second variation of the method for producing a battery according to the first embodiment has the same configuration as the method for producing a battery according to the first embodiment, except for step ST2.
[0066] As shown in Fig. 6, a CO2 laser is irradiated onto the side surface of the laminate 100 using a galvano scanner GS (step ST32). In this step, similar to step ST2 shown in Fig. 1, the CO2 laser is irradiated so that the laser light spot moves along paths P1a, P2 to P9, and P10a. The trajectories of the laser light spot on paths P1a and P10a are the same as those of the laser light spot on paths P1 and P10, respectively.
[0067] In step ST32, it is preferable to irradiate the laminate 100 with a CO2 laser so that the amount of heat applied to the laminate 100 in passes P1a and P10a is greater than the amount of heat applied to the laminate 100 in the other passes P2 to P9.
[0068] Specifically, in step ST32, the CO2 laser is irradiated so that the output of the CO2 laser in the pass P1a and the pass P10a is higher than the output of the CO2 laser in the other passes P2 to P9. More specifically, the output of the CO2 laser in the pass P1a and the pass P10a is, for example, 140% to 160%, specifically, 150%, of the output of the CO2 laser in the other passes P2 to P9.
[0069] In step ST32, the CO2 laser may be irradiated so that the scanning speed in the path P1a and the path P10a is slower than the scanning speed in the other paths P2 to P9.
[0070] In step ST32, the CO2 laser may be irradiated so that the number of scans in pass P1a and pass P10a is greater than the number of scans in the other passes P2 to P9. In step ST32, the CO2 laser may be irradiated so that the pitch in pass P1a and pass P10a is narrower than the pitch in the other passes P2 to P9.
[0071] The path P1a is closer to the pressure restraint portion PRU than the other paths P2 to P9. The path P10a is closer to the pressure restraint portion PRD than the other paths P2 to P9. The resin films 5 in the paths P1a and P10a dissipate heat by passing through the pressure restraint portions PRU and PRD, respectively. The resin films 5 in the paths P1a and P10a are located outside the laminate 100 compared to the resin films 5 in the other paths P2 to P9. Therefore, the resin films 5 in the paths P1a and P10a tend to dissipate heat and are less likely to be welded compared to the resin films 5 in the other paths P2 to P9. Therefore, according to the modified example 2 of the manufacturing method for the battery according to the above-mentioned embodiment 1, the amount of heat supplied by the irradiation of the CO2 laser in the paths P1a and P10a can be increased to weld the resin films 5 in the paths P1 and P10.
[0072] <Modification 3> 7A and 7B, a third variation of the method for producing a battery according to embodiment 1 will be described. The third variation of the method for producing a battery according to embodiment 1 has the same configuration as the method for producing a battery according to embodiment 1, except for step ST2.
[0073] Using the galvano scanner GS shown in FIG. 2D, as shown in FIG. 7A, the side surface of the laminate 100 is irradiated with a CO2 laser (step ST42). Specifically, the CO2 laser is irradiated so that a laser light spot by the CO2 laser moves along paths P31 to P34. The paths P31 to P34 each extend along the interface between the multiple resin films 5. By selectively irradiating the interfaces between the multiple resin films 5 with the CO2 laser, the interfaces between the multiple resin films 5 are preferentially welded. As shown in FIG. 7B, multiple welded parts A21 are formed at the interfaces between the multiple resin films 5. After performing step ST42, the battery 200 is formed. In the battery 200, the multiple welded parts A21 can prevent liquid or foreign matter from passing between the multiple resin films 5. Since the volume of the multiple welded parts A21 is smaller than the volume of the welded part A2 shown in FIG. 2E, the amount of CO2 laser irradiation required to form the multiple welded parts A21 is small. In other words, energy efficiency can be improved.
[0074] <Example 2> Next, a second example of the battery manufacturing method according to the first embodiment will be described with reference to FIGS. 8A and 8B.
[0075] A negative electrode active material layer is formed on one main surface of a current collector, and a positive electrode active material layer is formed on the other main surface of the current collector (step ST51). The current collector is a foil. The current collector functions as an electrode body in the bipolar battery produced by this production method.
[0076] Subsequently, a plurality of resin films are arranged so as to sandwich the outer periphery of the current collector obtained in step ST51, and the current collector and the resin films are welded together (step ST52).
[0077] Subsequently, the current collector welded to the resin film in step ST52 and a separator are laminated to obtain a laminate (step ST53).
[0078] Finally, the region of the resin film of the laminate 100B shown in FIG. 8A is pressurized and restrained, and a CO2 laser is irradiated onto the surface of the resin film using the following work conditions, laser oscillation conditions, and laser trajectory conditions to weld the resin film (step ST54).
[0079] The workpiece conditions were that the material of the resin film was modified polyethylene, the thickness of the resin film was 19.2 mm, and the number of layers of the resin film was 91. The main surface of the resin film was a square with a side length of 140 mm. The laser oscillation conditions were that the laser type was a CO2 pulse laser, the wavelength was 9400 μm, the output was 215 W, the frequency was 50 kHz, the duty was 45%, and the spot size was 0.8 mm. The laser trajectory conditions were, as shown in Figure 8B, that the scanning distance was 140 mm, the pitch was 0.8 mm, and the number of passes was 20. The laser trajectory conditions were that the number of repetitions was 50, and the scanning speed was 6000 mm / sec. The processing time was 30.753 seconds.
[0080] In step ST54, the pressure restraint parts PRU2 and PRD2 shown in FIG. 8A were used. The pressure restraint parts PRU2 and PRD2 are a pair of plate-like bodies made of bakelite. The four corners of the pressure restraint parts PRU2 and PRD2 are fastened by bolts (not shown). The main surfaces of the pressure restraint parts PRU2 and PRD2 are substantially rectangular, measuring 130 mm x 195 mm. The thickness of the pressure restraint parts PRU2 and PRD2 is 20 mm. The ends of the pressure restraint parts PRU2 and PRD2 are covered with aluminum tape 71. Each glass cloth 72 covers the boundary between the pressure restraint part PRU2 and the aluminum tape 71, and the boundary between the pressure restraint part PRD2 and the aluminum tape 71. The ends of the laminate 100B are located at the boundary between the glass cloth 72 and the aluminum tape 71. The pressure restraint parts PRU2 and PRD2 sandwich the laminate 100B and the dummy 800 to pressurize and restrain them. The dummy 800 has approximately the same shape and rigidity as the stack 100B, and therefore ensures that the pressure restraint portions PRU2, PRD2 are approximately parallel to each other.
[0081] The present invention is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present invention. In addition, the present invention can be implemented by appropriately combining the above-described embodiment and examples thereof. [Explanation of symbols]
[0082] 1 positive electrode, 2 negative electrode, 3 separator, 4 foil, 5 resin film, 5a opening, 6 component, 10 electrode body, 50 resin film group, 51-54, 51+N resin film, 51a-54a, 54b-54b, 51+Na, 51+Nb main surface, 71 aluminum tape, 72 glass cloth, 100, 100A, 100B laminate, 200 battery, A1 end, A2, A21 welding part, AU1 unit location, AU2 deep part, AU3 surface, GS galvanometer scanner, L1 laser, L1a, L2a, LNa, L1+Na transmitted light, L1b, L2b, L1+Nb absorbed light, L1c reflected light, P1-P10, P1a, P10a, P21-P28, P31-P34 Path, PRD, PRD2, PRU, PRU2 Pressurized restraint
Claims
1. The electrode assembly includes a plurality of electrode bodies and a sealing portion. The plurality of electrode bodies are stacked, The sealing portion includes a welding portion that seals between ends of the plurality of electrode bodies, A plurality of sealing members are disposed between the ends of the plurality of electrode assemblies. 2 The method includes a step of heat-welding the plurality of sealing members by irradiating a laser to form the welded portion. How batteries are manufactured.
2. In the above step, a galvanometer scanner is used to measure the CO 2 irradiating a laser; A method for producing the battery according to claim 1 .
3. The CO 2 The laser output is 100W or more and 300W or less, The CO 2 The laser scanning speed is 4000 mm / sec or more and 6000 mm / sec or less. A method for producing the battery according to claim 2.
4. The plurality of sealing members include a polyolefin. A method for producing the battery according to claim 1 or 2.
5. The plurality of sealing members are films having a thickness of 120 μm, and when the film is irradiated with light having a wavelength of 9.4 μm and the optical axis of the light extends in the thickness direction of the film, the absorptance of the light by the film is 10% or more and 30% or less. A method for producing the battery according to claim 1 or 2.
Citation Information
Patent Citations
Method of joining resin member and method of manufacturing well chip for inspection
JP2015160334A
Manufacturing method of power storage module
JP2021082450A
Manufacturing method of power storage device
JP2023000059A