Water-absorbing composition for water barrier sheet, and water barrier sheet using the same

A water-absorbing composition of resin powder and fibers enhances the flexibility and water-blocking properties of sheets, preventing leakage by controlling particle size and distribution, addressing the limitations of conventional resin-based sheets.

JP2024169932APending Publication Date: 2024-12-06LIVEDO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023086802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional water-blocking sheets using water-absorbing resin powder are not suitable for preventing water leakage and lack flexibility.

Method used

A water-absorbing composition comprising a mixture of water-absorbing resin powder and fibers, with a specific mass ratio and particle size distribution, to enhance flexibility and prevent leakage.

Benefits of technology

The composition provides a water-blocking sheet with high flexibility and effective prevention of water leakage even when holes form, maintaining integrity and reducing spillage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169932000003
    Figure 2024169932000003
  • Figure 2024169932000004
    Figure 2024169932000004
  • Figure 2024169932000005
    Figure 2024169932000005
Patent Text Reader

Abstract

To provide a water-absorbing composition which can prevent water leakage of a water barrier sheet, and can enhance flexibility of the water barrier sheet.SOLUTION: A water-absorbing composition for a water barrier sheet is used in a water barrier sheet, and contains (X) water-absorbing resin powder and (Y) water-absorbing fibers, wherein a mass ratio ((X) / (Y)) of (X) the water-absorbing resin powder to (Y) the water-absorbing fibers in the water-absorbing composition is 90 / 10 to 99 / 1, a percentage content of particles which are contained in 100 mass% of (X) the water-absorbing resin powder and have a particle diameter of 105 μm or less is 15 mass% or less, and pure water liquid permeation speed of the water-absorbing composition is 0.5 mL / min or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-absorbing composition, and more particularly to a water-absorbing composition used in a water-blocking sheet. [Background technology]

[0002] Waterproof sheets are used in bank protection works at coasts and rivers, to prevent water leakage from reservoirs, and to prevent sewage leakage into the ground at waste disposal sites. For such waterproof sheets, a waterproof sheet with water-absorbent resin powder disposed on the outer surface side of the base sheet has been proposed. Even if a hole is formed in the base sheet, such waterproof sheets can prevent water leakage by expanding the water-absorbent resin powder.

[0003] For example, Patent Document 1 describes a water-absorbent composite sheet for waterproof sheets, characterized by having a substrate and approximately spherical water-absorbent resin particles intermittently fixed onto the substrate (see Patent Document 1 (Claim 1, paragraphs 0065-0079)). Also, Patent Document 2 describes a waterproof sheet, characterized by overlapping water-absorbent sheets on the top and bottom of a water-absorbing and swelling polymer sheet of a gelling substance and quilting the resulting sheets, and laminating a water-blocking sheet on the bottom surface of the quilted water-absorbent sheet to form an integrated sheet (see Patent Document 2 (Claim 1, paragraphs 0008-0010)). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-056160 A [Patent Document 2] Japanese Patent Application Publication No. 8-074223 Summary of the Invention [Problem to be solved by the invention]

[0005] Waterproof sheets using water-absorbent resin powder have been proposed in the past, but the water-absorbent resin powder used in disposable diapers, etc. has been repurposed, and no water-absorbent compositions suitable for waterproof sheets have been considered.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a water-absorbent composition for use in a waterproof sheet, which can better prevent water leakage from the waterproof sheet and increase the flexibility of the waterproof sheet. [Means for solving the problem]

[0007] The water-absorbent composition for water-shielding sheets of the present invention is a water-absorbent composition used for water-shielding sheets, and is characterized in that it contains (X) water-absorbent resin powder and (Y) water-absorbent fibers, the mass ratio ((X) / (Y)) of the (X) water-absorbent resin powder to the (Y) water-absorbent fibers in the water-absorbent composition is 90 / 10 to 99 / 1, the content of particles with a particle diameter of 105 μm or less contained in 100 mass% of the (X) water-absorbent resin powder is 15 mass% or less, and the pure water permeation rate of the water-absorbent composition is 0.5 mL / min or less.

[0008] Since the water-absorbing composition of the present invention contains a predetermined amount of (Y) water-absorbent fibers, leakage of (X) water-absorbent resin powder is suppressed when a hole is made in the water-shielding sheet, and water leakage from the water-shielding sheet is further prevented. Furthermore, since the water-absorbing composition of the present invention contains a predetermined amount of (Y) water-absorbent fibers, the flexibility of the water-absorbing layer formed from the water-absorbent composition is high, and the flexibility of the obtained water-shielding sheet is improved. Effect of the Invention

[0009] By using the water-absorbing composition of the present invention in a waterproof sheet, it is possible to obtain a waterproof sheet which is highly flexible and can better prevent water leakage even if a hole is formed in the base sheet. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of an example of a waterproof sheet of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the configuration of a nail hole waterproof tester. [Diagram 3] FIG. 2 is a plan view showing a holed portion of a sample for a nail hole waterproofing test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Water-absorbing composition for waterproof sheets] The water-absorbent composition for water-shielding sheets of the present invention (hereinafter, sometimes simply referred to as the "water-absorbent composition") is a water-absorbent composition used for water-shielding sheets, and contains (X) water-absorbent resin powder and (Y) water-absorbent fibers.

[0012] The water-absorbing composition of the present invention contains a predetermined amount of water-absorbent fibers (Y), which have the effect of preventing the movement of water-absorbent resin powder (X). Therefore, when a hole is made in the water-shielding sheet, the water-absorbent fibers (Y) prevent the water-absorbent resin powder (X) from leaking out. In addition, by blending the water-absorbent fiber (Y), aggregation of the water-absorbent resin powder (X) is suppressed, and therefore the flexibility of the water-absorbent layer formed from the water-absorbent composition is increased, thereby improving the flexibility of the resulting waterproof sheet.

[0013] The mass ratio ((X) / (Y)) of the (X) water absorbent resin powder to the (Y) water absorbent fiber in the water absorbent composition is preferably 90 / 10 or more, more preferably 91 / 9 or more, even more preferably 95 / 5 or more, and is preferably 99 / 1 or less, more preferably 98.5 / 1.5 or less, even more preferably 98 / 2 or less. When the mass ratio ((X) / (Y)) is 90 / 10 or more, the water impermeability of the waterproof sheet is good, and when it is 99 / 1 or less, the flexibility of the waterproof sheet is good.

[0014] ((X) Water-absorbing resin powder) The water-absorbing composition contains (X) water-absorbing resin powder. The (X) water-absorbing resin powder is an aggregate of water-absorbing resin particles. The shape of the particles constituting the (X) water-absorbing resin powder is not particularly limited, and examples thereof include irregularly crushed, scale-like, pearl-like, rice grain-like, and the like.

[0015] The mass average particle diameter (μm) of the water absorbent resin powder (X) is preferably 35 μm or more, more preferably 40 μm or more, even more preferably 50 μm or more, particularly preferably 105 μm or more, and is preferably 4,000 μm or less, more preferably 3,500 μm or less, even more preferably 3,000 μm or less, particularly preferably 1,000 μm or less. If the mass average particle diameter is 35 μm or more, splices are unlikely to occur during swelling, and if it is 4,000 μm or less, excellent water impermeability is exhibited.

[0016] The mass average particle size is measured using a Rotap test sieve shaker and standard sieves (JIS Z8801-1:2019) according to the method described in Perry's Chemical Engineers Handbook, 6th Edition (McGraw-Hill Book Company, 1984, p. 21). Specifically, JIS standard sieve meshes with nominal openings of 4000 μm, 1000 μm, 500 μm, 250 μm, 150 μm, 105 μm, 74 μm, and 34 μm are stacked from the top in this order, as well as a tray. 50 g of the powder to be measured is placed on the top sieve and shaken for 5 minutes with a Rotap test sieve shaker. The mass of each sieve and the powder on the tray is weighed, and the total is taken as 100 mass%, and the mass fraction of the particles on each sieve is calculated. Plot these values ​​on a logarithmic probability chart {horizontal axis is sieve opening (particle size) and vertical axis is mass fraction}, then draw a line connecting each point to determine the particle size corresponding to a mass fraction of 50% by mass, which is the mass average particle size.

[0017] The content of particles having a particle diameter of 105 μm or less (particles passing through a sieve with an opening of 105 μm) contained in 100% by mass of the (X) water absorbent resin powder is 15% by mass or less, more preferably 13% by mass or less, and further preferably 10% by mass or less. If the content of particles having a particle diameter of 105 μm or less is 15% by mass or less, the spill resistance of the water absorbent resin powder of the water shielding sheet becomes good.

[0018] The (X) water absorbent resin powder may contain particles having a particle diameter of 105 μm or less. In this case, the content of particles having a particle diameter of 105 μm or less contained in 100% by mass of the (X) water absorbent resin powder is preferably 2% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. If the content of particles having a particle diameter of 105 μm or less is 2% by mass or more, the water impermeability of the water shielding sheet can be further improved.

[0019] The water-absorbent resin powder (X) preferably has a content of particles having a particle diameter of 4000 μm or less of 90 mass % or more, more preferably 93 mass % or more, and further preferably 95 mass % or more. When the content of particles having a particle diameter of 4000 μm or less is 90 mass % or more, the water-absorbent resin powder exhibits excellent water-impermeability.

[0020] The particle size distribution of the water absorbent resin powder (X) can be adjusted by crushing the water absorbent resin or classifying the powder. The crushing method is not particularly limited, and crushing devices such as a hammer crusher, an impact crusher, a roll crusher, and an airflow crusher may be used. The classification method is not particularly limited, and examples thereof include sieving and airflow classification.

[0021] 〔composition〕 The water-absorbing resin constituting the water-absorbing resin powder is not particularly limited, and any conventionally known water-absorbing resin can be used. As the water-absorbing resin, a synthetic water-absorbing resin is preferable.

[0022] The water absorbent resin constituting the water absorbent resin powder is preferably one obtained by polymerizing a monomer composition containing (a1) a water-soluble ethylenically unsaturated monomer and / or (a2) a hydrolyzable monomer which generates (a1) a water-soluble ethylenic monomer by hydrolysis, and (b) an internal crosslinking agent.

[0023] ((a1) Water-soluble ethylenically unsaturated monomer) The (a1) water-soluble ethylenically unsaturated monomer is a water-soluble monomer having one ethylenically unsaturated group in the molecule. The water-soluble monomer means a monomer that has the property of dissolving at least 100 g in 100 g of water at 25° C. The (a1) water-soluble ethylenically unsaturated monomer is preferably a monomer having at least one water-soluble substituent and an ethylenically unsaturated group.

[0024] Examples of the water-soluble substituent include a carboxy group, a sulfo group, a sulfoxy group, a phosphono group, a hydroxy group, a carbamoyl group, an amino group, or salts thereof, as well as ammonium salts. The water-soluble substituent may have only one type, or may have two or more types. The water-soluble substituent is preferably a salt of a carboxy group (carboxylate), a salt of a sulfo group (sulfonate), or an ammonium salt.

[0025] The salts include alkali metal salts such as lithium, sodium, and potassium; and alkaline earth metal salts such as magnesium and calcium. The ammonium salt may be any of primary to tertiary amine salts or quaternary ammonium salts. Among these salts, from the viewpoint of absorption characteristics, alkali metal salts and ammonium salts are preferred, alkali metal salts are more preferred, and sodium salts are even more preferred.

[0026] The water-soluble ethylenically unsaturated monomer having a carboxy group and / or a salt thereof is preferably an unsaturated carboxylic acid having 3 to 30 carbon atoms and / or a salt thereof. Specific examples of the water-soluble ethylenically unsaturated monomer having a carboxy group include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, and cinnamic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, and itaconic acid; and monoalkyl (carbon number 1 to 8) esters of unsaturated dicarboxylic acids such as maleic acid monobutyl ester, fumaric acid monobutyl ester, maleic acid ethylcarbitol monoester, fumaric acid ethylcarbitol monoester, citraconic acid monobutyl ester, and itaconic acid glycol monoester. In the description of the present invention, "(meth)acrylic" means "acrylic" and / or "methacrylic".

[0027] Specific examples of the water-soluble ethylenically unsaturated monomer having a sulfo group include aliphatic or aromatic vinyl sulfonic acids such as vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, and α-methylstyrene sulfonic acid; (meth)acryloxypropyl sulfonic acid, 2-hydroxy-3-(meth)acryloxypropyl sulfonic acid, 2-(meth)acryloylamino-2,2-dimethylethanesulfonic acid, 3-(meth)acryloxyethanesulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, and 3-(meth)acrylamide-2-hydroxypropanesulfonic acid; and (meth)acryloyl-containing alkyl sulfonic acids; alkyl (meth)allyl sulfosuccinate esters.

[0028] Examples of the water-soluble ethylenically unsaturated monomer having a sulfooxy group include sulfate esters of hydroxyalkyl(meth)acrylates; sulfate esters of polyoxyalkylene mono(meth)acrylates; and the like.

[0029] Examples of the water-soluble ethylenically unsaturated monomer having a phosphono group include hydroxyalkyl (meth)acrylate phosphate monoesters, hydroxyalkyl (meth)acrylate phosphate diesters, and alkyl (meth)acrylate phosphonic acids.

[0030] Examples of the water-soluble ethylenically unsaturated monomer having a hydroxy group include monoethylenically unsaturated alcohols having 3 to 15 carbon atoms, such as (meth)allyl alcohol and (meth)propenyl alcohol, and monoethylenically unsaturated carboxylic acid esters and monoethylenically unsaturated ethers of divalent to hexavalent polyols, such as alkylene glycols having 2 to 20 carbon atoms, glycerin, sorbitan, diglycerin, pentaerythritol, and polyalkylene (having 2 to 4 carbon atoms) glycols (weight average molecular weight: 100 to 2000). Specific examples of these include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, triethylene glycol (meth)acrylate, and poly-oxyethylene-oxypropylene mono(meth)allyl ether.

[0031] Examples of the water-soluble ethylenically unsaturated monomer having a carbamoyl group include (meth)acrylamide; N-alkyl (C1-8) (meth)acrylamides such as N-methylacrylamide; N,N-dialkyl (C1-8) acrylamides such as N,N-dimethylacrylamide and N,N-di-n- or i-propylacrylamide; N-hydroxyalkyl (C1-8) (meth)acrylamides such as N-methylol (meth)acrylamide and N-hydroxyethyl (meth)acrylamide; and N,N-dihydroxyalkyl (C1-8) (meth)acrylamides such as N,N-dihydroxyethyl (meth)acrylamide.

[0032] Examples of the water-soluble ethylenically unsaturated monomer having an amino group include an amino group-containing ester of a monoethylenically unsaturated mono- or di-carboxylic acid, and an amino group-containing amide of a monoethylenically unsaturated mono- or di-carboxylic acid. Examples of the amino group-containing ester of a monoethylenically unsaturated mono- or di-carboxylic acid include dialkylaminoalkyl(meth)acrylate, di(hydroxyalkyl)aminoalkyl ester, and morpholinoalkyl ester, and examples of such ester include dimethylaminoethyl(meth)acrylate, diethylamino(meth)acrylate, morpholinoethyl(meth)acrylate, dimethylaminoethyl fumarate, and dimethylaminoethyl maleate. Examples of the amino group-containing amide of a monoethylenically unsaturated mono- or di-carboxylic acid include monoalkyl(meth)acrylamide, and examples of such amide include dimethylaminoethyl(meth)acrylamide and diethylaminoethyl(meth)acrylamide. Examples of the water-soluble ethylenically unsaturated monomer having an amino group include vinylpyridines such as 4-vinylpyridine and 2-vinylpyridine, in addition to the above.

[0033] ((a2) Hydrolyzable Monomer) The (a2) hydrolyzable monomer is a monomer that can generate (a1) water-soluble ethylenically unsaturated monomer by hydrolysis under the action of water at 50° C. and, if necessary, a catalyst (such as an acid or a base). The (a2) hydrolyzable monomer may be hydrolyzed either during or after polymerization, but is preferably hydrolyzed after polymerization from the viewpoint of the molecular weight of the resulting water absorbent resin.

[0034] The hydrolyzable monomer (a2) is not particularly limited, but is preferably an ethylenically unsaturated monomer having at least one hydrolyzable substituent that becomes a water-soluble substituent upon hydrolysis. Examples of the hydrolyzable substituent include a group containing an acid anhydride, a group containing an ester bond, and a cyano group.

[0035] As the ethylenically unsaturated monomer having a group containing an acid anhydride, an unsaturated dicarboxylic acid anhydride having 4 to 20 carbon atoms is used, and examples thereof include maleic anhydride, itaconic anhydride, and citraconic anhydride. Examples of ethylenically unsaturated monomers having a group containing an ester bond include lower alkyl esters of monoethylenically unsaturated carboxylic acids such as methyl (meth)acrylate and ethyl (meth)acrylate; and esters of monoethylenically unsaturated alcohols such as vinyl acetate and (meth)allyl acetate. Examples of ethylenically unsaturated monomers having a cyano group include vinyl group-containing nitrile compounds having 3 to 6 carbon atoms, such as (meth)acrylonitrile and 5-hexenenitrile.

[0036] As the (a1) water-soluble ethylenically unsaturated monomer and (a2) hydrolyzable monomer, those described in Japanese Patent No. 3648553, JP-A No. 2003-165883, JP-A No. 2005-75982, and JP-A No. 2005-95759 can be further used.

[0037] The water-soluble ethylenically unsaturated monomer (a1) and the hydrolyzable monomer (a2) may be used alone or in a mixture of two or more kinds. The same applies when the water-soluble ethylenically unsaturated monomer (a1) and the hydrolyzable monomer (a2) are used in combination. When the water-soluble ethylenically unsaturated monomer (a1) and the hydrolyzable monomer (a2) are used in combination, the molar ratio (a1 / a2) is preferably 75 / 25 or more, more preferably 85 / 15 or more, even more preferably 90 / 10 or more, particularly preferably 91 / 9 or more, and is preferably 99 / 1 or less, more preferably 95 / 5 or less, even more preferably 93 / 7 or less, particularly preferably 92 / 8 or less. When the molar ratio (a1 / a2) is within the above range, the absorption performance is further improved.

[0038] ((a3) Other vinyl monomers) The monomer composition may contain (a3) ​​other vinyl monomers copolymerizable with the (a1) water-soluble ethylenically unsaturated monomer and (a2) hydrolyzable monomer. As the (a3) ​​other vinyl monomer, hydrophobic vinyl monomers and the like can be used, but are not limited thereto.

[0039] Examples of the (a3) ​​other vinyl monomers include (i) aromatic ethylenic monomers having 8 to 30 carbon atoms, (ii) aliphatic ethylenic monomers having 2 to 20 carbon atoms, and (iii) alicyclic ethylenic monomers having 5 to 15 carbon atoms.

[0040] Examples of the (i) aromatic ethylenic monomer having 8 to 30 carbon atoms include styrene, α-methylstyrene, vinyltoluene, hydroxystyrene and other styrenes, vinylnaphthalene, dichlorostyrene and other halogen-substituted styrenes. Examples of the (ii) aliphatic ethylene monomer having 2 to 20 carbon atoms include alkenes such as ethylene, propylene, butene, isobutylene, pentene, heptene, diisobutylene, octene, dodecene, and octadecene, and alkadienes such as butadiene and isoprene. Examples of the (iii) alicyclic ethylene monomer having 5 to 15 carbon atoms include monoethylenically unsaturated monomers such as pinene, limonene, and indene; and polyethylene vinyl polymerizable monomers such as cyclopentadiene, bicyclopentadiene, and ethylidenenorbornene.

[0041] As the (a3) ​​other vinyl monomers, those described in Japanese Patent No. 3648553, JP-A No. 2003-165883, JP-A No. 2005-75982, and JP-A No. 2005-95759 can be further used.

[0042] When the (a3) ​​other vinyl monomer is used, the content (mol%) of the (a3) ​​other vinyl monomer is preferably 0.01 mol% to 5 mol% based on the total amount (100 mol%) of the (a1) water-soluble ethylenically unsaturated monomer and the (a2) hydrolyzable monomer, more preferably 0.05 mol% to 3 mol%, even more preferably 0.08 mol% to 2 mol%, and most preferably 0.1 mol% to 1.5 mol%. From the viewpoint of absorption characteristics, the content of the (a3) ​​other vinyl monomer is most preferably 0 mol%.

[0043] ((b) Internal crosslinking agent) Examples of the (b) internal crosslinking agent include (b1) an internal crosslinking agent having two or more ethylenically unsaturated groups, (b2) an internal crosslinking agent having at least one functional group capable of reacting with a water-soluble substituent and having at least one ethylenically unsaturated group, and (b3) an internal crosslinking agent having at least two or more functional groups capable of reacting with a water-soluble substituent.

[0044] Examples of the (b1) internal crosslinking agent having two or more ethylenically unsaturated groups include bis(meth)acrylamide having 8 to 12 carbon atoms, poly(meth)acrylate of polyol having 2 to 10 carbon atoms, polyallylamine having 2 to 10 carbon atoms, poly(meth)allyl ether of polyol having 2 to 10 carbon atoms, etc. Specific examples of these include N,N'-methylenebis(meth)acrylamide, ethylene glycol di(meth)acrylate, poly(polymerization degree 2 to 5) ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, glycerin (di or tri)acrylate, trimethylolpropane triacrylate, diallylamine, triallylamine, triallyl cyanurate, triallyl isocyanurate, tetraallyloxyethane, pentaerythritol diallyl ether, pentaerythritol triallyl ether, pentaerythritol tetraallyl ether, diglycerin di(meth)acrylate, etc.

[0045] Examples of the (b2) internal crosslinking agent having at least one functional group capable of reacting with a water-soluble substituent and having at least one ethylenically unsaturated group include ethylenically unsaturated compounds having an epoxy group with 6 to 8 carbon atoms, ethylenically unsaturated compounds having a hydroxyl group with 4 to 8 carbon atoms, and ethylenically unsaturated compounds having an isocyanato group with 4 to 8 carbon atoms. Specific examples of these include glycidyl (meth)acrylate, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, and isocyanatoethyl (meth)acrylate.

[0046] (b3) Examples of the internal crosslinking agent having at least two functional groups capable of reacting with a water-soluble substituent include polyhydric alcohols, polyhydric glycidyls, polyhydric amines, polyhydric aziridines, and polyhydric isocyanates. Examples of the polyhydric glycidyl compounds include ethylene glycol diglycidyl ether and glycerin diglycidyl ether. Examples of the polyhydric amine compounds include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and polyethyleneimine. Examples of the polyhydric aziridine compounds include 2,2-bishydroxymethylbutanol-tris(3-(1-aziridinyl)propionate), 1,6-hexamethylenediethyleneurea, and diphenylmethane-bis-4,4'-N,N'-diethyleneurea. Examples of the polyhydric isocyanate compounds include 2,4-tolylenediisocyanate and hexamethylenediisocyanate. These internal crosslinking agents may be used alone or in combination of two or more kinds.

[0047] As the (b) internal crosslinking agent, from the viewpoint of absorption performance and the like, (b1) an internal crosslinking agent having two or more ethylenically unsaturated groups is preferable, a poly(meth)allyl ether of a polyol having 2 to 10 carbon atoms is more preferable, triallyl cyanurate, triallyl isocyanurate, tetraallyloxyethane or pentaerythritol triallyl ether is further preferable, and pentaerythritol triallyl ether is most preferable.

[0048] As the (b) internal crosslinking agent, those described in Japanese Patent No. 3648553, JP-A-2003-165883, JP-A-2005-75982, and JP-A-2005-95759 can also be used.

[0049] The content (mol%) of the (b) internal crosslinking agent is preferably 0.001 mol% or more, more preferably 0.005 mol% or more, even more preferably 0.01 mol% or more, and is preferably 5 mol% or less, more preferably 3 mol% or less, even more preferably 1 mol% or less, based on the total amount (100 mol%) of the (a1) water-soluble ethylenically unsaturated monomer and the (a2) hydrolyzable monomer.Within this range, the absorption performance (especially the absorption amount and absorption speed) becomes even better.

[0050] The monomer composition can be polymerized by a conventional method, such as solution polymerization, emulsion polymerization, suspension polymerization, or reversed-phase suspension polymerization. The form of the polymerization liquid during polymerization may be a thin film, a spray, or the like. The polymerization can be controlled by adiabatic polymerization, temperature-controlled polymerization, or isothermal polymerization.

[0051] When the suspension polymerization method or the reversed-phase suspension polymerization method is applied as the polymerization method, conventionally known dispersants such as sucrose esters, phosphoric esters, and sorbitan esters, and protective colloids such as poval, α-olefin-maleic anhydride copolymers, and polyethylene oxide can be used as necessary. In the case of the reversed-phase suspension polymerization method, the polymerization can be carried out using a solvent such as cyclohexane, normal hexane, normal heptane, toluene, and xylene. As the polymerization method, the solution polymerization method is preferred, and the aqueous solution polymerization method is more preferred because it does not require the use of an organic solvent and is advantageous in terms of production costs.

[0052] The hydrogel (composed of a cross-linked polymer and water) obtained by polymerization can be chopped as necessary. The size (longest diameter) of the gel after chopping is preferably 50 μm to 10 cm, more preferably 100 μm to 2 cm, and even more preferably 1 mm to 1 cm. Within this range, the drying property in the drying step is further improved. The chopping can be performed by a known method, for example, using a conventional chopping device such as a Bex mill, a rubber chopper, a Farma mill, a mincing machine, an impact crusher, or a roll crusher.

[0053] When a solvent (organic solvent, water, etc.) is used in the polymerization, it is preferable to distill off the solvent after the polymerization. When the solvent contains an organic solvent, the content (mass%) of the organic solvent after distillation is preferably 0 mass% to 10 mass% relative to the mass (100 mass%) of the crosslinked polymer, more preferably 0 mass% to 5 mass%, even more preferably 0 mass% to 3 mass%, and most preferably 0 mass% to 1 mass%. When the content of the organic solvent is within the above range, the absorption performance (particularly the water retention capacity) of the water absorbent resin powder becomes even better.

[0054] When the solvent contains water, the moisture content (mass%) after distillation is preferably 0 mass% to 20 mass% relative to the mass (100 mass%) of the crosslinked polymer (water absorbent resin powder), more preferably 1 mass% to 10 mass%, even more preferably 2 mass% to 9 mass%, and most preferably 3 mass% to 8 mass%. When the moisture content (mass%) is within the above range, the absorption performance becomes even better.

[0055] The organic solvent content and moisture content are determined from the mass loss of the sample before and after heating using an infrared moisture meter (KETT, "JE400" etc.: 120±5°C, 30 minutes, atmospheric humidity before heating 50±10% RH, lamp specifications 100V, 40W).

[0056] Examples of a method for distilling off the solvent (including water) include distillation (drying) with hot air at a temperature of 80°C to 230°C, thin-film drying using a drum dryer heated to 100°C to 230°C, (heated) reduced pressure drying, freeze drying, drying using infrared rays, decantation, filtration, and the like.

[0057] The water-containing gel obtained by polymerization is dried to obtain a water-absorbent resin powder (crosslinked polymer). Although the water-absorbent resin powder is generally subjected to a surface crosslinking treatment, the water-absorbent resin powder of the present invention is not subjected to a surface crosslinking treatment. By not subjecting the surface crosslinking treatment, the pure water permeability rate of the water-absorbent composition described later is significantly decreased.

[0058] The (X) water-absorbent resin powder may be one obtained by crushing water-absorbent resin particles that have been subjected to a surface cross-linking treatment. That is, a water-absorbent resin powder manufactured for other uses than a water-shielding sheet, in which water-absorbent resin particles that have been subjected to a surface cross-linking treatment are crushed to expose a surface that has not been subjected to the surface cross-linking treatment, can be used as the (X) water-absorbent resin powder. Even when such a water-absorbent resin powder obtained by crushing water-absorbent resin particles that have been subjected to a surface cross-linking treatment is used, the pure water permeation rate of the water-absorbing composition can be reduced.

[0059] In addition, as the (X) water-absorbent resin powder, a product obtained by crushing absorbed water-absorbent resin particles, mixing with a polyvalent metal salt to separate water, and then performing an acid treatment may be used. That is, used water-absorbent resin particles that have been used in some water-absorbent article and absorbed water can be crushed, dehydrated, and then acid-treated to regenerate the water-absorbing performance, and the resulting water-absorbent resin powder can be used as the (X) water-absorbent resin powder. Even with such a regenerated water-absorbent resin powder, the pure water permeability rate of the water-absorbing composition can be reduced by adjusting the particle size. In addition, since the used water-absorbent resin particles are crushed before the dehydration treatment, they may be subjected to a surface cross-linking treatment.

[0060] ((Y) Water-absorbent fiber) The water-absorbing composition contains (Y) water-absorbent fiber. The (Y) water-absorbent fiber is a fiber having water-absorbing properties. Absorption of water means that liquid water penetrates into the fiber by capillary action or the like.

[0061] The (Y) water absorbent fiber preferably has a water absorption amount of 0.2 g or more, more preferably 0.5 g or more, and even more preferably 1.0 g or more per 1 g of fiber, and preferably has a water absorption amount of 5.0 g or less, more preferably 3.5 g or less, and even more preferably 2.0 g or less per 1 g of fiber.

[0062] The number average fiber length of the (Y) water-absorbent fiber is preferably 1.2 mm or more, more preferably 1.5 mm or more, and even more preferably 1.7 mm or more, and is preferably 10 cm or less, more preferably 8 cm or less, and even more preferably 6 cm or less. If the number average fiber length of the (Y) water-absorbent fiber is 1.2 mm to 10 cm, the shape retention of the water-absorbent composition for water-blocking sheet is excellent. The number average fiber length of the (Y) water-absorbent fiber is measured in accordance with JIS P8226 (2006).

[0063] Examples of the (Y) water-absorbent fiber include cellulose fiber, acetate fiber, polyvinyl alcohol fiber, ethylene vinyl alcohol fiber, and polyacrylic acid sodium salt fiber. The cellulose fibers include natural cellulose fibers and regenerated cellulose fibers. The natural cellulose fibers include cotton, hemp, pulp, etc. The pulp includes wood pulp made from wood, non-wood pulp made from leaves, grass, straw, etc., waste paper pulp made from waste paper, etc., and regenerated pulp recovered from used absorbent articles, etc. The sodium polyacrylate fiber may be a fiber in which at least a part of the carboxyl groups of the polyacrylic acid fiber is modified to a sodium salt, for example, a fiber having a two-layer structure with an inner layer made of polyacrylic acid and an outer layer made of sodium polyacrylate. The sodium polyacrylate fiber may be a fiber in which polyacrylic acid fiber is heated in an aqueous sodium solution to carry out hydrolysis and crosslinking, and about 30% by mass of the polyacrylic acid constituting the fiber is modified to sodium polyacrylate.

[0064] The acetate fiber is a semi-synthetic fiber obtained by esterifying cellulose with acetate. Examples of the cellulose acetate fiber include cellulose diacetate fiber (esterification degree: 2.22 to 2.76) in which 74% or more and less than 92% of the hydroxyl groups of cellulose are esterified with acetate, and cellulose triacetate fiber (esterification degree: 2.76 or more) in which 92% or more of the hydroxyl groups of cellulose are esterified with acetate, and cellulose diacetate fiber is preferred. The esterification degree is the average number of hydroxyl groups substituted with acetyl groups per glucose unit in cellulose.

[0065] (Water absorbent composition) The water-absorbing composition contains (X) water-absorbent resin powder and (Y) water-absorbent fiber in a predetermined mass ratio, and the pure water permeation rate of the water-absorbing composition is 0.5 mL / min or less, preferably 0.4 mL / min or less, and more preferably 0.3 mL / min or less. If the pure water permeation rate is 0.5 mL / min or less, the water-impermeability of the water-shielding sheet is improved. The lower limit of the pure water permeation rate of the water-absorbing composition is 0 mL / min.

[0066] The pure water permeability of the water-absorbing composition can be adjusted by the particle size of the (X) water-absorbent resin powder and the amount of the (Y) water-absorbent fiber blended in. For example, the smaller the particle size of the (X) water-absorbent resin powder, the smaller the pure water permeability, and the greater the amount of the (Y) water-absorbent fiber blended in, the greater the pure water permeability.

[0067] The water-absorbing composition may contain additives such as preservatives, antifungal agents, antibacterial agents, antioxidants, ultraviolet absorbers, colorants, deodorants, inorganic powders, and organic fibrous materials. When these additives are contained, the content (mass%) of the additives is preferably 0.001 mass% to 10 mass%, more preferably 0.01 mass% to 5 mass%, further preferably 0.05 mass% to 1 mass%, and most preferably 0.1 mass% to 0.5 mass%, relative to the water-absorbing composition (100 mass%).

[0068] [Waterproof sheet] The waterproof sheet of the present invention comprises a first sheet, a second sheet laminated on the first sheet, and a water-absorbent layer disposed between the first sheet and the second sheet.

[0069] (water absorption layer) The water shielding sheet is characterized in that the water absorbing layer contains the water absorbing composition described above. By containing the water absorbing composition described above, the water shielding sheet has high flexibility and can better prevent water leakage even if a hole is formed in the base sheet.

[0070] The water impermeable sheet has a water absorbent layer having a water absorbent composition content of 350 g / m per unit area. 2 More preferably, 375 g / m 2 More preferably, 400 g / m 2 More than 700g / m 2 Preferably less than 675 g / m 2 Less than 650 g / m 2 The content is 350 g / m or less. 2 If it is more than 700g / m, the water impermeability is good. 2 If it is below this value, the sheet will be easy to install.

[0071] (1st sheet, 2nd sheet) The first sheet and the second sheet are for preventing water leakage, and liquid-impermeable sheets are used. The first sheet and the second sheet are joined to each other at the periphery of the water-shielding sheet so that the water-absorbent composition does not leak out. The first sheet and the second sheet may be joined by using an adhesive or by heat fusion.

[0072] The liquid-impermeable sheet is not particularly limited as long as it has sufficient strength as a waterproof sheet and can prevent liquid from penetrating. The liquid-impermeable sheet is preferably flexible, and is preferably made of a resin, elastomer, or rubber. Examples of the resin include thermoplastic resins such as polyolefin resins (polyethylene, polypropylene, etc.), polyester resins (polyethylene terephthalate, etc.), polyvinyl chloride resins, polyacrylic resins (polymethyl methacrylate, etc.), and polyamide resins (polyamide 6, polyamide 66). Examples of the elastomer include styrene-based elastomers such as styrene-isobutylene block copolymers and styrene-butadiene block copolymers, and polyolefin-based elastomers such as ethylene-vinyl acetate copolymers.

[0073] The thickness of the first sheet and the second sheet is not particularly limited as long as the sheet has sufficient strength as a waterproof sheet and can prevent liquid penetration. The thickness of the first sheet and the second sheet is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more, and is preferably 2000 μm or less, more preferably 1000 μm or less, and even more preferably 500 μm or less.

[0074] (Nonwoven fabric) The water-blocking sheet may have a nonwoven fabric disposed between the first sheet and the water-absorbent composition and / or between the second sheet and the water-absorbent composition. By disposing the nonwoven fabric, even if the first sheet or the second sheet is torn, leakage of the water-absorbent resin powder to the outside can be further suppressed. The nonwoven fabric is preferably disposed so as to cover the entire surface of the water-absorbing layer. It is preferable that the nonwoven fabric is not disposed at the joint between the first sheet and the second sheet.

[0075] The type of the nonwoven fabric is not particularly limited, and may be a spunbonded nonwoven fabric, a meltblown nonwoven fabric, a thermally bonded nonwoven fabric, a chemically bonded nonwoven fabric, a needle-punched nonwoven fabric, etc. The fibers constituting the nonwoven fabric are not particularly limited, but polyester resin fibers, polyamide resin fibers, polyolefin resin fibers, etc. are preferred.

[0076] The nonwoven fabric has a basis weight of 50 g / m 2 More preferably, 75 g / m 2 More preferably, 100 g / m 2 More than 500g / m 2 Preferably less than 400 g / m 2 More preferably, 300 g / m or less 2 The nonwoven fabric has a basis weight of 50 g / m or less. 2 If the density is more than 500g / m, the leakage of the water-absorbent resin powder can be further suppressed. 2 If the thickness is below this range, the waterproof sheet will have high flexibility and be easy to handle.

[0077] In the case where the water-shielding sheet has nonwoven fabrics disposed between the first sheet and the water-absorbent composition and between the second sheet and the water-absorbent composition, these nonwoven fabrics may be joined by needle punching. By joining these pairs of nonwoven fabrics, the water-absorbent composition can be prevented from shifting and becoming unevenly distributed inside the water-shielding sheet.

[0078] (adhesive layer) When the water-impermeable sheet has a nonwoven fabric disposed between the first sheet and the water-absorbent composition and / or between the second sheet and the water-absorbent composition, an adhesive layer may be disposed between the nonwoven fabric and the first sheet and / or between the nonwoven fabric and the second sheet. By disposing the adhesive layer, even if the first sheet or the second sheet is torn, leakage of the water-absorbent composition to the outside can be further suppressed. The adhesive layer is preferably disposed so as to cover the entire surface of the water-absorbent layer. The adhesive layer may also be disposed at the joint between the first sheet and the second sheet, and the first sheet and the second sheet may be joined by the adhesive layer.

[0079] The adhesive constituting the adhesive layer is preferably a hot melt adhesive, and examples of the hot melt adhesive include thermoplastic resins such as polyolefin resins (polyethylene, polypropylene, etc.), polyester resins (polyethylene terephthalate, etc.), polyvinyl chloride resins, polyacrylic resins (polymethyl methacrylate, etc.), polyamide resins (polyamide 6, polyamide 66), and polyurethane resins.

[0080] The adhesive layer has a basis weight of 10 g / m 2 More preferably, it is 20 g / m or more. 2 More preferably, 30 g / m 2 More than 100g / m 2 Preferably less than 80 g / m 2 Less than 70 g / m, more preferably 70 g / m 2 The adhesive layer has a basis weight of 10 g / m or less. 2 If the density is more than 100 g / m, leakage of the water-absorbent resin powder can be further suppressed. 2 If the thickness is below this range, the waterproof sheet will have high flexibility and be easy to handle.

[0081] (Surface non-woven fabric) The waterproof sheet may have a surface nonwoven fabric disposed on the outer surface side of the first sheet and / or the second sheet. By disposing the surface nonwoven fabric, damage to the first sheet and / or the second sheet can be prevented.

[0082] (Water-resistant sheet) The thickness of the waterproof sheet is not particularly limited, and is preferably 1 mm or more, more preferably 2 mm or more, and even more preferably 3 mm or more, and is preferably 10 mm or less, more preferably 8 mm or less, and even more preferably 6 mm or less.

[0083] The width of the waterproof sheet may be appropriately adjusted depending on the application, and is preferably, for example, 1 m to 3 m. The width of the water absorption layer is preferably 95% to 98% of the width of the waterproof sheet, which is 100%. The length of the waterproof sheet is not particularly limited.

[0084] The mass per unit area of ​​the waterproof sheet is 500 g / m 2 More preferably, 750 g / m 2 More preferably, 1000 g / m 2 More than 2000g / m 2 Preferably less than 1750 g / m 2 More preferably, 1500 g / m 2 The mass per unit area of ​​the waterproof sheet is the mass of the portion where the water absorption layer is disposed.

[0085] (Implementation) The waterproof sheet of the present invention will be described below with reference to Fig. 1. Fig. 1 is a schematic cross-sectional view of the waterproof sheet.

[0086] The waterproof sheet 1 comprises a first sheet 11, a second sheet 12 laminated on the first sheet, and a water absorbent layer 20 disposed between the first sheet 11 and the second sheet 12. The first sheet 11 and the second sheet 12 are formed to have the same shape in a plan view, and are joined to each other at the peripheral portion of the waterproof sheet.

[0087] The water-absorbing composition is disposed in the water-absorbing layer 20. The width of the water-absorbing layer 20 is formed narrower than the widths of the first sheet 11 and the second sheet 12, and the water-absorbing layer 20 is not disposed in the joint between the first sheet 11 and the second sheet 12.

[0088] A first nonwoven fabric 31 is disposed between the first sheet 11 and the water absorbent layer 20. A second nonwoven fabric 32 is disposed between the second sheet 12 and the water absorbent layer 20. The first nonwoven fabric 31 and the second nonwoven fabric 32 have substantially the same shape in plan view as the water absorbent layer 20, and are disposed so as to cover the entire surface of the water absorbent layer 20.

[0089] A first adhesive layer 41 is disposed between the first sheet 11 and the first nonwoven fabric 31. A second adhesive layer 42 is disposed between the second sheet 12 and the second nonwoven fabric 32. The shapes of the first adhesive layer 41 and the second adhesive layer 42 in a plan view are formed to be substantially the same as the shapes of the first sheet 11 and the second sheet 12 in a plan view. The first sheet 11 and the second sheet 12 are joined at their peripheral portions by the first adhesive layer 41 and the second adhesive layer 42.

[0090] Even if holes occur in the first sheet 11 and the second sheet 12 of the waterproof sheet 1, water leakage is prevented by the water-absorbent resin powder arranged in the water-absorbing layer 20 expanding due to moisture that penetrates through the holes. EXAMPLES

[0091] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.

[0092] [Production of water-absorbent resin powder] 155 parts by mass of acrylic acid (water-soluble ethylenically unsaturated monomer (a1-1)), 0.698 parts by mass of pentaerythritol triallyl ether (internal crosslinking agent (b1)), and 445 parts by mass of deionized water were stirred and mixed while maintaining the temperature at 1°C. Nitrogen was introduced into the mixture to reduce the amount of dissolved oxygen to 0.1 ppm or less, and then 0.310 parts by mass of an aqueous hydrogen peroxide solution (concentration 1% by mass), 1.16 parts by mass of an aqueous ascorbic acid solution (concentration 1% by mass), and 2.33 parts by mass of an aqueous 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide] solution (concentration 0.5% by mass) were added and mixed to initiate polymerization. After the temperature of the mixture reached 70°C, polymerization was carried out at 70±5°C for about 10 hours to obtain a hydrogel (1).

[0093] Next, 500 parts by mass of this hydrous gel (1) was chopped with a mincer (manufactured by ROYAL, "12VR-400K") while adding and mixing with 128 parts by mass of an aqueous sodium hydroxide solution (concentration 48.5% by mass) to obtain a chopped gel (2). The chopped gel (2) was further dried with a ventilated band dryer to obtain a dried body. The dried body was crushed several times using a juicer mixer (manufactured by Oster, "OSTERIZER BLENDER") until it passed through a sieve mesh with an opening of 850 μm.

[0094] Finally, the powder that passed through the sieve with an opening of 850 μm was sieved using a sieve with an opening of 105 μm to obtain a water absorbent resin powder (x1) having a particle size of 105 μm to 850 μm remaining on the sieve, and a water absorbent resin powder (x2) having a particle size of 105 μm or less that passed through the sieve.

[0095] [Production of water-absorbing composition] (Water absorbent composition 1) 90 parts by mass of the water absorbent resin powder (x1) and 10 parts by mass of the water absorbent resin powder (x2) were blended to obtain a water absorbent resin powder (X1-10). A water absorbent composition 1 was obtained by blending 98 parts by mass of this water absorbent resin powder (X1-10) and 2 parts by mass of pulp (pulp made from Southern Yellow Pine, a softwood produced in the United States, having a number average fiber length of 2.0 mm to 2.5 mm).

[0096] (Water absorbent composition 2) Water absorbent composition 2 was obtained in the same manner as water absorbent composition 1, except that the blending amounts of water absorbent resin powder (X1-10) and pulp were changed to 91 parts by mass of water absorbent resin powder (X1-10) and 9 parts by mass of pulp.

[0097] (Comparative water absorbent composition 1) Comparative water absorbent composition 1 was obtained in the same manner as water absorbent composition 1, except that the blending amounts of water absorbent resin powder (X1-10) and pulp were changed to 100 parts by mass of water absorbent resin powder (X1-10).

[0098] (Comparative water absorbent composition 2) Comparative water absorbent composition 2 was obtained in the same manner as water absorbent composition 1, except that the blending amounts of water absorbent resin powder (X1-10) and pulp were changed to 88 parts by mass of water absorbent resin powder (X1-10) and 12 parts by mass of pulp.

[0099] (Comparative water absorbent composition 3) Comparative water absorbent composition 3 was obtained in the same manner as water absorbent composition 1, except that the formulation was changed to 97.8 parts by mass of water absorbent resin powder (X1-10), 0.2 parts by mass of silica (AEROSIL (registered trademark) 200 manufactured by Nippon Aerosil), and 2 parts by mass of pulp.

[0100] (Water absorbent composition 3) 87 parts by mass of the water absorbent resin powder (x1) and 13 parts by mass of the water absorbent resin powder (x2) were blended to obtain a water absorbent resin powder (X1-13). The water-absorbing resin powder (X1-13) (98 parts by mass) and pulp (2 parts by mass) were blended together to obtain a water-absorbing composition 3.

[0101] (Water absorbent composition 4) A water-absorbing composition 4 was obtained by blending 98 parts by mass of the water-absorbing resin powder (x1) and 2 parts by mass of pulp.

[0102] (Comparative water absorbent composition 4) 84 parts by mass of the water absorbent resin powder (x1) and 16 parts by mass of the water absorbent resin powder (x2) were blended to obtain a water absorbent resin powder (X1-16). A comparative water-absorbing composition 4 was obtained by blending 98 parts by mass of this water-absorbing resin powder (X1-16) and 2 parts by mass of pulp.

[0103] (Water absorbent composition 5) While 100 parts by mass of the water absorbent resin powder (x1) was stirred at high speed (Hosokawa Micron Co., Ltd., high-speed stirring turbulizer: rotation speed 2000 rpm), 0.1 parts by mass of ethylene glycol diglycidyl ether, 1.0 parts by mass of propylene glycol and 1.6 parts by mass of water were added to a mixed liquid, which was mixed uniformly, and then heated at 120°C for 45 minutes to obtain a surface-crosslinked water absorbent resin powder (X2). The water absorbent resin powder (X2) was pulverized several times using a juicer mixer (manufactured by Oster, "OSTERIZER BLENDER") until it passed through a sieve with an opening of 850 μm. Further, it was sieved using a sieve with an opening of 105 μm to obtain a water absorbent resin powder (X3) having a particle size of 105 μm to 850 μm remaining on the sieve. The water-absorbing resin powder (X3) (98 parts by mass) and pulp (2 parts by mass) were blended to obtain a water-absorbing composition 5.

[0104] (Water absorbent composition 6) The water-absorbent resin powder (X2) was swelled 25 times with salt water (concentration 1% by mass), and then a calcium chloride aqueous solution (concentration 30% by mass) was added to release the water that had been retained. The powder after water release was washed with water and dried at 40°C for 2 hours to obtain powder (X4). The water content of this powder was 2.5 g / g. The dried powder (X4) was ground several times using a juicer mixer (Oster, "OSTERIZER BLENDER"), and then a mixture of 3.7 parts by mass of hydrogen chloride, 6.8 parts by mass of water, and 90.0 parts by mass of ethanol was added until the pH of the powder (X4) reached 6.0. Thereafter, the powder (X4) was washed with a mixed liquid of 50 parts by mass of isopropanol and 50 parts by mass of water, and dried at 80°C for 1 hour. Thereafter, the powder was sieved using sieves with openings of 105 μm and 850 μm to obtain a water absorbent resin powder (X5) having a particle size of 105 μm to 850 μm which passed through the sieve with openings of 850 μm and remained on the sieve with openings of 105 μm. A water-absorbing composition 6 was obtained by blending 98 parts by mass of this water-absorbing resin powder (X5) and 2 parts by mass of pulp.

[0105] [Table 1]

[0106] The pure water permeability rate of the water-absorbing composition obtained above was measured.

[0107] (Pure water flow rate) 0.02 g of the water-absorbing composition as a sample and 100 mL of pure water were placed in a 100 mL glass beaker and left for 60 minutes to swell the water-absorbing composition. Separately, a cylindrical filtration tube was prepared at the bottom end of the opening of a vertically standing cylinder (inner diameter 25.4 mm) equipped with a wire mesh (opening 150 μm, Sansho, sintered stainless steel filter 30SUS) and a capillary tube (inner diameter 4 mm, length 8 cm) with a cock (inner diameter 2 mm), and the entire contents of the beaker including the swollen measurement sample were placed in the cylindrical tube with the cock closed. Next, a cylindrical rod with a diameter of 2 mm and a wire mesh with a diameter of 25 mm and a mesh size of 150 μm at the tip was inserted into the filtration cylinder so that the wire mesh and the measurement sample were in contact with each other, and a weight was placed on the measurement sample so that a load of 1.0 kPa was applied. After leaving it in this state for 1 minute, the cock was opened to allow the liquid to flow, and the time (T1) (seconds) required for the liquid level in the filtration cylinder to reach the 40 mL scale line from the 60 mL scale line (i.e., 20 mL of liquid passed through) was measured, and the liquid passing rate was calculated. Pure water flow rate (mL / min)=(T1) / 20 The measurements were performed five times (n=5), one value from each of the top and bottom was deleted, and the average of the remaining three values ​​was used as the measured value. These measurements were performed at 23±2°C and a relative humidity of 50±5%, and the samples were stored in the same environment for at least 24 hours before the measurements. The pure water permeability rate was evaluated according to the following criteria. ◎: Less than 0.1mL / min, ○: 0.1mL / min or more, less than 0.5mL / min ×: 0.5mL / min or more

[0108] [Manufacturing of waterproof sheets] The first nonwoven fabric (polyester long fiber nonwoven fabric (weight 120g / m 2 ) was cut to a length of 60 cm and a width of 60 cm, and one side of this first nonwoven fabric was coated with a synthetic rubber hot melt adhesive (TN-202Z, manufactured by MORESCO) to a thickness of 10 μm. Next, on the surface of the first nonwoven fabric to which the adhesive was applied, any one of the water-absorbing compositions obtained above was applied in a weight of 500 g / m2 within a range (length 50 cm, width 50 cm) 5 cm inward from the peripheral edge of the first nonwoven fabric.2 The mixture was uniformly spread so as to form a water absorbing layer. Second nonwoven fabric (polyester long fiber nonwoven fabric (weight 120g / m 2 )) was cut to a length of 60 cm and a width of 60 cm, and a synthetic rubber-based hot melt adhesive (TN-202Z, manufactured by MORESCO) was applied to one side of this second nonwoven fabric to a thickness of 10 μm. A second nonwoven fabric was laminated on the surface of the first nonwoven fabric on which the water-absorbing composition had been sprayed, with the adhesive facing inward, and the resulting laminate was pressed to obtain a water-absorbing body. A synthetic rubber-based hot melt adhesive (TN-202Z, manufactured by MORESCO) was applied to both sides of the obtained water absorbent body to a thickness of 80 μm, and then a liquid-impermeable sheet (polyethylene sheet, thickness 50 μm) 60 cm long and 60 cm wide was attached to both sides. The edges of the liquid-impermeable sheet were folded back inward and glued and fused to obtain a waterproof sheet.

[0109] The obtained waterproof sheet was subjected to a nail hole waterproofing test, a flexibility test and a water-absorbent composition spillage test. The results are shown in Table 2.

[0110] (Nail hole watertightness test) The configuration of the nail hole water impermeability tester is shown in Fig. 2, and the drilling area of ​​a sample for the nail hole water impermeability test is shown in Fig. 3. The nail hole water impermeability tester has two flanged acrylic pipes (inner diameter R = 20 cm) 91, 92, covers 93, 94 provided on the openings of the pipes, and a wire mesh (8 mesh) 95 placed between the pipes 91, 92. A test piece (waterproof sheet) 96 was placed on a wire mesh 95, and five through holes 95a were opened using a nail for slate tiles (length 30 mm, maximum diameter 3.3 mm, minimum diameter 2.9 mm, distance between maximum diameter (minimum diameter) and maximum diameter (minimum diameter) 1.3 mm). The through holes were formed so that the distance d between the through holes was 5 cm, as shown in FIG. 3. A wire mesh 95 and a test piece 96 were sandwiched between pipes 91 and 92 from above and below, and flanges 91a and 92a were fixed with bolts 97. 500 g of pure water was poured into the upper pipe 91 as test water 98. Thereafter, the openings of pipes 91 and 92 were sealed with lids 93 and 94, respectively, and the presence or absence of liquid leakage (liquid migration to the lower pipe 92) was confirmed after 24 hours. The test was carried out on 10 test pieces of each waterproof sheet in a liquid temperature of 25°C, and the results were evaluated according to the following criteria. ○: 0 pieces had liquid leakage ×: 1 to 4 leaks ××: 5 or more leaks

[0111] (Flexibility test) A waterproof sheet 60 cm long and 60 cm wide was manually wrapped around a paper tube with an outer diameter of 7.5 cm to check whether it could be completely wrapped, and was evaluated according to the following criteria. ◎:Can be wrapped around 〇: It can be wrapped around, but it breaks ×: Cannot be wrapped

[0112] (Water-absorbent composition spill test) A waterproof sheet 60 cm long and 60 cm wide was cut around the periphery, leaving the center, and adjusted to a width of 20 cm and a length of 20 cm. The cut surface was then sealed with adhesive tape to prevent the contents from spilling out, and a test specimen was prepared. As with the nail hole waterproof test, five through holes were formed in the center and around the test specimen. The test piece was placed in the sieve frame of a vibrating sieve machine (small vibrating sieve machine "KS-300" manufactured by Labnect) equipped with a sieve mesh with an opening of 2.00 mm (10 mesh). After vibrating the vibrating sieve machine for 10 minutes, the presence or absence of the water-absorbing composition spilling out from the upper and lower surfaces of the test piece was confirmed, and the test piece was evaluated according to the following criteria. ⊚: No water-absorbing composition was observed on the surface of the test piece or at the outlet of the vibrating sieve. ◯: The water-absorbing composition was not observed at the discharge port of the vibrating sieve machine, but was observed on the surface of the test piece. ×: The water-absorbing composition was confirmed at the outlet of the vibrating sieve.

[0113] [Table 2]

[0114] Water impermeable sheets 1 to 6 have water absorbent layers formed from water absorbent compositions 1 to 6. These water absorbent compositions 1 to 6 have a mass ratio ((X) / (Y)) of (X) water absorbent resin powder to (Y) water absorbent fiber of 90 / 10 to 99 / 1, a content of particles having a particle diameter of 105 μm or less contained in 100 mass% of (X) water absorbent resin powder of 15 mass% or less, and a pure water permeation rate of the water absorbent composition of 0.5 mL / min or less. These water shielding sheets 1 to 6 were excellent in flexibility and water impermeability, and also suppressed spillage of the water absorbent composition. Among these, water shielding sheets 1, 2, 4 to 6, in which the content of particles having a particle diameter of 105 μm or less contained in 100 mass% of (X) water absorbent resin powder is 10 mass% or less, further suppressed spillage of the water absorbent composition. In addition, comparing water shielding sheets 1 and 4, it is found that the one in which (X) water absorbent resin powder contains particles having a particle diameter of 105 μm or less has a slower pure water permeability speed and thus a higher water impermeability.

[0115] Comparative waterproof sheet 1 is a case where the water-absorbent composition does not contain the water-absorbent fiber (Y). This comparative waterproof sheet 1 had poor flexibility. Comparative water-shielding sheets 2 and 3 are those in which the pure water permeation rate of the water-absorbing composition exceeds 0.5 mL / min. These comparative water-shielding sheets 2 and 3 were inferior in water-shielding property. Comparative water-shielding sheet 4 is a case where (X) the content of particles having a particle diameter of 105 μm or less contained in 100% by mass of water-absorbent resin powder exceeds 15% by mass. This comparative water-shielding sheet 4 was unable to suppress spillage of the water-absorbent composition. [Industrial Applicability]

[0116] INDUSTRIAL APPLICABILITY The waterproof sheet of the present invention can be suitably used for bank protection works on coasts and rivers, for preventing water leakage in reservoirs, and for preventing leakage of wastewater into the ground at waste disposal sites. [Explanation of symbols]

[0117] 1: waterproof sheet, 11: first sheet, 12: second sheet, 20: water absorbing layer, 31: first nonwoven fabric, 32: second nonwoven fabric, 41: first adhesive layer, 42: second adhesive layer

Claims

1. A water-absorbing composition for use in a water shielding sheet, comprising: (X) water-absorbent resin powder and (Y) water-absorbent fiber, The mass ratio ((X) / (Y)) of the water-absorbent resin powder (X) to the water-absorbent fiber (Y) in the water-absorbent composition is 90 / 10 to 99 / 1; The content of particles having a particle diameter of 105 μm or less contained in 100% by mass of the (X) water absorbent resin powder is 15% by mass or less, A water-absorbing composition for a water-shielding sheet, characterized in that the pure water permeability rate of the water-absorbing composition is 0.5 mL / min or less.

2. The water-absorbent composition for water-shielding sheets according to claim 1, wherein the (Y) water-absorbent fiber is at least one selected from the group consisting of cellulose fiber, acetate fiber, polyvinyl alcohol fiber, ethylene vinyl alcohol fiber, and polyacrylic acid sodium salt fiber.

3. 2. The water-absorbing composition for a water-blocking sheet according to claim 1, wherein the water-absorbing resin powder (X) is obtained by crushing water-absorbing resin particles that have been subjected to a surface cross-linking treatment.

4. The water-absorbing composition for water-blocking sheets according to claim 1, wherein the water-absorbing resin powder (X) is obtained by crushing water-absorbent resin particles that have absorbed water, mixing the crushed particles with a polyvalent metal salt to remove water, and then treating the crushed particles with an acid.

5. A water-absorbing layer is disposed between a first sheet, a second sheet laminated on the first sheet, and a water-absorbing layer disposed between the first sheet and the second sheet. The water-absorbing layer contains the water-absorbing composition according to any one of claims 1 to 4, The content of the water-absorbing composition per unit area of ​​the water-absorbing layer is 350 g / m 2 ~700g / m 2 A waterproof sheet characterized by:

Citation Information

Patent Citations

  • Water-barrier sheet

    JP1996074223A

  • Water absorptive composite sheet for water barrier sheet, its manufacturing method and water barrier sheet