gasket
Patent Information
- Application Number
- JP2023539754
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-22
- Filing Date
- 2021-12-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-13
AI Technical Summary
Existing sealing components in semiconductor manufacturing, such as fluorinated elastomers, suffer from gas permeation issues with small molecules like O2 and N2, while all-metal gaskets require precise seating and polishing, and dual-gasket solutions necessitate nitrogen purging, posing challenges in achieving effective gas barrier performance under harsh conditions.
A gasket composed of two parts: a flexible elastomer (e.g., perfluoroelastomer) and a rigid, low-permeability material (like metal) is designed, where the metal part is firmly fixed to the elastomer, forming a strong bond to prevent gas permeation by aligning perpendicular to the sealing interface.
The dual-part gasket effectively reduces or prevents gas permeation, maintaining high vacuum or pressure within devices by combining the flexibility of elastomers with the impermeability of metals, without the need for complex installation procedures.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] GASKET FOR PREVENTING GAS PERMEATION UNDER HIGH VACUUM CONDITIONS FIELD OF THE DISCLOSURE The present invention relates to gaskets, particularly O-rings, and methods of forming the gaskets, which are useful as sealing components used in semiconductor wafer processing techniques. [Background technology]
[0002] In order to more fully describe the technical field to which the present invention pertains, several patents and publications are cited herein, the entire disclosures of each of which are incorporated herein by reference.
[0003] Sealing components (O-rings, gaskets, etc.) are exposed to harsh conditions such as high temperatures and many types of organic solvents and gases, some of which can be corrosive, reactive, or otherwise erosive. Fluorinated elastomers are widely used in sealing components in various industries because they have desirable elastic properties, low chemical reactivity, and high heat resistance. Devices using sealing components formed from fluorinated elastomers can achieve high vacuum or pressure conditions because such sealing components can function effectively even when used under such harsh conditions.
[0004] Sealing components used in semiconductor manufacturing technology, such as chamber seals for vacuum or deposition process equipment, are exposed to special gases (e.g., deposition process gases or chamber cleaning gases) and plasma. Since semiconductor wafer processing is performed under high temperatures, such sealing components also require high heat resistance. Based on the excellent properties mentioned above, fluorinated elastomers are good candidates for use under harsh conditions, but gas permeation is an issue because fluorinated elastomers can only permeate small molecular gases (e.g., O2 or N2) at only 1×10 -4Pa) permeation. All-metal gaskets are sometimes used for such purposes because metal can prevent gas permeation. However, because metal has relatively low flexibility, all-metal gaskets must be carefully seated and bolted in place to provide an optimal seal. Furthermore, when metal gaskets are used, the flanges that contact the metal gasket must be polished to a mirror finish. Another conventional technique uses a combination of two gaskets, one a perfluoroelastomer gasket with high heat resistance and the other a partially fluorinated elastomer gasket with low gas permeation. However, the implementation of this technique is not an easy task because a nitrogen gas purge is required between the two seals. Thus, there is still an urgent need for flexible sealing components that can prevent the permeation of small molecule gases.
[0005] US Pat. No. 9,290,838(B) discloses a diffusion-resistant metal-coated O-ring having a malleable metal coating on at least a portion of the surface of the O-ring. Summary of the Invention [Means for solving the problem]
[0006] Provided herein is a gasket useful for semiconductor wafer process technology. The gasket is located between two components and can prevent or reduce the transmission of low molecular gas (e.g., O2 or N2) between the two components. The gasket of the present technology is formed of two parts. The first part is made of elastomer (fluoroelastomer, particularly perfluoroelastomer), and the second part is made of rigid material (such as metal) with low gas permeability. The second part is rigidly fixed to the first part, so that the gas transmission between the two components is substantially reduced or completely prevented. [Brief description of the drawings]
[0007] [Figure 1]1 is a cross-sectional view of a portion of one embodiment of a gasket of the present invention positioned between two components to be sealed. [Figure 1a] FIG. 2 is a cross-sectional view of FIG. 1, with the arrows indicating the applied force sealing the two components with the gasket. [Diagram 2] 1 is a cross-sectional view of a portion of another embodiment of a gasket of the present invention positioned between two components to be sealed. [Figure 2a] FIG. 3 is a cross-sectional view of FIG. 2, with the arrows indicating the applied force sealing the two components with the gasket. [Diagram 3] 13 is a cross-sectional view of a portion of yet another embodiment of a gasket of the present invention positioned between two components to be sealed. [Figure 3a] FIG. 4 is a cross-sectional view of FIG. 3, with the arrows indicating the applied force sealing the two components with the gasket. [Figure 4] FIG. 2 is a plan view of the gasket of the present invention. [Figure 4a] FIG. 2 is a side cross-sectional view of a gasket of the present invention. [Diagram 5] FIG. 2 is a cross-sectional side view of a gasket of the present invention in sealing engagement with two components. [Figure 5a] FIG. 2 is a cross-sectional perspective view of a gasket of the present invention in sealing engagement with two components. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The gasket of the present invention includes two components: (A) a first component made from an elastomer and (B) a second component made from a material having less gas permeable and less flexible properties than the elastomer.
[0009] The first part is made of an elastomer. In particular, fluorinated elastomers are preferred due to their excellent properties, such as desirable elasticity, low chemical reactivity, good solvent resistance, and high heat resistance. Fluoroelastomers (FKM) and perfluoroelastomers (FFKM) can be used. Conventional fluoroelastomers include copolymerized units of tetrafluoroethylene, vinylidene fluoride, or another partially fluorinated comonomer, such as fluoro(methyl vinyl ether), and a cure site monomer. Conventional perfluoroelastomers include copolymerized units of tetrafluoroethylene, perfluoro(methyl vinyl ether), and a cure site monomer. Suitable fluoroelastomers include, but are not limited to, those described in U.S. Patent No. 8,765,876 issued to Bish et al. Fluoroelastomers may be synthesized by the methods described in Kaiser, RJ, et al., "Synthesis of Transparent Fluorocarbon Elastomers: Effect of Crosslinker Type and Electron Beam Irradiation Level on Physical and Mechanical Behavior", Journal of Applied Polymer Science, Vol. 27, pages 957-968 (1982), and references cited therein. Suitable perfluoroelastomers include, but are not limited to, those described in U.S. Pat. No. 6,281,296 issued to MacLachlan et al. and U.S. Pat. No. 6,191,208 issued to Kohtaro Takahashi, and may be prepared by the methods described in these references.
[0010] The first part, due to its desirable elastic properties, functions to prevent gas leakage (i.e. gas diffusion) and maintain high pressure or high vacuum in the device in which the gasket is used. The first part is made of a flexible material (elastomer), which provides flexibility of the sealing structure and smoothness of the surface of the sealing structure when the gasket is adapted to the sealing component. The first part, when the gasket is used in the sealing structure, is compressed to a linear compression rate of 3-40%, preferably a linear compression rate of 10-30%, which line is the maximum diameter of the cross section of the first part perpendicular to the radius of the gasket. This line is shown as aa, for example, in Figures 4a and 5, and as an arrow in Figures 1a, 2a, and 3a. As used herein, the term "perpendicular" refers to a direction parallel to the line aa.
[0011] The second part is made of a material that has properties of less gas permeability and less flexibility than elastomers. Any material that meets this requirement can be used, but metals and metal alloys are preferred due to their rigidity and low gas permeability. Metals or metal alloys that have low reactivity with chamber cleaning gases or plasmas are more preferred. In this regard, aluminum or aluminum alloys can be used. Metals of note for use in the second part are stainless steel 304, 316, and aluminum A1000, A5000, and A6000 series. The permeability of these metals to small molecule gases is considered to be zero or at least substantially zero when used at the thicknesses described herein. As used herein, the term "substantially zero" refers to a value greater than zero and less than 1×10 -8 This refers to pressure below Pa.
[0012] The second part has a thickness. The thickness depends on the size of the first part and the material of the second part. The thickness should be such that the second part does not break or undergo irreversible bending deformation due to the compressive forces shown as arrows in Figures 1a, 2a and 3a when the gasket is located between the two components to be sealed. Such breakage or deformation may be observed by visual inspection. Alternatively, a high gas permeability may indicate that the second part is damaged.
[0013] For example, if the second part is made of aluminum, the thickness of the aluminum is preferably about 0.2 to about 10 mm when the cross-section of the elastomer (first part) along line aa has a diameter of 3.5±0.10 mm. Again, high gas permeability may indicate that the second part is insufficiently thick.
[0014] The second part acts as a gas permeation barrier to small molecule gases. The elastomer can essentially prevent air from leaking, but small amounts of small molecule gases such as oxygen or nitrogen gas can permeate the elastomer. -4 Even the permeability that produces pressures of Torr is enough to destroy some processes, such as deposition processes or semiconductor wafer processes.
[0015] The second part is made of a less flexible material, but should be in full contact with the surfaces of both components of the sealing structure. To ensure full contact, the second part may be compressed vertically, i.e., along the lines shown as aa in Figures 4a and 5 and as arrows in Figures 1a, 2a, and 3a, to a linear compression of less than 5%.
[0016] The first part of the gasket must be firmly bonded to the second part of the gasket.
[0017] When the first part is made of a perfluoroelastomer and the second part is made of a metal or metal alloy, the gasket can be manufactured by the following steps: (a) providing a metal part of a gasket (meaning a second part comprising metals and metal alloys), the surface of the metal part to be bonded to the perfluoroelastomer is chemically or mechanically treated; (b) compression molding the curable perfluoroelastomer composition onto a surface of a metal part; It can be formed by:
[0018] In step (a), the surface of the metal part is treated chemically or mechanically to form a strong metal-perfluoroelastomer bond. Because perfluoroelastomers are chemically inert, bonding of metal surfaces to perfluoroelastomers is difficult. A typical example of chemical pretreatment of metal surfaces is an adhesion primer or bonding agent. Such chemicals can be coated on the surface of the metal part to improve the bond strength between the perfluoroelastomer and the metal part. Another example of strong bonding between metal and perfluoroelastomer is the use of an anchor effect by roughening the surface of the metal, for example by creating scratches or pores. Acid etching, galvanizing chromate treatment, sandblasting, laser etching, and anodizing can be used. When the metal is aluminum or an aluminum alloy, the method disclosed in European Patent No. 1,855,864(B) by Minowa et al. can be used to anodize the surface of aluminum (alloy) to form a porous surface.
[0019] In step (b), the curable perfluoroelastomer composition is used to form a perfluoroelastomer part (i.e., the first part) on the metal part. Usually, perfluoroelastomers are amorphous polymeric compositions having copolymerized units of at least two main perfluoromonomers. Typically, one of the main comonomers is a perfluoroolefin, and the other is a perfluorovinyl ether. Representative perfluoroolefins include tetrafluoroethylene and hexafluoropropylene. Suitable perfluorovinyl ethers include those of formula (I): CF2 = CFO(RfO) n (Rf'O) m Rf” (I) In the formula, Rf and Rf' are different linear or branched perfluoroalkylene groups having 2 to 6 carbon atoms, m and n are independently 0 to 10, and Rf'' is a perfluoroalkyl group having 1 to 6 carbon atoms.
[0020] Other suitable fluoroelastomers and perfluoroelastomers are described in the Bish, Kaiser, MacLachlan, and Takahashi references cited above.
[0021] The curable perfluoroelastomer composition is compression molded onto the porous surface of the metal part. The mold is in the shape of a gasket. The metal part is placed in the mold before the curable perfluoroelastomer composition is placed in the mold. Molding is performed under pressure and at elevated temperature for a time sufficient to at least partially cure (i.e., vulcanize or crosslink) the perfluoroelastomer and bond it to the metal surface. The bond is enhanced by the perfluoroelastomer compound flowing under pressure into the porous surface structure of the metal before crosslinking. Optionally, the resulting perfluoroelastomer-metal part may be postcured at elevated temperature for a time sufficient to improve the physical properties of the elastomer and the bond strength of the cured elastomer to the metal surface. The postcure may be performed in an air oven or in an inert atmosphere. Typical compression molding conditions are 4-8 minutes at a temperature of 180-220°C. Typical postcure conditions are 5-48 hours at a temperature of 250-315°C. Similar molding processes are described in the MacLachlan and Takahashi patents referenced above.
[0022] For example, when used to form a seal for a vacuum chamber or pressurized vessel, the gasket is placed between two components to seal the gap between the two components. Preferably, the first and second components are positioned such that when the gasket is installed as a seal between the two components, the first component is proximal to the vacuum side of the two components and the second component is proximal to the external atmosphere side of the two components such that gas transmission between the two components is reduced or prevented.
[0023] Referring now to the drawings, in which like reference numbers indicate corresponding structures throughout the figures, and in particular to FIG. 1, a cross-sectional view of one embodiment of the gasket (100) of the present invention is shown. The gasket (100) is formed of an elastomer (11) and a metal (21), preferably aluminum, which are rigidly connected to each other. The gasket (100) is located between two components (31, 41) and seals the gap between the two components (31, 41). When the gasket is used in semiconductor manufacturing technology, the inner elastomer side (11) of the gasket (100) is exposed to vacuum or to special gases (such as deposition process gases or chamber cleaning gases) and plasmas present inside the sealed components (50). A second part, a metal or metal alloy (21), is located on the outside of the gasket (100) to prevent gas permeation. The metal or metal alloy part (21) is located in a vertical direction perpendicular to the surfaces of the two components (31, 41).
[0024] In other words, the second part (21) is fixed to the first part (11), and the first part and the second part are positioned such that when the gasket (100) is installed as a seal between the two components (31, 41), the first part (11) is proximal to the vacuum or process side (50) of the two components (31, 41) and the second part (21) is proximal to the external atmosphere side of the two components (31, 41) so that gas permeation into the space (50) defined by the two components (31, 41) is reduced or prevented.
[0025] FIG. 2 shows a cross-sectional view of another embodiment of a gasket (100) formed from a metal part (21) and an elastomeric part (11). As in FIG. 1, the metal part is located on the outside and the elastomeric part is located on the inside (50) of the gasket. In addition, the cross-sectional view of the gasket is approximately circular. Advantageously, the overall view of the gasket shown in FIG. 2 resembles the shape of a conventional gasket formed from a fluorinated elastomer, such as a torus or an O-ring. Thus, the gasket shown in FIG. 2 can be applied in conventional applications and provides improved sealing as described above without elaborate and expensive retooling to change the structure of the sealing components (31, 41) of current equipment.
[0026] In particular, in Figures 1 and 2, the interface between the elastomer (11) and the metal (21) is cylindrical with a circular cross section of constant diameter and a vertical axis, i.e., perpendicular to the plane of the gasket and to the surfaces of the two components (31, 41).
[0027] Referring now to FIG. 3, a cross-sectional view of another embodiment of the present invention is shown in which a gasket (100) is located between two components (31, 41) to be sealed. As in FIGS. 1 and 2, the elastomeric part (11) is located inside the gasket, proximal to the interior (50) of the sealed chamber. Also as in FIG. 2, the overall view of the gasket (100) is similar to that of a conventional gasket. However, the embodiment of FIGS. 1 and 2 is distinguished from the embodiment of FIG. 3 by the shape of the interface between the elastomer (11) and the metal (21). The interface between the elastomer and the metal in FIG. 3 is not accurately depicted as a cylinder with a circular cross-section with a constant diameter and a vertical axis, i.e., an axis perpendicular to the surfaces of the two components (31, 41). Rather, this interface is a curved shape. Although its cross-section is circular, its diameter is not constant with respect to the distance between the sealing components (31, 41). Any shape of contact is suitable for use in this orientation, provided that thorough contact and proper bonding between the elastomer (11) and metal (21) can be achieved by the methods described herein.
[0028] 1a, 2a, and 3a, the embodiments of Figures 1, 2, and 3 have been replicated with the addition of arrows showing the sealing force applied perpendicularly to the sealing components (31, 41). In all three of the illustrated embodiments, the second part (21) is oriented perpendicular to the direction of gas permeation between the two components. Gas moving from the exterior of the sealed chamber to its interior (50) must move in a direction represented by a vector having a component perpendicular to the perpendicular direction shown by the arrows.
[0029] A person skilled in the art can design a metal part (21) adapted for application of a force having a specified magnitude and direction in a given linear compression. Design choices include the choice of metal and cross section of the metal part (21). For example, in comparison with the gasket (100) of Figures 1 and 1a, the gasket (100) as shown in Figures 2 and 2a may be used for a seal requiring a larger than typical force to be applied in a vertical direction, and the gasket (100) as shown in Figures 3 and 3a may be used for a seal requiring a smaller than typical force to be applied in a vertical direction.
[0030] 4, a plan view of gasket 100 shows lines bb and cc in the plane of gasket 100. Additionally, elastomeric part 11 is proximal to interior 50 of sealed components (31, 41), which are not shown in FIG.
[0031] 4a, this cross-sectional view of gasket 100 shows a vertical axis aa perpendicular to lines bb and cc in the plane of the gasket, lines bb and cc not shown in FIG.
[0032] Now referring to Figure 5, the sealed structure includes two sealing components (31, 41) and a gasket (100). Each component (31, 41) has a surface parallel to the surface of the other component, and the gasket (100) is disposed between the two parallel surfaces to seal the components (31, 41) and prevent gas leakage to the interior (50). The second part (21) is fixed to the first part (11) in a direction perpendicular to the direction of the parallel surfaces of the components (31, 41). In other words, the second part (21) is fixed to the first part (11) in a direction parallel to the line aa.
[0033] Referring now to FIG. 5a, a cross-sectional perspective view of a gasket (100) in sealing engagement with two components (31, 41) shows the second part (21) forming continuous contact with the surfaces of each component (31, 41).
[0034] Although a circular gasket such as a torus or O-ring is shown in Figures 4 and 5a, the gasket of the present invention may have any shape known for gaskets or required by the design of the equipment to be sealed. Other conventional shapes for gaskets include ovals and rectangles with rounded corners, e.g., squares.
[0035] Although not shown in the drawings, either or both sealing components (31, 41) may be provided with one or more holes in addition to the holes sealed by the gasket of the present invention. These holes may be sealed from gas permeation by the gasket of the present invention or by other means. For example, the sealing components (31, 41) may be provided with holes for gas inlet valves, vacuum ports, or openings into which instruments may be inserted, including, but not limited to, heaters, pressure gauges, electrodes, and probes such as temperature probes, Langmuir probes, or QMS probes.
[0036] The following examples are presented to further illustrate the present invention. These examples, which represent preferred modes presently contemplated for carrying out the invention, are intended to illustrate, but not to limit, the invention. EXAMPLES
[0037] Test sample Test sample 1: Newly developed gasket shown in Figure 1 Test sample 2: Newly developed gasket shown in Figure 2 Test Sample 3: A conventional O-ring made from a perfluoroelastomer (AS568 228 O-ring made from FFKM) Test Sample 4: A conventional O-ring made from a fluorinated elastomer (AS568 228 O-ring made from FKM)
[0038] Test sample 1 and test sample 2 were FFKM (11) and aluminum (21) bonded parts made by the co-curing molding process. The curable perfluoroelastomers were prepared according to the methods described in the above-cited U.S. Pat. Nos. 6,281,296 and 6,191,208 and EP 1,855,864(B). The bonding method is also disclosed by EP 1,855,864(B). Test sample 3 and test sample 4 were obtained commercially.
[0039] Vacuum seal gas permeation testing equipment and method Test-1 The test instrument is a vacuum chamber with a stainless steel AS568 228 O-ring sized flange for vacuum sealing. A vacuum pump and a QMS (quadrupole mass spectrometer) are attached to the chamber. Ribbon heaters are attached around the periphery of the chamber and a thermostatted mantle heater is attached around the flange to heat the instrument to above 200°C.
[0040] The two-piece gaskets of the test samples (Test Samples 1, 3, and 4) were attached to the flanges of the instrument to create a vacuum seal. The chamber was heated to 1×10 -7 The chamber was heated to an ultra-vacuum level of 100 Pa. The ribbon heaters kept the chamber constantly heated at 100°C. When the mantle heater around the flange was off, the flange temperature was 52°C due to heating by the ribbon heater around the chamber. The vacuum was maintained by running the vacuum pump continuously. The heater around the flange was increased in temperature to 200°C at a rate of 2.5°C / min by the mantle heater around the flange, while the heater around the chamber was still set at 100°C.
[0041] The air pressure in the vacuum chamber resulting from seal permeation was measured by the QMS when the temperature of the heater around the flange was recorded at 100° C., 150° C., and 200° C. At these temperatures, the partial pressures of N2 and O2 were also measured.
[0042] Test-2 An aluminum flange was also prepared for test sample 2. Due to the difference in thermal conductivity between stainless steel and aluminum, the measurement start temperature was 66°C. Transmission measurements were performed 10 times to confirm repeatability against temperature thermal cycles. Since the flange was made of aluminum, the surface of test sample 2 was inspected by a 3D image measuring instrument model VHX-7000 of KEYENCE Corp., Itasca, IL, after the test to ensure that the flange had no physical damage that would make it unsuitable for repeated use. No scratches were found on the surface.
[0043] Gas permeability (air, N2, and O2) test results. Test-1 The air permeability results are shown in Table 1, the N2 permeability results are shown in Table 2, and the O2 results are shown in Table 3. All gas permeabilities reported herein are in Pascals (Pa).
[0044] [Table 1]
[0045] [Table 2]
[0046] [Table 3]
[0047] Test-2 The air permeability results are shown in Table 4, the N2 permeability results are shown in Table 5, and the O2 results are shown in Table 6.
[0048] [Table 4]
[0049] [Table 5]
[0050] [Table 6]
[0051] After completion of test 2, no damage to the flange was observed.
[0052] Although certain preferred embodiments of the present invention have been described and specifically exemplified above, it is not intended that the present invention be limited to such embodiments. Rather, while many of the features and advantages of the present invention have been set forth in the foregoing description, together with details of the structure and function of the present invention, it should be understood that the present disclosure is merely illustrative, and that changes may be made in the details, particularly with respect to the shape, size and arrangement of parts, within the principles of the present invention to the maximum extent indicated by the broad general meaning of the terms in which the appended claims are expressed.
Claims
1. 1. A gasket for sealing two components from gas transmission, said gasket comprising: (A) a first component comprising an elastomer; (B) a second component comprising a material that is less gas permeable and less flexible than the elastomer; and Including, the second component is secured to the first component, and the first and second components are positioned such that, when the gasket is installed as a seal between the two components, the first component is proximate to a vacuum side of the two components and the second component is proximate to an external atmosphere side of the two components such that gas transmission between the two components is reduced or prevented. gasket.
2. The gasket of claim 1 , wherein the second part is oriented perpendicular to a direction of gas permeation between the two components.
3. The gasket of claim 1 , wherein the contact portion of the first component and the second component is cylindrical in shape.
4. The gasket of claim 1 , wherein the first component comprises a fluorinated elastomer.
5. The gasket of claim 1 , wherein the first component comprises a perfluoroelastomer.
6. The gasket of claim 1 , wherein the second component comprises a metal or a metal alloy.
7. The gasket of claim 1 , wherein the second component comprises aluminum or an aluminum alloy.
8. 8. The gasket of claim 7, wherein the aluminum or aluminum alloy contact surface has pores, and at least a portion of the elastomer is inserted into the pores by compression molding.
9. A method of manufacturing a gasket for sealing two components from gas permeation, said gasket comprising: (A) a first part made from an elastomer; and (B) a second part made from a metal or metal alloy, said method comprising: (a) providing a metal part made of a metal or metal alloy, the surface of said metal part to be bonded to a perfluoroelastomer being chemically or mechanically treated; (b) compression molding a curable perfluoroelastomer composition onto the surface of the metal component; A method comprising:
10. A sealing structure comprising two components and the gasket of claim 1, each component having surfaces facing parallel to each other, the gasket is disposed between the two surfaces to seal the component against gas leakage; the second part is fixed to the first part in a direction perpendicular to the direction of gas permeation between the two components; Sealed structure.
11. The sealed structure of claim 10, wherein the first part is compressed to a linear compression rate of 3 to 40%.
12. The sealed structure of claim 10 , wherein the second part forms continuous contact with the surface of each component.
13. The sealing structure of claim 10 used for high vacuum sealing of equipment used in semiconductor manufacturing processes or flat panel display manufacturing processes.