Method for recycling poly(vinyl butyral) from multilayer poly(vinyl butyral) sheets.

JP2024502490A5Active Publication Date: 2024-10-29SOLUTIA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023541913
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-11
Filing Date
2022-01-07
Publication Date
2024-10-29
Estimated Expiration
2042-01-07

AI Technical Summary

Technical Problem

Conventional methods for recycling multilayer poly(vinyl butyral) sheets result in visual defects due to the incompatibility of poly(vinyl butyral) compounds in the skin and core layers, leading to inferior products with haze issues.

Method used

A method involving grinding the multilayer sheets to obtain granules, adding additional plasticizer to separate soft poly(vinyl butyral), and using techniques like decantation, filtration, or centrifugation to enrich the granules with rigid poly(vinyl butyral), producing a varnish that can be used to form high-quality interlayers.

Benefits of technology

The method effectively recovers rigid poly(vinyl butyral) with minimal haze, enabling the production of high-quality interlayers suitable for laminated glass applications, reducing waste and environmental impact while lowering production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2022150528000001
    Figure 2022150528000001
Patent Text Reader

Abstract

A method for recovering stiff poly(vinyl butyral) from a plasticized poly(vinyl butyral) multi-layer sheet containing stiff poly(vinyl butyral) and soft poly(vinyl butyral) is disclosed. The method includes the steps of grinding the plasticized poly(vinyl butyral) multi-layer sheet to obtain granules, adding additional plasticizer to the granules to remove at least a portion of the soft poly(vinyl butyral), and physically separating the granules from the resulting solution.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This disclosure relates to the field of recycling polymer interlayers for multiple layer glass panels having at least one polymer interlayer sheet having a plurality of poly(vinyl butyral) components. [Background technology]

[0002]

[0002] Laminated safety glass used in automotive windshields and architectural safety glass typically consists of two sheets of glass laminated together with a plasticized polymer interlayer between them. Poly(vinyl butyral) ("PVB") is generally the major component in the polymer interlayer.

[0003]

[0003] Poly(vinyl butyral) resins are typically mixed with plasticizers before being melt extruded into sheets. Poly(vinyl butyral) resins and plasticizers are typically manufactured by a synthetic process that begins with the use of non-renewable raw materials. Poly(vinyl butyral) is obtained by the reaction of poly(vinyl alcohol) and butyraldehyde. The properties of poly(vinyl butyral) are determined by its molecular structure, residual hydroxyl content, and residual acetate content, which are characterized by parameters such as its molecular weight and its distribution.

[0004]

[0004] In recent years, multi-layer poly(vinyl butyral) interlayers for laminated glass have been marketed and are finding increasing application in laminated safety glass. Multi-layer interlayers can provide enhanced acoustic insulation by having a softer layer ("core layer") in the center of the sheet. Typically, the core layer composition differs from the composition of the outer layers ("skin layers") with respect to the amount of plasticizer relative to the amount of polymer. The plasticizer content is typically higher in the core layer than in the skin layers. To allow for such differences in composition between the layers, the PVB compound in the core layer has a different composition from the PVB compound in the skin layers with respect to hydroxyl group content or even residual poly(vinyl acetate) content.

[0005]

[0005] Conventional multi-layer interlayers, such as three-ply acoustical interlayers, contain a soft core layer of a single poly(vinyl butyral) ("PVB") resin with low residual hydroxyl content and high amounts of conventional plasticizers, and two stiff skin layers with significantly higher residual hydroxyl content (see, for example, U.S. Pat. Nos. 5,340,654, 5,190,826, and 7,510,771). Interlayers having the reverse configuration, i.e., one stiff layer sandwiched between two softer layers, have been found to improve the impact performance of glass panels and can also be designed for acoustical properties.

[0006]

[0006] The following briefly describes how multi-layer glass panels are generally produced in combination with these interlayers. First, at least one polymer interlayer sheet (single or multi-layer) is placed between two substrates, and any excess interlayer is trimmed from the edges to create an assembly. It is not uncommon for multiple polymer interlayer sheets, or a polymer interlayer sheet with multiple layers (or a combination of both) to be placed within the two substrates to create a multi-layer glass panel with multiple polymer interlayers. Air is then removed from the assembly by an applicable process or method known to those skilled in the art, for example, by nip rollers, vacuum bags, or another degassing mechanism. In addition, the interlayer is partially pressed to the substrate by any method known to those skilled in the art. In the final step, this preliminary adhesion is made more permanent by a high temperature and high pressure lamination process, or any other method known to those skilled in the art, such as, but not limited to, an autoclave process, to form the final unitary structure.

[0007]

[0007] The cut-off pieces or substandard homogeneous poly(vinyl butyral) sheet products can be reused in the sheet manufacturing process. After grinding, the chips or flakes can be added back into the feedstock of the extrusion process. The PVB raw material can also be taken back from the laminated glass after it has served its purpose in practical application. See US Patent Application No. 2009 / 0209667. However, when applying such practice to multilayer sheets, re-extrusion will cause certain visual defects due to the presence of the core layer. Due to the difference in poly(vinyl butyral) composition between the PVB compounds in the skin and core layers, these materials do not mix well in the melt phase. This causes a certain type of visible haze in laminated glass containing PVB sheets where small pieces of multilayer sheets are used in the raw material feed, which makes the product of poor visual quality not suitable for sale in the market.

[0008]

[0008] Recycling poly(vinyl butyral) multilayer sheets from substandard finished sheet products that cannot be reused, and from laminated glass that has fulfilled its primary function and is about to be discarded, can be an economical and environmental step forward. Compared to producing virgin poly(vinyl butyral) resin, recycling finished sheet products is less costly, and also reduces the environmental footprint of poly(vinyl butyral) resin and sheet production. Thus, maximizing scrap reuse is not only a competitive advantage, but also an environmentally sound practice.

[0009]

[0009] US Patent Application Publication No. 2003 / 0191202 discloses a method for separating target polymers and their additives from a polymer-containing material, which allows the recovery of both the target polymer and the additives. Based on the principle of selective precipitation, the target polymer is precipitated and subsequently separated from the additives present in the solution and dissolved foreign polymers. Separation of the additives from the solution is carried out in a further step.

[0010]

[0010] US Patent Application Publication No. US2009 / 0209667 discloses a method for recycling poly(vinyl butyral) resin and incorporating the poly(vinyl butyral) resin into laminated glass and other articles. The poly(vinyl butyral) resin is recovered from waste laminated glass by a well-defined process, which includes the steps of granulating the laminated glass, solvent extraction of plasticizers and impurities, dissolving the poly(vinyl butyral), pre-filtration of insoluble contaminants, color removal by adsorption or bleaching, post-filtration of carbon particles, precipitation of poly(vinyl butyral), and washing, stabilizing, and drying the poly(vinyl butyral) resin. In one embodiment, a method is disclosed for separating two poly(vinyl butyral) resins from a single batch of granules. For this embodiment, a solvent is chosen for the dissolving step that selectively dissolves the first poly(vinyl butyral) resin but not the second poly(vinyl butyral) resin at a suitable temperature.

[0011]

[0011] There remains a need for a method to recycle PVB scrap materials. Summary of the Invention

[0012] In one aspect, the present invention relates to a method for recovering stiff poly(vinyl butyral) from a plasticized poly(vinyl butyral) multilayer sheet containing stiff poly(vinyl butyral) and soft poly(vinyl butyral). According to one aspect of the invention, the method will include the step of grinding the plasticized poly(vinyl butyral) multilayer sheet to obtain poly(vinyl butyral) granules. Additional plasticizer may be added to the granules to remove at least a portion of the soft poly(vinyl butyral) from the poly(vinyl butyral) granules, such that the granules are enriched in stiff poly(vinyl butyral). According to a further aspect, the granules enriched in stiff poly(vinyl butyral) may be separated from the soft poly(vinyl butyral) and the additional plasticizer, for example, using one or more techniques selected from decantation, filtration, or centrifugation, leaving a varnish containing the soft poly(vinyl butyral) and the additional plasticizer.

[0013]

[0013] In one aspect, the method of the present invention may further include one or more steps of adding a further additional plasticizer to the granules to remove the further portion of the soft poly(vinyl butyral) from the granules, and then separating the granules from the further additional portion of the soft poly(vinyl butyral) and the further additional plasticizer using one or more techniques selected from decantation, filtration, or centrifugation to leave a varnish containing the further additional portion of the soft poly(vinyl butyral) and the further additional plasticizer.

[0014] In accordance with a further aspect of the invention, the resulting varnish is used to produce a poly(vinyl butyral) interlayer.

[0015]

[0015] Further aspects of the invention are disclosed and claimed herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016]

[0016] Thus, in one aspect, the present invention relates to a method for recovering stiff poly(vinyl butyral) from a plasticized poly(vinyl butyral) multi-layer sheet containing stiff poly(vinyl butyral) and soft poly(vinyl butyral). According to the present invention, the method may include the step of grinding the plasticized poly(vinyl butyral) multi-layer sheet to obtain poly(vinyl butyral) granules. The granules may be in the form of, but are not limited to, flakes or chips.

[0017]

[0017] The invention may further comprise adding additional plasticizer to the poly(vinyl butyral) granules and washing or removing at least a portion of the soft poly(vinyl butyral) from the poly(vinyl butyral) granules so that the granules are enriched in stiff poly(vinyl butyral). The stiff poly(vinyl butyral) enriched granules are thus in a solid form, facilitating separation of the granules from the resulting soft poly(vinyl butyral) and additional plasticizer. The invention therefore also comprises separating the stiff poly(vinyl butyral) enriched granules from the soft poly(vinyl butyral) and additional plasticizer, described herein as varnish, using, for example, one or more techniques selected from decantation, filtration, or centrifugation.

[0018] In a further aspect, the invention may further comprise one or more additional steps of adding a further additional plasticizer to the granules to remove a further portion of the soft poly(vinyl butyral) from the granules, and then separating the granules from the further portion of the soft poly(vinyl butyral) and the further additional plasticizer varnish using one or more techniques selected from decantation, filtration, or centrifugation. In each of the steps according to the invention, the additional plasticizer used may be the same as or different from the plasticizer present in the plasticized poly(vinyl butyral) multilayer sheet.

[0019]

[0019] Thus, as used herein, the term "varnish" is used to describe the resulting soft poly(vinyl butyral) and additional plasticizer when the granules are enriched with stiff poly(vinyl butyral) granules through the use of plasticizer.

[0020] Surprisingly, it has been discovered that plasticizers, such as those typically used to plasticize PVB, can be used to selectively wash out a portion of the soft poly(vinyl butyral) from a granulated poly(vinyl butyral) mixture to yield stiff poly(vinyl butyral) enriched granules and a varnish which can be used to produce poly(vinyl butyral) interlayers.

[0021] In one embodiment, according to any of the preceding embodiments, the soft poly(vinyl butyral) may have a residual hydroxyl content of about 8% to about 12%. In yet another embodiment, the stiff poly(vinyl butyral) may have a residual hydroxyl content of about 15% to about 25%.

[0022] In a further embodiment, the plasticized poly(vinyl butyral) multilayer sheet according to any of the preceding embodiments may include triethylene glycol bis(2-ethylhexanoate) present as a plasticizer.

[0023]

[0023] In yet another aspect, according to any of the preceding aspects, the plasticized poly(vinyl butyral) multilayer sheet may further comprise another advantageous substance, such as dihexyl adipate, or bis(2-ethylhexyl) adipate, or Benzoflex 9-88 benzoate, present as a plasticizer.

[0024]

[0024] In another embodiment, according to any of the preceding embodiments, the additional plasticizer is selected from one or more of esters of polybasic acids or polyhydric alcohols. In a further embodiment, the additional plasticizer may be selected from one or more of triethylene glycol bis(2-ethylhexanoate), tetraethylene glycol bis(2-ethylhexanoate), triethylene glycol bis(2-ethylbutyrate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, bis(2-ethylhexyl)adipate, bis(2-ethoxyethyl)adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, adipic acid polymer, soybean oil, or epoxidized soybean oil.

[0025] In one embodiment, according to any of the preceding embodiments, triethylene glycol bis(2-ethylhexanoate) is present in the flexible poly(vinyl butyral) in an amount of about 60 phr to about 100 phr. In another embodiment, the additional plasticizer added to the poly(vinyl butyral) granules in step b) comprises triethylene glycol bis(2-ethylhexanoate).

[0026] In a further embodiment, according to any of the preceding embodiments, the difference between the residual hydroxyl content of the soft poly(vinyl butyral) and the residual hydroxyl content of the stiff poly(vinyl butyral) is at least 4.0 weight percent.

[0027] In yet another embodiment, the stiff poly(vinyl butyral) contained in the plasticized poly(vinyl butyral) multilayer sheet according to any of the preceding embodiments comprises from about 30 phr to about 45 phr of a plasticizer.

[0028] In one aspect, according to any of the preceding aspects, the soft poly(vinyl butyral) may be isolated from the mixture of soft poly(vinyl butyral) and additional plasticizer resulting from step b) by one or more of sedimentation, filtration, centrifugation, evaporation, or precipitation to isolate the soft poly(vinyl butyral). In another aspect, the invention relates to a poly(vinyl butyral) sheet comprising the isolated soft poly(vinyl butyral), and a laminated glass comprising the poly(vinyl butyral) sheet.

[0029]

[0029] In a further aspect, the resulting varnish of soft poly(vinyl butyral) and plasticizer, according to any of the preceding aspects, may be used directly, optionally with removal of water, to produce a poly(vinyl butyral) sheet or interlayer comprising the varnish, without first isolating the soft poly(vinyl butyral) from the plasticizer.

[0030] In yet another aspect, according to any of the preceding aspects, the invention relates to poly(vinyl butyral) sheets comprising the separated, rigid, poly(vinyl butyral)-enriched particulates recovered according to the method of the invention. In yet another aspect, the invention relates to laminated glass comprising these poly(vinyl butyral) sheets comprising the rigid, poly(vinyl butyral)-enriched particulates.

[0031]

[0031] In yet another aspect, according to any of the preceding aspects, the method may further include a step of subjecting the varnish of the soft poly(vinyl butyral) and additional plasticizer to one or more of precipitation, filtration, centrifugation, evaporation, or precipitation to isolate the soft poly(vinyl butyral).

[0032] In a further aspect, according to any of the preceding aspects, the method may further comprise the step of adding a varnish of soft poly(vinyl butyral) and additional plasticizer to the poly(vinyl butyral) composition.

[0033]

[0033] In still a further aspect, the method according to any of the preceding aspects may further comprise forming the poly(vinyl butyral) composition into a sheet.

[0034]

[0034] In another aspect, according to any of the preceding aspects, the method may further include the step of adding a varnish of soft poly(vinyl butyral) and additional plasticizer to the poly(vinyl butyral) composition containing a whitening agent to form a translucent intermediate layer.

[0035] In yet another aspect, according to any of the preceding aspects, the method may further include the step of adding a varnish of soft poly(vinyl butyral) and additional plasticizer to the clear poly(vinyl butyral) formulation.

[0036]

[0036] In yet another aspect, according to any of the preceding aspects, the invention relates to a poly(vinyl butyral) sheet comprising an isolated flexible poly(vinyl butyral) according to any of the preceding aspects, and in yet another aspect, the invention relates to a laminated glass comprising a poly(vinyl butyral) sheet according to any of the preceding aspects.

[0037] In yet another aspect, according to any of the preceding aspects, the invention may relate to a poly(vinyl butyral) sheet comprising the separated, stiff poly(vinyl butyral)-enriched particles of any of the preceding aspects.

[0038]

[0038] In yet another aspect, according to any of the preceding aspects, the invention may relate to a laminated glass comprising a poly(vinyl butyral) sheet of any of the preceding aspects.

[0039]

[0039] The term "rigid poly(vinyl butyral)" refers to a poly(vinyl butyral) resin, or blend of poly(vinyl butyral) resins, which is significantly stiffer than a "soft poly(vinyl butyral)" as further described herein and which typically forms the skin or stiff layer of a multilayer poly(vinyl butyral) sheet.

[0040] The term "soft poly(vinyl butyral)" refers to a poly(vinyl butyral) resin, or blend of poly(vinyl butyral) resins, which is significantly softer than a "rigid poly(vinyl butyral)" as further described herein and which typically forms the core or soft layer of a multi-layer poly(vinyl butyral) multilayer sheet. The soft or core poly(vinyl butyral) layer is typically sandwiched between two stiff or skin poly(vinyl butyral) layers to form the multi-layer poly(vinyl butyral) multilayer sheet.

[0041]

[0041] The term "plasticizer" as used herein generally refers to a molecule or blend of molecules that plasticizes and thereby softens a polymer, specifically poly(vinyl butyral), at low plasticizer content, as further described herein. Additionally, the plasticizers that are useful as additional plasticizers according to the present invention, when present in higher amounts as additional plasticizers, aid in the removal of soft poly(vinyl butyral) from the granulated poly(vinyl butyral) mixture by selectively washing or partially dissolving the soft poly(vinyl butyral), due in part to the higher affinity or compatibility of the core layer for the plasticizer, as evidenced by its lower residual hydroxyl group content.

[0042] In some embodiments, the additional plasticizer has a hydrocarbon segment of less than 20, less than 15, less than 12, or less than 10 carbon atoms. Suitable additional plasticizers for use according to the invention include, among others, esters of polybasic acids or polyhydric alcohols. Suitable plasticizers include, for example, triethylene glycol bis(2-ethylhexanoate) ("3-GEH"), tetraethylene glycol bis(2-ethylhexanoate), triethylene glycol bis(2-ethylbutyrate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, bis(2-ethylhexyl) adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, adipic acid polymers, soybean oil, and epoxidized soybean oil, and mixtures thereof. A more preferred plasticizer is 3-GEH. Additionally, plasticizers that are compatible at high temperatures may be preferred to further increase the fluidity of the interlayer.

[0043]

[0043] The term "poly(vinyl butyral) multilayer sheet" as used herein refers to a sheet composed of various layers of poly(vinyl butyral) resin, the various layers being typically soft or core layers with stiff or skin layers on each side of the core layer. Thus, the poly(vinyl butyral) multilayer sheet of the present invention comprises at least one soft poly(vinyl butyral) and at least one stiff poly(vinyl butyral).

[0044] When it is said that the poly(vinyl butyral) multilayer sheet is ground to obtain a granulated poly(vinyl butyral) mixture, it means that the size is reduced by any suitable means, for example, a grinder, to obtain granules, chips, or flakes, etc., all of which may be considered as granules according to the present invention. In this granulation step, the granulation can be carried out using any suitable equipment, which may be, for example, a commercially available granulator, such as a Granutec granulator (East Douglas, Mass., USA). The scrap is granulated to reduce the particle size. The granulation of the scrap can result in individual granules having a length of less than 2.6 centimeters, or between 0.1 and 1.0 centimeters, or between 0.4 and 0.8 centimeters. While granules with a size of more than 2.6 centimeters can be used, it is generally desirable to granulate the sheet to a smaller size, which results in a larger granule total surface area. At any point during granulation, the granulated flakes can be sieved to remove contaminants that have been liberated from the poly(vinyl butyral).

[0045] When it is said that the additional plasticizer is added to the poly(vinyl butyral) granules, it means that the plasticizer added in this step is in addition to the plasticizer contained in the plasticized poly(vinyl butyral) multilayer sheet. In fact, both the soft poly(vinyl butyral) and the rigid poly(vinyl butyral) will already contain a plasticizer. The additional plasticizer may be the same plasticizer present in the soft poly(vinyl butyral) and / or the rigid poly(vinyl butyral), or it may be different from that present in the soft poly(vinyl butyral) and / or the rigid poly(vinyl butyral). The amount of additional plasticizer added is sufficient to assist in removing or washing at least a portion of the soft poly(vinyl butyral) from the poly(vinyl butyral) granules to obtain a varnish of soft poly(vinyl butyral) and plasticizer.

[0046]

[0046] When it is said that at least a portion of the soft poly(vinyl butyral) is removed from the poly(vinyl butyral) granules, it is meant that a portion of the soft poly(vinyl butyral) is washed or dissolved from the granules. The granules may then be separated from the soft poly(vinyl butyral) and additional plasticizer according to one or more of the following techniques, decantation, filtration, or centrifugation, as further described herein. Alternatively, the varnish may be used directly to form a poly(vinyl butyral) layer or sheet, or, optionally, a portion of the additional plasticizer and / or water may be separated from the varnish prior to the formation of a poly(vinyl butyral) sheet or layer from the varnish.

[0047] When we say that the granules are enriched in stiff poly(vinyl butyral), we mean that the relative amount of stiff poly(vinyl butyral) in the granules is higher than it was before some of the soft poly(vinyl butyral) was washed from the granules.

[0048] In one embodiment, the soft or core poly(vinyl butyral), or blends of soft poly(vinyl butyrals), may have a residual hydroxyl content of about 5% to about 15%, as further described herein. Alternatively, the residual hydroxyl content of the core poly(vinyl butyral) may be about 7% to about 13, or 8% to 12%, or as further described herein.

[0049] In one embodiment, the soft or core poly(vinyl butyral), or blends of soft poly(vinyl butyral), as further described herein, may have a residual acetate content of about 0% to about 18%. Alternatively, the residual acetate content may be less than 10%, or less than 5%, or less than 2%, or less than 1%, or as further described herein.

[0050] The amount of plasticizer in the flexible or core poly(vinyl butyral), or in a blend of flexible poly(vinyl butyrals), may be from about 50 phr to about 150 phr, or from 55 phr to 120 phr, or from 60 to 100 phr.

[0051] In another embodiment, the rigid poly(vinyl butyral), or blend of rigid poly(vinyl butyral), may have a residual hydroxyl content of about 12% to about 28%, as further described herein. Alternatively, the residual hydroxyl content of the rigid poly(vinyl butyral) may be about 15% to about 25%, or 18% to 20%, or as further described herein.

[0052] In another embodiment, the rigid poly(vinyl butyral), or blends of rigid poly(vinyl butyral), as further described herein, may have a residual acetate content of from about 0% to about 18%. Alternatively, the residual acetate content of the rigid poly(vinyl butyral) may be less than 10%, or less than 5%, or less than 2%, or less than 1%, or as further described herein.

[0053] In other embodiments, the residual hydroxyl content of the core layer can be the same as, greater than, or less than the residual hydroxyl content of the resin in the skin layers. In various embodiments, the core resin, or the skin resin, or both of these resins, may contain less than 30 wt.% residual ester groups, less than 25 wt.%, less than 20 wt.%, less than 15 wt.%, less than 13 wt.%, less than 10 wt.%, less than 7 wt.%, less than 5 wt.%, or less than 1 wt.% residual ester groups, calculated as polyvinyl esters, for example acetate esters, with the remainder being acetals such as butyraldehyde acetal, but optionally isobutyraldehyde acetal groups, 2-ethylhexanal acetal groups, or a mixture of any two of butyraldehyde acetal, isobutyraldehyde acetal, and 2-ethylhexanal acetal groups, or other acetal groups such as those discussed elsewhere herein.

[0054] In one embodiment, the multi-layered intermediate layer may include a first skin polymer layer comprising a plasticized poly(vinyl butyral) having a molecular weight less than about 140,000 Daltons, a second core polymer layer comprising a plasticized poly(vinyl butyral) having a molecular weight greater than about 140,000 Daltons, and a third skin polymer layer comprising a plasticized poly(vinyl butyral) having a molecular weight less than about 140,000 Daltons. The second polymer layer is disposed between the first and third polymer layers, providing two skin layers and a central core layer.

[0055] In various embodiments of the interlayer of the present disclosure, the interlayer may include about 30 to about 60 phr (parts per hundred parts of resin) of total plasticizer. While the total plasticizer content is shown above, the plasticizer content in the skin or core layers may differ from the total plasticizer content. In addition, the skin and core layers may have different plasticizer contents since the plasticizer content of each respective layer at equilibrium is determined, at least in part, by its respective residual hydroxyl group content. For example, if, at equilibrium, the combined thickness of the skin layers is equal to that of the core layer, the interlayer may include two skin layers, each having 38 phr of plasticizer, and a core layer having 75 phr of plasticizer, for a total plasticizer amount of the interlayer of about 54.3 phr. For thicker or thinner skin layers, the total plasticizer amount for the interlayer may vary accordingly.

[0056] In other embodiments, the amount of plasticizer in the blend of stiff or skin poly(vinyl butyral), or soft poly(vinyl butyral), may be from about 20 phr to about 60 phr, or from 25 phr to 50 phr, or from 30 to 45 phr.

[0057]

[0057] In further embodiments, the difference between the residual hydroxyl content of the soft poly(vinyl butyral) and the rigid poly(vinyl butyral) is at least 6%, or at least 5%, or at least 4%, or from 4% to 8%, or from 5% to 10%, or as further described herein.

[0058]

[0058] Thus, in various embodiments, the residual hydroxyl group content of the poly(vinyl butyral) resins for the skin and core layers may vary. The resin for the core layer may contain, for example, about 9 to about 18 weight percent (wt.%) residual hydroxyl groups, calculated as PVOH, about 9 to about 16 wt.% residual hydroxyl groups, calculated as PVOH, or about 9 to about 14 wt.% residual hydroxyl groups, calculated as PVOH. The resin for the skin layer may contain, for example, about 13 to about 35 weight percent (wt.%) residual hydroxyl groups, calculated as PVOH, about 13 to about 30 wt.% residual hydroxyl groups, calculated as PVOH, or about 15 to about 22 wt.% residual hydroxyl groups, calculated as PVOH, and for certain embodiments, about 17.25 to about 22.25 wt. residual hydroxyl groups, calculated as PVOH, or as described elsewhere herein. The resin for the core layer, or for the skin layer, or for both the skin layer and the core layer may also contain less than 20 wt.%, less than 15 wt.%, less than 13 wt.%, less than 11 wt.%, less than 9 wt.%, less than 7 wt.%, less than 5 wt.%, or less than 1 wt.% residual ester groups, calculated as polyvinyl esters, e.g., acetate esters, the remainder being acetals, preferably butyraldehyde acetals, but optionally containing small amounts of other acetal groups, e.g., 2-ethylhexanal groups (see, e.g., U.S. Pat. No. 5,137,954, the entire disclosure of which is incorporated herein by reference).

[0059] In one embodiment, the flexible poly(vinyl butyral), rigid poly(vinyl butyral), and / or plasticized poly(vinyl butyral) multilayer sheets, or any other poly(vinyl butyral) described herein, can be any of the following: dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate, isodecyl benzoate, 2-ethylhexyl benzoate, diethylene glycol benzoate, butoxyethyl benzoate, butoxyethyoxyethyl benzoate, butoxyethoxyethoxyethyl benzoate, propylene glycol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol dibenzoate, In some embodiments, the plasticizer may include a plasticizer selected from one or more of the following: 2,2,4-trimethyl-1,3-pentanediol benzoate isobutyrate, 1,3-butanediol dibenzoate, diethylene glycol di-o-toluate, triethylene glycol di-o-toluate, dipropylene glycol di-o-toluate, 1,2-octyl dibenzoate, tri-2-ethylhexyl trimellitate, di-2-ethylhexyl terephthalate, bis-phenol A bis(2-ethylhexanoate), di-(butoxyethyl) terephthalate, di-(butoxyethyoxyethyl) terephthalate, bis(2-ethoxyethyl) adipate, or those further described herein.

[0060] In various embodiments, the additional plasticizers added are dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate, isodecyl benzoate, 2-ethylhexyl benzoate, diethylene glycol benzoate, butoxyethyl benzoate, butoxyethyoxyethyl benzoate, butoxyethoxyethoxyethyl benzoate, propylene glycol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol benzoate isobutyrate, 1,3-butanediol dibenzoate ... The plasticizer may comprise one or more of benzoate, diethylene glycol di-o-toluate, triethylene glycol di-o-toluate, dipropylene glycol di-o-toluate, 1,2-octyl dibenzoate, tri-2-ethylhexyl trimellitate, di-2-ethylhexyl terephthalate, bisphenol A bis(2-ethylhexanoate), di-(butoxyethyl) terephthalate, di-(butoxyethyoxyethyl) terephthalate, or as further described herein, which may be the same as or different from the plasticizer in the poly(vinyl butyral) just described, as further described herein. Additional plasticizers or further plasticizers suitable as plasticizers in the soft poly(vinyl butyral) are described elsewhere herein.

[0061] As noted above, the poly(vinyl butyral) multilayer sheets of the present invention typically include a stiff poly(vinyl butyral) layer and a soft poly(vinyl butyral) layer. As noted above, the core layer typically includes a soft poly(vinyl butyral) layer sandwiched between stiff poly(vinyl butyral) skin layers to form the poly(vinyl butyral) multilayer sheets of the present invention.

[0062] In one embodiment, the amount of additional plasticizer added to the poly(vinyl butyral) granules is sufficient to wash, extract, or selectively dissolve a portion of the soft poly(vinyl butyral).

[0063]

[0063] In another embodiment, the amount of additional plasticizer added to the poly(vinyl butyral) granules is sufficient to suspend the rigid poly(vinyl butyral) granules of the mixture, thus forming a rigid poly(vinyl butyral) suspension.

[0064] In yet another embodiment, the additional plasticizer is added to the poly(vinyl butyral) granules in a continuous process, for example to form a countercurrent process, removing at least a portion of the soft poly(vinyl butyral) from the poly(vinyl butyral) granules so that the granules become enriched in the stiff poly(vinyl butyral). The granules may then be separated from the resulting varnish mixture of the soft poly(vinyl butyral) and the additional plasticizer, or the varnish may be used without separating the additional plasticizer from the soft poly(vinyl butyral), or with only partial separation of the additional plasticizer from the soft poly(vinyl butyral), or with separation of only the water from the mixture.

[0065] In a further aspect of the invention, the method may include a further step, after the physical separation step, of subjecting the soft poly(vinyl butyral) from the resulting mixture of soft poly(vinyl butyral) and additional plasticizer to one or more of sedimentation, filtration, centrifugation, evaporation, or precipitation to isolate the soft poly(vinyl butyral).

[0066] In a further aspect, the present invention relates to poly(vinyl butyral) sheets comprising isolated rigid poly(vinyl butyral), and laminated glass comprising these poly(vinyl butyral) sheets.

[0067]

[0067] In a further aspect, the present invention relates to poly(vinyl butyral) sheets comprising flexible poly(vinyl butyral), whether or not the flexible poly(vinyl butyral) is first isolated from plasticizers, and laminated glass comprising these poly(vinyl butyral) sheets.

[0068] When we say that the rigid poly(vinyl butyral) is separated from the poly(vinyl butyral) mixture by decantation or settling, we mean that the liquid is separated from the rigid poly(vinyl butyral) solids, for example, by allowing the solids to settle to the bottom of a container to remove the bulk of the additional plasticizer from the granules.

[0069] When it is said that the rigid poly(vinyl butyral) is separated by filtration, it is meant that the particulate rigid poly(vinyl butyral) solids are filtered from the plasticizer.

[0070] When we say that the stiff poly(vinyl butyral) is separated from a mixture by centrifugation, we mean that the solids are separated from the liquid using a centrifuge.

[0071]

[0071] The present invention may be further understood in accordance with the further description that follows.

[0072]

[0072] Thus, in one aspect, the multi-layered poly(vinyl butyral) sheets of the present invention may include an interlayer comprising one or more stiff skin layers and a soft core layer. In one embodiment, these multi-layered interlayer sheets may include a first polymer layer (skin layer) comprising a stiff plasticized poly(vinyl butyral) resin, a second polymer layer (core layer) comprising a soft plasticized poly(vinyl butyral) resin or a blend thereof having the same or different residual hydroxyl group content, and optionally a third polymer layer (skin layer) comprising a stiff plasticized poly(vinyl butyral) resin. The second or core polymer layer is disposed adjacent to the first polymer layer. If there are three or more layers, the second polymer layer may be disposed between the first and third polymer layers, resulting in two skin layers and a central core layer.

[0073] In embodiments, the second or core poly(vinyl butyral) resin may be present in an amount from about 2 weight percent to about 45 weight percent, or from about 5 weight percent to about 40 weight percent.

[0074] Plasticizers work by embedding themselves between polymer chains, spacing them apart (increasing the "free volume"), thus significantly lowering the glass transition temperature (Tg) of the polymer resin (typically by 0.5-4 degrees Celsius / phr), making the material softer. In this regard, the amount of plasticizer in the interlayer can be adjusted to affect the glass transition temperature (Tg). The glass transition temperature (Tg) is the temperature that marks the transition of the interlayer from a glassy state to a rubbery state. Generally, the higher the plasticizer loading, the lower the Tg. Conventional interlayers have generally had Tg's in the range of about 0° C. for acoustical (noise suppression) interlayers to about 45° C. for hurricane and aircraft interlayer applications.

[0075]

[0075] The glass transition temperature of the interlayer also correlates with the stiffness of the interlayer; the higher the glass transition temperature, the stiffer the interlayer. Generally, an interlayer having a glass transition temperature of about 30°C or higher increases windshield strength and torsional rigidity. On the other hand, a soft interlayer (generally characterized by an interlayer having a glass transition temperature less than about 30°C) contributes to sound attenuation effects (i.e., acoustic properties). The multilayer interlayer of the present disclosure combines these two advantageous properties (i.e., strength and acoustics) by utilizing harder or stiffer skin layers (e.g., stiff / soft / stiff) laminated with a softer core layer, the skin layers having increased flowability at autoclave temperatures. In various embodiments, the multilayer interlayer generally includes skin layers having a glass transition temperature of about 30°C to about 55°C, and a core layer having a glass transition temperature of about 0°C to about 10°C.

[0076] In an embodiment, the plasticizer used herein is selected from the group consisting of dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate, isodecyl benzoate, 2-ethylhexyl benzoate, diethylene glycol benzoate, butoxyethyl benzoate, butoxyethyoxyethyl benzoate, butoxyethoxyethoxyethyl benzoate, propylene glycol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol Benzoate isobutyrate, 1,3-butanediol dibenzoate, diethylene glycol di-o-toluate, triethylene glycol di-o-toluate, dipropylene glycol di-o-toluate, 1,2-octyl dibenzoate, tri-2-ethylhexyl trimellitate, di-2-ethylhexyl terephthalate, bisphenol A bis(2-ethylhexanoate), di-(butoxyethyl) terephthalate, di-(butoxyethyoxyethyl) terephthalate, and mixtures thereof, or as described elsewhere herein. In embodiments, the plasticizer may be a mixture of two or more plasticizers. In embodiments, the intermediate layer may further comprise a second high refractive index plasticizer having a refractive index of at least 1.460. In other embodiments, the intermediate layer may further comprise a plasticizer having a refractive index of less than about 1.450.

[0077] In embodiments, the percent haze may be less than 0.5% (measured by ASTM D1003-61 (Re-approved 1977)-Procedure A using Illuminant C at a 2 degree observation angle).

[0078] In an embodiment, the residual hydroxyl content of the third or rigid poly(vinyl butyral resin) is typically the same as the residual hydroxyl content of the first rigid poly(vinyl butyral resin) and typically differs from that in the second or core poly(vinyl butyral resin). In an embodiment, the difference between the core residual hydroxyl content and the skin residual hydroxyl content is at least 4.0 weight percent, or at least 6.0 weight percent.

[0079] In embodiments, the second poly(vinyl butyral) resin is present in an amount from about 2 weight percent to about 45 weight percent, or from about 5 weight percent to about 40 weight percent.

[0080] In embodiments, the polymer interlayer has at least two different glass transition temperatures (T g ) and have at least two different glass transition temperatures (T g ) is at least 5°C.

[0081] In an embodiment, the residual hydroxyl content of the third or skin poly(vinyl butyral resin) is the same as the residual hydroxyl content of the first or core poly(vinyl butyral) resin.

[0082]

[0082] A multilayer panel is also disclosed. The multilayer panel includes at least one rigid substrate and a polymer interlayer or a multilayer polymer interlayer as disclosed herein. The panel has improved optical properties.

[0083] In one embodiment of the present invention, a single plasticizer such as triethylene glycol bis(2-ethylhexanoate) or a mixture thereof with dihexyl adipate may be used.

[0084]

[0084] Thus, the present invention relates to a method for preferentially removing, washing, or partially dissolving soft poly(vinyl butyral) resin from poly(vinyl butyral) granules using a plasticizer as an extractant, by exploiting the differential solubility of the PVB component in the plasticizer. This is distinct from the use of traditional solvents. Thus, the present invention provides a method for recovering raw material for reintroduction into the manufacturing process, optionally without first isolating the soft poly(vinyl butyral) resin from the plasticizer.

[0085]

[0085] Because of the differences in cloud points of PVB resins of different compositions, specifically as measured by the residual % PVOH in the plasticizer, the technique allows the use of temperature as an important parameter for the effective separation of the different PVB components. In this regard, the additional plasticizer may be added to the poly(vinyl butyral) granules at a temperature of at least 25°, or at least 30°C, or from about 25°C to about 90°C, or from 30°C to about 60°C, or as disclosed elsewhere herein.

[0086]

[0086] The present invention also describes a method for removing the extracted PVB resin from the plasticizer extract to allow repeated use of the plasticizer in a recycling process.

[0087]

[0087] Thus, the present invention describes a method for removing the extracted poly(vinyl butyral) from the plasticizer to allow repeated use of the solvent in the extraction. The poly(vinyl butyral) compound isolated from the multilayer poly(vinyl butyral) sheet with an acceptable purity for reuse is the result of a method that includes a step described in the present invention as fractionation, extraction, or selective dissolution. In this context, fractionation, extraction, or selective dissolution means that primarily the soft poly(vinyl butyral) is removed or washed from the poly(vinyl butyral) granules, while the stiff poly(vinyl butyral) resin remains primarily in the poly(vinyl butyral) granules as a solid in the solvent, possibly in a swollen state.

[0088]

[0088] Poly(vinyl butyral) compounds are components of multi-layer poly(vinyl butyral) sheets, with each layer being composed of poly(vinyl butyral) and plasticizer having a different composition with respect to the poly(vinyl butyral) composition, i.e., different residual hydroxyl or acetate content, and plasticizer content. Generally, the amount of plasticizer relative to the amount of poly(vinyl butyral) is different. Significant extraction of poly(vinyl butyral) compounds from multi-layer sheet granules is typically obtained after crushing substandard sheets into smaller flakes, generally in the size range of 3-30 mm.

[0089] The degree of separation depends on the plasticizer applied, for example, extraction of the core layer PVB from a poly(vinyl butyral) multilayer sheet using triethylene glycol bis(2-ethylhexanoate) proceeds to such an extent that 25-50% of the core layer PVB is removed in a single fractionation step. Repeated extractions will increase the degree of separation between the different poly(vinyl butyral) compounds. Typically, extraction is obtained when the multilayer sheet or parts thereof are exposed to specific solvents in the temperature range between 25 and 100° C., with extraction times for one extraction cycle ranging from 5 minutes to several days.

[0090]

[0090] Conventional multi-layer interlayers, such as three-ply acoustical interlayers, typically contain a soft core layer consisting of a single poly(vinyl butyral) ("PVB") resin with low residual hydroxyl content and a high amount of conventional plasticizers, and two stiff skin layers with significantly higher residual hydroxyl content (see, for example, U.S. Pat. Nos. 5,340,654, 5,190,826, and 7,510,771). Thus, isolated soft poly(vinyl butyral) may be recycled to form the core layer of a three-ply acoustical interlayer, or a varnish of soft poly(vinyl butyral) and plasticizer may be used directly to form the soft poly(vinyl butyral) layer without first separating the two. The residual hydroxyl content and amount of plasticizer in the PVB core resin are optimized so that the interlayer provides optimal acoustic properties for multi-ply glass panels, such as windshields and windows installed in vehicles and buildings, under ambient conditions.

[0091]

[0091] As used herein, the terms "polymer interlayer sheet," "interlayer," and "polymer melt sheet" may generally refer to a single layer sheet or a multilayer interlayer. A "single layer sheet," as the name suggests, is a single polymer layer extruded as one layer. A multilayer interlayer sheet, on the other hand, may include multiple layers, including separately extruded layers, coextruded layers, or any combination of separately extruded layers and coextruded layers. Thus, a multilayer interlayer sheet may include, for example, two or more single layer sheets combined ("multilayer sheet"), two or more layers coextruded together ("coextruded sheet"), two or more coextruded sheets combined, a combination of at least one single layer sheet and at least one coextruded sheet, a combination of a single layer sheet and a multilayer sheet, and a combination of at least one multilayer sheet and at least one coextruded sheet. In various embodiments of the present disclosure, a multi-layered interlayer sheet comprises at least two polymer layers (e.g., single or multiple layers coextruded and / or laminated together) disposed in direct contact with one another, where each layer comprises a polymer resin, as more fully detailed below. As used herein for multi-layered interlayers having at least three layers, "skin layer" generally refers to the outer layer of the interlayer, and "core layer" generally refers to the inner layer. Thus, one exemplary embodiment would be skin layer / / core layer / / skin layer.

[0092]

[0092] PVB resins are produced by the known acetalization process by reacting polyvinyl alcohol ("PVOH") with butyraldehyde in the presence of an acid catalyst, isolating, stabilizing, and drying the resin. Such acetalization processes are disclosed, for example, in U.S. Patent Nos. 2,282,057 and 2,282,026, and in Vinyl Acetal Polymers, in Encyclopedia of Polymer Science & Technology, 3rd edition, Volume 8, pp. 381-399 (2003) by BEWade, the entire disclosures of which are incorporated herein by reference. The resins are commercially available in various forms, for example, as Butvar® resins from Solutia Inc., a wholly owned subsidiary of Eastman Chemical Company.

[0093]

[0093] As used herein, residual hydroxyl content in PVB (calculated as % vinyl alcohol or % PVOH by weight) refers to the amount of hydroxyl groups remaining on the polymer chain after the process is completed. For example, PVB can be produced by hydrolyzing poly(vinyl acetate) to poly(vinyl alcohol (PVOH) and then reacting the PVOH with butyraldehyde. In the process of hydrolyzing poly(vinyl acetate), typically not all of the acetate pendant groups are converted to hydroxyl groups. Furthermore, the reaction with butyraldehyde typically does not result in all of the hydroxyl groups being converted to acetal groups. As a result, in any final PVB resin, there will typically be residual acetate groups (as vinyl acetate groups), and residual hydroxyl groups (as vinyl hydroxyl groups) present as pendant groups on the polymer chain. As used herein, residual hydroxyl group content and residual acetate content are measured on a weight percent (wt.%) basis according to ASTM D1396.

[0094]

[0094] The PVB resins of the present disclosure typically have a molecular weight of greater than 50,000, or less than 500,000, or from about 50,000 to about 500,000 daltons, or from about 70,000 to about 500,000 daltons, or from about 100,000 to about 425,000 daltons, as measured by size exclusion chromatography using low angle laser light scattering. As used herein, the term "molecular weight" refers to weight average molecular weight.

[0095]

[0095] Various adhesion control agents ("ACAs") can be used in the interlayer of the present disclosure to control adhesion of the interlayer sheet to glass. In various embodiments of the interlayer of the present disclosure, the interlayer can include from about 0.003 to about 0.15 parts ACA per 100 parts resin, from about 0.01 to about 0.10 parts ACA per 100 parts resin, and from about 0.01 to about 0.04 parts ACA per 100 parts resin. Such ACAs include, but are not limited to, ACAs disclosed in U.S. Patent No. 5,728,472, the entire disclosure of which is incorporated herein by reference, residual sodium acetate, potassium acetate, magnesium bis(2-ethylbutyrate), and / or magnesium bis(2-ethylhexanoate).

[0096]

[0096] Other additives may be added to the interlayer to enhance its performance in the final product and to impart certain additional properties to the interlayer, including, but not limited to, dyes, pigments, stabilizers (e.g., UV stabilizers), antioxidants, antiblocking agents, flame retardants, IR absorbers or blockers (e.g., indium tin oxide, antimony tin oxide, lanthanum hexaboride (LaB6), and cesium tungsten oxide), processing aids, flow additives, lubricants, impact modifiers, nucleating agents, heat stabilizers, UV absorbers, dispersants, surfactants, chelating agents, coupling agents, adhesives, primers, reinforcing additives, and fillers, among other additives known to those skilled in the art.

[0097]

[0097] The plasticizer or mixture of plasticizers in the skin and core layers are selected so that the multilayer acoustic interlayer exhibits acceptable levels of haze and visible transmission. In various embodiments, the plasticizer is selected from a high refractive index plasticizer, a mixture of two or more high refractive index plasticizers, or a mixture of a conventional plasticizer and a high refractive index plasticizer. In various embodiments, the high refractive index plasticizer is selected to eliminate possible strong haze resulting from blending two or more resins with different residual hydroxyl group content. In various embodiments of the present disclosure, the haze is less than 5%, less than 3%, and less than 1%, less than 0.3%.

[0098]

[0098] As used herein, plasticizers having a refractive index of about 1.450 or less are referred to as "conventional plasticizers". Conventional plasticizers include, but are not limited to, triethylene glycol bis(2-ethylhexanoate) ("3-GEH"), triethylene glycol bis(2-ethylbutyrate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, tetraethylene glycol bis(2-ethylhexanoate), dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, di(butoxyethyl)adipate, bis(2-butoxyethyl)adipate, and bis(2-(2-butoxyethoxy)ethyl)adipate, dibutyl sebacate, dioctyl sebacate, and mixtures thereof. These plasticizers have a refractive index of about 1.442 to about 1.449. In comparison, PVB resins have a refractive index of approximately 1.485 to 1.495. 3-GEH (refractive index = 1.442) is the most common plasticizer present in interlayers manufactured for a variety of properties and applications.

[0099] In various embodiments, for both the core and the skin layers, the high refractive index plasticizer is selected such that the refractive index of the plasticizer is at least about 1.460, or greater than about 1.460, or greater than about 1.470, or greater than about 1.480, or greater than about 1.490, or greater than about 1.500, or greater than 1.510, or greater than 1.520. As used herein, a "high refractive index plasticizer" is a plasticizer having a refractive index of at least about 1.460. In some embodiments, the high refractive index plasticizer is used in conjunction with a conventional plasticizer, and in some embodiments, when included, the conventional plasticizer is triethylene glycol di-(2-ethylhexanoate) ("3-GEH"), and the refractive index of the plasticizer mixture is at least 1.460. As used herein, the refractive index (also known as the index of refraction) of a plasticizer or resin used throughout this disclosure is either measured according to ASTM D542 at a wavelength of 589 nm and 25° C., or is reported in the literature according to ASTM D542.

[0100]

[0100] Examples of plasticizers having a high refractive index that may be used include, but are not limited to, polyadipates (RI of about 1.460 to about 1.485), epoxides (RI of about 1.460 to about 1.480), phthalates and terephthalates (RI of about 1.480 to about 1.540), benzoates (RI of about 1.480 to about 1.550), and other specialty plasticizers (RI of about 1.490 to about 1.520). Examples of high refractive index plasticizers include, but are not limited to, esters of polybasic acids or polyhydric alcohols, polyadipates, epoxides, phthalates, terephthalates, benzoates, toluates, mellitates, and other specialty plasticizers, among others. Examples of suitable high refractive index plasticizers include, but are not limited to, dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate, isodecyl benzoate, 2-ethylhexyl benzoate, diethylene glycol benzoate, propylene glycol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol benzoate isobutyrate, 1,3-butanediol dibenzoate, diethylene glycol di-o-toluate, triethylene glycol di-o-toluate, dipropylene glycol di-o-toluate, 1,2-octyl dibenzoate, tri-2-ethylhexyl trimellitate, di-2-ethylhexyl terephthalate, bisphenol A bis(2-ethylhexanoate), ethoxylated nonylphenol, and mixtures thereof.

[0101] In various embodiments of the interlayer of the present disclosure, the interlayer comprises a total plasticizer of more than 5 phr, about 5 to about 120 phr, about 10 to about 90 phr, about 20 to about 70 phr, about 30 to about 60 phr, or less than 120 phr, or less than 90 phr, or less than 60 phr, or less than 40 phr, or less than 30 phr. Although the total plasticizer content is shown above, the plasticizer content in the skin layer or core layer may differ from the total plasticizer content. In addition, as disclosed in U.S. Pat. No. 7,510,771 (the entire disclosure of which is incorporated herein by reference), the skin layer and the core layer may have different plasticizer types and plasticizer contents in the ranges discussed above, since the plasticizer content of each respective layer at equilibrium is determined by the respective residual hydroxyl group content of the layers. For example, in equilibrium, if the combined thickness of the skin layers is equal to that of the core layer, the intermediate layer may include two skin layers, each having 30 phr of plasticizer, and a core layer having 65 phr of plasticizer, for a total plasticizer amount for the intermediate layer of about 45.4 phr. For thicker or thinner skin layers, the total plasticizer amount for the intermediate layer will vary accordingly. In various embodiments of the present invention, the plasticizer content of the core layer and the skin layers differs by at least 8 phr, or at least 9 phr, or at least 10 phr, or at least 12 phr, or at least 13 phr, or at least 14 phr, or at least 15 phr, or at least 16 phr, or at least 17 phr, or at least 18 phr, or at least 19 phr, or at least 20 phr, or at least 25 phr or more. As used herein, the amount of plasticizer, or any other component in the intermediate layer, may be measured on a weight per weight basis as parts per hundred parts of resin (phr). For example, if 30 grams of plasticizer are added to 100 grams of polymer resin, then the plasticizer content of the resulting plasticized polymer will be 30 phr. As used herein, when the plasticizer content of an interlayer is given, the plasticizer content is determined based on the phr of plasticizer in the mix or melt used to produce the interlayer.

[0102]

[0102] The final intermediate layer, whether formed by extrusion or coextrusion, will generally have a randomly roughened topography as it is formed via melt fracture of the polymer melt as it exits the extrusion die, and may additionally be embossed over the randomly roughened surface on one or both sides (e.g., a skin layer) by any embossing method known to those skilled in the art.

[0103]

[0103] While all methods for the production of polymer interlayer sheets known to those skilled in the art are considered possible methods for producing the polymer interlayer sheets described herein, this application focuses on polymer interlayer sheets produced by extrusion and coextrusion processes. The final multi-ply glass panel laminates of the present invention are formed using lamination processes known in the art.

[0104]

[0104] Generally, the thickness or gauge of the polymeric interlayer sheet will range from about 15 mils to about 100 mils (about 0.38 mm to about 2.54 mm), about 15 mils to about 60 mils (about 0.38 mm to about 1.52 mm), about 20 mils to about 50 mils (about 0.51 mm to about 1.27 mm), and about 15 mils to about 35 mils (about 0.38 mm to about 0.89 mm). In various embodiments, each of the layers, such as the skin and core layers of the multilayer interlayer, may have a thickness of about 1 mil to about 99 mils (about 0.025 mm to about 2.51 mm), about 1 mil to about 59 mils (about 0.025 mm to about 1.50 mm), 1 mil to about 29 mils (about 0.025 mm to about 0.74 mm), or about 2 mils to about 28 mils (about 0.05 mm to about 0.71 mm).

[0105]

[0105] In the embodiments described below, the polymer resin is referred to as poly(vinyl butyral) PVB, although it will be understood by those skilled in the art that the polymer may be any polymer suitable for use in multilayer panels. Exemplary polymers include polyvinyl acetal (PVA) (e.g., PVB or the isomeric poly(vinyl isobutyral) (PVisoB), polyurethane (PU), poly(ethylene-co-vinyl acetate) (EVA), polyvinyl chloride (PVC), poly(vinyl chloride-co-methacrylate), polyethylene, polyolefins, ethylene acrylate ester copolymers, poly(ethylene-co-butyl acrylate), silicone elastomers, epoxy resins, as well as acid copolymers such as ethylene / carboxylic acid copolymers derived from any of the aforementioned possible thermoplastic resins. Polymers that can be used for the interlayer include, but are not limited to, polymers and ionomers thereof, and combinations of the foregoing. PVB and its isomeric polymer PVisoB, polyvinyl chloride, and polyurethanes are particularly useful polymers for the interlayer in general, with PVB (and its isomeric polymers) being particularly preferred. For example, a multi-layered interlayer can consist of PVB / / PVisoB / / PVB. Other examples include PVB / / PVC / / PVB or PVB / / PU / / PVB. Further examples include PVC / / PVB / / PVC or PU / / PVB / / PU.

[0106] As used herein, a multi-layer panel may include a single substrate, such as glass, acrylic, or polycarbonate, on which a polymer interlayer sheet is disposed, and most commonly, a polymer film is further disposed over the polymer interlayer. The combination of polymer interlayer sheet and polymer film is commonly referred to in the art as bilayer. A typical multi-layer panel having a bilayer structure is (glass) / / (polymer interlayer sheet) / / (polymer film), where the polymer interlayer sheet may include multiple interlayers as described above. The polymer film provides a smooth, thin, rigid substrate that provides better optical properties than would normally be obtained with the polymer interlayer sheet alone, and functions as a performance enhancing layer. The polymer film differs from the polymer interlayer sheet used herein in that the polymer film does not provide the necessary puncture resistance and glass retention properties by itself, but rather provides performance enhancements such as infrared absorption properties. Poly(ethylene terephthalate) ("PET") is the most commonly used polymer film. Generally, as used herein, a polymer film is thinner than a polymer sheet, such as about 0.001 to 0.2 mm thick.

[0107]

[0107] The interlayers of the present disclosure will be most commonly utilized in multi-layer panels that include two substrates, such as a pair of glass sheets (or other rigid materials known in the art, such as polycarbonate or acrylic), with the interlayer disposed between the two substrates. One example of such a structure would be (glass) / / (polymer interlayer sheet) / / (glass), where the polymer interlayer sheet can include a multi-layer interlayer as described above. These examples of multi-layer panels are not meant to be limiting in any way, as one of ordinary skill in the art will readily recognize that numerous structures other than those described above can be made using the interlayers of the present disclosure.

[0108] A typical glass lamination process includes the following steps: (1) assembling two substrates (e.g., glass) and an interlayer; (2) briefly heating the assembly by IR radiation or convection means; (3) passing the assembly through pressure nip rolls for a first degassing; (4) heating the assembly a second time to about 60°C to about 120°C to provide sufficient temporary adhesion to the assembly and seal the edges of the interlayer; (5) passing the assembly through a second pressure nip roll to further seal the edges of the interlayer and allow further handling; and (6) autoclaving the assembly at a temperature between 135°C to 150°C and a pressure between 180 psig to 200 psig for about 30 to 90 minutes. As known by those skilled in the art, the actual steps, as well as times and temperatures, may vary as needed.

[0109]

[0109] Other means known in the art and commercially practiced for use in degassing the interlayer-glass interface (steps 2-5) include vacuum bag and vacuum ring processes in which a vacuum is utilized to remove air.

[0110]

[0110] As previously indicated, transparency is a parameter used to describe the polymer interlayers disclosed herein. Transparency is determined by measuring the haze value or percent haze. Testing for percent haze is performed using a haze meter such as Model D25 available from Hunter Associates (Reston, VA) using Illuminant C at a 2 degree observation angle in accordance with ASTM D1003-61 (Re-approved 1977)-Procedure A. The polymer interlayer is laminated with a pair of clear glass sheets (commercially available from Pittsburgh Glass Works, Pennsylvania), each 2.3 mm thick, and the haze value is measured. The interlayers of the present disclosure have a percent haze of less than about 5%, less than about 4%, less than about 3%, less than about 2%, less than about 1%, or less than about 0.3%.

[0111]

[0111] Transmittance, or percent visible transmittance (%T vis ) is also used to describe the polymer interlayers disclosed herein. Transmittance is also measured with a haze meter, such as Model D25 available from Hunter Associates (Reston, VA), using an Illuminant D65 at a 10 degree observation angle. The polymer interlayer is laminated with a pair of clear glass sheets, each 2.3 mm thick (commercially available from Pittsburgh Glass Works, Pennsylvania), and the %T vis The polymer interlayers of the present disclosure have a %T of greater than 85 for interlayers containing only ACA, UV stabilizer, and antioxidant additives, or greater than 80% for interlayers containing additional additives such as pigments, IR absorbers or blockers as mentioned above. vis Polymer interlayers containing high levels of pigments and / or dyes can be used to achieve low %T, such as in raw material colored or pigmented polymer interlayers, if desired. vis It may have a value.

[0112]

[0112] Refractive index (RI) was measured according to ASTM D542. Reported RI values ​​were obtained at a wavelength of 589 nm and at 25°C.

[0113]

[0113] Glass transition temperature (T g ) may be determined by dynamic mechanical thermal analysis (DMTA). DMTA measures the storage (elastic) modulus in Pascals (G'), loss (viscous) modulus in Pascals (G"), and tan delta (=G" / G') of a sample as a function of temperature and temperature sweep rate at a given frequency. Herein, a frequency of 1 Hz and a temperature sweep rate of 3°C / min were used. T g is determined by the position of the tan delta peak on the temperature scale in °C.

[0114]

[0114] The damping loss factor (η) may be measured by Mechanical Impedance Measurement as described in ISO 16940. A laminated glass rod sample, 25 mm wide, 300 mm long, with a pair of 2.3 mm clear glass, is prepared and excited at the rod's center point by a vibrator shaker (Bruel and Kjaer). An impedance head (Bruel and Kjaer) is used to measure the force and velocity of vibration that excites the rod to oscillate, and the resulting transfer function is recorded on a National Instrument data acquisition and analysis system. The loss factor at the first vibration mode is calculated using the half-power method.

[0115]

[0115] "Sound Transmission Loss" (STL) is determined for laminates of fixed dimensions at a fixed temperature of 20°C using ASTM E90 (2009). A "reference panel" of 2.3 mm clear glass / / "reference interlayer" / / 2.3 mm clear glass is measured to have a coincidence frequency at 3,150 Hz, and an STL of 31 dB at the coincidence frequency, where the "reference interlayer" is produced by blending and melt extruding 100 parts of poly(vinyl butyral) resin with 18-19 wt.% residual hydroxyl content, and 2 wt.% vinyl acetate residual, 38 parts by weight of 3-GEH plasticizer, and other common additives (as described above). The reference interlayer has a thickness of 0.76 mm and a glass transition temperature of 30°C. The inventive or comparative multilayer interlayer is laminated with 2.3 mm clear glass by the method described above to make a reference (or test) laminated glass panel. The panel has dimensions of 50 cm x 80 cm. The STL of the test panel at the coincidence frequency of the "reference panel", for example, the STL at 3,150 Hz, is used to evaluate the sound insulation properties of the panel.

[0116]

[0116] Unless otherwise indicated, all numbers used in the specification and claims expressing the quantities of mixture components, properties such as molecular weights, reaction conditions, and the like, should be understood in all cases to be modified by the term "about". Thus, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximations that may vary depending on the desired properties sought to be obtained by the present invention. At the very least, each numerical parameter should be construed in light of the number of significant digits reported and by applying ordinary rounding techniques. Moreover, ranges presented in the present disclosure and claims are specifically intended to include the entire range, not just the endpoints. For example, a range presented as 0 to 10 is intended to disclose all integers between 0 and 10, such as 1, 2, 3, 4, all fractions between 0 and 10, such as 1.5, 2.3, 4.57, 6.1113, and the endpoints 0 and 10.

[0117]

[0117] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values ​​set forth in the specific examples are intended to be reported precisely given the measuring methods used, however, any numerical value inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.

[0118]

[0118] It should be understood that the reference to one or more process steps does not exclude the presence of additional process steps before or after the combined recited steps, or intervening process steps that are explicitly identified. Furthermore, unless otherwise indicated, the names of process steps, mixture components, or other aspects of information disclosed or claimed in this application, using letters or numbers or the like, are shorthand means for identifying separate activities or mixture components, and the recited letters can be arranged in any order.

[0119]

[0119] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. For example, n References to alcohol equivalents include multiple C n Alcohol equivalents are intended to be included. Thus, even the use of words such as "at least one" or "at least a portion" in one place is not intended to imply that other uses of "a," "an," and "the" exclude multiple referents, unless the context clearly dictates otherwise. Similarly, the use of words such as "at least a portion" in one place is not intended to imply that "all" is intended by the absence of such words in other places, unless the context clearly dictates otherwise.

[0120]

[0120] As used herein, the term "and / or," when used in a list of two or more items, means that any one of the listed items may be taken alone, or any combination of two or more of the listed items may be taken. For example, if a composition is described as containing components A, B, and / or C, the composition may contain A alone; B alone; C alone; a combination of A and B; a combination of A and C; a combination of B and C; or a combination of A, B, and C.

[0121]

[0121] Unless otherwise specifically indicated, the present invention may be further illustrated by the following examples of embodiments thereof, but it will be understood that these examples are included merely for illustrative purposes and are not intended to limit the scope of the invention. EXAMPLES

[0122] Example 1

[0122] A sample of the multilayer sheet was cut into pieces of approximately 15 mm. 300 g of the multilayer chips and 700 g of triethylene glycol bis(2-ethylhexanoate) (3-GEH) were charged into a 1 L glass reactor equipped with a stirrer. The mixture was stirred and heated to 80°C and maintained for 2 hours. The resulting batch was cooled to room temperature and filtered using a Buchner funnel with 1 mm holes. 5 g of water was added to 500 g of the filtrate, stirred for 1 hour, and the mixture was allowed to settle overnight before centrifugation. After centrifugation, 455 g of clear 3-GEH centrate and 45 g of sediment (water and core layer PVB) were obtained.

[0123] Example 2 A sample of the multilayer sheet was cut into pieces of approximately 1.27 centimeters (0.5 inches). 300 g of the multilayer chips, 245 g of 3-GEH, and 455 g of the centrate from Example 1 were charged into a 1 L glass reactor. The mixture was stirred and heated to 70° C. and maintained for 4 hours. The resulting batch was cooled to room temperature and filtered using a Buchner funnel (with 1 mm holes). 5 g of water containing 1% KOAC was added to 500 g of the filtrate and stirred for 1 hour. The mixture was allowed to settle overnight before centrifugation. After centrifugation, 480 g of clear 3-GEH centrate and 20 g of sediment (water and PVB compound with composition 2) were obtained.

[0124] Example 3 300 g of multilayer chips, 245 g of 3-GEH, and 455 g of centrate from the above example were charged into a 1 L glass reactor. The mixture was stirred and heated to 70° C. and maintained for 4 hours. The resulting batch was cooled to 5° C. and filtered using a Buchner funnel (with 1 mm holes). 5 g of water was added to 524 g of filtrate, stirred for 10 minutes, and the mixture was allowed to settle overnight before centrifugation. After centrifugation, 480 g of clear 3-GEH centrate and 20 g of sediment (PVB with water and composition 2) were obtained.

[0125] [Table 1]

[0126] Examples 1-3 describe the treatments applied to samples of granulated multilayer sheet obtained after grinding and passing through a 12 mm screen. The total thickness of the multilayer sheet was 0.84 mm, the core layer thickness was 0.11 mm. The overall plasticizer content was 42.1, the skin layer plasticizer was 38, and the core layer plasticizer was 75. The skin layer PVB had a hydroxyl content of 19% and an acetate content of about 1.5%. The core layer PVB had a hydroxyl content of 11% and an acetate content of about 1%.

[0127] Example 4

[0125] The multilayer sheet sample was cut into small pieces with at least one dimension of <6 mm. 250 g of multilayer chips and 750 g of triethylene glycol bis(2-ethylhexanoate) (3-GEH) were charged into a 2 L equipment equipped with a stirrer. The liquid was stirred to 65°C before the addition of the solids, and continued to be stirred at 55°C for 2 hours after the addition. The slurry batch was transferred to a Büchner funnel with a 1 mm hole for solid-liquid separation. 33 g of 25% potassium acetate aqueous solution was added to 664 g of the filtrate and stirred before cooling and centrifugation. After centrifugation, the 3-GEH centrate was obtained as a liquid phase, and the resulting sediment was a mixture of water, 3-GEH, and core layer PVB. The varnish sediment was heated to about T 130°C at atmospheric pressure in a jacketed stainless steel stirred tank. It was maintained for 24 hours until the temperature increased further (indicating that all the water had been removed), after which the mixture was allowed to cool, yielding a varnish.

[0128] Example 5 Varnish recycled for product 1 Approximately 87.6 pounds of virgin PVB resin, 6.2 pounds of multilayer PVB flake, 20.5 pounds of triethylene glycol bis(2-ethylhexanoate), and 16.1 pounds of varnish were blended together. The entire mixture was mixed in a batch mixer before being discharged into an extruder for PVB sheet extrusion.

[0129] Example 6 Varnish recycled for product 2

[0127] 87.6 pounds of PVB resin, 12.7 pounds of multilayer PVB flake, 3.2 pounds of calcium carbonate, 20.5 pounds of triethylene glycol bis(2-ethylhexanoate), and 16.1 pounds of varnish were blended together in a batch mixer before being discharged into an extruder for PVB sheet extrusion.

[0130] Example 7 Varnish recycled for product 3

[0128] 100 pounds of PVB core resin, 60 pounds of triethylene glycol bis(2-ethylhexanoate) and 15.0 pounds of varnish were blended together. The entire mixture was mixed in a batch mixer before being discharged into an extruder for PVB sheet coextrusion to make a multi-layer PVB product.

[0131] [Table 2]

Claims

1. 1. A process for recovering stiff poly(vinyl butyral) from a plasticized poly(vinyl butyral) multi-layer sheet containing stiff poly(vinyl butyral) and soft poly(vinyl butyral), comprising the steps of: a. pulverizing a plasticized poly(vinyl butyral) multi-layer sheet to obtain poly(vinyl butyral) granules; b. adding additional plasticizer to the poly(vinyl butyral) granules and removing at least a portion of the soft poly(vinyl butyral) from the poly(vinyl butyral) granules to obtain granules enriched in stiff poly(vinyl butyral) and a varnish of soft poly(vinyl butyral) and additional plasticizer; c. physically separating the granules enriched in stiff poly(vinyl butyral) from the varnish of soft poly(vinyl butyral) and additional plasticizer; The method includes:

2. The method of claim 1, further comprising the step of adding water and optionally potassium acetate to the varnish to separate the additional plasticizer from the water and core layer mixture.

3. The method of claim 1 , wherein the step of physically separating the particulate matter is carried out using one or more techniques selected from decantation, filtration, or centrifugation.

4. 4. The method of claim 1, wherein the step of removing at least a portion of the soft poly(vinyl butyral) from the poly(vinyl butyral) granules comprises selectively washing the soft poly(vinyl butyral) from the poly(vinyl butyral) granules.

5. d. adding additional plasticizer to the now stiff poly(vinyl butyral) enriched granules to remove additional portions of the soft poly(vinyl butyral) from the granules; e. separating the granules from the additional portion of the soft poly(vinyl butyral) and the additional plasticizer using one or more techniques selected from decantation, filtration, or centrifugation; The method of claim 1 , further comprising:

6. 6. The method of any one of claims 1 to 5, wherein the additional plasticizer is selected from one or more of esters of polybasic acids or polyhydric alcohols.

7. 7. The method of any one of claims 1 to 6, wherein the additional plasticizer is added to the poly(vinyl butyral) granules at a temperature of from about 25°C to about 90°C.

8. 8. The method of any one of claims 1 to 7, wherein the additional plasticizer is selected from one or more of triethylene glycol bis(2-ethylhexanoate), tetraethylene glycol bis(2-ethylhexanoate), triethylene glycol bis(2-ethylbutyrate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, bis(2-ethylhexyl)adipate, bis(2-ethoxyethyl)adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, adipic acid polymers, soybean oil, or epoxidized soybean oil.

9. The method of any one of claims 1 to 8, wherein the flexible poly(vinyl butyral) has a residual hydroxyl content of from about 8% to about 12%.

10. 10. The method of any one of claims 1 to 9, wherein the stiff poly(vinyl butyral) has a residual hydroxyl content of from about 15% to about 25%.

11. 11. The method of any one of claims 1 to 10, wherein the flexible poly(vinyl butyral) has a residual acetate content of less than about 15%.

12. 12. The method of any one of claims 1 to 11, wherein the stiff poly(vinyl butyral) has a residual acetate content of less than about 5%.

13. 13. The method of any one of claims 1 to 12, wherein the soft poly(vinyl butyral) contained in the plasticized poly(vinyl butyral) multilayer sheet comprises triethylene glycol bis(2-ethylhexanoate) present as a plasticizer.

14. 14. The method of any one of claims 1 to 13, wherein the soft poly(vinyl butyral) contained in the plasticized poly(vinyl butyral) multilayer sheet further comprises dihexyl adipate present as a plasticizer.

15. 15. The method of any one of claims 1 to 14, wherein triethylene glycol bis(2-ethylhexanoate) is present in the flexible poly(vinyl butyral) in an amount from about 60 phr to about 100 phr.

16. 16. The method of any one of claims 1 to 15, wherein the additional plasticizer added to the poly(vinyl butyral) granules in step b) comprises triethylene glycol bis(2-ethylhexanoate).

17. 17. The method of any one of claims 1 to 16, wherein the difference between the residual hydroxyl content of the soft poly(vinyl butyral) and the residual hydroxyl content of the stiff poly(vinyl butyral) is at least 4.0 weight percent.

18. 18. The method of any one of claims 1 to 17, wherein the stiff poly(vinyl butyral) contained in the plasticized poly(vinyl butyral) multi-layer sheet comprises from about 30 phr to about 45 phr of a plasticizer.

19. 19. The method of any one of claims 1 to 18, further comprising subjecting the varnish of the soft poly(vinyl butyral) and additional plasticizer to one or more of precipitation, filtration, centrifugation, evaporation, or precipitation to isolate the soft poly(vinyl butyral).

20. 20. The method of any one of claims 1 to 19, further comprising the step of adding a varnish of soft poly(vinyl butyral) and additional plasticizer to the poly(vinyl butyral) composition.

21. 21. The method of claim 20, further comprising forming the poly(vinyl butyral) composition into a sheet.

22. 22. The method of any one of claims 1 to 21, further comprising the step of adding a varnish of soft poly(vinyl butyral) and additional plasticizer to the poly(vinyl butyral) composition containing a whitening agent to form a translucent intermediate layer.

23. 23. The method of any one of claims 1 to 22, further comprising the step of adding a varnish of soft poly(vinyl butyral) and additional plasticizer to the clear poly(vinyl butyral) formulation.

24. 20. A poly(vinyl butyral) sheet comprising the isolated flexible poly(vinyl butyral) of claim 19.

25. 22. A laminated glass comprising the poly(vinyl butyral) sheet of claim 21.

26. 26. A poly(vinyl butyral) sheet comprising the separated, stiff poly(vinyl butyral)-enriched particles of any one of claims 1 to 25.

27. 27. A laminated glass comprising the poly(vinyl butyral) sheet of any one of claims 1 to 26.