Abstract
Description
[Technical field]
[0001] The present disclosure relates to polyesters suitable for use as impact modifiers, and biodegradable polymer compositions incorporating such impact modifiers. [Background technology]
[0002] Petroleum-based polymers such as polyethylene (PE), polypropylene (PP), or polyethylene terephthalate (PET) have been used for many years in a wide variety of applications. Although such polymers may offer good strength, barrier properties, and / or printability characteristics, unfortunately, they do not readily decompose or decay after disposal, either in landfills or through home composting techniques. That is, films, bags, and other materials made from such polymers may reside in landfills for centuries after disposal.
[0003] As a result, there is an ever-increasing demand for alternative polymers that can be derived from biological sources, biodegradable, and / or compostable. Examples of such polymers include poly(lactic acid) and poly(hydroxyalkanoates). While such biopolymers offer the obvious advantages of biodegradability and / or compostability, it is typically desirable to blend the biopolymers with various additives to improve their physical properties.
[0004] If the additives blended into the biopolymer are not biodegradable and / or compostable, the environmental benefits of the biopolymer are diminished. As a result, it would be desirable to provide additives for use with biopolymers, such as those incorporated into poly(lactic acid) and poly(hydroxyalkanoates), that are themselves biodegradable and / or compostable. Summary of the Invention
[0005] These and other needs are met by compostable polyester according to the present disclosure.
[0006] In a first aspect, the present disclosure provides a polyester. According to one particular embodiment, the polyester is made of: (1) about 15 to about 40 weight percent isosorbide monomer repeat units, (2) about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, and (3) about 10 to about 20 weight percent polyhydric alcohol monomer repeat units. All of these weight percentages are based on the total weight of the polyester.
[0007] The polyester also has a weight average molecular weight of at least 8000 Daltons as specified by ASTM D5296-05.More preferably, the polyester has a weight average molecular weight of from about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
[0008] In certain embodiments, the dicarboxylic acid or dicarboxylic anhydride is preferably succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalic anhydride, 1,8-naphthalenedicarboxylic acid, dimethyl 1,8-naphthalate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, mellitic acid, trimellitic anhydride, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid , partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate new polymer, polybutylene terephthalate new polymer, and mixtures thereof.
[0009] More preferably, the dicarboxylic acid or dicarboxylic anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.
[0010] In a particularly preferred embodiment, the dicarboxylic acid or dicarboxylic anhydride is made from a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester preferably has about 25 to about 35 weight percent succinic acid or succinic anhydride and about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0011] In some embodiments, the polyhydric alcohol is preferably selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and poly(oxyalkylene) polyols containing ethylene oxide, propylene oxide, or butylene oxide monomer repeat units, and mixtures thereof.
[0012] More preferably, the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof. Even more preferably, the polyhydric alcohol comprises 1,3-propanediol.
[0013] In some examples, the dicarboxylic acid or dicarboxylic anhydride preferably comprises succinic acid or succinic anhydride, and the polyhydric alcohol preferably comprises 1,3-propanediol.
[0014] In alternative embodiments, isosorbide can be omitted from the polyester. In such examples, the polyester is made of: (1) about 35 to about 65 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, where the dicarboxylic acid or dicarboxylic anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof; and (2) about 35 to about 65 weight percent polyhydric alcohol monomer repeat units.
[0015] In a preferred embodiment, the dicarboxylic acid or dicarboxylic anhydride is made of a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 30 to about 40 weight percent succinic acid or succinic anhydride and about 10 to about 20 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0016] Suitable polyhydric alcohols for the alternative polyesters are the same as those described above for the isosorbide-containing polyesters. Similarly, for the alternative polyesters, the weight average molecular weight of the polyester is at least 8000 Daltons as specified by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
[0017] In a second aspect, the disclosure provides a polymer composition. The polymer composition typically comprises about 50 to about 95 weight percent of a biodegradable polymer, the degradable polymer being selected from the group consisting of poly(lactic acid), poly(hydroxyalkanoates), and mixtures thereof. The polymer composition also comprises about 5 to about 50 weight percent of an impact modified polyester. The impact modified polyester, in turn, is made of: (1) about 15 to about 40 weight percent isosorbide monomer repeat units, based on the total weight of the polyester; (2) about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, based on the total weight of the polyester; and (3) about 10 to about 20 weight percent polyhydric alcohol monomer repeat units, based on the total weight of the polyester. The impact modified polyester also has a weight average molecular weight of at least 8000 Daltons, as specified by ASTM D5296-05.
[0018] In certain embodiments, the dicarboxylic acid or dicarboxylic anhydride is preferably succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalic anhydride, 1,8-naphthalenedicarboxylic acid, dimethyl 1,8-naphthalate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride. The compound is selected from the group consisting of mellitic acid, trimellitic anhydride, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate new polymer, polybutylene terephthalate new polymer, and mixtures thereof.
[0019] More preferably, the dicarboxylic acid or dicarboxylic anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.
[0020] In a particularly preferred embodiment, the dicarboxylic acid or dicarboxylic anhydride is made from a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester preferably has about 25 to about 35 weight percent succinic acid or succinic anhydride and about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0021] In some embodiments, the polyhydric alcohol is preferably selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and ethylene oxide, propylene oxide, or butylene oxide monomer repeat units. and mixtures thereof.
[0022] More preferably, the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof. Even more preferably, the polyhydric alcohol comprises 1,3-propanediol.
[0023] In some examples, the dicarboxylic acid or dicarboxylic anhydride preferably comprises succinic acid or succinic anhydride, and the polyhydric alcohol preferably comprises 1,3-propanediol.
[0024] According to certain embodiments, the polymer composition more preferably comprises from about 60 to about 85 weight percent of the biodegradable polymer and from about 5 to about 30 weight percent of the impact modified polyester. Even more preferably, the polymer composition comprises from about 7.5 to about 15 weight percent of the impact modified polyester.
[0025] In some examples, the biodegradable polymer preferably comprises poly(lactic acid). In other embodiments, the biodegradable polymer preferably comprises at least one poly(hydroxyalkanoate). In some embodiments, the biodegradable polymer preferably comprises a mixture of poly(lactic acid) and poly(hydroxyalkanoate). For example, in some embodiments, the polymer composition can comprise about 5 to about 25 weight percent poly(lactic acid) and about 70 to about 90 weight percent of at least one poly(hydroxyalkanoate), based on the total weight of the polymer composition.
[0026] According to certain embodiments in which the polymer composition comprises poly(hydroxyalkanoates), the at least one poly(hydroxyalkanoate) is preferably made of poly-3-hydroxybutyrate-co-3-hydroxyhexanoate (“P(3HB-co-3HHx)”).
[0027] In some instances, the (3HB-co-3HHx) is preferably made up of about 75 to about 99 mole percent hydroxybutyrate and about 1 to about 25 mole percent hydroxyhexanoate. More preferably, the (3HB-co-3HHx) is made up of about 93 to about 98 mole percent hydroxybutyrate and about 2 to about 7 mole percent hydroxyhexanoate.
[0028] In yet other embodiments, the at least one poly(hydroxyalkanoate) can include a terpolymer made of about 75 to about 99.9 mole percent 3-hydroxybutyrate monomer repeat units, about 0.1 to about 25 mole percent 3-hydroxyhexanoate monomer repeat units, and about 0.1 to about 25 mole percent of a third 3-hydroxyalkanoate monomer repeat unit having 5 to 12 carbon atoms.
[0029] According to certain embodiments, the at least one poly(hydroxyalkanoate) preferably has a weight average molecular weight of about 50,000 Daltons to about 2.5 million Daltons as specified by ASTM D5296-05.More preferably, the at least one poly(hydroxyalkanoate) has a weight average molecular weight of about 500,000 Daltons to about 750,000 Daltons as specified by ASTM D5296-05.
[0030] The polymer composition may also include additional additives. In some embodiments, the polymer composition comprises from about 1 to about 10 weight percent of at least one plasticizer and from about 0.1 to about It may also include 5 weight percent of at least one nucleating agent, and from about 0.1 to about 10 weight percent of a bulking agent.
[0031] In some instances, the polymeric composition can include additional biodegradable polymers in addition to poly(lactic acid) and / or poly(hydroxyalkanoate). That is, in certain embodiments, the polymeric composition can also include about 5 to about 50 weight percent of at least one biodegradable polymer selected from the group consisting of poly(caprolactone), poly(ethylene sebacate), poly(butylene succinate), poly(butylene succinate-co-adipate), poly(butylene adipate terephthalate), poly(vinyl acetate), and mixtures thereof.
[0032] According to certain embodiments, the polymer composition is preferably biodegradable as specified using ASTM standard D5988. Additionally, in some embodiments, the polymer composition is preferably home compostable as specified using ASTM standard D6868.
[0033] The present disclosure also provides various end products that can be formed from the polymer composition. That is, according to one embodiment, the present disclosure provides a molded sheet made of the polymer composition. In a second embodiment, the present disclosure provides a molded article made of the polymer composition, the molded article being formed by thermoforming, injection molding, or blow molding. In another embodiment, the present disclosure provides a film made of the polymer composition, the film being a blown film or a cast film. In yet another embodiment, the present disclosure provides a fiber made of the polymer composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The present disclosure provides, for the first time, novel polyesters suitable for use as impact modifiers in biodegradable and / or compostable polymer compositions.
[0035] Generally, polyesters are made of at least three different monomer repeat units derived from (1) isosorbide, (2) succinic acid or succinic anhydride, and (3) 1,3-propanediol. In terms of amounts, polyesters are typically made of (1) about 15 to about 40 weight percent isosorbide monomer repeat units, (2) about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, and (3) about 10 to about 20 weight percent polyhydric alcohol monomer repeat units.
[0036] A variety of dicarboxylic acids and dicarboxylic anhydrides are contemplated as suitable for use in preparing the polyesters. For example, the dicarboxylic acid or dicarboxylic anhydride may be succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalic anhydride, 1,8-naphthalenedicarboxylic acid, dimethyl 1,8-naphthalate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, mellitic acid, trimellitic anhydride, mellitic acid, phthalic anhydride, mellitic ... The acid anhydride may be suitably selected from the group consisting of acid anhydrides, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate new polymer, polybutylene terephthalate new polymer, and mixtures thereof.
[0037] More preferably, the dicarboxylic acid or dicarboxylic anhydride is succinic acid or succinic anhydride. , nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.
[0038] In a particularly preferred embodiment, the dicarboxylic acid or dicarboxylic anhydride is made from a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester preferably has about 25 to about 35 weight percent succinic acid or succinic anhydride and about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0039] A range of polyhydric alcohols are also believed to be suitable for the polyesters. Examples of suitable polyhydric alcohols may be selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and poly(oxyalkylene) polyols containing ethylene oxide, propylene oxide, or butylene oxide monomer repeat units, and mixtures thereof.
[0040] More preferably, the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof. Even more preferably, the polyhydric alcohol comprises 1,3-propanediol.
[0041] In particularly preferred embodiments, the dicarboxylic acid or dicarboxylic anhydride preferably comprises succinic acid or succinic anhydride and the polyhydric alcohol preferably comprises 1,3-propanediol.
[0042] The polyester also has a weight average molecular weight of at least 8000 Daltons as specified by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
[0043] Generally, the polyesters can be prepared by charging isosorbide to a reaction flask or other reactor equipped with a nitrogen inlet, vacuum capability, heating, and stirring. The isosorbide is first melted and then vacuum degassed as a molten mass. The diacid is then added and the contents of the flask are reacted at temperatures up to 220°C until water evolution subsides, at which point any remaining glycol is charged. Esterification is completed at temperatures up to 220°C and low vacuum pressures of 3.3 kPa.
[0044] In alternative embodiments, isosorbide can be omitted from the polyester. In such examples, the polyester is made of: (1) about 35 to about 65 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, where the dicarboxylic acid or dicarboxylic anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof; and (2) about 35 to about 65 weight percent polyhydric alcohol monomer repeat units.
[0045] In a preferred embodiment, the dicarboxylic acid or dicarboxylic anhydride is made of a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof. For this embodiment, the polyester is preferably about 30 to about 40 weight percent succinic acid or succinic anhydride and about 10 to about 20 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0046] Suitable polyhydric alcohols for the alternative polyesters are the same as those described above for the isosorbide-containing polyesters. Similarly, for the alternative polyesters, the weight average molecular weight of the polyester is at least 8000 Daltons as specified by ASTM D5296-05. More preferably, the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
[0047] The polyesters according to the present disclosure are suitable for use as impact modifiers in polymer compositions. As used herein, "impact modifiers" are additives used to improve the durability and toughness of polymer resins, where toughness is measured as the area under the stress-strain curve of standard tensile elongation and modulus tests. Polymer toughness can also be correlated with testing by notched Izod test. The higher the impact number a polymer exhibits, the higher the toughness is likely to be.
[0048] The polyesters according to the present disclosure are also preferably biodegradable as specified using ASTM standard D5511. Additionally, in some embodiments, the polyesters are preferably home compostable as specified using ASTM standard D6868.
[0049] The present disclosure also provides a polymeric composition comprising the polyester as described. Generally, the polymeric composition combines an impact-modified polyester with at least one biodegradable polymer, the at least one biodegradable polymer being selected from the group consisting of poly(lactic acid), poly(hydroxyalkanoates), and mixtures thereof. Typically, the polymeric composition comprises about 5 to about 50 weight percent of the impact-modified polyester, and about 50 to about 95 weight percent of the biodegradable polymer selected from the group consisting of poly(lactic acid), poly(hydroxyalkanoates), and mixtures thereof.
[0050] More preferably, the polymer composition comprises from about 60 to about 85 weight percent of the biodegradable polymer and from about 5 to about 30 weight percent of the impact modified polyester. Even more preferably, the polymer composition comprises from about 7.5 to about 15 weight percent of the impact modified polyester.
[0051] Again, the impact modifier used in the polymer composition is a polyester according to the disclosure above, i.e., the impact modified polyester is made of: (1) about 15 to about 40 weight percent isosorbide monomer repeat units, (2) about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, and (3) about 10 to about 20 weight percent polyhydric alcohol monomer repeat units. The impact modified polyester also has a weight average molecular weight of at least 8000 Daltons as specified by ASTM D5296-05.
[0052] In some instances, the biodegradable polymer preferably comprises poly(lactic acid). In other embodiments, the biodegradable polymer preferably comprises at least one poly(hydroxyalkanoate). Moreover, in certain embodiments, the biodegradable polymer preferably comprises a mixture of poly(lactic acid) and poly(hydroxyalkanoate). For example, In some embodiments, the polymer composition can include about 5 to about 25 weight percent poly(lactic acid) and about 70 to about 90 weight percent of at least one poly(hydroxyalkanoate), based on the total weight of the polymer composition.
[0053] According to certain embodiments in which the polymer composition comprises poly(hydroxyalkanoates), the at least one poly(hydroxyalkanoate) is preferably made of poly-3-hydroxybutyrate-co-3-hydroxyhexanoate (“P(3HB-co-3HHx)”).
[0054] In some instances, the (3HB-co-3HHx) is preferably made up of about 75 to about 99 mole percent hydroxybutyrate and about 1 to about 25 mole percent hydroxyhexanoate. More preferably, the (3HB-co-3HHx) is made up of about 93 to about 98 mole percent hydroxybutyrate and about 2 to about 7 mole percent hydroxyhexanoate.
[0055] In yet other embodiments, the at least one poly(hydroxyalkanoate) can include a terpolymer made of about 75 to about 99.9 mole percent 3-hydroxybutyrate monomer repeat units, about 0.1 to about 25 mole percent 3-hydroxyhexanoate monomer repeat units, and about 0.1 to about 25 mole percent of a third 3-hydroxyalkanoate monomer repeat unit having 5 to 12 carbon atoms.
[0056] According to certain embodiments, the at least one poly(hydroxyalkanoate) preferably has a weight average molecular weight of about 50,000 Daltons to about 2.5 million Daltons as specified by ASTM D5296-05.More preferably, the at least one poly(hydroxyalkanoate) has a weight average molecular weight of about 500,000 Daltons to about 750,000 Daltons as specified by ASTM D5296-05.
[0057] The polymer composition may also include additional additives. For example, the polymer composition may include a plasticizer, a nucleating agent, and / or a bulking agent. In some embodiments, the polymer composition may also include about 1 to about 10 weight percent of at least one plasticizer, about 0.1 to about 5 weight percent of at least one nucleating agent, and about 0.1 to about 10 weight percent of a bulking agent.
[0058] Suitable nucleating agents for use in the polymeric composition can be selected, for example, from the group consisting of pentaerythritol, boron nitride, poly(hydroxybutyrate), inositol, clay, dipentaerythritol, sorbitol, and mixtures thereof.
[0059] Suitable fillers for use in the polymer composition can be selected from the group consisting of, for example, aragonite, clay, calcium carbonate, cellulose, nanocellulose, talc, kaolinite, montmorillonite, bentonite, silica, chitin, starch, diatomaceous earth, titanium dioxide, nanoclay, mica, and mixtures thereof.
[0060] Suitable plasticizers for use in the polymer composition include, for example, sebacic acid esters, citrate esters, fatty adipic acid esters, fatty succinic acid esters, and fatty glucaric acid esters, lactate esters, alkyl diesters, citrate esters, alkyl methyl esters, dibenzoate esters, propylene carbonate, caprolactone diols having a number average molecular weight of 200 to 10,000 g / mol, poly(ethylene) glycols having a number average molecular weight of 400 to 10,000 g / mol, vegetable oil esters, long chain alkyl acids, adipate esters, glycerol, isosorbide derivatives, or mixtures thereof, HALLGREEN IM-8830 esters, HALLGREEN R-8010 esters, hydroxybutyrate ... The copolymer may be selected from the group consisting of polyhydroxyalkanoate copolymers containing at least 18 mole percent hydroxyalkanoate monomer repeat units other than hydroxyalkanoate, and mixtures thereof.
[0061] Moreover, in certain embodiments, the polymeric composition can include additional biodegradable polymers in addition to poly(lactic acid) and / or poly(hydroxyalkanoate). That is, in certain embodiments, the polymeric composition can also include about 5 to about 50 weight percent of at least one biodegradable polymer selected from the group consisting of poly(caprolactone), poly(ethylene sebacate), poly(butylene succinate), poly(butylene succinate-co-adipate), poly(butylene adipate terephthalate), poly(vinyl acetate), and mixtures thereof.
[0062] According to certain embodiments, the entire polymer composition is preferably biodegradable as specified using ASTM standard D5988. Additionally, in some embodiments, the polymer composition is preferably home compostable as specified using ASTM standard D6868.
[0063] A variety of end products can be formed from the polymer composition according to the present disclosure. That is, according to one embodiment, the present disclosure provides a molded sheet made of the polymer composition. In a second embodiment, the present disclosure provides a molded article made of the polymer composition, the molded article being formed by thermoforming, injection molding, or blow molding. In another embodiment, the present disclosure provides a film made of the polymer composition, the film being a blown film or a cast film. In yet another embodiment, the present disclosure provides a fiber made of the polymer composition.
[0064] Embodiment The present disclosure is further illustrated by the following embodiments:
[0065] Embodiment 1. A polyester comprising: from about 15 to about 40 weight percent isosorbide monomer repeat units, based on the total weight of the polyester; from about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, based on the total weight of the polyester; and from about 10 to about 20 weight percent polyhydric alcohol monomer repeat units, based on the total weight of the polyester, the polyester having a weight average molecular weight of at least 8000 Daltons as determined by ASTM D5296-05.
[0066] Embodiment 2. The dicarboxylic acid or dicarboxylic anhydride is succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalic anhydride, 1,8-naphthalenedicarboxylic acid, dimethyl 1,8-naphthalate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, mellitic acid, trimellitic anhydride. 2. The polyester of embodiment 1, wherein the polyester is selected from the group consisting of hydrates, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate new polymer, polybutylene terephthalate new polymer, and mixtures thereof.
[0067] Embodiment 3. The dicarboxylic acid or dicarboxylic anhydride is succinic acid, succinic anhydride, nadic anhydride, methylnadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C3 6 dimer acid, and mixtures thereof.
[0068] Embodiment 4. The polyester of any one of the preceding embodiments, wherein the dicarboxylic acid or dicarboxylic anhydride comprises a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof.
[0069] Embodiment 5. The polyester of any one of the preceding embodiments, wherein the polyester comprises about 25 to about 35 weight percent succinic acid or succinic anhydride, and about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0070] Embodiment 6. The polyester of any one of the preceding embodiments, wherein the polyhydric alcohol is selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and poly(oxyalkylene) polyols containing ethylene oxide, propylene oxide, or butylene oxide monomeric repeat units, and mixtures thereof.
[0071] Embodiment 7. The polyester of any one of the preceding embodiments, wherein the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof.
[0072] Embodiment 8. The polyester of any one of the preceding embodiments, wherein the polyhydric alcohol comprises 1,3-propanediol.
[0073] Embodiment 9. The polyester of any one of the preceding embodiments, wherein the dicarboxylic acid or dicarboxylic anhydride comprises succinic acid or succinic anhydride, and the polyhydric alcohol comprises 1,3-propanediol.
[0074] Embodiment 10. The polyester of any one of the preceding embodiments, wherein the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
[0075] Embodiment 11. A polymeric composition comprising: about 50 to about 95 weight percent of a biodegradable polymer selected from the group consisting of poly(lactic acid), poly(hydroxyalkanoates), and mixtures thereof; and about 5 to about 50 weight percent of an impact modified polyester, the impact modified polyester comprising about 15 to about 40 weight percent isosorbide monomer repeat units, based on the total weight of the polyester; about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, based on the total weight of the polyester; and about 10 to about 20 weight percent polyhydric alcohol monomer repeat units, based on the total weight of the polyester, the polyester having a weight average molecular weight of at least 8000 Daltons as determined by ASTM D5296-05.
[0076] Embodiment 12. The dicarboxylic acid or dicarboxylic anhydride is succinic acid, succinic anhydride, glutaric acid, pimelic acid, undecanoic acid, dodecanoic acid, dodecanedioic acid, suberic acid, azelaic acid, sebacic acid, adipic acid, phthalic anhydride, dimethyl terephthalate, terephthalic acid, isophthalic acid, 1,8-naphthalic anhydride, 1,8-naphthalenedicarboxylic acid, dimethyl 1,8-naphthalate, dimethyl isophthalate, phthalic acid, pyromellitic anhydride, mellitic anhydride, mellitic acid, trimellitic anhydride. 12. The polymer composition of embodiment 11, wherein the polymer is selected from the group consisting of water, 3,3'4,4'-benzophenonetetracarboxylic anhydride, 3,3'4,4'-benzophenonetetracarboxylic acid, trimellitic acid, nadic anhydride, methyl nadic anhydride, C36 dimer acid, partially hydrogenated C36 dimer acid, polyethylene terephthalate recycled polymer, polybutylene terephthalate recycled polymer, polyethylene terephthalate new polymer, polybutylene terephthalate new polymer, and mixtures thereof.
[0077] Embodiment 13. The polymer composition of embodiment 11 or 12, wherein the dicarboxylic acid or dicarboxylic anhydride is selected from the group consisting of succinic acid, succinic anhydride, nadic anhydride, methyl nadic anhydride, sebacic acid, C36 dimer acid, partially hydrogenated C36 dimer acid, and mixtures thereof.
[0078] Embodiment 14. The polymer composition of any one of embodiments 11 to 13, wherein the dicarboxylic acid or dicarboxylic anhydride comprises a mixture of (1) succinic acid or succinic anhydride and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof.
[0079] Embodiment 15. The polymer composition of any one of embodiments 11 to 14, wherein the polyester comprises about 25 to about 35 weight percent succinic acid or succinic anhydride, and about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
[0080] Embodiment 16. The polymer composition of any one of embodiments 11 to 15, wherein the polyhydric alcohol is selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and poly(oxyalkylene) polyols containing ethylene oxide, propylene oxide, or butylene oxide monomer repeat units, and mixtures thereof.
[0081] Embodiment 17. The polymer composition of any one of embodiments 11 to 16, wherein the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof.
[0082] Embodiment 18. The polymer composition of any one of embodiments 11 to 17, wherein the polyhydric alcohol comprises 1,3-propanediol.
[0083] Embodiment 19. The polymer composition of any one of embodiments 11 to 18, wherein the dicarboxylic acid or dicarboxylic anhydride comprises succinic acid or succinic anhydride and the polyhydric alcohol comprises 1,3-propanediol.
[0084] Embodiment 20. The polymer composition of any one of embodiments 11 to 19, wherein the impact modified polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
[0085] Embodiment 21. The polymer composition of any one of embodiments 11 to 20, wherein the polymer composition comprises about 60 to about 85 weight percent of the biodegradable polymer and about 5 to about 30 weight percent of the impact modified polyester.
[0086] Embodiment 22. The polymer composition of any one of embodiments 11 to 21, wherein the biodegradable polymer comprises poly(lactic acid).
[0087] Embodiment 23. The polymer composition of any one of embodiments 11 to 22, wherein the biodegradable polymer comprises at least one poly(hydroxyalkanoate).
[0088] Embodiment 24. The polymer composition of embodiment 23, wherein the at least one poly(hydroxyalkanoate) comprises poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)").
[0089] Embodiment 25. The polymer composition of embodiment 24, wherein the P(3HB-co-3HHx) comprises from about 75 to about 99 mole percent hydroxybutyrate and from about 1 to about 25 mole percent hydroxyhexanoate.
[0090] Embodiment 26. The polymer composition of embodiment 24, wherein the P(3HB-co-3HHx) comprises from about 93 to about 98 mole percent hydroxybutyrate and from about 2 to about 7 mole percent hydroxyhexanoate.
[0091] Embodiment 27. The polymer composition of embodiment 23, wherein the at least one poly(hydroxyalkanoate) comprises a terpolymer made of about 75 to about 99.9 mole percent 3-hydroxybutyrate monomer repeat units, about 0.1 to about 25 mole percent 3-hydroxyhexanoate monomer repeat units, and about 0.1 to about 25 mole percent of a third 3-hydroxyalkanoate monomer repeat unit having 5 to 12 carbon atoms.
[0092] Embodiment 28. The at least one poly(hydroxyalkanoate) is in accordance with ASTM 24. The polymer composition of embodiment 23, having a weight average molecular weight of about 50,000 Daltons to about 2.5 million Daltons as determined by D5296-05.
[0093] Embodiment 29. The at least one poly(hydroxyalkanoate) is in accordance with ASTM 24. The polymer composition of embodiment 23, having a weight average molecular weight of about 500,000 Daltons to about 750,000 Daltons as determined by D5296-05.
[0094] Embodiment 30. The polymer composition of any one of embodiments 11 to 29, wherein the polymer composition comprises about 5 to about 25 weight percent of poly(lactic acid) and about 70 to about 90 weight percent of at least one poly(hydroxyalkanoate).
[0095] Embodiment 31. The polymer composition of any one of embodiments 11 to 30, further comprising: from about 1 to about 10 weight percent of at least one plasticizer; from about 0.1 to about 5 weight percent of at least one nucleating agent; and From about 0.1 to about 10 weight percent of a bulking agent.
[0096] Embodiment 32. The polymer composition of any one of embodiments 11 to 31, wherein the polymer composition is biodegradable as specified using ASTM standard D5988.
[0097] Embodiment 33. The polymer composition of any one of embodiments 11 to 32, wherein the polymer composition is home compostable as specified using ASTM standard D6868.
[0098] Embodiment 34. The polymeric composition of any one of embodiments 11 to 33, further comprising about 5 to about 50 weight percent of at least one biodegradable polymer selected from the group consisting of poly(caprolactone), poly(ethylene sebacate), poly(butylene succinate), poly(butylene succinate-co-adipate), poly(butylene adipate terephthalate), poly(vinyl acetate), and mixtures thereof.
[0099] Embodiment 35. A molded sheet comprising the polymer composition of any one of embodiments 11 to 34.
[0100] Embodiment 36. A molded article comprising the polymer composition of any one of embodiments 11 to 34, the article being formed by thermoforming, injection molding, or blow molding.
[0101] Embodiment 37. A film comprising the polymer composition of any one of embodiments 11 to 34, wherein the film is a blown film or a cast film.
[0102] Embodiment 38. A fiber comprising the polymer composition according to any one of embodiments 11 to 34. EXAMPLES
[0103] The following non-limiting examples illustrate various additional aspects of the present invention. Unless otherwise stated, temperatures are in degrees Celsius and percentages are weight percent based on the dry weight of the formulation.
[0104] Example 1 A reaction flask equipped with nitrogen inlet and vacuum capability was charged with 800 grams of isosorbide and 5 grams of phosphorous acid. The reaction temperature was increased to 100°C and the flask contents were pulled to full vacuum and then released with an inert gas such as nitrogen for three vacuum cycles. Subsequently, 1279 grams of succinic acid was charged and one more vacuum cycle was performed. The reactor temperature was then increased up to 220°C all the while allowing water to distill off into the receiver. Once the water evolution had subsided, the reactor was charged with 416 grams of propanediol. Again, the temperature was slowly increased up to 210°C. Towards the end of the reaction, 1 gram of tin(II) ethylhexanoate was added and a vacuum was applied. The material was maintained until the appropriate molecular weight specifications were obtained.
[0105] Example 2 A 1514L stainless steel reactor equipped with nitrogen inlet and vacuum capability was charged with 416 kg isosorbide and 2.27 kg phosphorous acid. The reaction temperature was increased to 100°C and the reactor contents were pumped to full vacuum and then released with an inert gas such as nitrogen for three vacuum cycles. 590 kg succinic acid was then charged and one more vacuum cycle was performed. The reactor temperature was then increased to a maximum of 220°C, all the while allowing water to distill off into the receiver. Once water evolution had subsided, the reactor was charged with 216 kg propanediol. Again, the temperature was slowly increased to a maximum of 210°C. Towards the end of the reaction, ethyl hexane was added. Stannous acid, 453 grams, was added. The material was held until the appropriate molecular weight specification was obtained.
[0106] Example 3 A reaction flask equipped with nitrogen inlet and vacuum capability was charged with 575 grams of isosorbide, 888 grams of partially hydrodistilled dimer acid, and 5 grams of phosphorous acid. The reaction temperature was increased to 100°C and the reactor contents were pulled to full vacuum and then released with an inert gas such as nitrogen for three vacuum cycles. Subsequently, 733 grams of succinic acid were charged and one more vacuum cycle was performed. The reactor temperature was then increased up to 220°C, all the while allowing water to distill off into the receiver. Once water evolution had subsided, 299 grams of propanediol were charged to the reactor. Again, the temperature was slowly increased up to 220°C. Towards the end of the reaction, 1 gram of tin(II) ethylhexanoate was added and a vacuum was applied. The material was maintained until the appropriate molecular weight specifications were obtained.
[0107] Example 4 A reaction flask equipped with nitrogen inlet and vacuum was charged with 2314 grams of the polyester of Example 2 and 186 grams of methyl naphthalene anhydride. The reactor temperature was increased to a maximum of 220° C. while water was distilled off into the receiver. Towards the end of the reaction, 0.63 grams of tin(II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.
[0108] Example 5 A reaction flask equipped with nitrogen inlet and vacuum capability was charged with 1,124 grams of 1,6-hexanediol, 548 grams of succinic acid, and 827 grams of methylnaphthalene anhydride. The reactor temperature was then increased to a maximum of 210° C. while water was distilled off into the receiver. Towards the end of the reaction, 0.63 grams of tin(II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.
[0109] Example 6 A reaction flask equipped with nitrogen inlet and vacuum capability was charged with 1,155 grams of 1,6-hexanediol, 563 grams of succinic acid, and 783 grams of nadic anhydride. The reactor temperature was then increased to a maximum of 210° C. while water was distilled off into the receiver. Towards the end of the reaction, 0.63 grams of tin(II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.
[0110] Example 7 A reaction flask equipped with nitrogen inlet and vacuum capability was charged with 1,6-hexanediol, 1191 grams, succinic acid, 871 grams, and 438 grams of methylnaphthalene anhydride. The reactor temperature was then increased to a maximum of 210° C. while water was distilled off into the receiver. Towards the end of the reaction, 0.63 grams of tin(II) ethylhexanoate was added. The material was maintained until the appropriate molecular weight specification was obtained.
[0111] Examples 8 to 20 In each of these examples, a polymer composition was prepared incorporating one of the impact modifier polyesters of Examples 1-7. The polymer compositions were extruded on a 27 mm twin screw Entek kneading extruder. For Examples 8-15, 19, and 20, samples of the extruded material were tested for tensile strength and elongation according to ATSM D638 (Type I specimens) using an Instron 34TM-10. Impact strength testing was performed according to ATSM D256 (Test Method A) using an Instron 9050 testing machine. For Examples 16-18, samples of the extruded material were extruded on an Instron CEAST 9050 Pendulum The Impact System testing apparatus was used to test for resilience according to ASTM D4812-19.
[0112] For each example, a control sample was also prepared, extruded, and tested in the same manner as the test sample. In each example, the composition of the control sample was the same as that of the test sample, except that the impact modifier polyester was omitted from the polymer composition.
[0113] Example 8 In a 27 mm kneading extruder, 42.5 kg of PHA, 453 grams of pentaerythritol, and 172 grams of Joncryl 4468 were added, along with 2.27 kg of the reaction product of Example 1, and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 26,379 kPa (vs. 24,097 kPa for the control); an elongation of 8.9% (vs. 10.6% for the control), and an impact strength of 0.344 J / cm (vs. 0.288 J / cm for the control).
[0114] Example 9 In a 27 mm kneading extruder, 40 kg of PHA, 453 grams of pentaerythritol, and 340 grams of Joncryl 4468 were added, along with 4.53 kg of the reaction product of Example 1, and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 24,242 kPa (vs. 24,097 kPa for the control); an elongation of 11.3% (vs. 10.6% for the control), and an impact strength of 0.408 J / cm (vs. 0.288 J / cm for the control).
[0115] Example 10 In a 27 mm kneading extruder, 40 kg of PHA, 317 grams of Joncryl 4468, and 453 grams of pentaerythritol were added 4.5 kg of the reaction product of Example 1 and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 19,981 kPa (vs. 27,303 kPa for the control); an elongation of 2.2% (vs. 9.3% for the control); and an impact strength of 0.259 J / cm (vs. 0.301 J / cm for the control).
[0116] Example 11 In a 27 mm kneading extruder, 37.6 kg of PHA, 498 grams of Joncryl 4468, and 453 grams of pentaerythritol were added to 6.8 kg of the reaction product of Example 1, and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 26,745 kPa (vs. 27,303 kPa for the control); an elongation of 11.5% (vs. 9.3% for the control), and an impact strength of 0.256 J / cm (vs. 0.301 J / cm for the control).
[0117] Example 12 In a 27 mm kneading extruder, 40.6 kg of PHA and 227 kg of boron nitride were added with 4.53 kg of the reaction product of Example 1 and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 19,960 kPa (vs. 24,097 kPa for the control); an elongation of 11.8% (vs. 10.6% for the control), and an impact strength of 0.232 J / cm (vs. 0.288 J / cm for the control).
[0118] Example 13 In a 27 mm compounder extruder, 42.9 kg of PHA and 227 grams of boron nitride were added to 2.27 kg of the reaction product of Example 6 and the compounder extruder was run. The plastic was tested and had a tensile strength of 16,899 kPa (vs. 24,097 kPa for the control); elongation of 15.5% (vs. 10.6% for the control); and impact strength of 0.275 J / cm (vs. 0.25% for the control). and the control exhibited 0.288 J / cm.
[0119] Example 14 In a 27 mm kneading extruder, 40.6 kg of PHA and 227 grams of boron nitride were added, along with 4.53 kg of the reaction product of Example 6, and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 12,941 kPa (vs. 24,097 kPa for the control); an elongation of 16.6% (vs. 10.6% for the control), and an impact strength of 0.324 J / cm (vs. 0.288 J / cm for the control).
[0120] Example 15 In a 27 mm kneading extruder, 40.6 kg of PHA and 227 grams of boron nitride were added to 4.53 kg of the reaction product of Example 5, and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 19167 kPa (vs. 24097 kPa for the control); an elongation of 18.4% (vs. 10.6% for the control), and an impact strength of 0.277 J / cm (vs. 0.288 J / cm for the control).
[0121] Example 16 In a 27 mm kneader extruder, 42.87 kg of PHA and 227 grams of boron nitride were added to 2.27 kg of the reaction product of Example 6, and the kneader extruder was run. The plastic was tested and had a restoring force of 66.9 kJ / m 2 For comparison, the control is 14.5 kJ / m 2 It was.
[0122] Example 17 In a 27 mm kneader extruder, 40.6 kg of PHA and 227 grams of boron nitride were added to 4.53 kg of the reaction product of Example 6, and the kneader extruder was run. The plastic was tested and had a restoring force of 67.1 kJ / m 2 For comparison, the control is 14.5 kJ / m 2 It was.
[0123] Example 18 In a 27 mm kneader extruder, 40.6 kg of PHA and 227 grams of boron nitride were added to 4.53 kg of the reaction product of Example 7, and the kneader extruder was run. The plastic was tested and had a restoring force of 39.5 kJ / m 2 For comparison, the control is 14.5 kJ / m 2 It was.
[0124] Example 19 In a 27 mm kneader extruder, 40.6 kg of PHA and 227 grams of boron nitride were added to 4.53 kg of the reaction product of Example 4, and the kneader extruder was run. The plastic was tested and had a restoring force of 11.1 kJ / m 2 For comparison, the control is 2.34 kJ / m 2 It was.
[0125] Example 20 In a 27 mm kneading extruder, 44 kg of PHA and 1.36 kg of the reaction product of Example 3 were added and the kneading extruder was run. The plastic was tested and exhibited a tensile strength of 1386 kPa (vs. 1572 kPa for the control), an elongation of 5.3% (vs. 5.6% for the control), and an impact strength of 0.167 J / cm (vs. 0.301 J / cm for the control).
[0126] From the above, it can be seen that impact modified polyesters according to the present disclosure can provide a wide variety of mechanical property improvements over bioplastic systems. For example, a four-fold increase in impact strength or an 11% increase in elongation can be achieved without a corresponding loss in tensile strength. That is, the impact modified polyesters of the present disclosure allow the mechanical properties of the bioplastic system to be tailored to the specific end use application.
[0127] The foregoing description of preferred embodiments of the present invention has been presented for purposes of illustration and description. They are not intended to be exhaustive or to limit the invention to the precise forms disclosed. Obvious modifications or variations are possible in light of the above teachings. The embodiments have been chosen and described in an effort to provide the best explanation of the principles of the invention and its practical application, thereby enabling those skilled in the art to utilize the invention in various embodiments with various modifications as suited to particular intended uses. All such modifications and variations are within the scope of the present invention, as defined by the appended claims, when interpreted in accordance with the breadth to which they are fairly, legally, and equitably entitled.
Claims
1. A polyester comprising: from about 15 to about 40 weight percent isosorbide monomer repeat units, based on the total weight of the polyester; from about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, based on the total weight of the polyester; and from about 10 to about 20 weight percent polyhydric alcohol monomer repeat units, based on the total weight of the polyester; having a weight average molecular weight of at least 8000 Daltons as specified by ASTM D5296-05; The dicarboxylic acid or dicarboxylic anhydride includes a mixture of (1) succinic acid or succinic anhydride, and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof; The polyester.
2. 2. The polyester of claim 1, wherein the polyester comprises from about 25 to about 35 weight percent succinic acid or succinic anhydride, and from about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
3. 2. The polyester of claim 1, wherein the polyhydric alcohol is selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and poly(oxyalkylene) polyols containing ethylene oxide, propylene oxide, or butylene oxide monomer repeat units, and mixtures thereof.
4. 2. The polyester of claim 1, wherein the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof.
5. The polyester of claim 1 , wherein the polyhydric alcohol comprises 1,3-propanediol.
6. 10. The polyester of claim 1, wherein the polyester has a weight average molecular weight of about 10,000 to about 15,000 Daltons as specified by ASTM D5296-05.
7. 1. A polymer composition comprising: from about 50 to about 95 weight percent of a biodegradable polymer selected from the group consisting of poly(lactic acid), poly(hydroxyalkanoates), and mixtures thereof; and from about 5 to about 50 weight percent of an impact modified polyester; The impact-modified polyester is from about 15 to about 40 weight percent isosorbide monomer repeat units, based on the total weight of the polyester; from about 25 to about 60 weight percent dicarboxylic acid or dicarboxylic anhydride monomer repeat units, based on the total weight of the polyester; and from about 10 to about 20 weight percent polyhydric alcohol monomer repeat units, based on the total weight of the polyester; the polyester has a weight average molecular weight of at least 8000 Daltons as specified by ASTM D5296-05; The dicarboxylic acid or dicarboxylic anhydride includes a mixture of (1) succinic acid or succinic anhydride, and (2) nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid, and mixtures thereof; The polymer composition.
8. 8. The polymer composition of claim 7, wherein the polyester comprises about 25 to about 35 weight percent succinic acid or succinic anhydride and about 10 to about 25 weight percent nadic anhydride, methyl nadic anhydride, C36 dimer acid, or partially hydrogenated C36 dimer acid.
9. 8. The polymer composition of claim 7, wherein the polyhydric alcohol is selected from the group consisting of glycerin, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl, neopentyl glycol, propylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, trimethylene glycol, 1,1,1-trimethylolethane, 1,2,3-trimethylolpropane, methylpropanediol, pentaerythritol, and poly(oxyalkylene) polyols containing ethylene oxide, propylene oxide, or butylene oxide monomeric repeat units, and mixtures thereof.
10. 8. The polymer composition of claim 7, wherein the polyhydric alcohol is selected from the group consisting of 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, methylpropanediol, and mixtures thereof.
11. The polymer composition of claim 7, wherein the polyhydric alcohol comprises 1,3-propanediol.
12. 8. The polymer composition of claim 7, wherein said impact modified polyester has a weight average molecular weight of 10,000 to 15,000 Daltons as specified by ASTM D5296-05.
13. 8. The polymeric composition of claim 7, wherein the polymeric composition comprises about 60 to about 85 weight percent of the biodegradable polymer, and about 5 to about 30 weight percent of the impact modified polyester.
14. The polymer composition of claim 7 , wherein the biodegradable polymer comprises poly(lactic acid).
15. The polymer composition of claim 7 , wherein the biodegradable polymer comprises at least one poly(hydroxyalkanoate).
16. 16. The polymer composition of claim 15, wherein said at least one poly(hydroxyalkanoate) comprises poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)").
17. 17. The polymer composition of claim 16, wherein the P(3HB-co-3HHx) comprises from about 75 to about 99 mole percent hydroxybutyrate and from about 1 to about 25 mole percent hydroxyhexanoate.
18. 17. The polymer composition of claim 16, wherein the P(3HB-co-3HHx) comprises from about 93 to about 98 mole percent hydroxybutyrate and from about 2 to about 7 mole percent hydroxyhexanoate.
19. 16. The polymer composition of claim 15, wherein the at least one poly(hydroxyalkanoate) comprises a terpolymer made of about 75 to about 99.9 mole percent 3-hydroxybutyrate monomer repeat units, about 0.1 to about 25 mole percent 3-hydroxyhexanoate monomer repeat units, and about 0.1 to about 25 mole percent of a third 3-hydroxyalkanoate monomer repeat unit having from about 5 to about 1 to about 2 carbon atoms.
20. 16. The polymer composition of claim 15, wherein the at least one poly(hydroxyalkanoate) has a weight average molecular weight of from 50,000 Daltons to 2.5 million Daltons as specified by ASTM D5296-05.
21. 16. The polymer composition of claim 15, wherein the at least one poly(hydroxyalkanoate) has a weight average molecular weight of from 500,000 Daltons to 750,000 Daltons as specified by ASTM D5296-05.
22. 8. The polymeric composition of claim 7, wherein the polymeric composition comprises about 5 to about 25 weight percent of poly(lactic acid) and about 70 to about 90 weight percent of the at least one poly(hydroxyalkanoate), based on a total weight of the polymeric composition.
23. In addition: from about 1 to about 10 weight percent of at least one plasticizer; from about 0.1 to about 5 weight percent of at least one nucleating agent; and about 0.1 to about 10 weight percent of a bulking agent; The polymer composition of claim 7 comprising:
24. 8. The polymer composition of claim 7, wherein the polymer composition is biodegradable as specified using ASTM standard D5988.
25. 8. The polymer composition of claim 7, wherein the polymer composition is home compostable as specified using ASTM standard D6868.
26. 8. The polymeric composition of claim 7, further comprising from about 5 to about 50 weight percent of at least one biodegradable polymer selected from the group consisting of poly(caprolactone), poly(ethylene sebacate), poly(butylene succinate), poly(butylene succinate-co-adipate), poly(butylene adipate terephthalate), poly(vinyl acetate), and mixtures thereof.
27. A molded sheet comprising the polymer composition of claim 7.
28. 10. A molded article comprising the polymer composition of claim 7, said article being formed by thermoforming, injection molding, or blow molding.
29. 10. A film comprising the polymer composition of claim 7, the film being a blown film or a cast film.
30. A fiber comprising the polymer composition of claim 7.