Liquid-applied sound deadening mat for flooring and composition for making same
A sound deadening mat using a polymer foam matrix with crosslinked rubber and inorganic aggregates addresses the limitations of conventional materials, offering effective sound insulation and durability in residential flooring applications.
Patent Information
- Application Number
- JP2024510717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-09-15
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024535991000008 
Figure 2024535991000001 
Figure 2024535991000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubbery composite mat for flooring and underlayment comprising a polymer foam matrix of A) one or more rigid vinyl or acrylic water-based emulsion polymers, preferably acrylic or styrene acrylate water-based emulsion polymers, and B) one or more flexible vinyl or acrylic water-based emulsion polymers, preferably acrylic or styrene acrylate water-based emulsion polymers, and dispersed therein, C) a combination of (i) particulate inorganic aggregate and (ii) particulate and pulverulent crosslinked rubber particles, and a trowelable water-based composition comprising the aqueous emulsion polymers A) and B) in the foam and the granular and pulverulent rubber particles. More specifically, the present invention relates to a polymer foam matrix of A) one or more hard acrylic or styrene acrylate aqueous emulsion polymers, and B) one or more soft acrylic or styrene acrylate aqueous emulsion polymers, further comprising (i) a foam stabilizer of an organic acid salt having 12 to 24 carbon atoms, e.g., a calcium fatty acid salt, and (ii) an organic blowing agent, e.g., an alkyl polyglucoside, dispersed in the polymer foam matrix. C) (i) A polymer foam matrix having a sieve particle size of 0.3 to 4 mm and a sieve particle size of 0.18 to 0.4 g / cm. 3 and (ii) a combination of granular and pulverulent crosslinked rubber particles, and a trowelable aqueous composition comprising the polymer foam and the granular and pulverulent rubber particles. The invention further relates to a method of using the trowelable aqueous composition, comprising: C) mixing, as one component, (i) the inorganic aggregate, and (ii) the granular or pulverulent crosslinked rubber particles or a combination thereof with another aqueous component comprising a foam of the aqueous emulsion polymers A) and B) to make a trowelable mixture or mortar, and applying the mortar to a substrate such as concrete or an underlayment.
[0002] Introduction Sound insulation is a growing need in structures such as multi-family residential building structures. Noise pollution can contribute to illnesses including stress-related diseases, high blood pressure, hearing loss, sleep disorders, and loss of productivity. In particular, noise from upper floors of buildings with multiple floors, especially sounds caused by high heels, chairs, falling objects, etc., have proven to be a major source of noise pollution. Currently, noise pollution is gradually being regulated as it negatively affects the lives of millions of people around the world. In parts of China, floating floors have been required to have a layer of sound-deadening material in recent years to achieve the standards of relevant codes in residential construction. Furthermore, traditional sound insulation materials used in the market, such as various polystyrene foams, e.g., EPS foam or XPS foam materials, glass fiber wool, and precast polyurethane foam mats, pose many challenges, including issues regarding leveling, cracks, odor and toxic gases, and volatile organic compounds (VOC) emissions, as well as the need for additional joint treatment for precast mats, the presence of sound bridges, etc.
[0003] WO 2015051526(A1) to Dow Global Technologies LLC discloses a multi-layer article for use in surfacing a running track, where each of the top and base layers includes a layer of an acrylic emulsion polymer having a measured glass transition temperature (measured Tg) of −5° C. or less, a second harder acrylic emulsion polymer having a measured Tg of 15° C. or more, a crosslinker, and vulcanized or crosslinked rubber particles having a sieve size of 0.1 to 6 mm. The compositions used to form the layers of the multi-layer article are not storage stable, lack the porosity to provide acceptable indoor sound deadening, and it is not possible to achieve a low toxicity and odorless composition that can be used indoors.
[0004] The inventors have sought to provide a seamless, low odor sound deadening mat suitable for use in residential flooring, and to provide a storage stable, low VOC water based or aqueous composition, such as a two-component aqueous composition, for making the sound deadening mat that can be safely mixed, applied and used on-site. Summary of the Invention
[0005] In accordance with the present invention, a trowelable aqueous composition of an aqueous polymeric foam-forming component and a rubbery composite component is provided comprising: As the aqueous polymer foam forming component, A) 10-60% by weight, preferably 15-50% by weight, of one or more rigid vinyl or acrylic aqueous emulsion polymers, preferably acrylic or styrene acrylate aqueous emulsion polymers, having a measured glass transition temperature (measured Tgh) of 5-40°C, or preferably 10-35°C, or preferably 15-30°C, when measured by differential scanning calorimetry (DSC) comprising heating to 160°C, rapidly cooling to -80°C at 10°C / min, then increasing the temperature at 10°C / min to 160°C while collecting DSC curve data and recording the midpoint of the inflection of the resulting DSC curve as Tgh; B) 5 to 50% by weight, preferably 7 to 40% by weight, of one or more soft vinyl or acrylic aqueous emulsion polymers, preferably acrylic or styrene acrylate aqueous emulsion polymers, having a measured glass transition temperature (measured Tgs) of 5 to -35°C, or preferably -8 to -35°C, or preferably -10 to -25°C, or preferably -10 to -17°C, when measured by differential scanning calorimetry (DSC) which involves heating to 160°C, rapidly cooling at 10°C / min to -80°C, then increasing the temperature at 10°C / min to 160°C while collecting DSC curve data and recording the midpoint of the inflection of the resulting DSC curve as the Tgs; C) (i) 0.5 to 3% by weight of a foam stabilizer of an organic acid salt having 12 to 24 carbon atoms, such as a calcium fatty acid salt, preferably calcium stearate; and (ii) 0.05 to 0.75% by weight or preferably 0.1 to 0.5% by weight of an organic foaming agent, preferably an alkyl polyglucoside. As the rubber composite component, D) (i) 20-60% by weight, or preferably 20-48% by weight, of the sieve particle size of 0.3-4 mm, or 0.3-3 mm, or preferably 0.5-2.5 mm, and having a particle size of 0.18-0.4 g / cm3 Or preferably 0.24 to 0.37 g / cm 3 a lightweight inorganic aggregate, such as porous light sand, mesoporous silica, mesostructured silica, or expanded clay aggregate, having a density of D) (ii) 20-60% or 20-48% by weight of (a) crosslinked rubber granules having a sieve size of 0.5-4 mm, or 0.5-3 mm, or for example 0.5-2.5 mm, preferably ethylene propylene diene (EPDM) rubber or ethylene propylene (EPM) rubber granules, or (b) crosslinked rubber particles having a sieve size of less than 0.1-0.5 mm, preferably EPDM or EPM rubber powder, or preferably a mixture of (a) granular crosslinked rubber particles and (b) finely divided crosslinked rubber particles, for example in a weight ratio of (a):(b) of 99:1 to 20:80, Including, All weight percentages in the trowelable aqueous composition add up to 100% and are based on the total weight of all materials used to form the trowelable aqueous composition. Further, the weight ratio of rubbery composite components to aqueous polymeric foam forming components may range from 1:3 to 2:1, or such as from 1:2 to 2:1. Still further, the solids weight ratio of total A) rigid vinyl or acrylic aqueous emulsion polymers to total B) flexible vinyl or acrylic aqueous emulsion polymers may range from 2:3 to 6:1, or preferably from 3:2 to 5:1. Preferably, the weight ratio of D)(i) lightweight inorganic aggregate to the total weight of aqueous emulsion polymers A) and B) in the trowelable aqueous composition is 1:1 or less, such as in the range of 1:4 to 1:1.
[0006] The trowelable aqueous composition according to the present invention may further comprise, in the aqueous polymeric foam-forming components, 0.1 to 1.5 wt. % of one or more thickeners, such as anionic thickeners or preferably hydrophobically modified anionic thickeners; or 0.1 to 1.5 wt. % of one or more dispersants, such as sodium polycarboxylate dispersants; or any combination thereof. Still further, the trowelable aqueous composition may comprise added water, for example, in an amount of 10 to 50 wt. %, or 20 to 50 wt. %, based on the total weight of all materials used to form the trowelable aqueous composition. Water may be added to the aqueous polymeric foam-forming components to improve their processability.
[0007] Preferably, the measured Tg of A) the rigid vinyl or acrylic aqueous emulsion polymer (measured Tgh) and the measured Tg of B) the flexible vinyl or acrylic aqueous emulsion polymer (measured Tgs) differ by at least 15° C., such as from 15 to 75° C., or preferably by at least 20° C. The trowelable aqueous composition according to the present invention may further comprise, in the rubbery composite component, 0 to 10 wt % of wood fibers or palm fibers or a combination thereof, such as any one or more of wood fibers and / or palm fibers having an average length of less than 12 mm.
[0008] In another aspect of the present invention, a rubber-like composite sound deadening mat for flooring and underlayment comprises: A) 10-60% by weight or preferably 15-50% by weight of one or more rigid vinyl or acrylic aqueous emulsion polymers, preferably acrylic or styrene acrylate aqueous emulsion polymers, having a measured glass transition temperature (measured Tgh) of 5-40°C, or preferably 10-35°C, or preferably 15-30°C, when measured by differential scanning calorimetry (DSC) comprising heating to 160°C, rapidly cooling to -80°C at 10°C / min, then increasing the temperature at 10°C / min to 160°C while collecting DSC curve data and recording the midpoint of the inflection of the resulting DSC curve as Tgh; and B) 3-35% by weight of one or more rigid vinyl or acrylic aqueous emulsion polymers, preferably acrylic or styrene acrylate aqueous emulsion polymers, having a measured glass transition temperature (measured Tgh) of 5-40°C, or preferably 10-35°C, or preferably 15-30°C, when measured by differential scanning calorimetry (DSC) comprising heating to 160°C, rapidly cooling to -80°C at 10°C / min, then increasing the temperature at 10°C / min to 160°C, % by weight or preferably 5 to 32% by weight of one or more soft vinyl or acrylic aqueous emulsion polymers, preferably acrylic or styrene acrylate aqueous emulsion polymers, having a measured glass transition temperature (measured Tgs) of 5 to -35°C, or preferably -8 to -35°C, or preferably -10 to -25°C, or preferably -10 to -17°C, when measured by differential scanning calorimetry (DSC) comprising heating to 160°C, rapidly cooling at 10°C / min to -80°C, then increasing the temperature at 10°C / min to 160°C while collecting DSC curve data and recording the midpoint of the inflection of the resulting DSC curve as the Tg. A polymer foam matrix comprising: C) (i) 0.5 to 5% by weight of a foam stabilizer of an organic acid salt having 12 to 24 carbon atoms, such as a calcium fatty acid salt, and (ii) 0.05 to 1% by weight or preferably 0.1 to 0.75% by weight of an organic foaming agent, such as an alkyl polyglucoside. a polymer foam matrix, Dispersed in the polymer foam matrix are 30-70 or preferably 35-60 wt. % of D)(i) 25-75 wt. % or 25-65 wt. % of the polymer foam matrix having a sieve size of 0.3-4 mm, or 0.3-3 mm, or preferably 0.5-2.5 mm, and a density of 0.18-0.4 g / cm. 3 , or preferably 0.24 to 0.37 g / cm 3D) (ii) 25 to 75% by weight or 25 to 65% by weight of (a) crosslinked rubber granules having a sieve size of 0.5 to 4 mm, or 0.5 to 3 mm, or preferably 0.5 to 2.5 mm, preferably ethylene propylene diene (EPDM) rubber or ethylene propylene (EPM) rubber granules, or (b) finely divided crosslinked rubber particles having a sieve size of less than 0.1 to 0.5 mm, preferably EPDM rubber or EPM rubber powder, or a mixture of (a) granular crosslinked rubber particles and (b) finely divided crosslinked rubber particles, for example in a weight ratio (a):(b) of 99:1 to 20:80 (a). Including, All weight percentages in the polymer foam matrix add up to 100% and are based on the total weight of materials used to form the polymer foam matrix; Additionally, all weight percentages in the rubbery composite add up to 100% and are based on the total weight of materials used to form the rubbery composite.
[0009] Preferably, when the rubbery composite component of the trowelable aqueous composition or sound deadening mat comprises a mixture of D)(ii) crosslinked rubber (a) granules and (b) pulverulent crosslinked rubber particles, the weight ratio of D)(ii)(a) granular crosslinked rubber particles and D)(ii)(b) pulverulent crosslinked rubber particles may be in the range of 12:1 to 1:2, or preferably 4:1 to 1:1.2.
[0010] In yet another aspect, the present invention further comprises: D) (i) mixing an inorganic aggregate with D) (ii) (a) the mixture of granular crosslinked rubber and (b) the pulverulent crosslinked rubber particles to form a rubber-like composite component; mixing, or preferably mixing and shearing, mixing and stirring, or a combination of mixing, shearing, and stirring, the aqueous emulsion polymers A) and B), C)(i) a foam stabilizer, and C)(ii) an organic blowing agent to form an aqueous polymeric foam forming component; combining the rubbery composite component and the aqueous polymeric foam forming component to form a trowelable mixture; applying the trowelable mixture to a substrate, such as concrete or an underlayment, to form a mat layer; The method may further include drying or curing the matte layer, such as by allowing the matte layer to stand, preferably without heating, for 20 to 60 hours.
[0011] In the process according to the invention, the weight ratio of rubbery composite components to aqueous polymeric foam forming components, regardless of solids content, may range from 1:3 to 2:1, or such as from 1:2 to 2:1. Thus, the materials are mixed, poured or spread, and then dried or cured. [Brief description of the drawings]
[0012] [Figure 1] 1 shows an example of an acoustic impedance tube test setup used to test sound deadening mats made in accordance with the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] According to the present invention, a sound-absorbing mat that provides suitable compression resistance for use in flooring applications includes an aqueous acrylic or vinyl polymer foam-forming matrix component and a dispersion composite of lightweight aggregate and at least one or a mixture of crosslinked rubber granules and crosslinked rubber powder. The sound-absorbing mat is made from a material that exhibits good sound absorption in impact sound and acoustic impedance tests, has low compression, provides some insulation, has low odor, and is low toxicity. The mat itself is continuous and formed similarly to a mortar layer and can be made into any desired shape. Thus, the mat is seamless, with all surfaces, boundaries, and edges completely sealed, leaving no or no sound bridging. Since these materials are water-based, they are not flammable during use. However, the sound-absorbing mat itself is completely dry and water-repellent, resulting in a relatively low water absorption rate and low risk of molding and decay problems.
[0014] Unless otherwise indicated, temperature and pressure conditions are room temperature (23±2° C.) and standard pressure (101.3 kPa), also referred to as "ambient conditions." Additionally, all conditions include 50±10% relative humidity (RH) unless otherwise indicated.
[0015] Unless otherwise indicated, any term containing parentheses alternatively refers to the entire term as if the parentheses were not present, and the term without the parentheses, and combinations of each alternative. Thus, the term "(meth)acrylate" refers independently to an acrylate, a methacrylate, a mixture or combination thereof, or a combination of two or more of these.
[0016] The singular terms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Unless otherwise specified, terms used herein have the same meaning as commonly understood by one of ordinary skill in the art.
[0017] All ranges are inclusive and combinable, for example the term "measured Tg of 5-40°C, or preferably 10-35°C, or preferably 15-30°C" would include each of 5-40°C, or 10-40°C, or 5-35°C, or 5-30°C, or 5-15°C, or 5-10°C, or preferably 10-35°C, or preferably 10-30°C, or preferably 10-15°C, or preferably 15-40°C, or preferably 15-30°C, or preferably 15-35°C, or preferably 30-40°C, or preferably 30-35°C, or preferably 35-40°C.
[0018] As used herein, the term "aqueous" refers to a carrier or solvent that includes water and one or more water-miscible organic solvents, such as alkyl ethers, up to 10% by weight of the total solvent or carrier.
[0019] As used herein, the term "ASTM" refers to publications of ASTM International, West Conshohocken, PA.
[0020] As used herein, the term "BS EN", including number and publication date, refers to engineering standards published by BSI Standards Limited, 389 Chiswick High Road, London, W4 4AL, UK.
[0021] As used herein, the terms "GB" or "GB / Z" or "GB / T", including number and publication date, refer to various Chinese national standards published by China Standards Press, No. 2A, West Heping Street, Chaoyang District, Beijing 100029, China.
[0022] As used herein, the term "calculated glass transition temperature" or "calculated Tg" means a value calculated using the following Fox equation (Fox, Bull. Am. Physics Soc., Volume 1, Issue No. 3, page 123 (1956)): 1 / Tg(calculation)=Σ w(M1) / Tg(M1)+w(M2) / Tg(M2)+...w(M n ) / Tg(M n ) where Tg(calculated) is the calculated glass transition temperature for the copolymer; w(M1) is the weight fraction of monomer M1 in the copolymer, w(M2) is the weight fraction of monomer M2 in the copolymer; w(M n ) is the weight fraction of monomer Mn in the copolymer, Tg(M1) is the glass transition temperature of the homopolymer of M1; Tg(M2) is the glass transition temperature of the homopolymer of M2; Tg(M n ) is the glass transition temperature of the Mn homopolymer, All temperatures are in °K.
[0023] The glass transition temperatures of homopolymers can be found, for example, in Polymer Handbook, edited by J. Brandrup and EH Immergut, Wiley Interscience Publishers, New York, 1999 at pages VI / 193-277.
[0024] As used herein, the term "measured Tg" refers to the glass transition temperature or Tg of a given polymer composition as measured by differential scanning calorimetry (DSC) using, for example, a TA Instruments Q2000 (TA Instruments, New Castle, Del.) calorimeter, where a sample of the polymer composition was heated to 160° C., rapidly cooled to −80° C. at 10° C. / min, and then the temperature was increased at 10° C. / min to 160° C. while data was collected, and the midpoint of the inflection of the resulting DSC curve was recorded as the Tg.
[0025] As used herein, the term "polymer" refers to a polymeric compound prepared by reacting (i.e., polymerizing) monomers of the same or different types, including both homopolymers and interpolymers of all kinds. The term "copolymer" refers to a polymer prepared by polymerization of at least two different monomers as reactants, including copolymers prepared from two different monomers, as well as polymers prepared from more than two different monomers, such as terpolymers, tetrapolymers (four different monomers), etc. As used herein, the term "homopolymer" refers to a polymer that contains repeat units derived from a single monomer, but does not exclude residual amounts of other components used in the preparation of the homopolymer, such as chain transfer agents.
[0026] As used herein, the term "solids" or "total solids" refers to any material that does not volatilize during the curing or application of the composition according to the present invention, regardless of its state of matter. Water, ammonia, non-reactive volatile substances, liquid carriers, and volatile solvents are not considered to be solids. Furthermore, unless otherwise specified, the term "solids", when referring to an individual substance, refers to a crystalline or amorphous substance that does not flow appreciably under moderate stress, has a definite ability to resist forces that tend to deform it, and retains a definite size and shape under normal conditions.
[0027] As used herein, the term "substantially free of volatile organic compounds" means that the composition contains only organic solvents, including amines, ethers, glycols, and all other organic solvents in a given composition, in a total amount of less than 100 g / L or 100 g / kg, or preferably less than 50 g / L or 50 g / kg, based on the total weight of the composition.
[0028] The aqueous polymer foam forming components include A) a blend of one or more rigid vinyl or acrylic aqueous emulsion polymers with rigid vinyl or acrylic aqueous emulsion polymers. The combination of the rigid and flexible polymers allows for the rapid formation of a foam with sufficient elasticity to provide a foam that will not collapse in flooring applications.
[0029] The vinyl or acrylic emulsion polymers useful in the present invention may contain one or more copolymerized ethylenically unsaturated nonionic vinyl or acrylic monomers. As used herein, the term "nonionic monomer" refers to a polymerizable monomer that does not have an ionic charge at pH=1-14. Examples of suitable ethylenically unsaturated nonionic monomers are selected from the group consisting of (meth)acrylic acid ester monomers and arylene monomers such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, nonyl methacrylate, isodecyl methacrylate, lauryl methacrylate, hydroxyethyl methacrylate, 1,3-butanediol dimethacrylate, and hydroxypropyl methacrylate; styrene and alkyl-substituted styrenes; (meth)acrylamide; (meth)acrylonitrile; or mixtures thereof. The ethylenically unsaturated nonionic monomer preferably comprises a (meth)acrylic acid ester monomer, or a combination thereof with styrene.
[0030] The hard vinyl or acrylic emulsion polymers A) useful in the present invention may comprise, in polymerized form, a total of 70% or more, or 75% or more, or 80% or more, or 99.5% or less, 95% or less, or 90% or less by weight of any one or more copolymerized nonionic monomers, based on the solids weight of the emulsion polymer A). The soft vinyl or acrylic emulsion polymers B) useful in the present invention may comprise, in polymerized form, a total of 70% or more, or 75% or more, or 80% or more, or 99.5% or less, 95% or less, or 90% or less by weight of any one or more copolymerized nonionic monomers, based on the solids weight of the emulsion polymer B).
[0031] The hard and soft vinyl or acrylic emulsion polymers A) and B) useful in the present invention may each contain one or more copolymerized ethylenically unsaturated monomers having one or more functional groups. The functional groups may be selected from carboxyl, carboxylate, carbonyl, acetoacetate, alkoxysilane, carboxyl, ureido, amide, imide, amino groups, or mixtures thereof. Preferably, ethylenically unsaturated monomers having carboxyl or carboxylate groups are used, such as methacrylic acid or its salts. Examples of suitable functional group-containing ethylenically unsaturated monomers include ethylenically unsaturated carboxylic acids or dicarboxylic acids such as acrylic acid or methacrylic acid, itaconic acid, and maleic acid; amides, preferably N-alkylamides or hydroxyalkyl esters of the above carboxylic acids, such as acrylamide, methacrylamide, N-methylol acrylamide, N-methylol methacrylamide, 2-hydroxyethyl acrylamide, 2-hydroxyethyl methacrylamide, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, and hydroxypropyl methacrylate; or mixtures thereof. Adhesion-promoting functional groups can include, for example, acetoacetate, alkoxysilane, carboxyl, ureido, or amino groups.
[0032] The rigid vinyl or acrylic emulsion polymers A) useful in the present invention may contain, in polymerized form, a total of 0.01% or more, or 0.05% or more, or 0.1% or more, or 20% or less, 10% or less, or 5% or less by weight of any one or more copolymerized functional group-containing ethylenically unsaturated monomers, based on the solids weight of the emulsion polymer A).
[0033] The flexible vinyl or acrylic emulsion polymers B) useful in the present invention may contain, in polymerized form, a total of 0.01% or more, or 0.05% or more, or 0.1% or more, or 20% or less, 10% or less, or 5% or less by weight of any one or more copolymerized functional group-containing ethylenically unsaturated monomers, based on the solids weight of the emulsion polymer B).
[0034] Preferably, each of the hard vinyl or acrylic emulsion polymer A) and the soft vinyl or acrylic emulsion polymer B) comprises in polymerized form a total of 70 to 99.5 weight percent of one or more copolymerized ethylenically unsaturated nonionic monomers and a total of 0.5 to 10 weight percent of one or more copolymerized ethylenically unsaturated monomers having one or more functional groups, based on the solids weight of polymer A) or B), respectively.
[0035] The aqueous emulsion polymers A) and B) useful in the present invention can be prepared by polymerization techniques well known in the art, preferably by aqueous free radical emulsion polymerization. Suitable aqueous emulsion polymerization techniques are well known in the polymer art and include multi-stage polymerization processes. For a given monomer, the proportion of monomer based on the total weight of monomer used in preparing the aqueous dispersion of acrylic (co)polymer is substantially the same as the proportion of such monomer copolymerized based on the solids weight of acrylic (co)polymer. One suitable aqueous emulsion polymerization method includes the use of a surfactant. Suitable surfactants can include, for example, sodium laureth sulfate, sodium alkyl sulfosuccinate, or alkyl alcohol alkoxylate. The amount of surfactant used is in the range of 0.01 wt% or more, 0.3 wt% or more, or even 0.5 wt% or more, and at the same time 10 wt% or less, 5 wt% or less, or even 2 wt% or less, based on the total weight of monomer used to make a given polymer.
[0036] In order to control the molecular weight of the resulting emulsion polymer, the emulsion polymerization may be carried out in the presence of a chain transfer agent. Examples of suitable chain transfer agents include 3-mercaptopropionic acid, dodecyl mercaptan, methyl 3-mercaptopropionate, benzenethiol, alkyl mercaptan azelate, or mixtures thereof. The concentration of the chain transfer agent may be in the range of 0.01% by weight or more, 0.05% by weight or more, or even 0.1% by weight or more, or 5% by weight or less, 3% by weight or less, or 2% by weight or less, based on the total weight of the monomers used to make the emulsion polymer.
[0037] The aqueous emulsion polymers A) and B) may have a solids content in the range of 30% by weight or more, 35% by weight or more, or 40% by weight or more, or 70% by weight or less, 68% by weight or less, or 65% by weight or less, based on the total weight of the emulsion.
[0038] Rigid vinyl or acrylic emulsion polymers A) useful in the present invention may have a measured Tgh of 5° C. or more, 10° C. or more, 15° C. or more, or 50° C. or less, 35° C. or less, or 30° C. or less. Suitable commercially available rigid vinyl or acrylic emulsion polymers A) can include, for example, RHOPLEX™ 2500 acrylic emulsion available from The Dow Chemical Company.
[0039] Flexible vinyl or acrylic emulsion polymers B) useful in the present invention may have a measured Tgs of -5° C. or less, or -8° C. or less, or -10° C. or less, while at the same time being -50° C. or more, -35° C. or more, or -17° C. or more. Suitable commercially available flexible vinyl or acrylic emulsion polymers B) can include, for example, ELASTENE™ 2848NG, RHOPLEX™ EC-1791, and PHOPLEX™ EC-2540 acrylic emulsions, all available from The Dow Chemical Company (ELASTENE and PHOPLEX are trademarks of The Dow Chemical Company).
[0040] To improve the durability of the foam in the mortar upon application, the aqueous polymeric foam forming component further comprises one or more foam stabilizers such as C)(i) a calcium stearate water emulsion, or a salt of a fatty acid having 12 to 18 carbon atoms, or a mixture of aliphatic carboxylic acids having about 16 to 20 carbon atoms (especially when the acid is saturated, e.g., sodium or potassium stearate), and salts of fatty acids having 12 to 24 carbon atoms, such as oleic acid, tallow fatty acid, and tall oil fatty acid. The total amount of C)(i) the one or more foam stabilizers may range from 0.5 to 3 weight percent, based on the total weight of all materials used to form the trowelable aqueous composition.
[0041] To form an air-entraining matrix or foam, the aqueous polymeric foam-forming component further comprises C)(ii) one or more organic blowing agents, such as an alkyl polyglucoside blowing agent, an alkyl sulfonate, such as sodium alkyl sulfonate or sodium alkyl benzene sulfonate, or mixtures thereof. The C)(ii) organic blowing agent forms a foam of the aqueous emulsion polymer composition upon shearing and / or stirring of the composition. The total amount of C)(ii) organic blowing agent may range from 0.05 to 0.75 wt.%, such as 0.05 to 0.5 wt.%, or preferably 0.1 to 0.5 wt.%, based on the total weight of all materials used to form the trowelable aqueous composition.
[0042] To maintain consistency and homogeneity in the trowelable aqueous composition of the present invention, one or more thickeners may be included, such as hydrophobically modified anionic thickeners, hydrophobically modified alkali swellable emulsions (HASEs), hydrophobically modified acrylic copolymers such as ACRYSOL™ TT935 (Dow). The hydrophobically modified acrylic copolymers contain two or more hydrophobic groups, such as aryl or phenyl groups, or C4 or higher alkyl groups. The total amount of the one or more thickeners may range from 0.05 to 1.5% by weight, such as 0.1 to 1.5% by weight, based on the total weight of all materials used to form the trowelable aqueous composition.
[0043] To improve the homogeneity of the trowelable aqueous composition, the aqueous polymeric foam forming components may further include one or more dispersants, such as an alkali metal polycarboxylate, e.g., sodium polyacrylate. A suitable sodium polymethacrylate dispersant is sold as OROTAN™ 1850E (Dow). The total amount of the one or more dispersants may range from 0.05 to 1.5% by weight, e.g., 0.1 to 1.5% by weight, based on the total weight of all materials used to form the trowelable aqueous composition.
[0044] To improve the overall workability of the trowelable aqueous composition of the present invention, a small amount of water may be added to the aqueous polymeric foam forming components when mixed with the rubbery composite components. The amount of water added may range from 0 to 50% by weight, based on the total weight of all materials used to form the trowelable aqueous composition.
[0045] The rubber-like composite component of the trowelable aqueous composition of the present invention includes D)(i) a lightweight inorganic aggregate that allows for durable porosity in sound deadening mats made therefrom. Suitable porous lightweight aggregates can include, for example, light sand, or sintered silicates or clays. D)(i) a lightweight inorganic aggregate has a density of 180 to 400 kg / m 3 (0.18~0.4g / cm 3 ) or 240~370kg / m 3 (0.24~0.37g / cm 3 ). Suitable lightweight mineral aggregates may have a sieve size of 0.3 to 4 mm, or 0.3 to 3 mm, or 0.3 to 2.5 mm, or 0.7 to 2 mm, or preferably 0.5 to 2.5 mm. D) (i) The total amount of lightweight mineral aggregates may range from 15 to 60% by weight, or 20 to 60% by weight, or preferably 25 to 55% by weight, or preferably less than 25 to 50% by weight, based on the total weight of all materials used to form the trowelable aqueous composition.
[0046] The rubbery composite component further comprises D)(ii) pulverulent crosslinked rubber particles as particles or fines, granules, or mixtures thereof. The (a) crosslinked rubber granules are larger than the (b) pulverulent crosslinked rubber particulates. The (a) crosslinked rubber granules may have a sieve size of 0.5-4 mm, or such as 0.5-2.5 mm. The (a) crosslinked rubber particles have a sieve size of less than 0.5 mm. The crosslinked rubber improves sound insulation. Preferably, to reduce odor and toxicity, the D)(ii)a) crosslinked rubber granules or particles comprise ethylene propylene diene (EPDM) rubber.
[0047] D)(i) The total amount of lightweight inorganic aggregate may range from 20 to 60% by weight, or preferably from 25 to 55% by weight, based on the total weight of all materials used to form the trowelable aqueous composition.
[0048] The amount of D)(ii) crosslinked rubber (a) grains and / or (b) fine particles relative to the amount of D)(i) lightweight inorganic aggregate may be increased to improve the crack resistance, sound deadening, and resilience of the sound deadening mat. Preferably, the total amount of rubbery composite components in the trowelable aqueous composition may be selected such that when the trowelable aqueous composition is dried or cured to form the sound deadening mat, the total weight ratio of rubbery composite component solids to aqueous polymeric foam-forming component solids is in the range of 1:3 to 2:1, such as 1:3 to 2.5:1, or such as 1:2 to 2:1, or such as 1:1.6 to 2:1.
[0049] Any type of crosslinked or vulcanized rubber, such as natural rubber, synthetic rubber, and derivatives thereof, may be used as D)(ii)(a) grains and / or (b) particles in the rubbery composite component of the present invention. Suitable rubbers include, for example, diene-based polymers such as polyisoprene, cis-1,4-polyisoprene, EPDM, ethylene propylene rubber (EPM), butadiene rubber, nitrile rubber (including nitrile diene rubber), such as acrylonitrile butadiene styrene rubber (ABS), styrene butadiene rubber (SBR), acrylonitrile-butadiene, cis-1,4-polybutadiene, crosslinked acrylic rubber, hydrogenated nitrile, nitrile rubber, neoprene rubber, chloroprene rubber, halogenated butyl rubber, and reclaimed rubber, such as recycled tire rubber or ground tire rubber (GTR). The crosslinked rubber may be vulcanized (crosslinked) or peroxidized rubber and may contain one or more of a crosslinking agent, sulfur, or vulcanization accelerator. Preferably, the crosslinked rubber (a) granules and / or (b) particles of the present invention have little odor, do not contain sulfur, and do not contain toxic substances such as heavy metals, etc. Examples of preferred crosslinked rubber (a) granules and / or (b) particles are EPDM, EPM, and SBR.
[0050] The crosslinked rubber particles D)(ii)(b) of the present invention may comprise pulverulent crosslinked rubber and may have a sieve size of less than 0.5 mm, less than 0.3 mm, less than 0.1 mm, or even less than 0.05 mm. Alternatively, they may comprise particles having a sieve size of 0.5-4 mm, or 0.5-3 mm, or preferably 0.5-2.5 mm. Alternatively, they may comprise a mixture of pulverulent crosslinked rubber and crosslinked rubber particles.
[0051] When used as a sound deadening mat or as a composition for making a sound deadening mat in floor mat, underlayment, and underlayment applications according to the invention, the trowelable aqueous composition should withstand compressive forces without more than a slight shrinkage of, for example, less than 5% of the original thickness of the sound deadening mat or the layer of dried or hardened material that constitutes the sound deadening mat, such as about 0.05%, for example preferably less than 3%, or more preferably 2% or less. Preferably, the weight ratio of D)(i) lightweight inorganic aggregate to the total weight of the aqueous emulsion polymers A) and B) in the trowelable aqueous composition is 1:1 or less, for example in the range of 1:4 to 1:1. Thus, the weight ratio of D)(i) lightweight inorganic aggregate solids to the total solids weight of the aqueous emulsion polymers A) and B) can be preferably 3:1 or less, for example in the range of 1:8 to 2.5:1.
[0052] For further improvement in sound insulation and tensile strength, the rubbery composite component and dispersed rubbery composite portion of the present invention may further comprise wood or palm fibers, such as any having an average length of less than 12 mm or less than 10 mm. The total amount of such wood or palm fibers may range from 0 to 10% by weight, based on the total weight of all materials used to form the trowelable aqueous composition.
[0053] The present invention is not limited by the shape of the D)(ii) finely divided crosslinked rubber (a) granules and / or (b) particles. The crosslinked rubber may be in the form of, for example, chopped rubber, rubber pellets, rubber strands, or particles such as crumb rubber, or rubber powder, which particulate forms are commercially available and produced by methods known to those skilled in the art.
[0054] According to the method of using the trowelable aqueous composition of the present invention, the aqueous polymeric foam-forming component and the rubbery composite component can be mixed separately and independently by any conventional means to form a mortar or by simple mixing. For example, the components can be mixed by hand or using a low shear mixer such as a cement mixer. The aqueous polymeric foam-forming component may be foamed using a static mixer or a medium or high shear mixer such as a homogenizer or other conventional foam mixing equipment before mixing with the rubbery composite component. The rubbery composite component of the present invention is dry mixed before mixing with the aqueous polymeric foam-forming component. Furthermore, the aqueous polymeric foam-forming component and the trowelable aqueous composition may be mixed in the same mixer that mixes either the aqueous polymeric foam-forming component or the rubbery composite component itself.
[0055] In the method of the present invention, applying the trowelable aqueous composition of the present invention to form a sound deadening mat may include applying the composition to or onto a concrete slab to form a layer in a conventional manner, such as by using a trowel, squeegee, roller, scree, and / or float, such as in a plaster, primer, or skim coat manner.
[0056] After the trowelable aqueous composition has dried or cured, the method of the present invention may further include applying a layer of cement, stucco, or gypsum skim to complete the installation of the underlayment. EXAMPLES
[0057] The following examples illustrate the invention. Unless otherwise indicated, all parts and percentages are by weight, all temperatures are in °C, and all preparation and testing procedures are carried out at ambient conditions at room temperature of 23 °C and pressure (1 atm). The following abbreviations have been used in the following examples and in Tables 1, 2, and 3: AA: acrylic acid, AM: acrylamide, BA: n-butyl acrylate, HEMA: 2-hydroxyethyl methacrylate, MAA: methacrylic acid, MMA: methyl methacrylate, Sty: styrene.
[0058] The following materials were used in the following examples (all commercially available components were used as received).
[0059] Rigid styrene acrylic emulsion polymer: a one-stage styrene acrylic emulsion polymer made by stepwise addition emulsion polymerization of 1.0 glacial acrylic acid (GAA) / 2.0 AM / 0.2 adhesion promoter monomer / 47.8 Sty / 49 BA with a measured Tg of 21°C (DSC TA Instruments Q2000 (TA Instruments, New Castle, DE); sample heated to 160°C, then rapidly cooled (10°C / min) to -80°C in 3 minutes, then ramped at 10°C / min to 160°C); Soft Styrene Acrylic Emulsion Polymer: A one-stage styrene acrylic emulsion polymer made by stepwise addition emulsion polymerization of 0.5 HEMA / 1.9 AM / 28 Sty / 69.6 BA and has a measured Tg of -11°C; Water: Tap water; Foam stabilizer: Xianbang C-405 calcium stearate salt aqueous emulsion, Shanghai Xianbang Chemicals Co.Ltd, Shanghai, PRC; Foaming Agent: TRITON™ CG-110 alkyl polyglucoside foaming agent, The Dow Chemical Company (Dow), Midland, MI; Thickener: Acrysol™ TT935 hydrophobically modified anionic thickener, Dow; Dispersant: Orotan™ 1850E sodium polyacrylate, Dow Light sand: mainly composed of SiO2, 0.27g / cm 3 Sand with a density of 1.01kg / m² (Suzhou Lvcheng Lightweight Green Materials Co.Ltd.Suzhou,PRC); EPDM Granules: Ethylene Propylene Diene (EPDM) rubber, sieve size 0.2-2mm according to manufacturer's report (grain size, Guangzhou Chuanao Sports Facilities Co.Ltd.,Guangzhou PRC); EPDM rubber powder: sieve size 177 μm, <80 mesh (as reported by manufacturer, Guangzhou Chuanao Sports); Recycled tire rubber powder: size: <0.5mm (according to manufacturer's report, Fujian Aoxiang, Fuzhou, PRC); Recycled foam rubber powder derived from latex mattresses (Jiangxi Wandao New Materials Co. Ltd., Nanchang, PRC); SBR recycled rubber powder (sieve size <0.5mm as reported by manufacturer, Fujian Aoxiang); Wood flour A: size 1.18mm or <16 mesh (as reported by manufacturer, SDC lab, Shanghai); Wood flour B: size 0.5-1.18mm or 16-30 mesh (as reported by manufacturer, SDC lab); Palm fiber: Length: <12mm (as reported by manufacturer, KNAAP (Thailand) Co. Ltd.); Precast PU foam mat: Made by basic addition polymerization of diol or polyol, diphenylmethane diisocyanate (MDI), and water, with a maximum density of 700 kg / m 3 Polyurethane foam with a density of 10 ...
[0060] [Table 1] * A comparative example is shown.
[0061] Sound-absorbing mat: Unless otherwise indicated, to make sound-absorbing mats for the examples, the specified materials in each of the liquid and powder components were mixed separately according to the formulations shown in Table 1 above and Tables 3 and 4 below, and then mixed together uniformly to form a mortar. The mortar was cast onto a piece of release paper placed on a 300 x 300 x 5 mm stainless steel frame, and the mortar thus cast was formed into a layer by smoothing it with a stainless steel trowel. For thinner mats, a lower percentage of the mortar was cast into the frame. After curing for 24 hours, the mats were cut into the desired size for testing.
[0062] The thickness of the sound-absorbing mats tested was determined in accordance with BS EN 12431:2013 Thermal insulating products for building applications-Determination of thickness for floating floor insulating products.
[0063] Test Methods: The following test methods were used in the following examples: Impact Sound Insulation: The sound deadening mats used were 5 mm thick and had a rectangular surface with dimensions of 22 cm L x 30 cm W. The thickness of the mat in Example 1 was 3 mm, and the thickness of the mat in Example 2 was 5 mm. To evaluate the impact sound insulation performance of different sound deadening mat materials, a rectangular pillar (box) of expanded polystyrene board (5 cm thick) with an open top was constructed. The box had a height of 60 cm and an internal cavity size of 30 cm W x 20 cm L, with back and front rectangular holes (30 cm W x 5 cm L) each located horizontally at a height of exactly 15 cm from the bottom. The sound deadening mat was held in place between two expanded polystyrene board "C" panels, each 30 cm long and with a square cross section of 5 cm x 5 cm with a 1 cm x 1 cm channel or groove running lengthwise to receive each side of the sound deadening mat, which was slid into the box hole so that it was lying parallel to the bottom of the box. A steel ball (1000 g, diameter 6.35 cm) was held at the top height of the box and dropped from the top of the box onto each sound deadening mat to generate impact sound. A noise measuring device was placed inside the box under the sample holder to receive the noise underneath the sound deadening mat. Each sound deadening mat was measured five times and the average was reported. Precast PU foam mat samples with thicknesses of 3 mm and 5 mm, respectively, were used for comparison. The results of the impact sound insulation test are shown in Table 5 below.
[0064] Sound insulation impedance tube test: The sound insulation impedance tube test was carried out according to GB / Z 27764-2011 Acoustics-Determination of sound transmission loss in impedance tubes-Transfer matrix method (China Standards Press, Beijing, China). To form each sound-proof mat, each specified mortar from Table 3 below was cured at room temperature for 48 hours, and then each mat was cut into two circular pieces with diameters of 100 mm and 30 mm, respectively. The thicknesses of the sound-proof mats used independently in any of the following examples or comparative examples 1-11 were all 5 mm. A precast PU foam mat with a thickness of 5 mm was used as comparative example 12 in the sound insulation impedance test. In the test, the equipment used included a series of two impedance tubes (SW series Shengwang Technology Company). The components of the apparatus are shown as arranged in the test in Figure 1 and include the sound-deadening mat (16) to be tested, one of a set of two impedance tubes (18) (individual tubes not shown) with tapered diameter and different maximum inner diameter (30mm and 100mm), four sound pressure sensors including a microphone (22), and a power amplifier (10) connected via a USB connection (4) to a four-channel data acquisition device (6) via an audio signal output (8) and to a PCU (2) running a software analysis system (VA-LAB Basic and IMP Module, Beijing Shengwang Acoustics Technology Corporation, Beijing). The impedance tube (14) comprises a sound source tube (14), an extended sound-deadening tube (18) or receiving tube, and an impedance tube end (20). The apparatus comprises a loudspeaker (12) connected to the upper or open end of the impedance tube (14). When measuring the sound insulation performance of a material, a four-microphone sound transmission method was used, which involved recording or sensing a different sound source tube (14) and receiving tube (18) for each microphone (22). The basic parameters during the test are shown in Table 2 below.To eliminate any undue error in testing, the results reported are the average of three independent experiments for each sound deadening mat. The results are shown in Table 7 below. The data represents the effective sound insulation over a wide range of different frequencies.
[0065] [Table 2]
[0066] Compressibility: The specified materials in each of the liquid and powder parts were mixed separately according to the formula shown in Table 4 below, which was used to make mortar, which was then molded into sound-deadening mats. After the mats were cured at room temperature for 48 hours, each mat was cut into 20 mm x 20 mm squares. The starting thickness of all mats was approximately 5 mm. A precast PU foam mat with a thickness of 5 mm was used as Comparative Example 12. The thicknesses of the sound-deadening mats were measured under different loads: dL, thickness of the sample under a load of 250 Pa; dF, thickness of the sample under a load of 2 kPa; d50K, thickness of the sample under a load of 50 kPa; dB, thickness of the sample under a load of 2 kPa after applying an additional load (48 kPa) for a short time. The thicknesses dL, dF, d50K, and dB were determined sequentially in order on the same sound-deadening mat after determining their initial thickness. The compression ratio is calculated as [(dF-d50K) / dF] x 100%. The results are shown below in Table 6. The method for measuring the thickness after compression testing was as follows.
[0067] Each sound deadening mat was placed on a rigid, flat, level base plate to ensure that the entire mat surface area of each sound deadening mat was in contact with the base plate, with any overcoats or coatings on the opposite side of the base plate. To measure dL, each tested sound deadening mat was loaded into an apparatus that exerted a pressure of 250 Pa for a period of 120±5 seconds, and then the thickness after pressure was measured to the nearest 0.1 mm. To measure dF, each tested sound deadening mat was loaded into an apparatus that exerted a pressure of 2 kPa for a period of 120±5 seconds, and then the thickness after pressure was measured to the nearest 0.1 mm. To measure d50k, each tested sound deadening mat was loaded into an apparatus that exerted an additional pressure of 48 kPa (in addition to 2 kPa) for a period of 120±5 seconds, and then the thickness after pressure was measured to the nearest 0.1 mm. Finally, to measure thickness dB, each sound deadening mat tested was loaded only into an apparatus exerting a pressure of 2 kPa (after removing the 48 kPa pressure) for a period of 120±5 seconds, and then the thickness after pressure was measured to the nearest 0.1 mm. Thickness was determined as the distance measured between a rigid flat base plate on which the specimen rested and a rigid flat pressure plate exerting different specified pressures on the upper surface of the specimen.
[0068] Workability: Each specified material was formed by uniformly mixing the liquid and powder parts in a high speed mixer for 3 minutes to prepare a trowelable mixture and a sprayable material. The concrete substrate surface was moistened before testing. The surface of the fresh mixture of the specified material was smoothed with a steel trowel, and the smoothness of the material and the flatness of the material surface when applied were visually evaluated, and the workability was evaluated by a person skilled in the art according to the following scores:
[0069] Machinability assessment scores: 0, not machinable; 1, very poor; 2, poor; 3, acceptable; 4, good; 5, very good.
[0070] [Table 3] * A comparative example is shown.
[0071] [Table 4] * A comparative example is shown.
[0072] [Table 5] * - Comparative examples are shown. 1. Thickness is 5 mm unless otherwise specified. 2. Same materials as in Comparative Example 12. 3. Same formulation as in Example 9.
[0073] [Table 6] * Comparative Examples: 1. Same formulation as Comparative Example 12.
[0074] As shown in Table 5 above, the noise levels obtained using the sound deadening mats of the present invention of Examples 9B and 9C were comparable to those obtained from the precast PU foam mats of Comparative Examples 12B and 12C, and were far superior to those obtained from fiber cement.
[0075] As shown in Table 6 above, the compression modulus obtained from testing of the inventive sound deadening mat of Example 13 made using a trowelable aqueous composition comprising a 1:1 weight ratio of rubber-like composite component and aqueous polymer foam forming component was comparable to the compression modulus obtained from the precast PU foam mat of Comparative Example 12D, and was much better than the results obtained from pads made from Comparative Examples 14 (hard polymer only) and 15 (soft polymer only).
[0076] As shown in Table 7 below, inventive Examples 6-7 and 9 provided good processability and consistent sound deadening from low to high frequencies. Inventive Example 6 provided sound deadening at low frequencies comparable to the PU foam mat of Comparative Example 12. Too much light sand or crosslinked rubber impairs processability, as shown in Comparative Examples 4 and 5. In Comparative Example 5, even though a pad was made using a trowelable aqueous composition containing a rubber-like composite component and an aqueous polymeric foam-forming component in a weight ratio of 1:1.5, processability remained an issue. As shown in Comparative Example 5, a higher than preferred amount of the aqueous polymeric foam-forming component results in inconsistent sound deadening at low frequencies. The composition of Comparative Example 10 provides processability and sound deadening, but too much light sand results in a composition with excessive compaction for adequate durability.
[0077] [Table 7] * A comparative example is shown.
Claims
1. A trowelable aqueous composition of an aqueous polymeric foam-forming component and a rubbery composite component, comprising: As the aqueous polymer foam forming component, A) 10 to 60 weight percent of one or more rigid vinyl or acrylic aqueous emulsion polymers having a measured glass transition temperature (measured Tgh) of 5 to 40° C. as measured by differential scanning calorimetry (DSC) comprising heating to 160° C., rapidly cooling at 10° C. / min to −80° C., then increasing the temperature at 10° C. / min to 160° C. while collecting DSC curve data and recording the midpoint of the inflection of the resulting DSC curve as Tgh; B) 5 to 50 weight percent of one or more flexible vinyl or acrylic aqueous emulsion polymers having a measured Tg (measured Tgs) of 0 to -35°C when measured by differential scanning calorimetry (DSC) comprising heating to 160°C, rapidly cooling at 10°C / min to -80°C, then increasing the temperature at 10°C / min to 160°C while collecting DSC curve data and recording the midpoint of the inflection of the resulting DSC curve as the Tgs; C) (i) 0.5 to 3 wt. % of a foam stabilizer of an organic acid salt having 12 to 24 carbon atoms, and (ii) 0.05 to 0.75 wt. % of an organic blowing agent; As the rubber composite component, D) (i) 20 to 60% by weight of a sieve particle size of 0.3 to 4 mm and 0.18 to 0.4 g / cm 3 a lightweight inorganic aggregate having a density of D) (ii) 20 to 60% by weight of crosslinked rubber (a) particles having a sieve size of 0.5 to 4 mm, or (b) particles having a sieve size of 0.1 to less than 0.5 mm, or a mixture of (a) granular crosslinked rubber particles and (b) pulverulent crosslinked rubber particles, the weight ratio of (a):(b) being 99:1 to 20:80, Including, A trowelable aqueous composition, wherein all weight percentages in said trowelable aqueous composition add up to 100% and are based on the total weight of all materials used to form said trowelable aqueous composition.
2. 2. The trowelable waterborne composition of claim 1, wherein the measured Tg (measured Tgh) of the A) rigid vinyl or acrylic waterborne emulsion polymer and the measured Tg (measured Tgs) of the B) flexible vinyl or acrylic waterborne emulsion polymer differ by 15° C. to 75° C.
3. 2. The trowelable aqueous composition of claim 1, wherein said measured Tgh is in the range of 10 to 35°C and said measured Tgs is in the range of -8 to -35°C.
4. 2. The trowelable waterborne composition of claim 1, wherein said B) soft vinyl or acrylic waterborne emulsion polymer in said waterborne polymeric foam forming component comprises 7 to 40 weight percent based on the total weight of all materials used to form said trowelable waterborne composition.
5. 2. The trowelable waterborne composition of claim 1, wherein the solids weight ratio of total A) hard vinyl or acrylic waterborne emulsion polymer to total B) soft vinyl or acrylic waterborne emulsion polymer is in the range of 2:3 to 6:
1.
6. 2. The trowelable aqueous composition of claim 1, comprising C)(i) calcium stearate as a foam stabilizer.
7. 2. The trowelable aqueous composition of claim 1, comprising C)(ii) an alkyl polyglucoside as an organic blowing agent.
8. 2. The trowelable waterborne composition of claim 1, wherein said D)(i) lightweight inorganic aggregate is selected from porous light sand, mesoporous silica, mesostructured silica, or expanded clay aggregate.
9. 2. The trowelable aqueous composition of claim 1, wherein the D)(ii)(a) crosslinked rubber granules comprise ethylene propylene diene (EPDM) rubber granules or ethylene propylene (EPM) rubber granules, or the D)(ii)(b) crosslinked rubber particles comprise ethylene propylene diene (EPDM) rubber crumb or ethylene propylene (EPM) rubber crumb, or both.
10. In said aqueous polymeric foam forming components, 0.1-1.5 wt. % of one or more hydrophobically modified anionic thickeners; 0.1 to 1.5 wt. % of one or more dispersants; The trowelable aqueous composition of claim 1 further comprising:
11. 13. A method of using the trowelable aqueous composition of claim 1, comprising: mixing the D) (i) lightweight inorganic aggregate and the D) (ii) crosslinked rubber (a) particles or (b) finely divided crosslinked rubber particles, or a mixture of the (a) particles of crosslinked rubber and the (b) finely divided crosslinked rubber particles, to form a rubber-like composite component; mixing said vinyl or acrylic aqueous emulsion polymers A) and B), said C)(i) foam stabilizer, and C)(ii) organic blowing agent to form an aqueous polymeric foam forming component; combining said rubbery composite component and said aqueous polymeric foam forming component to form a trowelable mixture; applying the trowelable mixture to a substrate to form a matte layer; drying or curing the matte layer; and A method comprising: