Glass container for storing pharmaceutical compositions
Glass pharmaceutical vials with reduced sidewalls and chemical strengthening address mechanical and durability issues, improving performance and sustainability while reducing material usage and breakage risks.
Patent Information
- Application Number
- JP2024516600
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-09
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-04
AI Technical Summary
Glass containers used for pharmaceutical products face challenges with mechanical performance, leading to breakage, reduced production efficiency, and potential contamination due to cracks or breaks, while traditional methods to enhance mechanical performance increase material usage and costs.
Designing glass pharmaceutical vials with reduced sidewall thickness and optional organic coatings, adhering to specific ISO dimensions, and employing chemical strengthening processes to improve mechanical strength and durability.
The reduced thickness vials exhibit enhanced mechanical performance, reduced material usage, and improved chemical durability, minimizing breakage and contamination risks, thus enhancing production efficiency and sustainability.
Smart Images

Figure 2024536026000001_ABST
Abstract
Description
Description of Related Applications
[0001] This application claims the benefit of U.S. Provisional Patent Application No. 63 / 250,497, filed September 30, 2021, entitled "Glass Containers For Storing Pharmaceutical Compositions," and U.S. Provisional Patent Application No. 63 / 277,488, filed November 9, 2021, entitled "Pharmaceutical Containers Including High CTE Sealing Assembly Encircling Outer Surface Of Container," the entire contents of which are incorporated herein by reference. [Technical field]
[0002] FIELD OF THE DISCLOSURE This disclosure relates generally to glass containers, and more specifically to glass containers for storing pharmaceutical compositions, such as glass pharmaceutical vials. [Background technology]
[0003] Historically, glass has been used as a preferred material for packaging pharmaceutical products due to its hermeticity, optical clarity, and superior chemical durability compared to other materials. Specifically, glasses used for pharmaceutical packaging must have adequate chemical durability so as not to affect the stability of the pharmaceutical composition contained therein. Glasses with adequate chemical durability include glass compositions within the ASTM standard "Type 1B" glass compositions that have a proven history of chemical durability.
[0004] However, the use of glass for such applications is limited by its mechanical performance. In particular, breakage can be costly for pharmaceutical manufacturers because breakage in the filling line requires adjacent unbroken containers to be discarded, as the container may contain fragments of the broken container. Breakage can also require the filling line to be slowed or stopped, reducing production yields. Breakage can also result in loss of active drug, which can lead to increased costs. Furthermore, less than catastrophic breakage (i.e., the glass cracks but does not break) can cause the contents to lose their sterility, which can also lead to costly product recalls. Summary of the Invention [Problem to be solved by the invention]
[0005] In addition to mechanical performance, it is also desirable to reduce the overall glass usage to provide more environmentally friendly and sustainable packaging for pharmaceuticals.
[0006] Thus, there is a need for glass containers used to store pharmaceutical compositions that have improved and sustainable mechanical performance. [Means for solving the problem]
[0007] According to a first aspect of the present disclosure, a glass pharmaceutical vial comprises a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D being equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial of size designation X as defined by ISO 8362-1:2018, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. iwhere s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1:2018, and the glass pharmaceutical vial comprises a compliance factor of at least 1.75 as determined in accordance with the Vial Compliance Test.
[0008] A second aspect of the present disclosure may include the glass pharmaceutical vial of the first aspect, further comprising a horizontal strength coefficient of at least 0.5, determined according to a horizontal compression test.
[0009] A third aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the first or second aspects, further comprising an exterior organic coating and a horizontal strength coefficient of at least 1.5 determined according to a horizontal compression test.
[0010] A fourth aspect of the present disclosure may include the glass pharmaceutical vial of any one of the first to third aspects, further comprising an outer organic coating.
[0011] A fifth aspect of the present disclosure may include the glass pharmaceutical vial according to the fourth aspect, wherein the outer organic coating is an organic coating having a thickness of 20 nm or more and 40 nm or less.
[0012] A sixth aspect of the present disclosure may include the glass pharmaceutical vial according to the fourth aspect, further comprising a breakage modulus of at least 50, determined according to a pendulum impact test.
[0013] A seventh aspect of the present disclosure may comprise the glass pharmaceutical vial according to the fourth aspect, further comprising a low temperature storage factor, determined according to a freeze-thaw test, of at least 2.25.
[0014] An eighth aspect of the present disclosure may include the glass pharmaceutical vial of any one of the first to seventh aspects, formed from Type I, Class B glass according to ASTM standard E438-92.
[0015] A ninth aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the first to seventh aspects, wherein the glass pharmaceutical vial is formed from an aluminosilicate glass composition.
[0016] A tenth aspect of the present disclosure is a method for manufacturing a gypsum lath comprising the steps of: i The glass pharmaceutical vial of any one of the first to ninth aspects, wherein the sidewall of the glass pharmaceutical vial having a mass of 10% or more correlates with a reduction in the mass of the glass used to make the glass pharmaceutical vial.
[0017] An eleventh aspect of the present disclosure is a method for manufacturing a gypsum lath comprising the steps of: i The glass pharmaceutical vial may include the glass pharmaceutical vial of any one of the first to tenth aspects, wherein a sidewall of the glass pharmaceutical vial having a thermal conductivity of 100 .mu.m or less correlates with a 5% or greater reduction in the amount of energy used to convert the glass pharmaceutical vial from the glass tubing blank.
[0018] A twelfth aspect of the present disclosure is a method for manufacturing a gypsum lath comprising the steps of: i The glass pharmaceutical vial may comprise the glass pharmaceutical vial of any one of the first to eleventh aspects, wherein a sidewall of the glass pharmaceutical vial having a
[0019] A thirteenth aspect of the present disclosure provides a method for manufacturing a gypsum lath comprising the steps of: i The glass pharmaceutical vial may include the glass pharmaceutical vial of any one of the first to twelfth aspects, wherein a sidewall of the glass pharmaceutical vial having a thickness of 0.01 mm or less correlates with a 20% or greater reduction in the amount of energy used to separate the glass pharmaceutical vial from the glass tubing blank.
[0020] A fourteenth aspect of the present disclosure is a glass pharmaceutical vial that meets the U.S.P. <660> The glass pharmaceutical vial according to any one of the first to thirteenth aspects may comprise a glass pharmaceutical vial having Type 1 chemical durability according to
[0021] A fifteenth aspect of the present disclosure may comprise the glass pharmaceutical vial according to any one of the first to fourteenth aspects, further comprising a dynamic shock coefficient of less than 0.9, determined according to a dynamic shock test.
[0022] A sixteenth aspect of the present disclosure may comprise the glass pharmaceutical vial according to any one of the first to fifteenth aspects, further comprising a FWHM factor of at least 1.2, determined according to a dynamic impact test.
[0023] A seventeenth aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the first to fourteenth aspects, further comprising a dynamic impact coefficient of less than 0.9, determined in accordance with a dynamic impact test, and a FWHM coefficient of at least 1.2, determined in accordance with a dynamic impact test.
[0024] According to an eighteenth aspect of the present disclosure, a glass pharmaceutical vial comprises a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D of the glass body is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1:2018, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1:2018, and the glass pharmaceutical vial comprises a compliance factor of at least 1.75 as determined in accordance with the Vial Compliance Test.
[0025] A nineteenth aspect of the present disclosure may include the glass pharmaceutical vial of the eighteenth aspect, further comprising a horizontal strength coefficient of at least 0.5 as determined according to a horizontal compression test.
[0026] A twentieth aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the eighteenth or nineteenth aspects, further comprising an outer organic coating and a horizontal strength coefficient of at least 1.5 determined according to a horizontal compression test.
[0027] A twenty-first aspect of the present disclosure may comprise the glass pharmaceutical vial according to any one of the eighteenth to twentieth aspects, further comprising an outer organic coating.
[0028] A twenty-second aspect of the present disclosure may include the glass pharmaceutical vial of the twenty-first aspect, wherein the outer organic coating is an organic coating having a thickness of 20 nm or more and 40 nm or less.
[0029] A twenty-third aspect of the present disclosure may comprise the glass pharmaceutical vial of the twenty-first aspect, further comprising a breakage modulus of at least 50 as determined according to a pendulum impact test.
[0030] A twenty-fourth aspect of the present disclosure may comprise the glass pharmaceutical vial according to the twenty-first aspect, further comprising a low temperature storage coefficient of at least 2.25 as determined in accordance with a freeze-thaw test.
[0031] A twenty-fifth aspect of the present disclosure may include the glass pharmaceutical vial of any one of the eighteenth to twenty-fourth aspects, wherein the glass pharmaceutical vial is formed from Type I, Class B glass according to ASTM standard E438-92.
[0032] A twenty-sixth aspect of the present disclosure may include the glass pharmaceutical vial of any one of the eighteenth to twenty-fourth aspects, wherein the glass pharmaceutical vial is formed from an aluminosilicate glass composition.
[0033] A twenty-seventh aspect of the present disclosure is a method for manufacturing a gypsum lath comprising the steps of: iThe glass pharmaceutical vial of any one of the eighteenth to twenty-sixth aspects, wherein the sidewall of the glass pharmaceutical vial having a mass of at least 10% correlates with a reduction in the mass of the glass used to make the glass pharmaceutical vial.
[0034] A twenty-eighth aspect of the present disclosure is a method for manufacturing a gypsum lath having an average wall thickness T i The glass pharmaceutical vial of any one of the eighteenth to twenty-seventh aspects, wherein a sidewall of the glass pharmaceutical vial having a thickness of about 100 nm to about 150 nm correlates with a 5% or greater reduction in the amount of energy used to convert the glass pharmaceutical vial from the glass tubing blank.
[0035] A twenty-ninth aspect of the present disclosure is a method for manufacturing a gypsum lath comprising the steps of: i The glass pharmaceutical vial may comprise any one of the eighteenth to twenty-eighth aspects, wherein a sidewall of the glass pharmaceutical vial having a
[0036] A thirtieth aspect of the present disclosure provides a sintered body having an average wall thickness T i The glass pharmaceutical vial of any one of the eighteenth to twenty-ninth aspects, wherein a sidewall of the glass pharmaceutical vial having a diameter of about 100 mm or more correlates with a 20% or greater reduction in the amount of energy used to separate the glass pharmaceutical vial from the glass tubing blank.
[0037] A thirty-first aspect of the present disclosure is a glass pharmaceutical vial that is <660> The glass pharmaceutical vial according to any one of the eighteenth to thirtieth aspects may comprise a glass pharmaceutical vial having Type 1 chemical durability according to the present invention.
[0038] A thirty-second aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the eighteenth to thirty-first aspects, further comprising a dynamic impact coefficient of less than 0.9, determined in accordance with a dynamic impact test.
[0039] A thirty-third aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the eighteenth to thirty-second aspects, comprising a FWHM factor of at least 1.2, determined according to a dynamic impact test.
[0040] A thirty-fourth aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the eighteenth to thirty-first aspects, further comprising a dynamic impact coefficient of less than 0.9, determined in accordance with a dynamic impact test, and a FWHM coefficient of at least 1.2, determined in accordance with a dynamic impact test.
[0041] According to a thirty-fifth aspect of the present disclosure, a glass pharmaceutical vial comprises a glass body including a sidewall enclosing an interior volume, an outer diameter D, and an outer organic coating on the sidewall, wherein the outer diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1:2018, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018 for which 116% of the diameter d1 is equal to or greater than D, and wherein the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1:2018, and the glass pharmaceutical vial comprises a breakage factor of at least 50 as determined in accordance with a pendulum impact test.
[0042] A thirty-sixth aspect of the present disclosure may comprise the glass pharmaceutical vial of the thirty-fifth aspect, wherein the outer organic coating has a thickness of 20 nm or more and 40 nm or less.
[0043] A thirty-seventh embodiment of the present disclosure may comprise the glass pharmaceutical vial according to any one of the thirty-fifth or thirty-sixth embodiments, further comprising a low temperature storage factor of at least 2.25 as determined according to a freeze-thaw test.
[0044] A thirty-eighth embodiment of the present disclosure may comprise the glass pharmaceutical vial of any one of the thirty-fifth to thirty-seventh embodiments, further comprising a compliance factor of at least 1.75 as determined pursuant to a vial compliance test.
[0045] A thirty-ninth aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the thirty-fifth to thirty-eighth aspects, further comprising a horizontal strength coefficient of at least 1.5 as determined according to a horizontal compression test.
[0046] A fortieth aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the thirty-fifth to thirty-ninth aspects, further comprising a dynamic impact coefficient, determined in accordance with a dynamic impact test, of less than 0.9.
[0047] A forty-first aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the thirty-fifth to fortieth aspects, further comprising a FWHM factor of at least 1.2, determined according to a dynamic impact test.
[0048] A forty-second aspect of the present disclosure may comprise the glass pharmaceutical vial of any one of the thirty-fifth to thirty-ninth aspects, further comprising a dynamic impact coefficient of less than 0.9, determined in accordance with a dynamic impact test, and a FWHM coefficient of at least 1.2, determined in accordance with a dynamic impact test.
[0049] Additional features and advantages of the embodiments described herein are set forth in the detailed description which follows, and in part will be readily apparent to those skilled in the art from that description, or may be learned by practicing the embodiments described herein, including the following detailed description, the claims, and the accompanying drawings.
[0050] It is to be understood that both the foregoing general description and the following detailed description are intended to describe the various embodiments and provide an overview or framework for understanding the nature and features of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated into and constitute a part of this specification. The drawings illustrate the various embodiments described herein and, together with the description, serve to explain the principles and operation of the claimed subject matter. [Brief description of the drawings]
[0051] [Figure 1] FIG. 1 illustrates a glass container in the form of a glass pharmaceutical vial, according to one or more embodiments described herein. [Diagram 2] FIG. 1 is a schematic depiction of a cross-section of a glass container having a low-friction coating according to one or more embodiments shown and described herein. [Diagram 3] FIG. 2 is a schematic depiction of a partial cross-sectional view of another embodiment of a pharmaceutical container according to one or more embodiments shown and described herein. [Figure 4] FIG. 2 is a schematic depiction of a partial cross-sectional view of another embodiment of a pharmaceutical container according to one or more embodiments shown and described herein. [Diagram 5] FIG. 1 graphically illustrates the outer diameter surface temperature (y-axis) as a function of tube wall thickness (x-axis) upon separation of the formed glass vial from the tube. [Figure 6] FIG. 1 graphically illustrates the inner diameter surface temperature (y-axis) as a function of tube wall thickness (x-axis) upon separation of the formed glass vial from the tube. [Figure 7A] FIG. 1 shows a plot of sodium and boron vaporization (y-axis) as a function of temperature (x-axis). [Figure 7B] FIG. 1 is a plot showing a model of the elemental fraction of sodium in the gas phase (y-axis) as a function of temperature (x-axis) for an aluminosilicate glass. [Figure 8]FIG. 1 shows a plot of sodium and boron vaporization (y-axis) as a function of glass viscosity (x-axis). [Figure 9] FIG. 1 shows a plot illustrating the temperature profile (y-axis) during separation of glass containers containing different wall thicknesses (x-axis). [Figure 10] FIG. 1 shows a plot showing titer (y-axis) for measuring surface hydrolysis resistance as a function of wall thickness of glass containers containing different wall thicknesses (x-axis). [Figure 11A] FIG. 1 shows a plot showing extractable elements (y-axis) of glass pharmaceutical vials with different thicknesses (x-axis) measured by inductively coupled plasma mass spectrometry (ICP-MS), where the test solutions include an acidic pH. [Figure 11B] FIG. 1 shows a plot showing extractable elements (y-axis) of glass pharmaceutical vials with different thicknesses (x-axis) measured by inductively coupled plasma mass spectrometry (ICP-MS), where the test solutions include a basic pH. [Figure 11C] FIG. 1 shows a plot showing extractable elements (y-axis) of glass pharmaceutical vials with different thicknesses (x-axis) measured by Inductively Coupled Plasma Mass Spectroscopy (ICP-MS), where the test solution is water. [Figure 12] FIG. 1 shows a plot of separated part rate (y-axis) as a function of tube wall thickness (x-axis) for the tube-to-vial conversion process. [Figure 13] FIG. 1 shows a plot of separated part rate (y-axis) as a function of tube wall thickness (x-axis) for the tube-to-vial conversion process. [Figure 14] FIG. 2 illustrates a plot of aggregate height (y-axis) as a function of wall thickness (x-axis) for standard and insulated flange designs according to one or more embodiments shown and described herein. [Figure 15] FIG. 1 shows a plot of vial neck thickness (y-axis) as a function of tube wall thickness (x-axis). [Figure 16]FIG. 1 shows a plot of vial neck outer diameter (y-axis) as a function of tube wall thickness (x-axis). [Figure 17] FIG. 1 shows a plot of vial neck outer diameters for glass pharmaceutical vials with standard wall thicknesses and thin-walled glass pharmaceutical vials according to one or more embodiments shown and described herein. [Figure 18] FIG. 13 illustrates the process window for the location of the rail capper during the rail capper experiments described herein. [Figure 19] FIG. 13 shows a schematic depiction of a limit table used in accumulator experiments. [Figure 20A] FIG. 13 shows a plot showing accumulated jams (y-axis) as a function of run time (x-axis) obtained during an accumulator experiment. [Figure 20B] FIG. 1 shows a plot showing required intervention (y-axis) as a function of run time (x-axis) obtained during an accumulator experiment. [Figure 21] FIG. 1 shows a schematic depiction of the vial compliance test described herein. [Figure 22A] FIG. 1 shows a schematic depiction of the test site for the vial compliance test described herein. [Figure 22B] FIG. 2 is a plot showing the temperature profile of an annealing furnace used to anneal embodiments of glass containers described herein. [Diagram 23] FIG. 13 is a plot showing displacement-load data for measurements performed with the Vial Compliance Test described herein. [Figure 24] FIG. 1 illustrates a plot showing average sidewall compliance (y-axis) as a function of wall thickness (x-axis) for glass pharmaceutical vials according to one or more embodiments shown and described herein. [Diagram 25] FIG. 1 shows a schematic representation of the mesh of a glass pharmaceutical vial used for finite element analysis. [Figure 26]FIG. 1 shows a schematic depiction of the boundary conditions implemented for the finite element analysis described herein. [Figure 27] FIG. 13 shows plots demonstrating mesh convergence validation of the finite element analysis described herein. [Figure 28] FIG. 13 illustrates a plot showing compliance measurements along with experimental measurements that demonstrate the validity of the finite element model used to determine the compliance of glass containers described herein. [Figure 29] FIG. 1 shows a schematic depiction of the apparatus used for the dynamic impact testing described herein. [Diagram 30] FIG. 1 shows a box plot showing the peak load (y-axis) of different glass pharmaceutical vials (x-axis) measured according to a dynamic impact test. [Diagram 31] FIG. 13 illustrates a plot showing load impact profiles for glass pharmaceutical vials of different thicknesses according to one or more embodiments shown and described herein. [Diagram 32] FIG. 1 illustrates a schematic depiction of a vial-on-vial fixture for abrading glass containers according to one or more embodiments shown and described herein. [Diagram 33] FIG. 1 illustrates a schematic depiction of a setup used to measure the horizontal compressive strength of a glass container according to one or more embodiments shown and described herein. [Diagram 34] FIG. 1 illustrates a schematic depiction of a setup used to measure the vertical compressive strength of a glass container according to one or more embodiments shown and described herein. [Diagram 35] FIG. 2 illustrates a plot showing the horizontal compressive strength of as-converted glass containers according to one or more embodiments shown and described herein. [Diagram 36] FIG. 2 illustrates a plot showing horizontal compressive strength of glass containers according to one or more embodiments shown and described herein, where the glass containers are allowed to wear prior to testing. [Figure 37]FIG. 2 illustrates a plot showing the vertical compressive strength of a glass container according to one or more embodiments shown and described herein. [Figure 38] FIG. 1 shows a schematic depiction of the apparatus used for the pendulum impact testing described herein. [Figure 39] FIG. 1 illustrates a schematic of a vial holder used in the pendulum impact testing described herein. [Diagram 40] FIG. 1 is a schematic illustrating the drop angle of the apparatus used for the pendulum impact testing described herein. [Diagram 41] FIG. 2 shows a schematic of an impactor used in the pendulum impact testing described herein. [Diagram 42] FIG. 1 is a schematic front view of a vial holder used in pendulum impact testing. [Diagram 43] FIG. 13 shows a schematic top view of a vial holder used in pendulum impact testing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0052] Reference will now be made in detail to embodiments of glass containers described herein, examples of which are illustrated in the accompanying drawings. Wherever possible, the same reference numerals are used throughout the drawings to refer to the same or similar parts. One embodiment of a glass container, specifically a glass pharmaceutical vial, is shown in FIG. 1. As used herein, the terms "glass container," "vial," and "glass pharmaceutical vial" may be used interchangeably to refer to a container made from glass. In an embodiment, the glass pharmaceutical vial comprises a glass body including a sidewall enclosing an interior volume. The outer diameter D of the glass body is 84% to 116% of the diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D. However, the sidewalls of glass pharmaceutical vials have an average wall thickness Ti and s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1. Various embodiments of glass containers, such as glass pharmaceutical vials, are described in further detail herein with specific reference to the accompanying drawings.
[0053] As used herein, ranges can be expressed as from "about" one particular value, and / or to "about" another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, by use of the antecedent "about," it will be understood that the particular value forms another embodiment. It will further be understood that the endpoints of each of the ranges are significant both in relation to the other endpoint, and independently of the other endpoint.
[0054] Directional terms used herein (e.g., up, down, right, left, front, back, top, bottom) are intended to refer only to the drawings in which they are drawn and are not intended to imply absolute orientations.
[0055] Unless expressly stated otherwise, it is in no way intended that the methods described herein be construed as requiring that their steps be performed in a particular order, or as requiring a particular orientation of any apparatus. Thus, where a method claim does not actually recite the order in which its steps are to be followed, or where any apparatus claim does not actually recite an order or orientation for individual components, or where the steps are not otherwise specifically recited in the claim or description to be limited to a particular order, or where no particular order or orientation for the apparatus components is recited, no order or orientation is intended to be inferred in any way. This applies to all possible implicit bases for interpretation, including logical considerations regarding the arrangement of steps, operational flow, order of components, or orientation of components, the plain meaning derived from grammatical construction or punctuation, and the number or type of embodiments described in the specification.
[0056] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a" component includes aspects having two or more such components unless the context clearly dictates otherwise.
[0057] The term "chemical durability," as used herein, refers to the ability of a glass pharmaceutical vial to resist degradation when exposed to specified chemical conditions. Specifically, the chemical durability of the glass pharmaceutical vials described herein may be evaluated according to the following established materials testing standard: USP Glass Grains Test. <660> DIN 12116, dated March 2001, entitled "Testing of glass - Resistance to attack by a boiling aqueous solution of hydrochloric acid - Method of test and classification"; ISO 695:1991, entitled "Glass -- Resistance to attack by a boiling aqueous solution of mixed alkali -- Method of test and classification"; and ISO 720:1985, entitled "Glass -- Hydrolytic resistance of glass grains at 121 degrees C -- Method of test and classification". In addition to the above referenced standards, the chemical durability of glass can also be evaluated in accordance with ISO 719:1985, "Glass -- Hydrolytic resistance of glass grains at 98 degrees C -- Method of test and classification". The ISO 719 standard is a less rigorous version of the ISO 720 standard, and glasses that meet a specified classification in the ISO 720 standard are expected to also meet the corresponding classification in the ISO 719 standard. The chemical durability of glass pharmaceutical vials is evaluated using a USP test entitled "Surface Glass Test," which evaluates the durability of the glass surface. <660> and / or in accordance with European Pharmacopoeia 3.2.1 entitled "Glass Containers For Pharmaceutical Use".The classifications associated with each standard are explained in further detail herein.
[0058] The term "delamination" as used herein refers to the phenomenon in which glass particles are released from the glass surface after a series of leaching, corrosion, and / or weathering reactions. Typically, the particles are silica-rich glass flakes, or lamellae, which arise from the interior surface of a container as a result of the leaching of modifying ions or weak network formers, such as boron, into a solution contained within the container. These flakes, or lamellae, can typically be 1 nm to 2 μm thick and greater than about 50 μm wide. Because these flakes, or lamellae, are composed primarily of silica, the flakes, or lamellae, generally do not further decompose after being released from the glass surface.
[0059] A further method of characterizing the chemical durability of a glass container involves determining the tendency of the glass container to delaminate. As described in US Patent Application Publication No. 2021 / 0080448, the entire contents of which are incorporated herein by reference, the tendency of the glass container to delaminate as described herein can be measured in terms of a "chemical durability ratio" (CDR), which indicates the level of non-uniformity of the inner surface of the vial through the ratio of the "untreated" titer value to the "etched" titer value of the container. Methods for measuring the CDR of a glass container are described in more detail herein.
[0060] Surface compressive stress is measured using a commercially available instrument such as a surface stress meter (FSM), e.g., FSM-6000 manufactured by Orihara Seisakusho Co., Ltd. (Japan). Surface stress measurement relies on measuring the stress optical coefficient (SOC), which is related to the birefringence of the glass ceramic. SOC is measured according to procedure C (glass disk method) described in ASTM standard C770-16, entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient", the entire contents of which are incorporated herein by reference. Depth of compression (DOC) is measured with FSM in conjunction with Scattered Light Polariscope (SCALP) technology, known in the art. FSM measures the compression depth of potassium ion exchange, while SCALP measures the compression depth of sodium ion exchange. Maximum central tension (CT) values are measured using SCALP technology, known in the art.
[0061] As used herein, the phrase "depth of compression" (DOC) refers to the location in an article where a compressive stress transitions to a tensile stress.
[0062] In the context of this disclosure, when a "2 ml" vial is referenced without the ISO 8362-1 standard, the referenced "2 ml" vial includes an outer diameter of 16.25 mm, an outer flange diameter of 31 mm, a height of 31 mm, and a conventional wall thickness of 1.2 mm. When a "3 ml" vial is referenced without the ISO 8362-1 standard, the referenced "3 ml" vial includes an outer diameter of 16.75 mm, an outer flange diameter of 13.15 mm, a height of 37.7 mm, and a conventional wall thickness of 1.1 mm.
[0063] Traditionally, the mechanical properties of glass containers, such as glass pharmaceutical vials, have been increased by adding material to the container, i.e., by making parts of the container or the entire container thicker, thereby increasing the container's ability to withstand mechanical damage (e.g., impacts, drops, abrasions, etc.) without catastrophic failure. However, adding material to a glass container increases the overall cost of the container and can reduce manufacturing throughput because the addition of glass can lengthen certain forming operations, such as forming a glass container from a glass tube. This also increases the amount of glass required to make such containers, which reduces manufacturing efficiency and increases shipping costs due to the added weight.
[0064] However, contrary to the widely accepted practice of adding material to a container to enhance its mechanical properties, it has been found that the mechanical properties of a container can be enhanced by actually removing material from certain parts of the container, such as making the sidewall of the container thinner for a glass container with the same outer diameter. In particular, it has been found that reducing the thickness of the sidewall of a glass container can increase the flexibility of the glass container, thereby allowing the container to better withstand certain mechanical damage with reduced risk of breakage. Thus, the glass containers described herein, such as the glass pharmaceutical vials described herein, are formed with a sidewall that is reduced in thickness compared to a conventional glass vial with the same outer diameter. For example, reducing the thickness of the sidewall by 15% or more can result in a glass container that has improved mechanical properties as well as other practical benefits.
[0065] Referring now to FIG. 1, one embodiment of a glass container 100 for storing a pharmaceutical formulation is depicted generally in cross section. The glass container 100 generally includes a body 112. The body 112 extends between an inner surface 114 and an outer surface 116, includes a central axis A, and generally encloses an interior volume 118. In the embodiment of the glass container 100 shown in FIG. 1, the body 112 generally includes a sidewall 120 and a bottom portion 122. The sidewall 120 transitions to the bottom portion 122 via a lower end portion 124. In the depicted embodiment, the glass container 100 includes a flange 126, a neck 128 extending from the flange 126, and a shoulder 130 extending between the neck 128 and the sidewall 120. In the embodiment, the glass container 100 is symmetrical about the central axis A, and each of the sidewall 120, the neck 128, and the flange 126 are substantially cylindrical. The body 112 has an average wall thickness T extending from the inner surface 114 to the outer surface 116, as depicted in FIG. i In an embodiment, the sidewall 120 and neck 128 have an average wall thickness T i may be the same.
[0066] In an embodiment, the glass container 100 comprises a borosilicate glass composition, such as Type I, Class B glass according to ASTM standard E438-92, USP <660> Alternatively, the glass container 100 may be formed from an alkali aluminosilicate glass composition that meets the Type I criteria, such as those disclosed in U.S. Pat. No. 8,551,898, which is incorporated herein by reference in its entirety, and sold by Corning® Incorporated as Valor® glass, or an alkaline earth aluminosilicate glass, such as those described in U.S. Pat. No. 9,145,329, which is incorporated herein by reference in its entirety. In an embodiment, the glass container 100 may be constructed from a soda-lime glass composition. However, it should be understood that the particular type of glass composition that forms the glass container is not particularly limited, and other suitable glass compositions are contemplated.
[0067] 1 as having a particular form element (i.e., a vial), it is understood that the glass container 100 may have other form elements, including, but not limited to, Vacutainers®, cartridges, syringes, ampoules, bottles, flasks, vials, tubes, beakers, etc. Additionally, it is understood that the glass containers described herein may be used in a variety of applications, including, but not limited to, pharmaceutical packaging, beverage containers, etc.
[0068] Traditionally, glass containers (e.g., glass pharmaceutical vials) have standardized dimensions and fill volumes. For example, ISO 8362-1:2018, entitled "Injection containers and accessories," defines the dimensions of standard size containers. In particular, ISO 8362-1 describes the sidewall thickness "s1," the outside diameter "d1," and the full capacity "c1" of glass vials, as shown in Table 1A below.
[0069] [Table 1A]
[0070] As evident from Table 1A, standardized glass containers typically have characteristic attributes such as outer diameter, inner diameter, wall thickness, and full (overflow) capacity. It has now been discovered that by reducing the wall thickness of a glass container below the wall thickness defined by the standard, unexpected benefits may be realized. In particular, benefits resulting from reducing the wall thickness of standardized glass containers may include improved mechanical properties, as described herein, in addition to benefits related to manufacturability, chemical durability, thermal properties, inspection-related properties, and sustainability.
[0071] In the embodiments described herein, the wall thickness of the glass container is reduced relative to the wall thickness specified in a particular standard, such as the ISO 8362-1 standard referenced herein. However, it should be understood that other standards for glass containers are available from other standards organizations, such as, for example, the Glass Packaging Institute (GPI). Such standards may be similar to the ISO 8362-1 standard, but may also deviate from the ISO 8362-1 standard.
[0072] Additionally, pharmaceutical companies may have their own standardized dimensions and other characteristic attributes for glass containers, such as glass pharmaceutical vials. For example, but not by way of limitation, pharmaceutical companies may utilize glass pharmaceutical vials with outer diameters and / or wall thicknesses that are similar to, but deviate from, the same dimensions of a particular standard, such as ISO 8362-1. As an example, a glass pharmaceutical vial that is functionally equivalent to a 2R glass vial under the ISO 8362-1 standard may have a wall thickness of 1.1 mm, which deviates from the specified standard for 2R glass vials under the standard. Similarly, a glass pharmaceutical vial that is functionally equivalent to a 2R glass vial under the ISO 8362-1 standard may have an outer diameter of 17 mm, which deviates from the specified standard for 2R glass vials under the standard.
[0073] Thus, containers that deviate from the ISO 8362-1 standard are common in commerce, however such containers may likewise benefit from reduced wall thickness.
[0074] As described herein, some commercially common glass containers, such as commercially common glass pharmaceutical containers, may have attributes such as dimensions that differ from standardized glass containers for a particular standard. For example, a glass container may have attributes that differ from a defined standard by, for example, 2%, 4%, 6%, 8%, 10%, 12%, 14%, or even 16%. Such variations may cause a particular glass container to be subject to more than one designation according to a widely known standard, such as the ISO8362-1 standard, or to fall outside any size designation under the standard. For example, a glass container that is functionally equivalent to a 2R glass container under the ISO8362-1 standard may have a larger wall thickness than a 2R glass container under the ISO8362-1 standard, but retain other characteristics of the 2R glass container under the standard. Similarly, a glass container functionally equivalent to a 2R glass container under ISO 8362-1 standard may have a larger outer diameter than a 2R glass container under ISO 8362- standard, but retain other properties of the 2R glass container under said standard. Such a situation may make it difficult to determine an appropriate reduced wall thickness. However, the reduced wall thickness of such a glass container can be determined taking into account deviations from the standard, as described in more detail herein.
[0075] Referring to Table 1B below, in an embodiment, the reduced average wall thickness T of an "off-spec" glass container having attribute variations is ican be determined taking into account the variation of the outer diameter of the glass container relative to the standard outer diameter d1 of the container defined by ISO 8362-1. In this embodiment, the upper and lower outer diameter limits are set based on a ±16% variation from the standardized outer diameter d1 under ISO 8362-1 (i.e., a variation of 84% to 116% of the standardized outer diameter d1). For example, in an embodiment, the glass container 100 may have an outer diameter D (FIG. 1) equal to 84% to 116% of the outer diameter d1 of a glass vial of size designation X defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R defined by ISO 8362-1.
[0076] [Table 1B]
[0077] In an embodiment, a glass container 100, e.g., a glass pharmaceutical vial, comprises a sidewall 120 enclosing an interior volume and a glass body 112 including an outer diameter D, as described herein. The outer diameter D of the glass body 112 is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, for which 116% of the diameter d1 is equal to or greater than D. It is understood that in the order of size designations under ISO 8362-1, 2R is the smallest size designation, 3R is the next smallest size designation, and in the order of 2R to 100R, 100R is the largest size designation. That is, in terms of vial sizing, 2R<3R<4R<6R<8R<10R<15R<20R<25R<30R<50R<100R. For these embodiments, the sidewalls of the glass pharmaceutical vials have an average wall thickness T iwhere s1 is the wall thickness of the smallest size designation X for which 116% of the size designation diameter d1 is equal to or greater than the outer diameter D of the glass container.
[0078] Referring to Table 1B as an example, a hypothetical commercially common but "non-standard" glass container has an outer diameter D of 26 mm. The outer diameter D of 26 mm is within 84% to 116% of the diameter d1 of the ISO 8362-1 vial size designations 10R, 15R, 20R, 25R, and 30R. That is, the outer diameter D of 26 mm is within the range of 84%*d1 to 116%*d1 (i.e., within the range of 20.16 mm to 27.84 mm) for the vial size designations 10R and 15R, and within the range of 84%*d1 to 116%*d1 (i.e., within the range of 25.2 mm to 34.8 mm) for the vial size designations 20R, 25R, and 30R. However, the smallest vial size designation for which 116% of the diameter d1 of the vial size designation is equal to or greater than the outer diameter D is the vial size designation 10R (i.e., 116%*d1(10R)=27.84 mm, which is equal to or greater than 26 mm). That is, in this example, the smallest vial size designation X=10R. Therefore, the wall thickness T of the hypothetical glass container (whose outer diameter D is equal to 26 mm) is i is less than or equal to 0.85*s1, where s1 is the wall thickness of the 10R vial size designation under ISO 8362-1.
[0079] With further reference to Table 1B, as another example, a hypothetical glass container that is commercially common but "nonstandard" has an outer diameter D of 41 mm. The outer diameter D of 41 mm is within 84% to 116% of the diameter d1 of the ISO 8362-1 vial size designations 50R and 100R. That is, the outer diameter D of 41 mm is within the range of 84%*d1 to 116%*d1 (i.e., within the range of 30.6 mm to 46.4 mm) for the vial size designation 50R, and within the range of 84%*d1 to 116%*d1 (i.e., within the range of 39.48 mm to 54.52 mm) for the vial size designation 100R. However, the smallest vial size designation for which 116% of the diameter d1 of the vial size designation is equal to or greater than the outer diameter D is the vial size designation 50R (i.e., 116%*d1(50R)=46.4 mm, which is equal to or greater than 41 mm). That is, in this example, the smallest vial size designation X=50R. Therefore, the wall thickness T of a hypothetical glass container (with an outer diameter D equal to 41 mm) is i is less than or equal to 0.85*s1, where s1 is the wall thickness of the 50R vial size designation under ISO 8362-1.
[0080] As another example, a hypothetical commercially common but "nonstandard" glass container has an outer diameter D of 21 mm. The outer diameter D of 21 mm is within 84% to 116% of the diameter d1 of the ISO 8362-1 vial size designations 6R, 8R, 10R, and 15R. That is, the outer diameter D of 21 mm is within the range of 84%*d1 to 116%*d1 (i.e., within the range of 18.48 mm to 25.52 mm) for the vial size designations 6R and 8R, and within the range of 84%*d1 to 116%*d1 (i.e., within the range of 20.16 mm to 27.84 mm) for the vial size designations 10R and 15R. However, the smallest vial size designation for which 116% of the diameter d1 of the vial size designation is equal to or greater than the outer diameter D is the vial size designation 6R (i.e., 116%*d1(6R)=25.52 mm, which is equal to or greater than 21 mm). That is, in this example, the smallest vial size designation X=6R. Therefore, the wall thickness T of the hypothetical glass container (whose outer diameter D is equal to 21 mm) isi is less than or equal to 0.85*s1, where s1 is the wall thickness of the 6R vial size designation under ISO 8362-1.
[0081] In an embodiment, the outer diameter D of the glass body 112 is greater than or equal to 84% and less than or equal to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest vial size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is greater than or equal to D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of the smallest size designation X for which 116% of the diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X for which 116% of the diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X for which 116% of the diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X for which 116% of the diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X for which 116% of the diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X for which 116% of diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial.
[0082] In an embodiment, a glass container 100, e.g., a glass pharmaceutical vial, comprises a sidewall 120 enclosing an interior volume and a glass body 112 including an outer diameter D, as described herein. The outer diameter D of the glass body 112 is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, in which the diameter d1 is equal to or greater than D. It is understood that in the order of size designations under ISO 8362-1, 2R is the smallest size designation, 3R is the next smallest size designation, and in the order of 2R to 100R, 100R is the largest size designation. That is, in terms of vial sizing, 2R<3R<4R<6R<8R<10R<15R<20R<25R<30R<50R<100R. For these embodiments, the sidewalls of the glass pharmaceutical vials have an average wall thickness T i where s1 is the wall thickness of the smallest size designation X whose diameter d1 of the size designation is equal to or greater than the outer diameter D of the glass container.
[0083] Referring to Table 1B as an example, a hypothetical commercially common but "non-standard" glass container has an outer diameter D of 26 mm. The outer diameter D of 26 mm is within 84% to 116% of the diameter d1 of the ISO 8362-1 vial size designations 10R, 15R, 20R, 25R, and 30R. That is, the outer diameter D of 26 mm is within the range of 84%*d1 to 116%*d1 (i.e., within the range of 20.16 mm to 27.84 mm) for the vial size designations 10R and 15R, and within the range of 84%*d1 to 116%*d1 (i.e., within the range of 25.2 mm to 34.8 mm) for the vial size designations 20R, 25R, and 30R. However, the smallest vial size designation whose diameter d1 is equal to or greater than the outer diameter D is the vial size designation 20R (i.e., d1(20R)=30 mm, which is equal to or greater than 26 mm). That is, in this example, the smallest vial size designation X=20R. Therefore, the wall thickness T of the hypothetical glass container (whose outer diameter D is equal to 26 mm) is i is less than or equal to 0.85*s1, where s1 is the wall thickness of the 20R vial size designation under ISO 8362-1.
[0084] Still referring to Table 1B, as another example, a hypothetical glass container that is commercially common but "nonstandard" has an outer diameter D of 41 mm. The outer diameter D of 41 mm is within 84% to 116% of the diameter d1 of the ISO 8362-1 vial size designations 50R and 100R. That is, the outer diameter D of 41 mm is within the range of 84%*d1 to 116%*d1 (i.e., within the range of 30.6 mm to 46.4 mm) for the vial size designation 50R, and within the range of 84%*d1 to 116%*d1 (i.e., within the range of 39.48 mm to 54.52 mm) for the vial size designation 100R. However, the smallest vial size designation whose diameter d1 is equal to or greater than the outer diameter D is the vial size designation 100R (i.e., d1(100R)=47 mm, which is equal to or greater than 41 mm). That is, in this example, the smallest vial size designation X=100R. Therefore, the wall thickness T of a hypothetical glass container (with an outer diameter D equal to 41 mm) isi is less than or equal to 0.85*s1, where s1 is the wall thickness of the 100R vial size designation under ISO 8362-1.
[0085] As another example, the outer diameter D of a hypothetical commercially common but "nonstandard" glass container is 21 mm. The outer diameter D of 21 mm is within 84%-116% of the diameter d1 of the ISO 8362-1 vial size designations 6R, 8R, 10R, and 15R. That is, the outer diameter D of 21 mm is within the range of 84%*d1-116%*d1 (i.e., within the range of 18.48 mm-25.52 mm) for the vial size designations 6R and 8R, and within the range of 84%*d1-116%*d1 (i.e., within the range of 20.16 mm-27.84 mm) for the vial size designations 10R and 15R. However, the smallest vial size designation whose diameter d1 is equal to or greater than the outer diameter D is the vial size designation 6R (i.e., d1(6R)=22 mm, which is equal to or greater than 21 mm). That is, in this example, the smallest vial size designation X=6R. Therefore, the wall thickness T of a hypothetical glass container (with an outer diameter D equal to 21 mm) is i is less than or equal to 0.85*s1, where s1 is the wall thickness of the 6R vial size designation under ISO 8362-1.
[0086] In an embodiment, the outer diameter D of the glass body 112 is greater than or equal to 84% and less than or equal to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest vial size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 in which the diameter d1 is greater than or equal to D, and the glass pharmaceutical vial has a sidewall with an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of the smallest size designation X whose diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T iwhere s1 is the wall thickness of the smallest size designation X whose diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X whose diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X whose diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X whose diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial. In an embodiment, the sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the smallest size designation X whose diameter d1 is equal to or greater than the outer diameter D of the glass pharmaceutical vial.
[0087] In an embodiment, the glass container 100 is a glass pharmaceutical vial having an outer diameter D between 13.44 mm and 18.56 mm, and a sidewall having an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0088] In an embodiment, the glass container 100 is a glass pharmaceutical vial having an outer diameter D between 18.48 mm and 25.52 mm, and a sidewall having an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0089] In an embodiment, the glass container 100 is a glass pharmaceutical vial having an outer diameter D between 20.16 mm and 27.84 mm, and a sidewall having an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0090] In an embodiment, the glass container 100 is a glass pharmaceutical vial having an outer diameter D between 25.2 mm and 34.8 mm, and a sidewall having an average sidewall thickness of 1.02 mm or less, 0.84 mm or less, 0.72 mm or less, 0.6 mm or less, 0.48 mm or less, or even 0.36 mm or less.
[0091] In an embodiment, the glass container 100 is a glass pharmaceutical vial having an outer diameter D between 33.6 mm and 46.4 mm, and a sidewall having an average sidewall thickness of 1.275 mm or less, 1.05 mm or less, 0.9 mm or less, 0.75 mm or less, 0.6 mm or less, or even 0.45 mm or less.
[0092] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with an outer diameter D between 39.48 mm and 54.52 mm, and an average sidewall thickness of 1.445 mm or less, 1.19 mm or less, 1.02 mm or less, 0.85 mm or less, 0.68 mm or less, or even 0.51 mm or less.
[0093] In other embodiments, the glass container 100 has an outer diameter D (FIG. 1) equal to the outer diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1.
[0094] However, the thickness T of the sidewall 120 of the glass container 100 described herein i may be less than the thickness s1 of a container having the same outer diameter under ISO 8362-1. In embodiments, the sidewall of a glass pharmaceutical vial described herein has an average wall thickness T that is less than s1. iwhere s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1, where X is one of the size designations 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1. For example, a glass container having an outer diameter D equal to the outer diameter d1 of a container having a size designation of 2R under ISO 8362-1 will have an average sidewall thickness T that is less than s1 of a container having a size designation of 2R under ISO 8362-1. i (i.e., T i <1.0±0.04). In an embodiment, the sidewall of the glass container has an average wall thickness T i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1. In an embodiment, the sidewall of the glass container has an average wall thickness T i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1. In an embodiment, the sidewall of the glass container has an average wall thickness T i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1. In an embodiment, the sidewall of the glass container has an average wall thickness T i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1. In an embodiment, the sidewall of the glass container has an average wall thickness T i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1. In an embodiment, the sidewall of the glass container has an average wall thickness T i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1.
[0095] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 2R, an outer diameter D equal to 16 mm ± 0.15 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0096] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 3R, an outer diameter D equal to 16 mm ± 0.15 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0097] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 4R, an outer diameter D equal to 16 mm ± 0.15 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0098] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 6R, an outer diameter D equal to 22 mm ± 0.2 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0099] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 8R, an outer diameter D equal to 22 mm ± 0.2 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0100] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 10R, an outer diameter D equal to 24 mm ± 0.2 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0101] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 15R, an outer diameter D equal to 24 mm ± 0.2 mm, and an average sidewall thickness of 0.85 mm or less, 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, 0.4 mm or less, or even 0.3 mm or less.
[0102] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 20R, an outer diameter D equal to 30 mm ± 0.25 mm, and an average sidewall thickness of 1.02 mm or less, 0.84 mm or less, 0.72 mm or less, 0.6 mm or less, 0.48 mm or less, or even 0.36 mm or less.
[0103] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 25R, an outer diameter D equal to 30 mm ± 0.25 mm, and an average sidewall thickness of 1.02 mm or less, 0.84 mm or less, 0.72 mm or less, 0.6 mm or less, 0.48 mm or less, or even 0.36 mm or less.
[0104] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 30R, an outer diameter D equal to 30 mm ± 0.25 mm, and an average sidewall thickness of 1.02 mm or less, 0.84 mm or less, 0.72 mm or less, 0.6 mm or less, 0.48 mm or less, or even 0.36 mm or less.
[0105] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a sidewall with a size of 50R, an outer diameter D equal to 40 mm ± 0.4 mm, and an average sidewall thickness of 1.275 mm or less, 1.05 mm or less, 0.9 mm or less, 0.75 mm or less, 0.6 mm or less, or even 0.45 mm or less.
[0106] In an embodiment, the glass container 100 is a glass pharmaceutical vial having a size of 100R, an outer diameter D equal to 47 mm ± 0.5 mm, and a sidewall having an average sidewall thickness of 1.445 mm or less, 1.19 mm or less, 1.02 mm or less, 0.85 mm or less, 0.68 mm or less, or even 0.51 mm or less.
[0107] chemical strengthening As described herein, the glass container may be chemically strengthened by an ion exchange process. In embodiments, a chemically strengthened glass container 100 having a thinner sidewall may provide enhanced reliability. In particular, destruction of the product contained within the glass container may occur in the event of a through crack even without catastrophic failure of the container. However, the reduced thickness of the sidewall may increase the central tension introduced during the chemical strengthening process. The relatively higher central tension, coupled with the reduced thickness, promotes crack branching and separation of the vial into multiple pieces (e.g., five or more) upon crack initiation, as compared to glass containers having a larger wall thickness. The enhanced crack branching and separation promotes "self-clearing" of the container upon through crack initiation, reducing the likelihood of crack propagation delay, thereby avoiding the risk of product destruction in a cosmetically intact, but otherwise hermetic, glass container.
[0108] Additionally, when a glass container 100 having a thinner sidewall is chemically strengthened, the process of chemical strengthening to a desired surface compressive stress and compression depth may occur more quickly as a result of the glass container having a reduced fictive temperature, thereby reducing the time and / or temperature required to achieve the desired properties, which may increase throughput of the chemical strengthening process and / or reduce the cost of the chemical strengthening process.
[0109] In embodiments, the glass container may have a compressive stress layer that extends from the surface of the glass container into the thickness of the glass to a compression depth of 25 μm or more, or even 35 μm or more. In some embodiments, the compression depth may be 40 μm or more, or even 50 μm or more. The surface compressive stress of the glass article may be 250 MPa or more, 350 MPa or more, or even 400 MPa or more. The compression depth (i.e., 25 μm or more) and compressive stress (i.e., 250 MPa or more) can be achieved by ion-exchanging the glass article in a molten salt bath of 100% KNO3 (or a mixed salt bath of KNO3 and NaNO3) at a temperature of 500°C or less, or even 450°C or less, for a period of 5 hours or less, or even 4.5 hours or less. In some embodiments, the period to achieve these compression depths and compressive stresses may be 4 hours or less, or even 3.5 hours or less. The temperature to achieve these compression depths and compressive stresses may be 400°C or less, or even 350°C or less.
[0110] coating In embodiments, the glass container 100 may include a coating disposed on at least a portion of the exterior surface 116 of the glass body 112. In embodiments, the coating may be a heat resistant coating as disclosed in U.S. Patent No. 10,273,049, which is incorporated herein by reference in its entirety. In embodiments, the coating may be an organic coating as described in U.S. Patent No. 9,763,852, which is incorporated herein by reference in its entirety. However, it should be understood that other coatings, both organic and inorganic, are contemplated and possible.
[0111] FIG. 2 generally depicts a cross-section of a coated glass product, specifically a coated glass container 200. The coated glass container 200 comprises a glass body 202 and a low-friction coating 220. The glass body 202 has a glass container wall 204 extending between an exterior surface 208 (i.e., a first surface) and an interior surface 210 (i.e., a second surface). The interior surface 210 of the glass container wall 204 defines an interior volume 206 of the coated glass container 200. The low-friction coating 220 is positioned on at least a portion of the exterior surface 208 of the glass body 202. In some embodiments, the low-friction coating 220 may be positioned on substantially the entire exterior surface 208 of the glass body 202. The low-friction coating 220 has an exterior surface 222 and a glass body contact surface 224 at the interface of the glass body 202 and the low-friction coating 220. A low friction coating 220 may be adhered to the glass body 202 on the outer surface 208 .
[0112] In embodiments, a coating of an inorganic material, such as titania, is applied to at least a portion of the exterior surface of the glass body, either by soot deposition or vapor deposition processes. The titania coating has a lower coefficient of thermal expansion than the glass onto which it is deposited. As the coating and glass cool, the titania shrinks less than the glass, and as a result, the surface of the glass body is under tension. In these embodiments, it is understood that the surface compressive stress and depth of layer are measured from the surface of the coating, not the surface of the coated glass container. Although the inorganic coating material is described herein as including titania, it is understood that other inorganic coating materials having suitably low coefficients of thermal expansion are also contemplated. In embodiments, the inorganic coating may have a coefficient of friction of less than 0.7 against a similarly coated container. The inorganic coating may also be thermally stable at temperatures of 250° C. or greater, as further described herein.
[0113] In embodiments, a glass container can be strengthened by a glass container having a high modulus coating with a thermal expansion coefficient equal to or greater than that of the underlying glass container. Strengthening is achieved by the difference in thermal expansion imparting compressive stress to the glass surface (balanced by the tension of the high modulus coating) while the difference in modulus imparts damage resistance. It should be understood that in these embodiments, the surface compressive stress and layer depth are measured from the surface of the glass container, not the surface of the coated glass container. The high modulus makes it less susceptible to scratches and damage, and the underlying compressive layer prevents scratches and defect propagation. Exemplary material combinations to demonstrate this effect are a sapphire coating on a 33 expansion borosilicate glass, or a zirconium oxide coating deposited on a 51 expansion borosilicate glass.
[0114] Based on the above, it should be understood that in embodiments, the glass container may include a compressive stress layer that extends from at least the outer surface of the body to the wall thickness of the glass container. The compressive stress layer improves the mechanical strength of the glass container compared to a glass container that does not include a compressive stress layer. The compressive stress layer also improves the damage resistance of the glass container such that the glass container can withstand greater surface damage (i.e., scratches, chips, etc. that extend deep into the wall thickness of the glass container) without breaking compared to a glass container that does not include a compressive stress layer. It should also be understood that in these embodiments, the compressive stress layer may be formed on the glass container by ion exchange, by heat tempering, by forming the glass container from laminated glass, or by applying a coating to the glass container. In some embodiments, the compressive stress layer may be formed by a combination of these techniques.
[0115] As discussed in more detail below, coated thin-walled glass containers can provide benefits related to manufacturing as well as the mechanical performance of the glass container. In some embodiments, the glass container is subjected to a convert-to-coat process, and the converted glass container is immediately subjected to a coating process, such as those disclosed in U.S. Patent Nos. 10,273,049 and 9,763,852. Such a process reduces or prevents the introduction of defects in the thin walls of the glass container, thereby improving the mechanical performance of the glass container.
[0116] In embodiments of the glass container described herein that include a coating, the coating may be an organic coating that is applied to the glass container according to the following procedure: The glass container is washed with deionized water, blown dry with nitrogen, and dip coated with a 0.1% solution of APS (aminopropylsilsesquioxane), which may enhance coupling of the coating to the glass (i.e., the APS is the "coupling agent layer"). The APS coating is dried in a convection oven at 100°C for 15 minutes. A polymer layer, such as a polymer precursor layer, is then applied to the glass container. In embodiments, the polymer precursor layer may be a polyimide precursor layer. In embodiments, the polymer layer is applied to the glass container by dip coating, spray coating, or the like. For example, in embodiments, the glass container may be immersed in a 0.1% solution of Novastrat® 800 polyamic acid in a 15 / 85 toluene / DMF solution, or a 0.1% to 1% poly(pyromellitic dianhydride-co-4,4′-oxydianiline) amic acid solution (Kapton precursor) in N-methyl-2-pyrrolidone (NMP). In the example coated glass container described herein, the coating was formed from a 0.1% to 1% poly(pyromellitic dianhydride-co-4,4′-oxydianiline) amic acid solution in N-methyl-2-pyrrolidone (NMP). The coated glass container can then be heated to 150° C. and held for 20 minutes to evaporate the solvent. The coated glass container can then be placed in a 300° C. preheated oven for 30 minutes to cure the coating and form a glass container having a low friction, thermally stable polymer coating, specifically a low friction, thermally stable polyimide coating. However, it should be understood that other coating compositions and application methods may be utilized for the thin-walled glass containers of the present disclosure.For example, without limitation, in embodiments, the coating need not include a coupling agent layer.As another example, the coating need not include a separate coupling agent layer, such as in embodiments where the coupling agent and polymer layer are applied in a single layer.
[0117] In embodiments, the low friction coating may be relatively thin. For example, without limitation, the low friction coating may have a thickness of about 1 μm or less. In some embodiments, the low friction coating may have a thickness of about 100 nm or less. In other embodiments, the low friction coating may be about 90 nm or less, about 80 nm or less, about 70 nm or less, about 60 nm or less, about 50 nm or less, or about 25 nm or less. In embodiments, the low friction coating may have a thickness of 10 nm to 100 nm, 10 nm to 90 nm, 10 nm to 80 nm, 10 nm to 70 nm, 10 nm to 60 nm, 10 nm to 50 nm, 10 nm to 40 nm, 10 nm to 30 nm, 10 nm to 25 nm, or even 10 nm to 20 nm, or any range or subrange formed from these endpoints. In embodiments, the low friction coating may have a thickness of 20 nm to 100 nm, 20 nm to 90 nm, 20 nm to 80 nm, 20 nm to 70 nm, 20 nm to 60 nm, 20 nm to 50 nm, 20 nm to 40 nm, 20 nm to 30 nm, or even 20 nm to 25 nm, or any range or subrange formed from these endpoints. In the example coated glass containers described herein, the coating had a thickness in the range of 20 nm to 40 nm. The use of such a relatively thin coating in combination with a reduced thickness sidewall as disclosed herein promotes certain surprising mechanical and performance benefits (e.g., compliance, impact, horizontal / vertical compression, freeze-thaw, etc.) as further demonstrated and described herein.
[0118] The coated glass container described herein can be thermally stable after heating to a temperature of at least 260°C for 30 minutes. As used herein, the phrase "thermally stable" means that the low-friction coating applied to the glass article, as described in U.S. Pat. No. 9,763,852, remains substantially intact on the surface of the glass article after exposure to high temperatures, such that the mechanical properties of the coated glass article, specifically the coefficient of friction and horizontal compressive strength, are only minimally affected, if at all. This indicates that the low-friction coating remains attached to the glass surface after exposure to high temperatures and continues to protect the glass product from mechanical damage, such as abrasion, impact, and the like.
[0119] Reduced flange volume In an embodiment, the glass container 100 is formed with an area of reduced glass volume relative to the same area of a standardized glass container of the same type and size. For example, the flange 126 of a size X glass container 100 may be modified to include a smaller volume than the flange of a size X glass vial as defined by ISO 8362-1, where X is one of the following size designations: 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R. Such flanges are described, for example and without limitation, in U.S. Provisional Patent Application No. 63 / 277,488, which is incorporated herein by reference in its entirety. In addition to requiring less glass usage, glass containers including modified flange areas may provide functional benefits. For example, the modified flanges may enable improved sealing mechanisms for vials subjected to relatively low storage temperatures.
[0120] Glass containers, such as vials and syringes, used to store pharmaceutical compositions are typically sealed via stoppers or other closures to preserve the integrity of the contents. The closures are typically made of synthetic rubber and other elastomers. Such materials are beneficially high in permeation resistance and elasticity to facilitate insertion into the container and seal the interior of the container. However, the elasticity of commonly used closure materials may decrease at low temperatures. For example, synthetic rubbers currently used as closure materials may include a transition temperature of -70°C or higher and -10°C or lower. Below the transition temperature, closures constructed of such synthetic rubbers may behave as solids and may not be able to expand elastically to compensate for the relatively large difference between the thermal expansion coefficients of the glass and the crimped caps used to secure the closures to the containers. With this in mind, existing closure assemblies for pharmaceutical containers may break at temperatures of -20°C or lower. The glass containers and closure assemblies described below include reduced flange volumes and improved functionality in cryogenic storage applications.
[0121] 3, an embodiment of a glass container 300 is shown, including a glass container 302 and a sealing assembly 304. Although not described in detail herein, the glass container 302 and the sealing assembly 304 may include similar structures and features as the glass container 100 described herein and shown in FIG. 1. As shown in FIG. 3, the glass container 302 includes a neck 306 that extends to a flange 308 defined by an upper sealing surface 310, a lower surface 312, and an outer surface 314. As shown in FIG. 3, the outer surface 314 of the flange 308 is recessed radially inwardly to define a cutout portion 316 of the flange 308. The outer surface 314 of the flange 308 includes an upper surface portion 318 opposite the lower surface 312 and extending from an outermost edge 320 of the flange 308, and a vertical surface portion 322. The vertical surface portion 322 extends from a mating surface portion 324 of the upper surface portion 318 to the upper sealing surface 310. In an embodiment, the vertical surface portion 322 extends perpendicular to the upper surface portion 318. In an embodiment, an interface surface portion 324 extending between the upper surface portion 318 and the vertical surface portion 322 forms a chamfer. The upper surface portion 318, the outermost edge 320, and the lower surface 312 of the flange 308 cooperate to define a protrusion 326. It should be noted that in an embodiment, the seal assembly 304 is not provided with sharp corners, but rather, any angular surfaces should be chamfered or rounded to avoid stress concentrations.
[0122] In an embodiment, the sealing assembly 304 includes a stopper 328 and a metal-containing cap 330. However, it should be understood that in an embodiment, the metal-containing cap 330 may not be provided. The stopper 328 includes a sealing portion 332 terminating at an outer edge 334 and a rim 336 extending from the outer edge 334 of the sealing portion 332. The sealing portion 332 has an outer diameter D2 defined by the distance between the outer edges 334 of the sealing portion 332. When the stopper 328 is positioned on the glass container 302, the sealing portion 332 extends over the upper sealing surface 310 of the flange 308 and covers an opening 338 formed in the glass container 302. The rim 336 extends from the outer edge 334 of the sealing portion 332 at least partially along the outer surface 314 of the flange 308. 3, the rim 336 includes a bottom surface 340 that forms a gap between the upper surface portion 318 of the flange 308, an inner surface 342 that contacts the vertical surface portion 322 of the flange 308, and an interface portion 344 that extends between the bottom surface 340 of the rim 336 and the inner surface 342 of the rim 336. The bottom surface 340, the inner surface 342, and the interface portion 344 of the rim 336 are received within the cutout portion 316 of the flange 308. In embodiments in which the interface portion 324 of the flange 308 forms a chamfer, the interface portion 344 of the rim 336 also forms a nested chamfer. In embodiments in which a metal-containing cap 330 is provided, the protrusion 326 is provided between a bottom surface 340 of the rim 336 and an inner surface 346 of the metal-containing cap 330, specifically a lower portion 348 of the metal-containing cap 330 that extends radially inward along the underside 312 of the flange 308 toward the neck 306. Thus, the protrusion 326 of the flange 308 separates the rim 336 of the stopper 328 from the lower portion 348 of the metal-containing cap 330.
[0123] As discussed above, it will be appreciated that when the glass container 300 is subjected to relatively low storage temperatures, because the coefficient of thermal expansion of the stopper 328 is greater than the coefficient of thermal expansion of the glass container 302, the rim 336 of the stopper 328 shrinks around and toward the flange 308 of the glass container 302, thereby increasing the seal formed between the stopper 328 and the flange 308 of the glass container 302. More specifically, the sealing portion 332 of the stopper 328 shrinks during the relatively low storage temperatures such that the outer diameter D2 between the outer edges 334 of the sealing portion 332 decreases, resulting in the rim 336 becoming tighter around the outer surface 314 of the flange 308.
[0124] 4, a further embodiment of a glass container 400 is shown, including a glass container 402 and a sealing assembly 404. It should be understood that the glass container 400 is similar to the glass container 300 described herein and shown in FIG. 3, except for the mating surface portion 324 of the flange 308 and the mating surface portion 344 of the rim 336. As described herein and shown in FIG. 3, the mating surface portion 324 of the flange 308 and the mating surface portion 344 of the rim 336 of the glass container 300 form corresponding chamfers. However, the glass container 400 shown in FIG. 4 includes a mating surface portion 406 formed on the flange 308 and a mating surface portion 408 formed on the rim 336, each of which are arc-shaped and correspond to one another so as to nest with one another. The arc-shaped mating surface portions 406, 408 provide a smooth mating surface between the flange 308 and the rim 336 without sharp edges that may cause gaps between the flange 308 and the rim 336. Such gaps can result in air pockets forming between them or allowing air to escape through the seal that is formed.
[0125] It has been discovered that glass containers including flanges with reduced glass volumes, as shown in Figures 3 and 4, can provide unique advantages in the context of the thin-walled glass containers described herein. In addition to reducing the amount of glass material required to manufacture a glass container, thereby contributing to the sustainability aspects of the present disclosure, the reduced flange volume can also provide manufacturability benefits, which will be described in more detail in this disclosure.
[0126] While embodiments of glass containers having reduced flange volumes are described herein, it should be understood that such reduced flange volume flanges are optional, and glass containers having reduced wall thicknesses described herein need not also have reduced flange volume flanges.
[0127] chemical durability In addition to the increased mechanical properties of the glass container 100 due to the relatively thin sidewall, other properties of the glass container 100 may also be increased. For example, the chemical durability of the glass container 100, particularly the tendency to delaminate, may be improved when the glass container is formed with a relatively thin sidewall. When a glass article containing volatile species such as sodium and / or boron (e.g., more than 0.1 mol%, e.g., more than 0.5 mol%, more than 1 mol%, more than 2 mol%, more than 4 mol% Na2O and / or B2O3) is heated (e.g., when a glass tube is converted into a glass container such as a glass vial), the sodium and / or boron may volatilize and be released from the surface of the glass. The volatilized sodium and / or boron may subsequently condense at the cooler portions of the glass container surface, causing compositional inhomogeneity on the glass container surface. Such compositional inhomogeneity on the glass container surface may lead to a decrease in chemical durability and an increase in the tendency to delaminate on the glass surface.
[0128] The rate at which sodium and / or boron volatilizes correlates with the surface temperature of the glass. In the process of reforming glass tubes into glass pharmaceutical vials during conversion (such as the conversion process described in US Patent Application Publication No. 2022 / 0048804), the glass is heated by a gas / oxygen burner outside the glass tube. The heat is conducted through the thickness of the glass until the desired glass viscosity is achieved for reforming. Thermal modeling shows that once the necessary thickness viscosity is reached to facilitate thermal separation, a gradient of 150° C. can exist through the thickness of the glass during separation (i.e., when the formed or partially formed glass container is separated from the glass tube after formation). To achieve the correct average viscosity, the inner surface of the glass tube will have a very high viscosity and the outer surface will have a relatively low viscosity. As the glass thickness decreases (i.e., as the thickness of the glass container sidewall decreases), the thermal gradient will decrease and therefore the inner surface temperature will decrease at the same average thickness viscosity. Minimizing the inside surface temperature reduces the volatilization of sodium and / or boron, thereby improving the chemical durability of the resulting glass container.
[0129] FIG. 5 graphically illustrates the temperature profile for a 1.2 mm thick tube (baseline) and reduced thickness tubes as a function of wall thickness. An outside diameter (OD) temperature of 1450° C. was assumed to be the glass temperature to promote proper separation. A one-dimensional thermal scaling model was developed to evaluate the through-thickness viscosity and tensile force during separation. Using this model, the OD temperature was adjusted until the average through-thickness viscosity and tensile force for a given wall thickness were the same as the baseline conditions. Going from a 1.2 mm thick wall to a 0.5 mm wall, the outside surface temperature decreased by 180° C. For a wall thickness of 0.85 mm, the decrease in surface temperature was still 90° C. This data indicates that a lower separation temperature (i.e., the temperature used to separate the formed glass container from the remainder of the glass tube) can be used for thinner wall thicknesses. A lower separation temperature may reduce volatilization in the glass, which in turn may improve the chemical durability of the glass.
[0130] Referring now to FIG. 6, the same thermal scaling model was used to evaluate the temperature at the inside diameter (ID) of the tube at separation. As depicted in FIG. 6, the ID temperature at separation was reduced by 31° C. to 37° C. from the baseline for the thin walled tubes. As discussed above with respect to FIG. 5, a lower separation temperature may reduce volatilization in the glass, thus improving the chemical durability of the glass.
[0131] To further understand the effect of decreasing the glass temperature during separation on the volatilization of chemical species in the glass, a model was developed to determine the sodium vaporization rate as a function of the glass surface temperature. The model was based on Corning® Valor® aluminosilicate glass. The model demonstrated that even small changes in surface temperature can result in large changes in the reaction rate (i.e., volatilization rate). Figure 7A shows the equilibrium elemental fractions of sodium and boron in the gas phase as a function of temperature for Type 1B glass and aluminosilicate glass. Figure 7B shows the modeling results and model equations relating the sodium elemental fraction in the gas phase to temperature. Figure 8 shows the equilibrium elemental fractions of sodium and boron in the gas phase as a function of viscosity for Type 1B glass and Corning® Valor® aluminosilicate glass. As expected, an increase in glass temperature (i.e., a decrease in glass viscosity) correlates with an increase in the equilibrium levels of sodium and boron in the gas phase. The sodium evolution rate of Corning® Valor® aluminosilicate glass is shown in Table 2 for various wall thicknesses.
[0132] [Table 2]
[0133] As the equation in Figure 7A shows, the amount of sodium evolved during heating is a function of speed and time. The ID temperature model assumed the same part speed, but running the process faster reduces the exposure time. As shown in Table 2, for thin walled tubes / containers, the amount of sodium evolved on the inside surface can be reduced by up to 36%, which can improve the chemical durability of the resulting glass container.
[0134] Boron volatilization during conversion of glass tubes to glass containers is known to cause internal delamination of the vials, resulting in contamination of some pharmaceutical compositions. Similar to sodium volatilization, boron volatilization in glass tubes and containers with thinner side walls may also be mitigated due to the reduced side wall thickness resulting in shorter process times and lower surface temperatures.
[0135] Additionally, the reduced conversion time and surface temperature may also improve the chemical durability of the resulting glass container by better maintaining the uniformity of the glass composition in areas of the glass container that undergo significant modification during the conversion process. To experimentally verify that the glass containers described herein may achieve lower separation temperatures during conversion, temperature profiles were measured immediately prior to pulling the glass container from the tube (i.e., separating it) for a 3 ml vial with a wall thickness of 0.7 mm, a 3 ml vial with a wall thickness of 0.85 mm, and a 3 ml vial with a wall thickness of 1.1 mm. As can be seen from the temperature profiles shown in FIG. 9, the thinner walled vial could be pulled from the glass tube (i.e., separated from the glass tube) at a lower separation temperature than the thicker walled vial. This result suggests that the inner surface of the vial also experiences a reduced peak temperature when pulled during separation. Additionally, as discussed in more detail below, the reduced temperature experienced during separation should reduce the extent of sodium and boron volatilization and maintain good chemical durability.
[0136] To experimentally test this theory, the USP <660> Surface hydrolysis resistance (SHR) measurements according to the "Surface Glass Test" were performed on the isolated bottoms of glass containers corresponding to the separation temperature profile shown in Figure 9. The resulting SHR values for isolated bottoms having wall thicknesses of 0.7 mm, 0.85 mm, and 1.1 mm are shown in Figure 10. The results indicate that glass containers formed with thinner side walls allow separation at a lower temperature, and this separation at a lower temperature improves the surface hydrolysis resistance of the inner surface of the isolated bottom of the glass container. However, the surface hydrolysis resistance of the fully converted glass container also depends on the time and heat exposure the glass container experiences during aggregation and bottoming.
[0137] The glass containers described herein have chemical durability and resistance to degradation as determined in accordance with DIN 12116, ISO 695, ISO 720, ISO 719, and the CDR test method introduced above and described in further detail below.
[0138] Specifically, the DIN 12116 standard is a measure of the resistance of glass to degradation when placed in an acidic solution. Briefly, the DIN 12116 standard utilizes a ground glass sample of known surface area, which is weighed and then contacted with a proportional amount of boiling 6M hydrochloric acid for six hours. The sample is then removed from the solution, dried, and reweighed. The mass of glass lost during exposure to the acidic solution is a measure of the acid resistance of the sample, with lower numbers indicating greater durability. The results of the test are reported in units of half mass per surface area, specifically mg / dm2. 2 The DIN 12116 standard is divided into individual classes. Class S1 is 0.7 mg / dm 2 Class S2 shows a weight loss of up to 0.7 mg / dm 2 to 1.5 mg / dm 2 Class S3 indicates a weight loss of up to 1.5 mg / dm 2 to 15 mg / dm 2 Class S4 indicates a weight loss of up to 15 mg / dm 2The weight loss is greater than 1.
[0139] The ISO 695 standard is a measure of the resistance of glass to degradation when placed in a basic solution. Briefly, the ISO 695 standard utilizes a ground glass sample, which is weighed and then placed in a solution of boiling 1M NaOH + 0.5M Na2CO3 for 3 hours. The sample is then removed from the solution, dried, and reweighed. The mass of glass lost during exposure to the basic solution is a measure of the sample's resistance to alkali, with lower numbers indicating greater durability. Like the DIN 12116 standard, the ISO 695 results are reported in units of mass per surface area, specifically mg / dm2. 2 The ISO 695 standard is divided into individual classes: Class A1 is 75 mg / dm 2 Class A2 indicates a weight loss of up to 75 mg / dm 2 to 175 mg / dm 2 Class A3 indicates a weight loss of up to 175 mg / dm 2 The weight loss is greater than 1.
[0140] The ISO 720 standard is a measure of the resistance of glass to degradation in CO2-free purified water. Briefly, the ISO 720 protocol utilizes crushed glass particles, which are contacted with CO2-free purified water under autoclave conditions (121°C, 2 atm) for 30 minutes. The solution is then colorimetrically titrated with dilute hydrochloric acid until the pH is neutral. The amount of HCl required to titrate to a neutral solution is then converted to the equivalent of Na2O extracted from the glass, reported in μg Na2O per weight of glass, with lower values indicating greater durability. The ISO 720 standard is divided into individual types. Type HGA1 indicates an extractable equivalent of up to 62 μg Na2O per gram of glass tested, Type HGA2 indicates an extractable equivalent of greater than 62 μg to 527 μg Na2O per gram of glass tested, and Type HGA3 indicates an extractable equivalent of greater than 527 μg to 930 μg Na2O per gram of glass tested.
[0141] The ISO 719 standard is a measure of the resistance of glass to degradation in CO2-free purified water. Briefly, the ISO 719 protocol utilizes crushed glass particles, which are contacted with CO2-free purified water at a temperature of 98 °C and 1 atm pressure for 30 minutes. The solution is then colorimetrically titrated with dilute hydrochloric acid until the pH is neutral. The amount of HCl required to titrate to a neutral solution is then converted to the equivalent amount of Na2O extracted from the glass and reported in μg Na2O per weight of glass, with lower values indicating greater durability. The ISO 719 standard is divided into individual types. Type HGB1 exhibits an extraction equivalent of up to 31 μg Na2O, Type HGB2 exhibits an extraction equivalent of from 31 to 62 μg Na2O, Type HGB3 exhibits an extraction equivalent of from 62 to 264 μg Na2O, Type HGB4 exhibits an extraction equivalent of from 264 to 620 μg Na2O, and Type HGB5 exhibits an extraction equivalent of from 620 to 1085 μg Na2O. The glass compositions described herein have ISO 719 hydrolysis resistance of Type HGB2 or better, with some embodiments having the hydrolysis resistance of Type HGB1.
[0142] As mentioned above, USP <660> Another glass particle test that is often used in conjunction with the "surface glass test" is the USP <660> The "glass grain test" is a method for determining the type of glass used. Briefly, the glass grain test involves the use of crushed glass grains, which are contacted with CO2-free purified water at a temperature of 121°C and 1 atmosphere for 30 minutes. The solution is then colorimetrically titrated with dilute hydrochloric acid until the pH is neutral. The amount of HCl required to titrate to a neutral solution is determined and used to classify the glass as Type I (Type I borosilicate glass) or Type II / III (soda-lime-silica glass). If the amount of titrant per gram of glass is 10ml or less, the glass is considered Type I. If the amount of titrant per gram of glass is greater than 10ml / less than or equal to 0.85ml, the glass is considered Type II / III.
[0143] The glass containers described herein have an acid resistance of at least class S3 according to DIN 12116 both before and after ion-exchange toughening, with some embodiments having an acid resistance of at least class S2, or even S1, after ion-exchange toughening. In some other embodiments, the glass containers may have an acid resistance of at least class S2 both before and after ion-exchange toughening, with some embodiments having an acid resistance of class S1 after ion-exchange toughening. Additionally, the glass containers described herein have a base resistance according to ISO 695 of at least class A2 both before and after ion-exchange toughening, with some embodiments having a base resistance of at least class A1 after ion-exchange toughening. Additionally, the glass containers described herein have a hydrolysis resistance of ISO 720 type HGA2 both before and after ion-exchange toughening, with some embodiments having a hydrolysis resistance of type HGA1 after ion-exchange toughening, and some other embodiments having a hydrolysis resistance of type HGA1 both before and after ion-exchange toughening. The glass containers described herein have an ISO 719 hydrolysis resistance of Type HGB2 or better, with some embodiments having a hydrolysis resistance of Type HGB1. When referring to the above referenced classifications according to DIN 12116, ISO 695, ISO 720 and ISO 719, it should be understood that a glass composition or glass article having "at least" the specified classification means that the performance of the glass composition is equal to or better than the specified classification. For example, a glass container having a DIN 12116 acid resistance of "at least class S2" may have a DIN 12116 classification of either S1 or S2.
[0144] The method for assessing the CDR of glass containers involves (1) a hydrolysis test of the untreated surface, (2) an etching step to remove any chemical inhomogeneities that may be present, and (3) a second hydrolysis test of the "etched" surface. The "untreated" containers are <660> The surface is treated according to the glass test, with one notable deviation: the fill volume is 12.5% of the full capacity. Because of the reduced fill volume, an additional vessel is required to produce the amount of solution required for the titration. The titer is recorded as the "untreated" response.
[0145] Second USP <660> Surface glass testing is performed on the "etched" vessels to measure the bulk glass response, again at a reduced fill of 12.5%. The etching process removes material that has been deposited or entrained during the conversion or shaping process. At least 1 μm (depth) of the surface is removed using a mixture of HCl / HF acid with a target concentration of 2.3M HF / 4.6M HCl. The vessels are exposed to this solution for a minimum of 3 minutes. These conditions are sufficient for most Type 1 glass compositions, and mass loss is measured to confirm sufficient depth of surface removal. After exposure to the target acid solution, any acidic residues within the vessels are removed by immersion in two room temperature water baths for 5 minutes each. The vessels are then rinsed several times with high purity water. The vessels used for the "etched" response are the retained vessels from the "untreated" tests.
[0146] "Etched" containers are USP <660> According to the surface glass test, a reduced fill volume (12.5% of full volume) is used to process. The resulting titrant volume is recorded as the "etched" titrant response. The ratio of the recorded titrant volumes is calculated (*by the reduced volume) as follows: TIFF2024536026000005.tif11114
[0147] The CDR value represents the risk of delamination, with containers with uniform surface chemistry exhibiting a low ratio and the lowest risk of delamination.
[0148] From the CDR results, USP <660> It was shown that vials and pharmaceutical containers considered "Type I" in the European Pharmacopoeia (Ph.Eur.3.2.1) can contain a wide range of chemical durability. The CDR method has been demonstrated to quantitatively distinguish populations with known variability in performance (i.e., delamination populations). Thus, the CDR method can be used to compare glass containers with different manufacturing histories to better understand the effect that various processing parameters may have on the delamination resistance of the resulting glass container. Containers with uniform surface chemistry have the lowest risk of delamination and exhibit low CDR ratios.
[0149] In addition to the CDR method described above, the chemical durability of the glass containers described herein was also evaluated to determine the inorganic element concentrations that can be extracted from the container in the presence of solutions. The extractables test method involves the use of various pH solutions that are added to the glass container to better understand the potential interactions between the container and the pharmaceutical product stored therein. Three solutions are used to evaluate the thin-walled glass containers: a pH 3 solution of HCl (ACS grade) + 18 MΩ H2O, a pH neutral 18 MΩ H2O, and a pH 10 solution of NH4OH (ACS grade) + 18 MΩ H2O. The converted glass containers are washed with 18 MΩ H2O and then air dried in a laminar flow hood. The glass containers are then filled to 90% full with one of the test solutions. The samples are then capped using Teflon coated septa and aluminum caps. The water samples are aged in an autoclave cycle with a 1 hour hold at 121°C. The total cycle time, including heating and cooling, is 2 hours. The acid and base solutions are aged for 4 days in a static incubator at 70 °C. Once the solutions have cooled to room temperature, they are transferred from the glass containers to pre-cleaned centrifuge tubes. The solutions are analyzed by inductively coupled plasma mass spectrometry (ICP-MS). The ICP-MS instrument is used according to standard operating procedures and daily calibration standards (CAL-19-368).
[0150] The chemical durability results for the CDR and ICP-MS methods described above are presented below in a discussion of the manufacturing benefits of glass containers formed with sidewalls of reduced thickness compared to conventional glass vials of the same outer diameter.
[0151] Thermal properties Without being bound by theory, it is believed that glass containers 100 formed with thinner sidewalls may have a lower thermal mass and therefore may have a shorter cooling time during tube manufacture and tube-to-vial conversion. By decreasing the cooling time, the fictive temperature of the glass may be increased, which is known to improve the chemical strengthening ability of glass. In particular, by increasing the fictive temperature of the glass, the glass container may be chemically strengthened to a desired surface compressive stress and layer depth more quickly than a glass container having a higher fictive temperature. As discussed above, this may increase the throughput of the chemical strengthening process and / or reduce the cost of the chemical strengthening process.
[0152] Additionally, it is believed that glass containers 100 formed with thinner sidewalls may reduce thermal stresses in the glass resulting from the tube-to-vial conversion process, which may reduce or eliminate the need for a post-formation annealing step used to remove residual thermal stresses.
[0153] Additionally, glass containers 100 formed with thinner sidewalls may experience lower thermal shock stresses, and therefore may be able to increase temperature more slowly during processing and / or avoid processes to reduce the risk of thermal shock damage, such as using preheat chambers during processing, thereby increasing manufacturing throughput and reducing manufacturing costs.
[0154] Furthermore, for glass containers 100 formed with thinner side walls, bending stresses resulting from processes that freeze the contents of the container, such as during cryogenic storage and freeze-drying, may be better withstood by the thin-walled glass container with the external coating when compared to uncoated conventional glass containers having the same outer diameter. Although glass containers with thinner side walls are generally expected to have increased breakage rates due to their smaller cross-sectional area, limiting the allowable peak stresses resulting from the expansion of the contents, it has been unexpectedly found that outer coated glass containers formed with reduced thicknesses can withstand freezing conditions better than uncoated conventional glass containers having the same outer diameter. Without wishing to be bound by theory, it is believed that the increased compliance resulting from the thin walls, combined with the avoidance of defect formation provided by the external coating, results in a glass container with improved resistance to breakage under freeze-thaw conditions.
[0155] To examine this theory, coated glass pharmaceutical vials with an ISO 8362-1 size designation of 2R and a wall thickness of 0.7 mm (70% of conventional wall thickness) and uncoated glass pharmaceutical vials with an ISO 8362-1 size designation of 2R and a wall thickness of 1.0 mm (conventional) were subjected to identical freezing conditions (hereafter referred to as the "freeze-thaw test") and freeze-thaw survival rates were measured. The coating applied to the glass pharmaceutical vials with reduced wall thickness was a low-friction, thermally stable polyimide coating as described above. To replicate fill-line damage, a 20 mm 30 N scratch was applied to the exterior surface of the glass container (i.e., the coating of the coated vial or the glass of the uncoated vial) using the vial-on-vial fixture 700 shown in FIG. 32. The vial-on-vial fixture 700 and the method of applying scratches to the exterior surface of the glass container are described in more detail herein. The glass containers were then filled to 50% of full capacity with 5% mannitol solution and placed in a -40°C freezer for at least 24 hours, then removed from the freezer and allowed to cool naturally. One hundred samples per vial type were tested. If no fracture was observed after the sample had cooled, the sample was considered to have "survived" the freeze-thaw test. The freeze-thaw survival rate was determined by calculating the percentage of the sample population that survived the freeze-thaw test.
[0156] The freeze-thaw survival rate of the exterior coated glass containers with a reduced wall thickness of 0.7 mm was 99%, while the freeze-thaw survival rate of the uncoated glass pharmaceutical vials with a wall thickness of 1.0 mm was 44%. The low friction coating applied to the thin-walled glass containers in this experiment was a polyimide coating as described herein, with a coating thickness of 20 nm to 40 nm. The results indicate that exterior coated glass containers, such as the exterior coated glass pharmaceutical vials described herein, exhibit improved breakage resistance under low temperature storage conditions compared to conventional glass vials with the same outer diameter. That is, it was unexpectedly found that reducing the thickness of the vial sidewall and including a thin coating on the vial sidewall have a synergistic effect of improving the mechanical performance of the glass container under freezing (and thawing) conditions.
[0157] In embodiments, the term “low temperature storage modulus” as used herein refers to a temperature coefficient of thermal expansion (TCS) that is equal to or less than 0.85*s1. iwhere s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and (ii) the freeze-thaw survivability of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1. In an embodiment, the term "cold storage modulus" refers to a glass container (or an exterior coated glass container, if a coating is present) including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 in which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the freeze-thaw survivability of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1. In embodiments, the term "cold storage modulus" as used herein refers to the temperature coefficient of thermal expansion (TCS) of a glass vial (or an exterior coated glass vial, if a coating is present) that includes a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, in which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. iwhere s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the freeze-thaw survivability of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1.
[0158] In some embodiments, the outer coated glass container 100 may have a cold storage coefficient of at least 1.5, at least 1.75, at least 2.0, or at least 2.25.
[0159] Additionally, glass containers 100 formed with thinner side walls have a lower thermal mass, allowing the glass to cool more quickly, which in turn allows the contents to freeze and nucleate on the side walls of the container. Without wishing to be bound by theory, it is believed that by promoting nucleation on the side walls of the container in addition to the bottom of the container, the contents of the glass container can be frozen more quickly.
[0160] In general, glass containers 100 formed with thinner sidewalls can be heated and / or cooled faster than glass containers formed with relatively thicker sidewalls, resulting in energy savings and faster throughput rates in any process requiring thermal manipulation of glass containers.
[0161] manufacturability Reducing the thickness of the sidewall of the glass container can also improve the manufacturability of the glass container. In particular, reducing the thickness of the sidewall of the glass container can increase the throughput of the tube-to-vial conversion process, allowing more glass containers to be produced per unit time. For context regarding the tube-to-vial conversion process, see U.S. Patent Application Publication No. 2022 / 0048804.
[0162] The throughput / rate of the tube-to-vial conversion process can be calculated based on the step of thermally separating the formed containers from the tube feedstock, as this step of the conversion process is typically the rate-limiting step in converting standard vials, such as ISO 8362-1 vials. Furthermore, one skilled in the art can quantify metrics based on thermal separation by considering that the wall thickness of the glass tubes is constant and that the thermal separation process typically involves heating the same area across three successive stations of a tube-to-vial converter.
[0163] The heat capacity equation can be used to model the thermal separation process. In particular, the thermal energy q during the thermal separation process can be defined as: q=m C p ·ΔT (Formula 1) where q is the thermal energy, m is the mass, and C p is the specific heat capacity and ΔT is the change in temperature. The mass m is expressed in terms of the cross-sectional area A of the glass tube, as follows: A = π / 4 [OD 2 -ID 2 ]=π / 4[OD 2 -(OD-2 Wall) 2 ] (Formula 2) where OD is the outside diameter of the glass tube, ID is the inside diameter of the glass tube, and Wall is the thickness of the side wall of the glass tube.
[0164] Specific heat capacity C p is constant for a given glass composition. The temperature change ΔT is relatively constant for a given transducer machine setting (i.e., from room temperature to the separation temperature).
[0165] Consider a tube-to-vial conversion process that converts a glass tube with an outer diameter of 16 mm and a wall thickness of 1 mm into a glass pharmaceutical vial. If a glass tube with a larger wall thickness (e.g., greater than 1.0 mm) were used in the same process (i.e., the same thermal separation process with the same burner settings), the glass tube would not separate because the increased area (i.e., mass) of the relatively thick glass would not achieve the desired viscosity (i.e., the glass would be too cold) to facilitate separation. That is, if the heating rate of the burner used for thermal separation were to remain constant, the part speed of the tube-to-vial conversion process would need to be slowed down to heat the glass tube sufficiently for thermal separation. However, if a glass tube with a thinner wall thickness (e.g., less than 1.0 mm) were used and the heating rate of the burner used for thermal separation were to remain constant, the part speed of the tube-to-vial conversion process may be increased to maintain the same total heat input into the glass tube to facilitate thermal separation.
[0166] Therefore, the part rate of the tube-to-vial conversion process is inversely proportional to the cross-sectional area of the tube for a given process setting: Part speed ∝ 1 / area (Eq. 3) It is.
[0167] This relationship has been experimentally verified. Figure 12 shows the separation rate as a function of tube cross-sectional area at constant burner power for 3 ml vials with wall thicknesses of 0.7 mm, 0.85 mm, and 1.1 mm. As can be seen from Figure 12, the separation rate is inversely proportional to the cross-sectional area of the tube. Thus, the use of glass tubes with reduced sidewall thickness is expected to increase the part rate of the tube-to-vial conversion process, and thereby increase the overall throughput of the tube-to-vial conversion process, since other steps can be sped up for thinner walled vials as well. Alternatively, the same part rate can be achieved by lowering the flame temperature and energy usage in the tube-to-vial conversion process when producing vials with reduced wall thickness.
[0168] Another step in the tube-to-vial conversion process is the heating and forming of the flange portion of the vial. This processing step, referred to herein as "aggregation," is different for thin-walled glass containers because the tube length, or "aggregation height," required to produce a flange with the same glass volume is larger. For example, to produce a glass vial with a flange of dimensions defined by ISO 8362-1, a larger aggregation height is required because the relatively thin glass tube has less glass per unit length. Thus, the question arises as to whether the aggregation rate, e.g., mm of tube per second, of a vial with a thinner wall can be increased so that the aggregation step can be performed in the same or shorter time as the aggregation step of a vial of the same size with a conventional wall thickness (e.g., as defined by ISO 8362-1). It has been discovered that the aggregation rate can be significantly increased by slightly increasing the heat output from the gas burner used to heat the glass tube during the aggregation step. To confirm this, an aggregation study was conducted in which glass pharmaceutical vials, having a 2R size designation according to ISO 8362-1 and formed from Type 1B borosilicate glass with thicknesses of 1.0 mm and 0.7 mm, were converted to change heat output while controlling the gas flow rate to the burner. With only an 8% increase in gas flow rate to the burner, the aggregation rate increased by 181%. This increase was maintained throughout an aggregation stage of approximately 500 vials for each of the 1.0 mm and 0.7 mm 2R vials (see Table 13 for specific values). This increase in aggregation rate was sufficient to achieve the same aggregate part rate (vials per minute, "VPM") of 47 VPM for the 0.7 mm 2R vials as was obtained with the 1.0 mm 2R vials. Additionally, and importantly, the increase in burner power during the aggregation step did not diminish the chemical durability of the 0.7 mm glass vials.
[0169] In particular, the surface hydrolysis resistance (SHR) of the vial inner surface obtained from the aggregation study was compared with the above USP <660> The test was evaluated according to the "Glass Surface Test" USP <660> The test was repeated using 10 specimens each of 0.7 mm and 1.0 mm wall thicknesses, and the results are shown in Table 3A below.
[0170] [Table 3A]
[0171] The SHR measurements shown in Table 3A show that 2R vials with a wall thickness of 0.7 mm and produced using 8% higher burner power (to increase aggregation rate) performed just as well as 2R vials with a wall thickness of 1.0 mm in the USP <660> maintains a Type I or Type II classification (i.e., less than 1.6 ml HCl 0.01M titer) according to USP <660> Vials having Type I and Type II classification according to are considered to have high hydrolytic resistance.
[0172] Table 3B below shows the results of the vials from the aggregate study. <usp>660 "Glass Particle Test" results are shown.
[0173] [Table 3B]
[0174] Three sets of glass particles from 2R glass pharmaceutical vials with a wall thickness of 0.7 mm and three sets of glass particles from 2R glass pharmaceutical vials with a wall thickness of 1.0 mm were measured according to USP <660> The vials were tested under the "Glass Particle Test". For 2R 0.7 mm wall thickness vials, the average value of the titrant volume (ml / g) per gram of glass tested was 0.035, and for 2R 1.0 mm wall thickness vials, the average value of the titrant volume (ml / g) per gram of glass tested was 0.038. Therefore, pharmaceutical vials made of 2R glass with a wall thickness of 0.7 mm meet the USP <660> It maintained its Type I designation in accordance with the "glass bead test."
[0175] The delamination tendency of glass pharmaceutical vials was measured in terms of chemical durability ratio and the method for determining CDR introduced and explained above. CDR measurements were performed using two 2R glass pharmaceutical vials with a wall thickness of 0.7 mm and two 2R glass pharmaceutical vials with a wall thickness of 1.0 mm. The results of the CDR measurements are shown in Table 4 below.
[0176] [Table 4]
[0177] The CDR measurements shown in Table 4 indicate that 2R vials with a wall thickness of 0.7 mm and manufactured using 8% higher burner power (to increase aggregation rate) do not have an increased tendency for delamination compared to 2R glass pharmaceutical vials with a wall thickness of 1.0 mm aggregated at lower burner power.
[0178] Finally, to further evaluate the effect of the reduction in wall thickness of glass pharmaceutical vials on the resulting chemical durability, the ICP-MS method for measuring extractable elements described above was performed using 2R glass pharmaceutical vials formed from type 1B borosilicate glass and having a wall thickness of 0.7 mm, and 2R glass pharmaceutical vials having a wall thickness of 1.0 mm. The vials used for the ICP-MS measurements were manufactured during the aggregation study described above. The ICP-MS testing described herein involved three samples filled with each of the three solutions for each vial type (0.7 mm 2R and 1.0 mm 2R), and two aliquots were measured from each sample. The results of the ICP-MS measurements are shown in Figures 11A-11C. The differences in the concentrations of extractable elements shown in Figures 11A-11C are expected based on the variability of a typical conversion process. Therefore, the ICP-MS results reinforce the chemical durability results discussed above in further proving that the increased burner power utilized to aggregate thin-walled glass pharmaceutical vials at faster rates did not sacrifice the resulting chemical durability.
[0179] Although the glass vials in the foregoing examples were formed from Type 1B borosilicate glass, it is believed that vials formed from aluminosilicate glasses, such as Corning®'s Valor® aluminosilicate glass, would exhibit similar trends with respect to SHR and CDR and ICP-MS measurements, at least because aluminosilicate glasses, particularly boron-free or low-boron aluminosilicate glasses, generally have chemical durability equal to or greater than Type 1B borosilicate glass.
[0180] The ability of the glass containers having reduced wall thickness described herein to maintain chemical durability properties despite being aggregated at higher burner power may be at least partially attributed to the reduced thermal gradients associated with the relatively thin walls. Furthermore, it is believed that the burner power during the aggregation step can be further increased without sacrificing chemical durability such that the thin-walled glass containers disclosed herein achieve aggregation rates higher than those achievable with corresponding vials of conventional wall thickness as defined by ISO 8362-1.
[0181] To explain further, the part rate or total cycle time of the tube-to-vial conversion process is the sum of the index time (i.e., the time it takes to move the glass tube from station to station in the machine) and the residence time of the glass tube at each station (i.e., the time the glass tube spends in front of the burner of the tube-to-vial conversion process). For the same tube size, the part rate can be successfully scaled using residence time and a mass flow controller (MFC) to fuel the burner. For example, consider a glass tube with an outer diameter of 16.00 mm and a sidewall thickness of 1.00 mm being converted into glass pharmaceutical vials in a tube-to-vial conversion process running at a part rate of 45 vials per minute (VPM). Assume the index time of the tube-to-vial conversion process is 0.30 seconds. The total cycle time is 60 / 45=1.33 seconds. The residence time is 1.33-0.30 seconds=1.03 seconds. If the process is slowed to 35 VPM, the new total cycle time is 60 / 35 = 1.71 seconds. The dwell time is 1.71 - 0.30 seconds = 1.41 seconds. The dwell time is reduced by 37% for a process with a part speed of 45 vials per minute (VPM). Therefore, to maintain the same heat output, the fuel flow rate through the MFC must be reduced by 37%. Conversely, if the dwell time goes from 1.41 seconds to 1.03 seconds, the part speed increases from 35 VPM to 45 VPM, which is an increase of 29%.
[0182] Therefore, only the tube cross-section and machine index time are required to evaluate the impact of glass tubes with reduced sidewall thickness on the part rates of a tube-to-vial conversion process (assuming that it is possible to increase the aggregation rate at least as much as the separation rate). The results of this analysis are graphically shown in Figure 13 for three different glass tube dimensions (16.75 mm OD x 1.1 mm wall thickness; 24 mm OD x 1.0 mm wall thickness; and 30 mm OD x 1.2 mm wall thickness) as well as a baseline tube-to-vial conversion process (i.e., VPM rates of 45 VPM, 35 VPM, and 25 VPM, respectively). Notably, the analysis of the process using three different dimensions of glass tubes and their corresponding part rates illustrates the impact of reducing the wall thickness of glass tubes, which may result in different baseline rates. Cross-sectional area scaling was used to generate new conversion rates based on different tube wall thicknesses ranging from 0.5 mm to 1.2 mm. It is believed that the use of glass tubes with reduced sidewall thickness, as shown in FIG. 13, will significantly increase the part rate of the tube-to-vial conversion process, thereby increasing the overall throughput of the tube-to-vial conversion process.
[0183] Table 5 below includes data on the effect of reducing the wall thickness of glass tubing on the part velocity (VPM) in a tube-to-vial conversion process. In Table 5, "CS" refers to the cross-sectional area of the glass tube used to form the vial, and "CS ratio" refers to the ratio of the cross-sectional area of the glass tube to the cross-sectional area of a glass tube having an outer diameter of 16.75 mm and a wall thickness of 1.1 mm. In particular, the tube-to-vial conversion part velocity was calculated for a 16.75 mm outer diameter glass tube having a wall thickness of 1.2 mm to 0.5 mm. This calculation shows that the part velocity (VPM) of the tube-to-vial conversion process can be increased by using glass tubes with reduced wall thickness. That is, the throughput of the tube-to-vial conversion process can be increased by reducing the wall thickness of the glass tubing material used in the tube-to-vial conversion process.
[0184] [Table 5]
[0185] In view of the above, it is believed that the use of glass tubes with reduced sidewall thickness will increase the part rate of the tube-to-vial conversion process, thereby increasing the overall throughput of the tube-to-vial conversion process.
[0186] Reduced flange volume As discussed above, in some embodiments, the glass container 100 is formed with an area of reduced glass volume relative to the same area of a standardized glass container of the same type and size. For example, the flange 126 of a size X glass container 100 may be modified to include a smaller volume than the flange of a size X glass vial as defined by ISO 8362-1, where X is one of the following size designations: 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R. Such an embodiment is shown in Figures 3 and 4. It has been discovered that such a design can reduce consolidation time (i.e., the time required to consolidate the softened glass of the tube to form the flange portion of the container) because less glass is required to form the flange, thereby reducing the required consolidation height. The consolidation height required to produce the reduced flange volume relative to the standard flange is shown in Figure 14. The demonstrated reduction in consolidation height reduces the amount of heating required during the consolidation step of the conversion process. Thus, for the same burner power, producing flanges with reduced volume, such as those discussed above for cryogenic storage applications, will reduce the time required to consolidate the glass into the flange. Thus, the combination of reduced wall thickness and reduced flange volume synergistically increases the overall throughput of the tube-to-vial conversion process by separately increasing the separation rate and decreasing the time required for consolidation.
[0187] An additional benefit of reduced flange volume is that the annealing step may be reduced or eliminated. Residual stresses from the conversion process typically require an annealing cycle to remove the stress and obtain a uniform vial stress distribution. However, it has been found that glass articles with thinner walls have reduced residual thermal stresses as a result of the reduced thermal gradients across the thickness of the sidewalls during cooling. However, for example, the flanges of glass pharmaceutical vials cool from the aggregate conversion process in a relatively thick state and therefore do not benefit from the thinner walls to the same extent as the sidewalls of the vials. Thus, the flanges suffer higher thermal gradients and corresponding residual stresses upon cooling. Thus, in some embodiments, the glass article has an area of reduced flange volume with reduced thermal gradients upon cooling, similar to the sidewalls of the disclosed thin-walled glass containers. Thus, the combination of reduced wall thickness and reduced flange volume may be particularly advantageous when reducing or eliminating annealing cycles, as it reduces the residual thermal stresses that the annealing step is intended to relieve.
[0188] Vial neck shape As briefly discussed above with reference to the reduced flange volume (see Figures 3 and 4), the formed glass pharmaceutical vial may be filled with a pharmaceutical composition and then capped using a capping machine. During the capping process, the neck 128 of the vial may come into contact with a part of the capping machine called the rail. Contact between the rail of the capping machine and the neck 128 of the glass pharmaceutical vial may result in cosmetic damage to the neck 128 of the glass pharmaceutical vial, or even a serious defect (i.e., a defect more serious than a superficial cosmetic damage) that may reduce the strength of the glass pharmaceutical vial and result in vial failure and product loss.
[0189] It has now been found that reducing the thickness of the sidewall of a glass pharmaceutical vial can not only reduce the thickness of the neck 128 of the glass pharmaceutical vial, but also reduce the outside diameter of the neck 128, thereby reducing the risk of contact between the rails of a capping machine and the neck 128 of the glass pharmaceutical vial, thereby reducing the potential for damage to the glass pharmaceutical vial. Referring to FIG. 1, the inside neck diameter (neck ID) N of a glass container is ID If is held constant, a glass container formed from a thinner side wall will have a smaller neck outer diameter (neck OD) N OD (assuming that the neck wall thickness is not intentionally increased). The flange outer diameter F OD is typically fixed according to the vial specifications.
[0190] In particular, for most vials, glass tubing with a sidewall thickness of 1.0 mm or less results in a glass pharmaceutical vial with a neck outer diameter sufficient to avoid damage from the rails of a capping machine. For example, FIG. 15 shows the relationship between tube wall thickness and the neck thickness of the resulting glass vial (i.e., glass vials with size designations of 6R and 2 ml (with European Standard Blowback (ESBB))). As shown in FIG. 15, as the tube wall thickness decreases, the neck thickness also decreases. FIG. 16 shows the relationship between tube wall thickness and the neck outer diameter of the resulting glass vial (i.e., glass vials with size designations of 6R and 2 ml). As shown in FIG. 16, as the tube wall thickness decreases, the neck outer diameter also decreases. As described herein, reducing the neck outer diameter of a glass pharmaceutical vial helps to avoid contact with the rails of a capping machine, which in turn reduces or mitigates damage to the glass pharmaceutical vial. That is, reducing the wall thickness of glass pharmaceutical vials can help avoid damage to the glass pharmaceutical vials during filling and capping.
[0191] Figure 17 shows the measured neck outer diameter data (30 vials of each) for 3ml thin-walled vials (wall thickness 0.7mm) and 3ml standard-walled vials (wall thickness 1.1mm). As can be seen, the thin-walled vials have an outer neck diameter that is at least 2mm smaller than the outer neck diameter of the corresponding standard-walled vial. One specific manufacturing benefit of the smaller neck outer diameter is the larger process window for the location of the rail capper that can avoid damage and breakage of the vial.
[0192] To understand the process window of the rail capper location with respect to damage caused to the neck of the vial, a vial capping experiment was conducted, the results of which demonstrate how a vial with a smaller neck outer diameter allows for a wider process window. FIG. 18 shows the process window of the rail capper location during the experiment, where two vial sizes were tested: 10R and 10ml. The "large 10R" and "large 10mL" vials, with neck outer diameters greater than 16.5mm and greater than 16.1mm, respectively, represent vials with conventional wall thickness. The "small 10R" and "small 10mL" vials, with neck outer diameters less than 16.5mm and less than 16.1mm, respectively, represent vials formed with relatively thin walls. The numbers in FIG. 18 correspond to the incremental positions at which the capper can be positioned relative to the rail capper device. As can be seen, the operating range of the capper is greater for vials with smaller neck outer diameters. Thus, it has been demonstrated that the outer neck diameter of the vial can be reduced by using thinner walls, which in turn allows for a larger operating window for the rail capper position. Furthermore, a larger operating window for the rail capper would reduce the probability of the neck being damaged during cap crimping due to the increased distance between the cap crimping tool and the vial neck.
[0193] Filling Line Profit The glass containers described herein include increased compliance relative to conventional glass containers. The increased flexibility of the glass container 100 due to the thinner sidewall 120 reduces the probability of process disruptions and breakages associated with misalignment of the glass container with filling line equipment such as star wheels and screw feeds. In particular, the increased flexibility of the glass container 100 formed with the thinner sidewall reduces the filling line forces on the container during a sudden stop event on the filling line. That is, the increased flexibility of the glass container 100 due to the thinner sidewall distributes the forces over a larger area as the container flexes under an applied load, reducing the overall force per unit area on the container. Such reduced forces result in less stress on the container, which suffers less damage and ultimately breaks.
[0194] Additionally, the combination of increased flexibility of the glass containers and the presence of a low friction coating applied to the exterior surface of the glass containers has a synergistic effect that provides several benefits. To demonstrate these benefits, accumulator table experiments were conducted in which uncoated 1.1 mm 3 ml vials and coated 0.7 mm 3 ml vials were monitored for jams and intervention events. The phrase "intervention rate" refers to the rate of events (events per hour (eph)) that require human intervention to repair a jam or stoppage along the filling line. These events may be caused by, for example, but not limited to, jams due to interactions between containers or containers and equipment, stoppages due to broken containers, etc., each of which may cause downtime and / or underutilization of equipment on the filling line. The phrase "jam rate" specifically refers to the rate of jams per minute.
[0195] Coating compositions, application procedures, and coating thicknesses are described herein. The accumulator experiments involved flowing vials through a restrictor table 450, shown in FIG. 19, at 400 vials per minute, a speed typical of a filling line. The restrictor table 450 includes a table surface 451, a track 452 that includes a paddle position gauge (not shown in FIG. 19), and a positioning block 453 used to position a wedge-shaped Delrin paddle 454 in the path of the vial (labeled "vial flow direction" in FIG. 19). The table surface 451 is circular in shape and has a diameter of 42 inches (106.68 cm). The track 452 extends radially from the center of the table surface 451 and includes a longitudinal axis 452-1. The paddle 454 includes a longitudinal axis 454-1 and has a longitudinal length of approximately 8 inches (20.32 cm). Paddle 454 is connected to positioning block 453 via rod 453-1. Zero line 454-2 extends from the connection point of paddle 454 to rod 453-1 in a direction parallel to longitudinal axis 452-1 of track 452. Paddle 454 can be rotated such that the angle θ between longitudinal axis 454-1 of paddle 454 and zero line 454-2 can be adjusted, thereby adjusting the gap t between outer tip 454-3 of paddle 454 and circumferential boundary 451-1 of table surface 451 as well as the angle between the approaching vial and paddle 454. g In the accumulator experiment, the angle θ was set to 80° and the gap t g The rotation speed of the table surface 451 was set to 3.8 rpm (approximately 0.063 s -1 ) was set.
[0196] FIG. 20A shows the number of jams recorded over a one hour period for each of the tested vial types. As can be seen, there were significantly fewer jam events associated with the test run of the 0.7 mm vials, which may be at least partially attributed to the combination of improved vial compliance and the low friction coating. While flowing the vials through the limit table 450 at a rate of 400 vials per minute, the jam rate for the 0.7 mm vials was about 2.4 jams / min, and the jam rate for the 1.0 mm vials was about 3.2 jams / min. Thus, in embodiments of the coated glass containers described herein, the jam rate may be 3 jams / min or less, 2.75 jams / min or less, or even 2.5 jams / min or less.
[0197] Additionally, as shown in Figure 20B, the coated 2R vials with a wall thickness of 0.7 mm required significantly less line intervention. While flowing vials through restrictor table 450 at a rate of 400 vials per minute for one hour, the intervention rate for the 2R vials with a wall thickness of 0.7 mm was approximately 47 eph, while the intervention rate for the uncoated 2R vials with a wall thickness of 1.0 mm was approximately 94 eph.
[0198] In embodiments, the coated glass containers described herein have a coating composition of 1.0×R I It can have the following intervention rates, R I is the intervention ratio for an uncoated glass container having a conventional thickness. In an embodiment, the intervention ratio is 0.90×R I Below, 0.80×R I Below, 0.70×R I Below, 0.60×R I Less than or equal to 0.50×R I It may be the following.
[0199] Without wishing to be bound by theory, it is believed that these improvements result from the combination of the increased compliance of thin-walled vials and the presence of a low-friction coating. Furthermore, the improved filling performance of thin-walled vials may allow filling lines using such thin-walled vials to be run at higher speeds while requiring the same amount of intervention as vials with conventional thicknesses that are run at relatively slower speeds. Thus, in some embodiments, an exterior-coated glass container with reduced wall thickness can be run at a higher speed on a filling line compared to a conventional glass vial with the same outer diameter but lacking compliance and an exterior coating.
[0200] mechanical performance As discussed above, glass containers, such as glass pharmaceutical vials, formed with a sidewall of reduced thickness compared to a conventional glass vial having the same diameter may have certain mechanical advantages. In particular, reducing the thickness of the sidewall increases the flexibility or compliance of the vial under an applied load directed perpendicular to the sidewall. As the sidewall flexes in response to an applied load, the force of the applied load is distributed over a larger area of the sidewall. Thus, for a given applied load, a vial with a more flexible sidewall will experience a lower peak load at the load point than a vial with a stiffer sidewall (i.e., thicker). In particular, as the vial flexes in response to an applied load, the force of the applied load is distributed over a larger area. Furthermore, under certain loading conditions, the possibility of surface damage and / or breakage can be reduced by reducing the overall stress of the material per unit area. This is especially true for externally coated vials, such as the coating compositions and application procedures disclosed in U.S. Patent Nos. 10,273,049 and 9,763,852, discussed above. It has been unexpectedly found that reducing the thickness of the vial sidewall and including a thin coating on the vial sidewall has a synergistic effect of improving the mechanical performance of the glass container.
[0201] For example, by reducing the thickness of the sidewall of the vial, the strength of the vial is reduced. However, if the vial is provided with an external coating, this coating can limit the introduction of defects to the glass surface on the filling line, or even during shipping and handling. Compared with uncoated conventional vials (i.e., vials with a larger thickness), coated thin-walled vials have increased resistance to damage and breakage during shipping as well as during typical pharmaceutical filling line processes. This is unexpected, at least because it is generally understood that by reducing the thickness of a glass article, such as a glass container, the tendency of the glass article to mechanical breakage increases.
[0202] Additionally, it has been found that frictional stresses experienced, for example, during vial-to-vial contact, may be reduced in glass containers 100 having thinner sidewalls 120 due to increased sidewall flexibility. Specifically, during a friction event, the sidewalls of the glass container may flex, increasing the surface area at the contact point, thereby distributing the frictional forces over a larger area, thereby lowering the frictional stress per unit area. This may result in less surface damage to the glass during a friction event. Less surface damage (e.g., less scuffs, scratches, glass cracks, etc.) reduces the propensity for breakage and failure due to fewer crack initiation sites. This increased flexibility may also be used to increase line speeds of pharmaceutical filling lines beyond those used with containers having relatively thick sidewalls.
[0203] compliance The Vial Compliance Test is used to measure the compliance of glass containers as described herein, particularly glass pharmaceutical vials as described herein. The Vial Compliance Test involves quasi-static mechanical loading of the exterior surface of the sidewall of the glass container and is conducted according to the following procedure.
[0204] The vial compliance test apparatus 500 shown in FIG. 21 is used to perform compliance measurements on glass containers as described herein, and in particular on glass pharmaceutical vials as described herein. The glass container 100 is positioned in a fixture 510 that supports the bottom half of the glass container 100. The fixture 510 includes a left support structure 512 and a right support structure 514, each of which is configured to support a portion of the circumference of the glass container 100 in the bottom quadrant of the glass container 100. The support structures 512, 514 are stainless steel. In particular, each support structure 512, 514 supports approximately 60-70 degrees of the circumference of the glass container 100 in the bottom quadrant of the glass container 100 (α=20 degrees), as shown in FIG. 21. The circumferentially supported portion of the bottom quadrant of the glass container 100 generally extends from the vertical parting line 100-2 of the glass container 100 to approximately 20 degrees below the horizontal parting line 100-1 of the glass container 100. However, the supported portion of the glass container 100 changes slightly as the glass container 100 flexes in response to an applied load.
[0205] A universal testing machine (UTM) is used to perform vial compliance testing. In particular, a 1 / 8 inch (approximately 0.32 cm) hardened steel ball 516 is pressed into the exterior surface 116 of the sidewall 120 and a displacement-load curve is recorded. The force between the hardened steel ball 516 and the glass container 100 is increased from 0 to 400 N at a displacement rate of 0.25 mm / min. The compliance of the glass container is determined by fitting a straight line to the displacement-load data in the region of applied force between 100 N and 250 N, with the slope of the line being the compliance.
[0206] Referring to FIG. 22A, the vial compliance test involves making three local compliance measurements at the following locations along the sidewall 120: the center of the sidewall 120 (v c ); adjacent to the lower end portion 124 (v h ); and a position adjacent to the shoulder 130 (v s 22A, adjacent the lower end portion 124, sidewall test location v h is 1 mm away from the bottom portion-to-sidewall transition in a direction parallel to the central axis. As shown in FIG. 22A, the sidewall test location v adjacent to the shoulder 130 s is located 1 mm away from the shoulder-to-sidewall transition along the sidewall 120 in a direction parallel to the central axis. c v h and v s The average sidewall compliance of the glass container is determined by averaging the center sidewall compliance, the bottom portion compliance, and the shoulder compliance.
[0207] Vial compliance testing was performed using glass pharmaceutical vials with an ISO 8362-1 size designation of 2R and standard 3 ml vials (as described above). For the 2R vials, testing was performed using (i) borosilicate glass vials with a wall thickness as defined by ISO 8362-1 (i.e., 1.0 mm) and (ii) borosilicate glass vials with a wall thickness that is 0.7 times or less than the standard wall thickness as defined by ISO 8362-1 (i.e., 0.7 mm for vials with a conventional wall thickness of 1.0 mm). For the 3 ml vial compliance measurements, testing was performed using borosilicate glass vials with a wall thickness of 1.1 mm. Additionally, for the 3 ml compliance measurements, testing was performed using aluminosilicate (Corning® Valor®) ion-exchange glass vials and non-ion-exchange glass vials, with the non-ion-exchange vials having a wall thickness of 0.55 mm and the ion-exchange vials having wall thicknesses of 0.7 mm and 1.1 mm. All vials tested for compliance were annealed in a furnace following the LEHR temperature profile shown in Figure 22B. For the ion exchange treatment of the aluminosilicate glass vials for which compliance was measured, the glass containers were placed in a molten salt bath containing KNO3 at 470 °C for 5.5 hours. The resulting surface compressive stresses of the 1.1 mm and 0.7 mm ion exchange vials were approximately 500 MPa and 511 MPa, respectively. The compression depths of the 1.1 mm and 0.7 mm ion exchange vials were approximately 69 μm and 63 μm, respectively. None of the vials tested for compliance were provided with an external coating. The data obtained from the compliance measurements are shown in Figure 23, where the compliance measurements shown were averaged over 10 tests for each vial type / location. The individual compliances determined for the three locations along the sidewall of the glass containers are determined by evaluating the displacement-load slope in the elastic region spanning 100 N to 50 N of applied force. The resulting individual compliance measurements (average values over 10 tests) for each vial type are shown in Table 6 below.
[0208] [Table 6]
[0209] Table 7 below shows the average sidewall compliance (i.e., v h , v s , and v c The average sidewall compliance values shown in Table 7 are plotted in FIG. 24 as a function of wall thickness.
[0210] [Table 7]
[0211] In an embodiment, the term "compliance factor" refers to (i) the sidewall compliance of a glass pharmaceutical vial comprising a glass body having a sidewall enclosing an interior volume and an outer diameter D equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1) and (ii) the average sidewall compliance of a glass pharmaceutical vial of size X having a sidewall thickness s1 as defined by ISO 8362-1. In an embodiment, the term "compliance factor" refers to the ratio between (i) the average sidewall compliance of a glass pharmaceutical vial having a sidewall enclosing an interior volume and a glass body having an outer diameter D, where the outer diameter D of the glass body is 84% to 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the glass pharmaceutical vial sidewall has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the average sidewall compliance of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1. In an embodiment, the term "compliance factor" may refer to the ratio between (i) the average sidewall compliance of a glass pharmaceutical vial having a sidewall enclosing an interior volume and a glass body having an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, X being the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which diameter d1 is equal to or greater than D, and the glass pharmaceutical vial sidewall has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the average sidewall compliance of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1.
[0212] For ease of discussion, the glass pharmaceutical vial associated with the denominator of the compliance factor may also be referred to as the "parent vial." Table 8 below shows the measured compliance factors for borosilicate 2R vials with a reduced wall thickness of 0.7 mm and ion-exchange aluminosilicate 3 ml vials with a reduced wall thickness of 0.7 mm.
[0213] [Table 8]
[0214] Accordingly, an embodiment of the present disclosure provides a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a compliance factor, determined in accordance with a vial compliance test, of at least 1.5, at least 1.75, at least 2.0, or even at least 2.25. An embodiment is a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a compliance factor determined in accordance with a vial compliance test of at least 1.5, at least 1.75, at least 2.0, or even at least 2.25. An embodiment includes a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a compliance factor, determined in accordance with a vial compliance test, of at least 1.5, at least 1.75, at least 2.0, or even at least 2.25.
[0215] To evaluate the effect of wall thickness on sidewall compliance for other standard size glass containers, a finite element analysis (FEA) was performed using ANSYS engineering simulation software. A representative mesh used for the simulation is shown in Figure 25 (2R structure). All simulated vial structures were created using the specifications provided by ISO 8362-1, except for the standard 3 ml vial, which does not have a corresponding ISO 8362-1 size designation. The material parameters entered into the model were Young's modulus, which was set to 70.88 GPa, and Poisson's ratio, which was set to 0.199.
[0216] The boundary conditions used for the FEA compliance measurement simulations were set to match the vial compliance test fixture 500 described above and shown in FIG. 26. Thus, the exterior surface 116 of the modeled vial's sidewall 120 was constrained in all directions along 60 degrees of the vial's circumference in each of the vial's bottom quadrants. The constrained portion 100-b begins 10 degrees away from the horizontal dividing line 100-1 and extends downward toward the vertical dividing line 100-2 as shown in FIG. 26. A hardened steel ball 516 of 1 N / mm was used to represent the hardened steel ball 516 used in the physical measurements described above. 2 A surface load of v was applied within a small area (0.5 mm × 1.0 mm). The simulated compliance is calculated by dividing the displacement at the load location by the total applied load. To verify mesh convergence, meshes of various levels of coarseness (default element edge length in mm (ANSYS parameters)) were implemented and the results were compared. The difference in the calculated compliance values for the coarsest mesh against the finest mesh was within 2%, indicating that mesh coarseness in this range has a relatively small effect on the simulated compliance measurements. The results of the convergence study are shown in Figure 27. A mesh size corresponding to an element edge length of 0.9 mm was used for the simulations. Compliance measurement simulations were performed at the same three locations on each modeled vial as the vial compliance tests described herein (i.e., v h , v s , and v c ).
[0217] 28 is a plot showing compliance measurements along with experimental measurements that demonstrate the validity of the finite element model used to determine the compliance of the glass containers described herein. As can be seen, the finite element model captures the general trend of compliance as a function of thickness and also shows the compliance at different sidewall locations, i.e., v h , v s , and v c It also captures individual measurements of compliance for various vial types in the
[0218] The modeled compliance coefficients for the 2R and 3 ml vials with reduced wall thickness are shown below in Table 9. As shown in Table 9, the modeled compliance coefficients were within 20% of the experimentally measured compliance coefficients for each of the vials.
[0219] [Table 9]
[0220] After the model was validated according to the above procedure, numerous simulations were performed for the remaining ISO 8362-1 vial size designations to determine modeled compliance coefficients for vials with reduced wall thickness, the results of which are presented in Table 10 below.
[0221] [Table 10]
[0222] The modeling results reveal that by reducing the wall thickness of the glass container, increased compliance is obtained across the range of ISO 8362-1 vial sizes. It should be understood that a consistent compliance factor of greater than 2.0 across the range of ISO 8362-1 vial sizes with reduced wall thickness is not an expected result. The modeled compliance factor shown in Table 10 corresponds to a 30% wall thickness reduction, but the resulting improvement in compliance over an ISO-8362-1 vial of the same size having a wall thickness defined by ISO 8362-1 was greater than 100% for each of the simulated vials. Although a similarly surprising compliance factor of about 2 was obtained via physical measurements of the 2R and 3 ml size thin-walled vials (above), it was not expected that the reduced wall thickness would consistently improve the compliance of the sidewall 120 across the range of ISO 8362-1 vial sizes, at least in part because the geometry of the vials in the vicinity of the tested locations differs between ISO 8362-1 vial sizes.
[0223] In light of the modeling results discussed above, an embodiment of the present disclosure provides a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is a wall thickness of a glass vial of size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a compliance of at least 2.0, at least 2.05, or even at least 2.1 as determined in accordance with a vial compliance test. An embodiment includes a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% or more and 116% or less of a diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, X being the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a compliance factor determined in accordance with a vial compliance test of at least 2.0, at least 2.05, or even at least 2.1. An embodiment includes a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a compliance factor of at least 2.0, at least 2.05, or even at least 2.1, as determined in accordance with a vial compliance test.
[0224] One benefit provided by the improved compliance of the glass container described herein is the ability to distribute impact forces over a larger area of the vial, thereby reducing the peak stress experienced by the vial.As discussed above, it is believed that reducing peak stress can reduce the possibility of surface damage and / or breakage.Dynamic impact testing is used to evaluate the ability of the glass pharmaceutical vial described herein to distribute peak stress during impact.
[0225] The dynamic impact test is performed by the apparatus 600 shown in FIG. 29. The apparatus 600 used for the dynamic impact test includes a linear belt slide 610 with an impactor 620 and a fixture 630 for holding the glass container 100 at one end of the belt slide 610. The glass container 100 is restrained by the fixture 630 with the belt slide 610 on one side of the glass container 100 and the load cell 640 on the other side of the glass container 100. The fixture 630 is the same as the fixture 510 described above with respect to the vial compliance test. Thus, the fixture 630 supports the glass container 100 in the same manner as described above with respect to the vial compliance test, but the fixture 630 is oriented vertically for the dynamic impact test. The impactor 620 includes a weight of 300 grams and has a spherical tip 622. The spherical tip 622 is the same as the 1 / 8 inch hardened steel ball 516 described above with respect to the vial compliance test. The impactor 620 has velocities of 150 mm / s and 300 mm / s and is used for the vial compliance test (i.e., v s , v h and v c ) to impact the sidewall 120 of the vial at the same location as described above for the load cell 640. During the impact, load time data is recorded by the load cell 640 to evaluate the ability of the vial to distribute stress during the impact event. The peak load is recorded for each test. The measurements of the dynamic impact test are shown in FIG. 30 and correspond to five measurements for each vial type / location. With the exception of the borosilicate 2R vials having a wall thickness of 0.7 mm, the vials tested according to the dynamic impact test were the same as those described above with respect to compliance measurements (i.e., the borosilicate 2R vials having a wall thickness of 0.7 mm and tested for compliance as described above were not tested under the dynamic impact test).
[0226] As is evident from FIG. 30, the vials containing reduced wall thickness exhibited a reduction in peak load as measured by load cell 640. It was therefore discovered that the increased compliance of the vial resulting from the reduced wall thickness provides the vial with the ability to redistribute impact loads over a larger area to reduce localized stress concentrations in the vial. This result was observed for 3 ml vials having three different wall thicknesses: 1.1 mm, 0.7 mm, and 0.55 mm. c This is more evident in FIG. 31, which shows the impact load profile at 0.7 mm and 0.55 mm sidewall thickness. By comparing the impact load profiles, it can be seen that the stiffer 1.1 mm vial experienced a significantly higher peak stress, albeit for a shorter period of time. Without wishing to be bound by theory, it is believed that the higher localized stress concentrations may result in damage and / or breakage of the vial. Therefore, it is believed that the reduced peak stress load experienced by the vials with 0.7 mm and 0.55 mm sidewall thicknesses may contribute to improved mechanical performance in terms of damage resistance.
[0227] Two identifiable characteristics exhibited by dynamic impact testing of glass containers formed with sidewalls of reduced thickness compared to conventional glass vials having the same outer diameter are the peak load and full width at half maximum (FWHM) seen in the impact load profile.
[0228] In embodiments, the term “dynamic shock modulus” refers to the peak load (v h , v s , and v c (the average of measurements taken at 0.85*s1) (where D is equal to the diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1) i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1), and (ii) the peak load (v h , v s , and v c In an embodiment, the term "dynamic shock modulus" refers to the ratio between the peak load (v h , v s , and v c (The outer diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1), and (ii) the peak load (v h , v s , and v c In an embodiment, the term "dynamic shock modulus" may also be used to refer to the ratio between the peak load (v h , v s , and v c (the outer diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 whose diameter d1 is equal to or greater than D; and the sidewall of the glass pharmaceutical vial has an average wall thickness T equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1), and (ii) the peak load (v h , v s , and v c It may also be used to refer to the ratio between the mean value of the measurements taken at
[0229] In an embodiment, the term “FWHM factor” refers to (i) the FWHM (v h , v s , and v c (the average of measurements taken at 0.85*s1, where D is equal to the diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1 i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1), and (ii) the FWHM (v h , v s , and v c In addition, in an embodiment, the term "FWHM factor" refers to the ratio between (i) the FWHM (v h , v s , and v c (the outside diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D; and the sidewall of the glass pharmaceutical vial has an average wall thickness T equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1), and (ii) the FWHM of a glass pharmaceutical vial having a sidewall thickness as defined by ISO 8362-1, v h , v s , and v c Also, in embodiments, the term "FWHM factor" may be used to refer to the ratio between (i) the FWHM (v h , v s , and v c (the outer diameter D of the glass body is equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial of size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 whose diameter d1 is equal to or greater than D; and the sidewall of the glass pharmaceutical vial has an average wall thickness T equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1), and (ii) the FWHM of a glass pharmaceutical vial having a sidewall thickness as defined by ISO 8362-1, v h , v s , and v c The mean value of measurements taken at may also be used to refer to the ratio between the mean value of measurements taken at
[0230] The dynamic duty cycle of a 3 ml ion-exchange aluminosilicate vial having a wall thickness of 0.70 mm versus a 3 ml ion-exchange aluminosilicate vial having a wall thickness of 1.1 mm was determined to be 0.74. The FWHM coefficient of a 3 ml ion-exchange aluminosilicate vial having a wall thickness of 0.70 mm versus a 3 ml ion-exchange aluminosilicate vial having a wall thickness of 1.1 mm was determined to be 1.48.
[0231] Accordingly, an embodiment of the present disclosure provides a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a dynamic shock coefficient determined in accordance with a dynamic impact test that is less than 1.0, less than 0.9, or less than 0.8. Embodiments include a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a dynamic shock coefficient determined in accordance with a dynamic impact test that is less than 1.0, less than 0.9, or less than 0.8. Embodiments include a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a dynamic impact coefficient of less than 1.0, less than 0.9, or less than 0.8, as determined in accordance with a dynamic impact test.
[0232] Accordingly, an embodiment of the present disclosure provides a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a FWHM factor determined in accordance with a dynamic impact test of at least 1.2, at least 1.3, at least 1.4, or at least 1.45. Embodiments include a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% or more and 116% or less of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is 0.85*s1 or less. i where s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a FWHM factor determined in accordance with a dynamic impact test of at least 1.2, at least 1.3, at least 1.4, or at least 1.45. Embodiments include a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a FWHM factor, determined in accordance with a dynamic impact test, of at least 1.2, at least 1.3, at least 1.4, or at least 1.45.
[0233] Compressive strength As discussed above, reducing the thickness of a glass container sidewall generally reduces the strength of the glass container (at least in the context of quasi-static loading). However, without wishing to be bound by theory, it is believed that increasing the compliance of the glass container sidewall can help distribute compressive loads throughout the glass container, including minimizing the strength penalty that results from thinner walls.
[0234] The glass containers described herein, such as the glass pharmaceutical vials described herein, have a horizontal compressive strength. The horizontal compressive strength described herein is measured using a horizontal compression test, which involves positioning a glass pharmaceutical vial horizontally between two parallel steel platens with a load surface parallel to the central axis A of the glass pharmaceutical vial. A mechanical load is then applied to the glass container 100 with the platens in a direction perpendicular to the central axis A of the glass pharmaceutical vial. The horizontal compressive strength is measured using "as converted" glass pharmaceutical vials (annealed according to the furnace temperature profile shown in FIG. 22B, but without an external coating) and abraded glass pharmaceutical vials, i.e., annealed vials with a 20 mm 30 N scratch applied to the exterior surface of the sidewall in the manner described below. The vials scratched prior to testing are meant to reflect the compressive strength of the vials after they have suffered the surface damage that they typically experience during manufacturing, shipping, and handling. For the compression tested samples having a coating, the coating composition, application procedure, and coating thickness are described herein above.
[0235] The vial-on-vial fixture 700 shown in FIG. 32 is used to scratch the outermost surface of a coated or uncoated glass pharmaceutical vial to be tested. The vial-on-vial fixture 700 can be used to scratch a first glass container 710, such as glass container 100, with a second glass container 720 to replicate the vial-on-vial contact during a manufacturing run. The vial-on-vial fixture 700 includes a first clamp 712 and a second clamp 722 arranged in a cross configuration. The first clamp 712 includes a first fixed arm 714 attached to a first base 716. The first fixed arm 714 is attached to the first glass container 710 and holds the first glass container 710 stationary relative to the first clamp 712. Similarly, the second clamp 722 includes a second fixed arm 724 attached to a second base 726. A second fixed arm 724 is attached to a second glass container 720 and holds it stationary relative to a second clamp 722. The first glass container 710 is positioned on the first clamp 712 and the second glass container 720 is positioned on the second clamp 722 such that the central axis A of the first glass container 710 and the central axis A of the second glass container 720 are at an angle of approximately 90° to each other and are positioned on a horizontal plane defined by the x and y axes.
[0236] The scratch can be characterized by a selected normal pressure and scratch length applied by the vial-on-vial fixture 700 to the contact area 730. Unless otherwise stated, the scratch on the abraded glass pharmaceutical vial 100 for the horizontal compression procedure includes a 20 mm scratch caused by a normal load of 30 N. When the glass container 100 is positioned between the two platens for testing, the scratch is located at the point furthest from the platens and is oriented parallel to the central axis A of the glass container 100.
[0237] Once the 30N scratch has been built into the sidewall 120 of the glass container 100, the glass container 100 is prepared for horizontal compression testing according to the following procedure. With reference to FIG. 33, before being placed between the upper platen 810 and the lower platen 820, the glass container 100 is wrapped with 2 inch (5.08 cm) tape (Scotch 3M 471) and the overhangs on each end of the glass container 100 are folded around each end of the glass container 100. The glass container 100 is then positioned within an index card 830 (Oxford 3×5 index card) that is stapled around the glass container. The purpose of the tape and index card is to contain any broken glass. The prepared glass container 100 is then positioned between two parallel platens 810, 820 as shown in FIG. 33. The load rate for the horizontal vial compression test is 0.5 in. (1.27 cm) / min, which means that the platens 810, 820 move towards each other at a rate of 0.5 in. (1.27 cm) / min. Horizontal compressive strength is measured at 25°C ± 2°C and 50% ± 5% relative humidity. Horizontal compressive strength is a measurement of the peak load at failure, and horizontal compressive strength can be given as the probability of failure at a selected normal compressive load. As used herein, failure occurs when the glass container bursts under horizontal compression in at least 50% of the samples. 50 samples are tested for each glass vial type evaluated.
[0238] In an embodiment, the term "horizontal strength coefficient" refers to (i) the horizontal compressive strength of a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) comprising a glass body having a sidewall enclosing an interior volume and an outer diameter D, where D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1) and (ii) the horizontal compressive strength of a glass pharmaceutical vial of size X having a sidewall thickness s1 as defined by ISO 8362-1. Also, in embodiments, the term "horizontal strength coefficient" refers to the horizontal compressive strength of (i) a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) that includes a glass body including a sidewall enclosing an interior volume and an outer diameter D, where D is 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1 i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the horizontal compressive strength of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1. Also, in embodiments, the term "horizontal strength coefficient" refers to the horizontal compressive strength of (i) a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) that includes a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 in which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the horizontal compressive strength of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1.
[0239] Figure 35 shows the horizontal compressive strength of as-converted glass vials (without surface scratches and no external coating) measured according to the Horizontal Compression Test described above. The results shown in Figure 35 correspond to: (i) an aluminosilicate 2 ml vial with a wall thickness of 0.85 mm, (ii) a borosilicate 2 ml vial with a wall thickness of 1.2 mm; (iii) a borosilicate 2R vial with a wall thickness of 0.7 mm; and (iv) a borosilicate vial with a wall thickness of 1.0 mm. The horizontal strength factor of the 2R borosilicate vial with a wall thickness of 0.70 mm relative to the 2R borosilicate vial with a wall thickness of 1.0 mm was determined to be 0.75. Accordingly, an embodiment of the present disclosure provides a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a horizontal strength coefficient, determined in accordance with a horizontal compression test, of at least 0.5, at least 0.65, at least 0.7, or at least 0.75. An embodiment of the disclosure is a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a horizontal strength coefficient determined in accordance with a horizontal compression test of at least 0.5, at least 0.65, at least 0.7, or at least 0.75. An embodiment of the present disclosure includes a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a horizontal strength coefficient, determined in accordance with a horizontal compression test, of at least 0.5, at least 0.65, at least 0.7, or at least 0.75.
[0240] As discussed above, providing an external coating on a glass pharmaceutical vial can limit the formation of defects that may occur on the filling line or even during shipping and handling. Compared to uncoated conventional vials, the coated thin-walled vials have increased resistance to damage and breakage during shipping and typical pharmaceutical filling line processes. To demonstrate the increased resistance to damage and breakage of the glass pharmaceutical vials described herein, the vials were provided with the external coating described above, the glass vials were polished to have surface damage typically experienced during manufacturing, shipping, and handling, and then subjected to horizontal compression testing. The resulting horizontal compression strength of the externally coated glass pharmaceutical vials was then used to determine the horizontal strength coefficient of the externally coated glass pharmaceutical vials described herein in the manner described above.
[0241] Figure 36 shows the horizontal compressive strength of several glass vials determined in accordance with the horizontal compression test described above, the vials having a 20 mm 30 N scratch applied to their surface in the manner described above. The results shown in Figure 36 correspond to: (i) a coated aluminosilicate 2 ml vial having a wall thickness of 0.85 mm; (ii) an uncoated borosilicate 2 ml vial having a wall thickness of 1.2 mm; (iii) a coated borosilicate 2R vial having a wall thickness of 0.7 mm; and (iv) an uncoated borosilicate vial having a wall thickness of 1.0 mm. The horizontal strength factor of the outer coated 2R borosilicate vial having a wall thickness of 0.70 mm relative to the 2R borosilicate vial having a wall thickness of 1.0 mm was determined to be 1.97 when the tested vial had a 20 mm 30 N scratch applied to it. Accordingly, an embodiment of the present disclosure provides an exterior coated glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes an outer coated glass pharmaceutical vial comprising a horizontal strength coefficient, determined in accordance with a horizontal compression test, of at least 1.5, at least 1.6, at least 1.7, at least 1.8, or at least 1.9. An embodiment of the disclosure is a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a horizontal strength coefficient determined in accordance with a horizontal compression test of at least 1.5, at least 1.6, at least 1.7, at least 1.8, or at least 1.9. Embodiments include a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a horizontal strength coefficient, determined in accordance with a horizontal compression test, of at least 1.5, at least 1.6, at least 1.7, at least 1.8, or at least 1.9.
[0242] It has been unexpectedly found that applying a coating to the exterior surface of a 0.7 mm vial can negate the loss in strength associated with the reduced thickness compared to a conventional glass vial having the same exterior diameter. Thus, versus an uncoated 2R glass pharmaceutical vial having a conventional wall thickness of 1.0 mm, an externally coated 2R glass pharmaceutical vial as described herein, having a wall thickness that is 70% of the conventional vial wall thickness, exhibited a 97% improvement in horizontal compressive strength.
[0243] The glass containers described herein, such as the glass pharmaceutical vials described herein, also have a vertical compression strength. The vertical compression strength described herein is measured using a vertical compression test, which involves positioning the glass container 100 vertically between two parallel steel platens oriented normal to the central axis A of the glass pharmaceutical vial. A mechanical load is then applied to the glass container 100 with the platens normal to the central axis A of the glass pharmaceutical vial. The vertical compression strength was determined using abraded glass pharmaceutical vials, i.e., the vials were scratched with a 20 mm 30 N scratch as described above. Similar to the vials tested in horizontal compression, the vials tested for vertical compression strength were annealed according to the furnace temperature profile shown in FIG. 22B. Similar to the horizontal compression test, the vials are scratched prior to testing to replicate the surface damage that glass vials may experience during manufacturing, shipping, and handling. The 30N scratches on the sidewall 120 of the glass container 100 are oriented parallel to the central axis A of the glass container 100.
[0244] To prepare the glass container 100 for the vertical compression test, the glass container 100 is wrapped with a 1.5 inch (3.81 cm) piece of tape (Scotch 3M 471) and a 1 inch (2.54 cm) piece of tape (Scotch 3M 471) is placed on the bottom of the sample so that the glass container sits flat on the lower platen 820. The overhang of the tape placed on the bottom of the glass container 100 is folded against the side of the glass container 100. The prepared glass container 100 is then positioned between two parallel platens 810, 820 as shown in FIG. 34. The loading rate for the vertical vial compression test is 0.2 inches (0.508 cm) / min, which means that the platens 810, 820 move towards each other at a rate of 0.2 inches (0.508 cm) / min. The vertical compression strength is measured at 25°C ± 2°C and 50% ± 5% relative humidity. Vertical compressive strength is a measure of the load at failure, and can be given as the probability of failure at a selected normal compressive load. As used herein, failure occurs when at least 50% of the samples of the glass pharmaceutical vials burst under vertical compression. 50 samples are tested for each glass vial type evaluated.
[0245] In an embodiment, the term "vertical strength coefficient" refers to (i) the vertical compressive strength of a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) comprising a glass body having a sidewall enclosing an interior volume and an outer diameter D, where D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1) and (ii) the vertical compressive strength of a glass pharmaceutical vial of size X having a sidewall thickness s1 as defined by ISO 8362-1. Also, in embodiments, the term "vertical strength coefficient" refers to the vertical compressive strength of (i) a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) that includes a glass body including a sidewall enclosing an interior volume and an outer diameter D, where D is 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the vertical compressive strength of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1. Also in embodiments, the term "vertical strength factor" refers to the vertical compressive strength of (i) a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) having a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 in which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the vertical compressive strength of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1.
[0246] Figure 37 shows the vertical compression strength of several glass vials determined in accordance with the above described vertical compression test, the vials having a 20mm 30N scratch applied to their surface in the manner described above. The results shown in Figure 37 correspond to: (i) a coated aluminosilicate 2ml vial having a wall thickness of 0.85mm, (ii) an uncoated borosilicate 2ml vial having a wall thickness of 1.2mm; (iii) a coated borosilicate 2R vial having a wall thickness of 0.7mm; and (iv) an uncoated borosilicate vial having a wall thickness of 1.0mm. The vertical strength factor of the outer coated 2R borosilicate vial having a wall thickness of 0.70mm relative to the uncoated 2R borosilicate vial having a wall thickness of 1.0mm was determined to be 1.33 when the tested vial had a 20mm 30N scratch applied to it. Accordingly, an embodiment of the present disclosure provides an exterior coated glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i wherein s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes an exterior coated glass pharmaceutical vial comprising a vertical strength coefficient determined in accordance with a vertical compression test of at least 1.1, at least 1.2, or at least 1.3. An embodiment of the present disclosure is a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation as defined by ISO 8362-1 of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a vertical strength coefficient determined in accordance with a vertical compression test of at least 1.1, at least 1.2, or at least 1.3. An embodiment of the present disclosure includes a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% or more and 116% or less of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a vertical strength coefficient, determined in accordance with a vertical compression test, of at least 1.1, at least 1.2, or at least 1.3.
[0247] It has been unexpectedly found that applying a coating to the exterior of a 0.7 mm vial can negate the strength loss associated with thinner walls. Thus, versus a 2R glass pharmaceutical vial having a conventional wall thickness of 1.0 mm, an exterior coated glass pharmaceutical vial disclosed herein having a wall thickness that is 70% of the conventional vial wall thickness exhibited a 30% improvement in vertical compressive strength.
[0248] Breakage resistance Without wishing to be bound by theory, it is believed that the improved compliance of the vial resulting from the thinner walls has a synergistic relationship with the avoidance of defect formation provided by the exterior coating, producing a glass container with improved breakage resistance compared to glass containers lacking this combination of features.
[0249] To evaluate the resistance to breakage of the outer coated glass pharmaceutical vial described herein against a glass pharmaceutical vial having the same ISO 8362-1 size designation but with a thickness defined by ISO 8362-1, a "breakage coefficient" is determined according to a pendulum impact test. The pendulum impact test is performed using a pendulum device 900 shown in FIG. 38 according to the following test procedure. First, a 20 mm 30 N scratch is made on the side of the vial using a vial-on-vial fixture 700 shown in FIG. 32. The scratch extends in a direction parallel to the central axis A of the glass container 100 along the outer surface 116 of the sidewall 120. Referring to FIG. 1, the midpoint of the scratch is located at a distance of approximately 1 / 2h2 from the bottom of the vial.
[0250] The vial is then placed in the vial holder 910 as shown in Figures 38 and 39. The vial holder 910 is made of stainless steel and has dimensions as shown in Figures 42 (front view) and 43 (top view) (dimensions in mm). Referring to Figure 39, the sides of the vial are supported by left and right vial brackets 920 and 930, which extend from the base 940 of the vial holder 910 and terminate before reaching the transition point between the side wall 120 and the shoulder 130 of the glass container 100. The glass container is placed such that the front and back of the glass container, i.e., the area between the vial brackets, are exposed and the back of the glass container 100 contacts the back 950 of the vial holder 910. The glass container 100 is oriented such that the scratch is positioned 90 degrees from the front of the vial holder 910 such that the scratch is positioned substantially in the center of one of the vial brackets 920, 930. As can be seen in FIG. 39, the front surface of the glass container 100 extends beyond the vial brackets 920, 930 to define an impact area 100-a against which the impactor strikes, as will be described in more detail below.
[0251] The vial impactor 960 used for the pendulum impact test comprises a hardened steel semi-cylinder having a longitudinal axis perpendicular to the central axis A of the glass container 100 when the glass container 100 is positioned in the vial holder 910. The semi-cylinder forming the vial impactor 960 has a radius of 10 mm and a length of 40 mm. A close-up of the vial impactor 960 can be seen in FIG. 41. The vial impactor 960 is positioned at the distal end of the pendulum arm 970 of the pendulum device 900. The proximal end of the pendulum arm is connected to a pivot 980 that allows adjustment of the pendulum arm 970 to various drop positions. The drop positions are measured in terms of angle β shown in FIG. 40, which is the angle between the pendulum arm 970 and a horizontal line 980-1 extending from the pivot 980. The pivot 980 is supported by a vertical support beam 990 via a standard bearing (not shown). The pendulum apparatus 900 includes a load cell (not shown) that contacts the back of the glass container 100 when the glass container 100 is placed in the vial holder 910. During the pendulum impact test, the load cell records force-time data.
[0252] 1 and 38, the pendulum arm 970 is configured so that the hardened steel vial impactor 960 impacts the glass container 100 at a vertical position corresponding to a distance of ½h2 from the bottom of the glass container 100. For purposes of the pendulum impact testing described herein, the drop position is set at 35 degrees, which corresponds to an impulse between 0.08 and 0.12 Newton seconds.
[0253] At least five samples are tested for each vial (having the same processing history), although more samples may be tested to increase the confidence level of the results. A sample is considered to have "survived" the pendulum impact test if no fracture is observed after impact under the conditions specified above. The survival rate is determined by calculating the percentage of the sample population that survived the pendulum impact test. For example, if the sample population tested was 10 and no fracture was observed in five samples after impact under the conditions specified above, the survival rate of the corresponding vial type would be 50%. The results obtained from the pendulum impact test measurements are shown in Table 11 below. All samples tested in the pendulum impact test were annealed according to the furnace temperature profile shown in Figure 22B, and none of the aluminosilicate vials tested were ion-exchanged.
[0254] [Table 11]
[0255] In an embodiment, the term "breakage coefficient" refers to (i) the viability of a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) comprising a glass body having a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to the diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i where s1 is the wall thickness of a glass vial of size X as defined by ISO 8362-1) and (ii) the viability of a glass pharmaceutical vial of size X having a sidewall thickness s1 as defined by ISO 8362-1. Also in embodiments, the term "breakage coefficient" refers to the percentage of viability of a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) that includes a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the viability of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1. Also, in an embodiment, the term "breakage coefficient" refers to the percentage of viability of a glass pharmaceutical vial (or an externally coated glass pharmaceutical vial, if a coating is present) that has a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being equal to or greater than 84% and equal to or less than 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, in which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i where s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1) and (ii) the viability of a glass pharmaceutical vial of size X having a sidewall thickness as defined by ISO 8362-1.
[0256] The breakage coefficient of an outer coated 0.85 aluminosilicate vial with a wall thickness of 0.85 mm against an uncoated 2R borosilicate vial with a wall thickness of 1.2 mm was determined to be >95 (survival rate of 2R borosilicate vials with a wall thickness of 1.2 mm was less than 1%) when the tested vials were scratched with a 20 mm 30 N scratch.
[0257] Accordingly, an embodiment of the present disclosure provides an exterior coated glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is less than or equal to 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes an outer coated glass pharmaceutical vial comprising a breakage coefficient of at least 50, at least 60, at least 70, at least 80, at least 90, or at least 95 as determined in accordance with a pendulum impact test. An embodiment of the disclosure is a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, where the outer diameter D is equal to or greater than 84% and equal to or less than 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which 116% of the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is a wall thickness of a glass vial having a size designation X as defined by ISO 8362-1, the glass pharmaceutical vial comprising a breakage factor determined in accordance with a pendulum impact test of at least 50, at least 60, at least 70, at least 80, at least 90, or at least 95. An embodiment of the present disclosure includes a glass pharmaceutical vial comprising a glass body including a sidewall enclosing an interior volume and an outer diameter D, the outer diameter D of the glass body being 84% to 116% of the diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1, X being the smallest size designation of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1 for which the diameter d1 is equal to or greater than D, and the sidewall of the glass pharmaceutical vial has an average wall thickness T that is equal to or less than 0.85*s1. i wherein s1 is the wall thickness of a glass vial of size designation X as defined by ISO 8362-1, and the glass pharmaceutical vial includes a breakage coefficient of at least 50, at least 60, at least 70, at least 80, at least 90, or at least 95, as determined in accordance with a pendulum impact test.
[0258] inspection Forming glass pharmaceutical vials with reduced thickness sidewalls may also improve visual and automated inspection of glass pharmaceutical vials. In particular, glass pharmaceutical vials are typically inspected using visual inspection and / or automated vision systems to detect defects and / or non-conformities, such that vials having these defects and / or non-conformities may be discarded. Without wishing to be bound by theory, it is believed that forming glass pharmaceutical vials with reduced thickness sidewalls may improve the surface quality of the glass pharmaceutical vials by minimizing and / or mitigating defects caused by tooling and the like.
[0259] Improved surface quality may also enhance visual and / or automated inspection of glass pharmaceutical vials, facilitating detection of defects and / or non-conformities. In particular, glass pharmaceutical vials with improved optical transmission and reflectance properties may enhance defect contrast detection, thereby improving automated inspection systems.
[0260] It is further believed that glass tubing blanks formed from thinner walls may be manufactured with fewer defects, and thus glass containers formed from glass tubing blanks having reduced wall thickness may contain fewer defects, leading to improved inspection-related properties of the glass containers described herein.
[0261] Sustainability and Costs Importantly, forming glass pharmaceutical vials with reduced sidewall thickness enables more sustainable, lower cost pharmaceutical packaging. In particular, forming glass pharmaceutical vials with reduced sidewall thickness results in vials that utilize less glass material than a conventional glass vial having the same outer diameter D. The reduction in glass material also translates into lighter packaging, which, when scaled up, reduces fuel consumption in shipping the finished product.
[0262] Table 12 below shows the amount of glass material required to make 2R glass pharmaceutical vials with reduced wall thicknesses of 0.7 mm and 0.5 mm for vials with conventional flange designs and vials with reduced flange volume designs. Since the density of the glass can be considered constant throughout the container, the reduced volume of glass required to produce a particular vial can be used to calculate the reduced glass mass.
[0263] [Table 12]
[0264] It has been found that glass pharmaceutical vials having a wall thickness of 0.7 times or less than the wall thickness of a glass pharmaceutical container of the same ISO 8362-1 size designation can be formed using less than 90%, less than 85%, or even less than 80% of the glass mass used to form a glass pharmaceutical vial of the same size designation having a wall thickness defined by ISO 8362-1. Thus, embodiments of the present disclosure provide a method for forming glass pharmaceutical vials having an average wall thickness T that is 0.85*s1 or less. i The present disclosure also includes glass pharmaceutical vials in which the sidewall of the glass pharmaceutical vial having a wall thickness of 0.7 times that of a glass pharmaceutical container of the same size ISO 8362-1 size designation, when designed with a reduced flange volume, correlates with a reduction of 10% or more, 15% or more, or even 20% or more of the mass of glass used to make the vial. Additionally, when glass pharmaceutical vials are designed with a reduced flange volume as discussed in the above embodiments, glass pharmaceutical vials with a reduced wall thickness of 0.7 times that of a glass pharmaceutical container of the same size ISO 8362-1 size designation may be formed using less than 84%, less than 80%, less than 76%, or even less than 72% of the mass of glass used to form a glass pharmaceutical vial of the same size designation having a thickness as defined by ISO 8362-1. Thus, embodiments of the present disclosure provide glass pharmaceutical vials with an average wall thickness T that is less than or equal to 0.85*s1. i that correlates with a 16% or greater, 20% or greater, 24% or greater, or 28% or greater reduction in the mass of glass used to make the vial. Thus, the reduction in wall thickness of glass containers described herein leads to more glass containers being produced for a given amount of glass.
[0265] Reducing the glass material in the container also reduces raw material costs since less glass is used to manufacture the glass tubing blank that forms the container.
[0266] Glass containers formed with reduced wall thickness may also have increased fill capacity relative to conventional glass containers with the same outer diameter. For example, a glass pharmaceutical vial described herein having a 2R size designation according to ISO 8362-1 but with a reduced wall thickness (70% of the standard wall thickness according to ISO 8362-1) could hold 9% more fluid volume than a glass pharmaceutical vial of size 2R with a thickness defined by ISO 8362-1. Similarly, a glass pharmaceutical vial described herein having a 10R size designation according to ISO 8362-1 but with a reduced wall thickness (70% of the standard wall thickness according to ISO 8362-1) could hold 6% more fluid volume than a glass pharmaceutical vial of size 10R with a thickness defined by ISO 8362-1.
[0267] As described herein, with respect to manufacturing throughput, reducing the thickness of the sidewall of the glass container may increase manufacturing throughput since the thinner glass tubing forming the glass container may be heated more quickly to the temperature required for the tube-to-vial conversion process. As described below, this results in reduced energy usage during the manufacture of the glass container. Similarly, the reduced thermal mass of the glass container due to the reduced sidewall thickness may improve the efficiency of any heating and / or cooling process used in the manufacture of the glass container or in the subsequent processing of the glass container. For example, the depyrogenation, freezing, and lyophilization processes may be completed with less energy consumption due to the relatively lower thermal mass of the glass container with reduced wall thickness compared to a conventional glass container having the same outer diameter D. Additionally, the reduced mass and improved compliance of the vial may increase the speed of the filling line, resulting in a more efficient filling line.
[0268] In addition to the sustainability improvements mentioned above, glass containers with reduced wall thickness may also lead to an overall reduction in CO2 emissions. With regard to the tube-to-vial conversion process, glass containers formed with reduced wall thickness may require less heating to accomplish the various steps of the conversion process. To investigate this theory, a gas usage study was conducted to determine whether the gas usage required for conversion of thin-walled glass containers could be reduced compared to corresponding glass containers formed with conventional thicknesses. Table 13 below shows the gas usage for the conversion of 2R glass pharmaceutical vials formed from glass tubing material with three different wall thicknesses.
[0269] [Table 13]
[0270] As can be seen from Table 13 above, the overall gas (i.e., energy) required to convert a 2R vial having a wall thickness of 0.7 times the wall thickness defined by ISO 8362-1 from glass tubing stock can be reduced by 11% compared to a 2R glass pharmaceutical vial having a conventional wall thickness (i.e., 1 mm). Furthermore, specifically with respect to the separation step of the conversion process, the energy required to separate a 2R vial having a wall thickness of 0.7 times the wall thickness defined by ISO 8362-1 from the glass tubing stock can be reduced by 44% compared to a 2R glass pharmaceutical vial having a conventional wall thickness (i.e., 1 mm). Thus, embodiments of the present disclosure include glass pharmaceutical vials that can be converted from glass tubing stock using less than 95%, less than 94%, less than 93%, less than 92%, less than 91%, or even less than 90% of the energy required to convert a glass pharmaceutical vial of the same ISO 8362-1 size designation having a thickness defined by ISO 8362-1. Thus, embodiments of the present disclosure provide a wall thickness T that is equal to or less than 0.85*s1. i that correlates with a 5% or greater, 6% or greater, 7% or greater, 8% or greater, 9% or greater, or even 10% or greater reduction in the amount of energy used to convert the glass pharmaceutical vial from the glass tubing material.
[0271] Additionally, embodiments of the present disclosure include glass pharmaceutical vials that can be separated from glass tubing blanks using less than 80%, less than 75%, less than 70%, less than 65%, or even less than 60% of the energy required to separate glass pharmaceutical vials of the same ISO 8362-1 size designation having a thickness as defined by ISO 8362-1. Thus, embodiments of the present disclosure include glass pharmaceutical vials that can be separated from glass tubing blanks using less than 80%, less than 75%, less than 70%, less than 65%, or even less than 60% of the energy required to separate glass pharmaceutical vials of the same ISO 8362-1 size designation having a thickness as defined by ISO 8362-1. i that correlates with a 20% or greater, 25% or greater, 30% or greater, 35% or greater, or even 40% or greater reduction in the amount of energy used to separate the glass pharmaceutical vial from the glass tubing blank. The above-described energy reductions associated with thinner walls will translate into a proportionate reduction in the amount of CO2 emitted per converted glass vial.
[0272] In addition to the energy savings and emissions reductions associated with the tube-to-vial conversion process, it has been found that such benefits are also realized with respect to the manufacture of the glass tubing blank used to form the tubes.
[0273] To investigate the potential for CO2 emission reductions associated with the production of reduced thickness glass tubing stock for use in the manufacture of thin wall glass containers as described herein, a study was performed to determine the CO2 emissions per vial associated with 2R glass pharmaceutical vials with reduced wall thicknesses of 0.7 mm and 0.5 mm. The amount of natural gas required to provide the amount of glass tubing stock required to manufacture 2R glass pharmaceutical vials was determined and the associated CO2 emissions are shown in Table 14 below.
[0274] [Table 14]
[0275] Further emissions studies were conducted comparing the total CO2 emissions per vial (including tube manufacturing and processing) for 2R, 10R, and 20R vials with wall thicknesses of 1.0mm, 0.7mm, and 0.5mm, and the results are presented in Table 15 below.
[0276] [Table 15]
[0277] In some cases, the glass tubing blanks with reduced wall thickness may result in a lower tubing yield. Thus, the resulting emissions per vial may vary slightly from the ISO 8362-1 vial size. Although the manufacturing process of the glass tubing blanks could be modified to improve the tubing yield, the results of this study show that by reducing the wall thickness to 0.7 times the wall thickness defined by ISO 8362-1, the overall CO2 emissions can be reduced by at least 5%, considering both the raw glass to glass tubing blank conversion process and the tube to glass conversion process. Thus, embodiments of the present disclosure include glass pharmaceutical vials that can be manufactured with 95% of the CO2 emissions, 90% of the CO2 emissions, or even 85% of the CO2 emissions required to manufacture glass pharmaceutical vials of the same ISO 8362-1 size designation with an average wall thickness T that is 0.85*s1 or less. Thus, embodiments of the present disclosure include glass pharmaceutical vials that can be manufactured with 95% of the CO2 emissions, 90% of the CO2 emissions, or even 85% of the CO2 emissions required to manufacture glass pharmaceutical vials of the same ISO 8362-1 size designation with an average wall thickness T that is 0.85*s1 or less. i that correlates with a 5% or greater, 10% or greater, or even 15% or greater reduction in the amount of CO2 emitted to manufacture the glass pharmaceutical vial.
[0278] Without wishing to be bound by theory, it is believed that reducing the sidewall thickness of glass containers relative to conventional glass containers (such as those described in ISO 8362-1) can significantly reduce the CO2 emissions of processes associated with filling and transporting glass containers.
[0279] Regarding the CO2 emission reduction rate associated with transportation, there is a model to assume the emission reduction rate considering the overall shipping weight, emission factors provided by EPA (https: / / www.epa.gov / sites / default / files / 2018-03 / documents / emission-factors_mar_2018_0.pdf), and an arbitrary distance of 2,300 miles. For the overall shipping weight, the model includes the weight of the vials, the weight of the pallet used to carry the vials, the weight of the truck (https: / / www.energy.gov / eere / vehicles / fact-620-april-26-2010-class-8-truck-tractor-weight-component), and the weight of an empty 53 foot trailer (https: / / bigrigpros.com / how-much-does-an-empty-semi-trailer-weigh / ). Table 16 below shows the model assumptions and the corresponding model results.
[0280] [Table 16]
[0281] The model results shown in Table 16 above indicate that a reduction in wall thickness to 0.7 times the wall thickness specified by ISO 8362-1 can reduce transport-related CO2 emissions by 7% (5.7g CO2 → 5.3g CO2). Furthermore, a reduction in wall thickness to 0.5 times the wall thickness defined by ISO 8362-1 can reduce CO2 emissions by 15% (5.7g CO2 → 4.9g CO2).
[0282] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments described herein without departing from the spirit and scope of the claimed subject matter. Therefore, this specification is intended to cover modifications and variations of the various embodiments described herein, such modifications and variations being within the scope of the appended claims and their equivalents.
[0283] Although embodiments of glass containers are described herein as having a sidewall with reduced thickness while maintaining the same outer diameter as a conventional glass container, or an outer diameter that is 84% to 116% of that of a conventional glass container, it should be understood that other embodiments are envisioned and possible. For example, a glass container may have a sidewall with reduced thickness as described herein. However, the glass container may be configured such that the inner diameter is the same as a conventional glass container, or the inner diameter is 84% to 116% of that of a conventional glass container, and the outer diameter is less than the outer diameter of a conventional glass container. In such embodiments, the glass container is considered to have the same properties (i.e., mechanical behavior, chemical durability, etc.) as the embodiments of glass containers described herein that have a reduced wall thickness but the same outer diameter as a conventional glass container, or an outer diameter that is 84% to 116% of that of a conventional glass container.
[0284] Additionally, while the present disclosure is primarily directed to glass containers converted from glass tubes, embodiments of the present disclosure also include formed glass containers that include thin walls. Formed glass containers will exhibit many of the improvements of converted glass containers. For example, regardless of the manufacturing method used to create the glass container, glass containers that include thinner walls may require less glass and energy to manufacture and provide similar mechanical performance benefits associated with improved compliance resulting from thin walls.
[0285] Preferred embodiments of the present invention will be described below in detail.
[0286] EMBODIMENT 1 1. A glass pharmaceutical vial comprising: a glass body including a sidewall enclosing an interior volume and an outer diameter D; the outer diameter D of the glass body is greater than or equal to 84% and less than or equal to 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1:2018, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018 in which 116% of the diameter d1 is greater than or equal to D; The sidewall of the glass pharmaceutical vial has an average wall thickness T i wherein s1 is the wall thickness of said glass vial of size designation X as defined by ISO 8362-1:2018; The glass pharmaceutical vial comprises a compliance factor of at least 1.75 as determined in accordance with a vial compliance test. Glass pharmaceutical vials.
[0287] EMBODIMENT 2 2. The glass pharmaceutical vial of embodiment 1, comprising a horizontal strength coefficient of at least 0.5 as determined according to a horizontal compression test.
[0288] EMBODIMENT 3 2. The glass pharmaceutical vial of embodiment 1, wherein said glass pharmaceutical vial comprises an exterior organic coating and a horizontal strength coefficient of at least 1.5 determined according to a horizontal compression test.
[0289] EMBODIMENT 4 2. The glass pharmaceutical vial of embodiment 1, wherein the glass pharmaceutical vial comprises an exterior organic coating.
[0290] EMBODIMENT 5 5. The glass pharmaceutical vial of embodiment 4, wherein the exterior organic coating is an organic coating having a thickness of 20 nm or more and 40 nm or less.
[0291] EMBODIMENT 6 5. The glass pharmaceutical vial of embodiment 4, wherein said glass pharmaceutical vial comprises a breakage modulus of at least 50 as determined according to a pendulum impact test.
[0292] EMBODIMENT 7 5. The glass pharmaceutical vial of embodiment 4, wherein said glass pharmaceutical vial comprises a low temperature storage factor, determined in accordance with a freeze-thaw test, of at least 2.25.
[0293] EMBODIMENT 8 2. The glass pharmaceutical vial of embodiment 1, wherein the glass pharmaceutical vial is formed from Type I, Class B glass according to ASTM standard E438-92.
[0294] EMBODIMENT 9 2. The glass pharmaceutical vial of embodiment 1, wherein the glass pharmaceutical vial is formed from an aluminosilicate glass composition.
[0295] EMBODIMENT 10 The average wall thickness T is less than or equal to 0.85*s1 i 2. The glass pharmaceutical vial of embodiment 1, wherein the sidewall of the glass pharmaceutical vial having a mass of 10% or more correlates with a reduction in the mass of glass used to make the glass pharmaceutical vial.
[0296] EMBODIMENT 11 The average wall thickness T is less than or equal to 0.85*s1 i 2. The glass pharmaceutical vial of embodiment 1, wherein the sidewall of the glass pharmaceutical vial having a .gtoreq..gtoreq..times ...
[0297] EMBODIMENT 12 The average wall thickness T is less than or equal to 0.85*s1 i 2. The glass pharmaceutical vial of embodiment 1, wherein said sidewall of said glass pharmaceutical vial having a cross-sectional area of about 100 mm correlates with a 5% or greater reduction in the amount of CO2 emitted to create said glass pharmaceutical vial.
[0298] EMBODIMENT 13 The average wall thickness T is less than or equal to 0.85*s1 i 2. The glass pharmaceutical vial of embodiment 1, wherein the sidewall of the glass pharmaceutical vial having a diameter of 10 mm or less correlates with a 20% or greater reduction in the amount of energy used to separate the glass pharmaceutical vial from a glass tubing blank.
[0299] EMBODIMENT 14 The glass pharmaceutical vial is compliant with USP <660> 2. The glass pharmaceutical vial of embodiment 1, having a Type 1 chemical durability according to
[0300] EMBODIMENT 15 2. The glass pharmaceutical vial of embodiment 1, wherein said glass pharmaceutical vial comprises a dynamic impact coefficient, determined in accordance with a dynamic impact test, of less than 0.9.
[0301] EMBODIMENT 16 2. The glass pharmaceutical vial of embodiment 1, wherein said glass pharmaceutical vial comprises a FWHM factor of at least 1.2, determined according to a dynamic impact test.
[0302] EMBODIMENT 17 The glass pharmaceutical vial is A dynamic impact coefficient of less than 0.9, as determined in accordance with a dynamic impact test; and a FWHM factor of at least 1.2, as determined in accordance with said dynamic impact test. 2. The glass pharmaceutical vial of embodiment 1, comprising:
[0303] EMBODIMENT 18 1. A glass pharmaceutical vial comprising: a glass body including a sidewall enclosing an interior volume and an outer diameter D; the outer diameter D of the glass body is equal to a diameter d1 of a glass vial of size X as defined by ISO 8362-1:2018, where X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018; The sidewall of the glass pharmaceutical vial has an average wall thickness T i where s1 is the wall thickness of the glass vial of size X as defined by ISO 8362-1:2018; The glass pharmaceutical vial comprises a compliance factor of at least 1.75 as determined in accordance with a vial compliance test. Glass pharmaceutical vials.
[0304] EMBODIMENT 19 19. The glass pharmaceutical vial of embodiment 18, comprising a horizontal strength coefficient of at least 0.5 as determined according to a horizontal compression test.
[0305] EMBODIMENT 20 19. The glass pharmaceutical vial of embodiment 18, wherein said glass pharmaceutical vial comprises an exterior organic coating and a horizontal strength coefficient of at least 1.5 determined according to a horizontal compression test.
[0306] EMBODIMENT 21 19. The glass pharmaceutical vial of embodiment 18, wherein the glass pharmaceutical vial comprises an exterior organic coating.
[0307] EMBODIMENT 22 22. The glass pharmaceutical vial of embodiment 21, wherein the external organic coating is an organic coating having a thickness of 20 nm or more and 40 nm or less.
[0308] EMBODIMENT 23 22. The glass pharmaceutical vial of embodiment 21, wherein said glass pharmaceutical vial comprises a breakage coefficient of at least 50, determined according to a pendulum impact test.
[0309] EMBODIMENT 24 22. The glass pharmaceutical vial of embodiment 21, wherein said glass pharmaceutical vial comprises a low temperature storage factor, determined in accordance with a freeze-thaw test, of at least 2.25.
[0310] EMBODIMENT 25 The glass pharmaceutical vial of embodiment 18, wherein said glass pharmaceutical vial is formed from Type I, Class B glass according to ASTM standard E438-92.
[0311] EMBODIMENT 26 19. The glass pharmaceutical vial of embodiment 18, wherein the glass pharmaceutical vial is formed from an aluminosilicate glass composition.
[0312] EMBODIMENT 27 The average wall thickness T is less than or equal to 0.85*s1 i 19. The glass pharmaceutical vial of embodiment 18, wherein the sidewall of the glass pharmaceutical vial having a mass of 10% or more correlates with a reduction in the mass of glass used to make the glass pharmaceutical vial.
[0313] EMBODIMENT 28 The average wall thickness T is less than or equal to 0.85*s1 i 19. The glass pharmaceutical vial of embodiment 18, wherein said sidewall of said glass pharmaceutical vial having a .gtoreq..gtoreq..times ...
[0314] EMBODIMENT 29 The average wall thickness T is less than or equal to 0.85*s1 i 19. The glass pharmaceutical vial of embodiment 18, wherein said sidewall of said glass pharmaceutical vial having a cross-sectional area of about 100 mm correlates with a 5% or greater reduction in the amount of CO2 emitted to create said glass pharmaceutical vial.
[0315] EMBODIMENT 30 The average wall thickness T is less than or equal to 0.85*s1 i 19. The glass pharmaceutical vial of embodiment 18, wherein the sidewall of the glass pharmaceutical vial having a diameter of 100 mm or less correlates with a 20% or greater reduction in the amount of energy used to separate the glass pharmaceutical vial from a glass tubing blank.
[0316] EMBODIMENT 31 The glass pharmaceutical vial is compliant with USP <660> 19. The glass pharmaceutical vial of embodiment 18, having a Type 1 chemical durability according to
[0317] EMBODIMENT 32 19. The glass pharmaceutical vial of embodiment 18, wherein said glass pharmaceutical vial comprises a dynamic impact coefficient, determined in accordance with a dynamic impact test, of less than 0.9.
[0318] EMBODIMENT 33 19. The glass pharmaceutical vial of embodiment 18, wherein said glass pharmaceutical vial comprises a FWHM factor of at least 1.2, determined according to a dynamic impact test.
[0319] EMBODIMENT 34 The glass pharmaceutical vial is A dynamic impact coefficient of less than 0.9, as determined in accordance with a dynamic impact test; and a FWHM factor of at least 1.2, as determined in accordance with said dynamic impact test. 19. The glass pharmaceutical vial of embodiment 18, comprising:
[0320] EMBODIMENT 35 1. A glass pharmaceutical vial comprising: a glass body including a sidewall enclosing an interior volume, an outer diameter D, and an outer organic coating disposed on the sidewall; the outer diameter D of the glass body is greater than or equal to 84% and less than or equal to 116% of a diameter d1 of a glass vial having a size designation X as defined by ISO 8362-1:2018, where X is the smallest size designation among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018 in which 116% of the diameter d1 is greater than or equal to D; The sidewall of the glass pharmaceutical vial has an average wall thickness T i wherein s1 is the wall thickness of said glass vial of size designation X as defined by ISO 8362-1:2018; The glass pharmaceutical vial has a breakage coefficient of at least 50, as determined according to a pendulum impact test. Glass pharmaceutical vials.
[0321] EMBODIMENT 36 36. The glass pharmaceutical vial of embodiment 35, wherein the external organic coating has a thickness of 20 nm or more and 40 nm or less.
[0322] EMBODIMENT 37 36. The glass pharmaceutical vial of embodiment 35, comprising a low temperature storage factor, determined in accordance with a freeze-thaw test, of at least 2.25.
[0323] EMBODIMENT 38 36. The glass pharmaceutical vial of embodiment 35, comprising a compliance factor of at least 1.75 as determined in accordance with a vial compliance test.
[0324] EMBODIMENT 39 36. The glass pharmaceutical vial of embodiment 35, comprising a horizontal strength coefficient of at least 1.5 as determined according to a horizontal compression test.
[0325] EMBODIMENT 40 36. The glass pharmaceutical vial of embodiment 35, wherein said glass pharmaceutical vial comprises a dynamic impact coefficient, determined in accordance with a dynamic impact test, of less than 0.9.
[0326] EMBODIMENT 41 36. The glass pharmaceutical vial of embodiment 35, wherein said glass pharmaceutical vial comprises a FWHM factor of at least 1.2, determined according to a dynamic impact test.
[0327] EMBODIMENT 42 The glass pharmaceutical vial is A dynamic impact coefficient of less than 0.9, as determined in accordance with a dynamic impact test; and a FWHM factor of at least 1.2, as determined in accordance with said dynamic impact test. 36. The glass pharmaceutical vial of embodiment 35, comprising:< / usp>
Claims
1. 1. A glass pharmaceutical vial comprising: a glass body including a sidewall enclosing an interior volume and an outer diameter D; The outer diameter D of the glass body is the diameter d of a glass vial of size designation X defined by ISO 8362-1:2018. 1 X is 84% or more and 116% or less of the diameter d among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R defined by ISO 8362-1:2018. 1 is the smallest size designation for which 116% is equal to or greater than D, The sidewall of the glass pharmaceutical vial has a thickness of 0.85*s 1 The average wall thickness T i s 1 is the wall thickness of the glass vial of size designation X as defined by ISO 8362-1:2018; The glass pharmaceutical vial comprises a compliance factor of at least 1.75 as determined in accordance with a vial compliance test. Glass pharmaceutical vials.
2. 10. The glass pharmaceutical vial of claim 1 comprising a horizontal strength coefficient of at least 0.5 as determined in accordance with a horizontal compression test.
3. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial comprises an exterior organic coating and a horizontal strength coefficient of at least 1.5 determined pursuant to a horizontal compression test.
4. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial comprises an exterior organic coating.
5. 5. The glass pharmaceutical vial of claim 4, wherein said outer organic coating is an organic coating having a thickness of 20 nm to 40 nm.
6. 5. The glass pharmaceutical vial of claim 4, wherein said glass pharmaceutical vial comprises a modulus of failure of at least 50 as determined in accordance with a pendulum impact test.
7. 5. The glass pharmaceutical vial of claim 4, wherein said glass pharmaceutical vial comprises a low temperature storage factor, determined pursuant to a freeze-thaw test, of at least 2.
25.
8. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial is formed from Type I, Class B glass according to ASTM standard E438-92.
9. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial is formed from an aluminosilicate glass composition.
10. 0.85*s 1 The average wall thickness T i 10. The glass pharmaceutical vial of claim 1, wherein said sidewall having a mass of about 10% or more correlates with a reduction in the mass of glass used to make said glass pharmaceutical vial.
11. 0.85*s 1 The average wall thickness T i 10. The glass pharmaceutical vial of claim 1, wherein said sidewall of said glass pharmaceutical vial having a thermal conductivity of about 1000 .mu.m correlates with a 5% or greater reduction in the amount of energy used to convert said glass pharmaceutical vial from a glass tubing blank.
12. 0.85*s 1 The average wall thickness T i The sidewall of the glass pharmaceutical vial is formed with CO 2 evacuated to create the glass pharmaceutical vial. 2 2. The glass pharmaceutical vial of claim 1, wherein the glass pharmaceutical vial has a viscosity of 100:1 or more.
13. 0.85*s 1 The average wall thickness T i 10. The glass pharmaceutical vial of claim 1, wherein said sidewall of said glass pharmaceutical vial having a diameter of about 10 mm is correlated with a 20% or greater reduction in the amount of energy used to separate said glass pharmaceutical vial from a glass tubing blank.
14. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial has a Type 1 chemical durability according to USP <660>.
15. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial comprises a dynamic shock coefficient, determined in accordance with a dynamic impact test, of less than 0.
9.
16. 10. The glass pharmaceutical vial of claim 1, wherein said glass pharmaceutical vial comprises a FWHM coefficient of at least 1.2, determined pursuant to a dynamic impact test.
17. The glass pharmaceutical vial is A dynamic impact coefficient of less than 0.9, as determined in accordance with a dynamic impact test; an FWHM factor of at least 1.2, as determined in accordance with the Dynamic Impact Test; 2. The glass pharmaceutical vial of claim 1, comprising:
18. 1. A glass pharmaceutical vial comprising: a glass body including a sidewall enclosing an interior volume and an outer diameter D; The outer diameter D of the glass body is the diameter d of a glass vial of size X defined by ISO 8362-1:2018. 1 and X is one of 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R as defined by ISO 8362-1:2018; The sidewall of the glass pharmaceutical vial has a thickness of 0.85*s 1 The average wall thickness T i s 1 is the wall thickness of the glass vial of size X as defined by ISO 8362-1:2018; The glass pharmaceutical vial comprises a compliance factor of at least 1.75 as determined in accordance with a vial compliance test. Glass pharmaceutical vials.
19. 20. The glass pharmaceutical vial of claim 18 comprising a horizontal strength coefficient of at least 0.5 as determined in accordance with a horizontal compression test.
20. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial comprises an exterior organic coating and a horizontal strength coefficient of at least 1.5 determined pursuant to a horizontal compression test.
21. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial comprises an exterior organic coating.
22. 22. The glass pharmaceutical vial of claim 21, wherein said exterior organic coating is an organic coating having a thickness of 20 nm to 40 nm.
23. 22. The glass pharmaceutical vial of claim 21, wherein said glass pharmaceutical vial comprises a modulus of failure of at least 50 as determined in accordance with a pendulum impact test.
24. 22. The glass pharmaceutical vial of claim 21, wherein said glass pharmaceutical vial comprises a low temperature storage factor, determined pursuant to a freeze-thaw test, of at least 2.
25.
25. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial is formed from Type I, Class B glass according to ASTM standard E438-92.
26. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial is formed from an aluminosilicate glass composition.
27. 0.85*s 1 The average wall thickness T i 20. The glass pharmaceutical vial of claim 18, wherein said sidewall having a mass of 0.1 to 0.5 mm correlates with a 10% or greater reduction in the mass of glass used to make said glass pharmaceutical vial.
28. 0.85*s 1 The average wall thickness T i 20. The glass pharmaceutical vial of claim 18, wherein said sidewall of said glass pharmaceutical vial having a thermal conductivity of about 1000 .mu.m correlates with a 5% or greater reduction in the amount of energy used to convert said glass pharmaceutical vial from a glass tubing blank.
29. 0.85*s 1 The average wall thickness T i The sidewall of the glass pharmaceutical vial is formed with CO 2 evacuated to create the glass pharmaceutical vial. 2 20. The glass pharmaceutical vial of claim 18, wherein the glass pharmaceutical vial has a viscosity that correlates with a 5% or greater reduction in the amount of
30. 0.85*s 1 The average wall thickness T i 20. The glass pharmaceutical vial of claim 18, wherein said sidewall of said glass pharmaceutical vial having a diameter of about 10 mm correlates with a 20% or greater reduction in the amount of energy used to separate said glass pharmaceutical vial from a glass tubing blank.
31. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial has a Type 1 chemical durability according to USP <660>.
32. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial comprises a dynamic shock coefficient, determined in accordance with a dynamic impact test, of less than 0.
9.
33. 20. The glass pharmaceutical vial of claim 18, wherein said glass pharmaceutical vial comprises a FWHM coefficient of at least 1.2, determined pursuant to a dynamic impact test.
34. The glass pharmaceutical vial is A dynamic impact coefficient of less than 0.9, as determined in accordance with a dynamic impact test; an FWHM factor of at least 1.2, as determined in accordance with the Dynamic Impact Test; 20. The glass pharmaceutical vial of claim 18, comprising:
35. 1. A glass pharmaceutical vial comprising: a glass body including a sidewall enclosing an interior volume, an outer diameter D, and an exterior organic coating disposed on the sidewall; The outer diameter D of the glass body is the diameter d of a glass vial of size designation X defined by ISO 8362-1:2018. 1 X is 84% or more and 116% or less of the diameter d among 2R, 3R, 4R, 6R, 8R, 10R, 15R, 20R, 25R, 30R, 50R, and 100R defined by ISO 8362-1:2018. 1 is the smallest size designation for which 116% is equal to or greater than D, The sidewall of the glass pharmaceutical vial has a thickness of 0.85*s 1 The average wall thickness T i s 1 is the wall thickness of the glass vial of size designation X as defined by ISO 8362-1:2018; The glass pharmaceutical vial has a breakage coefficient of at least 50, as determined according to a pendulum impact test. Glass pharmaceutical vials.
36. 36. The glass pharmaceutical vial of claim 35, wherein said outer organic coating has a thickness of 20 nm or more and 40 nm or less.
37. 36. The glass pharmaceutical vial of claim 35, comprising a low temperature storage factor, determined in accordance with a freeze-thaw test, of at least 2.
25.
38. 36. The glass pharmaceutical vial of claim 35 comprising a compliance factor of at least 1.75 as determined pursuant to a vial compliance test.
39. 36. The glass pharmaceutical vial of claim 35, comprising a horizontal strength coefficient of at least 1.5 as determined in accordance with a horizontal compression test.
40. 36. The glass pharmaceutical vial of claim 35, wherein said glass pharmaceutical vial comprises a dynamic shock coefficient, determined in accordance with a dynamic impact test, of less than 0.
9.
41. 36. The glass pharmaceutical vial of claim 35, wherein said glass pharmaceutical vial comprises an FWHM coefficient of at least 1.2, determined in accordance with a dynamic impact test.
42. The glass pharmaceutical vial is A dynamic impact coefficient of less than 0.9, as determined in accordance with a dynamic impact test; an FWHM factor of at least 1.2, as determined in accordance with the Dynamic Impact Test; 36. The glass pharmaceutical vial of claim 35, comprising:
Citation Information
Patent Citations
Glass articles with low-friction coatings
CN104271346A
Lyophilization of dextran compound
JP1996126685A
Glass articles with low-friction coatings