Setting control compositions for cementitious systems

A synergistic set control composition using hydroxymonocarboxylic acid, borate, and carbonate sources with a polyol in cementitious systems addresses the challenge of maintaining workability and early strength development, achieving balanced performance.

JP2024536208AInactive Publication Date: 2024-10-04CONSTRUCTION RESEARCH & TECHNOLOGY GMBH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024519494
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-29
Filing Date
2022-09-28
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing set control compositions for cementitious systems fail to improve workability over long periods without compromising early compressive strength, and known retarders often cause undue retardation or inadequate strength development.

Method used

A set control composition comprising hydroxymonocarboxylic acid or its salt, a borate source, and a carbonate source, along with a polyol, synergistically retards early aluminate reactions while allowing gradual hardening, maintaining workability and promoting early strength development.

Benefits of technology

The composition effectively extends the workability of cementitious systems while ensuring significant strength development occurs at an early stage, balancing initial workability with rapid hardening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536208000026
    Figure 2024536208000026
  • Figure 2024536208000001
    Figure 2024536208000001
  • Figure 2024536208000002
    Figure 2024536208000002
Patent Text Reader

Abstract

A setting control composition for cementitious systems comprising: a) (a-1) a hydroxymonocarboxylic acid or a salt thereof, in which (a-1) accounts for at least 90% of the carboxyl groups relative to the total number of carboxyl groups in (a-1) and (a-2) below, and (a-2) optionally a polycarboxylic acid or a salt thereof having a carboxylic acid equivalent, calculated by dividing the molecular weight of the polycarboxylic acid by the number of carboxylic acid functional groups, of 333 or less; b) a borate source (b-1) in a weight ratio of b) to a) ranging from 1.2 to 20; and (b-2) a viscosity at 25°C of 0.1 g·L -1 and c) at least one of an inorganic carbonate having a water solubility of not less than 1.0 and a carbonate source selected from an organic carbonate, and a polyol in a weight ratio of c) to a) ranging from 1.0 to 10. The set control composition for cementitious systems effectively improves the workability of cementitious systems over a long period of time without compromising early compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to set control compositions for cementitious systems and construction compositions comprising set control compositions.

[0002] It is known to add dispersants to aqueous slurries or powdered hydraulic binders to improve their workability, i.e. their mixability, spreadability, sprayability, pumpability or flowability. Such admixtures are capable of preventing the formation of solid aggregates and dispersing already existing particles and those newly formed by hydration, thus improving the workability. This effect is exploited in the preparation of construction compositions containing hydraulic binders such as cement, lime, gypsum, hemihydrate or anhydrite. To convert the powdered binder into a freshly mixed, workable form, substantially more mixing water is required than is required for the subsequent hydration and hardening process. The voids formed in the concrete body by the excess water lead to a reduction in mechanical strength and resistance due to the subsequent evaporation of the water. To reduce the proportion of excess water at a given working consistency and / or to improve the workability at a given water / binder ratio, admixtures, commonly called water reducers or plasticizers, are used.

[0003] When cementitious systems hydrate, ettringite is generally produced in a rapid reaction. This reaction is responsible for the setting of the cement paste, i.e., the hardening of the paste to a certain consistency. The initial setting time is the time when the paste starts to lose plasticity, and the final setting time is the time when the paste completely loses plasticity. The formation of ettringite is also responsible for the development of early compressive strength of the cementitious composition. The final hardening of the cement paste, i.e., the increase in mechanical strength, is mainly due to the formation of calcium silicate hydrate (CSH) phases upon the subsequent reaction of C3S with C2S in the clinker. However, the newly formed micro-ettringite crystals tend to deteriorate the workability or fluidity of the cementitious composition. To slow down the reaction and improve the workability, it is known to add set control agents or retarders to the composition. These commonly known retarders delay the onset of hydration by inhibiting the dissolution of reactive cement components, especially aluminates, and / or by masking calcium ions to slow down the hydration reaction. These mechanisms influence both the early aluminate reaction to form ettringite and the subsequent formation of the CSH phase.

[0004] It is well known in the art that the addition of commonly known retarders, such as small molecule hydroxyl carboxylic acids with strong cement-binding properties like tartaric, citric or gluconic acid, has a retarding or slowing effect on early ettringite formation, as well as a more pronounced effect on the later reaction phase involving CSH formation. Such additions are used to adjust the initial setting time and the time at which final strength is established. At higher dosages, these effects can be driven to the extent that the cement paste is effectively "aged" for hours or even days with very slow or essentially no strength development.

[0005] US Patent No. 5,792,252 relates to a cement admixture containing an alkali metal carbonate and a mono- or dicarboxylic acid or its alkali metal salt, or an alkali metal salt of a tricarboxylic acid.

[0006] U.S. Pat. No. 4,175,975 relates to water-soluble salts of low molecular weight polyacrylic acids which work in conjunction with inorganic salts to reduce the water demand of dispersed inorganic solids such as Portland cement.

[0007] WO 2019 / 077050 describes a setting control composition for cementitious systems comprising an amine-glyoxylic acid condensate and at least one of a borate source and a carbonate source.

[0008] There continues to be a need for additional set control compositions for cementitious systems that effectively improve the workability of cementitious systems over the long term without compromising early compressive strength.

[0009] The above problem is solved by a setting control composition for cementitious systems, comprising: a) (a-1) accounts for at least 90% of the carboxyl groups of the following (a-1) and (a-2), (a-1) a hydroxymonocarboxylic acid or a salt thereof, and (a-2) optionally, a polycarboxylic acid having a carboxylic acid equivalent of 333 or less, which is calculated by dividing the molecular weight of the polycarboxylic acid by the number of carboxylic acid functional groups, or a salt thereof; b) in a weight ratio of b) to a) in the range of 1.2 to 20 (b-1) a borate source; (b-2) 0.1 g L at 25°C -1 a carbonate source selected from inorganic carbonates having a water solubility of at least At least one of the following: c) a polyol in a weight ratio of c) to a) ranging from 1.0 to 10. The problem is solved by a setting control composition comprising:

[0010] All three components must be present simultaneously in the cementitious system and are crucial to performance. The absence of any one of the components severely impacts performance. In one embodiment, a premix of components a), b) and c) constitutes the setting control composition that is added to the cementitious composition. The composition may be made directly in the cementitious system by adding the components separately directly to the cementitious system.

[0011] Although the above components a-1), b) and c) have been used individually or as sub-combinations lacking at least one of the above components, it has surprisingly been found that all combinations of components a-1), b) and c) according to the invention act synergistically, even in the essential absence of polycarboxylic acid a-2). Components a-1) and b) are applied at relatively high dosages that may cause excessive retardation of the cementitious system if the components are added alone (see, for example, Comparative Examples 20-a and 20-b below). The set control composition of the invention has an excellent retarding effect mainly on premature aluminate reactions and only a slight effect on CSH formation. Crystalline ettringite has a water content of 26 moles of H2O per mole of ettringite, i.e., per equivalent of Al2O3. Inhibition of ettringite formation leads to improved initial workability, since less water is chemically bound in ettringite and no free water is physically adsorbed on the newly formed crystal surfaces. Despite the improvements in early workability, a significant "step-hardening" effect is observed once ettringite formation begins, with significant strength development occurring at an early stage, for example as early as 2-3 hours.

[0012] The setting control composition according to the invention comprises a retarder a) selected from (a-1) and optionally (a-2), with (a-1) accounting for at least 90% of the carboxyl groups relative to the total number of carboxyl groups of (a-1) and (a-2). It is believed that the retarder stabilizes the aluminate phase, thereby retarding the dissolution of the aluminate phase or inhibiting the precipitation of ettringite crystals and / or preventing the growth of ettringite crystal seeds, or by a combination of all effects, inhibits the rapid formation of ettringite from the aluminate phase originating from the hydraulic binder.

[0013] Component (a-1) is a hydroxymonocarboxylic acid or its salt. In general, such hydroxymonocarboxylic acids or their salts are known per se and allow an open time extension acting both on the early and on the late hydration phases.

[0014] Suitable hydroxymonocarboxylic acids or their salts are preferably α-hydroxymonocarboxylic acids and their salts, including glycolic acid, gluconic acid, lactic acid, 2,3-dihydroxypropanoic acid, and their salts and mixtures thereof. The hydroxymonocarboxylic acids can be used as free acids or in partially or completely neutralized form, i.e., as salts. The cations are not particularly limited and can be selected from alkali metals, such as sodium or potassium, and ammonium cations. Sodium gluconate is particularly preferred.

[0015] Component (a-2) is a polycarboxylic acid or a salt thereof having a carboxylic acid equivalent of 333 or less. Component (a-2) may be included in a limited amount as long as component (a-1) accounts for at least 90% of the carboxyl groups based on the total number of carboxyl groups in components (a-1) and (a-2).

[0016] In one embodiment, the set control composition is essentially free of polycarboxylic acids having a carboxylic acid equivalent of 333 or less, and salts thereof, such as amine-glyoxylic acid condensates, such as melamine-glyoxylic acid condensates, urea-glyoxylic acid condensates, melamine-urea-glyoxylic acid condensates or polyacrylamide-glyoxylic acid condensates, or salts thereof. For example, component (a-1) can account for at least 95%, preferably 98%, more preferably 100% of the carboxyl groups, based on the total number of carboxyl groups in (a-1) and (a-2).

[0017] The term polycarboxylic acid, as used herein, refers to compounds that contain two or more carboxylic acid functional groups in their molecular structure. This includes low molecular weight compounds with two or three carboxylic acid functional groups, such as citric acid or tartaric acid. The term "polycarboxylic acid" further includes polymeric compounds composed of monomer units incorporating carboxylic acid functional groups and, optionally, further monomer units. The polycarboxylic acids can be used as free acids or in partially or completely neutralized form, i.e. as salts. The cations are not particularly limited and can be selected from alkali metals, such as sodium or potassium, and ammonium cations. Only polycarboxylic acids with a carboxylic acid equivalent of 333 or less, or salts thereof, are envisaged to act as cement retarders in the sense of the present invention, i.e. mainly to retard the early hydration phase (ettringite). On the other hand, higher molecular weight or polymeric compounds with a higher carboxylic acid equivalent, meaning that the carboxylic acids are incorporated further apart, have a negligible retarding effect.

[0018] For molecules with low molecular weight, the number of carboxylic acid groups can be counted. The carboxylic acid equivalent of a low molecular weight compound can be determined as the molecular weight divided by the number of carboxylic acid functional groups in the molecular structure. This means, for example, that citric acid, which has a molecular weight of 192 g / mol and three carboxylic acid groups, has a carboxylic acid equivalent of 192 / 3=64.

[0019] For polymeric polycarboxylic acids with higher molecular weight or molecular weight distribution, the carboxylic acid equivalent can be determined by weighing a sample of the polymeric polycarboxylic acid and titrating the carboxylic acid group. Alternatively, for polymeric polycarboxylic acids with known carboxylic acid group density, the carboxylic acid equivalent of the polymeric polycarboxylic acid can be determined as the reciprocal of the carboxylic acid group density expressed as equivalents per gram of polymer. This means, for example, that a polymeric polycarboxylic acid with a milliequivalent number of 3.0 meq / g has a carboxylic acid equivalent of 1 / 0.003=333.

[0020] The molecular weight of the polycarboxylic acid is 25000 g / mol or less, preferably, the molecular weight is in the range of 1000 to 25000 g / mol, and most preferably, the molecular weight is in the range of 1000 to 5000 g / mol. The molecular weight can be measured by gel permeation chromatography (GPC) as shown in detail in the experimental section.

[0021] Component b) is at least one of (b-1) a borate source and (b-2) a carbonate source.

[0022] The presence of a borate or carbonate source ensures that the formulation water is initially highly concentrated with boric acid or carbonate ions, which are believed to adsorb to the mineral phase surfaces and prevent the hydroxymono- and / or polycarboxylic acids from adsorbing to the mineral phase surfaces, thus the latter remaining in the pore solution and initially preventing the formation of ettringite in the pore solution prior to setting.

[0023] The borate source typically comprises an inexpensive borate compound that can be rapidly dissolved. Suitable borate sources include borax, boric acid, metaborate, colemanite and hexahydroborate.

[0024] Only carbonate sources with sufficient water solubility are suitable to achieve the desired effect. The carbonate source should have a concentration of 0.1 g L at 25 °C. -1The inorganic carbonate may be an inorganic carbonate having a water solubility of 700 mg / kg or more. The water solubility of the inorganic carbonate is suitably determined in water having a starting pH value of 7. It is understood that the pH value at the solubility limit is higher than the starting pH value.

[0025] Inorganic carbonate can be selected from alkali metal carbonate, such as sodium carbonate, sodium hydrogen carbonate, potassium carbonate or lithium carbonate, and alkaline earth metal carbonate, such as magnesium carbonate, that meets the required water solubility.It is also possible to use guanidine carbonate as inorganic carbonate.Sodium carbonate, potassium carbonate, sodium hydrogen carbonate and potassium hydrogen carbonate, especially sodium carbonate and sodium hydrogen carbonate, are particularly preferred.

[0026] Alternatively, the carbonate source is selected from organic carbonates. "Organic carbonate" refers to an ester of carbonic acid. The organic carbonate is hydrolyzed in the presence of the cementitious system to release carbonate ions. In one embodiment, the organic carbonate is selected from ethylene carbonate, propylene carbonate, glycerol carbonate, dimethyl carbonate, di(hydroxyethyl)carbonate or mixtures thereof, preferably ethylene carbonate, propylene carbonate and glycerol carbonate, or mixtures thereof, in particular ethylene carbonate and / or propylene carbonate. Mixtures of inorganic carbonates and organic carbonates can also be used.

[0027] The weight ratio of component b) to component a) is in the range of 1.2 to 20, preferably 1.2 to 8.0, for example, 4.0 to 6.0.

[0028] The ratio of component b) to component a) varies depending on the application of the cementitious system. For some applications, such as shotcrete, a higher ratio of up to 20 may be required to sufficiently prolong the setting time without compromising early strength development. For other applications, the ratio typically ranges from 1.2 to 8.0.

[0029] If the amount of carbonate and / or borate source is excessive, the cementitious system will exhibit poor workability, whereas if the amount is too low, it will set too quickly.

[0030] Component c) is a polyol. The polyol is used in a weight ratio of component c) to a) ranging from 1.0 to 10, preferably from 5.0 to 9.0.

[0031] Polyols such as glycerol are believed to chelate calcium ions, e.g. of calcium sulfate or C3A, especially under the alkaline pH conditions of the cementitious mix, resulting in accelerated dissociation of the calcium ions. Chelation of the calcium ions also stabilizes calcium in solution and accelerates dissolution of calcium aluminate phases, making the aluminates from these calcium aluminate phases more available, resulting in a better / more complete utilization of the total amount of clinker available in the respective binder composition.

[0032] "Polyol" is intended to denote a compound having at least two alcoholic hydroxyl groups in the molecule, for example 3, 4, 5 or 6 alcoholic hydroxyl groups. Polyols having adjacent hydroxyl groups are preferred. Polyols having at least three hydroxyl groups attached consecutively to three carbon atoms are most preferred.

[0033] The ability of a polyol to chelate calcium ions and thereby stabilize calcium in solution can be evaluated by a calcium aluminate precipitation test. In one embodiment, in a calcium aluminate precipitation test in which a test solution obtained by adding 20 mL of a 1 mol / L aqueous NaOH solution and 50 mL of a 25 mmol / L aqueous NaAlO2 solution to 400 mL of a 1 wt % aqueous solution of the polyol is titrated with a 0.5 mol / L aqueous CaCl2 solution at 20° C., the polyol inhibits calcium aluminate precipitation up to a calcium concentration of 75 ppm, preferably 90 ppm.

[0034] In this test, the precipitation of calcium aluminate is detected by turbidity. Initially, the test solution is a clear solution. The clear test solution is titrated with an aqueous solution of CaCl2 at a constant application rate of, for example, 2 mL / min, as described above. Continued addition of CaCl2 causes calcium aluminate to precipitate and changes the optical properties of the test solution by turbidity. The maximum calcium concentration before the onset of turbidity (Ca 2+ The titration endpoint, expressed as the time elapsed to the starting point, can be calculated.

[0035] In a preferred embodiment, the polyol is selected from compounds consisting only of carbon, hydrogen and oxygen and does not contain a carboxyl group (COOH) in the molecule.

[0036] In another preferred embodiment, the polyol is selected from compounds consisting only of carbon, hydrogen and oxygen and does not contain any carboxyl (COOH) or carbonyl (C=O) groups in the molecule. The term "carbonyl" is understood to encompass the tautomer of the C=O group, i.e., the pair of double-bonded carbon atoms adjacent to a hydroxyl group (-C=C(OH)-).

[0037] In one embodiment, the polyol is a monosaccharide, oligosaccharide, water-soluble polysaccharide, or a polysaccharide of the general formula (PI): [ka] [In the formula, X is [ka] where: R is -CH2CH3, -CH2OH, -NH2; n is an integer from 1 to 4; m is an integer from 1 to 8. or a dimer or trimer of a compound of general formula (PI).

[0038] In one embodiment, the polyol is selected from saccharides.Useful saccharides include monosaccharides such as glucose and fructose; disaccharides such as lactose and sucrose; trisaccharides such as raffinose; and water-soluble polysaccharides such as amylose and maltodextrin.Monosaccharides and disaccharides are particularly preferred, especially sucrose.

[0039] Compounds of formula (PI) where X is (P-Ia) are generally referred to as sugar alcohols. Sugar alcohols are organic compounds that contain one hydroxyl group (-OH) attached to each carbon atom, typically derived from sugar. Useful sugar alcohols are mannitol, sorbitol, xylitol, arabitol, erythritol and glycerol. Of these, erythritol and glycerol are particularly preferred. It is envisioned that carbonates of polyhydric alcohols, such as glycerol carbonate, can serve as polyol sources.

[0040] Compounds of formula (PI) where X is (P-Ib) include pentaerythritol, tris(hydroxymethyl)aminomethane and tris(hydroxymethyl)propane.

[0041] Compounds of formula (PI) where X is (P-Ic) include triethanolamine.

[0042] A dimer or trimer refers to a compound in which two or three molecules of general formula (PI) are linked via ether bridges, formally derived from a condensation reaction with the elimination of one or two molecules of water. Examples of dimers and trimers of compounds of formula (PI) include dipentaerythritol and tripentaerythritol.

[0043] The set control composition may further comprise a dispersant. Dispersants useful for cement applications are known per se. For purposes herein, the term dispersant includes plasticizers and superplasticizers.

[0044] It will be appreciated that many useful dispersants contain carboxyl groups, salts thereof, or hydrolyzable groups that release carboxyl groups upon hydrolysis. Preferably, the number of milliequivalents of carboxyl groups contained in these dispersants (or carboxyl groups that can be released upon hydrolysis of hydrolyzable groups contained in the dispersants) is less than 3.0 meq / g, assuming all carboxyl groups are in unneutralized form.

[0045] Examples of useful dispersants include: - a comb polymer having a carbon-containing backbone with pendant cement anchoring groups and polyether side chains attached thereto; - a non-ionic comb polymer having a carbon-containing backbone with pendant hydrolyzable groups and polyether side chains attached, the hydrolyzable groups releasing cement anchoring groups upon hydrolysis; - Al, in which polyvalent metal cations are present in superstoichiometric amounts, calculated as cation equivalents, based on the sum of the negative and anion-forming groups of the polymeric dispersant. 3+ , Fe 3+ or Fe 2+ colloidal dispersion preparations of polyvalent metal cations such as dimethylformamide, ... sulfonated melamine-formaldehyde condensates, - lignosulfonates, sulfonated ketone-formaldehyde condensates, sulfonated naphthalene-formaldehyde condensates, - a phosphonate-containing dispersant, preferably comprising at least one polyalkylene glycol unit, - A mixture of them Examples include:

[0046] Preferably, the dispersant d) is present in a weight ratio of d) to a) ranging from 0.05 to 20.

[0047] Particularly preferred are comb polymers having a carbon-containing backbone with pendant cement anchoring groups and polyether side chains attached. The cement anchoring groups are negative and / or anion generating groups such as carboxylic acid, phosphonic acid or phosphoric acid groups or their anions. The anion generating groups are acid groups present in the polymer dispersant which can be converted to the respective negative groups under alkaline conditions.

[0048] Preferably, the structural units comprising negative and / or anion generating groups have the general formula (Ia), (Ib), (Ic) and / or (Id): [ka] [In the formula, R 1 is H, C1-C4 alkyl, CH2COOH or CH2CO-XR 3A , preferably H or methyl; X is NH-(C n1 H 2n1 ) or O-(C n1 H 2n1 ) with n1=1, 2, 3 or 4 or a chemical bond, the nitrogen or oxygen atom being bonded to a CO group, R 2 is OM, PO3M2 or O-PO3M2, except that R 2 is OM, X is a chemical bond, R 3A is PO3M2 or O-PO3M2]; [ka] [In the formula, R 3 is H or C1-C4 alkyl, preferably H or methyl; n is 0, 1, 2, 3 or 4; R 4 is PO3M2 or O-PO3M2]; [ka] [In the formula, R5 is H or C1-C4 alkyl, preferably H; Z is O or NR 7 and R 7 is H, (C n1 H 2n1 )-OH, (C n1 H 2n1 )-PO3M2, (C n1 H 2n1 )-OPO3M2, (C6H4)-PO3M2 or (C6H4)-OPO3M2; n1 is 1, 2, 3, or 4]; [ka] [In the formula, R 6 is H or C1-C4 alkyl, preferably H; Q is NR 7 or O, R 7 is H, (C n1 H 2n1 )-OH, (C n1 H 2n1 )-PO3M2, (C n1 H 2n1 )-OPO3M2, (C6H4)-PO3M2 or (C6H4)-OPO3M2; n1 is 1, 2, 3 or 4] where each M is independently H or a cationic equivalent.

[0049] Preferably, the structural units comprising polyether side chains have the general formula (IIa), (IIb), (IIc) and / or (IId): [ka] [In the formula, R 10 , R 11 and R 12 are each independently H or C1-C4 alkyl, preferably H or methyl; Z 2 is O or S, E is C2-C6 alkylene, cyclohexylene, CH2-C6H 10 , 1,2-phenylene, 1,3-phenylene or 1,4-phenylene; G is O, NH or CO-NH, or E and G together are a chemical bond A is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; n2 is 0, 1, 2, 3, 4 or 5; a is an integer of 2 to 350, preferably 10 to 150, and more preferably 20 to 100; R 13 is H, an unbranched or branched C1-C4 alkyl group, CO-NH2 or COCH3; [ka] [In the formula, R 16 , R 17 and R 18 are each independently H or C1-C4 alkyl, preferably H; E 2 C2-C6 alkylene, cyclohexylene, CH2-C6H 10 , 1,2-phenylene, 1,3-phenylene or 1,4-phenylene, or a chemical bond; A is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; n2 is 0, 1, 2, 3, 4 or 5; L is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; a is an integer of 2 to 350, preferably 10 to 150, and more preferably 20 to 100; d is an integer of 1 to 350, preferably 10 to 150, more preferably 20 to 100; R 19 is H or C1-C4 alkyl, R 20 is H or C1-C4 alkyl]; [ka] [In the formula, R 21 , R 22 and R 23 are independently H or C1-C4 alkyl, preferably H; W is O, NR 25 or N, V is W=O or NR 25 1 if W=N, 2 if W=N, A is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; a is an integer of 2 to 350, preferably 10 to 150, and more preferably 20 to 100; R 24 is H or C1-C4 alkyl, R 25 is H or C1-C4 alkyl]; [ka] [In the formula, R 6 is H or C1-C4 alkyl, preferably H; Q is NR 10 , N or O; V is Q=O or NR 10 1 if Q=N, 2 if Q=N, R 10 is H or C1-C4 alkyl, A is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; a is an integer of 2 to 350, preferably 10 to 150, and more preferably 20 to 100. where each M is independently H or a cationic equivalent.

[0050] The molar ratio of structural unit (I) to structural unit (II) varies from 1:3 to about 10:1, preferably from 1:1 to 10:1, more preferably from 3:1 to 6:1. The polymeric dispersants comprising structural units (I) and (II) can be prepared by conventional methods, for example by free radical polymerization or controlled radical polymerization. The preparation of the dispersants is described, for example, in EP-A-0894811, EP-A-1851256, EP-A-2463314 and EP-A-0753488.

[0051] Many useful dispersants contain carboxyl groups, salts thereof, or hydrolyzable groups that release carboxyl groups upon hydrolysis. Preferably, the number of milliequivalents of carboxyl groups contained in these dispersants (or carboxyl groups that can be released upon hydrolysis of hydrolyzable groups contained in the dispersants) is less than 3.0 meq / g, assuming all carboxyl groups are in unneutralized form.

[0052] More preferably, the dispersant is selected from the group of polycarboxylic ethers (PCE). In PCE, the negative groups are carboxylic acid and / or carboxylate groups. The PCE is preferably obtained by radical copolymerization of polyether macromonomers with monomers containing negative and / or anion-generating groups. Preferably, at least 45 mol %, preferably at least 80 mol %, of all structural units constituting the copolymer are structural units of polyether macromonomers or monomers containing negative and / or anion-generating groups.

[0053] A further class of suitable comb polymers having a carbon-containing backbone with pendant cement anchoring groups and polyether side chains attached thereto comprises structural units (III) and (IV): [ka] [In the formula, T is phenyl, naphthyl, or heteroaryl having 5 to 10 ring atoms, one or two of which are heteroatoms selected from N, O, and S; n3 is 1 or 2, B is N, NH or O, with the proviso that when B is N, n3 is 2, and when B is NH or O, n3 is 1; A is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; a2 is an integer from 1 to 300; R 26 is H, C1~C 10 alkyl, C5-C8 cycloalkyl, aryl, or heteroaryl having 5-10 ring atoms, one or two of which are heteroatoms selected from N, O, and S. The structural unit (IV) comprises structural units (IVa) and (IVb): [ka] [In the formula, D is phenyl, naphthyl, or heteroaryl having 5 to 10 ring atoms, one or two of which are heteroatoms selected from N, O, and S; E 3 is N, NH, or O, except that E 3 When is N, m is 2, and E 3 is NH or O, m is 1; A is C2-C5 alkylene or CH2CH(C6H5), preferably C2-C3 alkylene; b is an integer from 0 to 300; M is independently H or a cation equivalent]; [ka] [In the formula, V 2 is phenyl or naphthyl, R 8 , O.H., O.R. 8 , (CO)R 8, COOM, COOR 8 , SO3R 8 and NO2, R 7A is COOM, OCH2COOM, SO3M or OPO3M2, M is H or a cationic equivalent; R 8 is C1-C4 alkyl, phenyl, naphthyl, phenyl-C1-C4 alkyl or C1-C4 alkylphenyl] is selected from.

[0054] Polymers comprising structural units (III) and (IV) are obtained by polycondensation of an aromatic or heteroaromatic compound having polyoxyalkylene groups attached to an aromatic or heteroaromatic core, an aromatic compound having a carboxylic acid, sulfonic acid or phosphoric acid moiety, and an aldehyde compound, such as formaldehyde.

[0055] In one embodiment, the dispersant is a non-ionic comb polymer having a carbon-containing backbone with pendant hydrolyzable groups and polyether side chains attached, where the hydrolyzable groups release cement anchoring groups upon hydrolysis. Advantageously, the structural unit containing the polyether side chain is one of the general formulae (IIa), (IIb), (IIc) and / or (IId) discussed above. The structural unit with the pendant hydrolyzable group is preferably derived from an acrylic acid ester monomer, more preferably a hydroxyalkyl acrylic monoester and / or a hydroxyalkyl diester, most preferably hydroxypropyl acrylate and / or hydroxyethyl acrylate. The ester functional groups hydrolyze to (deprotonated) acid groups on exposure to water, preferably at an alkaline pH provided by mixing the cementitious binder with water, and the resulting acid functional groups then form a complex with the cement component.

[0056] In one embodiment, the dispersant is Al 3+ , Fe 3+ or Fe 2+and a polymeric dispersant containing negative and / or anion generating groups and polyether side chains. The polyvalent metal cation is present in a superstoichiometric amount, calculated as a cation equivalent, based on the sum of the negative and anion generating groups of the polymeric dispersant. Such dispersants are described in further detail in WO 2014 / 013077, which is incorporated herein by reference.

[0057] Suitable sulfonated melamine-formaldehyde condensates are of the type often used as plasticizers for hydraulic binders (also called MFS resins). Sulfonated melamine-formaldehyde condensates and their preparation are described, for example, in CA 2172004, DE 4411797, U.S. Pat. No. 4,430,469, U.S. Pat. No. 6,555,683 and CH 686186, as well as in Ullmann's Encyclopedia of Industrial Chemistry, 5th Ed., vol. A2, page 131 and Concrete Admixtures Handbook - Properties, Science and Technology, 2. Ed., pages 411, 412. Preferred sulfonated melamine-formaldehyde condensates are represented by the (highly simplified and idealized) formula: [ka] The molar weight is preferably in the range of 2500 to 80000. In addition, it is possible to incorporate other monomers by condensation into the sulfonated melamine units. Urea is particularly suitable. In addition, further aromatic units such as gallic acid, aminobenzenesulfonic acid, sulfanilic acid, phenolsulfonic acid, aniline, ammoniobenzoic acid, dialkoxybenzenesulfonic acid, dialkoxybenzoic acid, pyridine, pyridinemonosulfonic acid, pyridinedisulfonic acid, pyridinecarboxylic acid and pyridinedicarboxylic acid may be incorporated by condensation. An example of a melamine sulfonate-formaldehyde condensate is the Melment® product sold by Master Builders Solutions Deutschland GmbH.

[0058] Suitable lignosulfonates are products obtained as by-products in the paper industry. They are described in Ullmann's Encyclopedia of Industrial Chemistry, 5th Ed., vol. A8, pages 586, 587. Lignosulfonates can be represented by the highly simplified and idealized formula: [ka] The lignosulfonates have a molar weight of 2000 to 100000 g / mol. Generally, the lignosulfonates are present in the form of their sodium, calcium and / or magnesium salts. Examples of suitable lignosulfonates are the Borresperse products sold by Borregaard LignoTech, Norway.

[0059] Suitable sulfonated ketone-formaldehyde condensates are products incorporating mono- or diketones as the ketone component, preferably acetone, butanone, pentanone, hexanone or cyclohexanone. Condensates of this type are known and are described, for example, in WO 2009 / 103579. Sulfonated acetone-formaldehyde condensates are preferred. These are generally represented by the formula (according to J. Plank et al., J. Appl. Poly. Sci. 2009, 2018-2024): [ka] [In the formula, m2 and n5 are each generally 10 to 250, and M 2 is Na + and the like, the ratio m2:n5 generally ranging from about 3:1 to about 1:3, more particularly from about 1.2:1 to 1:1.2. Furthermore, it is also possible to incorporate other aromatic units by condensation, such as gallic acid, aminobenzenesulfonic acid, sulfanilic acid, phenolsulfonic acid, aniline, ammoniobenzoic acid, dialkoxybenzenesulfonic acid, dialkoxybenzoic acid, pyridine, pyridinemonosulfonic acid, pyridinedisulfonic acid, pyridinecarboxylic acid and pyridinedicarboxylic acid. An example of a suitable sulfonated acetone-formaldehyde condensate is the Melcret K1L product sold by Master Builders Solutions Deutschland GmbH.

[0060] Suitable sulfonated naphthalene-formaldehyde condensates are products obtained by sulfonation of naphthalene and subsequent polycondensation with formaldehyde. These are described in references including Concrete Admixtures Handbook - Properties, Science and Technology, 2. Ed., pages 411-413, and Ullmann's Encyclopedia of Industrial Chemistry, 5th Ed., vol. A8, pages 587, 588. Sulfonated naphthalene-formaldehyde condensates include those of the formula [ka] The units include:

[0061] Typically, molar weights (Mw) of 1000 to 50000 g / mol are obtained. Furthermore, it is also possible to incorporate other aromatic units by condensation, such as gallic acid, aminobenzenesulfonic acid, sulfanilic acid, phenolsulfonic acid, aniline, ammoniobenzoic acid, dialkoxybenzenesulfonic acid, dialkoxybenzoic acid, pyridine, pyridinemonosulfonic acid, pyridinedisulfonic acid, pyridinecarboxylic acid and pyridinedicarboxylic acid. An example of a suitable sulfonated β-naphthalene-formaldehyde condensate is the Melcret 500 L product sold by Master Builders Solutions Deutschland GmbH.

[0062] Generally, phosphonate-containing dispersants incorporate phosphonic acid groups and pendant polyether groups.

[0063] Suitable phosphonate-containing dispersants have the formula: R-(OA 2 ) n6 -N-[CH2-PO(OM 3 2)2]2 [In the formula, R is H or a hydrocarbon residue, preferably C1-C 15 is an alkyl radical, A 2 are independent of C2~C 18 alkylene, preferably ethylene and / or propylene, most preferably ethylene; n6 is an integer of 5 to 500, preferably 10 to 200, and most preferably 10 to 100; M 3 is H, alkali metal, 1 / 2 alkaline earth metal and / or amine] This is due to.

[0064] The setting control composition according to the invention can be present as a solution or dispersion, in particular an aqueous solution or dispersion. The solution or dispersion preferably has a solids content of 10-50% by weight, in particular 25-35% by weight. Alternatively, the setting control composition according to the invention can be present as a powder. The setting control composition according to the invention can be introduced into the mixing water or during the mixing of the mortar or concrete.

[0065] The set control composition can be used to control the setting time of various cementitious binders, such as portland cement, calcium aluminate cement, and sulfoaluminate cement. In one embodiment, the cementitious binder comprises a mixture of portland cement and aluminate cement, or a mixture of portland cement and sulfoaluminate cement, or a mixture of portland cement, aluminate cement, and sulfoaluminate cement. In particular, the set control composition is used in construction compositions in which the concentration of total available aluminate is controlled.

[0066] The present invention relates to a construction composition comprising: i) a cementitious binder comprising one or more calcium silicate mineral phases and one or more calcium aluminate mineral phases; ii) optionally, an external aluminate source; iii) Optionally, an external sulfate source. Including, The construction composition comprises iv) iv-a) (a-1) accounts for at least 90% of the total number of carboxyl groups in (a-1) and (a-2) below; (a-1) a hydroxymonocarboxylic acid or a salt thereof, and (a-2) optionally, a polycarboxylic acid having a carboxylic acid equivalent of 333 or less, which is calculated by dividing the molecular weight of the polycarboxylic acid by the number of carboxylic acid functional groups, or a salt thereof; iv-b) In a weight ratio of iv-b) to iv-a) in the range of 1.2 to 20 (b-1) a borate source; (b-2) 0.1 g L at 25°C -1 a carbonate source selected from inorganic carbonates having a water solubility of at least At least one of the following: iv-c) a polyol in a weight ratio of iv-c) to iv-a) ranging from 1.0 to 10; A setting control composition comprising The present invention also relates to a construction composition further comprising:

[0067] In one embodiment, the construction composition comprises calcium aluminate mineral phase + Al(OH)4 from any external aluminate source per 100 g of cementitious binder i) - The molar ratio of the total available aluminates to sulfate is 0.4 to 2.0.

[0068] The amounts of available aluminate and the molar ratios of total available aluminate to sulfate shown allow for high early strengths to be obtained, which are important from the standpoint of productivity, for example for increasing the turnover rate of moulds during the manufacture of precast concrete elements.

[0069] Optionally, the construction composition contains dispersants iv-d).

[0070] Generally, the amount of cementitious binder i) in the building composition is at least 8% by weight, preferably at least 10% by weight, more preferably at least 15% by weight and most preferably at least 20% by weight, based on the solid content of the building composition.

[0071] Components iv-a) to iv-d) correspond to components a) to d) above. The above discussion and preferred embodiments apply to both the set control composition and the construction composition.

[0072] In one embodiment, the construction composition comprises, relative to the amount of cementitious binder i), - retarders iv-a) in an amount of 0.2 to 2% by weight, preferably 0.2 to 0.6% by weight, - a borate / carbonate source iv-b) in an amount of 0.8-2.5% by weight, preferably 1.0-2.0% by weight, - polyols iv-c) in amounts of 0.2 to 2.5% by weight; Includes.

[0073] The amount of borate / carbonate source iv-b) may be suitably varied within the ranges given above, but it has been found that the optimum amount of borate / carbonate source iv-b) added to the construction composition of the invention depends to some extent on the total available aluminate content. More specifically, the amount of borate / carbonate source iv-b) is: - 0.7-1.2% by weight when the total available aluminate content is in the range of 0.05-0.08 mol per 100 g of cementitious binder i) less than 0.05-0.08 mol per 100 g of cementitious binder; - 1.2-2.0% by weight when the total available aluminate content is in the range of 0.08-0.2 mol per 100 g of cementitious binder i)

[0074] The amount of polyol iv-c) can be varied appropriately within the above ranges, but it has been found that the optimum amount of polyol iv-c) added to the building composition of the invention depends to some extent on the fineness of the cement clinker. As a rule, the optimum amount of polyol iv-c) added to the building composition of the invention depends to some extent on the fineness of the cement clinker.2 / g, the amount of polyol iv-c) is 0.2-1 wt.% based on the amount of cementitious binder i), and the Blaine surface area is 4000 cm 2 / g, the amount of polyol iv-c) is from 1 to 2.5% by weight relative to the amount of cementitious binder i). However, additives such as fillers or auxiliary cementitious materials can obscure the Blaine surface area of ​​the clinker to some extent. The above principles therefore apply primarily to cementitious binders that essentially do not contain additives such as fillers or auxiliary cementitious materials. The Blaine surface area can be determined according to DIN EN 196-6.

[0075] Cementitious binder i) refers to a binder that hardens in water and contains cement. Cement is a sintered product obtained by burning a raw mixture at high temperature and contains ground clinker with hydraulically reactive calcium silicate and calcium aluminate mineral phases. The clinker is ground with or without additives. In one embodiment, all or part of the components iv-a), iv-b) and / or polyol iv-c) as defined above may already be present during the grinding of the clinker. It is also envisaged that only partial amounts of all or part of the components iv-a), iv-b) and / or polyol iv-c) are present during the grinding of the clinker, with the remainder being added later to the final concentration.

[0076] Typically, the calcium silicate mineral phase and the calcium aluminate mineral phase make up at least 90% by weight of the cementitious binder i), more preferably the calcium silicate mineral phase makes up at least 60% by weight of the cementitious binder i), more preferably at least 65% by weight, most preferably between 65 and 75% by weight.

[0077] For convenience, the mineralogical phases are referred to herein by their cement notation. The major compounds are represented by the type of oxide in the cement notation: C for CaO, M for MgO, S for SiO2, A for Al2O3, $ for SO3, F for Fe2O3, and H for H2O.

[0078] Suitably the calcium silicate mineral phase is selected from C3S (alite) and C2S (belite). The calcium silicate mineral phase provides the final strength properties.

[0079] Suitably the calcium aluminate mineral phase is selected from C3A, C4AF and C12A7, in particular C3A and C4AF.

[0080] In one embodiment, the cementitious binder i) is Portland cement, in particular ordinary Portland cement (OPC). The term "Portland cement" refers to any cement compound containing Portland clinker, in particular CEM I in the sense of section 5.2 of standard EN 197-1. A preferred cement is ordinary Portland cement (OPC) according to DIN EN 197-1. The phases that mainly constitute Portland cement are alite (C3S), belite (C2S), calcium aluminate (C3A), calcium ferroaluminate (C4AF) and other minor phases. Commercially available OPC may contain calcium sulfate (<7% by weight) or be essentially free of calcium sulfate (<1% by weight).

[0081] In an embodiment, the construction composition comprises calcium aluminate mineral phase + Al(OH)4 from any external aluminate source per 100 g of cementitious binder i) - Preferably, the construction composition contains at least 0.065 mol, in particular at least 0.072 mol, of total available aluminate per 100 g of cementitious binder i).

[0082] It has been found that construction compositions containing at least 0.05 mol of total available aluminate per 100 g of cementitious binder i) exhibit optimal performance in terms of open time before setting and early strength development. Otherwise, if the cementitious binder contains more than 0.2 mol of total available aluminate per 100 g of cementitious binder i), the early strength development is too rapid, resulting in a short open time.

[0083] Generally, the approximate percentages of major minerals in Portland cement are calculated by the Bogue formula based on the elemental composition of the clinker, determined for example using X-ray fluorescence (XRF). Such methods provide the oxide composition of the elements. That is, the amount of Al is reported as Al2O3. It has been found that cements with seemingly the same Al2O3 content exhibit quite different properties in terms of early strength and controllability by hydration control. Cements contain Al sources with very different mineralogy and solubility. The inventors have found that not all Al is available or accessible for the formation of ettringite. Only Al-containing mineral phases with adequate solubility in the aqueous environment of the cement paste participate in the formation of ettringite. Other Al-containing minerals, such as crystalline aluminum oxides, e.g. corundum, do not form aluminates in aqueous environments due to their limited solubility. As a result, elemental analysis alone cannot provide reliable values ​​of available aluminates.

[0084] "Available aluminates" are those that can be synthesized in an alkaline aqueous environment using Al(OH)4 - The term is intended to encompass mineral phases and Al-containing compounds capable of producing calcium aluminate phases, such as C3A (Ca3Al2O6), which dissolve in alkaline aqueous environments to produce Al(OH)4 - and Ca 2+ For purposes of this invention, Al(OH)4 - The concentration of mineral phases and Al-containing compounds capable of forming Al(OH)4 per 100 g of cementitious binder i) - It is expressed as moles of

[0085] Common calcium aluminate mineral phases are considered to be the source of available aluminates, as opposed to crystalline aluminum oxide. The amount of available aluminates in a given cementitious binder can therefore be determined by a method that can distinguish the mineral phases that make up the cementitious binder. A useful method for this purpose is the Rietveld refinement of X-ray diffraction (XRD) powder patterns. This software technique is used to refine various parameters, including lattice parameters, peak positions, intensities and shapes. This allows the calculation of theoretical diffraction patterns. If the calculated diffraction patterns are nearly identical to the data of the test sample, precise quantitative information regarding the mineral phases involved can be determined.

[0086] Generally, Al(OH)4 in an alkaline aqueous environment - The calcium aluminate mineral phases capable of producing are tricalcium aluminate (C3A), monocalcium aluminate (CA), mayenite (C12A7), grossite (CA2), Q phase (C20A13M3S3) or tetracalcium aluminoferrite (C4AF). In practice, when the cementitious binder i) is Portland cement, it is generally sufficient to evaluate only the following mineral phases: tricalcium aluminate (C3A), monocalcium aluminate (CA), mayenite (C12A7) and tetracalcium aluminoferrite (C4AF), in particular tricalcium aluminate (C3A) and tetracalcium aluminoferrite (C4AF).

[0087] Alternatively, the amount of available aluminate can be obtained by determining the total amount of Al from the elemental composition of the cementitious binder i) by, for example, XRF, and subtracting therefrom the amount of crystalline aluminum compounds that cannot form available aluminates, as determined by XRD and Rietveld refinement. This method also takes into account amorphous soluble aluminum compounds that can form available aluminates. Such crystalline aluminum compounds that cannot form available aluminates include compounds of the melilite family, such as gehlenite (C2AS), compounds of the spinel family, such as spinel (MA), mullite (Al2Al 2+2x S 2-2x O 10-x ) and corundum (Al2O3).

[0088] In one embodiment, the present invention utilizes a cementitious binder containing 0.05-0.2 mol of available aluminate from a calcium aluminate mineral phase, as determined, for example, by XRD analysis.

[0089] Alternatively, an external aluminate source ii) can be added if the cementitious binder i) inherently contains an insufficient concentration of available aluminate per 100 g of cementitious binder i).Thus, in some embodiments, the construction composition contains an external aluminate source ii).

[0090] The external aluminate source ii) provides the available aluminate as defined above. Preferably, the external aluminate source ii) is selected from calcium-free aluminate sources, such as aluminium(III) salts, aluminium(III) complexes, crystalline aluminium hydroxide, amorphous aluminium hydroxide; and calcium-containing aluminate sources, such as high alumina cements, sulphoaluminate cements or synthetic calcium aluminate mineral phases.

[0091] Useful aluminum(III) salts are readily synthesized in alkaline aqueous environments using the formula Al(OH)4 -Suitable aluminum(III) salts include, but are not limited to, aluminum halides, such as aluminum(III) chloride, and their corresponding hydrates, amorphous aluminum oxide, aluminum hydroxide, or mixed forms thereof, aluminum sulfate or sulfate-containing aluminum salts, such as potassium alum, and their corresponding hydrates, aluminum nitrate, aluminum nitrite, and their corresponding hydrates, aluminum complexes, such as aluminum triformate, aluminum triacetate, aluminum diacetate, and aluminum monoacetate, aluminum-containing metal-organic frameworks, such as aluminum fumarate, for example, Basolite™ A520, and M(II) aluminum oxohydrates, such as hydrogarnet. Aluminum(III) hydroxide may be crystalline or amorphous. Preferably, amorphous aluminum hydroxide is used.

[0092] High aluminate cement means a cement containing a high concentration, for example at least 30% by weight, of calcium aluminate phases. More precisely, said mineralogical phases of aluminate type include tricalcium aluminate (C3A), monocalcium aluminate (CA), mayenite (C12A7), tetracalcium aluminoferrite (C4AF), or some combination of these phases.

[0093] Sulfoaluminate cements typically have an eelimite content (chemical formula 4CaO·3Al2O3·SO3 or C4A3$ in cement notation) of more than 15% by weight.

[0094] A suitable synthetic calcium aluminate mineral phase includes amorphous mayenite (C12A7).

[0095] The construction composition comprises a sulfate source iii). The sulfate source is a compound capable of providing sulfate ions in an alkaline aqueous environment. Generally, the sulfate source has a concentration of at least 0.6 mmol g L at a temperature of 30° C.-1 The water solubility of the sulfate source is suitably determined in water with a starting pH value of 7.

[0096] In an embodiment, the molar ratio of total available aluminates to sulfates is in the range of 0.4 to 2.0, preferably 0.57 to 0.8, in particular about 0.67, i.e. the mixing ratio in the composition is adjusted so that the highest possible proportion of ettringite is formed from the available aluminates.

[0097] As mentioned above, commercially available Portland cement typically contains small amounts of sulfate sources. If the endogenous amount of sulfate is unknown, it can be determined by methods well known to those skilled in the art, such as elemental analysis by XRF. The sulfate sources commonly used in cement manufacture, alkaline earth metal sulfates, alkali metal sulfates, or mixed forms thereof, such as gypsum, hemihydrate, anhydrite, alkanite, thenardite, syngenite, langbeinite, are typically crystalline, so the amount can also be determined by XRD. The calculation of the molar ratio of total available aluminate to sulfate takes into account both the endogenous amount of sulfate source and any added external sulfate source.

[0098] Generally, the external sulfate source can be selected from calcium sulfate dihydrate, anhydrite, α- and β-hemihydrate, i.e., α-bassanite and β-bassanite, or mixtures thereof. Preferably, the calcium sulfate source is α-bassanite and / or β-bassanite. Other sulfate sources are alkali metal sulfates, such as potassium sulfate or sodium sulfate.

[0099] It is envisioned that the additive may function as a source of both aluminate and sulfate, such as aluminum sulfate 16-hydrate or aluminum sulfate 18-hydrate.

[0100] Preferably, the external sulfate source iii) is a calcium sulfate source. The calcium sulfate source is generally present in an amount of 3-20% by weight, preferably 10-15% by weight, relative to the amount of cementitious binder i).

[0101] In one embodiment, the construction composition further comprises at least one of a latent hydraulic binder, a pozzolanic binder, and a filler material.

[0102] For the purposes of the present invention, a "latent hydraulic binder" is preferably a binder with a molar ratio (CaO+MgO):SiO2 of 0.8 to 2.5, in particular 1.0 to 2.0. Generally, the abovementioned latent hydraulic binders can be selected from industrial and / or synthetic slags, in particular blast furnace slags, electrothermal phosphorus slags, steel slags and mixtures thereof. A "pozzolanic binder" can generally be selected from amorphous silica, preferably precipitated silica, fumed silica and microsilica, ground glass, metakaolin, aluminosilicates, fly ash, preferably lignite fly ash and anthracite fly ash, natural pozzolans, such as tuff, trass and volcanic ash, calcined clay, calcined shale, rice husk ash, natural and synthetic zeolites, and mixtures thereof.

[0103] The slag may be industrial slag, i.e., waste from an industrial process, or synthetic slag, the latter of which may be advantageous since industrial slag is not always available in consistent quantities and quality.

[0104] Blast furnace slag (BFS) is a waste product of the glass furnace process. Other materials are granulated blast furnace slag (GBFS) and ground granulated blast furnace slag (GGBFS), which is finely ground granulated blast furnace slag. Ground granulated blast furnace slag differs in terms of fineness of grinding and particle size distribution depending on its origin and processing method, where the fineness of grinding influences the reactivity. The Blaine value is used as a parameter of fineness of grinding and is typically between 200 and 1000 m. 2 kg -1 , preferably 300 to 500 m 2 kg -1Finer grinding results in higher reactivity.

[0105] However, for purposes of this invention, the expression "blast furnace slag" is intended to include material obtained from all levels of processing, grinding and qualities mentioned (i.e., BFS, GBFS and GGBFS). Blast furnace slag generally contains 30-45 wt.% CaO, about 4-17 wt.% MgO, about 30-45 wt.% SiO2 and about 5-15 wt.% Al2O3, typically about 40 wt.% CaO, about 10 wt.% MgO, about 35 wt.% SiO2 and about 12 wt.% Al2O3.

[0106] Electrochemical phosphorus slag is a waste product of electrochemical phosphorus production. It is less reactive than blast furnace slag and contains about 45-50% by weight CaO, about 0.5-3% by weight MgO, about 38-43% by weight SiO2, about 2-5% by weight Al2O3 and about 0.2-3% by weight Fe2O3, as well as fluorides and phosphates. Steelmaking slag is a waste product of various iron and steel making processes with widely different compositions.

[0107] Amorphous silica is preferably X-ray amorphous silica, that is, silica that does not show crystallinity by powder diffraction.The content of SiO2 in the amorphous silica of the present invention is advantageously at least 80% by weight, preferably at least 90% by weight.Precipitated silica is obtained on an industrial scale by a precipitation process starting from water glass.Precipitated silica from some manufacturing processes is also called silica gel.

[0108] Fumed silica is produced by the reaction of chlorosilanes, such as silicon tetrachloride, in a hydrogen / oxygen flame. Fumed silica is produced at temperatures between 50 and 600 m 2 g -1 It is an amorphous SiO2 powder with a particle size of 5 to 50 nm and a specific surface area of ​​100 nm.

[0109] Microsilica is a by-product of silicon or ferrosilicon production and also consists mainly of amorphous SiO2 powder. The particles have a diameter of about 0.1 μm. The specific surface area is 15-30 m2 g -1 That's about it.

[0110] Metakaolin is produced by dehydrating kaolin. At 100-200 °C, kaolin releases physically bound water, while at 500-800 °C, dehydroxylation occurs and the lattice structure collapses to form metakaolin (Al2Si2O7). Pure metakaolin therefore contains about 54% SiO2 and about 46% Al2O3 by weight.

[0111] Fly ash is generated during the combustion of coal, especially in power plants: Class C fly ash (brown coal fly ash) contains about 10% by weight of CaO according to WO 08 / 012438, while Class F fly ash (anthracite fly ash) contains less than 8% by weight, preferably less than 4% by weight, typically about 2% by weight of CaO.

[0112] For purposes of the present invention, a "filler material" may be, for example, silica, quartz, sand, crushed marble, glass spheres, granite, basalt, limestone, sandstone, calcite, marble, serpentine, travertine, dolomite, feldspar, gneiss, alluvial sand, any other durable aggregate and mixtures thereof. In particular, the filler does not function as a binder.

[0113] The invention also relates to the construction composition according to the invention in freshly mixed form, i.e. comprising water. Preferably, the ratio of water to cementitious binder i) is in the range of 0.2 to 3. In industrial practice, the ratio of water to cementitious binder depends on the application of the cementitious system. Some applications, such as backfilling of mines, require a high fluidity of the cement paste and require a ratio of water to cementitious binder of up to 3. For other applications, the ratio of water to cementitious binder is in the range of 0.2 to 0.7.

[0114] The freshly mixed construction composition may be, for example, concrete, mortar or grout.

[0115] The term "mortar" or "grout" refers to a cement paste with the addition of fine aggregates, i.e. aggregates with diameters between 150 μm and 5 mm (e.g. sand), and optionally extra-fine aggregates. Grout is a mixture of low enough viscosity to fill voids or gaps. Mortar has a high enough viscosity to support not only its own weight but also the weight of the masonry placed on it. The term "concrete" refers to mortar with the addition of coarse aggregates, i.e. aggregates with diameters greater than 5 mm.

[0116] The building composition can be provided as a dry mix, to which water is added on-site to obtain a freshly mixed building composition, or alternatively, the building composition can be provided as a premixed or freshly mixed composition.

[0117] The freshly mixed aqueous construction composition is obtained by mixing a powdered component C containing the cementitious binder i) and the sulfate source iii) with a liquid aqueous component W, components iv-a) and iv-b) being contained in one or both of components C and W. The polyol iv-c) and optionally the dispersant iv-d) are preferably contained in component W. The optional external aluminate source ii) is preferably contained in component C.

[0118] The order of addition of optional component v), i.e., at least one of the latent hydraulic binder, pozzolanic binder and filler material, depends primarily on the moisture content of component v). If component v) is supplied in essentially anhydrous form, it may be conveniently included in component C. Otherwise, and more typically, component v) is premixed with component W and component C is subsequently mixed in.

[0119] This mixing regime prevents the immediate formation of ettringite, which occurs when the cementitious binder i) is exposed to water without the simultaneous presence of components iv-a) and iv-b), which effectively control ettringite formation.

[0120] In a practical embodiment, components iv-a) and iv-b), polyol iv-c), and optionally dispersant iv-d) are dissolved in a portion of the mixing water and mixed with wet component v), e.g. sand. A premixed mix of cementitious binder i), sulfate source iii), optional external aluminate source ii), and optionally anhydrous component v), such as limestone, is then added to the mixture. The remaining water is then added to adjust the consistency.

[0121] Preferably, at least one of the latent hydraulic binder, the pozzolanic binder and the filler material v) has a viscosity of 500 to 1900 kg / m 2 of the freshly mixed construction composition. 3 , preferably 700 to 1700 kg / m 3 is present in an amount of

[0122] The construction compositions according to the invention are useful for applications such as the production of building materials, in particular concrete, e.g. in-situ concrete, finished concrete components, manufactured concrete components (MCP), precast concrete components, concrete products, cast concrete masonry, concrete bricks, cast-in-situ concrete, ready mixed concrete, air-cast concrete, shotcrete / mortar, concrete repair systems, 3D printed concrete / mortar, industrial cement flooring, one-component and two-component sealing slurries, slurries for ground or rock improvement and soil conditioning, screeds, filling and self-levelling compositions, e.g. joint fillers or self-levelling underlays, high performance concrete (HPC) and ultra high performance concrete (UHPC), Useful for sealed manufactured concrete slabs, building concrete, tile adhesives, renders, cementitious plasters, adhesives, sealants, cementitious coatings and paint systems, especially for tunnels, drainage ditches, screeds, mortars such as dry mortars, sag-resistant, flowable or self-levelling mortars, drainage mortars and concretes, or repair mortars, grouts such as joint grouts, non-shrink grouts, tile grouts, injection grouts, windmill grouts (wind turbine grouts), anchor grouts, flowable or self-levelling grouts, ETICS (External Insulation Composite Systems), EIFS grouts (External Insulation Finish Systems), swelling explosives, waterproofing membranes, or cementitious foams.

[0123] Working Example The invention is further illustrated by the accompanying figures and the following examples. [Brief description of the drawings]

[0124] [Figure 1] FIG. 1 shows a plot of photocurrent signal in mV versus application time of CaCl in a calcium aluminate precipitation test according to one embodiment of the present invention.

[0125] All weight percentages are understood as %bwoc, i.e. relative to the mass of the cementitious binder i).

[0126] method Calcium aluminate precipitation test For the calcium aluminate precipitation test, an automated titration module (Titrando 905, available from Metrohm) equipped with a high-performance pH electrode (iUnitrode with Pt1000, available from Metrohm) and a light sensor (Spectrosense 610 nm, available from Metrohm) was used. First, a solution of 400 mL of a 1 wt. % aqueous solution of the polyol under study and 20 mL of a 1 mol / L aqueous NaOH solution was equilibrated for 2 minutes in the automated titration module under stirring. Then, 50 mL of a 25 mmol / L aqueous NaAlO2 solution was added to it, followed by equilibration for another 2 minutes to obtain an essentially transparent test solution. In the next step, the test solution is titrated with a 0.5 mol / L aqueous CaCl2 solution applied at a constant rate of 2 mL / min. The temperature is kept constant at 20° C. throughout the experiment. The time elapsed until the inflection of the turbidity is recorded. For this purpose, the photocurrent signal in mV is plotted against the application time of the aqueous CaCl2 solution. From this plot, the starting point is determined as the intersection of the baseline tangent and the tangent to the curve after the curve is inflected.

[0127] Test procedure - Early strength development of mortar The mortar mixes were filled into respective steel mortar prisms (16 / 4 / 4 cm) and after 3 hours at a temperature of 20° C. and a relative humidity of 65% hardened mortar prisms were obtained. The hardened mortar prisms were demolded and the compressive strength (=comp. strength) was measured according to DIN EN 196-1. After 24 hours the mortar prisms were measured again.

[0128] Test Procedure - Setting Time The setting times were determined according to DIN EN 480 with a Vicat needle.

[0129] Reference Example: Calcium Aluminate Precipitation Inhibitory Properties of Polyols Various polyols were evaluated for their precipitation properties in a calcium aluminate precipitation test. The results are shown in the table below. For the control, 400 mL of a 1 wt. % aqueous solution of the polyol was replaced with 400 mL of double distilled water. The maximum calcium concentration before the onset of turbidity (Ca 2+ The titration end point, expressed as ), is calculated from the time elapsed to the starting point. FIG. 1 shows a plot of the photocurrent signal in mV against the time of application of CaCl2. Curve a) of FIG. 1 shows the result in the absence of polyol ("blank"). Curve b) of FIG. 1 shows the result of adding 1% triethanolamine. For curve b), a first tangent 1 and a second tangent 2, referred to as the "baseline tangent", are shown. From the baseline tangent 1 and the second tangent 2, the starting point in seconds can be determined as the intersection of the baseline tangent 1 and the second tangent 2.

[0130] [Table 1]

[0131] Preparation and evaluation of construction compositions Example 1: Mortar mix Mortar mixes 1-27 were prepared according to the basic recipe in Table 1 and further components were added as described in Table 2. Their early strength development was measured and the results are reported in Table 2. As cementitious binders Karlstadt CEM I 42.5 R (0.091 mol available total aluminate per 100 g) or Mergelstetten CEM I 52.5 R (0.082 mol available total aluminate per 100 g) or Burglengenfeld CEM I 52.5 R (0.075 mol total aluminate per 100 g) were used as indicated in Table 2.

[0132] [Table 2]

[0133] Mixing Procedure Crushed stone (2-5mm) was dried in a 70°C oven for 50 hours. Sand (0-4mm) was dried at 140°C for 68 hours. Afterwards, crushed stone and sand were stored at 20°C with 65% relative humidity for at least 2 days. Sodium gluconate and NaHCO3, 2.0% bwoc of glycerol, and 0.20% bwoc of polycarboxylate-based superplasticizer according to Table 2 were added to the total amount of mix water to obtain a liquid aqueous component. Subsequently, crushed stone, sand, cementitious binder, and anhydrite were added to a 5L Hobart mixer. The liquid aqueous components were added to it and the mixture was stirred at level 1 (107 rpm) for 2 minutes and at level 2 (198 rpm) for another 2 minutes to obtain a freshly mixed aqueous construction composition.

[0134] [Table 3-1] [Table 3-2]

[0135] Mixes 1-20 and 21-27 of the invention exhibit rapid strength development once setting begins, so the open time closely matches the setting time.

[0136] It is clear from Table 2 that the setting time increases with increasing amounts of carbonate source and sodium gluconate. Both carbonate and gluconate increase the setting time, but sodium gluconate has a stronger effect on the setting time compared to carbonate. The lower the aluminate content of the cement, the less reactive the cement is, and therefore less gluconate and carbonate is required for adequate setting time and retention of workability.

[0137] Example 2: High performance concrete for wall panels Various concrete mixes were prepared for casting the wall panels. The basic recipe is given in Table 3, and further ingredients were added according to Table 4.

[0138] [Table 4]

[0139] Comparative Examples X-1 and X-2 in Table 4 contain glyoxylic acid urea condensate as a retarder of the prior art. The table shows that the addition of sodium gluconate enhances the retardation effect. Comparative Examples X-3 and X-4 in Table 4 contain low molecular weight polycarboxylic acids (citric acid and phosphonobutane tricarboxylic acid glyoxylic acid) as retarders of the prior art. The table shows that the retardation effect is less pronounced than in the case of X-1 and X-2. The addition of sodium gluconate again leads to an extension of the setting time. Comparative Examples X-5 and X-6 in Table 4 contain polyacrylic acid as a retarder of the prior art. The table shows that the retardation effect is less pronounced than in the case of X-1 and X-2. The addition of sodium gluconate again leads to an extension of the setting time. Inventive Example X-7 shows a setting time comparable to that of Comparative Example X-2, while an increase in compressive strength after 3 hours is observed. Comparative Example X-8, in which the ratio of NaHCO3 to Na gluconate is outside the ratio range of 1.2-8.0, shows insufficient compressive strength after 3 hours.

[0140] [Table 5]

Claims

1. 1. A setting control composition for cementitious systems comprising: a) (a-1) accounts for at least 90% of the carboxyl groups of the following (a-1) and (a-2) based on the total number of carboxyl groups: (a-1) a hydroxymonocarboxylic acid or a salt thereof, and (a-2) optionally, a polycarboxylic acid having a carboxylic acid equivalent of 333 or less, which is calculated by dividing the molecular weight of the polycarboxylic acid by the number of carboxylic acid functional groups, or a salt thereof; b) in a weight ratio of b) to a) ranging from 1.2 to 20 (b-1) a borate source; (b-2) 0.1 g L at 25°C -1 a carbonate source selected from inorganic carbonates having a water solubility of at least At least one of the following: c) a polyol in a weight ratio of c) to a) ranging from 1.0 to 10.

1. A setting control composition comprising:

2. 2. The setting control composition according to claim 1, wherein (a-1) accounts for at least 95% of the carboxyl groups of (a-1) and (a-2) based on the total number of carboxyl groups of (a-1) and (a-2).

3. 3. The setting control composition of claim 1 or 2, wherein the inorganic carbonate is selected from sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, lithium carbonate and magnesium carbonate, and the organic carbonate is selected from ethylene carbonate, propylene carbonate and glycerol carbonate.

4. 400 mL of a 1% by weight aqueous solution of the polyol was mixed with 20 mL of a 1 mol / L NaOH aqueous solution and 25 mmol / L NaAlO 2 The test solution obtained by adding 50 mL of the aqueous solution was 0.5 mol / L CaCl 24. The setting control composition of claim 1, wherein the polyol inhibits calcium aluminate precipitation up to a calcium concentration of 75 ppm, preferably 90 ppm, in a calcium aluminate precipitation test by titration with an aqueous solution.

5. The polyol may be a monosaccharide, an oligosaccharide, a water-soluble polysaccharide, or a saccharide of the general formula (P-I): [Formula 1] [In the formula, X is [Case 2] where: R is -CH 2 CH 3 , -CH 2 OH, -NH 2 and n is an integer from 1 to 4, m is an integer from 1 to 8. or a dimer or trimer of a compound of general formula (PI).

6. The set control composition of claim 1 further comprising a dispersant d).

7. The dispersant is - comb polymers having a carbon-containing backbone with pendant cement anchoring groups and polyether side chains attached; - a non-ionic comb polymer having a carbon-containing backbone with pendant hydrolyzable groups and polyether side chains attached, the hydrolyzable groups releasing cement anchoring groups upon hydrolysis; - Al, in which the polyvalent metal cations are present in superstoichiometric amounts, calculated as cation equivalents, based on the sum of the negative and anion-forming groups of the polymeric dispersant. 3+ , Fe 3+ Or Fe 2+ colloidal dispersion preparations of polyvalent metal cations such as dimethylformamide, ... sulfonated melamine-formaldehyde condensates, - lignosulfonates, sulfonated ketone-formaldehyde condensates, sulfonated naphthalene-formaldehyde condensates, - a phosphonate-containing dispersant, which preferably comprises at least one polyalkylene glycol unit, and - Mixtures thereof The setting control composition of claim 6, wherein the setting control composition is selected from the group consisting of:

8. 1. A construction composition comprising: i) a cementitious binder comprising one or more calcium silicate mineral phases and one or more calcium aluminate mineral phases; ii) optionally, an external aluminate source; iii) Optionally, an external sulfate source. Including, The construction composition comprises: iv) iv-a) (a-1) accounts for at least 90% of the carboxyl groups of the following (a-1) and (a-2) based on the total number of carboxyl groups: (a-1) a hydroxymonocarboxylic acid or a salt thereof, and (a-2) optionally, a polycarboxylic acid having a carboxylic acid equivalent of 333 or less, which is calculated by dividing the molecular weight of the polycarboxylic acid by the number of carboxylic acid functional groups, or a salt thereof; iv-b) in a weight ratio of iv-b) to iv-a) ranging from 1.2 to 20 (b-1) a borate source; (b-2) 0.1 g L at 25°C -1 a carbonate source selected from inorganic carbonates having a water solubility of at least At least one of the following: iv-c) a polyol in a weight ratio of iv-c) to iv-a) ranging from 1.0 to 10. A setting control composition comprising The construction composition further comprising:

9. The construction composition comprises, per 100 g of cementitious binder i), the calcium aluminate mineral phase plus Al(OH) from any of the external aluminate sources. 4 - 9. The construction composition according to claim 8, which contains from 0.05 to 0.2 mol of total available aluminates, calculated as: and has a molar ratio of total available aluminates to sulfates of from 0.4 to 2.

0.

10. relative to the amount of cementitious binder i), iv-a) in an amount ranging from 0.2 to 2% by weight, iv-b) in an amount ranging from 0.8 to 2.5% by weight, iv-c) in an amount ranging from 0.2 to 2.5% by weight; 10. The construction composition of claim 8 or 9, comprising:

11. 11. The construction composition according to any one of claims 8 to 10, wherein the calcium silicate mineral phase and the calcium aluminate mineral phase account for at least 90% by weight of the cementitious binder i) and the calcium silicate mineral phase accounts for at least 60% by weight of the cementitious binder i).

12. The construction composition comprises: v) at least one of a latent hydraulic binder, a pozzolanic binder, and a filler material; 12. The construction composition of claim 8, further comprising:

13. 13. A construction composition according to any one of claims 8 to 12, wherein the external aluminate source ii) is selected from calcium-free aluminate sources, such as aluminium(III) salts, aluminium(III) complexes, crystalline aluminium hydroxide, amorphous aluminium hydroxide; and calcium-containing aluminate sources, such as high alumina cements, sulphoaluminate cements or synthetic calcium aluminate mineral phases.

14. 14. A construction composition according to any one of claims 8 to 13, wherein the external sulfate source iii) is a calcium sulfate source.

15. A construction composition according to any one of claims 8 to 14, in freshly mixed form, having a ratio of water to cementitious binder i) ranging from 0.2 to 3.

Citation Information

Cited By

  • Additive, cement-based composition and use thereof

    JP2026008654A