Highly water-absorbent resin composition and method for producing same

The use of a specific additive in the pulverization process addresses agglomeration issues in superabsorbent resin production, enhancing water absorption capacity and rate while reducing fine powder generation.

JP2024536319AActive Publication Date: 2024-10-04LG CHEM LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024520044
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-27
Filing Date
2022-10-28
Publication Date
2024-10-04
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Conventional methods for producing superabsorbent resins face challenges in the pulverization process due to agglomeration of hydrogel polymers, leading to increased generation of fine powder and reduced efficiency in water absorption performance and rate.

Method used

A method involving the use of a specific additive with a chemical structure represented by Formula 1, applied during the pulverization process to suppress agglomeration of hydrogel polymers, enhancing the pulverization properties and improving water absorption performance and rate.

Benefits of technology

The method effectively reduces fine powder generation and enhances the water absorption capacity and rate of superabsorbent resins by controlling agglomeration, resulting in improved physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536319000001_ABST
    Figure 2024536319000001_ABST
Patent Text Reader

Abstract

The present invention relates to a superabsorbent polymer composition and a method for producing the same, and more specifically, to a method for producing a superabsorbent polymer composition which contains an additive having a specific structure and can suppress aggregation of a hydrogel polymer during a pulverization step and improve the pulverization step performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0147025 dated October 29, 2021 and Korean Patent Application No. 10-2022-0140642 dated October 27, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a superabsorbent polymer composition and a method for producing the same, and more specifically, to a method for producing a superabsorbent polymer composition which contains an additive having a specific structure and can suppress aggregation of a hydrogel polymer during a pulverization step and improve the pulverization step performance. [Background technology]

[0003] Super absorbent polymer (SAP) is a synthetic polymeric substance that has the ability to absorb 500 to 1,000 times its own weight in water, and each developer has a different name for it, such as SAM (Super Absorbency Material), AGM (Absorbent Gel Material), etc. Such super absorbent polymers first came into practical use as sanitary products, and are now widely used as soil water retention agents for horticulture, water stoppers for civil engineering and construction, seedling sheets, freshness preserving agents in the food distribution field, and materials for packs.

[0004] Such superabsorbent polymers are widely used in the field of sanitary materials, such as diapers and sanitary napkins. In the sanitary materials, the superabsorbent polymers are generally contained in a dispersed state in the pulp. However, in recent years, efforts have been made to provide sanitary materials, such as diapers, with thinner thicknesses, and as part of these efforts, the pulp content has been reduced, or even going a step further, the development of so-called pulpless diapers, which do not use pulp at all, has been actively promoted.

[0005] In this way, in the case of sanitary materials in which the pulp content is reduced or no pulp is used, the superabsorbent polymer is contained at a relatively high ratio, and the superabsorbent polymer particles are inevitably contained in multiple layers in the sanitary materials. In order for the overall superabsorbent polymer particles contained in multiple layers in this way to more efficiently absorb a large amount of liquid such as urine, the superabsorbent polymer basically needs to exhibit not only high water absorption performance but also a fast water absorption speed.

[0006] On the other hand, such a superabsorbent resin is generally manufactured by a process of polymerizing a monomer to produce a hydrogel polymer containing a large amount of water, and then crushing the hydrogel polymer into resin particles having a desired particle size after coarsely crushing and drying. In particular, in the process of coarsely crushing the hydrogel polymer, the coarsely crushed hydrogel polymer aggregates or clumps together, which makes it difficult to crush the polymer.

[0007] As a result, in addition to improving the water retention capacity (CRC), which is a physical property that indicates the basic water absorption and water retention of superabsorbent polymers, and the absorbent capacity under pressure (AUP), which indicates the ability to retain absorbed liquid even under external pressure, there is a continuing demand for the development of technology that can increase the water absorption speed of superabsorbent polymers and technology that can improve the grinding process during processing. Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, the present invention relates to a method for producing a superabsorbent resin composition which contains an additive having a specific structure and which is capable of suppressing aggregation of a hydrogel polymer during a pulverization step and improving the pulverization processability. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides Superabsorbent resin particles containing a crosslinked polymer of a water-soluble ethylenically unsaturated monomer having an acidic group and an internal crosslinking agent; and A superabsorbent polymer composition is provided, comprising an additive represented by the following chemical formula 1:

[0010] [ka]

[0011] In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl,

[0012] [ka]

[0013] where one or more of these is a carbonyl or

[0014] [ka]

[0015] wherein m1, m2, and m3 each independently represent an integer from 1 to 8;

[0016] [ka]

[0017] are each linked to adjacent oxygen atoms,

[0018] [ka]

[0019] is the adjacent R 1 , R 2 and R 3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

[0020] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: Step 1: cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a polymer; neutralizing at least a portion of the acidic groups of the polymer (Step 2); (Step 3) preparing base resin particles by atomizing the polymer in the presence of an additive represented by the following formula 1: drying the base resin particles (Step 4); A method for producing a superabsorbent polymer composition is provided, comprising:

[0021] [ka]

[0022] In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl,

[0023] [ka]

[0024] where one or more of these is a carbonyl or

[0025] [ka]

[0026] wherein m1, m2, and m3 each independently represent an integer from 1 to 8;

[0027] [ka]

[0028] are each linked to adjacent oxygen atoms,

[0029] [ka]

[0030] is the adjacent R 1 , R 2 and R 3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9. Effect of the Invention

[0031] According to the superabsorbent resin composition and the method for producing the same of the present invention, the additive having a specific structure is added during the pulverization process of the hydrous gel polymer to suppress aggregation of the hydrous gel polymer particles, thereby making it possible to improve the pulverization processability, and thereby to improve the water absorption performance and water absorption speed of the superabsorbent resin. [Brief description of the drawings]

[0032] [Figure 1] 1 is a flowchart relating to a conventional method for producing a highly water-absorbent resin. [Diagram 2] 1 is a photograph showing examples of evaluation items in evaluating particle aggregation properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" and the like are intended to specify the presence of an implemented feature, step, component, or combination thereof, and should be understood not to preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.

[0034] Although the present invention can be modified in various ways and has various forms, specific embodiments are exemplified and described in detail below. However, it is not intended to limit the present invention to the specific disclosed embodiments, and it should be understood that the present invention includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0035] Hereinafter, the method for producing a superabsorbent polymer and the superabsorbent polymer will be described in more detail with reference to specific embodiments of the present invention.

[0036] Prior to this, the terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention, and the singular forms used herein include the plural forms unless the language clearly indicates otherwise.

[0037] The term "polymer" or "polymeric polymer" used in the present specification means a state in which a water-soluble ethylenically unsaturated monomer is polymerized, and can include all water content ranges or particle size ranges. Among the above polymers, a polymer having a water content (water content) of about 40% by weight or more in a state after polymerization and before drying can be called a hydrogel polymer, and particles of such a hydrogel polymer that have been crushed and dried can be called a crosslinked polymer.

[0038] In addition, the term "superabsorbent resin particles" refers to a particulate material that includes a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer that contains acidic groups and at least a portion of the acidic groups have been neutralized, and crosslinking the polymer with an internal crosslinking agent.

[0039] Furthermore, the term "superabsorbent polymer" refers to a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer containing acidic groups and at least a portion of the acidic groups being neutralized, or a powder-like base resin consisting of superabsorbent polymer particles obtained by pulverizing the crosslinked polymer, depending on the context, or is used to encompass all of the crosslinked polymers or base resins that have been subjected to additional processes, such as surface crosslinking, fine powder regranulation, drying, pulverization, classification, etc., to be in a state suitable for commercialization. Therefore, the term "superabsorbent polymer composition" is interpreted as including a composition containing a superabsorbent polymer, i.e., a plurality of superabsorbent polymer particles.

[0040] The term "fine powder" refers to superabsorbent resin particles having a particle size of less than 150 μm. The particle size of such resin particles can be measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP220.3 method.

[0041] The term "chopping" is also used to distinguish between cutting the hydrogel polymer into millimeter-sized pieces to increase drying efficiency and grinding to micrometer or regular particle levels.

[0042] Furthermore, the term "micronizing" refers to pulverizing a hydrogel polymer into particles having a particle size of several tens to several hundreds of micrometers, and is used to distinguish it from "chopping".

[0043] Meanwhile, conventional superabsorbent resins are manufactured by cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer, drying the hydrogel polymer thus formed, and then pulverizing it to a desired particle size. In this case, a chopping process is usually performed before the drying process to cut the hydrogel polymer into particles of several millimeters in size in order to facilitate drying of the hydrogel polymer and to increase the efficiency of the pulverization process. However, in this chopping process, the hydrogel polymer is not pulverized to the micro-sized particle level due to the stickiness of the hydrogel polymer, and becomes an aggregated gel. When such an aggregated gel-like hydrogel polymer is dried, a plate-shaped dried body is formed, and in order to pulverize it to the micro-sized particle level, a multi-stage pulverization process must be performed, which causes a problem of generating a lot of fine powder during the process.

[0044] Specifically, a flow chart of a conventional method for producing a superabsorbent polymer is shown in Fig. 1. Referring to Fig. 1, the conventional superabsorbent polymer has been produced through the following steps.

[0045] (neutralizing) neutralizing at least a portion of the acidic groups of the water-soluble ethylenically unsaturated monomer; (Polymerization) A step of cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer; (chopping) chopping the hydrogel polymer; (Drying) drying the chopped hydrogel polymer; and (Crushing / Classification) Crushing the dried polymer and classifying it into normal particles and fine powder;

[0046] As described above, the chopped hydrogel polymer has an aggregated gel shape of about 1 cm to 10 cm in size, and the chopped hydrogel polymer is stacked on a belt with a perforated plate at the bottom and dried by hot air supplied from the bottom or top. Since the polymer dried by the drying method has a plate shape rather than a granular shape, the crushing and classification step has been carried out by coarse crushing and classification so that the produced particles are normal particles, that is, particles having a particle size of 150 μm to 850 μm, and then fine crushing and classification again. Since the amount of fine powder separated in the final classification step in this manufacturing method is large, about 10 wt% to about 20 wt% of the total weight of the finally manufactured superabsorbent resin, the separated fine powder is mixed with an appropriate amount of water, regranulated, and then reused by feeding it into the chopping step or the pre-drying step.

[0047] However, in order to reuse such fine powder, problems have arisen such as an increase in the load on the equipment and / or the amount of energy used when the regranulated fine powder mixed with water is reintroduced into a grinding or drying process, and the fine powder remaining unclassified has led to a deterioration in the physical properties of the superabsorbent polymer.

[0048] Therefore, the inventors realized that in conventional manufacturing methods, the amount of fine powder generated is greatly affected by the grinding process, and focused on the fact that by adding a surfactant in the chopping process (atomization process) to grind the material finer than before, while at the same time controlling aggregation to produce particles in the form of aggregated fine particles, the amount of fine powder generated during the manufacturing process can be significantly reduced.

[0049] On the other hand, when a surfactant is added to a neutralized hydrogel polymer, the surfactant penetrates into the hydrogel polymer rather than existing at the interface of the hydrogel polymer due to the high hydrophilicity of the neutralized hydrogel polymer, and thus the surfactant cannot perform its role properly.

[0050] As a result of extensive research to solve this problem, it has been found that, unlike in the conventional method of producing a superabsorbent resin, polymerization is first carried out in a state where the acidic groups of a water-soluble ethylenically unsaturated monomer are neutralized, to form a polymer, and the hydrogel polymer is atomized in the presence of a surfactant and then the acidic groups of the polymer are neutralized, or the acidic groups of the polymer are neutralized to form a hydrogel polymer, and then the hydrogel polymer is atomized in the presence of a surfactant, or the acidic groups present in the polymer are neutralized simultaneously with the atomization, whereby a large amount of the surfactant is present on the surface of the polymer, thereby reducing the high adhesiveness of the polymer and preventing the polymer from excessively agglomerating, and thereby fully fulfilling the role of adjusting the agglomeration state to a desired level.

[0051] As a result, the polymer is produced into secondary particles in the form of aggregates of primary particles, and the subsequent pulverization and drying processes are carried out under milder conditions, thereby significantly reducing the amount of fine powder generated during the process.

[0052] In addition, when a polymer is pulverized in the presence of an additive having a specific structure of Chemical Formula 1 as described above, the hydrophobic functional group moiety contained in the additive imparts hydrophobicity to the surface of the pulverized superabsorbent resin particles, reducing interparticle friction and increasing the apparent density of the superabsorbent resin, while the hydrophilic functional group moiety contained in the additive also binds to the superabsorbent resin particles, preventing a decrease in the surface tension of the resin. As a result, the superabsorbent resin produced by the above-mentioned production method has a higher apparent density value while exhibiting the same level of surface tension as a resin that does not use such an additive.

[0053] In addition, if polymerization is first carried out in an unneutralized state to form a polymer, and then the acidic groups present in the polymer are neutralized, it is possible to form a polymer with longer chains, and it is possible to achieve the effect of reducing the content of water-soluble components that exist in an uncrosslinked state due to incomplete crosslinking.

[0054] The water-soluble component has a property of being easily dissolved when the superabsorbent resin comes into contact with a liquid, so if the content of the water-soluble component is high, the dissolved water-soluble component remains on the surface of most of the superabsorbent resin, making the superabsorbent resin sticky and causing a decrease in liquid permeability. Therefore, in terms of liquid permeability, it is important to maintain the content of the water-soluble component low.

[0055] In summary, the present inventors have confirmed that when a polymer is pulverized by mixing an additive having a specific structure represented by the following chemical formula 1, aggregation between pulverized hydrogel polymer particles is suppressed and the pulverization processability is improved, and thus the present invention has been completed. In particular, the particles contained in the superabsorbent polymer composition produced by the above production method are characterized by exhibiting an improved water absorption rate compared to the case where the additive is not used.

[0056] [ka]

[0057] In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl,

[0058] [ka]

[0059] where one or more of these is a carbonyl or

[0060] [ka]

[0061] wherein m1, m2, and m3 each independently represent an integer from 1 to 8;

[0062] [ka]

[0063] are each linked to adjacent oxygen atoms,

[0064] [ka]

[0065] is the adjacent R 1 , R 2 and R 3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

[0066] Specifically, the additive represented by the following Chemical Formula 1 has both a hydrophobic functional group and a hydrophilic functional group. Meanwhile, the water-soluble ethylenically unsaturated monomer has an acidic group (-COOH) and / or a neutralized acidic group (-COOH). - ), the surface of the polymer produced by polymerization contains acidic groups (-COOH) that do not participate in the polymerization and / or neutralized acidic groups (-COO - ) is present in a large amount. Therefore, when the additive is mixed with the polymer, the hydrophilic functional group of the additive is adsorbed to at least a part of the hydrophilic portion present on the surface of the polymer, and the surface of the polymer to which the additive is adsorbed exhibits hydrophobicity due to the hydrophobic functional group located at the other end of the additive. This makes it possible to suppress aggregation between the pulverized hydrogel polymer particles.

[0067] Hereinafter, the superabsorbent resin composition of one embodiment will be specifically described with respect to each component.

[0068] (Super absorbent resin composition) According to one embodiment of the invention, there is provided a superabsorbent polymer composition comprising superabsorbent polymer particles comprising a crosslinked polymer of a water-soluble ethylenically unsaturated monomer having an acidic group and an internal crosslinking agent; and an additive represented by the following chemical formula 1:

[0069] [ka]

[0070] In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl,

[0071] [ka]

[0072] where one or more of these is a carbonyl or

[0073] [ka]

[0074] wherein m1, m2, and m3 each independently represent an integer from 1 to 8;

[0075] [ka]

[0076] are each linked to adjacent oxygen atoms,

[0077] [ka]

[0078] is the adjacent R 1 , R 2 and R3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

[0079] In one embodiment, the superabsorbent polymer composition includes superabsorbent polymer particles including a crosslinked polymer of a water-soluble ethylenically unsaturated monomer having an acidic group and an internal crosslinking agent, the crosslinked polymer being a polymer of the water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal crosslinking agent, and the crosslinked polymer has a three-dimensional network structure in which the main chain formed by polymerization of the monomer is crosslinked by the internal crosslinking agent.

[0080] In other words, the superabsorbent resin composition of one embodiment includes superabsorbent resin particles including a crosslinked polymer between a water-soluble ethylenically unsaturated monomer having an acidic group and an internal crosslinking agent. In this way, when the crosslinked polymer has a three-dimensional network structure in which the main chain formed by polymerization of the monomer is crosslinked by the internal crosslinking agent, the water retention capacity and the pressurized water absorption capacity, which are various physical properties of the superabsorbent resin, can be significantly improved compared to when the crosslinked polymer has a two-dimensional linear structure that is not additionally crosslinked by the internal crosslinking agent.

[0081] The water-soluble ethylenically unsaturated monomer may be any monomer commonly used in the manufacture of superabsorbent resins. As a non-limiting example, the water-soluble ethylenically unsaturated monomer may be a compound represented by the following formula 2:

[0082] [Chemical formula 2] R-COOM'

[0083] In the above Chemical Formula 2, R is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M' is a hydrogen atom, a monovalent or divalent metal, an ammonium group or an organic amine salt.

[0084] Preferably, the monomer may be one or more selected from the group consisting of (meth)acrylic acid, and monovalent (alkali) metal salts, divalent metal salts, ammonium salts and organic amine salts of these acids.

[0085] In this way, when (meth)acrylic acid and / or its salt is used as the water-soluble ethylenically unsaturated monomer, it is advantageous to obtain a highly water-absorbent resin with improved water absorption. Other examples of the monomer that can be used include maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid or 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, (N,N)-dimethylaminoethyl (meth)acrylate, (N,N)-dimethylaminopropyl (meth)acrylamide, etc.

[0086] Here, the water-soluble ethylenically unsaturated monomer has an acidic group, and at least a portion of the acidic group is neutralized by a neutralizing agent in a neutralization step described below. At this time, as the neutralizing agent, a basic substance capable of neutralizing the acidic group, such as sodium hydroxide, potassium hydroxide, ammonium hydroxide, etc., is used, which will be described in more detail in the preparation method section described below.

[0087] In addition, the term "internal crosslinking agent" used in this specification is a term used to distinguish it from a surface crosslinking agent for crosslinking the surface of superabsorbent resin particles described later, and plays a role in crosslinking and polymerizing the unsaturated bonds of the water-soluble ethylenically unsaturated monomer described above. The crosslinking in this step is performed without distinction between the surface and the inside, but when the surface crosslinking process of the superabsorbent resin particles described later is performed, the particle surface of the finally produced superabsorbent resin has a structure crosslinked by the surface crosslinking agent, and the inside has a structure crosslinked by the internal crosslinking agent.

[0088] The internal crosslinking agent may be any compound that allows the introduction of crosslinking bonds during polymerization of the water-soluble ethylenically unsaturated monomer. Non-limiting examples of the internal crosslinking agent include N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, and hexanediol di(meth)acrylate. Polyfunctional crosslinking agents such as triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, pentaerythritol triallyl ether, ethylene glycol diglycidyl ether, propylene glycol, glycerin, or ethylene carbonate may be used alone or in combination, but are not limited thereto. Of these, pentaerythritol triallyl ether is preferably used.

[0089] The crosslinking polymerization of the water-soluble ethylenically unsaturated monomer in the presence of such an internal crosslinking agent is carried out by thermal polymerization, photopolymerization or hybrid polymerization in the presence of a polymerization initiator and, if necessary, a thickener, a plasticizer, a storage stabilizer, an antioxidant, etc., the details of which will be described later.

[0090] The highly water-absorbent resin particles may have a particle size of about 150 to about 850 μm, and the particle size may be measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP220.3 method.

[0091] The superabsorbent polymer composition further includes an additive represented by Chemical Formula 1. The additive is added so that the chopping step can be easily performed without agglomeration by mixing with the polymer as described above.

[0092] The additive represented by the formula 1 is a non-ionic surfactant and has excellent surface adsorption performance due to hydrogen bonding with unneutralized polymers, and is therefore suitable for achieving the desired aggregation control effect. On the other hand, in the case of an anionic surfactant that is not a non-ionic surfactant, NaOH, Na 2 SO 4 When mixed with a polymer neutralized with a neutralizing agent such as , it is adsorbed via the Na+ ions ionized to the carboxyl group substituents of the polymer, and when mixed with an unneutralized polymer, there is a problem that the adsorption efficiency for the polymer is relatively reduced due to competition with the anions of the carboxyl group substituents of the polymer.

[0093] Specifically, in the additive represented by the above chemical formula 1, the hydrophobic functional group is a terminal functional group R 1 , R 2 , R 3 The hydrophilic functional groups are the glycerol-derived moieties in the chain and the terminal hydroxyl groups (A n is a single bond and at the same time R nis hydrogen, n=1 to 3), but the glycerol-derived portion and the terminal hydroxyl group are hydrophilic functional groups that play a role in improving the adsorption performance to the polymer surface, thereby effectively suppressing the aggregation of the superabsorbent resin particles.

[0094] In the above formula 1, R 1 , R 2 , R 3 Each of the moieties (if not hydrogen) is independently a straight or branched chain alkyl having 6 to 18 carbon atoms, or a straight or branched chain alkenyl having 6 to 18 carbon atoms, where R 1 , R 2 , R 3 When the portion (if not hydrogen) is an alkyl or alkenyl having less than 6 carbon atoms, there is a problem that the chain length is too short to effectively control the aggregation of the milled particles. 1 , R 2 , R 3 If the moiety (if not hydrogen) is an alkyl or alkenyl having more than 18 carbon atoms, the mobility of the additive may be reduced and it may not be effectively mixed with the polymer, and the cost of the additive may increase, resulting in a high unit cost of the composition.

[0095] Preferably, R 1 , R 2 , R 3 is hydrogen or, if it is a straight or branched chain alkyl having 6 to 18 carbon atoms, it may be 2-methylhexyl, n-heptyl, 2-methylheptyl, n-octyl, n-nonyl, n-decanyl, n-undecanyl, n-dodecanyl, n-tridecanyl, n-tetradecanyl, n-pentadecanyl, n-hexadecanyl, n-heptadecanyl, or n-octadecanyl, or, if it is a straight or branched chain alkenyl having 6 to 18 carbon atoms, it may be 2-hexenyl, 2-heptenyl, 2-octenyl, 2-nonenyl, n-dekenyl, 2-undekenyl, 2-dodekenyl, 2-tridekenyl, 2-tetradekenyl, 2-pentadekenyl, 2-hexadekenyl, 2-heptadekenyl, or 2-octadekenyl.

[0096] The additive may be selected from compounds represented by the following formulas 1-1 to 1-14:

[0097] [ka] [ka] [ka]

[0098] The additive is contained in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the total content of the additives relative to the monomer in the composition is too low, the additives may have little effect of controlling aggregation, and the composition may contain superabsorbent resin particles that are not pulverized to a desired particle size. If the total content of the additives is too high, the balance between the water retention capacity and the pressurized water absorption capacity, which are various physical properties of the superabsorbent resin, may be reduced.

[0099] The content of the additive in the superabsorbent polymer composition can be measured by first adding 1 g of the superabsorbent polymer composition to 1 ml of distilled water, mixing thoroughly for 1 hour until swelling occurs, filtering the mixture to extract only the solution portion, and then performing HPLC analysis to analyze the content of the additive dissolved in the solution portion.

[0100] More specifically, the additive is included in an amount of 0.01 parts by weight or more, 0.02 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.5 parts by weight or more, and 10 parts by weight or less, 8 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer.

[0101] Meanwhile, at least a part of the additive may be present on the surface of the superabsorbent resin particles. Here, the meaning of "at least a part of the additive is present on the surface of the superabsorbent resin particles" means that at least a part of the additive is adsorbed or bonded to the surface of the superabsorbent resin particles. Specifically, the additives may be physically or chemically adsorbed on the surface of the superabsorbent resin. More specifically, the hydrophilic functional groups of the additives may be physically adsorbed to the hydrophilic portion of the surface of the superabsorbent resin by intermolecular forces such as dipole-dipole interaction. In this way, the hydrophilic portion of each of the additives may be physically adsorbed on the surface of the superabsorbent resin particles to surround the surface, and the hydrophobic portion of each of the additives may not be adsorbed on the surface of the resin particles, and each additive may be coated on the surface of the resin particles in the form of a kind of micelle structure.

[0102] Therefore, when at least a portion of the additive is present on the surface of the superabsorbent resin particles, the aggregation phenomenon between particles pulverized during the preparation process of the superabsorbent resin composition can be more effectively suppressed than when the entire additive of Formula 1 is present inside the superabsorbent resin particles, specifically, inside the crosslinked polymer.

[0103] Furthermore, since at least a portion of the additive is present on the surface of the superabsorbent resin particles, the superabsorbent resin composition containing the additive can have an improved water absorption rate compared to a composition that does not contain such an additive.

[0104] On the other hand, when the superabsorbent resin composition does not further include a surface cross-linked layer described later, it does not include any other hydrophilic additives other than the plurality of superabsorbent resin particles, the additive, and the hydrolysate of the additive produced by hydrolysis of the additive during the production process of the superabsorbent resin.

[0105] Specifically, the superabsorbent polymer composition of one embodiment does not contain a compound having many hydroxyl-containing glucose units in the molecule, such as microcrystalline cellulose. For example, when the superabsorbent polymer composition contains microcrystalline cellulose having an average particle size of 1 to 10 μm, such as AVICEL (registered trademark) PH-101, available from FMC Corporation and represented by the following chemical formula 3, the aggregation between the superabsorbent polymer particles is not suppressed by the many hydroxyl groups, and the effect of the above-mentioned additives may not be effectively exhibited.

[0106] [ka]

[0107] In addition, the superabsorbent polymer composition of one embodiment does not contain a hydrophilic additive such as polyethylene glycol, polypropylene glycol, poly(ethylene glycol)-poly(propylene glycol) copolymer, polyoxyethylene lauryl ether carboxylic acid, sodium polyoxyethylene lauryl ether carboxylate, lauryl sulfate, or sodium lauryl sulfate. Such additives are not sufficiently adsorbed on the surface of the crosslinked polymer, and there is a problem that the aggregation between superabsorbent polymer particles is not effectively suppressed. Therefore, when the superabsorbent polymer composition contains such a hydrophilic additive instead of the additive of Chemical Formula 1, the aggregation between particles is not suppressed after the crosslinked polymer is pulverized, and the superabsorbent polymer composition contains a large amount of fine powder and exhibits low water retention capacity and low apparent density.

[0108] Meanwhile, the superabsorbent resin composition may further include a surface cross-linked layer formed by additionally cross-linking the cross-linked polymer via a surface cross-linking agent on at least a part of the surface of the superabsorbent resin particle, in order to increase the surface cross-linking density of the superabsorbent resin particle. When the superabsorbent resin particle further includes a surface cross-linked layer as described above, the particle has a structure in which the cross-linking density is higher on the outside than on the inside.

[0109] The surface cross-linking agent can be any surface cross-linking agent that has been used in the manufacture of superabsorbent resins without any particular limitation. For example, the surface cross-linking agent can include one or more polyols selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,2-hexanediol, 1,3-hexanediol, 2-methyl-1,3-propanediol, 2,5-hexanediol, 2-methyl-1,3-pentanediol, 2-methyl-2,4-pentanediol, tripropylene glycol, and glycerol; one or more carbonate-based compounds selected from the group consisting of ethylene carbonate, propylene carbonate, and glycerol carbonate; epoxy compounds such as ethylene glycol diglycidyl ether; oxazoline compounds such as oxazolidinone; polyamine compounds; mono-, di-, or polyoxazolidinone compounds; or cyclic urea compounds; etc.

[0110] Specifically, one or more, two or more, or three or more of the above-mentioned surface cross-linking agents can be used as the surface cross-linking agent. For example, propylene glycol, ethylene carbonate, and propylene carbonate can be used.

[0111] The superabsorbent polymer composition may have a water absorption rate (vortex time) of 30 seconds or less, 27 seconds or less, 25 seconds or less, 20 seconds or less, 15 seconds or less, or 12 seconds or less, measured by a vortex method at 24.0°C. The smaller the water absorption rate, the better. The lower limit of the water absorption rate is theoretically 0 seconds, but may be, for example, 5 seconds or more, 8 seconds or more, or 10 seconds or more. The method for measuring the water absorption rate of the superabsorbent polymer will be described in more detail in the experimental examples below.

[0112] The superabsorbent polymer composition may have a centrifugation retention capacity (CRC) measured by EDANA method WSP241.3 of 39 g / g or more, or 40 g / g or more and 50 g / g or less, or 48 g / g or less, or 45 g / g or less. The method for measuring the water retention capacity will be described in more detail in the experimental examples described later.

[0113] Furthermore, the superabsorbent polymer composition may have an absorbency under pressure (AUP) at 0.7 psi measured by EDANA method WSP242.3 of 24.0 g / g or more, 25.0 g / g or more, 26.0 g / g or more, or 24.3 g / g or more, and may be 30 g / g or less, 28.0 g / g or less, or 26.0 g / g or less. The method for measuring the absorbency under pressure will be described in more detail in the experimental examples described later.

[0114] (Method of producing superabsorbent resin composition) On the other hand, the superabsorbent resin composition is Step 1: cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a polymer; neutralizing at least a portion of the acidic groups of the polymer (Step 2); (Step 3) preparing base resin particles by atomizing the polymer in the presence of an additive represented by the following formula 1: and drying the base resin particles (Step 4):

[0115] [ka]

[0116] In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl,

[0117] [ka]

[0118] where one or more of these is a carbonyl or

[0119] [ka]

[0120] wherein m1, m2, and m3 each independently represent an integer from 1 to 8;

[0121] [ka]

[0122] are each linked to adjacent oxygen atoms,

[0123] [ka]

[0124] is the adjacent R 1 , R 2 and R 3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

[0125] Hereinafter, the method for producing a superabsorbent resin according to one embodiment will be described in detail for each step.

[0126] (Stage 1) In one embodiment of the method for preparing a superabsorbent resin, a water-soluble ethylenically unsaturated monomer having an acidic group is cross-linked and polymerized in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer.

[0127] The steps include preparing a monomer composition by mixing the water-soluble ethylenically unsaturated monomer, an internal crosslinking agent, and a polymerization initiator, and thermally or photopolymerizing the monomer composition to form a polymer. At this time, the water-soluble ethylenically unsaturated monomer and the internal crosslinking agent are described above.

[0128] Here, the water-soluble ethylenically unsaturated monomer has an acidic group. As described above, in the conventional production of a superabsorbent resin, a monomer in which at least a part of the acidic group has been neutralized with a neutralizing agent is cross-linked to form a hydrogel polymer. Specifically, at least a part of the acidic group of the water-soluble ethylenically unsaturated monomer is neutralized in the step of mixing the water-soluble ethylenically unsaturated monomer having the acidic group, an internal cross-linking agent, a polymerization initiator, and a neutralizing agent.

[0129] However, according to one embodiment of the present invention, the water-soluble ethylenically unsaturated monomer is polymerized in a state where the acid group is not neutralized to form a polymer.

[0130] A water-soluble ethylenically unsaturated monomer (e.g., acrylic acid) in which the acid group is not neutralized is in a liquid state at room temperature and has high miscibility with the solvent (water) and exists in the form of a mixed solution in the monomer composition. However, a water-soluble ethylenically unsaturated monomer in which the acid group is neutralized is in a solid state at room temperature and has different solubility depending on the temperature of the solvent (water), with the solubility decreasing as the temperature decreases.

[0131] As described above, the water-soluble ethylenically unsaturated monomer in which the acid group is not neutralized has a higher solubility or miscibility in a solvent (water) than a monomer in which the acid group is neutralized, and does not precipitate even at a low temperature, so it is advantageous for long-term polymerization at low temperatures. As a result, a polymer having a higher molecular weight and a uniform molecular weight distribution can be stably formed by performing long-term polymerization using the water-soluble ethylenically unsaturated monomer in which the acid group is not neutralized.

[0132] Furthermore, it is possible to form a polymer having a longer chain, and the effect of reducing the content of water-soluble components that exist in an incompletely polymerized or incompletely crosslinked state and are not crosslinked can be achieved.

[0133] Furthermore, when the acidic groups of the monomers are not neutralized, polymerization is first performed to form a polymer, and then the polymer is neutralized and then micronized in the presence of the additive of Formula 1, or the acidic groups in the polymer are neutralized simultaneously with micronization, the additive of Formula 1 is present in a large amount on the surface of the polymer, and can sufficiently play a role in reducing the stickiness of the polymer.

[0134] The type of the water-soluble ethylenically unsaturated monomer in the monomer composition is the same as that described in the superabsorbent polymer composition. The concentration of the water-soluble ethylenically unsaturated monomer can be appropriately adjusted in consideration of the polymerization time and reaction conditions, and may be about 20 to about 60% by weight, or about 20 to about 40% by weight.

[0135] The type of the internal crosslinking agent in the monomer composition is the same as that described in the superabsorbent resin composition. The content of the internal crosslinking agent can be 0.01 to 5 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal crosslinking agent can be used in an amount of 0.01 parts by weight or more, 0.05 parts by weight or more, or 0.1 parts by weight or more and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.7 parts by weight or less based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the content of the internal crosslinking agent is too low, crosslinking does not occur sufficiently, making it difficult to achieve strength above an appropriate level, and if the content of the internal crosslinking agent is too high, the internal crosslinking density increases, making it difficult to achieve the desired water retention ability.

[0136] In addition, the polymerization initiator can be appropriately selected depending on the polymerization method, and when a thermal polymerization method is used, a thermal polymerization initiator can be used, when a photopolymerization method is used, a photopolymerization initiator can be used, and when a hybrid polymerization method (a method using both heat and light) is used, both a thermal polymerization initiator and a photopolymerization initiator can be used. However, even in the photopolymerization method, a certain amount of heat is generated by light irradiation such as ultraviolet irradiation, and a certain amount of heat is generated by the progress of the polymerization reaction, which is an exothermic reaction, so a thermal polymerization initiator may be additionally used.

[0137] The photopolymerization initiator can be used without any limitation on its composition as long as it is a compound capable of forming radicals by light such as ultraviolet light.

[0138] The photopolymerization initiator may be, for example, one or more selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acylphosphine include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate. More various photoinitiators are clearly described in "UV Coatings: Basics, Recent Developments and New Application" (Elsevier, 2007), p. 115, by Reinhold Schwalm, and are not limited to the above-mentioned examples.

[0139] In addition, the thermal polymerization initiator may be one or more selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid. Specifically, examples of persulfate initiators include sodium persulfate (Na 2 S 2 O 8 ), potassium persulfate (K 2 S 2 O 8 ), Ammonium persulfate ((NH 4 ) 2 S 2 O 8 Examples of azo initiators include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, and the like. dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc. More diverse thermal polymerization initiators are described in detail in Principle of Polymerization by Odian (Wiley, 1981), p. 203, and are not limited to the above-mentioned examples.

[0140] The polymerization initiator can be used in an amount of 2 parts by weight or less per 100 parts by weight of the water-soluble ethylenically unsaturated monomer. That is, if the concentration of the polymerization initiator is too low, the polymerization rate is slowed down and a large amount of residual monomer may be extracted in the final product, which is not preferable. On the other hand, if the concentration of the polymerization initiator is higher than the above range, the polymer chains forming the network become shorter, the content of water-soluble components increases, and the physical properties of the resin, such as the ability to absorb water under pressure, may decrease, which is not preferable.

[0141] The monomer composition may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.

[0142] The monomer composition containing the monomer may be in a solution state dissolved in a solvent such as water, and the solid content in the monomer composition in such a solution state, that is, the concentration of the monomer, the internal crosslinking agent, and the polymerization initiator, can be appropriately adjusted in consideration of the polymerization time, reaction conditions, etc. For example, the solid content in the monomer composition may be 10 to 80% by weight, or 15 to 60% by weight, or 30 to 50% by weight.

[0143] When the monomer composition has a solid content in this range, it is possible to utilize the gel effect phenomenon that appears in the polymerization reaction of a high-concentration aqueous solution to eliminate the need to remove unreacted monomers after polymerization, and to control the pulverization efficiency when pulverizing the polymer, as described below.

[0144] The solvent that can be used in this case is not limited in composition as long as it can dissolve the above-mentioned components. For example, one or more selected from water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, and N,N-dimethylacetamide can be used in combination.

[0145] According to one embodiment of the present invention, the step of polymerizing the monomer composition to form a polymer is carried out in a batch type reactor.

[0146] In a typical method for producing a superabsorbent polymer composition, the polymerization method is roughly divided into thermal polymerization and photopolymerization depending on the polymerization energy source. In general, when thermal polymerization is carried out, it is carried out in a reactor having a stirring shaft such as a kneader, and when photopolymerization is carried out, it is carried out in a reactor equipped with a movable conveyor belt or in a vessel with a flat bottom.

[0147] On the other hand, such polymerization methods generally have a short polymerization reaction time (eg, 1 hour or less), so that the molecular weight of the polymer is not large and the polymer has a broad molecular weight distribution.

[0148] On the other hand, when photopolymerization is carried out in a reactor equipped with a movable conveyor belt or a vessel with a flat bottom, the shaped hydrogel polymer obtained is usually a sheet-like hydrogel polymer having the width of the belt, and the thickness of the polymer sheet varies depending on the concentration and the injection speed or amount of the monomer composition injected, but is usually about 0.5 to about 5 cm.

[0149] However, if the thickness of the sheet-like polymer is too thin, the production efficiency is low when the monomer composition is supplied, which is not preferable, and if the thickness of the sheet-like polymer is increased for the sake of productivity, the polymerization reaction does not occur uniformly throughout the entire thickness, making it difficult to form a high-quality polymer.

[0150] In addition, in the polymerization in the reactor having a reactor agitator equipped with a conveyor belt, the polymerization is performed continuously by feeding new monomer composition to the reactor while moving the polymerization result, so that polymers having different polymerization rates are mixed, which makes it difficult to perform uniform polymerization throughout the monomer composition, and may result in deterioration of overall physical properties.

[0151] However, according to one embodiment of the present invention, the polymerization is carried out in a stationary batch reactor, so that there is little risk of polymers with different polymerization rates being mixed together, and thus a polymer with uniform quality can be obtained.

[0152] In addition, the polymerization step is carried out in a batch reactor having a predetermined volume, and the polymerization reaction is carried out for a longer time, for example, 3 hours or more, than in the case of carrying out continuous polymerization in a reactor equipped with a conveyor belt. Despite such a long polymerization reaction time, since the polymerization is carried out on unneutralized water-soluble ethylenically unsaturated monomer, the monomer does not precipitate well even if the polymerization is carried out for a long time, and therefore it is advantageous for long-term polymerization.

[0153] Meanwhile, the polymerization in the batch reactor of the present invention uses a thermal polymerization method, and the polymerization initiator may be a thermal polymerization initiator among the above-mentioned initiators.

[0154] Meanwhile, in one embodiment of the present invention, the polymerization can be initiated by adding a reducing agent that forms a redox couple with the initiator.

[0155] Specifically, the initiator and the reducing agent react with each other to form radicals when added to the polymer solution.

[0156] The formed radicals react with the monomer, and the oxidation-reduction reaction between the initiator and the reducing agent is highly reactive, so polymerization can be initiated even with only a small amount of initiator and reducing agent added, there is no need to increase the process temperature, low-temperature polymerization is possible, and changes in the physical properties of the polymer solution can be minimized.

[0157] The polymerization reaction using the oxidation-reduction reaction can be smoothly carried out at or below room temperature (25° C.) For example, the polymerization reaction is carried out at a temperature of 5° C. to 25° C. or 5° C. to 20° C.

[0158] In one embodiment of the present invention, when a persulfate initiator is used as the initiator, the reducing agent is sodium metabisulfite (Na 2 S 2 O 5 );Tetramethylethylenediamine (TMEDA);A mixture of iron(II) sulfate and EDTA (FeSO 4 / EDTA); sodium formaldehyde sulfoxylate; and disodium 2-hydroxy-2-sulfinoacetate.

[0159] For example, potassium persulfate can be used as the initiator and disodium 2-hydroxy-2-sulfinoacetate can be used as the reducing agent; ammonium persulfate can be used as the initiator and tetramethylethylenediamine can be used as the reducing agent; or sodium persulfate can be used as the initiator and sodium formaldehyde sulfoxylate can be used as the reducing agent.

[0160] In another embodiment of the present invention, when a hydrogen peroxide-based initiator is used as the initiator, the reducing agent is ascorbic acid; sucrose; sodium sulfite (Na 2 SO 3 ), Sodium Metabisulfite (Na2 S 2 O 5 );Tetramethylethylenediamine (TMEDA);A mixture of iron(II) sulfate and EDTA (FeSO 4 / EDTA); sodium formaldehyde sulfoxylate; disodium 2-hydroxy-2-sulfinoacetate; and disodium 2-hydroxy-2-sulfoacetate.

[0161] The polymer obtained by such a method can form a polymer having a high molecular weight and a uniform molecular weight distribution by polymerizing an unneutralized ethylenically unsaturated monomer, as described above, and the content of water-soluble components can be reduced.

[0162] The polymer obtained by such a method may have a water content of 30 to 80% by weight in a state of a hydrogel polymer. For example, the water content of the polymer may be 30% by weight or more, 45% by weight or more, or 50% by weight or more, and 80% by weight or less, 70% by weight or less, or 60% by weight or less.

[0163] If the moisture content of the polymer is too low, it may be difficult to secure an adequate surface area in the subsequent crushing step, and the polymer may not be crushed effectively. If the moisture content of the polymer is too high, the pressure applied in the subsequent crushing step may increase, making it difficult to crush the polymer to a desired particle size.

[0164] Meanwhile, in the present specification, the term "moisture content" refers to the amount of moisture in the total weight of a polymer, which is calculated by subtracting the weight of the polymer in a dry state from the weight of the polymer. Specifically, the moisture content is calculated by measuring the weight loss due to the evaporation of moisture in the polymer during the process of drying the polymer in a crumb state by increasing the temperature of the polymer by infrared heating. In this case, the drying conditions are a method of increasing the temperature from room temperature to about 180°C and then maintaining it at 180°C, and the total drying time is set to 40 minutes, including 5 minutes for the temperature increase step, and the moisture content is measured.

[0165] (Stage 2 and Stage 3) Next, a step (step 2) of neutralizing at least a portion of the acidic groups of the polymer; and a step (step 3) of micronizing the polymer in the presence of the additive represented by Chemical Formula 1 to prepare base resin particles are carried out.

[0166] First, the neutralizing agent used in step 2 may be a basic substance such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide that can neutralize acidic groups.

[0167] In addition, the degree of neutralization, which refers to the degree to which the acidic groups contained in the polymer are neutralized by the neutralizing agent, may be 50 to 90 mol%, or 60 to 85 mol%, or 65 to 85 mol%, or 65 to 75 mol%. The range of the degree of neutralization varies depending on the final physical properties, but if the degree of neutralization is too high, the water absorption capacity of the superabsorbent resin may decrease, and the concentration of carboxyl groups on the particle surface may be too low, making it difficult to perform surface crosslinking in the subsequent process, resulting in decreased water absorption properties or liquid permeability under pressure. Conversely, if the degree of neutralization is too low, not only will the water absorption capacity of the polymer decrease significantly, but it may also exhibit properties similar to elastic rubber, which are difficult to handle.

[0168] Next, the polymer is atomized in the presence of the additive represented by Chemical Formula 1 to prepare base resin particles (Step 3).

[0169] Here, the steps 2 and 3 are carried out sequentially, simultaneously, or alternately. That is, simultaneously with, before, or after the step 2, a step of atomizing the polymer in the presence of a surfactant is carried out (step 3).

[0170] This step is a step of atomizing the polymer in the presence of the additive of Chemical Formula 1, in which the polymer is not chopped into millimeter sizes, but is simultaneously chopped into sizes of tens to hundreds of micrometers and aggregated. That is, this is a step of producing secondary aggregate particles in which primary particles chopped into sizes of tens to hundreds of micrometers are aggregated by imparting appropriate adhesion to the polymer. The base resin particles, which are secondary aggregate particles produced in this step, have a normal particle size distribution and a significantly increased surface area, thereby significantly improving the water absorption rate.

[0171] In this manner, the polymer is mixed with the additive of Chemical Formula 1, and then the polymer is atomized in the presence of the additive of Chemical Formula 1 to produce base resin particles in the form of secondary agglomerated particles that are chopped and agglomerated in a state where the superabsorbent resin particles and the surfactant are mixed.

[0172] The additive represented by Formula 1 can be applied to the same content as that described above in relation to the superabsorbent polymer composition.

[0173] Here, the "base resin particles" are particles having a water content (moisture content) of about 30% by weight or more, and are formed by chopping and agglomerating a polymer into particles without a drying process, and therefore can have a moisture content of 30 to 80% by weight, preferably 70 to 80% by weight, similar to the polymer.

[0174] Meanwhile, the additive of the formula 1 can be used in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer used in the crosslinking polymerization to produce the polymer. If the additive of the formula 1 is used too little, it may not be evenly adsorbed on the surface of the polymer, and re-aggregation of particles may occur after pulverization, and if the surfactant is used too much, various physical properties of the final superabsorbent resin may be deteriorated. For example, the additive of the formula 1 can be used in an amount of 0.01 parts by weight or more, 0.015 parts by weight or more, or 0.1 parts by weight or more and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer.

[0175] The method of mixing the additive of Formula 1 with the polymer is not particularly limited as long as it can be uniformly mixed with the polymer, and can be appropriately adopted and used. Specifically, the additive of Formula 1 can be mixed in a dry state, dissolved in a solvent and mixed in a solution state, or melted and then mixed.

[0176] Among these, for example, the additive of Formula 1 is mixed in a state of solution dissolved in a solvent. In this case, any type of solvent can be used without limitation, whether it is an inorganic solvent or an organic solvent, but water is the most suitable in consideration of the ease of the drying process and the cost of the solvent recovery system. In addition, the solution can be mixed by putting the additive of Formula 1 and the polymer in a reaction vessel, putting the polymer in a mixer and spraying the solution, or continuously supplying the polymer and the solution to a continuously operating mixer and mixing them.

[0177] Meanwhile, according to one embodiment of the present invention, steps 2 and 3 are performed sequentially, simultaneously, or alternately.

[0178] That is, a neutralizing agent may be added to a polymer to neutralize the acidic groups first, and then the additive of Formula 1 may be added to the neutralized polymer to atomize the polymer mixed with the additive, or a neutralizing agent and an additive may be added simultaneously to the polymer to neutralize and atomize the polymer. Alternatively, the additive may be added first, and then the neutralizing agent may be added later. Alternatively, the neutralizing agent and the additive may be added alternately in a cross-like manner. Alternatively, the additive may be added first to atomize, and then the neutralizing agent may be added to neutralize, and an additive may be added additionally to the neutralized hydrogel polymer to perform an additional atomization process.

[0179] On the other hand, in order to achieve uniform neutralization of the entire polymer, it is preferable to allow a certain time lag between the addition of the neutralizing agent and the atomization step.

[0180] At least a portion or a substantial amount of the additive of Formula 1 may be present on the surface of the base resin particles.

[0181] Here, the additive of Formula 1 being present on the surface of the base resin particle means that at least a part or a substantial amount of the additive of Formula 1 is adsorbed or bound to the surface of the base resin particle. Specifically, the additive of Formula 1 may be physically or chemically adsorbed to the surface of the base resin particle. More specifically, the hydrophilic functional group of the additive of Formula 1 may be physically adsorbed to the hydrophilic part of the surface of the base resin particle by intermolecular forces such as dipole-dipole interaction. In this way, the hydrophilic part of the additive of Formula 1 may be physically adsorbed to the surface of the base resin particle and surround the surface, and the hydrophobic part of the additive of Formula 1 may not be adsorbed to the surface of the base resin particle, and the base resin particle may be coated with the additive of Formula 1 in the form of a kind of micelle structure. This is because the additive of Formula 1 is added not during the polymerization process of the water-soluble ethylenically unsaturated monomer but during the microparticulation step after polymer formation, and therefore can faithfully play the role of a surfactant compared to when the additive of Formula 1 is added during the polymerization process and exists inside the polymer, and particles with a large surface area can be obtained in the form of fine particles being aggregated by simultaneously pulverizing and agglomerating.

[0182] According to one embodiment, the step of preparing the base resin particles (step 3) is carried out using an atomizer.

[0183] The pulverizer includes a body portion including a transfer space into which a mixture of a polymer and an additive is transferred, a screw member rotatably installed within the transfer space to move the mixture, a drive motor to provide a rotational driving force to the screw member, and a cutter member installed in the body portion, including a perforated plate having a number of holes formed therein, for pulverizing the mixture while discharging it to the outside of the body portion.

[0184] According to one embodiment, said steps 2 and 3 are carried out sequentially, simultaneously or intersectingly, which is carried out using an atomizer.

[0185] In this case, the atomization device further includes a neutralizer injection nozzle installed inside the body portion, and the neutralizer is injected through the neutralizer injection nozzle, so that steps 2 and 3 are performed sequentially, simultaneously, or crosswise.

[0186] Specifically, the neutralizer is injected into the body through the neutralizer injection nozzle to neutralize at least a part of the acidic groups of the polymer having acidic groups in the mixture. Specifically, in the atomization device, the neutralizer is injected into the body through the neutralizer injection nozzle to neutralize at least a part of the acidic groups of the polymer having acidic groups in the mixture, and at the same time, the mixture is pulverized (atomized) while being discharged to the outside of the body through a porous plate.

[0187] Preferably, the neutralizing agent pulverized by the neutralizing agent injection nozzle is injected adjacent to the perforated plate. In this case, the neutralizing agent acts as a slip agent in the mixture when the mixture is discharged through the holes in the perforated plate while the neutralization process is being carried out, thereby reducing the load on the holes.

[0188] Preferably, the cutter member of the atomization device includes a perforated plate and a cutting knife disposed adjacent to the perforated plate on the outlet side of the body portion, and after the mixture passes through the perforated plate, it is more effectively crushed and atomized by the cutting knife.

[0189] In the pulverization device, the cutter member can include a plurality of perforated plates and a plurality of cutting knives. The arrangement order of the perforated plates and the cutting knives is not particularly limited, and they may be arranged sequentially, cross each other, or the perforated plates may be arranged in succession, or the cutting knives may be arranged in succession.

[0190] By including a plurality of perforated plates and cutting knives as described above, multiple atomizations are performed within a single atomization device. Meanwhile, a plurality of neutralizing agent injection nozzles may be disposed adjacent to any one or more of the perforated plates and cutting knives, and it is preferable that the neutralizing agent injection nozzle is disposed adjacent to the perforated plate in terms of improving slipperiness.

[0191] In the above-mentioned pulverization device, the hole size formed in the perforated plate may be 0.1 mm to 30 mm. Preferably, it may be 0.5 mm to 25 mm, 1 mm to 20 mm, or 1 mm to 10 mm. By using a perforated plate having the above-mentioned hole size, base resin particles having a desired particle size can be produced. When the cutter member includes a plurality of perforated plates as described above, the size of the holes formed in each of the perforated plates satisfies the above-mentioned range, and they may be the same or different from each other.

[0192] According to one embodiment of the invention, the step 3 may be performed multiple times, which may be performed using multiple atomizing devices, or using a single atomizing device including multiple perforated plates and / or multiple cutting knives, or some of the multiple atomizing devices may include multiple perforated plates and / or multiple cutting knives. The atomizing step is preferably performed 1-6 times or 1-4 times. When the step 3 is performed multiple times, the additive may be additionally added multiple times.

[0193] In the step (step 3) of preparing base resin particles by atomizing the polymer, the base resin particles may be atomized to have an average particle size of 50 μm to 600 μm, preferably 100 μm to 500 μm, 150 μm to 450 μm, or 200 μm to 400 μm. By satisfying the above particle size range, the polymer is prepared into secondary particles in the form of aggregated primary particles, and the subsequent pulverization and drying processes are carried out under milder conditions, thereby significantly reducing the amount of fine powder generated during the process.

[0194] In the present invention, the average particle size "Dn" means the particle size or particle diameter at the n% point of the cumulative particle number distribution according to the particle size. That is, D50 indicates the particle size at the 50% point of the cumulative particle number distribution according to the particle size, D90 indicates the particle size at the 90% point of the cumulative particle number distribution according to the particle size, and D10 indicates the particle size at the 10% point of the cumulative particle number distribution according to the particle size. The Dn can be measured using a laser diffraction method or the like. Specifically, the powder to be measured is dispersed in a dispersion medium and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through a laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution. D10, D50, and D90 can be measured by calculating the particle sizes at the 10%, 50%, and 90% points of the cumulative particle number distribution according to the particle size in the measuring device.

[0195] (Stage 4) Next, the base resin particles are dried (Step 4), thereby producing a superabsorbent resin composition containing the superabsorbent resin particles and the additive represented by Chemical Formula 1.

[0196] The drying is carried out so that the moisture content of each of the plurality of superabsorbent resin particles contained in the produced superabsorbent resin composition is about 10% by weight or less, specifically, about 0.1 to about 10% by weight.

[0197] In this case, the drying of the ground material is carried out in a moving type, which is distinguished from fixed-bed type drying by whether or not the material moves during drying.

[0198] In a typical method for producing a superabsorbent resin, the drying step is generally performed until the moisture content of the superabsorbent resin particles is less than 10% by weight. However, in the present invention, the aggregation is controlled by performing the atomization step in the presence of the additive of Chemical Formula 1, and the drying is performed so that the moisture content of the dried superabsorbent resin particles is 10% by weight to 20% by weight, preferably 10% by weight to 25% by weight. However, the present invention is not limited thereto. This has the advantage of showing a high moisture content and fundamentally preventing the generation of fine powder. In addition, it is preferable because the water absorption speed of the final superabsorbent resin composition can be improved.

[0199] For this purpose, the drying step is carried out in a moving type drying manner at a relatively low temperature. Such a moving type drying is different from a fixed-bed type drying in terms of whether or not the material moves during drying, and is preferable because it prevents aggregation between the chopped water-containing superabsorbent resin particles in the pulverized material to be dried and allows drying to be completed within a short period of time.

[0200] For this purpose, the drying step is carried out in a moving type drying manner at a relatively low temperature. Such a moving type drying is different from a fixed-bed type drying in terms of whether or not the material moves during drying, and is preferable because it prevents aggregation between the finely chopped base resin particles in the pulverized material to be dried and allows drying to be completed within a short period of time.

[0201] Specifically, the moving type drying refers to a method of drying while mechanically stirring the material. In this case, the direction in which the hot air passes through the material may be the same as or different from the direction in which the material circulates. Alternatively, the material may be circulated inside the dryer, and a heat transfer fluid (heat medium flow) may be passed through a separate pipe outside the dryer to dry the material. Meanwhile, fixed-bed type drying refers to a method in which the material to be dried is suspended at the bottom, such as a perforated iron plate through which air can pass, and hot air passes through the material from bottom to top to dry it.

[0202] The step of drying the base resin particles (step 4) may be performed using any commonly used fluidized dryer without any particular limitation, for example, a fluidized dryer such as a horizontal-type mixer, a rotary kiln, a paddle dryer, or a steam tube dryer.

[0203] The drying step (step 4) is carried out at a relatively low temperature of 150° C. or less, preferably 100° C. to 150° C., 100° C. to 130° C., or 105° C. to 115° C. Even when the drying step is carried out at a low temperature as described above, it is possible to produce superabsorbent resin particles having the desired particle size and physical properties without the desired aggregation.

[0204] Meanwhile, the drying temperature may be an internal driving temperature of the fluidized drying device to which the material to be dried is fed, and this can be adjusted by passing a heat transfer fluid (heat medium flow) through a separate pipe outside the dryer, but is not limited thereto.

[0205] The drying step (step 4) is carried out for 30 to 80 minutes, 30 to 60 minutes, or 40 to 50 minutes. Since there is little aggregation between the finely chopped polymer resin particles in the pulverized material to be dried, even if the drying step is carried out at a relatively low temperature for a short period of time, it is possible to produce superabsorbent resin particles having the desired particle size and physical properties.

[0206] (Additional Phase) Hereinafter, the method for preparing a superabsorbent polymer composition according to an embodiment of the present invention may further include a step of pulverizing and classifying the superabsorbent polymer particles, if necessary.

[0207] Specifically, the pulverization step is performed by pulverizing the dried superabsorbent resin particles to have a particle size on the normal particle level, that is, a particle size of 150 μm to 850 μm.

[0208] To this end, the crusher used may be specifically a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, or a disc cutter, but is not limited to the above-mentioned examples.

[0209] Alternatively, the grinding machine may be a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, a jog mill, or the like, but is not limited to the above examples.

[0210] Meanwhile, in the manufacturing method of the present invention, it is possible to realize superabsorbent resin particles having a smaller particle size distribution in the atomization step than in the conventional chopping step, and when moving type drying is performed, the moisture content after drying is maintained relatively high at 10% by weight or more. Therefore, even if the grinding is performed under mild conditions with less grinding force, it is possible to form a superabsorbent resin having a very high content of normal particle sizes of 150 μm to 850 μm, and the generation rate of fine powder can be significantly reduced.

[0211] The superabsorbent resin particles prepared as described above may contain superabsorbent resin particles having a particle size of 150 μm to 850 μm, i.e., normal particles, at a ratio of 80% by weight or more, 85% by weight or more, 89% by weight or more, 90% by weight or more, 92% by weight or more, 93% by weight or more, 94% by weight or more, or 95% by weight or more. The particle size of such resin particles can be measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP220.3 method.

[0212] In addition, the superabsorbent resin particles may contain less than about 20% by weight, less than about 18% by weight, less than about 15% by weight, less than about 13% by weight, less than about 10% by weight, specifically less than about 5% by weight, more specifically less than about 3% by weight of fine powder having a particle size of less than 150 μm relative to the total weight. This is in contrast to the case where a superabsorbent resin is produced by a conventional production method, which contains more than about 20% by weight to about 30% by weight of fine powder.

[0213] Next, the method for preparing a superabsorbent resin according to an embodiment of the present invention may include a step of thermally crosslinking the surface of the base resin powder in the presence of a surface crosslinker to prepare superabsorbent resin particles.

[0214] The surface cross-linking step induces a cross-linking reaction on the surface of the base resin powder in the presence of a surface cross-linking agent, and the unsaturated bonds of the water-soluble ethylenically unsaturated monomer remaining on the surface without being cross-linked are cross-linked by the surface cross-linking agent to form a superabsorbent resin with a high surface cross-linking density.

[0215] Specifically, a surface cross-linked layer is formed in a heat treatment process in the presence of a surface cross-linking agent, and the heat treatment process increases the surface cross-linking density, i.e., the external cross-linking density, while the internal cross-linking density remains unchanged. Thus, the superabsorbent resin having a surface cross-linked layer thus produced has a structure in which the external cross-linking density is higher than the internal cross-linking density.

[0216] The surface cross-linking step is carried out at a temperature of about 80° C. to about 250° C. More specifically, the surface cross-linking step is carried out at a temperature of about 100° C. to about 220° C., or about 120° C. to about 200° C., for about 20 minutes to about 2 hours, or about 40 minutes to about 80 minutes. When the above-mentioned surface cross-linking step conditions are satisfied, the surface of the highly water-absorbent resin particles is sufficiently cross-linked, and the water absorption capacity under pressure can be increased.

[0217] By satisfying such surface cross-linking process conditions (particularly, temperature rise conditions and reaction conditions at the maximum reaction temperature), a highly water-absorbent resin having excellent physical properties such as water absorption rate can be produced.

[0218] The temperature raising means for the surface crosslinking reaction is not particularly limited. Heating can be performed by supplying a heat medium or directly supplying a heat source. At this time, the type of heat medium that can be used can be a heated fluid such as steam, hot air, hot oil, etc., but is not limited to these, and the temperature of the heat medium to be supplied can be appropriately selected in consideration of the means of the heat medium, the heating rate, and the target temperature of the heat raising. On the other hand, the heat source to be directly supplied can be, but is not limited to the above-mentioned examples, heating by electricity and heating by gas.

[0219] Meanwhile, as the surface cross-linking agent contained in the surface cross-linking agent composition, all surface cross-linking agents that have been used in the manufacture of superabsorbent resins can be used without any particular restrictions.For example, the surface cross-linking agent can include one or more polyols selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,2-hexanediol, 1,3-hexanediol, 2-methyl-1,3-propanediol, 2,5-hexanediol, 2-methyl-1,3-pentanediol, 2-methyl-2,4-pentanediol, tripropylene glycol and glycerol; one or more carbonate-based compounds selected from the group consisting of ethylene carbonate and propylene carbonate; epoxy compounds such as ethylene glycol diglycidyl ether; oxazoline compounds such as oxazolidinone; polyamine compounds; mono-, di- or polyoxazolidinone compounds; or cyclic urea compounds; and the like. Preferably, the same internal crosslinking agent as described above can be used, for example, a diglycidyl ether compound of alkylene glycol such as ethylene glycol diglycidyl ether.

[0220] In the surface cross-linking step, a surface cross-linking agent composition containing an alcohol-based solvent and water in addition to a surface cross-linking agent may be used.

[0221] Such a surface cross-linking agent can be used in an amount of 0.001 to 2 parts by weight per 100 parts by weight of the superabsorbent resin particles. It is preferable that the content of the surface cross-linking agent is 0.005 parts by weight or more, 0.01 parts by weight or more, or 0.02 parts by weight or more, and 0.5 parts by weight or less, 0.3 parts by weight or less. By adjusting the content range of the surface cross-linking agent to the above-mentioned range, a superabsorbent resin exhibiting various physical properties such as excellent water absorption performance and liquid permeability can be produced.

[0222] Meanwhile, the surface cross-linking agent is added to the superabsorbent resin particles in the form of a surface cross-linking agent composition containing the surface cross-linking agent, and the method of adding the surface cross-linking agent composition is not particularly limited in its constitution. For example, the surface cross-linking agent composition and the superabsorbent resin particles are mixed in a reaction tank, the surface cross-linking agent composition is sprayed onto the superabsorbent resin particles, and the superabsorbent resin particles and the surface cross-linking agent composition are continuously fed to a continuously operating mixer to be mixed.

[0223] The surface cross-linking agent composition may further include water and / or a hydrophilic organic solvent as a medium. This has the advantage that the surface cross-linking agent can be uniformly dispersed on the base resin powder. At this time, the content of water and the hydrophilic organic solvent can be adjusted and applied by controlling the addition ratio with respect to 100 parts by weight of the highly water-absorbent resin particles in order to induce uniform dissolution / dispersion of the surface cross-linking agent and prevent the agglomeration phenomenon of the base resin powder, while optimizing the surface penetration depth of the surface cross-linking agent.

[0224] Meanwhile, in the method for producing a superabsorbent resin according to an embodiment of the present invention, various polyvalent metal salts, such as aluminum salts, such as aluminum sulfate, may be further used during surface cross-linking in order to further improve liquid permeability, etc. Such polyvalent metal salts are contained on the surface cross-linked layer of the finally produced superabsorbent resin.

[0225] According to one embodiment of the present invention, after the step of forming a surface cross-linked layer on at least a part of the surface of the superabsorbent resin particles, the method further includes at least one of a cooling step of cooling the superabsorbent resin particles having the surface cross-linked layer formed thereon, a hydration step of adding water to the superabsorbent resin particles having the surface cross-linked layer formed thereon, and a post-treatment step of adding an additive to the superabsorbent resin particles having the surface cross-linked layer formed thereon. At this time, the cooling step, the hydration step, and the post-treatment step are performed sequentially or simultaneously.

[0226] The additives added in the post-treatment step may be a liquid permeability improver, an anti-caking agent, a flowability improver, an antioxidant, etc., but the present invention is not limited thereto.

[0227] By selectively carrying out the cooling, hydration and post-treatment steps, the moisture content of the final superabsorbent polymer can be increased, resulting in the production of a higher quality superabsorbent polymer product.

[0228] According to another embodiment of the present invention, there is provided a superabsorbent polymer composition produced by the above-mentioned production method.

[0229] The superabsorbent polymer composition produced by the above-mentioned production method realizes a high water content without a separate additional water addition process or additive addition process, and has a low fine powder content. The water absorption properties, namely, water retention capacity (CRC) and absorbency under pressure (AUP), are at the same level or higher than those of superabsorbent polymers produced by conventional methods. At the same time, the content of water soluble components (EC) is low, so that a superabsorbent polymer excellent in all respects, such as water absorption speed, can be provided.

[0230] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.

[0231] Example - Preparation of superabsorbent resin composition Example 1 (Step 1) 1,000g of acrylic acid, 3.5g of pentaerythritol triallyl ether as an internal crosslinking agent, and 2,260g of water were mixed in a 5L glass container equipped with a stirrer and a thermometer, and stirred while maintaining the temperature at 5°C. Nitrogen was introduced into the glass container containing the mixture at 1,000cc / min for 1 hour to replace the nitrogen condition. Next, 13g of 0.3% hydrogen peroxide solution, 15g of 1% ascorbic acid solution, and 30g of 2% 2,2'-azobis-(2-amidinopropane) dihydrochloric acid solution were added as polymerization initiators, and 15g of 0.01% iron sulfate solution was added as a reducing agent to start polymerization. After the temperature of the mixture reached 85°C, the mixture was polymerized at 90±2°C for about 3 hours to obtain a polymer. The water content of the polymer was about 70% by weight.

[0232] (Steps 2 and 3) 1.19 g of A-1 compound in Table 1 as an additive of Chemical Formula 1 was dispersed in 52.27 g of water (preparation of 2 wt% aqueous dispersion), which was then mixed with 1,000 g of the polymer obtained in Step 1.

[0233] The mixture was passed once through a first atomizer equipped with a perforated plate containing a large number of holes with a hole size of 6 mm to carry out a primary atomization process.

[0234] Next, the mixture was repeatedly fed into a second atomizer equipped with a perforated plate having a number of holes with a hole size of 4 mm three times to carry out the second, third and fourth atomization processes.

[0235] In the secondary atomization step, 400 g of 32% NaOH aqueous solution was added through a neutralizer nozzle disposed adjacent to the perforated plate to carry out atomization and neutralization steps.

[0236] In the tertiary atomization process, 15% Na was added through a neutralizer nozzle disposed adjacent to the perforated plate. 2 SO 4 37.5 g of the aqueous solution was added, and the neutralization step was carried out together with atomization.

[0237] Finally, in the fourth atomization step, the atomization step was carried out without adding a neutralizing agent or a surfactant to obtain base resin particles.

[0238] The degree of neutralization of the base resin particles was 70 mol %.

[0239] After (Step 4), 1,000 g of the base resin particles were put into a rotary mixer fluidized dryer rotating at 100 rpm. The internal temperature of the dryer was maintained at 105° C. and drying was carried out for 60 minutes to obtain superabsorbent resin particles. The moisture content of the superabsorbent resin particles was 11 wt%.

[0240] Example 2 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-2 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0241] The moisture content of the final superabsorbent polymer particles after step 4 drying was 11 wt%.

[0242] Example 3 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-3 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0243] The moisture content of the final superabsorbent polymer particles after step 4 drying was 11 wt%.

[0244] Example 4 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-4 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0245] The moisture content of the final superabsorbent polymer particles after step 4 drying was 11 wt%.

[0246] Example 5 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-5 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0247] The moisture content of the final superabsorbent polymer particles after step 4 drying was 14 wt%.

[0248] Example 6 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-6 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0249] The moisture content of the final superabsorbent polymer particles after step 4 drying was 14 wt%.

[0250] Example 7 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-7 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0251] The moisture content of the final superabsorbent polymer particles after step 4 drying was 11 wt%.

[0252] Example 8 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-8 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0253] The moisture content of the final superabsorbent polymer particles after step 4 drying was 12 wt%.

[0254] Example 9 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-9 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0255] The moisture content of the final superabsorbent polymer particles after step 4 drying was 13 wt%.

[0256] Example 10 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-10 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0257] The moisture content of the final superabsorbent polymer particles after step 4 drying was 11 wt%.

[0258] Example 11 (Step 1) 1,000g of acrylic acid, 3.5g of pentaerythritol triallyl ether as an internal crosslinking agent, and 2,260g of water were mixed in a 5L glass container equipped with a stirrer and a thermometer, and stirred while maintaining the temperature at 5°C. Nitrogen was introduced into the glass container containing the mixture at 1,000cc / min for 1 hour to replace the nitrogen condition. Next, 13g of 0.3% hydrogen peroxide solution, 15g of 1% ascorbic acid solution, and 30g of 2% 2,2'-azobis-(2-amidinopropane) dihydrochloric acid solution were added as polymerization initiators, and 15g of 0.01% iron sulfate solution was added as a reducing agent to start polymerization. After the temperature of the mixture reached 85°C, the mixture was polymerized at 90±2°C for about 3 hours to obtain a polymer. The water content of the polymer was about 70% by weight.

[0259] (Steps 2 and 3) 0.595 g of A-1 compound in Table 1 as an additive of Chemical Formula 1 was dispersed in 52.27 g of water (preparation of 2 wt% aqueous dispersion), which was then mixed with 1,000 g of the polymer obtained in Step 1.

[0260] The mixture was passed once through a first atomizer equipped with a perforated plate containing a large number of holes with a hole size of 6 mm to carry out a primary atomization process.

[0261] Next, the mixture was repeatedly fed into a second atomizer equipped with a perforated plate having a number of holes with a hole size of 4 mm three times to carry out the second, third and fourth atomization processes.

[0262] In the secondary atomization step, 400 g of 32% NaOH aqueous solution was added through a neutralizer nozzle disposed adjacent to the perforated plate to carry out atomization and neutralization steps.

[0263] In the tertiary atomization process, 15% Na was added through a neutralizer nozzle disposed adjacent to the perforated plate. 2 SO 4 37.5 g of the aqueous solution was added, and the neutralization step was carried out together with atomization.

[0264] Finally, in the fourth pulverization process, 0.595 g of A-11 compound in Table 1 was dispersed in 52.27 g of water (to produce a 2 wt% aqueous dispersion) as an additive of Chemical Formula 1, and then this was fed into the second pulverization device containing the mixture from the third pulverization process to produce base resin particles. The degree of neutralization of the base resin particles was 70 mol%.

[0265] After (Step 4), 1,000 g of the base resin particles were put into a rotary mixer fluidized dryer rotating at 100 rpm. The internal temperature of the dryer was maintained at 105° C. and drying was carried out for 60 minutes to obtain superabsorbent resin particles.

[0266] The moisture content of the final superabsorbent polymer particles after drying in step 4 was 12 wt%.

[0267] Example 12 A superabsorbent polymer composition was prepared in the same manner as in Example 11, except that the A-1 compound was used as the additive of Chemical Formula 1 in the first pulverization step, and the A-2 compound in Table 1 was used instead of the A-11 compound as the additive of Chemical Formula 1 in the fourth pulverization step.

[0268] The moisture content of the final superabsorbent polymer particles after step 4 drying was 10 wt%.

[0269] Example 13 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-12 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0270] The moisture content of the final superabsorbent polymer particles after step 4 drying was 14 wt%.

[0271] Example 14 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the A-13 compound in Table 1 was used instead of the A-1 compound as the additive of Chemical Formula 1 in Example 1.

[0272] The moisture content of the final superabsorbent polymer particles after step 4 drying was 14 wt%.

[0273] Example 15 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that 0.595 g of the A-12 compound used in Example 13 and 0.595 g of the A-13 compound used in Example 14 were mixed together to use a total of 1.19 g of additives represented by Chemical Formula 1.

[0274] The moisture content of the final superabsorbent polymer particles after step 4 drying was 13 wt%.

[0275] Example 16 A superabsorbent polymer composition was prepared in the same manner as in Example 13, except that the amount of A-12, an additive of Chemical Formula 1, was increased to 2.38 g.

[0276] The moisture content of the final superabsorbent polymer particles after step 4 drying was 12 wt%.

[0277] Comparative Example 1 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the additive of Chemical Formula 1 was not used.

[0278] Comparative Examples 2 to 6, 8 and 9 A superabsorbent resin composition was prepared in the same manner as in Example 1, except that the additive of Chemical Formula 1 was replaced with an additive shown in Table 1 below.

[0279] Comparative Example 7 In a 3L glass container equipped with a stirrer and a thermometer, 100g (1.388mol) of acrylic acid, 0.16g of an internal crosslinking agent polyethylene glycol diacrylate (Mn=508), 0.008g of a photopolymerization initiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.12g of a thermal polymerization initiator sodium persulfate, and 123.5g of a 32% caustic soda solution were mixed at room temperature to prepare a monomer composition (neutralization degree of acrylic acid: 70mol%, solid content: 45wt%).

[0280] Thereafter, the monomer composition was supplied at a rate of 500 to 2000 mL / min onto a conveyor belt having a width of 10 cm and a length of 2 m, which rotated at a speed of 50 cm / min. 2 The polymerization reaction was allowed to proceed for 60 seconds under irradiation with ultraviolet light having an intensity of 1000 nm, thereby obtaining a hydrogel polymer having a water content of about 55% by weight.

[0281] Next, the hydrogel polymer obtained by the polymerization reaction was pulverized using a meat chopper without any additives. At this time, the water content of the hydrous superabsorbent resin particles contained in the final pulverized product was 55 wt%.

[0282] Thereafter, the pulverized material was dried in a convection oven capable of transferring airflow up and down by blowing hot air at 185°C from bottom to top for 20 minutes, and then again for 20 minutes by blowing it from top to bottom, thereby producing a superabsorbent resin having a final moisture content of 25 wt% after drying.

[0283] [Table 1A] [Table 1B]

[0284] Test Example For the superabsorbent polymer compositions prepared in the above Examples and Comparative Examples, particle aggregation characteristics, centrifugation retention capacity (CRC), absorbency under pressure (AUP), water absorption rate, and effective water absorption capacity were measured by the following methods, and the results are shown in Tables 3 and 4 below. Unless otherwise stated, all the processes for the evaluation of the physical properties below were carried out in a constant temperature and humidity room (23±2°C, relative humidity 45±10%), and the measurement data was the average value of three measurements to prevent measurement errors. In addition, in the evaluation of the physical properties below, saline or salt water means a 0.9 wt% sodium chloride (NaCl) aqueous solution.

[0285] (1) Evaluation of particle aggregation characteristics (i) 1,000 g of the unneutralized polymer (water content: 70 wt%) of Step 1 produced in each of the Examples and Comparative Examples was prepared. (ii) Next, 0.36 g of the additive of Formula 1 or the corresponding comparative compound was dispersed in 17.54 g of water at 80° C. (preparation of a 2.04 wt% aqueous dispersion), which was then mixed with 300 g of the polymer obtained in step 1.

[0286] The additives in step 2 or the corresponding comparative compounds were mixed in the form of an aqueous solution according to the type and content used in each Example and Comparative Example.

[0287] (iii) 300 g of the mixture was put into a Mincer equipped with a 3 mm Ψ hole and a 5T thick perforated plate and pulverized.

[0288] (iv) The pulverized material was subjected to a macroscopic evaluation of aggregation based on the discharge time, discharge amount, and the evaluation criteria in Table 2 below. The results are shown in Table 3.

[0289] In this case, the discharge time means the time (seconds) it takes for 200 g of ground material to be discharged from the mincer, and the more agglomeration is alleviated, the shorter the discharge time becomes.

[0290] The discharge amount means the ratio (wt%) of the content discharged through the outlet to the 300 g of the mixture input after the completion of the step (iii). As the agglomeration is alleviated, the amount of lumps remaining inside the mill decreases, and the discharge amount increases.

[0291] Moreover, photographs illustrating the evaluation items of ◯ and X in the macroscopic aggregation evaluation are shown in Figure 2(a) and (b), respectively.

[0292] [Table 2]

[0293] [Table 3]

[0294] 2, it was confirmed that when the unneutralized polymer and the additive of Chemical Formula 1 of the present application are added and pulverization is performed, the aggregation between particles after pulverization is suppressed, and the discharge time is short and the discharge amount is excellent, compared to when the additive is not used or a compound with a structure that does not match the additive is used. In addition, it was confirmed that the adhesive force and cohesive force of the mixture added to the mixer are reduced by the additive of Chemical Formula 1 of the present application, and more than 80% of the discharged material is discharged in the form of particles of 1 cm when evaluated with the naked eye.

[0295] (2)Centrifuge Retention Capacity (CRC) The water retention capacity of each resin composition in terms of the water absorption capacity under no load was measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP241.3.

[0296] Specifically, the highly water-absorbent resin compositions obtained in the Examples and Comparative Examples were classified using sieves of #30-50 to obtain resins. 0(g) (about 0.2 g) was uniformly placed in a nonwoven envelope, sealed, and then immersed in physiological saline (0.9 wt%) at room temperature. After 30 minutes, the water was removed from the envelope at 250 G for 3 minutes using a centrifuge, and the mass of the envelope W 2 The mass W (g) was measured after the same procedure was performed without using the resin. 1 (g) was measured.

[0297] Using the obtained masses, the CRC (g / g) was calculated according to the following formula 1, and the results are shown in Table 4.

[0298] [Formula 1] CRC(g / g) = {[W 2 (g)-W 1 (g)] / W 0 (g)}-1

[0299] (3) Absorbency under Pressure (AUP) The water absorbency at a pressure of 0.7 psi of each of the superabsorbent resin compositions of the above Examples and Comparative Examples was measured by EDANA method WSP242.3.

[0300] First, when measuring the water absorption capacity under pressure, the resin-classified powder used in the CRC measurement was used.

[0301] Specifically, a stainless steel wire mesh of 400 mesh was attached to the bottom of a plastic cylinder having an inner diameter of 25 mm. The water-absorbent resin composition W was placed on the wire mesh under conditions of room temperature and humidity of 50%. 0 The piston that can uniformly apply a load of 0.7 psi to the surface of the sample is slightly smaller than 25 mm in outer diameter, has no gap with the inner wall of the cylinder, and is designed so that the up and down movement is not hindered. At this time, the weight W 3 (g) was measured.

[0302] A glass filter with a diameter of 90 mm and a thickness of 5 mm was placed inside a petroleum dish with a diameter of 150 mm, and physiological saline solution consisting of 0.9% by weight of sodium chloride was placed at the same level as the upper surface of the glass filter. A sheet of filter paper with a diameter of 90 mm was placed on top of the glass filter. The measuring device was placed on the filter paper, and the liquid was absorbed under a load for one hour. After one hour, the measuring device was lifted up and its weight W 4 (g) was measured.

[0303] Using the obtained masses, the water absorption capacity under pressure (g / g) was calculated according to the following formula 2. The results are shown in Table 4.

[0304] [Formula 2] AUP(g / g) = [W 4 (g)-W 3 (g)] / W 0 (g)

[0305] (4)Surface tension:S / T In order to measure the surface tension of the superabsorbent polymer compositions of the Examples and Comparative Examples, 0.5 g of each superabsorbent polymer composition was added to 40 mL of 0.9% salt water, and the mixture was stirred at 350 rpm for 3 minutes. After the stirring was stopped, salt water containing the swollen superabsorbent polymer was obtained. The salt water was used as a measurement sample, and the surface tension of each superabsorbent polymer composition was measured using a surface tension meter (product name: Force Tensiometer-K100, manufactured by KRUSS Co., Ltd.), and the results are shown in Table 4.

[0306] (5) Bulk density (BD) 100g of the superabsorbent resin composition of the above-mentioned Examples and Comparative Examples was poured through a standard flow rate measuring device orifice and received in a container with a volume of 100ml, and the superabsorbent resin composition was scraped off so as to be horizontal, and the volume of the superabsorbent resin composition was adjusted to 100ml, and then the weight of only the superabsorbent resin composition excluding the container was measured.The weight of only the superabsorbent resin composition was then divided by the volume of the superabsorbent resin composition, 100ml, to obtain the apparent density corresponding to the weight of the superabsorbent resin composition per unit volume.

[0307] (6) Amount of fine powder generated The amount of fine powder generated from the superabsorbent polymer compositions of the above Examples and Comparative Examples was calculated as the ratio of the weight of resin having a particle size of less than 150 μm to the total weight after passing the produced superabsorbent polymer compositions once through a coarse grinder (under conditions of 2800 rpm, 0.4 mm clearance, and 1 mm mesh), and the results are shown in Table 4.

[0308] (7) Water absorption rate (Vortex time) The water absorption speed (vortex time) of the superabsorbent resin compositions of the above Examples and Comparative Examples was measured by the following method, and the results are shown in Table 4.

[0309] (i) First, 50 mL of 0.9% salt water was poured into a 100 mL flat-bottomed beaker using a 100 mL mass cylinder. (ii) Next, the beaker was placed in the center of a magnetic stirrer, and then a magnetic bar (diameter 8 mm, length 30 mm) was placed in the beaker. (iii) Thereafter, the stirrer was operated so that the magnetic bar was stirring at 600 rpm, and the lowest part of the vortex generated by stirring was brought into contact with the magnetic bar. (iv) After confirming that the temperature of the salt water in the beaker had reached 24.0°C, 2±0.01 g of a superabsorbent polymer composition sample was added while simultaneously starting a stopwatch. The time until the vortex disappeared and the liquid surface became completely horizontal was measured in seconds, and this was regarded as the water absorption rate.

[0310] [Table 4]

[0311] Referring to Table 4, when a superabsorbent polymer composition is prepared by adding an unneutralized polymer and the additive of the present invention represented by formula 1, the aggregation between particles after pulverization is suppressed compared to when no additive is used, when a compound with a different structure is used, or when the additive is mixed with a neutralized hydrogel polymer, and a composition containing superabsorbent polymer particles of a desired particle size can be prepared without an additional pulverization process after drying, thereby reducing the amount of fine powder. As a result, it can be confirmed that the superabsorbent polymer composition of this example has a significantly faster water absorption rate than the comparative example, and has water retention capacity and pressurized water absorption capacity at the same level or higher, while at the same time exhibiting a high apparent density without a decrease in surface tension.

Claims

1. Superabsorbent resin particles containing a crosslinked polymer of a water-soluble ethylenically unsaturated monomer having an acidic group and an internal crosslinking agent; and A superabsorbent resin composition comprising an additive represented by the following chemical formula 1: 【Chemistry 1】 In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl, 【Chemistry 2】 where one or more of these is a carbonyl or 【Chemistry 3】 wherein m1, m2, and m3 each independently represent an integer from 1 to 8; 【Chemistry 4】 are each linked to adjacent oxygen atoms, 【Chemistry 5】 is the adjacent R 1 , R 2 and R 3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

2. The additive is at least one selected from the compounds represented by the following formulas 1-1 to 1-14: The highly water-absorbent resin composition according to claim 1: 【Chemistry 6】 【Chemistry 7】 【Chemistry 8】

3. The additive is contained in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. The highly water-absorbent resin composition according to claim 1.

4. The high water absorbent resin particle further includes a surface cross-linked layer formed by additionally cross-linking the cross-linked polymer via a surface cross-linking agent on at least a part of the surface of the high water absorbent resin particle. The highly water-absorbent resin composition according to claim 1.

5. The superabsorbent resin composition comprises: The water absorption rate (vortex time) at 24.0°C by the vortex method is 30 seconds or less. The highly water-absorbent resin composition according to claim 1.

6. The superabsorbent resin composition comprises: Centrifugation retention capacity (CRC) according to EDANA WSP241.3 is 39.0 g / g or more; The highly water-absorbent resin composition according to claim 1.

7. The superabsorbent resin composition comprises: The absorbency under pressure (AUP) at 0.7 psi according to EDANA method WSP242.3 is 24.0 g / g or more; The highly water-absorbent resin composition according to claim 1.

8. A step of cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a polymer (step 1); neutralizing at least a portion of the acidic groups of the polymer (Step 2); (Step 3) preparing base resin particles by atomizing the polymer in the presence of an additive represented by the following formula 1: drying the base resin particles (step 4); Method for producing superabsorbent polymer composition: 【Chemistry 9】 In the above Chemical Formula 1, A 1 , A 2 and A 3 each independently represents a single bond, a carbonyl, 【Chemistry 10】 where one or more of these is a carbonyl or 【Chemistry 11】 wherein m1, m2, and m3 each independently represent an integer from 1 to 8; 【Chemistry 12】 are each linked to adjacent oxygen atoms, 【Chemistry 13】 is the adjacent R 1 , R 2 and R 3 are connected to R 1 , R 2 and R 3 each independently represents hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

9. The step of forming the polymer (step 1) is carried out in a batch type reactor. A method for producing the highly water-absorbent resin composition according to claim 8.

10. The steps 2 and 3 are carried out sequentially, simultaneously, or alternately; A method for producing the highly water-absorbent resin composition according to claim 8.

11. The additive is contained in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. A method for producing the highly water-absorbent resin composition according to claim 8.

12. The step of preparing the base resin particles (step 3) is carried out using an atomizer, The atomization device is a body portion including a transfer space therein through which a mixture of a polymer and an additive is transferred; A screw member rotatably provided within the transfer space to move the mixture; a drive motor for providing a rotational drive force to the screw member; a cutter member provided in the body portion, the cutter member including a perforated plate having a number of holes formed therein, the cutter member discharging the mixture to the outside of the body portion while pulverizing the mixture, A method for producing the highly water-absorbent resin composition according to claim 8.

13. Steps 2 and 3 are carried out sequentially, simultaneously, or alternately; Steps 2 and 3 are carried out using an atomizer; The atomization device is a body portion including a transfer space therein through which a mixture of a polymer and an additive is transferred; A screw member rotatably provided within the transfer space to move the mixture; a drive motor for providing a rotational drive force to the screw member; a cutter member provided in the body portion, the cutter member including a perforated plate having a number of holes formed therein, for discharging the mixture to the outside of the body portion while pulverizing the mixture; and a neutralizer injection nozzle provided inside the body portion. A method for producing the highly water-absorbent resin composition according to claim 8.

14. In the atomization device, A neutralizing agent is injected into the body through the neutralizing agent injection nozzle to neutralize at least a part of the acidic groups of the polymer having acidic groups in the mixture. A method for producing the highly water-absorbent resin composition according to claim 13.

15. The hole size formed in the perforated plate is 0.1 mm to 30 mm. A method for producing the highly water-absorbent resin composition according to claim 12.

16. The step of drying the base resin particles (step 4) is carried out in a moving type. A method for producing the highly water-absorbent resin composition according to claim 8.

17. The step of drying the base resin particles (step 4) comprises: This is carried out using a moving type dryer such as a horizontal-type mixer, a rotary kiln, a paddle dryer, or a steam tube dryer; A method for producing the highly water-absorbent resin composition according to claim 8.

18. The moisture content of the superabsorbent resin particles obtained in the step of drying the base resin particles (step 4) is 10% by weight to 20% by weight. A method for producing the highly water-absorbent resin composition according to claim 8.

19. The method further includes a step of forming a surface cross-linked layer on at least a part of the surface of the superabsorbent resin particles prepared in step 4 in the presence of a surface cross-linking agent. A method for producing the highly water-absorbent resin composition according to claim 8.

Citation Information

Patent Citations

  • Absorbing resin particle and manufacturing method thereof

    JP2011190426A

  • Surface crosslinking method and production method of water-absorbing resin

    JP2019052285A

  • Highly water-absorbent resin and method for producing the same

    JP2021504519A

  • Highly water-absorbent resin and method for producing the same

    JP2021505704A

  • Highly water-absorbent resin and method for producing the same

    JP2021505716A