Low-temperature lithium-ion battery electrolyte, its manufacturing method, and lithium-ion battery

The low-temperature lithium-ion battery electrolyte improves discharge capacity and stability by using fluorocarboxylic acid ester, fluorocarbonate ester, and 1,3-dioxane solvents with lithium bis(trifluoromethanesulfonyl)imide, addressing the low-temperature performance challenges of lithium-ion batteries.

JP2024536425AActive Publication Date: 2024-10-04HUBEI WANRUN NEW ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024521067
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-24
Filing Date
2022-12-26
Publication Date
2024-10-04
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges in low-temperature energy storage performance and cycle stability, particularly with carbonate-based electrolytes that solidify at low temperatures and have high impedance, limiting their application in electric vehicles and other low-temperature environments.

Method used

A low-temperature lithium-ion battery electrolyte comprising fluorocarboxylic acid ester as the main solvent, fluorocarbonate ester and 1,3-dioxane as co-solvents, combined with lithium bis(trifluoromethanesulfonyl)imide, to improve ionic conductivity and form stable interfacial phases at the electrode interfaces.

Benefits of technology

The electrolyte significantly enhances discharge specific capacity and capacity retention rate of lithium iron phosphate batteries under low-temperature conditions, achieving a discharge specific capacity of 90mAh/g at -30°C and maintaining stability over 50 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536425000001_ABST
    Figure 2024536425000001_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium ion batteries, and in particular to a low-temperature type lithium ion battery electrolyte and its manufacturing method, and a lithium ion battery. The low-temperature type lithium ion battery electrolyte of the present invention includes an electrolyte salt and an organic solvent, and the organic solvent includes a fluorocarboxylic acid ester, a fluorocarbonic acid ester, and 1,3-dioxane. The fluorocarboxylic acid ester has a low freezing point and is suitable as a low-temperature electrolyte solvent, and the fluorocarbonic acid ester is mixed with the fluorocarboxylic acid ester as a co-solvent to adjust the low-temperature performance and film-forming property of the electrolyte, and the introduction of 1,3-dioxane with a low freezing point and low viscosity obviously reduces the impedance of the battery. The low-temperature type lithium ion battery electrolyte of the present invention can effectively improve the low-temperature lithium ion conductivity, which is advantageous for the low-temperature capacity of a lithium ion battery, and can especially improve the discharge specific capacity and capacity retention rate of a lithium iron phosphate lithium ion battery under low-temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese invention patent application, application number 202211016568.3, filed on August 24, 2022, entitled "Low temperature lithium ion battery electrolyte and its manufacturing method, and lithium ion battery," the disclosure of which is incorporated herein by reference.

[0002] The present invention relates to the technical field of lithium ion batteries, and in particular to a low-temperature type lithium ion battery electrolyte and a manufacturing method thereof, and a lithium ion battery. [Background technology]

[0003] As the application range of lithium-ion batteries (LIBs) expands day by day, especially in the fields of electric vehicles, aerospace, and defense industries, there are higher requirements for the low-temperature charge-discharge performance of the batteries. However, there are still many technical challenges to improve the energy storage performance and cycle stability of lithium-ion batteries at low temperatures. In particular, the carbonate-based commercial electrolyte is prone to solidification at low temperatures and has high impedance, which limits the further application of lithium-ion batteries in the field of low-temperature electric vehicles.

[0004] Therefore, optimizing the electrolyte has become one of the research focuses for improving the low-temperature performance of lithium-ion batteries. Among many positive electrode materials, lithium iron phosphate is widely used in the electric vehicle field due to its high safety performance and low cost, but due to its low conductivity, it is waiting for improvement of its low-temperature performance. Therefore, lithium iron phosphate is used as a lithium-ion positive electrode, and research on the modification of low-temperature electrolyte for its suitability has been carried out, which has a certain market prospect.

[0005] Patent 202111011044.0 discloses a low-temperature lithium-ion battery electrolyte for a high-nickel ternary positive electrode, specifically comprising lithium difluorooxalate borate LiDFOB and a mixed solvent, the concentration of lithium difluorooxalate LiDFOB being 0.8-1.5 mol / L, and the mixed solvent being linear carbonate, cyclic carbonate and γ-butyrolactone.

[0006] This technical solution lowers the melting point of the electrolyte by adding gamma-butyrolactone, a low-melting organic solvent, to the basic solvent carbonate, thereby improving the low-temperature performance of lithium-ion batteries and improving the electrochemical performance of lithium-ion batteries under low-temperature conditions. However, there is still room for improvement in the low-temperature resistance of lithium-ion batteries.

[0007] The present invention has been made in view of these points. Summary of the Invention [Problem to be solved by the invention]

[0008] A first object of the present invention is to provide a low-temperature type lithium ion battery electrolyte that can effectively improve the discharge specific capacity and capacity retention rate of a lithium ion battery under low-temperature conditions.

[0009] The second object of the present invention is to provide a method for preparing said low-temperature type lithium ion battery electrolyte, which has simple steps, is easy to operate, and is convenient for practical popularization and large-scale application.

[0010] A third object of the present invention is to provide a lithium ion battery containing the above-mentioned low-temperature lithium ion battery electrolyte and having excellent electrochemical performance under low-temperature conditions. [Means for solving the problem]

[0011] In order to achieve the above object of the present invention, the following technical solutions are particularly adopted.

[0012] The present invention provides a low-temperature type lithium ion battery electrolyte, comprising an electrolyte salt and an organic solvent, The organic solvent includes a fluorocarboxylic acid ester, a fluorocarbonic acid ester, and 1,3-dioxane.

[0013] Additionally, the fluorocarboxylic acid ester includes diethyl fluoromalonate.

[0014] Furthermore, the fluorocarbonate includes fluoroethylene carbonate.

[0015] Furthermore, the electrolyte salt includes lithium bis(trifluoromethanesulfonyl)imide and / or lithium trifluoromethanesulfonylimide.

[0016] Preferably, the electrolyte salt comprises lithium bis(trifluoromethanesulfonyl)imide.

[0017] Furthermore, in the low-temperature lithium-ion battery electrolyte, the volume percentage of the fluorocarboxylic acid ester is >40%.

[0018] Preferably, in the low temperature type lithium ion battery electrolyte, the volume percentage of the fluorocarboxylic acid ester is 50% to 70%.

[0019] Further, the volume ratio of the fluorocarboxylate, the fluorocarbonate and the 1,3-dioxane is 90-40:5-50:5-30.

[0020] Preferably, the volume ratio of the fluorocarboxylate, the fluorocarbonate and the 1,3-dioxane is 55-65:15-25:15-25.

[0021] Furthermore, in the low-temperature type lithium ion battery electrolyte, the concentration of the electrolyte salt is 1.0 to 5.0 mol / L.

[0022] Preferably, in the low-temperature lithium-ion battery electrolyte, the concentration of the electrolyte salt is 1.5 to 2.5 mol / L.

[0023] The present invention further provides a method for preparing the low-temperature type lithium ion battery electrolyte as mentioned above, in which the low-temperature type lithium ion battery electrolyte is obtained after uniformly mixing an organic solvent and an electrolyte salt.

[0024] The present invention further provides a lithium-ion battery comprising a low temperature lithium-ion battery electrolyte as described above.

[0025] Furthermore, the positive electrode material of the lithium ion battery is lithium iron phosphate. Effect of the Invention

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] (1) The low-temperature lithium-ion battery electrolyte of the present invention uses a fluorocarboxylate as a main solvent, a fluorocarbonate and 1,3-dioxane as co-solvents, and is combined with lithium bis(trifluoromethanesulfonyl)imide, thereby significantly improving the low-temperature lithium ion conductivity and being advantageous for enabling a lithium ion battery to exhibit its capacity at low temperatures.

[0028] (2) The low-temperature lithium-ion battery electrolyte of the present invention uses lithium bis(trifluoromethanesulfonyl)imide as an electrolyte salt, which can form a stable inorganic component interfacial phase at the positive electrode, and fluoroethylene carbonate can form a stable inorganic component interfacial phase at the negative electrode, thereby significantly improving the cycle stability of the battery at low temperatures (-30°C).

[0029] (3) The low-temperature lithium-ion battery electrolyte of the present invention can significantly improve the discharge specific capacity and capacity retention rate of a lithium iron phosphate lithium-ion battery under low-temperature conditions. A LiFePO4 / Li battery assembled using the electrolyte can achieve a 0.2C discharge specific capacity of 90mAh / g in a low-temperature environment of -30°C. [Brief description of the drawings]

[0030] In the following, in order to more clearly describe the specific embodiments of the present invention or the technical solutions in the prior art, drawings required for the description of the specific embodiments or the prior art are briefly introduced. It is obvious that the drawings in the following description are some embodiments of the present invention, and those skilled in the art can obtain other drawings based on these drawings without any creative efforts. [Figure 1] 1 is a graph comparing the charge / discharge voltages at 2.7 to 4.2 V and the specific discharge capacity at −30° C. of batteries fabricated using the low-temperature lithium ion battery electrolyte of Example 7 of the present invention and the lithium ion battery electrolyte of Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The technical solutions of the present invention will be described below clearly and completely with reference to the drawings and specific embodiments. Those skilled in the art will understand that the examples described below are only some of the examples of the present invention, not all of the examples, and are merely for illustrating the present invention and should not be construed as limiting the scope of the present invention.

[0032] Based on the examples in the present invention, all other examples made by those skilled in the art without creative effort are within the scope of protection of the present invention. If no specific conditions are specified in the examples, they are in accordance with normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified, the reagents and equipment used are all normal and commercially available.

[0033] Hereinafter, a low-temperature type lithium ion battery electrolyte, a method for producing the electrolyte, and a lithium ion battery according to the embodiments of the present invention will be specifically described.

[0034] In some embodiments of the present invention, a low-temperature lithium-ion battery electrolyte is provided, the low-temperature lithium-ion battery electrolyte comprising an electrolyte salt and an organic solvent, The organic solvent includes a fluorocarboxylic acid ester, a fluorocarbonic acid ester, and 1,3-dioxane.

[0035] The low-temperature lithium-ion battery electrolyte of the present invention uses a fluorocarboxylate as a main solvent and a fluorocarbonate and 1,3-dioxane as co-solvents, and thus can effectively improve low-temperature lithium ion conductivity and is advantageous for enabling a lithium ion battery to exhibit its capacity at low temperatures.

[0036] Fluorocarboxylic acid esters have a low melting point, and the freezing point of the carboxylic acid ester can be further lowered by the fluoro. Since the fluorocarboxylic acid ester has a low melting point and lowers the freezing point of the electrolyte itself, the ionic conductivity of the electrolyte at low temperatures can be improved, thereby improving the low-temperature performance of the battery. In addition, the introduction of elemental fluorine is advantageous in improving interface performance.

[0037] Since fluorocarboxylic acid ester has poor film-forming properties, a fluorocarbonic acid ester is selected as a co-solvent and mixed with the fluorocarboxylic acid ester to adjust the film-forming properties of the electrolyte.

[0038] The introduction of 1,3-dioxane (DOL), which has a low freezing point and low viscosity, significantly reduces the impedance of lithium-ion batteries, thereby improving the discharge specific capacity and capacity retention rate of lithium-ion batteries, especially lithium iron phosphate lithium-ion batteries, under low temperature conditions.

[0039] In some embodiments of the present invention, the fluorocarboxylic acid ester comprises diethyl fluoromalonate.

[0040] Diethyl fluoromalonate (DEFM) is used as a solvent for the electrolyte. The bond energy between diethyl fluoromalonate and lithium ions is low, which is advantageous for the process of lithium ion insertion and removal at low temperatures.

[0041] In some embodiments of the present invention, the fluorocarbonate comprises fluoroethylene carbonate (4-Fluoro-1,3-dioxolan-2-one, FEC).

[0042] In some embodiments of the present invention, the electrolyte salt comprises lithium bis(trifluoromethanesulfonyl)imide and / or lithium trifluoromethanesulfonylimide, preferably the electrolyte salt comprises lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0043] Lithium bis(trifluoromethanesulfonyl)imide can be dissolved in a solvent at a high concentration, and has a high HOMO level and a low LUMO level, and decomposes at the positive electrode / negative electrode-electrolyte interface during the first charge to form an interfacial film with a high content of inorganic components, which can significantly improve the cycle stability of the battery at low temperatures (-30°C). Lithium bis(trifluoromethanesulfonyl)imide at an appropriate concentration has high ionic conductivity and can provide a stable fluorine-containing interfacial film.

[0044] HOMO is the highest occupied molecular orbital, and the higher the HOMO level, the easier the material will lose electrons. For electrolytes, the HOMO level can be used to determine the order of decomposition of each component during charging, meaning that the higher the HOMO level of a component, the easier it is to be oxidized to form a positive electrode electrolyte interfacial film, thereby preventing other components from coming into direct contact with the electrolyte during the subsequent charging and discharging processes, and suppressing side reactions at the positive electrode electrolyte interface.

[0045] The LUMO level is the lowest unoccupied orbital of a molecule, and the lower the LUMO level, the easier it is for the material to obtain electrons. For electrolytes, the LUMO level can be used to determine the order of decomposition of each component during the discharge process, meaning that the lower the LUMO level of a component, the easier it is to be reduced and form an interfacial film with the negative electrode electrolyte, thereby preventing direct contact between the electrode and the electrolyte during the subsequent charge and discharge process and suppressing side reactions at the interface.

[0046] The organic solvents of the low-temperature lithium-ion battery electrolyte of the present invention are fluorocarboxylic acid ester, fluoroethylene carbonate, and 1,3-dioxane. The fluorocarboxylic acid ester and fluorocarbonate have low melting points, which can lower the melting point of the electrolyte and improve the ionic conductivity of the electrolyte at low temperatures. The HOMO level of LiFSI is high, which can be preferentially decomposed and formed into a film on the surface of the positive electrode of a lithium-ion battery, improving the stability of the positive electrode-electrolyte interface.

[0047] The LUMO level of fluoroethylene carbonate is low, and it can be preferentially decomposed to form a film on the surface of the negative electrode of a lithium ion battery, improving the stability of the negative electrode-electrolyte interface. Therefore, the electrolyte of the present invention can improve the discharge specific capacity and capacity retention rate of a lithium ion battery at low temperatures (-30°C).

[0048] In some implementations of the invention, the low temperature lithium ion battery electrolyte includes lithium bis(trifluoromethanesulfonyl)imide, diethyl fluoromalonate, fluoroethylene carbonate, and 1,3-dioxane.

[0049] In some implementations of the invention, the volume percentage of fluorocarboxylic acid ester in the low temperature lithium ion battery electrolyte is >40%.

[0050] In some implementations of the present invention, the volume percentage of the fluorocarboxylic acid ester in the low-temperature lithium-ion battery electrolyte is 50% to 70%, and typically, but not limited to, for example, the volume percentage of the fluorocarboxylic acid ester in the low-temperature lithium-ion battery electrolyte is 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69% or 70%, etc., and preferably, the volume percentage of the fluorocarboxylic acid ester in the low-temperature lithium-ion battery electrolyte is 55% to 65%, more preferably 58% to 62%.

[0051] In some embodiments of the present invention, the volume ratio of fluorocarboxylic acid ester, fluorocarbonate and 1,3-dioxane is 90-40:10-50:1-30, and typically but not limited to, for example, the volume ratio of fluorocarboxylic acid ester, fluorocarbonate and 1,3-dioxane is 80:10:10, 70:15:15, 60:20:20, 50:25:25, 40:30:30, 80:10:5, 70:30:10, 60:10:5, 50:10:20, etc., and preferably, the volume ratio of fluorocarboxylic acid ester, fluorocarbonate and 1,3-dioxane is 55-65:15-25:15-25, and more preferably, the volume ratio of fluorocarbonate and 1,3-dioxane is 1:1.

[0052] In some embodiments of the present invention, the low-temperature lithium-ion battery electrolyte has an electrolyte salt concentration of 1.0 to 5.0 mol / L, typically but not limited to, for example, the low-temperature lithium-ion battery electrolyte has an electrolyte salt concentration of 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, 4.5 mol / L, or 5.0 mol / L, and preferably, the low-temperature lithium-ion battery electrolyte has an electrolyte salt concentration of 1.5 to 2.5 mol / L.

[0053] In some embodiments of the present invention, a method for preparing the low-temperature lithium-ion battery electrolyte is further provided, in which the low-temperature lithium-ion battery electrolyte is obtained after uniformly mixing the organic solvent and the electrolyte salt.

[0054] In some embodiments of the present invention, the organic solvent is an anhydrous organic solvent, and the method for producing the anhydrous organic solvent includes adding a water removing agent to the organic solvent and allowing the organic solvent to stand for 2 to 4 days, and preferably, the water removing agent is a molecular sieve having a type number of 3 Å, 4 Å, or 5 Å.

[0055] In some embodiments of the present invention, a lithium ion battery is further provided, comprising the low temperature lithium ion battery electrolyte described above.

[0056] In some embodiments of the present invention, the positive electrode material of the lithium ion battery is lithium iron phosphate.

[0057] In some embodiments of the present invention, a lithium ion battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte solution; Here, the positive electrode sheet is mainly made of a positive electrode active material, a conductive agent, a binder, and a dispersant, the positive electrode active material being LiFePO4, The negative electrode sheet is a lithium sheet, The electrolyte is the low-temperature lithium-ion battery electrolyte.

[0058] In some embodiments of the present invention, the conductive agent comprises conductive carbon black.

[0059] In some embodiments of the present invention, the binder comprises polyvinylidene fluoride.

[0060] In some embodiments of the present invention, the conductive agent comprises N-methyl-2-pyrrolidone.In some embodiments of the present invention, the separator comprises a polypropylene microporous film.

[0061] The LiFePO4 / Li battery assembled using the low-temperature lithium ion battery electrolyte of the present invention has a 0.2C discharge specific capacity of 90mAh / g in a low-temperature environment of -30°C, and can maintain a stable cycle.

[0062] (Examples 1 to 12) The manufacturing method of the low-temperature lithium-ion battery electrolyte in each Example is the same, and only the volume ratio of the solvents DEFM, FEC, and DOL used in the low-temperature lithium-ion battery electrolyte and the concentration of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) are different. The volume ratio of the solvents and the concentration of LiTFSI in each Example are shown in Table 1.

[0063] [Table 1]

[0064] A method for producing a low-temperature lithium-ion battery electrolyte includes the following steps: In a glove box protected by inert gas, diethyl fluoromalonate (DEFM), fluorocarbonate (FEC) and 1,3-dioxane (DOL) are mixed in a volume ratio, after mixing, 3Å molecular sieve desiccant is added, left to stand for 2 days, and then bis(trifluoromethanesulfonyl)imide lithium (LiTFSI) is added, the concentration of bis(trifluoromethanesulfonyl)imide lithium (LiTFSI) is controlled, and the mixture is stirred until it becomes clear. After uniform mixing, a low-temperature type lithium ion battery electrolyte can be obtained. The moisture content in the glove box is less than 0.1 ppm, and the oxygen content is less than 0.1 ppm. The model number of the 3Å molecular sieve desiccant is Alfa L05335-250g.

[0065] (Comparative Examples 1 to 5) The manufacturing method of the lithium ion battery electrolyte in each comparative example is the same, and only the type of organic solvent, the volume ratio, and the type and concentration of the electrolyte salt used in the lithium ion battery electrolyte are different, as specifically shown in Table 2.

[0066] [Table 2]

[0067] Here, EC is ethylene carbonate and DEC is diethyl carbonate.

[0068] A method for producing a lithium ion battery electrolyte includes the steps of: In an inert gas protected glove box, the organic solvent is mixed in a volume ratio, after mixing, 3Å molecular sieve dehydrator is added, left to stand for 2 days, and then electrolyte salt is added and stirred evenly, the concentration of electrolyte salt is controlled, and after uniform stirring, a lithium ion electrolyte solution can be obtained. The moisture content in the glove box is less than 0.1 ppm, and the oxygen content is less than 0.1 ppm. The model number of the 3Å molecular sieve dehydrator is Alfa L05335-250g.

[0069] (Test Example 1) Batteries were assembled using the low-temperature lithium ion battery electrolytes of Examples 1 to 12 and the lithium ion battery electrolytes of Comparative Examples 1 to 5 together with a lithium iron phosphate positive electrode and a lithium negative electrode, and electrochemical tests were performed using the following test methods.

[0070] First, a positive electrode sheet was prepared. The positive electrode active material was LiFePO4, the conductive agent was conductive carbon black (SuperP, Timcal Ltd.), the binder was polyvinylidene fluoride (PVDF, HSV900, Arkema), and the dispersant was N-methyl-2-pyrrolidone (NMP). The mixture was mixed in a mass ratio of LiFePO4:Super P:PVDF = 7:2:1, polished, and applied to an aluminum foil. After drying, roll pressing, and dicing, an electrode sheet was prepared. The active material on the electrode surface was 2 to 4 mg / cm2. 2 Then, in a glove box filled with argon gas, button batteries were fabricated, with a lithium sheet as the negative electrode and a microporous polypropylene film as the separator, and different electrolytes were used to obtain different batteries and conduct tests.

[0071] The electrochemical performance test was performed using a Neware electrochemical tester. The battery was activated by cycling twice at room temperature at 0.2C, then left at -30°C for 2 hours, and then cycled at a low temperature at a current density of 0.2C. The charge / discharge voltage range was 2.7 to 4.2V, and the test results are shown in Table 3. The lithium ion battery electrolyte of Example 1 and the lithium ion battery electrolyte battery of Comparative Example 5 were used to compare the charge / discharge voltages of 2.7 to 4.2V and the discharge specific capacity at -30°C. The lithium ion battery electrolyte battery of Comparative Example 5 was denoted as Baseline, and the low-temperature lithium ion battery electrolyte of Example 7 was denoted as LT-Electrolyte.

[0072] [Table 3]

[0073] As can be seen from FIG. 1, at a low temperature of -30°C, 0.2C multiplication factor, and 50 cycles, the discharge specific capacity and cycle stability of the battery assembled using the low-temperature lithium ion battery electrolyte of the present invention are obviously superior to those of the lithium ion battery electrolyte of Comparative Example 5.

[0074] As can be seen from Table 1, the discharge specific capacity is highest when the electrolyte solvent is a mixed solvent of diethyl fluoromalonate (DEFM), fluorocarbonate (FEC) and 1,3-dioxane (DOL) and the lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0075] Comparing Examples 1 to 12, it can be seen that Example 7 has the greatest effect. At a low temperature of -30°C, the discharge specific capacity of the LiFePO4 / Li battery is 90mAh / g, and the capacity retention rate at 50 cycles is close to 100%, which is far higher than other comparative examples.

[0076] As can be seen from a comparison of Examples 1 to 12, when the solvent components are a mixed solvent of diethyl fluoromalonate (DEFM), fluoroethylene carbonate (FEC) and 1,3-dioxane (DOL), the discharge specific capacity is highest when the occupancy rate of fluoroethylene carbonate is 20% and the occupancy rate of 1,3-dioxane is 20%. This is believed to be because FEC is advantageous for forming an inorganic interface rich in LiF at the negative electrode and is more stable at low temperatures, and the low viscosity of DOL is advantageous for reducing the ionic conductivity of the electrolyte at low temperatures.

[0077] As can be seen from a comparison between Examples 1 to 12 and Comparative Examples 1 to 4, the performance was best when the lithium salt was LiTFSI and the concentration was 2M. This is believed to be because LiTFSI preferentially decomposes to form an inorganic component interfacial film containing F, which is more stable, and the electrolyte has optimal viscosity and conductivity when the concentration is 2M.

[0078] As can be seen from Comparative Examples 1 to 4, in the case where LiTFSI is not contained, the effect of the solvent components being diethyl fluoromalonate (DEFM), fluoroethylene carbonate (FEC) and 1,3-dioxane (DOL) is also superior to that of ordinary carbonate (basic electrolyte), which is believed to be because the above mixed solvent has superior low-temperature conductivity and superior film-forming properties.

[0079] From the above, it can be seen from the comparison that the electrolyte solution using lithium bis(trifluoromethanesulfonyl)imide as the electrolyte salt, diethyl fluoromalonate (DEFM), fluoroethylene carbonate (FEC) and 1,3-dioxane (DOL) as the solvent can obviously improve the discharge specific capacity and capacity retention rate of the LiFePO4 / Li battery in a low temperature environment of -30°C, compared with Comparative Example 5. Here, the discharge specific capacity and cycle stability of the battery are best when DEFM:FEC:DOL=60:20:20 and the LiTFSI concentration is 2M.

[0080] The discharge specific capacity of the assembled LiFePO4 / Li battery at -30℃ is 90mAh / g, which is more stable.

[0081] Finally, it should be noted that the above embodiments are only used to describe the technical solutions of the present invention, and are not intended to limit the technical solutions of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art may still modify the technical solutions described in the above embodiments or equally replace some or all of the technical features thereof, and such modifications or replacements shall not cause the essence of the corresponding technical solutions to depart from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An electrolyte salt and an organic solvent are included, The organic solvent includes a fluorocarboxylic acid ester, a fluorocarbonic acid ester, and 1,3-dioxane. Low temperature lithium-ion battery electrolyte.

2. The fluorocarboxylic acid ester includes diethyl fluoromalonate. The low-temperature type lithium ion battery electrolyte according to claim 1.

3. The fluorocarbonate includes fluoroethylene carbonate. The low-temperature type lithium ion battery electrolyte according to claim 1.

4. the electrolyte salt comprises lithium bis(trifluoromethanesulfonyl)imide and / or lithium trifluoromethanesulfonylimide, Preferably, the electrolyte salt comprises lithium bis(trifluoromethanesulfonyl)imide. The low-temperature type lithium ion battery electrolyte according to claim 1.

5. In the low-temperature lithium-ion battery electrolyte, the volume percentage of the fluorocarboxylic acid ester is greater than 40%; Preferably, in the low-temperature lithium-ion battery electrolyte, the volume percentage of the fluorocarboxylic acid ester is 50% to 70%. The low-temperature type lithium ion battery electrolyte according to claim 1.

6. a volume ratio of the fluorocarboxylate, the fluorocarbonate and the 1,3-dioxane is 90 to 40:5 to 50:5 to 30; Preferably, the volume ratio of the fluorocarboxylic acid ester, the fluorocarbonic acid ester and the 1,3-dioxane is 55 to 65: 15 to 25: 15 to 25. The low-temperature type lithium ion battery electrolyte according to claim 1.

7. In the low-temperature lithium-ion battery electrolyte, the concentration of the electrolyte salt is 1.0 to 5.0 mol / L; Preferably, in the low-temperature lithium-ion battery electrolyte, the concentration of the electrolyte salt is 1.5 to 2.5 mol / L. The low-temperature type lithium ion battery electrolyte according to claim 1.

8. The organic solvent and the electrolyte salt are mixed uniformly to obtain a low-temperature lithium-ion battery electrolyte; The method for producing the low-temperature lithium-ion battery electrolyte according to any one of claims 1 to 7.

9. A low-temperature lithium-ion battery comprising the electrolyte according to any one of claims 1 to 7. Lithium-ion battery.

10. The positive electrode material of the lithium ion battery is lithium iron phosphate.

10. The lithium ion battery of claim 9.

Citation Information

Patent Citations

  • Battery and electrolyte, and battery pack, electronic apparatus, electric vehicle, power storage device and electric power system

    JP2013225388A

  • Nonaqueous electrolytic solution and nonaqueous electrolytic battery using the same

    JP2015195201A

  • Secondary battery

    JP2016131081A

  • Nonaqueous electrolyte solution for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    JP2017208186A

  • Electrolyte, electrochemical device, lithium ion secondary battery, and module

    JP2018106883A