Ester-containing benzoxazine monomers form polybenzoxazine vitrimers with exchangeable bonds, addressing the recyclability issue of thermoset polymers by providing self-healing and reprocessable materials with enhanced properties.
Patent Information
- Application Number
- JP2024521081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-07
- Filing Date
- 2022-10-06
- Publication Date
- 2024-10-04
AI Technical Summary
Existing thermoset polymers, including polybenzoxazines, cannot be recycled or reprocessed due to their permanent molecular structure, leading to environmental waste.
Development of ester-containing benzoxazine monomers that form polybenzoxazine derivative vitrimers through polymerization, allowing for self-healing, reshaping, and recyclability via exchangeable ester bonds and free aliphatic hydroxyl groups.
The resulting vitrimers exhibit thermoset properties like high temperature resistance, high strength, thermal stability, low water absorption, and chemical resistance while enabling recycling and reprocessing.
Smart Images

Figure 2024536430000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to the field of ester-containing benzoxazine derivative vitrimers, and processes for their preparation and use in various applications. [Background technology]
[0002] Composite materials are almost always made from thermosetting resins, which are the materials of choice for many applications due to their dimensional stability, mechanical properties, and creep / chemical resistance. However, as a result of their permanent molecular structure, they cannot be recycled or reprocessed and end up in landfills.
[0003] A chemical approach to address this drawback is the introduction of exchangeable chemical bonds, resulting in dynamic crosslinks. Polymer networks containing such exchangeable bonds are also known as covalent adaptive networks (CANs) (W. Denissen et al. - Wim Denissen, Johan M. Winne, and Filip E. Du Prez, Chem. Sci., 2016, 7, 30-38). CANs can be further classified into two groups, either dissociative or conjugated, depending on the exchange mechanism. First, chemical bonds are first broken and then reformed in a different location. The Diels-Alder reaction is the most common mechanism for dissociative CANs. Second, polymer networks are characterized by a fixed crosslink density that does not depolymerize upon heating. Because covalent bonds are broken only when new bonds are formed, these networks are permanent and dynamic. The first reported conjugated CANs (2005) were based on a light-mediated reaction using, for example, allyl sulfide. Later, a similar exchange mechanism was introduced by using trithiocarbonates and alternative radical generators.
[0004] In 2011, Leibler et al. (D. Montarnal, M. Capelot, F. Tournilhac and L. Leibler, Science, 2011, 334, 965-968) expanded the field of bonded CAN by adding a suitable transesterification catalyst to epoxy / acid or epoxy / anhydride polyester-based networks, resulting in persistent polyester / polyol networks that exhibit a slow decrease in viscosity upon heating. This characteristic of fused silica has not previously been observed in organic polymeric materials. Therefore, the inventors introduced the term vitrimers to these materials.
[0005] Vitrimers represent a third class of polymeric materials due to their exceptional functionality. The dynamic nature of this covalent network results from reversible chemical bonds, allowing the material to be repaired, recycled, and reprocessed like a thermoplastic. These exchange reactions are triggered by an external stimulus, most frequently temperature. The viscosity of vitrimers gradually decreases upon heating, relieving internal stresses while making the network malleable. Network integrity throughout the entire application range ensures mechanical and solvent resistance.
[0006] Following the prototypical vitrimer developed by Leibler et al. (cited above) in 2011, dynamic transesterification reactions have shown great importance over the past decade. These chemical exchanges, induced at high temperatures between ester bonds and hydroxyl groups, are responsible for topological rearrangements. The transesterification mechanism has been implemented in crosslinked networks to engineer self-repairable, recyclable, and reprocessable materials with tunable properties.
[0007] Demongeot et al. (A. Demongeot, R. Groote, H. Goossens, T. Hoeks, F. Tournilhac, and L. Leibler, Macromolecules, 2017, 50(16), 6117-6127) adapted the vitrimer concept to commercially available thermoplastics. Crosslinked polybutylene terephthalate (PBT) vitrimers based on transesterification were prepared by reactive extrusion. In addition to improving manufacturing techniques and the potential scope of these networks, the global environmental situation is prompting the scientific community to promote sustainable polymers derived from naturally occurring raw materials. Altuna et al. (FI Altuna, V. Pettarin, and R. Williams, Green Chem., 2013, 15, 3360-3366) attempted to produce a fully biobased polyester exhibiting properties reminiscent of vitrimers, starting from epoxidized soybean oil and aqueous citric acid. Furthermore, Legrand et al. (A. Legrand and C. Soulie-Ziakovic, Macromolecules, 2016, 49, 5893-5902) developed silica-reinforced epoxy vitrimer nanocomposites with enhanced properties, enabling an expansion of the application scale of vitrimer networks.
[0008] Polybenzoxazines are a new class of thermosetting resins with excellent mechanical and thermal properties. Like many other thermosetting resins, they cannot be remolded, reprocessed, or recycled. Some examples showing reasonable levels of healing ability have been reported (L. Zhang, Z. Zhao, Z. Dai, L. Xu, F. Fu, T. Endo, X. Liu, ACS Macro. Lett. 2019, 8, 5, 506-511; and Arslan M., Kiskan B., Y. Yagci, Sci. Rep. 2017, 7, 5207). However, polybenzoxazines remain a high-performance material class even when they do not exhibit any vitrimer capabilities. Such sustainable vitrimers could expand the use of polybenzoxazines toward smart coatings, reversible adhesives, and even recyclable matrix resins for composites. [Prior art documents] [Non-patent literature]
[0009] [Non-Patent Document 1] W.Denissen et al.-Wim Denissen,Johan M.Winne and Filip E.Du Prez,Chem.Sci.,2016,7,30-38 [Non-patent document 2] D.Montarnal, M.Capelot, F.Tournilhac and L.Leibler,Science,2011,334,965-968 [Non-patent document 3] A. Demongeot, R. Groote, H. Goossens, T. Hoeks, F. Tournilhac and L. Leibler, Macromolecules, 2017, 50(16), 6117-6127 [Non-patent document 4] FIAltuna, V.Pettarin and R.Williams,Green Chem.,2013,15,3360-3366 [Non-Patent Document 5] A.Legrand and C.Soulie-Ziakovic,Macromolecules,2016,49,5893-5902 [Non-patent document 6] L. Zhang, Z. Zhao, Z. Dai, L. Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has the technical problem of providing a solution to at least one of the drawbacks of the prior art cited above.
[0011] The present invention relates to ester-containing benzoxazine monomers of formula (I):
[0012] [ka]
[0013] where R is a linear or branched C1-C 20 Alkyl groups, preferably C1-C 12 alkyl groups, more preferably C1-C6 alkyl groups, optionally containing heteroatoms, selected from the group consisting of cyclo(C3-C6 alkyl) groups, heterocyclo(C3-C6 alkyl) groups, where the heteroatoms are N, S, Si and O, linear or branched C2-C 12 , preferably a C2-C6 alkenyl group, a substituted or unsubstituted straight or branched C2-C 12 , preferably a C2-C6 alkynyl group, a linear or branched C1-C6 alkyl or C2-C6 alkenyl substituted or unsubstituted phenyl group, -(CH2) n3 -phenyl groups (wherein n3 is an integer from 1 to 10), siloxane groups; R1 is the following formula 2.
[0014] [ka] R2 is the following formula 3.
[0015] [ka]
[0016] R p is H, linear or branched C1-C 20 , preferably C1 to C 12 , alkyl or alkoxy group, linear or branched C2-C 12 , preferably a C2-C6 alkenyl group or alkyleneoxy group, a substituted or unsubstituted linear or branched C2-C 12 , preferably C2 to C6 alkynyl groups, linear or branched C1 to C6, preferably C1 to C4, alkyl or C2 to C6, preferably C2 to C4 alkenyl substituted or unsubstituted phenyl groups, and the following formula 4:
[0017] [ka]
[0018] where: R1 and R2 in formula (I) are different; x1, x2, and x p are independently between 0 and 1; y1 = 1 - x1; y2 = 1 - x2y p =1-x p and x1, x2 and x p are both non-zero; p is 1 to 100; R1', R2', and R p' is independently selected from the group consisting of: -C-linear or branched C1-C6 alkyl or alkoxy groups, -C-linear or branched C2-C6 alkenyl or alkyleneoxy groups, -C-substituted or unsubstituted linear or branched C2-C6 alkynyl groups, and -C-linear or branched C1-C6 alkyl or C2-C6 alkenyl substituted or unsubstituted phenyl groups; R p '' is selected from the group consisting of a linear or branched C1-C6 alkyl or alkoxy group, a linear or branched C2-C6 alkenyl or alkyleneoxy group, a substituted or unsubstituted linear or branched C2-C6 alkynyl group, and a linear or branched C1-C6 alkyl or C2-C6 alkenyl substituted or unsubstituted phenyl group; R * is selected from the group consisting of linear or branched C1-C6 alkyl or alkoxy groups, cyclo(C3-C6 alkyl) groups, and heterocyclo(C3-C6 alkyl) groups, where the heteroatoms are selected from N, Si, S, and O, linear or branched C2-C6 alkenyl or alkyleneoxy groups, substituted or unsubstituted linear or branched C2-C6 alkynyl groups, linear or branched C1-C6 alkyl or C2-C6 alkenyl substituted or unsubstituted phenyl groups, —(CH2)n3-phenyl groups, and —(CH2)n3-O—(CH2)n4 groups, where n3 and n4 are independently integers from 1 to 10; R ** is R * is the same as O-, N-, Si- or S-(CH2) n3 -CH-(CH3)2 group, O-, N-, Si or S-(CH2) n3 -(CHZ) n4 -(CH3)2 group, O-, N-, Si- or S-(CH2) n3 -(CHZ) n4 -(CH2) n3 -CH3 group, O-, N-, Si- or S-(CHZ) n4 -(CH2) n3 -CH3 group, O-, N-, Si- or S-(CHZ) n4-[(CH2) n3 -CH3]2 group and O-substituted or unsubstituted C2-C6 straight or branched chain alkynyl groups, -(CH2) n3 -C≡N, polycyclic aromatic or heteroaromatic hydrocarbons, e.g., naphthalene, anthracene, fluorene, phenanthrene, including members optionally substituted with linear or branched C1-C6 alkyl or alkoxy groups, cyclo(C3-C6 alkyl), heterocyclo(C3-C6 alkyl), where the heteroatoms are selected from the group consisting of N, S, Si, and O, linear or branched C2-C6 alkenyl or alkyleneoxy groups, or substituted or unsubstituted wherein n3 and n4 are independently an integer of 1 to 10; Z is selected from the group consisting of a linear or branched C1 to C6 alkyl group or alkoxy group, a linear or branched C2 to C6 alkenyl group or alkyleneoxy group, and a linear or branched C1 to C6 alkyl or C2 to C6 alkenyl substituted or unsubstituted phenyl group, and at least one O atom is present or absent between two adjacent Cs; R *** is selected from the group consisting of H, OH, and O-linear or branched C1-C6 alkyl groups, 15 Alkyl group or C2-C 15 or one of the following alkenyl groups:
[0019] [ka]
[0020] The ester-containing benzoxazine monomers of the present invention are advantageously suitable for obtaining polybenzoxazine derivative vitrimers, which undergo polymerization with benzoxazine ring-opening and self-polymerization under heating to give polybenzoxazine derivative vitrimers. Depending on the specific monomer starting product, the vitrimers of the present invention exhibit self-repair, reshapeability, reworkability, and recyclability. In the remainder of this specification, benzoxazine vitrimers always refer to the polymerized form of the ester-linked benzoxazine monomers.
[0021] The properties of the polybenzoxazine derivative vitrimers are closely related to the properties of the ester-containing benzoxazine monomers.
[0022] As can be seen from formula (I), the monomer contains benzoxazine ring moieties that allow the monomer to crosslink upon heating, and the exchangeable ester bonds formed after crosslinking facilitate reprocessing of the resulting benzoxazine vitrimers. Benzoxazines impart thermoset properties such as high temperature and flammability capabilities, high strength, thermal stability, low water absorption, chemical resistance, low melt viscosity, and near-zero shrinkage.
[0023] The presence of ester linkages and free aliphatic hydroxyl groups is essential for the formation of a dynamic and reversible network of benzoxazine derivative vitrimers, allowing for recycling, reshaping, and reprocessing of the material. Hydroxyl-terminated amines close the oxazine ring, enabling transesterification. Therefore, the essential characteristics of the monomers of the present invention depend on the benzoxazine-containing moieties, ester linkages, and free aliphatic hydroxyl groups. The Tg of such polybenzoxazines can range from 25°C to 300°C.
[0024] x1, x2, and x p The values of x1, x2, and x can independently range from 0 to 1. p are not all 0, and y1, y2, and y p The values of are independently 1-x1, 1-x2 and 1-x pand more preferably between 0.5 and 1.
[0025] Preferably, R * represents a linear or branched C1-C4 alkyl or alkoxy group, a linear or branched C2-C4 alkenyl or alkyleneoxy group, an unsubstituted linear or branched C2-C4 alkynyl group, an unsubstituted phenyl group and a (CH2)n3-phenyl group, -(CH2) n3 -O-(CH2)n4 (wherein n3 and n4 are independently integers from 1 to 6);
[0026] More preferably, R * may be selected from the group consisting of —CH, —(CH)—CH, —(CH)—CH—[(CH)—CH], —C(CH), —(CH)—(CHH), —(CH)—CH═CH, —(CH)—C≡CH, —(CH)—O—(CH) (wherein n and n are independently integers from 1 to 4), phenyl, and —(CH)-phenyl.
[0027] Preferably, R ** is R * is the same as O-, N-, Si- or S-(CH2) n 3-CH-(CH3)2 group, O-, N-, Si- or S-(CH2) n3 -(CHZ) n4 -(CH3)2 group, O-, N-, Si- or S-(CH2) n3 -(CHZ) n4 -(CH2) n3 -CH3 group, O-, N-, Si- or S-(CHZ) n4 -(CH2) n3 -CH3 group, O-, N-, Si- or S-(CHZ) n4 -[(CH2) n3 -CH3]2 group and O-substituted or unsubstituted C2-C4 straight or branched chain alkynyl groups, -(CH2) n3and n3 and n4 are independently integers from 1 to 6, and Z is as defined above.
[0028] More preferably, R ** is the group R * or CH, -(CH) n3 -CH3, -(CH2) n3 -CH-[(CH2) n4 -CH3]2, -C(CH3)3, -(CH2) n3 -(C6H5), -(CH2) n3 -CH=CH2, -(CH2) n3 -C≡CH, O-(CH2) n3 -C≡CH, O-(CH2) n3 -C≡N,(CH2) n3 -C≡N and -(CH2) n3 -substituted or unsubstituted furan, phenyl (wherein n3 and n4 are independently integers from 1 to 4). R *** may be selected from the group consisting of H, OH, and O-linear or branched C1-C4 alkyl groups, 10 Alkyl group or C2-C 10 or one of those shown below in Formula 6.
[0029] [ka]
[0030] R *** is preferably selected from the group consisting of H, OH, and O-linear or branched C1-C3 alkyl groups, and may further include a linear or branched C1-C6 alkyl group or a C2-C6 alkenyl group or one of the groups shown in Formula 7 below, more preferably R *** is H.
[0031] [ka]
[0032] The term "substituted" as defined above relates to the presence of several straight or branched alkyl groups at C1 to C6.
[0033] The present invention also relates to a process for synthesizing an ester-containing benzoxazine monomer of formula (I), comprising the steps of:
[0034] [ka]
[0035] [ka]
[0036] [ka]
[0037] [ka]
[0038] x1, x2, x p and y1, y2, y p represents the ratio between the benzoxazine groups when prepared from the amino alcohol and other amine(s). In other words, x1, x2, x p and y1, y2, and yp can be defined as follows:
[0039]
number
[0040] Here, the number 2 shown below is the number of amino alcohols per R group.
[0041]
number
[0042] The number 3 shown below represents the number of amines (excluding the number of amino alcohols) per R group.
[0043]
number
[0044] The number 4 shown below is the total number of amino groups per R group.
[0045]
number
[0046] The number 5 shown below is the number of amino alcohols per R2 group.
[0047]
number
[0048] The number 6 shown below represents the number of amines (excluding the number of amino alcohols) per R2 group.
[0049]
number
[0050] The number 7 shown below is the total number of amino groups per R2 group.
[0051]
number
[0052] Here, the following number 8 is R p is the number of amino alcohols per group.
[0053]
number
[0054] The following number 9 is R p Indicates the number of amines (excluding the number of amino alcohols) per group.
[0055]
number
[0056] The following number 10 is R p is the total number of amino groups per group.
[0057]
number
[0058] The ester-containing benzoxazine monomer of the present invention is advantageously suitable for obtaining a polybenzoxazine derivative vitrimer by polymerization accompanied by benzoxazine ring-opening and self-polymerization under heating.
[0059] Applicants have shown that certain starting reactants provide ester-containing benzoxazine monomers which, after polymerization, give polybenzoxazine derivative vitrimers containing polymerized benzoxazine.
[0060] The benzoxazine ring, resulting from the reaction of certain compounds (II)-(VII), allows the material to crosslink (process) upon heating, and the exchangeable and reversible ester bonds and free aliphatic hydroxyl groups aid in reprocessing. The benzoxazine ring moiety imparts thermoset properties such as high-temperature and flammability performance, high strength, thermal stability, low water absorption, chemical resistance, low melt viscosity, and near-zero shrinkage.
[0061] The phenolic acid derivative (formula (II)) may more preferably be selected from the group consisting of mono-, di-, tri-hydroxybenzoic acid derivatives, anacardic acid derivatives, hydroxycinnamic acid derivatives, aliphatic X-hydroxyphenyl acid derivatives (X is 2-4), aliphatic diphenolic acid derivatives, or mixtures thereof.
[0062] The most preferred aliphatic mono-, di-, tri-hydroxybenzoic acid derivatives may be of formula (VIII):
[0063] [ka]
[0064] In the formula, R' is omitted, and the R1 to R5 groups are R *** wherein one of R1 to R5 is a hydroxyl group, at least one H is in the phenolic ortho position, and the remainder are as defined above.
[0065] In particular, in formula (VIII), at least one combination of R1 to R5 may be selected from the group consisting of: R1=OH, R2=H, R3=R4=R5=H or CH3 or CH2-CH3 or CH2-CH2CH3 or CH2-CH(CH3)2, R2=OH, R1=R3=H, R4=R5=H or CH3 or CH2-CH3 or CH2-CH2CH3 or CH2-CH(CH3)2, R3=OH, R2=R4=H, R1=R5=H or CH3 or CH2-CH3 or CH2-CH2CH3 or CH2-CH(CH3)2, R4=OH, R3=R5=H, R1=R2=H or CH3 or CH2-CH3 or CH2-CH2CH3 or CH2-CH(CH3)2, R5=OH, R1=H, R2=R3=R4=H or CH3 or CH2-CH3 or CH2-CH2CH3 or CH2-CH(CH3)2.
[0066] The most preferred anacardic acid derivatives may be those of formula (IX):
[0067] [ka]
[0068] [ka]
[0069] The most preferred hydroxycinnamic acid derivatives may be of formula (X):
[0070] [ka]
[0071] The most preferred aliphatic X-hydroxyphenyl acid derivatives may be selected from the group consisting of aliphatic hydroxyphenyl acids (X=1), di-hydroxyphenyl acids (X=2), aliphatic tri-hydroxyphenyl acids (X=3) and aliphatic tetra-hydroxyphenyl acids (X=4) of formula (XI), or mixtures thereof.
[0072] [ka]
[0073] R in the ring ***The number of R depends on the number of hydroxyl groups in the ring and must be at least one, preferably 1 to 3. *** is H toward the ortho position of the phenol, and the integer q is comprised of 1 to 3.
[0074] The most preferred diphenolic acid derivatives are those of formula (XII):
[0075] [ka]
[0076] where: In the above formula, -R a -CR b - the moiety is R'; At least one R *** (preferably 1-3) is H towards the ortho position of the phenol, alternatively R *** is as defined above, and R b is (CH2) n5 CH3, (CH2) n4 -(aliphatic C1-C6 aliphatic alkyl or alkoxy substituted or unsubstituted phenyl group) (wherein n5 is an integer of 1 to 12, preferably 1 to 10, more preferably 1 to 6), and -(CH2) n5 (CH(CH3)2), R a is (CH2) n6 (wherein n6 is an integer from 1 to 3), -CH(CH2) n6 -(CH3), -CH(CH(CH3)2), and -C(CH3)2; -(CH2) n6 is most preferred in order to reduce steric hindrance.
[0077] 4,4-bis(4-hydroxyphenyl)valeric acid (VA or DPA) is most preferred.
[0078] The polyfunctional molecule or oligomeric compound of formula (III) is important for selecting the processing temperature of the benzoxazine polymer.
[0079] The compounds of formula (III) advantageously have a p value of 1 to 30, more preferably 1 to 20, especially 1 to 10, and more preferably R p In the case of =H, C1~C 20 , preferably C1 to C 12 More preferably, it may represent C1 to C6 ethylenediol.
[0080] Bronsted acid catalysts are commonly used in Fischer esterification, including paratoluenesulfonic acid (p-TSA), anhydrous hydrochloric acid (HCl), phosphoric acid (H3PO4), methanoic acid (CH3-CO2H), sulfuric acid, tosylic acid, and Lewis acids such as scandium(III) triflate. The catalyst content can typically be 0.5% to 2% by weight.
[0081] Step a) may be advantageously carried out at a temperature ranging from 80°C to 150°C, most preferably from 100°C to 140°C, for the best synthesis yields of more than 95%, the temperature chosen depending on the nature of the reactants, i.e. the melting temperature of the reactant medium.
[0082] Advantageously, step a) is carried out for 12 to 24 hours to obtain a maximum yield of at least 95%, the duration being based on the reaction rate.
[0083] The stoichiometric ratio of the starting reactants, phenolic acid derivative:polyfunctional molecule or oligomer in step a) may preferably be 1.0-3.0 equivalents:1.0 equivalent, resulting in 1.0 equivalent of phenol-terminated oligomer or molecule.
[0084] The second step of this process, step b), corresponds to a Mannich condensation type reaction of the phenol-terminated oligomer or molecule of step a) ((IV)) with an amino alcohol (formula (V)), which is a primary amine derivative of formula (VI), and paraformaldehyde (formula (VII)), optionally in the presence of a catalyst. Step b) is therefore carried out in a more facile manner, as it does not require the use of an external catalyst.
[0085] Advantageously, the amino alcohol of formula (V) is a linear amino alcohol derivative R having a primary amine moiety and an aliphatic hydroxyl moiety in order to obtain the oxazine ring in the highest yield and under the best reaction conditions. * Contains a group.
[0086] The amino alcohol of formula (V) may more preferably be selected from 2-aminoethanol, 2-amino-2-methylpropanol, 5-aminopentan-1-ol, heptaminol, and diglycolamine, or mixtures thereof.
[0087] The primary amine derivatives may include R as defined above. ** The group is included.
[0088] Primary amine derivatives are R * and may further be selected from the group consisting of allylamine, methylamine, ethylamine, propylamine, butylamine, isopropylamine, hexylamine, cyclohexylamine, 2-aminofluorene, aminophenylacetylene, propargyl ether aniline, 4-aminobenzonitrile, furfurylamine and aniline, or mixtures thereof.
[0089] The temperature range of step b) may preferably be 80°C to 95°C, which can provide a maximum conversion yield of at least 75%.
[0090] Advantageously, step b) is carried out for a period of between 1 hour and 8 hours, most preferably between 1 hour and 5 hours, for a maximum yield of at least 75%.
[0091] One advantage of the present invention is that step b) is carried out without any catalyst.
[0092] The stoichiometric amounts of the starting reactants in step b), phenol-terminated oligomer or molecule, amino alcohol, primary amine derivative, and paraformaldehyde, respectively, are preferably 1.0 equivalent: x1 (1.0 equivalent to 18.0 equivalents): y1 (1.0 equivalent to 18.0 equivalents): 2.0 to 36.0 equivalents; or 1.0 equivalent: x2 (1.0 equivalent to 18.0 equivalents): y2 (1.0 equivalent to 18.0 equivalents): 2.0 to 36.0 equivalents; or 1.0 equivalent: x p (1.0 equivalent to 18.0 equivalent):y p (1.0 equivalent to 18.0 equivalents): 2.0 to 36.0 equivalents, resulting in 1.0 equivalent of ester-containing benzoxazine monomer, wherein x1, x2, and x3 are independently selected from the group consisting of x1, x2, x3, x4, x5, x6, x7, x8, x9, x10, x11, x12, x13, x14, x15, x16, x17, x18, x p = 0, 1 to 1, and y1 = 1 - x1, y2 = 1 - x2, and y p =1-x p Also, x1, x2, and x p The higher the independently, the higher the efficiency of the ROP is assumed to be.
[0093] The specific stoichiometric range depends on the equivalent ratio of the amino alcohol to the primary amine derivative. Note that a minimum amount is required for the reaction to occur. For example, the relative mole percent of the amino alcohol to the primary amine derivative is 10 mole percent to 90 mole percent, respectively. This also means that the primary amine can be omitted (0 mole percent) and only the amino alcohol can be used instead (100 mole percent). Furthermore, the selected stoichiometric range of both the amino alcohol / amine and paraformaldehyde preferably avoids the formation of any linear and / or aliphatic reaction by-products, such as oxazolidines, triaza derivatives, or condensed derivatives.
[0094] Preferentially, the entire process is carried out with bio-based reactants.
[0095] The monoester-benzoxazine synthesis may be most preferably solvent-free, although solvents may be added to dissolve the starting reactants. This process comprises a one-step synthesis, which is one of the advantages of the present invention.
[0096] Advantageously, the overall synthesis may generally not require any further monomer purification in order to practice the invention, although, if necessary, purification of the monomers may be carried out by any known technique (vacuum, distillation, etc.).
[0097] The reaction mixture of both steps a) and b) is stirred using a classical mechanical stirrer or any non-limiting means.
[0098] This process can be carried out by any known means known to those skilled in the art using suitable vessels on either a laboratory or industrial scale.
[0099] The present invention also relates to a process for preparing a polybenzoxazine derivative vitrimer, which comprises polymerizing an ester-containing benzoxazine monomer of the present invention (formula (I)) or as obtained by the above process at a temperature in the range of 100°C to 250°C for 1 hour to 24 hours to obtain a polybenzoxazine derivative vitrimer.
[0100] According to the process for preparing the vitrimer of the present invention, the polymerization step, which is the curing step, opens the benzoxazine rings, allowing them to react with themselves to form a three-dimensional network. Once cooled, the material retains its shape for several months, typically 12 months. Reheating to at least 100°C for several minutes exchanges the ester bonds with aliphatic hydroxyl groups, allowing the material to be reshaped, recycled, or reprocessed while maintaining structural integrity and covalent bond count. Considering that the Mannich condensation reaction is quantitative, approximately two hydroxyl groups can react with each ester bonded by transesterification (even after curing). The behavior of the vitrimer is governed by the glass transition (T) of the vitrimer, which can also be considered the temperature at which transesterification reactions significantly increase. V The behavior of the vitrimer was demonstrated through several experiments. After the curing step, the vitrimer was V By heating to higher temperatures, the initial shape of the vitrimer can be engineered into other original shapes. For example, the vitrimer can be crushed into a powder and reshaped or reprocessed at 150°C in a few minutes. However, the shape remains stable at room temperature.
[0101] The polymerization time depends on the curing temperature and / or the nature of the ester-containing benzoxazine monomer. The polymerization temperature is selected for a given monomer so that it is higher than the temperature required to synthesize the monomer. Generally, the higher the polymerization temperature, the shorter the curing time. For example, if the polymerization temperature is 250°C, the curing time can be at least 1 hour, and if the polymerization temperature is 100°C, the curing time can be 24 hours or less. Preferably, the curing temperature is 140°C to 200°C, more preferably 140°C to 180°C, and in the range of 140°C to 180°C, the curing time will be 1.5 to 3 hours, preferably 1.5 to 2.5 hours. Polymerization can be carried out by any known heating means, such as laser light and infrared light.
[0102] The process may include a post-polymerization step consisting of a heating step which may preferably be carried out at a higher temperature than the polymerization heating step.
[0103] The present invention also relates to polybenzoxazine derivative vitrimers obtainable by the above process, which exhibit at least one of the following characteristics: (i) T from -50℃ to 250℃ V value: preferably 130°C to 220°C, more preferably 130°C to 190°C, (ii) T of -50°C to 300°C, preferably 130°C to 200°C, more preferably 130°C to 180°C V Relaxation temperature value above value.
[0104] Vitrimer T V The value generally depends on the nature and content of the catalyst of step b), if present.
[0105] The relaxation temperature typically corresponds to the relaxation temperature of the vitrimer after a physical deformation, such as strain, e.g., twisting, is applied without any observed decomposition of the vitrimer. Advantageously, the vitrimer may also exhibit at least one of the following characteristics: The relaxation time is 0.5 seconds to 2 hours, preferably 1 second to 1 hour, and more preferably 5 seconds to 50 minutes. The relaxation time is conventionally defined as the time it takes for a sample to relax to a value corresponding to 1 / e (0.37) of the original elastic modulus. Generally, the higher the temperature, the shorter the relaxation time. For example, at temperatures between 120°C and 170°C, the relaxation time is approximately 150 to 200 seconds, and at temperatures between 150°C and 200°C, the relaxation time is 200 seconds or less, preferably 100 to 20 seconds. In some embodiments, the vitrimer can be deformed by 0.1% to 100% of its initial size. the activation energy associated with the relaxation time may be between 50 kJ / mol and 200 kJ / mol, preferably between 70 kJ / mol and 170 kJ / mol, more preferably between 100 kJ / mol and 160 kJ / mol; The processing temperature may be between 100°C and 250°C, preferably between 130°C and 250°C, more preferably between 150°C and 200°C, and most preferably between 150°C and 170°C.
[0106] The vitrimers according to the present invention also exhibit the highly advantageous characteristic of behaving as thermosetting and / or insoluble in many solvents, including but not limited to water, CHCl3, CHCl2, DMF, THF, aromatic solvents such as toluene and / or xylene, ketones, alcohols, or carboxylic acids. Swelling is observed in the range of 0-500% of the initial weight. To assess the formation of a crosslinked network, swelling experiments can be carried out in various solvents, such as acetone, chloroform, and water. Chloroform, among others, is the solvent that results in the highest swelling ratio of the vitrimer, approximately 100%. In acetone and water, the vitrimer swells by 40-50% and 20-30%, respectively.
[0107] The vitrimers of the present invention exhibit self-healing, reshapeable, reworkable, recyclable and reversible adhesive properties.
[0108] The vitrimer can form an interlayer between at least two substrates, such as metals, polymers, glass, and ceramic materials. The resulting composite can be prepared by placing at least one ester-containing benzoxazine monomer between the two substrates and then curing at a temperature that provides the vitrimer without altering the integrity of the substrates. Each substrate can be different from the others.
[0109] The metal substrate can be, but is not limited to, aluminum, iron, steel, and the like.
[0110] The polymer substrate can be polycarbonate, acrylic, polyamide, polyethylene, or terephthalate.
[0111] The benzoxazine vitrimers can then be advantageously used in a variety of technical fields, including but not limited to, electronics, aerospace, aviation, automotive, defense, and automotive fields.
[0112] The present invention also relates to a composition A comprising: a) an ester-containing benzoxazine derivative of formula (I), and b) at least one or more additional compounds of the organic molecule type, which may or may not contain a benzoxazine moiety.
[0113] Preferably, the organic molecule type may be a polymer with or without benzoxazine moieties.
[0114] The additional compounds may be used to improve the properties (ie, viscosity, mechanical and thermal properties) of either the monomer or the vitrimer, or both.
[0115] The polymer may be an epoxy resin, a bismaleimide resin, a phenolic or benzoxazine resin, a polyurethane, a polyamide, a polyolefin, a polyester, or a rubber. The ester-containing benzoxazine derivative of Formula I may be used in a weight ratio of 0.1 to 80% of the final composition.
[0116] The compounds of formula (I) can be used to impart vitrimer properties (self-healing, reworkability, etc.) to the polymers mentioned above.
[0117] The present invention also relates to a composition B comprising: a) an ester-containing benzoxazine monomer of formula (I), and b) A material selected from the group consisting of fillers, fibers, pigments, dyes, and plasticizers.
[0118] The additional compounds may be used to improve the properties (ie, viscosity, mechanical and thermal properties) of either the monomer or the vitrimer, or both.
[0119] The additional compounds can be carbon fiber, glass fiber, basalt fiber, hemp fiber, and bio-based fibers, clay, carbon black, silica, carbon nanotubes, graphene, any known means for thermal or mechanical reinforcement of composites.
[0120] The present invention also relates to the use of the vitrimer according to the invention as a reversible adhesive, sealant, coating or encapsulation system for substrates selected from the group consisting of metals, polymers, glasses and ceramic materials. Preferably, the metals and polymers are as defined above.
[0121] The present invention also relates to the use of the vitrimer according to the invention in a 3D printing process or an additive manufacturing process.
[0122] Other features and advantages of the present invention will be readily understood from the following detailed description and their drawings.
Brief Description of the Drawings
[0123] [Figure 1] Shows a schematic synthesis reaction for obtaining an ester-containing benzoxazine monomer of the BUTD-PA-mea / fa type, wherein when x1 or y1 = 0, when x2 or y2 = 0, R1' and R2' are -CH2-CH2-, x1 and y1 ≠ 0, and x2 and y2 ≠ 0, and in any case where 0.05 ≦ x1 < 1, 0 < y1 ≦ 0.95, and 0.05 ≦ x2 < 1, 0 < y2 ≦ 0.95, R1' and R2' are -CH2-C(CH3)-. [Figure 2a] Shows the NMR spectrum of the BUTD-PA-mea ester-containing benzoxazine monomer. [Figure 2b] Shows the DSC curve of BUTD-PA-mea. [Figure 2c] Shows the observed results of the isothermal rheology of BUTD-PA-mea at 140 °C. [Figure 3a] Shows the stress relaxation curves of the BUTD-PA-mea vitrimer at different temperatures. [Figure 3b] Shows an Arrhenius plot obtained from the stress relaxation experiment of the BUTD-PA-mea vitrimer. [Figure 4]Schematic synthetic reactions for obtaining HEXD-PA-mea / fa type ester-containing benzoxazine monomers are shown, where when x1 or y1 = 0, when x2 or y2 = 0, R1’ and R2’ are -CH2-CH2-, when x1 and y1 ≠ 0, as well as x2 and y2 ≠ 0, and in any case of 0.05 ≦ x1 < 1, 0 < y1 ≦ 0.95, and 0.05 ≦ x2 < 1, 0 < y2 ≦ 0.95, R1’ and R2’ are -CH2-C(CH3)-. [Figure 5a] The NMR spectrum of the HEXD-PA-mea ester-containing benzoxazine monomer is shown. [Figure 5b] The DSC curve of HEXD-PA-mea is shown. [Figure 5c] Observation results of the isothermal rheology of HEXD-PA-mea at 140 °C are shown. [Figure 6a] Stress relaxation curves of the HEXD-PA-mea vitrimer at different temperatures are shown. [Figure 6b] An Arrhenius plot obtained from the stress relaxation experiment of the HEXD-PA-mea vitrimer is shown. [Figure 7] Schematic synthetic reactions for obtaining CHXD-PA-mea / fa type ester-containing benzoxazine monomers are shown, where when x1 or y1 = 0, when x2 or y2 = 0, R1’ and R2’ are -CH2-CH2-, when x1 and y1 ≠ 0, as well as x2 and y2 ≠ 0, and in any case of 0.05 ≦ x1 < 1, 0 < y1 ≦ 0.95, and 0.05 ≦ x2 < 1, 0 < y2 ≦ 0.95, R1’ and R2’ are -CH2-C(CH(3))-. [Figure 8a] The NMR spectrum of the CHXD-PA-mea ester-containing benzoxazine monomer is shown. [Figure 8b] The DSC curve of CHXD-PA-mea is shown. [Figure 8c] Observation results of the isothermal rheology of CHXD-PA-mea at 140 °C are shown. [Figure 9a] Stress relaxation curves of the CHXD-PA-mea vitrimer at different temperatures are shown. [Figure 9b] Shows the Arrhenius plot obtained from the stress relaxation experiment of CHXD-PA-mea vitrimer. [Figure 10] Shows the schematic synthesis reaction for obtaining an ester-containing benzoxazine monomer of OCTD-PA-mea / fa type, where when x1 or y1 = 0, when x2 or y2 = 0, R1’ and R2’ are -CH2-CH2-, when x1 and y1≠0, as well as x2 and y2≠0, and in any case of 0.05≦x1<1, 0<y1≦0.95, and 0.05≦x2<1, 0<y2≦0.95, R1’ and R2’ are -CH2-C(CH3)-. [Figure 11a] Shows the NMR spectrum of the OCTD-PA-mea ester-containing benzoxazine monomer. [Figure 11b] Shows the DSC curve of OCTD-PA-mea. [Figure 11c] Shows the observation results of the isothermal rheology of OCTD-PA-mea at 140 °C. [Figure 12a] Shows the stress relaxation curves of OCTD-PA-mea vitrimer at different temperatures. [Figure 12b] Shows the Arrhenius plot obtained from the stress relaxation experiment of OCTD-PA-mea vitrimer.
[0124] All chemicals are commercially available and are used as purchased when the starting compounds are applicable.
Example 1
[0125] Synthesis of an ester-containing benzoxazine monomer from 1,4-butanediol (BUTD), 3-(4-hydroxyphenyl)propanoic acid (PA) as a phenolic acid derivative, and ethanolamine (mea) as a primary amine having an aliphatic OH.
[0126] Step a), the first step, is carried out in the presence of p-toluenesulfonic acid (p-TSA) introduced in a catalytic amount (1 wt%) with 1,4-butanediol (M = 90.12 g.mol-1 , 1 equivalent, 3 g) and 3-(4-hydroxyphenyl)propanoic acid (PA) (M = 166.18 g mol -1 This corresponds to a Fischer esterification between BUTD, PA, and p-TSA (2 equivalents, 11.06 g). BUTD, PA, and p-TSA were reacted together in the melt at 110 °C and stirred with mechanical stirring for 24 hours to yield 3-(4-hydroxyphenyl)propanoate ester-terminated 1,4-butanediol (BUTD-PA).
[0127] The second step (step b) was carried out to obtain the 3-(4-hydroxyphenyl)-propanoic acid ester-terminated BUTD (BUTD-PA) (M = 386.48 g mol -1 , 1 equivalent, 8 g), ethanolamine (mea) (M = 61.08 g.mol -1 , 2 equivalents, 2.53 g), and paraformaldehyde (PFA) (M = 30.03 g mol -1 , 4 equivalents, 2.49 g). All these reactants were reacted together in the melt at 85 °C and stirred with mechanical stirring for 8 h to give the ester-containing benzoxazine monomer designated BUTD-PA-mea (Figure 1).
[0128] Figure 2a) shows the NMR spectrum (AVANCE III HD Bruker spectrometer) of BUTD-PA-mea ester-containing benzoxazine monomer in DMSO-d6.
[0129] The DSC curve (Netzsch DSC 204 F1 Phoenix instrument) shows an exothermic peak beginning at a temperature of 110 °C with a maximum at 170 °C (Figure 2b). This peak corresponds to the opening of the benzoxazine ring upon heating. The second peak corresponds to the thermal decomposition of the ester bond, which was confirmed by TGA experiments.
[0130] The approximate gel point (tgel), defined as the crossing point between G′ and G″, was rapidly achieved after isothermal curing at 140 °C for 550 s (Fig. 2c). Example 2
[0131] Vitrimer synthesis from BUTD-PA-mea benzoxazine monomer
[0132] The BUTD-PA-mea benzoxazine monomer was cured at 150 °C for 1 h, allowing the benzoxazine ring to open and react with itself to form a 3D network vitrimer in the shape of a disk. The vitrimer behavior of this sample was demonstrated through several rheological experiments.
[0133] The viscoelastic properties of the BUTD-PA-mea vitrimer were examined by stress relaxation experiments recorded at 1% shear strain on an Anton Paar Physica MCR302 rheometer in plate-plate mode (Figure 3a). The relaxation time of the polymer was clearly significant and was recorded as 2 min at 150 °C.
[0134] The activation energy (Ea) of the transesterification reaction is obtained from the slope of the Arrhenius equation and is 102 kJ.mol -1 was obtained (Fig. 3b). Example 3
[0135] Synthesis of ester-containing benzoxazine monomers from 1,6-hexanediol (HEXD), 3-(4-hydroxyphenyl)propanoic acid (PA) as a phenolic acid derivative, and ethanolamine (mea) as a primary amine with an aliphatic OH.
[0136] The first step, step a), was carried out by the reaction of 1,6-hexanediol (M = 118.17 g mol ) in the presence of p-toluenesulfonic acid (p-TSA) introduced in a catalytic amount (1 wt %). -1 , 1 equivalent, 3 g) and 3-(4-hydroxyphenyl)propanoic acid (PA) (M = 166.18 g mol -1This corresponds to a Fischer esterification between 1,6-hexanediol (3-(4-hydroxyphenyl)propanoate ester, 2 equivalents, 8.44 g). HEXD, PA, and p-TSA were reacted together in the melt at 110 °C and stirred with mechanical stirring for 24 h to yield 3-(4-hydroxyphenyl)propanoate ester-terminated 1,6-hexanediol (HEXD-PA).
[0137] The second step (step b) was carried out to obtain 3-(4-hydroxyphenyl)-propanoic acid ester-terminated HEXD (HEXD-PA) (M = 414.53 g mol -1 , 1 equivalent, 8 g), ethanolamine (mea) (M = 61.08 g.mol -1 , 2 equivalents, 2.36 g), and paraformaldehyde (PFA) (M = 30.03 g mol -1 This corresponds to a Mannich condensation between 4 equivalents of HEXD-PA-mea (4 equivalents, 2.32 g). All these reactants were reacted together in the melt at 85 °C and stirred with mechanical stirring for 8 h to give the ester-containing benzoxazine monomer designated HEXD-PA-mea (Figure 4).
[0138] Figure 8a) shows the NMR spectrum (AVANCE III HD Bruker spectrometer) of HEXD-PA-mea ester-containing benzoxazine monomer in DMSO-d6.
[0139] The DSC curve (Netzsch DSC 204 F1 Phoenix instrument) shows an exothermic peak beginning at a temperature of 120 °C with a maximum at 185 °C (Figure 5b). This peak corresponds to the opening of the benzoxazine ring upon heating. The second peak corresponds to the thermal decomposition of the ester bond, which was confirmed by TGA experiments.
[0140] The approximate gel point (tgel), defined as the crossing point of G′ and G″, was rapidly achieved after isothermal curing at 140 °C for 1550 s (Fig. 5c). Example 4
[0141] Vitrimer synthesis from HEXD-PA-mea benzoxazine monomer The HEXD-PA-mea benzoxazine monomer was cured at 150 °C for 1 h, allowing the benzoxazine ring to open and react with itself to form a 3D network vitrimer in the shape of a disk. The vitrimer behavior of this sample was demonstrated through several rheological experiments.
[0142] The viscoelastic properties of the HEXD-PA-mea vitrimer were examined by stress relaxation experiments recorded at 1% shear strain in plate-plate mode on an Anton Paar Physica MCR302 rheometer (Figure 6a). The relaxation time of the polymer was clearly significant and was recorded as 88 s at 150 °C.
[0143] The activation energy (Ea) of the transesterification reaction is obtained from the slope of the Arrhenius equation and is 95 kJ.mol -1 was obtained (Fig. 6b). Example 5
[0144] Synthesis of ester-containing benzoxazine monomers from 1,4-cyclohexanedimethanol (CHXD), 3-(4-hydroxyphenyl)propanoic acid (PA) as a phenolic acid derivative, and ethanolamine (mea) as a primary amine with an aliphatic OH group.
[0145] The first step, step a), was carried out by the reaction of 1,4-cyclohexanedimethanol (M = 144.21 g mol ) in the presence of p-toluenesulfonic acid (p-TSA) introduced in a catalytic amount (1 wt %). -1 , 1 equivalent, 3 g) and 3-(4-hydroxyphenyl)propanoic acid (PA) (M = 166.18 g mol -1 This corresponds to a Fischer esterification between CHXD, PA, and p-TSA (2 equivalents, 6.91 g). CHXD, PA, and p-TSA were reacted together in the melt at 110 °C and stirred with mechanical stirring for 24 h to yield 3-(4-hydroxyphenyl)propanoate ester-terminated 1,4-cyclohexanedimethanol (CHXD-PA).
[0146] The second step (step b) was carried out to obtain 3-(4-hydroxyphenyl)-propanoic acid ester-terminated CHXD (HEXD-PA) (M = 440.57 g mol -1 , 1 equivalent, 8 g), ethanolamine (mea) (M = 61.08 g.mol -1 , 2 equivalents, 2.22 g), and paraformaldehyde (PFA) (M = 30.03 g mol -1 , 4 equivalents, 2.18 g). All these reactants were reacted together in the melt at 85 °C and stirred with mechanical stirring for 8 h to give the ester-containing benzoxazine monomer designated CHXD-PA-mea (Figure 7).
[0147] Figure 8a) shows the NMR spectrum (AVANCE III HD Bruker spectrometer) of CHXD-PA-mea ester-containing benzoxazine monomer in DMSO-d6.
[0148] The DSC curve (Netzsch DSC 204 F1 Phoenix instrument) shows an exothermic peak beginning at a temperature of 120 °C with a maximum at 185 °C (Figure 8b). This peak corresponds to the opening of the benzoxazine ring upon heating. The second peak corresponds to the thermal decomposition of the ester bond, which was confirmed by TGA experiments.
[0149] The approximate gel point (tgel), defined as the crossing point of G′ and G″, was rapidly achieved after isothermal curing at 140 °C for 1700 s (Fig. 8c). Example 6
[0150] Vitrimer synthesis from CHXD-PA-mea benzoxazine monomer The CHXD-PA-mea benzoxazine monomer was cured at 150 °C for 1 h, allowing the benzoxazine ring to open and react with itself to form a 3D network vitrimer in the shape of a disk. The vitrimer behavior of this sample was demonstrated through several rheological experiments.
[0151] The viscoelastic properties of the CHXD-PA-mea vitrimer were examined by stress relaxation experiments recorded at 1% shear strain in plate-plate mode on an Anton Paar Physica MCR302 rheometer (Figure 9a). The relaxation time of the polymer was clearly significant and was recorded as 202 min at 150 °C.
[0152] The activation energy (Ea) of the transesterification reaction is obtained from the slope of the Arrhenius equation and is 139 kJ.mol -1 was obtained (Fig. 9b). Example 7
[0153] Synthesis of ester-containing benzoxazine monomers from 1,8-octanediol (OCTD), 3-(4-hydroxyphenyl)propanoic acid (PA) as a phenolic acid derivative, and ethanolamine (mea) as a primary amine with an aliphatic OH.
[0154] The first step, step a), was carried out by the synthesis of 1,8-octanediol (OCTD) (M = 146.22 g mol ) in the presence of p-toluenesulfonic acid (p-TSA) introduced in a catalytic amount (1 wt %). -1 , 1 equivalent, 3 g) and 3-(4-hydroxyphenyl)propanoic acid (PA) (M = 166.18 g mol -1 This corresponds to a Fischer esterification between OCTD, PA, and p-TSA (2 equivalents, 6.91 g). OCTD, PA, and p-TSA were reacted together in the melt at 110 °C and stirred with mechanical stirring for 24 h to yield 3-(4-hydroxyphenyl)propanoate ester-terminated 1,8-octanediol (OCTD-PA).
[0155] The second step (step b) was carried out to obtain 3-(4-hydroxyphenyl)-propanoic acid ester-terminated OCTD (OCTD-PA) (M = 442.59 g mol -1 , 1 equivalent, 8 g), ethanolamine (mea) (M = 61.08 g.mol -1 , 2 equivalents, 2.21 g), and paraformaldehyde (PFA) (M = 30.03 g mol-1 , 4 equivalents, 2.17 g). All these reactants were reacted together in the melt at 85 °C and stirred with mechanical stirring for 8 hours to give the ester-containing benzoxazine monomer designated OCTD-PA-mea (Figure 10).
[0156] Figure 11a) shows the NMR spectrum (AVANCE III HD Bruker spectrometer) of OCTD-PA-mea ester-containing benzoxazine monomer in DMSO-d6.
[0157] The DSC curve (Netzsch DSC 204 F1 Phoenix instrument) shows an exothermic peak beginning at a temperature of 100 °C and a maximum at 180 °C (Figure 12b). This peak corresponds to the opening of the benzoxazine ring upon heating. The second peak corresponds to the thermal decomposition of the ester bond, which was confirmed by TGA experiments.
[0158] The approximate gel point (tgel), defined as the crossing point between G′ and G″, was rapidly achieved after isothermal curing at 140 °C for 640 s (Fig. 11c). Example 8
[0159] Vitrimer synthesis from OCTD-PA-mea benzoxazine monomer
[0160] The OCTD-PA-mea benzoxazine monomer was cured at 150 °C for 1 h, allowing the benzoxazine ring to open and react with itself to form a 3D network vitrimer in the shape of a disk. The vitrimer behavior of this sample was demonstrated through several rheological experiments.
[0161] The viscoelastic properties of the OCTD-PA-mea vitrimer were examined by stress relaxation experiments recorded at 1% shear strain on an Anton Paar Physica MCR302 rheometer in plate-plate mode (Figure 12a). The relaxation time of the polymer was clearly significant and was recorded as 68 s at 150 °C.
[0162] The activation energy (Ea) of the transesterification reaction is obtained from the slope of the Arrhenius equation and is 106 kJ.mol -1 was obtained (Fig. 12b).
Claims
1. a) an ester-containing benzoxazine monomer of formula (I) 【number】 Where: R is a linear or branched C 1 ~C 20 Alkyl group, cyclo(C 3 ~C 6 alkyl) group, heterocyclo (C 3 ~C 6 alkyl) groups, where the heteroatoms are selected from the group consisting of N, S, Si and O, linear or branched C 2 ~C 12 Alkenyl groups, substituted or unsubstituted linear or branched C 2 ~C 12 Alkynyl group, linear or branched C 1 ~C 6 Alkyl or C 2 ~C 6 alkenyl-substituted or unsubstituted phenyl groups, -(CH 2 ) n3 - a phenyl group (wherein n3 is an integer from 1 to 10), a siloxane group; R 1 teeth, 【number】 and ; R 2 teeth, 【number】 and R p is H, linear or branched C 1 ~C 20 Alkyl or alkoxy groups, linear or branched C 2 ~C 12 Alkenyl or alkyleneoxy groups, substituted or unsubstituted linear or branched C 2 ~C 12 Alkynyl group, linear or branched C 1 ~C 6 Alkyl or C 2 ~C 6 Alkenyl-substituted or unsubstituted phenyl groups and 【number】 selected from the group consisting of: Where: R in formula (I) 1 and R 2 is different; x 1 , x 2 , and x p is independently 0 to 1; y 1 = 1 - x 1 and y 2 = 1 - x 2 y p = 1 - x p and x 1 , x 2 and x p are not both zero; p is 1 to 100; R 1 ', R 2 ', and R p ' is independently C-linear or branched C 1 ~C 6 Alkyl or alkoxy group, -C-straight or branched C 2 ~C 6 Alkenyl or alkyleneoxy groups, -C-substituted or unsubstituted linear or branched C 2 ~C 6 Alkynyl groups, and -C-straight or branched C 1 ~C 6 Alkyl or C 2 ~C 6 alkenyl-substituted or unsubstituted phenyl groups; R p '' is a linear or branched C 1 ~C 6 Alkyl or alkoxy groups, linear or branched C 2 ~C 6 Alkenyl or alkyleneoxy groups, substituted or unsubstituted linear or branched C 2 ~C 6 Alkynyl groups, and linear or branched C 1 ~C 6 Alkyl or C 2 ~C 6 alkenyl-substituted or unsubstituted phenyl groups; R * is a linear or branched C 1 ~C 6 Alkyl or alkoxy group, cyclo(C 3 ~C 6 alkyl) group, heterocyclo (C 3 ~C 6 alkyl) groups, where the heteroatoms are selected from the group consisting of N, Si, S, and O, linear or branched C 2 ~C 6 Alkenyl or alkyleneoxy groups, substituted or unsubstituted linear or branched C 2 ~C 6 Alkynyl group, linear or branched C 1 ~C 6 Alkyl or C 2 ~C 6 alkenyl-substituted or unsubstituted phenyl groups, (CH 2 ) n 3 -phenyl group and -(CH 2 ) n 3 -O-(CH 2 ) n 4 wherein n3 and n4 are independently an integer from 1 to 10; R ** is R * is the same as O—, N—, Si— or S—(CH 2 ) n3 -CH-(CH 3 ) 2 Groups O—, N—, Si— or S—(CH 2 ) n 3 - (CHZ) n4 - (CH 3 ) 2 Groups O—, N—, Si— or S—(CH 2 ) n3 - (CHZ) n4 - (CH 2 ) n3 -CH 3 Groups O-, N-, Si- or S-(CHZ) n4 - (CH 2 ) n3 -CH 3 Groups O-, N-, Si- or S-(CHZ) n4 - [(CH 2 ) n3 -CH 3 ] 2 Group, O-substituted or unsubstituted C 2 -C 6 A straight or branched chain alkynyl group, -(CH 2 ) n3 Further included are members selected from the group consisting of -C≡N groups, polycyclic aromatic or heteroaromatic hydrocarbons (e.g., naphthalene, anthracene, fluorene, phenanthrene), which are optionally linear or branched C 1 -C 6 Alkyl or alkoxy group, cyclo(C 3 -C 6 Alkyl), heterocyclo(C 3 -C 6 alkyl), where the heteroatoms are N, S, Si, and O, linear or branched C 2 ~C 6 alkenyl or alkyleneoxy groups, or substituted or unsubstituted linear or branched C 2 ~C 6 alkynyl groups, wherein n3 and n4 are independently integers from 1 to 10, and Z is a linear or branched C 1 ~C 6 Alkyl or alkoxy groups, linear or branched C 2 ~C 6 Alkenyl or alkyleneoxy groups, and linear or branched C 1 ~C 6 Alkyl or C 2 ~C 6 alkenyl substituted or unsubstituted phenyl groups, wherein at least one O atom is present or absent between two adjacent C; R *** is H, OH, and O- straight or branched chain C 1 ~C 6 alkyl group, further comprising a straight or branched C 1 ~C 15 Alkyl group or C 2 ~C 15 or an alkenyl group of 【number】 Including, [0010] Where: [0025] is R 1 is the number of amino alcohols per group, [0030] is R 1 represents the number of amines (excluding the number of amino alcohols) per group, [0045] is R 1 is the total number of amino groups per group; Where: [0050] is R 2 is the number of amino alcohols per group, [006] is R 2 represents the number of amines (excluding the number of amino alcohols) per group, [0070] is R 2 is the total number of amino groups per group; Where: [0080] is R p is the number of amino alcohols per group, [0097] is R p represents the number of amines (excluding the number of amino alcohols) per group, [0010] is R p is the total number of amino groups per group.
2. The benzoxazine-containing ester monomer of claim 1. R * is a linear or branched C 1 ~C 4 Alkyl or alkoxy groups, linear or branched C 2 ~C 4 Alkenyl or alkyleneoxy groups, unsubstituted linear or branched C 2 ~C 4 Alkynyl groups, unsubstituted phenyl groups and (CH 2 ) n 3 -phenyl group, -(CH 2 ) n3 -O-(CH 2 ) n 4 wherein n3 and n4 are independently an integer from 1 to 6; R ** is R * is the same as O—, N—, Si or S—(CH 2 ) n3 -CH-(CH 3 ) 2 Groups, O—, N—, Si or S—(CH 2 ) n3 - (CHZ) n4 - (CH 3 ) 2 Groups, O—, N—, Si or S—(CH 2 ) n3 - (CHZ) n4 - (CH 2 ) n3 -CH 3 Groups, O-, N-, Si or S-(CHZ) n4 - (CH 2 ) n3 -CH 3 Groups, O-, N-, Si or S-(CHZ) n4 - [(CH 2 ) n3 -CH 3 ] 2 groups, and O-substituted or unsubstituted C 2 ~C 4 A linear or branched alkynyl group, wherein Z is as defined in claim 1, -(CH 2 ) n3 -C≡N, cyclo(C 3 ~C 4 Alkyl), heterocyclo(C 3 ~C 4 alkyl), polycyclic aromatic or heteroaromatic hydrocarbons, where the heteroatoms are selected from the group consisting of N, S, Si, and O, and optionally linear or branched C 1 ~C 4 Alkyl or alkoxy groups, linear or branched C 2 ~C 4 Substituted by an alkenyl group or an alkyleneoxy group, or a substituted or unsubstituted linear or branched C 2 ~C 4 substituted by an alkynyl group, wherein n3 and n4 are independently integers from 1 to 6; R *** is H, OH, and O- straight or branched chain C 1 ~C 4 alkyl groups, linear or branched C 1 ~C 10 Alkyl group or C 2 ~C 10 or an alkenyl group of 【Chemistry 6】 Further includes:
3. 3. An ester-containing benzoxazine monomer according to claim 1 or 2; R * is -CH 3 , -(CH 2 ) n 3 -CH 3 , -(CH 2 ) n 3 -CH-[(CH 2 ) n 4 -CH 3 ] 2 , -C(CH 3 ) 3 , (CH 2 ) n 3 - (C 6 H 5 ), -(CH 2 ) n 3 -CH=CH 2 , -(CH 2 ) n 3 -C≡CH, -(CH 2 ) n 3 -O-(CH 2 ) n 4 (wherein n3 and n4 are independently an integer from 1 to 4), phenyl, and -(CH 2 ) 3 - phenyl; R ** The group is R * or CH 3 , -(CH 2 ) n3 -CH 3 , -(CH 2 ) n3 -CH-[(CH 2 ) n4 -CH 3 ] 2 , -C(CH 3 ) 3 , (CH 2 ) n3 - (C 6 H 5 ), -(CH 2 ) n3 -CH=CH 2 , -(CH 2 ) n3 -C≡CH,O-(CH 2 ) n3 -C≡CH, O-(CH 2 ) n3 -C≡N, (CH 2 ) n3 -C≡N and -(CH 2 ) n3 - selected from the group consisting of substituted or unsubstituted furan, phenyl, where n3 and n4 are independently integers from 1 to 4; R *** is H, OH, and O- straight or branched chain C 1 ~C 3 alkyl groups, linear or branched C 1 ~C 6 Alkyl group or C 2 ~C 6 or an alkenyl group of 【Chemistry 7】 Further includes:
4. A process for synthesizing an ester-containing benzoxazine monomer of formula (I), comprising the steps of: a) at least one R on the phenol ring *** A phenolic acid derivative of formula (II) containing a group: 【Chemistry 8】 (wherein x is 0 to 1 and y=1-x). A polyfunctional molecule or oligomer of formula (III) 【Chemistry 9】 reacting in the presence of a Bronsted acid type catalyst at a temperature between 25° C. and 200° C. for 1 hour to 72 hours to produce a phenol-terminated oligomer or molecule (compound (IV)); b) reacting said compound (IV): an amino alcohol of formula (V): 【Chemistry 10】 a primary amine derivative of formula (VI), R ** -NH 2 (VI), and a mixture of paraformaldehyde of formula (VII) 【Chemistry 11】 m = 8 to 100 Reacting under stirring at a temperature range of 80° C. to 100° C. for 1 hour to 10 hours to obtain the compound of formula (I). (In the formula, R 1 , R 2 , R 1 ', R 2 ', R p , R * , R ** , R *** and x 1 , x 2 , x p , y 1 , y 2 , y p and p are as defined in any one of claims 1 to 3, R n ' is R 1 ' or R 2 ' and R 1 ' is R 2 ', provided that at least one R *** When R is in the ortho position relative to the -OH group, *** is H).
5. 5. The process of claim 4, wherein the phenolic acid derivative (formula (II)) is selected from the group consisting of mono-, di-, tri-hydroxybenzoic acid derivatives, anacardic acid derivatives, hydroxycinnamic acid derivatives, aliphatic X-hydroxyphenyl acid derivatives (X is 2-4), and aliphatic diphenolic acid derivatives, or mixtures thereof.
6. 6. The process according to claim 4 or 5, wherein the stoichiometric ratio of the starting reactants in step a) phenolic acid derivative:multifunctional molecule or oligomer, respectively, is 1.0-3.0 equivalents:1.0 equivalent, resulting in 1.0 equivalent of phenol terminated oligomer or molecule.
7. 7. The process of any one of claims 4 to 6, wherein the primary amine derivative is further selected from the group consisting of allylamine, methylamine, ethylamine, propylamine, butylamine, isopropylamine, hexylamine, cyclohexylamine, 2-aminofluorene, aminophenylacetylene, propargyl ether aniline, 4-aminobenzonitrile, furfurylamine and aniline, or mixtures thereof.
8. The process according to any one of claims 4 to 7, wherein the temperature range of step b) is from 80°C to 95°C.
9. The process according to any one of claims 4 to 8, wherein step b) is carried out for 1 to 8 hours.
10. The stoichiometric amounts of the starting reactants in step b), phenol-terminated oligomer or molecule, amino alcohol, primary amine derivative, and paraformaldehyde, are 1.0 equivalent: x 1 (1.0 equivalent 18.0 equivalent: y 1 (1.0 equivalent 18.0 equivalent: 2.0 to 36.0 equivalent or 1.0 equivalent: x 2 (1.0 equivalent 18.0 equivalent: y 2 (1.0 equivalent 18.0 equivalent: 2.0 to 36.0 equivalent or 1.0 equivalent: x p (1.0 equivalent 18.0 equivalents: yp(1.0 equivalent 18.0 equivalents: 2.0 to 36.0 equivalents, resulting in 1.0 equivalent of ester-containing benzoxazine monomer, where x 1 , x 2 and x p is independently 0, 1 to 1, and y 1 = 1 to x 1 , y 2 = 1 to x 2 and y p = 1 to x p The process according to any one of claims 4 to 9, wherein
11. A process according to any one of claims 4 to 10, wherein the relative mole % of amino alcohol to primary amine derivative is 10 mole % to 90 mole %, respectively.
12. A process for preparing polybenzoxazine derivative vitrimers, comprising the step of polymerizing an ester-containing benzoxazine monomer as claimed in any one of claims 1 to 3 or as obtained by the process as claimed in any one of claims 4 to 11, at a temperature in the range of 100°C to 250°C for 1 hour to 24 hours to obtain a polybenzoxazine derivative vitrimer.
13. A polybenzoxazine derivative vitrimer obtainable by the process according to claim 12, exhibiting at least one of the following characteristics: (i) T from −50° C. to 250° C. V value; preferably 130°C to 220°C, more preferably 130°C to 190°C; (ii) T of −50° C. to 300° C., preferably 130° C. to 200° C., more preferably 130° C. to 180° C. V Relaxation temperature value above value.
14. The polybenzoxazine derivative vitrimer according to claim 13, exhibiting at least one of the following characteristics selected from the group consisting of: the relaxation time is between 0.5 seconds and 2 hours, preferably between 1 second and 1 hour, more preferably between 5 seconds and 50 minutes; the activation energy associated with said relaxation time is between 50 kJ / mol and 200 kJ / mol, preferably between 70 kJ / mol and 170 kJ / mol, more preferably between 100 kJ / mol and 160 kJ / mol; the processing temperature is between 100°C and 250°C, preferably between 130°C and 250°C, more preferably between 150°C and 200°C, most preferably between 150°C and 170°C.
Citation Information
Patent Citations
Tannin-type benzoxazine and preparation method thereof
CN109134799A
Preparation of benzoxazine compounds in a solvent-free system
JP1997502452A