Nail sticker, method for manufacturing said nail sticker, and nail sticker set including said nail sticker

A nail sticker with a curved lower surface and manufacturing method using a support structure addresses the challenge of fitting gel nail stickers to unique nail shapes, ensuring better adherence and shape retention.

JP2024536520AActive Publication Date: 2024-10-04GLLUGA INC
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2024522475
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-21
Filing Date
2023-05-18
Publication Date
2024-10-04
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

Conventional nail stickers, particularly gel nail stickers, struggle to conform to the unique shapes of individual fingernails and toenails due to their flat bottom surfaces, leading to difficulty in adherence and maintaining a customized fit.

Method used

The nail sticker features a lower surface with a curved design that directs its center upward, allowing it to be molded to match the user's nail shape, and is manufactured using a support structure and pressure application to maintain this curvature during curing.

Benefits of technology

The solution enables easy customization of the nail sticker to fit individual nail shapes, enhances adhesive strength, and maintains the desired shape throughout the application and curing process, reducing deformation and improving user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536520000001_ABST
    Figure 2024536520000001_ABST
Patent Text Reader

Abstract

The present invention relates to a nail sticker that can be cured by ultraviolet light, and a lower surface of the nail sticker before being cured by ultraviolet light may include a curved surface that is curved such that a center of the nail sticker is directed upward.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nail sticker, a method for manufacturing the nail sticker, and a nail sticker set including the nail sticker. [Background technology]

[0002] As one of the ways people pursue physical beauty, the beauty industry has been developing at an accelerated pace and becoming more specialized. In particular, since the 20th century, the beauty industry has begun to popularize itself among the general public as the market has expanded rapidly. Within the beauty industry, nail art has rapidly developed in recent years as an essential element of the art of expressing the body, regardless of age or gender.

[0003] Originally, nail art was a branch of beauty art, a way to beautifully decorate the human body, and the length, shape, and color of nails have been expressed to reflect the cultural changes and values ​​of the times.

[0004] Among nail art, nail stickers in the shape of artificially created fingernails or toenails are used by many people. Previously, nail stickers were manufactured in a curved shape to resemble the shape of fingernails or toenails and supplied to consumers. Such nail stickers were supplied to consumers in a hardened, extruded form. However, because the shapes (especially the curvature) of each person's fingernails or toenails are different, there was a problem that it was difficult for the nail stickers, which have an inherently curved shape, to adhere closely to the consumer's fingernails or toenails.

[0005] As a solution to this problem, nail stickers containing UV-curable materials have recently been in the limelight. Specifically, nail stickers containing UV-curable materials have a flat bottom surface, and the user (consumer) deforms the nail sticker to fit their fingernail or toenail, and then irradiates UV light to harden the nail sticker. This allows the nail sticker to be closely attached to the consumer's fingernail or toenail, improving the adhesive strength of the nail sticker. Such nail stickers are also called gel nail stickers.

[0006] In addition, the thickness of the gel nail sticker may be somewhat thicker for various reasons. For example, in the case of a gel nail sticker that is long and has a shape that extends beyond the end of the fingernail or toenail in addition to the part that overlaps with the fingernail or toenail, the thickness may be thicker in order to maintain the shape. In addition, the thickness of the gel nail sticker may be somewhat thicker for cosmetic reasons, not necessarily for the above reasons.

[0007] In this way, if the gel nail sticker is thick, even if a user applies force to the gel nail sticker to change its shape to fit their fingernail or toenail, the gel nail sticker will easily return to its original shape, making it difficult to wear the gel nail sticker to fit the shape of their fingernail or toenail.

[0008] Therefore, there is a need for new technology that allows users to more effectively apply gel nail stickers to their fingernails or toenails. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Republic of Korea Patent Publication No. 10-2019-0014044 Summary of the Invention [Problem to be solved by the invention]

[0010] One problem to be solved by the present invention is to provide a nail sticker that can be easily shaped by a user to fit the shape of their own nails (fingernails or toenails).

[0011] Another object of the present invention is to provide a method for manufacturing the nail sticker.

[0012] Another object of the present invention is to provide a nail sticker set including the nail sticker. [Means for solving the problem]

[0013] According to one embodiment of the present invention, there is provided a nail sticker that can be cured by ultraviolet light, in which a lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface in which a center of the nail sticker is curved toward an upper portion.

[0014] According to another embodiment of the present invention, there is provided a method for manufacturing a nail sticker, the method including: a first step of placing a preliminary nail sticker that can be cured by ultraviolet light on a support part included in a support structure; and a second step of applying pressure toward an upper surface of the preliminary nail sticker to bring a lower surface of the preliminary nail sticker into close contact with an upper surface of the support part; the support part has a curved surface that is convex toward an upper portion, and the lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface that is curved such that a center of the nail faces toward the upper portion.

[0015] According to yet another embodiment of the present invention, a support structure including a support portion; and a nail sticker attached to an upper surface of the support, the upper surface of the support having a curved surface that is curved such that the center of the sticker faces upward, the nail sticker being curable by ultraviolet light, and a lower surface of the nail sticker before being cured by ultraviolet light having a curved surface that is curved such that the center of the nail sticker faces upward. Effect of the Invention

[0016] According to the present invention, compared to existing nail stickers that have a flat bottom surface, the bottom surface of the nail sticker of the present invention before hardening includes a curved surface in which the center of the nail sticker is curved toward the top, making it easier for users to shape the nail sticker to fit the shape of their own nails.

[0017] In addition, the nail sticker maintains its shape well even during the process of application and hardening of the nail sticker by the user, making it easy for the user to use and allowing the user to wear the nail sticker that best suits their nails. [Brief description of the drawings]

[0018] [Figure 1] 1 is a schematic diagram of a nail sticker according to an embodiment of the present invention. [Diagram 2] 1 is a photograph of a nail sticker according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a top view of a nail sticker according to one embodiment of the present invention. [Figure 4] 5 is a cross-sectional view of the nail sticker taken along the line xx′ in FIG. 3. [Diagram 5] 1 is a cross-sectional view of a preliminary nail sticker before being placed on a support. [Figure 6] FIG. 2 is a schematic diagram of a support as described herein. [Figure 7] 5A to 5C are schematic diagrams illustrating a method for manufacturing a nail sticker according to another embodiment of the present invention. [Figure 8] 5A to 5C are schematic diagrams illustrating a method for manufacturing a nail sticker according to another embodiment of the present invention. [Figure 9] 5A to 5C are schematic diagrams illustrating a method for manufacturing a nail sticker according to another embodiment of the present invention. [Figure 10] 1 is a schematic diagram of a nail sticker set according to one embodiment of the present invention. [Figure 11] 1 is a photograph of a nail sticker set according to an embodiment of the present invention. [Figure 12] 1 is a photograph of a nail sticker set according to an embodiment of the present invention. [Figure 13] This is a photograph of a nail sticker according to Example 1 of the present invention, specifically, a photograph of the nail sticker manufactured through steps 1 to 3 of the nail sticker manufacturing method described in the present invention immediately after it is peeled off from the support. [Figure 14] This is a photograph of a nail sticker according to Example 1 of the present invention, specifically, after the first and second steps of the manufacturing method of the nail sticker described in the present invention, the nail sticker is peeled off from the support and left for 24 hours. [Figure 15] This is a photograph of a nail sticker according to Example 2 of the present invention, specifically, a photograph of the nail sticker manufactured through steps 1 and 2 of the nail sticker manufacturing method described in the present invention immediately after it is peeled off from the support. [Figure 16] This is a photograph of a nail sticker according to Example 2 of the present invention, specifically, after the first and second steps of the manufacturing method of the nail sticker described in the present invention, the nail sticker is peeled off from the support and left for 24 hours. [Figure 17] 1 is a photograph of a nail sticker according to Comparative Example 1 of the present invention, taken immediately after the manufactured nail sticker was peeled off from the support. [Figure 18]This is a photograph of a nail sticker according to Comparative Example 1 of the present invention. Specifically, this is a photograph of the nail sticker after the first and second steps of the manufacturing method of the nail sticker described in the present invention, in which the nail sticker was peeled off from the support and left for 24 hours. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention is susceptible to various modifications and embodiments, and therefore, specific embodiments are shown by way of example in the drawings and will be described in detail in the detailed description.

[0020] However, it should be understood that this is not intended to limit the present invention to a specific embodiment, and includes any modifications, equivalents, or alternatives that fall within the spirit and technical scope of the present invention. In the description of the present invention, if a detailed description of related publicly known technology is deemed to obscure the gist of the present invention, the detailed description will be omitted.

[0021] The terms used in this application are merely used to describe specific embodiments and are not intended to limit the present invention. The singular expressions include the plural expressions unless otherwise clearly indicated in the context.

[0022] In the present invention, the terms "comprise" or "have" and the like are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described herein, but are to be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0023] In the present invention, being placed or located "on" can mean not only being present on an object in a state of direct contact, but also being placed or located on an object in a state of being spaced apart.

[0024] By nail herein is meant fingernails and / or toenails.

[0025] The thickness measured in the present invention can be confirmed via a Keyence VHX-970F device.

[0026] In this specification, the "maximum thickness" of a certain component means the thickest thickness of the component measured in a vertical direction from any fulcrum on the lower surface of the component.

[0027] The upper surface of the nail sticker in this specification means a surface exposed toward the upper direction when the R direction in Figs. 1 and 4 is the upper direction. Specifically, the upper surface of the nail sticker may be a surface where a coating layer is exposed to the outside. The lower surface of the nail sticker in this specification means a surface exposed toward the lower direction when the R' direction in Figs. 1 and 4 is the lower direction. Specifically, the upper surface of the nail sticker may be a surface where a base layer (specifically, an adhesive layer of the base layer) is exposed to the outside.

[0028] In this specification, a test for confirming the deformation rate can be performed with the nail sticker placed on a flat floor as shown in FIG.

[0029] The nail sticker of the present invention can refer to a nail sticker that can be deformed by a user to fit the user's nail and can be cured by UV irradiation when attached to the user's nail. Such a nail sticker is also called a gel nail sticker.

[0030] Therefore, the nail sticker of the present invention can mean a nail sticker that is not cured by ultraviolet light (a state in which the user is not irradiating ultraviolet light). In other words, it can mean the nail sticker of one embodiment of the present invention, the nail sticker manufactured by the nail sticker manufacturing method of another embodiment of the present invention, and all of the nail stickers included in the nail sticker set of yet another embodiment of the present invention, all of the nail stickers that are not cured by ultraviolet light (a state in which the user is not irradiating ultraviolet light).

[0031] In the present specification, when the nail sticker is cured by ultraviolet irradiation, the ultraviolet irradiation conditions may mean irradiation with ultraviolet light having a wavelength of 100 nm to 400 nm at an output of 100 W to 1800 W for 10 to 40 seconds.

[0032] <Nail sticker> The nail sticker means an artificial laminated structure manufactured for application to nails (fingernails and / or toenails). When considered for application to be applied, it is also called nail art or nail art sticker.

[0033] Specifically, when a consumer is provided with the nail sticker, the consumer can attach the nail art to the nail while deforming the shape of the nail sticker so that the nail sticker adheres closely to the nail, and then cure the nail sticker by irradiating it with ultraviolet light.

[0034] The nail sticker according to an embodiment of the present invention is a nail sticker that can be cured by ultraviolet light, and a lower surface of the nail sticker before being cured by ultraviolet light may include a curved surface that is curved such that a center of the nail sticker is curved toward an upper portion.

[0035] Fig. 1 is a schematic diagram of a nail sticker according to an embodiment of the present invention, and Fig. 2 is a photograph of the nail sticker. Referring to Fig. 1 and Fig. 2, the nail sticker according to an embodiment of the present invention may be in the shape of a nail. The nail sticker has a curved shape that is convex upward, rather than a flat bottom surface.

[0036] Fig. 3 is a top view of a nail sticker according to an embodiment of the present invention. Referring to Fig. 3, the nail sticker can include a long axis and a short axis. The long axis corresponds to an axis including an imaginary line segment corresponding to the longest arm of the nail sticker in a direction from the root of the nail to the end of the nail (the end adjacent to the fulcrum where the fingertip ends) when the nail sticker is worn on the nail (yy' in Fig. 3).

[0037] Here, the length of the nail sticker means the size of the nail sticker in the direction from the root of the nail to the end of the nail (the end adjacent to the fulcrum where the fingertip ends) when the nail sticker is attached to the nail. The short axis is perpendicular to the long axis and corresponds to an axis including an imaginary line segment corresponding to the width of the nail (the distance between both edges of the nail sticker adjacent to both sides of the nail) when the nail sticker is attached to the nail, and the length of the nail sticker can be accurately divided in two by the shortening. The center 100a of the nail sticker means the fulcrum where the long axis and short axis of the nail intersect.

[0038] 1 to 4, the lower surface 100b of the nail sticker before being cured by ultraviolet light may include a curved surface in which the center 100a of the nail sticker is curved upward. That is, the nail sticker of the present invention may have a shape in which the flat lower surface is curved by an external force and the center 100a of the nail sticker is curved upward.

[0039] Similarly, the upper surface of the nail sticker may include a curved surface that is curved so that the center 100a of the nail sticker faces upward. More specifically, when the nail sticker is placed on a flat floor so that the lower surface of the nail sticker before being cured by ultraviolet rays faces the flat floor, the center 100a of the nail sticker may be spaced apart from the floor.

[0040] Here, the lower surface 100b of the nail sticker may refer to the surface facing the user's nail, and specifically may be the surface including the surface where the adhesive layer is exposed to the outside. When the nail sticker is placed on a flat floor so that the lower surface of the nail sticker before being cured by ultraviolet rays faces the flat floor, at least a part of the edge of the nail sticker may contact the flat floor.

[0041] This type of shape is rarely seen in conventional nail stickers that are curable by ultraviolet light. Specifically, in the case of injection-molded hard nail stickers, if a nail-shaped mold is used, the bottom surface of the nail sticker can be manufactured to include a curved surface with the center of the nail sticker curved toward the top. However, nail stickers that are curable by ultraviolet light must have flexibility that allows users to mold them to fit the shape of their own nails, so soft materials must be used.

[0042] When such materials are used, if nail stickers are manufactured through a nail-shaped mold, the material will burn in the mold. In addition, according to the conventional method of manufacturing nail stickers, the nail stickers are manufactured by stacking layers that constitute the nail sticker on a flat floor, and the bottom surface of the nail sticker inevitably becomes flat during this process. When an external force is applied to a "nail sticker with a flat bottom surface" manufactured to give the bottom surface of a conventional nail sticker that can be cured by ultraviolet light, the shape is deformed the moment the external force is applied, but it is likely to return to a flat shape as soon as the external force is removed.

[0043] That is, in the conventional technology, it was never possible to manufacture nail stickers (gel nail stickers) that can be cured by ultraviolet light into a curved shape like a nail.

[0044] However, in the case of the nail sticker of the present invention, since a layer not found in the past is included, it can have a curved shape like a nail. Furthermore, "can have a curved shape" can mean that the nail sticker maintains a curved shape to a considerable degree.

[0045] Furthermore, the nail sticker of the present invention can be manufactured by a manufacturing method that has not been used in the past, so that the nail sticker can more effectively maintain its curved shape.

[0046] In short, the nail sticker of the present invention has a major feature in that the lower surface of the nail sticker before being hardened by ultraviolet light can include a curved surface that causes the center of the nail sticker to face upward, without the need for intentionally applying any external force (except natural forces such as gravity) to the nail sticker.

[0047] For example, the nail sticker of the present invention has a curved center of the underside of the nail sticker toward the upper part, and when the nail sticker is placed on a flat floor with the underside of the nail sticker facing the floor, it is possible that the center of the underside of the nail sticker will not come into contact with the flat floor even after 24 hours.

[0048] The nail sticker may include a soft layer. The soft layer may include a resin for the soft layer. The resin for the soft layer may include at least one of cellulose acetate butyrate and cellulose acetate propionate.

[0049] Therefore, in the manufacturing process of the nail sticker according to the embodiment of the present invention, the nail sticker can be easily deformed into a nail shape and the deformed shape of the nail sticker can be effectively maintained. That is, the use of the soft layer corresponds to a main factor that enables the lower surface of the nail sticker before being hardened by ultraviolet light to include a curved surface in which the center of the nail sticker is curved toward the upper part.

[0050] In addition, when a user applies a certain amount of force during the process of attaching the nail sticker, the soft layer can fill the gap between the nail and the nail sticker, effectively maintaining the filled shape, thereby reducing the foreign body sensation felt by the user and increasing the adhesive strength of the nail sticker.

[0051] Furthermore, when a portion of the nail sticker extends beyond the nail area, the soft layer can support the portion of the nail sticker that extends beyond the nail area so that it is not deformed. Even if the nail surface is uneven, the soft layer can be deformed so that more of the soft layer is placed on the concave portion of the nail surface by applying a certain force.

[0052] As a result, even if the nail surface is uneven, the surface of the applied nail sticker can have a smooth shape, improving aesthetics. Furthermore, the cellulose acetate butyrate and the cellulose acetate propionate have the advantage of being superior in shock absorption compared to other materials.

[0053] More specifically, the resin for the soft layer may include cellulose acetate butyrate, for example, the resin for the soft layer may be cellulose acetate butyrate. In this case, it has excellent impact absorption ability and durability, and when mixed with the UV-curable raw material for the soft layer, its ductility increases, so that the deformation of the soft layer due to external impact is irreversible due to the impact absorption effect, and the shape once deformed can be more easily maintained. Therefore, it is possible to provide a nail sticker having a nail shape to the user.

[0054] The resin for the soft layer may be contained in the soft layer in an amount of 10% by weight to 90% by weight, specifically 15% by weight to 75% by weight, more specifically 30% by weight to 65% by weight. When the above range is satisfied, the soft layer can be easily deformed at body temperature and the deformed shape of the soft layer can be maintained. Therefore, a nail sticker having a nail shape can be provided to the user.

[0055] The soft layer may further include an ultraviolet-curable material for the soft layer, so that the soft layer can be cured by ultraviolet irradiation.

[0056] The UV-curable raw material for the soft layer may include at least one selected from the group consisting of urethane acrylate oligomers, polyester acrylate oligomers, polyether acrylate oligomers, epoxy acrylate oligomers, polycarbonate acrylate oligomers, silicone acrylate oligomers, and acrylic acrylate oligomers.

[0057] Specifically, the UV-curable raw material for the soft layer may include at least one of a urethane acrylate oligomer, a polyester acrylate oligomer, and an epoxy acrylate oligomer.

[0058] The urethane acrylate oligomer is advantageous because it can be easily cured by ultraviolet light and has a certain degree of flexibility even after curing. In addition, the haze phenomenon can be minimized, so that the transparency of the coating layer can be maintained. The urethane acrylate oligomer may include at least one of a difunctional urethane acrylate oligomer, a tetrafunctional urethane acrylate oligomer, a hexafunctional urethane acrylate oligomer, and a nonafunctional urethane acrylate oligomer.

[0059] Specifically, the urethane acrylate oligomer may include at least one selected from the group consisting of PU210, PU280, PU640, and SC2404, which are products of Miwon, and CN9033 and CN9047, which are products of SATOMER. The weight average molecular weight of the urethane acrylate oligomer may be 1,000 g / mol to 1,000,000 g / mol, specifically, 1,000 g / mol to 100,000 g / mol. When the above range is satisfied, the workability can be significantly improved.

[0060] The epoxy acrylate oligomer has high reactivity, good hardness and abrasiveness, is easy to cure, has excellent flexibility, and can cure stably even when in contact with oxygen. The epoxy acrylate oligomer may have one or two functional groups, and when there is one functional group, it shows ductility, and the higher the number of functional groups, the more advantageous it is in terms of rigidity or thermal stability.

[0061] Specifically, the epoxy acrylate oligomer may include at least one selected from the group consisting of PE210, PE2120, and PE250, which are products of Miwon Co., Ltd. The weight average molecular weight of the epoxy acrylate oligomer may be 100 g / mol to 10,000 g / mol, specifically, 500 g / mol to 6,000 g / mol. Taking into consideration the solid content and viscosity of the soft layer forming composition, it is preferable that the weight average molecular weight is within the above range.

[0062] The polyester acrylate oligomer has excellent reactivity and adhesiveness superior to urethane acrylate oligomers and epoxy acrylate oligomers. The polyester acrylate oligomer may be an oligomer having 4 or 6 functional groups.

[0063] Specifically, the polyester acrylate oligomer may include at least one selected from the group consisting of PS4040, PS460, PS6300 Etermer 6311-100, 6312-100, and 6314C-60, which are products of Miwon Co., Ltd. The weight average molecular weight of the polyester acrylate oligomer may be 500 g / mol to 50,000 g / mol, specifically, 1,500 g / mol to 38,000 g / mol. When the above range is satisfied, processability and adhesive strength can be improved.

[0064] In the soft layer, the epoxy acrylate oligomer may be contained in an amount of 1 to 10 parts by weight, specifically 1 to 3 parts by weight, relative to 100 parts by weight of the urethane acrylate oligomer. In the soft layer, the polyester acrylate oligomer may be contained in an amount of 10 to 20 parts by weight, specifically 2 to 8 parts by weight, relative to 100 parts by weight of the urethane acrylate oligomer. When the above composition is satisfied, rapid hardening does not occur even when the soft layer is exposed to air, and durability can be maintained even after the nail sticker is attached.

[0065] Alternatively, the UV-curable raw material for the soft layer may include the urethane acrylate oligomer, and more specifically, may consist of the urethane acrylate oligomer.

[0066] The UV-curable raw material for the soft layer may be contained in the soft layer at 10% by weight to 90% by weight, specifically 15% by weight to 75% by weight, more specifically 30% by weight to 65% by weight. When the above range is satisfied, the soft layer maintains a soft physical property before UV irradiation, but has a very hard physical property after curing by UV irradiation.

[0067] In the soft layer, the weight ratio of the UV-curable raw material for the soft layer and the resin for the soft layer may be 10:90 to 90:10, specifically 20:80 to 80:20, more specifically 30:70 to 70:30. When the above range is satisfied, the impact absorption property of the resin for the soft layer and the viscosity of the UV-curable raw material for the soft layer are mixed, and the external impact energy absorption capacity is increased.

[0068] The photoinitiator for the soft layer serves to initiate a polymerization reaction by irradiation with ultraviolet light. Specifically, the photoinitiator may be an ultraviolet photoinitiator.

[0069] The photoinitiator for the soft layer may have an absorption wavelength band in the range of 200 nm to 600 nm.

[0070] The photoinitiator for the soft layer may include at least one selected from the group consisting of trimethylbenzoyl phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, but is not necessarily limited thereto.

[0071] The photoinitiator for the soft layer may be contained in the soft layer at 1 wt% to 10 wt%, specifically 1 wt% to 8 wt%, more specifically 2 wt% to 7 wt%. When the above range is satisfied, the nail sticker can have an appropriate hardness when the user cures the nail sticker.

[0072] The maximum thickness of the soft layer may be 250 μm to 2500 μm, specifically 700 μm to 2400 μm, more specifically 1000 μm to 2000 μm. When the above range is satisfied, the nail sticker of the present invention can be easily manufactured, in which the lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface in which the center of the nail sticker is curved toward the upper portion.

[0073] In addition, when the above range is satisfied, a sufficient amount of the soft layer can be moved to minimize the lift between the nail sticker and the nail. Furthermore, when a portion of the nail sticker extends beyond the nail area, the soft layer can more effectively support the extended and protruding portion of the nail sticker so that it is not deformed.

[0074] In addition, even if the nail surface is uneven, the movement of the soft layer allows more of the soft layer to be positioned sufficiently on the concave parts of the nail, so that the surface of the applied nail sticker can have a smoother shape.

[0075] In addition, since the soft layer may not have a high rate of change even when subjected to an external impact, the effect can be smoothly maintained. The maximum thickness of the soft layer may mean the largest thickness among thicknesses of the soft layer measured in a vertical direction from any fulcrum on the lower surface of the soft layer.

[0076] The soft layer may be a single layer, or alternatively, may be made up of two or more layers.

[0077] The nail sticker may further include a base layer, and the soft layer may be disposed on the base layer.

[0078] 4, the upper surface of the base layer 120 and the lower surface of the soft layer 110 may face each other or may be in contact with each other. That is, the soft layer 110 may be positioned on the base layer 120.

[0079] The substrate layer may include an adhesive layer that provides a chemical adhesion that allows the nail sticker to be attached to a nail, and the adhesive layer may be located below the nail sticker and may form at least a portion of the lower surface of the nail sticker.

[0080] The adhesive layer may constitute at least a part of the bottom surface of the nail sticker. The adhesive layer includes an adhesive component, which may correspond to an adhesive component commonly used in the art.

[0081] The base layer may further include a design layer. The design layer may be located between the adhesive layer and the soft layer. The design layer may include at least one of a color layer and a print layer. The design layer may include a pigment that imparts color to the nail sticker. The print layer may include particles for expressing a shape, various materials for aesthetics such as mica, etc.

[0082] A base film may be disposed on the lower surface of the base layer. The base film serves to prevent contamination of the adhesive layer and maintain the adhesive strength before using the nail sticker, and is removed when using the nail sticker. The base film may include components commonly used in the art.

[0083] The nail sticker may further include a coating layer.

[0084] Referring to FIG. 4 , in the nail sticker 100 , the coating layer 130 may be located on the soft layer 110 .

[0085] The coating layer may include an ultraviolet curing material for the coating layer and a resin for the coating layer.

[0086] Since the UV-curable raw material for the coating layer is included in the coating layer, the user can deform the nail sticker so that it adheres closely to the user's nail, and then irradiate the nail sticker with UV light to harden it according to the deformed shape of the nail sticker. As a result, the nail sticker and the fingernail / toenail can be bonded to each other in a completely adhered state, improving the adhesive strength of the nail sticker.

[0087] The UV-curable raw material for the coating layer may include at least one selected from the group consisting of urethane acrylate oligomers, polyester acrylate oligomers, polyether acrylate oligomers, epoxy acrylate oligomers, polycarbonate acrylate oligomers, silicone acrylate oligomers, and acrylic acrylate oligomers.

[0088] Specifically, the UV-curable raw material for the coating layer may include at least one of a urethane acrylate oligomer, a polyester acrylate oligomer, and an epoxy acrylate oligomer.

[0089] The urethane acrylate oligomer is advantageous in that it can be easily cured by ultraviolet light and has a certain degree of flexibility even after curing, and can minimize the haze phenomenon, thereby maintaining the transparency of the coating layer.

[0090] The urethane acrylate oligomer may include at least one of a difunctional urethane acrylate oligomer, a tetrafunctional urethane acrylate oligomer, a hexafunctional urethane acrylate oligomer, and a nonafunctional urethane acrylate oligomer.

[0091] Specifically, the urethane acrylate oligomer may include at least one selected from the group consisting of PU210, PU280, PU640, and SC2404, which are products of Miwon, and CN9033 and CN9047, which are products of SATOMER. The weight average molecular weight of the urethane acrylate oligomer may be 1,000 g / mol to 1,000,000 g / mol, specifically, 1,000 g / mol to 100,000 g / mol. When the above range is satisfied, the workability can be significantly improved.

[0092] The epoxy acrylate oligomer has high reactivity, good hardness and abrasiveness, is easy to cure, has excellent flexibility, and can cure stably even when in contact with oxygen. The epoxy acrylate oligomer may have one or two functional groups, and when there is one functional group, it shows ductility, and the higher the number of functional groups, the more advantageous it is in terms of rigidity or thermal stability.

[0093] Specifically, the epoxy acrylate oligomer may include at least one selected from the group consisting of PE210, PE2120, and PE250, which are products of Miwon Co., Ltd. The weight average molecular weight of the epoxy acrylate oligomer may be 100 g / mol to 10,000 g / mol, specifically, 500 g / mol to 6,000 g / mol. Taking into consideration the solid content and viscosity of the composition for forming a coating layer, it is preferable that the weight average molecular weight is within the above range.

[0094] The polyester acrylate oligomer has excellent reactivity and adhesiveness superior to urethane acrylate oligomer and epoxy acrylate oligomer. The polyester acrylate oligomer may be an oligomer having 4 or 6 functional groups. Specifically, the polyester acrylate oligomer may include at least one selected from the group consisting of PS4040, PS460, PS6300 Etermer 6311-100, 6312-100, and 6314C-60, which are products of Miwon.

[0095] The weight average molecular weight of the polyester acrylate oligomer may be 500 g / mol to 50,000 g / mol, specifically, 1,500 g / mol to 38,000 g / mol. When the weight average molecular weight is within the above range, the processability and adhesive strength can be improved.

[0096] In the coating layer, the epoxy acrylate oligomer may be contained in an amount of 1 part by weight to 10 parts by weight, specifically 1 part by weight to 3 parts by weight, relative to 100 parts by weight of the urethane acrylate oligomer.

[0097] In the coating layer, the polyester acrylate oligomer may be contained in an amount of 10 parts by weight to 20 parts by weight, specifically 2 parts by weight to 8 parts by weight, based on 100 parts by weight of the urethane acrylate oligomer.

[0098] When this composition is satisfied, rapid hardening does not occur even when the coating layer is exposed to air, and durability can be maintained even after the nail sticker is attached.

[0099] Alternatively, the UV-curable raw material for the coating layer may include the urethane acrylate oligomer, and more specifically, may consist of the urethane acrylate oligomer.

[0100] The UV-curable raw material for the coating layer may be contained in the coating layer at 10% by weight to 90% by weight, specifically 10% by weight to 60% by weight, more specifically 20% by weight to 50% by weight. When the above range is satisfied, the coating layer maintains a flexible physical property before UV irradiation, but has a very hard physical property after curing by UV irradiation.

[0101] The resin for the coating layer may control the fluidity of the coating layer to maintain its shape, and the composition for forming the coating layer may have an appropriate viscosity due to the resin for the coating layer, so that the coating layer may be formed in a desired shape.

[0102] The resin for the coating layer may be a thermoplastic resin for the coating layer having a glass transition temperature (Tg) of 30° C. to 200° C., specifically 50° C. to 120° C. When the resin for the coating layer satisfies the above range, the mobility of the resin for the coating layer is not high at room temperature, but the resin for the coating layer is appropriately mixed with the ultraviolet curing raw material in a drying oven during the manufacturing process of the nail sticker, so that the horizontal lines of the nail sticker can be smoothly formed.

[0103] The coating layer resin may include at least one selected from the group consisting of an acrylic coating layer resin, a nitrocellulose coating layer resin, an epoxy coating layer resin, a polyester coating layer resin, a polyvinyl coating layer resin, a urethane coating layer resin, and a vinyl acetate coating layer resin.

[0104] In particular, the resin for the coating layer may include a resin for an acrylic coating layer and a resin for a nitrocellulose coating layer. The glass transition temperature (Tg) of the resin for the acrylic coating layer may be 30° C. to 200° C., specifically, 50° C. to 120° C. The resin for the nitrocellulose coating layer may include Korea CNC HRS1 / 8~20SS type 1 / 8~1 / 2.

[0105] The nitrogen content of the resin for the nitrocellulose coating layer may be 11.5% to 12.2%, and specifically, it can be divided into 1 / 8 seconds to 20 seconds depending on the viscosity. When the above range is satisfied, low viscosity can be maintained and the solid content can be increased.

[0106] The resin for the coating layer may be contained in the coating layer in an amount of 10% by weight to 90% by weight, specifically 15% by weight to 75% by weight, more specifically 15% by weight to 70% by weight. When the resin for the coating layer is contained in the coating layer in an amount of 10% by weight to 90% by weight, specifically 15% by weight to 75% by weight, more specifically 15% by weight to 70% by weight, the resin is sufficiently less sticky that it can be handled at room temperature without any problems, and a round shape can be formed.

[0107] Meanwhile, the resin for the coating layer may include a thermosetting resin for the coating layer and a thermal initiator.

[0108] The coating layer may further include a photoinitiator for the coating layer.

[0109] The photoinitiator serves to initiate a polymerization reaction upon irradiation with ultraviolet light. Specifically, the photoinitiator may be an ultraviolet photoinitiator.

[0110] The photoinitiator may have an absorption wavelength band in the range of 200 nm to 600 nm.

[0111] The photoinitiator may include at least one selected from the group consisting of trimethylbenzoyl phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, but is not necessarily limited thereto.

[0112] The photoinitiator may be contained in the coating layer at 1 wt % to 10 wt %, specifically 1 wt % to 8 wt %, more specifically 2 wt % to 7 wt %. When the photoinitiator is contained in the coating layer at the content in the above range, the coating layer can have an appropriate hardness when the user cures the coating layer.

[0113] In some cases, the coating layer may contain a solvent. The solvent corresponds to the solvent used in forming the coating layer-forming composition for producing the coating layer, and is removed by drying during the production of the coating layer. However, a very small amount of the solvent may remain in the coating layer.

[0114] The nail sticker may further include a design expression layer disposed on the coating layer. The design expression layer may express a matte finish, a three-dimensional line, or a thick-film type three-dimensional figure such as a cone or a circular dome.

[0115] The maximum thickness of the nail sticker may be 500 μm to 2,500 μm, specifically 700 μm to 2,000 μm, more specifically 1,000 μm to 1,800 μm. When the thickness satisfies the above range, the nail sticker has high aesthetics, does not crack when cured by ultraviolet light, and reduces the phenomenon of pinching the nail.

[0116] When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being hardened by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 in an atmosphere at a temperature of 25°C may be 4% or less, specifically 0% to 3%, more specifically 0% to 2.1%.

[0117] [Formula 1] Deformation ratio = [(BA) / A] x 100 In the above formula 1, The A may mean the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor, and the B may mean the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor. In this specification, "on a flat floor" may mean directly above a flat floor.

[0118] The nail sticker has a deformation rate of 30% or less according to the following formula 1 in an atmosphere at 25° C., so that the shape of the nail sticker can be maintained to the maximum extent even during the process of delivering the product to the user. Also, the user can more easily shape the nail sticker to fit the shape of their own nails.

[0119] In addition, the nail sticker maintains its shape well even during the process of application and hardening of the nail sticker by the user, so the user can use it easily and wear the nail sticker that best suits their nails.

[0120] The deformation rate corresponds to a very low value compared to conventional UV-curable nail stickers. The main reason for such a low deformation rate may be that the nail sticker of this embodiment includes a soft layer.

[0121] More specifically, the deformation rate of the nail sticker may be 2.2% or less, more specifically, 0% to 2.2%, or 0% to 2.1%, in an atmosphere at a temperature of 25° C. In addition to the use of a soft layer, the nail sticker may be deformed into a nail shape and then heated during the manufacturing process of the nail sticker, which may be the main reason why such a lower deformation rate is shown.

[0122] When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being hardened by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 in an atmosphere at a temperature of -10°C may be 0.2% or less, specifically 0% to 0.2%, more specifically 0% to 0.1%.

[0123] [Formula 1] Deformation ratio = [(BA) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor, and the B means the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

[0124] The nail sticker has a deformation rate of 0.2% or less according to the following formula 1 in an atmosphere at a temperature of -10°C, so the shape of the nail sticker can be maintained even at low temperatures (e.g., when stored in a place with low temperature or in winter). Therefore, the shape of the nail sticker can be maintained to the maximum extent even during the process of supplying the product to the user.

[0125] When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being hardened by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 in an atmosphere at a temperature of 40°C may be 6% or less, specifically 4.5% or less, more specifically 0% to 4.3%, for example 0% to 3%.

[0126] [Formula 1] Deformation ratio = [(BA) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor, and the B means the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

[0127] The nail sticker has a deformation rate of 6% or less according to the following formula 1 in an atmosphere at a temperature of 40° C., so the shape of the nail sticker can be maintained even at high temperatures (e.g., when stored in a hot place or in summer). Therefore, the shape of the nail sticker can be maintained to the maximum extent even during the process of supplying the product to the user.

[0128] When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being hardened by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 in an atmosphere at a temperature of 60°C may be 8% or less, specifically 7% or less, more specifically 0% to 7%, for example 0% to 5%.

[0129] [Formula 1] Deformation ratio = [(BA) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor, and the B means the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

[0130] The nail sticker has a deformation rate of 6% or less according to the following formula 1 in an atmosphere at a temperature of 60° C., so the shape of the nail sticker can be maintained even at high temperatures (e.g., when stored in a hot place or in summer). Therefore, the shape of the nail sticker can be maintained to the maximum extent even during the process of supplying the product to the user.

[0131] When the nail sticker before being cured by ultraviolet rays is placed on a flat floor and the area including the center of the upper surface of the nail sticker is pressed with a force of 10 N using a push gauge device made by Imada, the lower surface of the center of the nail sticker can contact the floor. In other words, the nail sticker is not a hard molded product but is flexible, so it is a nail sticker (so-called gel nail sticker) that is easily deformed when an external force is applied.

[0132] <Manufacturing method of nail stickers> A method for manufacturing a nail sticker according to another embodiment of the present invention includes a first step of placing a preliminary nail sticker that can be cured by ultraviolet light on a support part included in a support structure; and a second step of applying pressure toward an upper surface of the preliminary nail sticker to bring a lower surface of the preliminary nail sticker into close contact with an upper surface of the support part, wherein the support part has a convex curved surface toward an upper portion, and the lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface that is curved such that a center of the nail sticker is curved toward an upper portion.

[0133] In the first step, the preliminary nail sticker 100' that can be cured by ultraviolet light may have a shape as shown in Fig. 5 before being placed on the support. That is, the preliminary nail sticker 100' may have a flat bottom surface or may have a curve, but the degree of curvature is not as severe as that of a general nail.

[0134] That is, before the spare nail sticker 100' is placed on the support structure, when the nail sticker is placed on the flat floor so that the bottom surface of the spare nail sticker 100' before being cured by ultraviolet light faces the flat floor, the bottom surface of the spare nail sticker can be flat.

[0135] The preliminary nail sticker 100' may include a soft layer 110, and may further include a base layer 120. Alternatively, the preliminary nail sticker may include a soft layer 110, a base layer 120, and a coating layer 130. Here, the soft layer, the base layer, and the coating layer have the same configurations as those of the soft layer, the base layer, and the coating layer described as including the nail sticker of the embodiment described above, and therefore the description thereof will be omitted.

[0136] 7, in the first step, a preliminary nail sticker 100' that can be cured by ultraviolet light (not yet cured by ultraviolet light) can be placed on a support structure 200 including a support portion 210 having a convex curved surface toward the top. FIG. 6 is a schematic diagram of the support structure 200.

[0137] The support structure 200 may include one or more support parts 210, specifically, two or more support parts 210. The support part 210 may have a convex curved surface toward the upper part, specifically, the support part 210 may have a nail shape. The preliminary nail sticker 100' may be placed on the support part 210 such that the lower surface of the preliminary nail sticker 100' is in contact with the upper surface of the support part 210.

[0138] The material of the upper surface of the support may include at least one selected from the group consisting of polyethylene, polypropylene, and silicone, and may specifically include polyethylene, and more specifically, the upper surface of the support may be made of polyethylene. Since the upper surface of the support includes polyethylene, the adhesive strength between the nail sticker and the support is not very large, and therefore, when the nail sticker is separated from the support, unintended deformation of the nail sticker can be minimized.

[0139] Referring to FIG. 8, in a second step, pressure is applied toward the upper surface of the preliminary nail sticker to bring the lower surface of the preliminary nail sticker into close contact with the upper surface of the support.

[0140] Specifically, the preliminary nail sticker can be attached to the support portion 210 by applying pressure to the upper surface of the preliminary nail sticker using a pressure-bonding member having a nail-shaped recess.

[0141] However, the present invention is not limited to this method, and other methods are possible for adhering the preliminary nail sticker to the support part 210. The nail sticker 100 according to the embodiment of the present invention can be manufactured by the second step. That is, the lower surface of the nail sticker before being cured by ultraviolet light may include a curved surface that is curved such that the center of the nail sticker is directed upward.

[0142] Referring to FIG. 9, the method for manufacturing the nail sticker may further include a third step of applying heat to the preliminary nail sticker 100' adhered to the support 210 after the second step.

[0143] This allows the nail sticker to more effectively maintain the nail shape (the lower surface of the nail sticker before being hardened by ultraviolet light includes a curved surface in which the center of the nail sticker is curved toward the upper surface). The heat applied in the third step may be heat at a temperature of 30°C to 70°C, specifically, heat at a temperature of 45°C to 55°C. When the above range is satisfied, there is an effect that the degree of change in the shape of the product during storage is significantly reduced while maintaining flexibility.

[0144] The heat can be applied for 20 seconds to 3 minutes, specifically 30 seconds to 2 minutes. The heat can be applied by applying hot air or near infrared rays.

[0145] <Nail sticker set> A nail sticker set according to another embodiment of the present invention includes a support structure including a support part; and a nail sticker attached to an upper surface of the support part; the upper surface of the support part includes a curved surface curved such that a center of the sticker faces upward, the nail sticker is curable by ultraviolet light, and an outer surface of the nail sticker before being cured by ultraviolet light includes a curved surface curved such that a center of the nail sticker faces upward.

[0146] Here, since the nail sticker is the same as the nail sticker of the embodiment described above, the physical properties of the nail sticker of the embodiment described above may be the same as the physical properties of the nail sticker (the nail sticker peeled off from the support structure) mentioned in this embodiment. Also, referring to Fig. 10, the support structure 200 may be the same as the support structure described in the other embodiment described above.

[0147] 10, in the nail sticker set 300, the nail sticker 100 is disposed on the support 210. The nail sticker 100 and the support 210 may both have a nail shape and overlap each other. That is, the lower surface of the nail sticker before being cured by ultraviolet light may include a curved surface in which the center of the nail sticker is curved toward the upper side, and the support may also have the same shape.

[0148] 11 and 12 are photographs of a nail sticker set according to an embodiment of the present invention. More than 50%, specifically more than 70%, more specifically 90% to 100%, for example 95% to 100%, of the lower surface of the nail sticker may be in contact with the upper surface of the support. This means that the nail sticker described in the present invention can effectively maintain the nail shape, and thus it is possible to minimize the separation of the lower surface of the nail sticker and the support structure from each other during the process of delivering the nail sticker to the user.

[0149] When the nail sticker is peeled off from the support and placed on a flat floor with the underside of the nail sticker before being cured by ultraviolet rays facing the flat floor, the center of the nail sticker may be spaced apart from the floor, which allows a user to more easily shape the nail sticker to fit the shape of their own nail.

[0150] In addition, the nail sticker maintains its shape well even during the process of application and hardening of the nail sticker by the user, making it easy for the user to use and allowing the user to wear the nail sticker that best suits their nails.

[0151] When the nail sticker is peeled off from the support and placed on a flat floor with the bottom surface of the nail sticker before being hardened by ultraviolet light facing the flat floor, the deformation rate according to the following formula 1 in an atmosphere at a temperature of 25°C may be 4% or less, specifically 0% to 3%, more specifically 0% to 2.1%.

[0152] [Formula 1] Deformation ratio = [(BA) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor, and the B means the maximum lateral length of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

[0153] The nail sticker has a deformation rate of 4% or less according to the following formula 1 in an atmosphere at a temperature of 25°C, so that the shape of the nail sticker can be maintained to the maximum extent even during the process of supplying the product to the user. Also, the user can more easily shape the nail sticker to fit the shape of their own nails. Also, the nail sticker can maintain its shape well even during the series of processes in which the user applies the nail sticker and hardens it, so that the user can use it easily and wear the nail sticker that fits the user's nails better.

[0154] The material of the upper surface of the support may include at least one selected from the group consisting of polyethylene, polypropylene, and silicone, and may specifically include polyethylene, and more specifically, the upper surface of the support may be made of polyethylene. Since the upper surface of the support includes polyethylene, the adhesive strength between the nail sticker and the support is not very strong, and therefore, when the nail sticker is separated from the support, unintended deformation of the nail sticker can be minimized.

[0155] The support structure may include one or more, specifically two or more supports, and the nail sticker set may include one or more, specifically two or more nail stickers.

[0156] Below, preferred embodiments are presented to aid in understanding the present invention. However, the above embodiments are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications fall within the scope of the appended claims.

[0157] <Examples and Comparative Examples> Example 1 (1) Prepare spare nail stickers A nail sticker was prepared, which included a base layer (maximum thickness: 150 μm) including an adhesive layer and a design layer, a soft layer (maximum thickness: 2000 μm) disposed on the base layer, and a coating layer (maximum thickness: 65 μm) disposed on the soft layer.

[0158] The soft layer contains 60% by weight of cellulose acetate butyrate, which is a resin for the soft layer, 38% by weight of urethane acrylate oligomer, which is an ultraviolet curing raw material for the soft layer, and 2% by weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, which is a photoinitiator for the soft layer.

[0159] The coating layer includes urethane acrylate, which is an ultraviolet curing raw material for the coating layer, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, which is a photoinitiator for the coating layer, and nitrocellulose, which is a resin for the coating layer.

[0160] (2) Forming spare nail stickers On the other hand, a support structure including a support part having an upper surface with a convex center like the upper surface of a nail was prepared. The preliminary nail sticker was placed on the upper surface of the support part. At this time, the adhesive layer on the lower surface of the preliminary nail sticker was in contact with the upper surface of the support part.

[0161] Then, pressure was applied to the upper surface of the preliminary nail sticker so that the lower surface of the preliminary nail sticker was in close contact with the upper surface of the support part included in the support structure, so that the preliminary nail sticker supported by the support part had a curved shape with the center pointing upward like a nail.

[0162] The preliminary nail sticker placed on the support structure was irradiated with near infrared rays and heated at a temperature of 50° C. for 2 minutes to produce a nail sticker set including the nail sticker and the support structure. There was no process of curing by irradiating with ultraviolet rays during the manufacturing process.

[0163] Example 2 (1) Prepare spare nail stickers A nail sticker was prepared, which included a base layer (maximum thickness: 150 μm) including an adhesive layer and a design layer, a soft layer (maximum thickness: 2000 μm) disposed on the base layer, and a coating layer (maximum thickness: 65 μm) disposed on the soft layer.

[0164] The soft layer contains 60% by weight of cellulose acetate butyrate, which is a resin for the soft layer, 38% by weight of urethane acrylate oligomer, which is an ultraviolet curing raw material for the soft layer, and 2% by weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, which is a photoinitiator for the soft layer.

[0165] The coating layer includes urethane acrylate, which is an ultraviolet curing raw material for the coating layer, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, which is a photoinitiator for the coating layer, and nitrocellulose, which is a resin for the coating layer.

[0166] (2) Forming spare nail stickers Meanwhile, a support structure including a support part having an upper surface with a convex center like the upper surface of a nail was prepared. The spare nail sticker was placed on the upper surface of the support part. At this time, pressure was applied toward the upper surface of the spare nail sticker, so that the adhesive layer on the lower surface of the spare nail sticker came into contact with the upper surface of the support part. As a result, the spare nail sticker supported by the support part had a curved shape with the center pointing up like a nail.

[0167] The preliminary nail sticker supported by the support was left at room temperature for 2 hours to manufacture a nail sticker set including the nail sticker and the support structure. No process of curing by irradiation with ultraviolet light was performed during the manufacturing process.

[0168] Comparative Example 1 (1) Prepare spare nail stickers A nail sticker was prepared, which included a base layer (maximum thickness: 150 μm) including an adhesive layer and a design layer, a first coating layer (maximum thickness: 2000 μm) disposed on the base layer, and a second coating layer (maximum thickness: 65 μm) disposed on the first coating layer.

[0169] The first coating layer contains 60% by weight of nitrocellulose as a resin for the first coating layer, 38% by weight of urethane acrylate oligomer as an ultraviolet curing raw material for the first coating layer, and 2% by weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide as a photoinitiator for the first coating layer.

[0170] The second coating layer includes urethane acrylate, which is an ultraviolet curing raw material for the second coating layer, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, which is a photoinitiator for the second coating layer, and nitrocellulose, which is a resin for the second coating layer.

[0171] (2) Forming spare nail stickers Meanwhile, a support structure was prepared, including a support part having an upper surface with a convex center like the upper surface of a nail. The spare nail sticker was placed on the upper surface of the support part. At this time, the adhesive layer on the lower surface of the spare nail sticker was in contact with the upper surface of the support part. Then, an external force was applied toward the upper surface of the spare nail sticker, so that the lower surface of the spare nail sticker was in close contact with the upper surface of the support part included in the support structure. As a result, the spare nail sticker supported by the support part had a curved shape with the center pointing up like a nail.

[0172] The preliminary nail sticker supported by the support portion was left at room temperature for 2 hours to prepare a nail sticker set including the nail sticker and the support structure.

[0173] There was no UV light curing step during the manufacturing process.

[0174] Experimental Example 1: Evaluation of whether the shape is maintained and the deformation rate (1) Evaluation at 25°C Immediately after separating the nail sticker of Example 1 from the support, the nail sticker (not cured by ultraviolet light) was placed on a flat floor. Specifically, when the nail sticker before curing was placed on the flat floor with the bottom surface of the nail sticker before curing facing downward, the center of the nail sticker was separated from the floor and maintained a curved shape with the center facing upward.

[0175] Specific results are shown in Table 1 and FIGS.

[0176] Fig. 13 is a photograph of the nail sticker of Example 1 immediately after it was produced, and Fig. 14 is a photograph of the nail sticker of Example 1 after it was left for 24 hours. Fig. 15 is a photograph of the nail sticker of Example 2 immediately after it was produced, and Fig. 16 is a photograph of the nail sticker of Example 2 after it was left for 24 hours. Fig. 17 is a photograph of the nail sticker of Comparative Example 1 immediately after it was produced, and Fig. 18 is a photograph of the nail sticker of Comparative Example 1 after it was left for 24 hours.

[0177] It can be seen that the nail stickers of Examples 1 and 2 maintained their shape even after 24 hours, whereas the nail sticker of Comparative Example 1 was unable to maintain its shape after 24 hours.

[0178] (2) Evaluation at -10℃, 40℃, and 60℃ The same experiment as above was carried out at −10° C., 40° C., and 60° C., respectively, and the results are shown in Table 1.

[0179] [Table 1]

[0180] The term "whether the shape is maintained" refers to whether the nail sticker maintains its curved shape with the center pointing upwards (whether the center of the bottom surface of the nail sticker maintains its state of being separated from the floor) when placed on a flat floor and left for 24 hours. In other words, it refers to whether the curved shape is maintained during the process of being supplied to consumers (O if maintained, X if not). The deformation rate was calculated according to the following formula 1.

[0181] [Formula 1] Deformation ratio = [(BA) / A] x 100 In the formula 1 and table 1, the A value is the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor, and the B value is the maximum width of the nail sticker measured after the nail sticker is left on the flat floor for 1 hour. [Explanation of symbols]

[0182] 100: Nail stickers 110: Soft layer 120: Base material layer 130: Coating layer 200: Support structure 210: Support part 300: Nail sticker set

Claims

1. A nail sticker that can be cured by ultraviolet light, The lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface that is curved so that the center of the nail sticker faces upward. Nail stickers.

2. When the nail sticker is placed on a flat floor such that the lower surface of the nail sticker before being cured by ultraviolet light faces the flat floor, the center of the nail sticker is spaced from the floor. The nail sticker according to claim 1.

3. When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being cured by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 is 4% or less in an atmosphere at a temperature of 25°C. The nail sticker according to claim 1. [Formula 1] Deformation ratio = [(B-A) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor; The B means the maximum width of the nail sticker measured one hour after the nail sticker was placed on the flat floor.

4. When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being cured by ultraviolet light facing the flat floor, the deformation rate according to the following formula 1 is 2.1% or less in an atmosphere at a temperature of 25°C. The nail sticker according to claim 1. [Formula 1] Deformation ratio = [(B-A) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor; The B means the maximum width of the nail sticker measured one hour after the nail sticker was placed on a flat floor.

5. When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being cured by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 is 0.2% or less in an atmosphere at a temperature of -10°C. The nail sticker according to claim 1. [Formula 1] Deformation ratio = [(B-A) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor; The B means the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

6. When the nail sticker is placed on a flat floor with the bottom surface of the nail sticker before being cured by ultraviolet light facing the flat floor, the deformation rate according to the following formula 1 is 6% or less in an atmosphere at a temperature of 40°C. The nail sticker according to claim 1. [Formula 1] Deformation ratio = [(B-A) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor; The B means the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

7. The nail sticker comprises at least one coating layer, The coating layer includes an ultraviolet curing material; The nail sticker according to claim 1.

8. The nail sticker includes a base layer, The substrate layer includes an adhesive layer. The nail sticker according to claim 1.

9. The adhesive layer is located under the nail sticker and constitutes at least a part of the lower surface of the nail sticker. The nail sticker according to claim 1.

10. When the nail sticker before being cured by ultraviolet light is placed on a flat floor and the upper surface of the nail sticker is pressed with a force of 10 N using a PUSH GAGE ​​device made by IMADA, the lower surface of the center of the nail sticker comes into contact with the floor. The nail sticker according to claim 1.

11. When the nail sticker is placed on a flat floor such that the lower surface of the nail sticker before being cured by ultraviolet rays faces the flat floor, at least a part of the edge of the nail sticker contacts the flat floor. The nail sticker according to claim 1.

12. The nail sticker includes a soft layer, The soft layer includes a resin for a soft layer, The resin for the soft layer contains at least one of cellulose acetate butyrate and cellulose acetate propionate. The nail sticker according to claim 1.

13. In the method for manufacturing nail stickers, The method for producing the nail sticker includes: A first step of placing a UV curable pre-nail sticker on a support included in a support structure; and a second step of applying pressure to the upper surface of the preliminary nail sticker to bring the lower surface of the preliminary nail sticker into close contact with the upper surface of the support. The support portion has a curved surface that is convex toward an upper portion, The lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface that is curved so that the center of the nail sticker faces upward. How to make nail stickers.

14. In the first stage, Before the preliminary nail sticker is placed on the support, When the nail sticker is placed on a flat floor so that a lower surface of the spare nail sticker before being cured by ultraviolet light faces the flat floor, the lower surface of the spare nail sticker is flat. The method for producing the nail sticker according to claim 13.

15. After the second step, The third step further includes applying heat to the preliminary nail sticker adhered to the support. The method for producing the nail sticker according to claim 13.

16. The heat applied in the third step is heat at a temperature of 30° C. to 70° C. The method for producing the nail sticker according to claim 15.

17. A support structure including a support portion; a nail sticker attached to an upper surface of the support, The upper surface of the support portion includes a curved surface that is curved such that the center of the nail sticker faces upward, The nail sticker is curable by ultraviolet light; The lower surface of the nail sticker before being cured by ultraviolet light includes a curved surface that is curved so that the center of the nail sticker faces upward. Nail sticker set.

18. 50% or more of the lower surface of the nail sticker is in contact with the upper surface of the support part. The nail sticker set according to claim 17.

19. When the nail sticker is peeled off from the support and placed on a flat floor such that the lower surface of the nail sticker before being cured by ultraviolet light faces the flat floor, the center of the nail sticker is separated from the floor. The nail sticker set according to claim 17.

20. When the nail sticker is peeled off from the support and placed on a flat floor with the bottom surface of the nail sticker before being cured by ultraviolet rays facing the flat floor, the deformation rate according to the following formula 1 is 4% or less in an atmosphere at a temperature of 25°C. The nail sticker set according to claim 17. [Formula 1] Deformation ratio = [(B-A) / A] x 100 In the above formula 1, The A means the maximum width of the nail sticker measured immediately after the nail sticker is placed on the flat floor; The B means the maximum width of the nail sticker measured one hour after the nail sticker is placed on the flat floor.

21. The material of the upper surface of the support portion includes at least one selected from the group consisting of polyethylene, polypropylene, and silicone. The nail sticker set according to claim 17.

22. The support structure includes two or more supports, The nail sticker set includes two or more nail stickers. The nail sticker set according to claim 17.

Citation Information

Patent Citations

  • Artificial nail for application to natural human nails

    DE202012012680U1

  • Method of manufacturing nail of artificial finger

    JP1992200503A

  • Nail tip-forming plate fitted to one's own nail and forming method for nail tip

    JP2004254877A

  • Method of manufacturing optical film, optical film, polarizing plate and liquid crystal display

    JP2008183758A

  • Manufacturing method for optical resin film and hard coat film

    JP2009082890A