New composite material for lithium secondary batteries, its preparation method and application
By uniformly embedding carbon atoms in nanosilicon at the atomic level, the composite material addresses structural instability and dispersion issues, enhancing the cyclic performance of silicon-based anodes in lithium-ion batteries.
Patent Information
- Application Number
- JP2024516719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-29
- Filing Date
- 2022-03-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-03-10
AI Technical Summary
Existing silicon-based anode materials for lithium-ion batteries face issues with structural destruction due to large body expansion during lithiation, poor conductivity, and difficulty in achieving uniform dispersion of silicon and carbon, leading to poor electrochemical performance.
A composite material is formed by thoroughly mixing a silicon source and a carbon source, resulting in carbon atoms being uniformly embedded at the atomic level within nanosilicon, forming an amorphous Si-C bond without SiC crystallization, with a carbon content of 0.5% to 50% and an average particle size of 1 nm to 50 μm.
The composite material exhibits a more stable structure with smaller body expansion during lithium insertion and desorption, improving cyclic characteristics and electrochemical performance in lithium batteries.
Smart Images

Figure 2024536764000001_ABST
Abstract
Description
[Technical field]
[0001] (cross reference) This application claims priority to a Chinese patent application filed with the China Patent Office on September 29, 2021, bearing application number 202111151405.1 and entitled "New composite material for lithium secondary batteries and its preparation method and application."
[0002] (Technical field) The present invention relates to the technical field of materials, in particular to a new type of composite material for lithium secondary batteries and its preparation method and application. [Background technology]
[0003] In recent years, with the rapid development of electronic technology and information industry, the development prospects of lithium-ion batteries are becoming more and more broad, and they have already been widely used in portable devices such as mobile phones, laptops, digital cameras, etc. In order to meet the ever-increasing needs for lithium-ion batteries with long cycle life, high energy density, and excellent rate characteristics in electric vehicles and large energy storage devices, many researchers are working to explore low-cost, high-quality electrode materials.
[0004] Among many new anode material candidates, silicon has an excellent theoretical specific capacity (4200 mAh g -1 ) has attracted much attention. However, the large volume expansion of silicon during the lithiation process leads to structural destruction and the formation of an unstable solid electrolyte interface (SEI) coating. Furthermore, silicon has poor intrinsic electrical conductivity, which significantly impairs the electrochemical performance of silicon, and the above problems have significantly hindered the practical application of silicon-based anodes.
[0005] Embedding silicon nanoparticles into carbon materials to prepare C / Si composite materials is one of the most effective methods, because it not only reduces the volume expansion of Si, but also combines the advantages of Si (high capacity) and carbon (good electrical conductivity and cycle stability). However, due to the relatively large surface energy of nanomaterials, they are prone to aggregation and it is difficult to achieve uniform dispersion in the carbon matrix, so the effect of improving electrochemical performance is poor. Patent Document 1 discloses a silicon-carbon composite anode material for lithium-ion batteries, but because mechanical mixing is used, the degree of mixing of silicon and carbon materials cannot achieve the expected effect, so that the cycle characteristics still cannot be significantly improved. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] China Patent Publication No. 106299277 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a new composite material for lithium secondary batteries and its preparation method and application. The silicon source and the carbon source are thoroughly mixed and then co-deposited, so that carbon atoms are uniformly embedded in the nanosilicon material at the atomic level. Compared with ordinary nanosilicon materials or silicon-carbon composite materials, the material has a more stable structure during the lithium insertion and extraction process, a smaller volume expansion, and better cycle properties when used in the negative electrode of a lithium battery. [Means for solving the problem]
[0008] In a first aspect, an embodiment of the present invention is a novel composite material for a lithium secondary battery, the novel composite material comprising nanosilicon and carbon atoms, the carbon atoms being uniformly distributed in the nanosilicon at the atomic level, the carbon atoms being bonded to silicon atoms to form amorphous Si-C bonds, and no crystallization peak of SiC being observed in X-ray diffraction (XRD); The solid-state nuclear magnetic resonance (NMR) measurement of the new composite material includes: 29 In the Si NMR spectrum, it is shown that when the silicon peak is at -70 ppm to -130 ppm, the Si-C resonance peak is present between 20 ppm and -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is (0.1, 5.0). The average particle size D of the new composite material 50 is 1 nm to 50 μm, and the mass of the carbon atoms accounts for 0.5% to 50% of the mass of the new composite material.
[0009] Preferably, the new composite material further contains oxygen element, which is dispersed inside or on the surface of the nanosilicon material, and the mass of the oxygen element accounts for 0.1% to 20% of the mass of the new composite material.
[0010] Preferably, the exotic composite material exists as a monomeric structure or the exotic composite material is deposited in or on a substrate, the monomeric structure comprising nanoparticles or nanowires.
[0011] In a second aspect, an embodiment of the present invention provides a method for preparing the novel composite material for a lithium secondary battery according to the first aspect, the method comprising: A silicon source, a carbon source, and a carrier gas are simultaneously blown into a reaction vessel in a proportional manner, and the temperature of the reaction vessel is controlled to 450°C to 1000°C and the reaction pressure is controlled to 0.1 atm to 10 atm; After the reaction is completed, the temperature is lowered to obtain the new composite material for lithium secondary batteries, or the product produced by the reaction during the reaction is introduced into a cooling chamber to obtain the new composite material for lithium secondary batteries; Includes.
[0012] Preferably, the silicon source is a silicon-containing vapor, specifically comprising one or more of the following combinations: monosilane, silicoethane, tetrafluorosilane, hexamethyldisilane, dimethylsiloxane; the carbon source comprises one or a combination of more of acetylene, methane, propylene, ethylene, propane, or ethanol; The carrier gas includes one or a combination of hydrogen, nitrogen, and argon.
[0013] In a third aspect, the present invention relates to an anode sheet comprising the novel composite material for lithium secondary batteries according to the first aspect above.
[0014] In a fourth aspect, an embodiment of the present invention relates to a lithium battery comprising the novel composite material for lithium secondary batteries according to the first aspect above. Effect of the Invention
[0015] The new composite material for lithium secondary batteries according to the present invention is obtained by thoroughly mixing a silicon source and a carbon source and then co-depositing them, thereby embedding carbon atoms uniformly into the nanosilicon material at the atomic level.Compared with conventional nanosilicon materials or silicon-carbon composite materials, the material has a more stable structure during the lithium insertion / extraction process, has a smaller volume expansion, and has better cycle characteristics when used in the anode of a lithium battery. [Brief description of the drawings]
[0016] Hereinafter, the technical solutions in the embodiments of the present invention will be described in more detail with reference to the drawings and examples.
[0017] [Figure 1] 1 is a flow chart of a method for preparing a new composite material for a lithium secondary battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 shows the XRD spectrum of the new composite material according to Example 1 of the present invention. [Diagram 3] FIG. 29Si NMR spectrum of the new composite material according to Example 1 of the present invention. [Figure 4] FIG. 29Si NMR spectrum of the new composite material according to Example 3 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be further described below with reference to the drawings and specific examples. However, it should be understood that these examples are merely for the purpose of explaining the present invention in more detail and are not intended to limit the present invention in any manner, i.e., they are not intended to limit the scope of protection of the present invention.
[0019] The new composite material for lithium secondary batteries of the present invention contains nanosilicon and carbon atoms, the carbon atoms are uniformly distributed in the nanosilicon at the atomic level, and the carbon atoms and silicon atoms are bonded to form amorphous Si-C bonds, and there is no SiC crystallization peak in the X-ray diffraction method (XRD). For solid-state NMR measurements of new composite materials, 29 In the Si NMR spectrum, it is shown that when the silicon peak is at -70 ppm to -130 ppm, the Si-C resonance peak is present between 20 ppm and -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is in the range of 0.1 to 5.0. Average particle size of the new composite material D 50 The diameter of the nanotube is between 1 nm and 50 μm, and the mass of carbon atoms accounts for 0.5% to 50% of the mass of the new composite material.
[0020] As an optional technical solution, the new composite material further contains oxygen elements, the oxygen elements being dispersed inside the nanosilicon material or on the surface of the material, and the mass of the oxygen elements accounts for 0.1% to 20% of the mass of the new composite material.
[0021] The novel composite materials of the present invention may exist as monomeric structures, which may comprise nanoparticles or nanowires, or may be deposited in or on a substrate.
[0022] The new composite material for lithium secondary batteries of the present invention can be prepared by the steps in the method shown in FIG. 1, which includes the following steps:
[0023] In step 110, a silicon source, a carbon source, and a carrier gas are simultaneously blown into the reaction vessel in a proportional manner, and the temperature of the reaction vessel is controlled to 450° C. to 1000° C., and the reaction pressure is controlled to 0.1 atm to 10 atm. Specifically, the silicon source is a silicon-containing vapor, specifically comprising one or more of the following combinations: monosilane, silicoethane, tetrafluorosilane, hexamethyldisilane, dimethylsiloxane; the carbon source comprises one or a combination of more of acetylene, methane, propylene, ethylene, propane, or ethanol; The carrier gas includes one or a combination of hydrogen, nitrogen, and argon.
[0024] In step 120, after the reaction is completed, the temperature is lowered to obtain the novel composite material for lithium secondary batteries, or the product produced by the reaction during the reaction is introduced into a cooling chamber to obtain the novel composite material for lithium secondary batteries.
[0025] Specifically, the reaction outcome can be controlled by removing the gas source.
[0026] The new composite material for lithium secondary batteries according to the present invention is obtained by thoroughly mixing a silicon source and a carbon source and then co-depositing them, thereby embedding carbon atoms uniformly in the nanosilicon material at the atomic level. The new composite material can be used to manufacture anode sheets for lithium secondary batteries such as lithium ion batteries and solid-state lithium batteries. Compared with conventional nanosilicon materials or silicon-carbon composite materials, the material has a more stable structure and smaller volume expansion during the lithium insertion / extraction process, and has better cycle characteristics when used in the anode of a lithium battery.
[0027] In order to better understand the technical solution of the present invention, several specific examples are given below to describe the specific process of preparing the new composite material for lithium secondary batteries according to the above embodiments of the present invention, as well as the method of applying the new composite material to the secondary batteries and the characteristics of the batteries.
[0028] Example 1 A mixed gas of silane, methane, and argon was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm at 1 L / min. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurements using a carbon and sulfur analyzer showed that the carbon content of the new composite material was 8%. The new composite material was measured by X-ray diffraction (XRD) to obtain an XRD spectrum. The results, as shown in Figure 2, showed that there was no SiC crystallization peak in the curve, indicating that the Si-C had an amorphous structure. For new composite materials 29 By performing solid-state nuclear magnetic resonance measurements of the Si spectrum, 29 A Si NMR spectrum was obtained, and it was found that a Si resonance peak appeared near -100 ppm and a Si-C vibration peak appeared near 0 ppm, as shown in the curve in Figure 3. The area ratio of the Si-C vibration peak to the Si resonance peak is 1.8.
[0029] Example 2 A mixed gas of silane at 1 L / min, methane at 0.2 L / min, and argon at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 2%.
[0030] Example 3 A mixed gas of silane at 1 L / min, methane at 0.2 L / min, and argon at 1 L / min is blown into a deposition chamber of a fluidized bed apparatus having a temperature of 700° C. and a pressure of 1 atm. A porous carbon material is in a fluidized state in the fluidized bed. A new type of composite material is obtained deposited on and within the porous carbon material in the collection chamber of the fluidized bed apparatus. For new composite materials 29 By performing solid-state nuclear magnetic resonance measurements of the Si spectrum, 29 A Si NMR spectrum was obtained, and as shown in the curves in Figure 4, a Si resonance peak appeared at around -80 ppm, and a Si-C vibration peak appeared at around -10 ppm, indicating that carbon is dispersed in the silicon material at the atomic level. The area ratio of the Si-C vibration peak to the Si resonance peak was 0.5, indicating that the content of carbon atoms inside the silicon-based material decreased as the relative concentration of methane decreased.
[0031] Example 4 A mixture of silane, methane, and argon gases was blown into a rotary furnace at 700℃ and 1 atm. After stopping the gas injection, the reaction is completed and the temperature is lowered to obtain the novel composite material of the present invention. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 7%.
[0032] Example 5 A mixture of silane, methane, and argon gases was blown into a rotary furnace at 900℃ and 1 atm. After stopping the gas injection, the reaction is completed and the temperature is lowered to obtain the novel composite material of the present invention. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 9%.
[0033] Example 6 A mixed gas of silane at 1 L / min, methane at 1 L / min, and argon at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 2 atm. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 10%.
[0034] Example 7 A mixed gas of silane, acetylene, and argon was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm at 1 L / min. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 15%.
[0035] Example 8 A mixed gas of silane at 1 L / min, acetylene at 3 L / min, and argon at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 35%.
[0036] Example 9 A mixed gas of silicon tetrafluoride at 1 L / min, methane at 1 L / min, and argon at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 5%.
[0037] Example 10 A mixed gas of dimethylsiloxane at 1 L / min, methane at 1 L / min, and argon at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 4% and the oxygen content was 10%.
[0038] Example 11 A mixed gas of dimethylsiloxane at 1 L / min, methane at 1 L / min, and hydrogen at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm. The novel composite material of the present invention is obtained in a collection chamber in the fluidized bed apparatus. Measurement using a carbon / sulfur analyzer revealed that the carbon content of the new composite material was 8%.
[0039] In order to better explain the properties of the new composite material obtained in the present invention, a comparison is made based on Comparative Example 1 and Comparative Example 2.
[0040] Comparative Example 1 A mixed gas of silane and argon at 1 L / min was blown into the deposition chamber of a fluidized bed apparatus at a temperature of 700°C and a pressure of 1 atm. The silicon-based material is obtained in a collection chamber in the fluidized bed apparatus. Measurements using a carbon / sulfur analyzer showed that the new composite material contained no carbon.
[0041] Comparative Example 2 The silicon-based material obtained in Comparative Example 1 was subjected to a vapor-phase carbon coating treatment, and the carbon coating amount was 8%.
[0042] The new composite materials of each of the above examples and the materials obtained in the comparative examples were each fabricated into a lithium metal button battery, and the capacity and initial coulombic efficiency were tested, with the results shown in Table 1. The new composite materials of each of the above examples and the materials obtained in the comparative examples were each composited with commercially available graphite to form a 450mAh / g composite material, which was then assembled into a button battery with lithium cobalt oxide and cycled under 1C / 1C to evaluate the cycle characteristics. The data are recorded and compared in Table 1.
[0043] [Table 1]
[0044] As can be seen from the comparison, the materials of the examples of the present invention can improve the cycle characteristics of the battery due to the uniform distribution of carbon atoms, and as the flow rate of the carbon source gas increases, the carbon content increases, and the capacity of the single unit and the initial coulombic efficiency are slightly reduced, but the cycle characteristics are obviously improved compared with those of Comparative Examples 1 and 2, and the silicon-based material of Example 3 can have better cycle characteristics by being deposited in the porous carbon, and when the materials of Examples 10 and 11 contain oxygen elements, the initial coulombic efficiency is low, but the cycle characteristics are still relatively good. In the two comparative examples, the use of carbon coating clearly improves the cycle characteristics of the battery, but there is still a large difference compared with the materials in the examples of the present invention that have a structure in which carbon is uniformly distributed.
[0045] The above specific embodiments further describe the objectives, technical solutions and beneficial effects of the present invention. The above are only specific embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0046] (Additional Note) (Appendix 1) A new composite material for lithium secondary batteries, comprising: The new composite material contains nano-silicon and carbon atoms, the carbon atoms are uniformly distributed in the nano-silicon at the atomic level, and the carbon atoms and silicon atoms are bonded to form amorphous Si-C bonds, and there is no crystallization peak of SiC in X-ray diffraction (XRD). The solid-state nuclear magnetic resonance (NMR) measurement of the new composite material includes: 29 In the Si NMR spectrum, it is shown that when the silicon peak is at -70 ppm to -130 ppm, the Si-C resonance peak is present between 20 ppm and -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is (0.1, 5.0). The average particle size D of the new composite material 50 is 1 nm to 50 μm, and the mass of the carbon atoms accounts for 0.5% to 50% of the mass of the new composite material; A new composite material for lithium secondary batteries.
[0047] (Appendix 2) The new composite material for lithium secondary batteries described in Appendix 1, characterized in that the new composite material further contains an oxygen element, the oxygen element is dispersed inside the nanosilicon material or on the surface of the material, and the mass of the oxygen element accounts for 0.1% to 20% of the mass of the new composite material.
[0048] (Appendix 3) The new composite material for lithium secondary batteries described in Appendix 1, characterized in that the new composite material exists as a monomer structure or the new composite material is deposited inside or on the surface of a substrate, and the monomer structure includes nanoparticles or nanowires.
[0049] (Appendix 4) A method for preparing the new composite material for lithium secondary batteries according to the above-mentioned Appendix 1, A silicon source, a carbon source, and a carrier gas are simultaneously blown into a reaction vessel in a proportional manner, and the temperature of the reaction vessel is controlled to 450°C to 1000°C and the reaction pressure is controlled to 0.1 atm to 10 atm; After the reaction is completed, the temperature is lowered to obtain the new composite material for lithium secondary batteries, or the product produced by the reaction during the reaction is introduced into a cooling chamber to obtain the new composite material for lithium secondary batteries; Including, A preparation method comprising the steps of:
[0050] (Appendix 5) The silicon source is a silicon-containing vapor, specifically comprising one or more of monosilane, silicoethane, tetrafluorosilane, hexamethyldisilane, and dimethylsiloxane; the carbon source comprises one or a combination of more of acetylene, methane, propylene, ethylene, propane, or ethanol; The carrier gas includes one or a combination of hydrogen, nitrogen, and argon; The preparation method according to claim 1,
[0051] (Appendix 6) A negative electrode sheet comprising the new composite material for lithium secondary batteries described in Appendix 1 above.
[0052] (Appendix 7) A lithium battery comprising the new composite material for lithium secondary batteries described in Appendix 1 above.
Claims
1. A new composite material for lithium secondary batteries, comprising: The novel composite material contains nano-silicon and carbon atoms, the carbon atoms are uniformly distributed in the nano-silicon at the atomic level, and the carbon atoms and silicon atoms are bonded to form amorphous Si-C bonds, and there is no crystallization peak of SiC in X-ray diffraction (XRD). The solid-state nuclear magnetic resonance (NMR) measurement of the new composite material includes: 29 In the Si NMR spectrum, it is shown that when the silicon peak is between −70 ppm and −130 ppm, the Si—C resonance peak is present between 20 ppm and −20 ppm, and the area ratio of the Si—C resonance peak to the silicon peak is (0.1, 5.0); The average particle size D of the new composite material 50 is 1 nm to 50 μm, and the mass of the carbon atoms accounts for 0.5% to 50% of the mass of the novel composite material; A new composite material for lithium secondary batteries.
2. The new composite material for lithium secondary batteries according to claim 1, characterized in that the new composite material further contains oxygen element, the oxygen element is dispersed inside the nanosilicon material or on the surface of the material, and the mass of the oxygen element accounts for 0.1% to 20% of the mass of the new composite material.
3. The new composite material for lithium secondary batteries according to claim 1, characterized in that the new composite material exists as a monomer structure or the new composite material is deposited within or on the surface of a substrate, and the monomer structure comprises nanoparticles or nanowires.
4. A method for preparing the new composite material for a lithium secondary battery according to claim 1, A silicon source, a carbon source, and a carrier gas are simultaneously blown into a reaction vessel in a proportional manner, and the temperature of the reaction vessel is controlled to 450° C. to 1000° C., and the reaction pressure is controlled to 0.1 atm to 10 atm; After the reaction is completed, the temperature is lowered to obtain the new composite material for lithium secondary batteries, or the product produced by the reaction during the reaction is introduced into a cooling chamber to obtain the new composite material for lithium secondary batteries; Including, A preparation method comprising the steps of:
5. The silicon source is a silicon-containing vapor, specifically comprising one or more of monosilane, silicoethane, tetrafluorosilane, hexamethyldisilane, and dimethylsiloxane; the carbon source comprises one or a combination of more of acetylene, methane, propylene, ethylene, propane, or ethanol; The carrier gas includes one or a combination of hydrogen, nitrogen, and argon; 2. The method according to claim 1 .
6. 13. A negative electrode sheet comprising the new composite material for lithium secondary batteries according to claim 1.
7. A lithium battery comprising the new composite material for lithium secondary batteries according to claim 1.
Citation Information
Patent Citations
Uniformly modified silicon monoxide negative electrode material and preparation method and application thereof
CN113258051A
Uniformly modified silicon-based lithium ion battery negative electrode material as well as preparation method and application thereof
CN113258052A
Silicon-carbon composite powder
JP2019021630A
Method for producing silicon-carbon composites
JP2019507096A
Amorphous silicon-carbon composite, its manufacturing method and lithium secondary battery including the same
JP2021506085A