Copolyamides and polymer films containing at least one lactam, a dicarboxylic acid, and 1,5-diamino-3-oxapentane
The copolyamide films, produced by polymerizing lactam with 1,5-diamino-3-oxapentane and C4-C12 dicarboxylic acid, address the stiffness and production challenges of existing polyamide films by offering high water vapor permeability, low oxygen permeability, and improved tear resistance, suitable for packaging.
Patent Information
- Application Number
- JP2024516947
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-17
- Filing Date
- 2022-09-06
- Publication Date
- 2024-10-08
AI Technical Summary
Existing polyamide films used for packaging are stiff, have low tear propagation resistance, and are not easily extrudable, with prior copolyamides exhibiting high stiffness, low transparency, and insufficient mechanical properties, making them costly and difficult to produce.
A copolyamide (CoPA) is produced by polymerizing a lactam with a monomer mixture containing 1,5-diamino-3-oxapentane, along with C4-C12 dicarboxylic acid, which results in films with improved water vapor permeability, mechanical properties, and reduced oxygen permeability, allowing for easier and less expensive production.
The copolyamide films exhibit high water vapor permeability (at least 2500 g*μm/(m²*d), low oxygen permeability (less than 1200 cm³*μm/(m²*d*bar), and enhanced tear propagation resistance, making them suitable for permeable packaging applications.
Smart Images

Figure 2024536779000001 
Figure 2024536779000002 
Figure 2024536779000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolyamide (CoPA) prepared by polymerizing a lactam (A) with a monomer mixture (M), the monomer mixture (M) comprising 1,5-diamino-3-oxapentane. The present invention further relates to a polymer film comprising at least one copolyamide (CoPA), a process for producing the polymer film, and the use of the polymer film (P) as a packaging film. [Background technology]
[0002] Polyamides are particularly important in industry because they are characterized by very good mechanical properties, among others high strength and toughness, good chemical stability and high abrasion resistance. They are used, for example, in the manufacture of fishing lines, climbing ropes and carpet backings. Polyamides are also used in the manufacture of packaging films and packaging sleeves.
[0003] A review of their use as packaging films and packaging sleeves, as well as their methods of manufacture, is given, for example, in Encyclopedia of Polymer Science and Engineering, 2nd Edition, Vol. 7, pp. 73-127; Vol. 10, pp. 684-695 (John Wiley & Sons, Inc., 1987). However, the polyamide films described therein have a very high stiffness and low tear propagation resistance.
[0004] For packaging films and sleeves it is therefore common to use copolyamides which combine the properties of different polyamides. The prior art describes a variety of copolyamides.
[0005] EP 0 352 562 describes films made from copolyamides, which are made from ε-caprolactam, preferably from 1 to 10 parts by weight of dimer acid and diamines. These can then be used to make flat or blown films. They are likewise suitable for making composite films. DE 28 46 596 describes mouldings made from copolyamides of caprolactam, fatty acid dimers and hexamethylenediamine. However, the thermoplastics described cannot be extruded into films.
[0006] In US Patent 4 387 184 multiphase polyamide compositions are described. These multiphase polyamide compositions comprise a polyamide matrix and a phase dispersed therein which also comprises a polyamide. These multiphase polyamide compositions can be processed into films. The disadvantages of the films described in US Patent 4 387 184 are that they have low or no transparency and also poor mechanical properties, in particular a high modulus and therefore high stiffness.
[0007] US Patent No. 5,888,597 discloses a thermoplastic film based on a polymer containing polyamide and polyether blocks, but the film has poor mechanical stability and is therefore applied, for example, to a polyethylene or PVC skeleton.
[0008] EP 0 761 715, for example, describes a film of a copolyetheramide for the production of waterproof rainwear; in order to achieve the properties of the film of the invention, a polyoxyalkylenediamine component having a molecular weight of at least 600 and not more than 6000 is essential. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] European Patent No. 0 352 562 [Patent Document 2] German Patent No. 28 46 596 [Patent Document 3] U.S. Pat. No. 4,387,184 [Patent Document 4] U.S. Patent No. 5,888,597 [Patent Document 5] European Patent No. 0761715 [Non-patent literature]
[0010] [Non-Patent Document 1] Encyclopedia of Polymer Science and Engineering, 2nd ed., Vol. 7, pp. 73-127; Vol. 10, pp. 684-695 (John Wiley & Sons, Inc., 1987) Summary of the Invention [Problem to be solved by the invention]
[0011] It was therefore an object of the present invention to provide a polyamide which is particularly suitable for the production of polymer films in which the disadvantages of the polymer films described in the prior art are absent or reduced in extent, and which should also be as simple and inexpensive to produce as possible.
[0012] It was likewise an object of the present invention to provide a polymer film (P) comprising polyamide, in which the disadvantages of the polymer films described in the prior art are absent or reduced in extent, and the polymer film (P) should be as simple and inexpensive to produce as possible. [Means for solving the problem]
[0013] The purpose is to have the following ingredients: (A) 60 to 95% by weight of at least one lactam; and (B) 5 to 40% by weight of a monomer mixture (M) containing the following components: (B1) At least one C4-C 12 dicarboxylic acids, and (B2) at least one diamine wherein component (B2) comprises 1,5-diamino-3-oxapentane, and said weight percentages of components (A) and (B) are based on the sum of said weight percentages of components (A) and (B), respectively. This was achieved by using copolyamide (CoPA), which is produced by polymerizing
[0014] Furthermore, this objective is achieved by the following ingredients: (A) 60 to 95% by weight of at least one lactam; and (B) 5 to 40% by weight of a monomer mixture (M) containing the following components: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). This is achieved by a polymer film (P) comprising at least one copolyamide (CoPA) produced by polymerizing Effect of the Invention
[0015] Surprisingly, it has been found that the polymer film (P) according to the invention has high water vapor permeability and mechanical properties suitable for the production of permeable packaging. In particular, the polymer film (P) according to the invention has a water vapor permeability (WVP) of at least 2500 g*μm / (m2), measured according to ASTM F 1249 at 23° C. and 85% RH. 2 *d), preferably at least 3000 g*μm / (m 2 *d), more preferably at least 3500 g*μm / (m 2 *d).
[0016] The polymer film (P) of the present invention also has a high tear propagation resistance. Moreover, the polymer film (P) of the present invention has a low oxygen permeability compared to the prior art.
[0017] Oxygen permeability measured according to ASTM F 1927 is 1500 cm 3 *μm / (m 2 *d*bar), preferably less than 1250 cm 3 *μm / (m 2 *d*bar), more preferably less than 1200 cm 3 *μm / (m 2 *d*bar). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will now be described in further detail.
[0019] Polymer Film (P) According to the invention, the polymer film (P) comprises at least one copolyamide (CoPA).
[0020] According to the invention, the polymer film (P) comprises the following components: (A) 60 to 95% by weight of at least one lactam; and (B) 5 to 40% by weight of a monomer mixture (M) containing the following components: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). The present invention includes at least one copolyamide (CoPA) prepared by polymerizing
[0021] "At least one copolyamide (CoPA)" is understood in the context of the present invention to mean either exactly one copolyamide (CoPA) or a mixture of two or more copolyamides (CoPA).
[0022] The at least one copolyamide (CoPA) is further described below.
[0023] The polymer film (P) has, for example, a thickness in the range from 0.1 μm to 1 mm, preferably a thickness in the range from 5 μm to 1 mm, particularly preferably a thickness in the range from 5 μm to 500 μm, very particularly preferably a thickness in the range from 5 μm to 100 μm, particularly preferably a thickness in the range from 7.5 μm to 100 μm.
[0024] The invention therefore also provides a polymer film (P) having a thickness in the range of 0.1 μm to 1 mm, preferably in the range of 5 μm to 1 mm, particularly preferably in the range of 5 μm to 500 μm, very particularly preferably in the range of 5 μm to 100 μm and particularly preferably in the range of 7.5 μm to 100 μm.
[0025] The polymer film (P) may comprise, in addition to the at least one copolyamide (CoPA), at least one further polymer (FP).
[0026] In the context of the present invention, "at least one further polymer (FP)" means either exactly one further polymer (FP) or a mixture of two or more further polymers (FP).
[0027] Suitable polymers as the at least one further polymer (FP) are all polymers known to the person skilled in the art. It will be clear that this at least one further polymer (FP) is different from the at least one copolyamide (CoPA).
[0028] Preferably, the at least one further polymer (FP) is selected from the group consisting of polyolefins, ethylene-vinyl alcohol, ethylene-vinyl acetate, polyethylene terephthalate, polyvinylidene chloride, maleic anhydride grafted polyolefins, polyesters, polyamides, and ionomers. More preferably, the at least one further polymer (FP) is selected from the group consisting of polyolefins, poly(ethylene-vinyl alcohol), poly(ethylene-vinyl acetate), polyethylene terephthalate, polyvinylidene chloride, polyamide 6, polyamide 6 / 66, and maleic anhydride grafted polyolefins. Most preferably, the at least one further polymer (FP) is selected from the group consisting of polyolefins, maleic anhydride grafted polyolefins, polyamide 6, polyamide 6 / 66, and ethylene-vinyl alcohol.
[0029] If the at least one further polymer (FP) is selected from the group consisting of polyolefins, it is further preferred that a maleic anhydride grafted polyolefin is used as the at least one further polymer (FP). Here, the at least one further polymer (FP) used can be a mixture of polyolefin and maleic anhydride grafted polyolefin. If the polymer film (P) is a multilayer film as described further below, it is also possible that the polymer film (P) comprises at least one first further layer of at least one further polymer (FP), where the at least one further polymer (FP) of the first further layer is selected from the group consisting of maleic anhydride grafted polyolefins, and the polymer film (P) comprises at least one second further layer of at least one further polymer (FP), where the at least one further polymer (FP) of the second further layer is selected from the group consisting of polyolefins. In the polymer film (P), the first further layer is then preferably present between the first layer and the second further layer comprising at least one copolyamide (CoPA).
[0030] Polyolefins are known per se to those skilled in the art. Preferred polyolefins are polypropylene (PP), low density polyethylene (LDPE), linear low density polyethylene (LLDPE) and very low density polyethylene (VLDPE).
[0031] Linear low density polyethylene (LLDPE) is a copolymer of ethylene and at least one C4-C8 α-olefin. Linear low density polyethylene (LLDPE) is distinguished by a long polymer chain with short side chains. The length of the side chains of linear low density polyethylene (LLDPE) is usually shorter than that of low density polyethylene (LDPE) and medium density polyethylene (MDPE). The melting point of linear low density polyethylene (LLDPE) is preferably in the range of 110-130°C and the density is 0.91-0.93 g / cm. 3 The range is.
[0032] Very low density polyethylene (VLDPE) are copolymers of ethylene and at least one C4-C8 α-olefin. They typically have melting points in the range of 110-130 °C and viscosity coefficients of 0.86-0.91 g / cm 3 The proportion of C4 to C8 α-olefins in VLDPE is generally higher than in LLDPE.
[0033] "C4-C8 α-olefins" is understood in the context of the present invention to mean linear and branched, preferably linear, alkylenes having 4 to 8 unsaturated carbon atoms in the α-position, i.e. having a C-C double bond in the α-position. Examples thereof are 1-butene, 1-pentene, 1-hexene, 1-heptene and 1-octene. 1-butene, 1-hexene and 1-octene are preferred.
[0034] Preferred poly(ethylene-vinyl acetate)s are copolymers of ethylene and vinyl acetate, for example, made using 82% to 99.9% by weight of ethylene and 0.1% to 18% by weight of vinyl acetate, preferably 88% to 99.9% by weight of ethylene and 0.01% to 12% by weight of vinyl acetate.
[0035] A preferred poly(ethylene-vinyl alcohol) can be obtained by complete or partial hydrolysis of the above-mentioned poly(ethylene-vinyl acetate). The poly(ethylene-vinyl alcohol) contains, for example, 50 to 75 mol % of ethylene and 25 to 50 mol % of vinyl alcohol, based on the total molar amount of the poly(ethylene-vinyl alcohol).
[0036] In the polymer film (P), the at least one further polymer (FP) may be present as a blend (mixture) with at least one copolyamide (CoPA). Blends of at least one copolyamide (CoPA) with polyamide 6 and / or polyamide 6 / 66 are particularly preferred.
[0037] Furthermore, according to the invention, it is possible and preferred that the polymer film (P) comprises at least one first layer comprising at least one copolyamide (CoPA) and that the polymer film (P) comprises at least one further layer comprising at least one further polymer (FP).
[0038] In this embodiment, the at least one first layer comprising at least one copolyamide (CoPA) is preferably free of further polymers (FP).
[0039] In the context of the present invention, "at least one first layer" means either exactly one first layer, or two or more first layers.
[0040] In the context of the present invention, "at least one further layer" means either exactly one further layer or two or more further layers, with two or more further layers being preferred.
[0041] Thus, the polymer film (P) comprises at least one first layer comprising at least one copolyamide (CoPA), and preferably the polymer film (P) further comprises at least one further layer, which comprises at least one further polymer (FP) selected from the group consisting of polyolefins, poly(ethylene-vinyl alcohol), poly(ethylene-vinyl acetate), polyethylene terephthalate, polyvinylidene chloride, polyamide 6, polyamide 6 / 66, and maleic anhydride grafted polyolefins.
[0042] The present invention therefore also provides a polymer film (P), wherein the polymer film (P) comprises at least one first layer comprising at least one copolyamide (CoPA), and wherein the polymer film (P) comprises at least one further layer, said at least one further layer comprising at least one further polymer (FP) selected from the group consisting of polyolefins, poly(ethylene-vinyl alcohol), poly(ethylene-vinyl acetate), polyethylene terephthalate, polyvinylidene chloride, polyamide 6, polyamide 6 / 66, and maleic anhydride grafted polyolefins.
[0043] If the polymer film (P) does not include any additional layers other than at least one first layer, this polymer film (P) is also called a "mono-film". If the polymer film (P) is a mono-film, it may include exactly one first layer and no additional layers. Similarly, it may include two or more first layers and no additional layers. If the polymer film (P) includes two or more first layers and is a mono-film, the two or more first layers all have the same composition.
[0044] When the polymer film (P) comprises at least one first layer comprising at least one copolyamide (CoPA) and at least one further layer comprising at least one further polymer (FP), the polymer film (P) is also called a multilayer film.
[0045] For example, the polymer film (P) in that case comprises 1 to 11 first layers comprising at least one copolyamide (CoPA) and 1 to 13 further layers comprising at least one further polymer (FP). Preferably, the polymer film (P) comprises 1 to 5 first layers comprising at least one copolyamide (CoPA) and 1 to 11 further layers comprising at least one further polymer (FP). Particularly preferably, the polymer film (P) comprises 1 to 3 first layers comprising at least one copolyamide (CoPA) and 1 to 7 further layers comprising at least one further polymer (FP).
[0046] In a preferred embodiment of the invention, the at least one first layer consists of at least one copolyamide (CoPA). Similarly, it is preferred that the at least one further layer consists of at least one further polymer (FP).
[0047] Thus, in the context of the present invention, the term "polymer film (P)" encompasses both mono-films and multi-layer films.
[0048] The invention therefore also provides a polymer film (P), which is a monofilm or a multilayer film.
[0049] As mentioned above, the polymer film (P) typically has a thickness in the range of 0.1 μm to 1 mm, preferably in the range of 5 μm to 1 mm, particularly preferably in the range of 5 μm to 500 μm, very particularly preferably in the range of 5 μm to 100 μm and especially preferably in the range of 7.5 μm to 100 μm.
[0050] If the polymer film (P) is a monofilm and comprises exactly one first layer, the first layer has the same thickness as the polymer film (P), i.e. for example in the range of 0.1 μm to 1 mm, preferably in the range of 5 μm to 1 mm, particularly preferably in the range of 5 μm to 500 μm, very particularly preferably in the range of 5 μm to 100 μm, particularly preferably in the range of 7.5 μm to 100 μm. If the polymer film (P) is a monofilm and comprises more than one first layer, the thickness of all first layers is smaller than the thickness of the polymer film (P). The sum of the thicknesses of the individual first layers in that case generally corresponds to the thickness of the polymer film (P). For example, in that case, at least one first layer comprising at least one copolyamide (CoPA) has a thickness in the range of 0.1 μm to 100 μm, preferably in the range of 0.5 μm to 100 μm, particularly preferably in the range of 1 μm to 50 μm, particularly preferably in the range of 1.5 μm to 15 μm.
[0051] If the polymer film (P) is a multilayer film, the thicknesses of the individual layers of the polymer film (P), i.e. the thickness of the at least one first layer comprising at least one copolyamide (CoPA) and the thickness of the at least one further layer comprising at least one further polymer (FP), are typically smaller than the thickness of the polymer film (P). The sum of the thicknesses of the individual layers then generally corresponds to the thickness of the polymer film (P).
[0052] For example, in that case, the at least one first layer comprising at least one copolyamide (CoPA) has a thickness in the range of 0.1 μm to 100 μm, preferably in the range of 0.5 μm to 100 μm, particularly preferably in the range of 1 μm to 50 μm, particularly preferably in the range of 1.5 μm to 15 μm.
[0053] In that case, the at least one further layer comprising at least one further polymer (FP) has a thickness for example in the range from 0.1 μm to 100 μm, preferably in the range from 0.5 to 100 μm, particularly preferably in the range from 1 to 50 μm and particularly preferably in the range from 1.5 to 15 μm.
[0054] The polymer film (P) may comprise at least one adhesion promoter. This embodiment is preferred when the polymer film (P) is a multilayer film.
[0055] In the context of the present invention, "at least one adhesion promoter" means either exactly one adhesion promoter or a mixture of two or more adhesion promoters.
[0056] If the polymer film (P) is a multilayer film, the at least one adhesion promoter may be present in at least one first layer together with the at least one copolyamide (CoPA). It is also possible for the at least one adhesion promoter to be present in at least one further layer together with the at least one further polymer (FP). Furthermore, the at least one adhesion promoter may be present as at least one additional layer in the polymer film (P). This embodiment is preferred.
[0057] If the at least one adhesion promoter is present as at least one additional layer in the polymer film (P), this at least one additional layer is preferably arranged between the at least one further layer comprising the at least one further polymer (FP) and the at least one first layer comprising the at least one copolyamide (CoPA). The at least one layer of adhesion promoter has a thickness of, for example, 0.1 μm to 100 μm, preferably in the range of 0.5 μm to 50 μm, particularly preferably in the range of 0.5 μm to 15 μm.
[0058] Suitable adhesion promoters are known per se to those skilled in the art. Preferred adhesion promoters are copolymers of ethylene and maleic anhydride or copolymers of ethylene and vinyl acetate. Preference is given to copolymers of linear low density polyethylene (LLDPE) grafted with maleic anhydride or copolymers of ethylene and vinyl acetate, which copolymers are produced with more than 18% by weight of vinyl acetate and less than 82% by weight of ethylene. Preferred adhesion promoters are commercially available, for example, from DuPont under the trade name Bynel 4105 or from Exxon under the trade name Escorene FL 00119.
[0059] The polymer film (P) may also contain additives, which are known to those skilled in the art and are, for example, selected from the group consisting of stabilizers, dyes, antistatic agents, tackifiers, antiblocking agents, processing aids, antioxidants, light stabilizers, UV absorbers, lubricants, and nucleation aids.
[0060] Suitable dyes are organic and inorganic pigments, for example sized titanium dioxide. Suitable tackifiers are, for example, polyisobutylene (PIB) or ethylene-vinyl acetate (EVA). Suitable antiblocking agents are, for example, silicon dioxide or calcium carbonate particles. Suitable light stabilizers are, for example, those called HALS (hindered amine light stabilizers). The processing aids or lubricants used may be, for example, ethylene bisstearamide (EBS) wax. Nucleation aids may be, for example, any kind of organic or inorganic crystallization nucleating agent, for example, talc.
[0061] The additive may be present either in at least one first layer or in at least one further layer. The additive may be present in only one of these layers. It is equally possible for the additive to be present in each of these layers.
[0062] When formed as a monofilm, the polymer film (P) of the present invention has reduced oxygen permeability and increased water vapor permeability compared to prior art PA 6 polymer films.
[0063] Copolyamide (CoPA) According to the invention, the copolyamide (CoPA) is a copolymer comprising the following components: (A) 60 to 95% by weight of at least one lactam; and (B) 5 to 40% by weight of a monomer mixture (M) containing the following components: (B1) At least one C4-C 12 dicarboxylic acids, and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). It is produced by polymerizing
[0064] According to the invention, the polymer film (P) comprises at least one copolyamide (CoPA).
[0065] In the context of the present invention, the terms "component A" and "at least one lactam" are used synonymously and therefore have the same meaning.
[0066] The same applies to the terms "component (B)" and "monomer mixture (M)". These terms are similarly used synonymously in the context of the present invention and therefore have the same meaning.
[0067] "At least one lactam" means in the context of the present invention either exactly one lactam or a mixture of two or more lactams. Exactly one lactam is preferred.
[0068] According to the invention, at least one copolyamide (CoPA) is produced by polymerizing 60% to 95% by weight of component (A) and 5% to 40% by weight of component (B), preferably at least one copolyamide (CoPA) is produced by polymerizing 65% to 90% by weight of component (A) and 10% to 35% by weight of component (B), very particularly preferably at least one copolyamide (CoPA) is produced by polymerizing 70% to 85% by weight of component (A) and 15% to 30% by weight of component (B), very particularly preferably at least one copolyamide (CoPA) is produced by polymerizing 60% to 85% by weight of component (A) and 15% to 40% by weight of component (B), where the weight percentages of components (A) and (B) are in each case based on the sum of the weight percentages of components (A) and (B).
[0069] Preferably, the sum of the weight percentages of components (A) and (B) is 100 weight percent.
[0070] It will be apparent that the weight percentages of components (A) and (B) are based on the weight percentages of components (A) and (B) prior to polymerization, i.e., when components (A) and (B) have not yet reacted with one another. During polymerization, the weight ratio of components (A) and (B) may change.
[0071] According to the invention, the copolyamide is prepared by polymerizing components (A) and (B). The polymerization of components (A) and (B) is known to those skilled in the art. Typically, the polymerization of components (A) and (B) is a condensation reaction. During the condensation reaction, component (A) reacts with components (B1) and (B2) present in component (B). This results in the formation of amide bonds between the individual components. Typically, component (A) is at least partially in open-chain form during the polymerization, i.e., as an amino acid.
[0072] The polymerization of components (A) and (B) can take place in the presence of a catalyst. Suitable catalysts are all catalysts known to those skilled in the art that catalyze the polymerization of components (A) and (B). Preferred catalysts are phosphorus compounds, such as sodium hypophosphite, phosphorous acid, triphenylphosphine, or triphenylphosphite.
[0073] The polymerization of components (A) and (B) forms a copolyamide, thus resulting in structural units derived from component (A) and structural units derived from component (B). The structural units derived from component (B) include structural units derived from components (B1) and (B2).
[0074] The polymerization of components (A) and (B) results in the formation of a copolymer, the copolyamide (CoPA), which may be a random copolymer but may also be a block copolymer. The copolyamide (CoPA) is preferably a random copolymer.
[0075] The invention therefore also provides a polymer film (P) in which at least one copolyamide (CoPA) is a random copolymer.
[0076] In the block copolymer, blocks of units derived from component (B) and blocks of units derived from component (A) are formed, which exist alternately.
[0077] In a random copolymer, the structural units derived from component (A) and the structural units derived from component (B) are present alternately. This alternating structure is present randomly. For example, two structural units derived from component (B) may be followed by a structural unit derived from component (A), which is then followed by a structural unit derived from component (B), which is then followed by a structural unit containing three structural units derived from component (A).
[0078] The preparation of at least one copolyamide preferably comprises the following steps: a) polymerizing components (A) and (B) to obtain at least one first copolyamide; b) pelletizing the at least one first copolyamide obtained in step a) to obtain at least one pelleted copolyamide; c) extracting the at least one pelletized copolyamide obtained in step b) with water to obtain at least one extracted copolyamide; d) subjecting the at least one extracted copolyamide obtained in step c) to a temperature (T T ) to obtain at least one copolyamide.
[0079] The present invention therefore also provides a polymer film (P), in which the copolyamide (CoPA) is produced by a process comprising the following steps: a) polymerizing components (A) and (B) to obtain at least one first copolyamide; b) pelletizing the at least one first copolyamide obtained in step a) to obtain at least one pelleted copolyamide; c) extracting the at least one pelletized copolyamide obtained in step b) with water to obtain at least one extracted copolyamide; d) subjecting the at least one extracted copolyamide obtained in step c) to a temperature (T T ) to obtain at least one copolyamide.
[0080] The polymerization in step a) can be carried out in any reactor known to those skilled in the art. Stirred tank reactors are preferred. Furthermore, it is possible to use auxiliaries known to those skilled in the art to improve the reaction control, such as antifoaming agents (e.g. polydimethylsiloxane (PDMS)) and, as catalyst, for example, an aqueous solution of sodium hypophosphite ("NHP", e.g. 0.2% by weight).
[0081] In step b), the at least one first copolyamide obtained in step a) may be pelletized by any method known to the person skilled in the art, such as strand pelletization or underwater pelletization.
[0082] The extraction in step c) may be carried out by any method known to the person skilled in the art.
[0083] During the extraction in step c), the by-products formed in step a) during the polymerization of components (A) and (B) are typically extracted from the at least one pelletized copolyamide.
[0084] In step d), the at least one extracted copolyamide obtained in step c) is dried. Drying methods are known to those skilled in the art. According to the invention, the at least one extracted copolyamide is dried at a temperature (T T ) is dried at temperature (T T ) is preferably equal to at least one glass transition temperature (T G(C) ) and the melting temperature (T M(C) ) lower.
[0085] Drying in step d) is typically carried out for a period in the range of from 1 to 100 hours, preferably in the range of from 2 to 50 hours, particularly preferably in the range of from 3 to 40 hours.
[0086] Drying in step d) is believed to further increase the molecular weight of the at least one copolyamide.
[0087] The at least one copolyamide typically has at least one glass transition temperature (T G(C) ) at least one glass transition temperature (T G(C) ) is, for example, in the range of 30°C to 70°C, preferably in the range of 40°C to 68°C, and particularly preferably in the range of 45°C to 65°C, as measured in accordance with ISO 11357-2:2013.
[0088] The present invention therefore also provides a method for determining the glass transition temperature (T G(C) ) is in the range of 30 to 70°C.
[0089] According to ISO 11357-2:2013, the glass transition temperature (T G(C) ) in the context of the present invention is the glass transition temperature (T G(C) ) related to
[0090] "Dry" in the context of the present invention means that the at least one copolyamide (CoPA) contains less than 1% by weight, preferably less than 0.5% by weight, particularly preferably less than 0.1% by weight of moisture, based on the total weight of the at least one copolyamide (CoPA). More preferably, "dry" means that the at least one copolyamide (CoPA) is free of water, and most preferably that the at least one copolyamide (CoPA) is free of solvent.
[0091] Additionally, at least one copolyamide (CoPA) typically has a melting temperature (T M(C) The melting temperature (T M(C) ) is, for example, in the range of 100 to 210°C, preferably in the range of 150 to 210°C, and particularly preferably in the range of 180 to 210°C, as measured in accordance with ISO 11357-3:2011.
[0092] The present invention therefore also provides a method for producing at least one copolyamide (CoPA) having a melting temperature (T M(C) ) and the melting temperature (T M(C) ) is in the range of 10 to 210°C, preferably 150 to 210°C.
[0093] The at least one copolyamide generally has a viscosity number (VN) in the range of 150 to 300 ml / g, measured on a 0.5% by weight solution of the at least one copolyamide in a mixture of phenol / o-dichlorobenzene in a weight ratio of 1:1. (C)The measurements are carried out as described in EN ISO 307:2007+Amd 1:2013, the only difference being that a mixture of phenol / o-dichlorobenzene in a weight ratio of 1:1 is used instead of the described solvent, sulfuric acid.
[0094] Preferably, the viscosity number (VN) of at least one copolyamide is (C) ) is in the range of 160 to 290 ml / g, more preferably in the range of 170 to 280 ml / g, measured on a 0.5% by weight solution of the at least one copolyamide in a mixture of phenol / o-dichlorobenzene in a weight ratio of 1:1.
[0095] The present invention therefore also provides that the at least one copolyamide has a viscosity number (VN) ranging from 150 to 300 ml / g, measured on a 0.5% by weight solution of the at least one copolyamide in a mixture of phenol / o-dichlorobenzene in a ratio of 1:1. (C) A polymer film (P) having a
[0096] Preferably, at least one copolyamide (CoPA) does not contain any polyoxyalkylene groups.
[0097] Component (A) Component (A) is at least one lactam.
[0098] Lactams are known per se to the person skilled in the art. According to the invention, lactams having 4 to 12 carbon atoms are preferred.
[0099] "Lactam" is understood in the context of the present invention to mean a cyclic amide having preferably 4 to 12, more preferably 6 to 12, carbon atoms in the ring.
[0100] Suitable lactams are, for example, 3-aminopropanolactam (propio-3-lactam; β-lactam; β-propiolactam), 4-aminobutanolactam (butyro-4-lactam; γ-lactam; γ-butyrolactam), 5-aminopentanolactam (2-piperidinone; δ-lactam; δ-valerolactam), 6-aminohexanolactam (hexano-6-lactam; ε-lactam; ε-caprolactam), 7-aminoheptanolactam (heptano-7-lactam; ζ-lactam; ζ-heptanolactam), tam), 8-aminooctanolactam (octano-8-lactam; eta-lactam; eta-octanolactam), 9-aminononanolactam (nonano-9-lactam; θ-lactam; θ-nonanolactam), 10-aminodecanolactam (decano-10-lactam; ω-decanolactam), 11-aminoundecanolactam (undecano-11-lactam; ω-undecanolactam), and 12-aminododecanolactam (dodecano-12-lactam; ω-dodecanolactam).
[0101] Thus, the present invention also provides a polymer film (P) in which component (A) is selected from the group consisting of 3-aminopropanolactam, 4-aminobutanolactam, 5-aminopentanolactam, 6-aminohexanolactam, 7-aminoheptanolactam, 8-aminooctanolactam, 9-aminononanolactam, 10-aminodecanolactam, 11-aminoundecanolactam and 12-aminododecanolactam.
[0102] Particularly preferably, component (A) is selected from the group consisting of 6-aminohexanolactam and 12-aminododecanolactam.
[0103] Very particularly preferably, component (A) is 6-aminohexanolactam.
[0104] The lactam may be unsubstituted or at least monosubstituted. When an at least monosubstituted lactam is used, its nitrogen atom and / or ring carbon atom may be C1-C 10Alkyl, C5-C6 cycloalkyl, and C5-C 10 It may have one, two or more substituents independently selected from the group consisting of aryl.
[0105] Appropriate C1~C 10 Alkyl substituents are, for example, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, and tert-butyl. Suitable C5-C6 cycloalkyl substituents are, for example, cyclohexyl. 10 The aryl substituents are phenyl and anthranyl.
[0106] It is preferable to use unsubstituted lactams, and more preferably γ-lactam (γ-butyrolactam), δ-lactam (δ-valerolactam) and ε-lactam (ε-caprolactam). Particularly preferred are δ-lactam (δ-valerolactam) and ε-lactam (ε-caprolactam), and especially preferred is ε-caprolactam.
[0107] Ingredient (B) According to the present invention, component (B) is a monomer mixture (M). The monomer mixture (M) comprises component (B1), i.e. at least one C4-C 12 dicarboxylic acid, and (B2), i.e. at least one diamine, one of the diamines (B2) being 1,5-diamino-3-oxapentane.
[0108] Monomer mixture (M) is understood in the context of the present invention to mean a mixture of two or more monomers, in which at least components (B1) and (B2) are present in the monomer mixture (M).
[0109] The monomer mixture (M) comprises, for example, in the range of 45 to 55 mol % of component (B1) and in the range of 45 to 55 mol % of component (B2), in each case based on the sum of the molar percentages of components (B1) and (B2), preferably based on the total molar amount of the monomer mixture (M).
[0110] Preferably, component (B) comprises in the range of 47 to 53 mol % of component (B1) and in the range of 47 to 53 mol % of component (B2), in each case based on the sum of the molar percentages of components (B1) and (B2), preferably based on the total molar amount of component (B).
[0111] More preferably, component (B) comprises in the range of 49 to 51 mol % of component (B1) and in the range of 49 to 51 mol % of component (B2), in each case based on the sum of the molar percentages of components (B1) and (B2), preferably based on the total molar amount of component (B).
[0112] The present invention therefore also provides a polymer film (P), in which component (B) comprises in the range of 45 to 55 mol % of component (B1) and in the range of 45 to 55 mol % of component (B2), in each case based on the total molar amount of component (B).
[0113] The sum of the molar percentages of components (B1) and (B2) present in component (B) usually equals 100 mole %.
[0114] The monomer mixture (M) preferably does not contain a polyoxyalkylene group.
[0115] The monomer mixture (M) may further comprise water.
[0116] Ingredients (B1) According to the present invention, component (B1) contains at least one C4-C 12 It is a dicarboxylic acid.
[0117] "Component (B1)" and "at least one C4-C 12 The terms "dicarboxylic acid" and "dicarboxylic acid" are used synonymously in the context of the present invention and therefore have the same meaning.
[0118] "At least one C4~C 12 "Dicarboxylic acid" (B1) in the context of the present invention means exactly one C4-C 12 Dicarboxylic acids or two or more C4-C12 It refers to any mixture of dicarboxylic acids.
[0119] "C4~C 12 "Dicarboxylic acid" is understood in the context of the present invention to mean aliphatic and / or aromatic compounds having 2 to 10 carbon atoms and two carboxyl groups (-COOH groups). The aliphatic and / or aromatic compounds may be unsubstituted or further at least monosubstituted. If the aliphatic and / or aromatic compounds are further at least monosubstituted, they may have one, two or more substituents which do not participate in the polymerization of components (A) and (B). Substituents of this kind are known to the skilled person and are, for example, alkyl or cycloalkyl substituents. Preferably, at least one C4-C 12 The dicarboxylic acid is unsubstituted.
[0120] Suitable components (B1) are, for example, selected from the group consisting of butanedioic acid (succinic acid), pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), heptanedioic acid (pimelic acid), octanedioic acid (suberic acid), nonanedioic acid (azelaic acid), decanedioic acid (sebacic acid), undecanedioic acid, dodecanedioic acid, terephthalic acid, and isophthalic acid.
[0121] Preferably, component (B1) is selected from the group consisting of pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), decanedioic acid (sebacic acid), dodecanedioic acid, terephthalic acid, and isophthalic acid.
[0122] Very particularly preferably, component (B1) is hexanedioic acid (adipic acid).
[0123] Thus, the present invention also provides a polymer film (P) in which component (B1) is selected from the group consisting of pentanedioic acid, hexanedioic acid, decanedioic acid, dodecanedioic acid, terephthalic acid, and isophthalic acid.
[0124] Particularly preferably, component (B1) is hexanedioic acid (adipic acid).
[0125] Ingredients (B2) The terms "component (B2)" and "at least one lactam" are used synonymously in the context of the present invention and therefore have the same meaning.
[0126] "At least one second diamine (B2)" is understood in the context of the present invention to mean either exactly one diamine (B2) or a mixture of two or more diamines (B2). According to the present invention, exactly one diamine (B2) is preferred.
[0127] Component (B2) according to the invention comprises 1,5-diamino-3-oxapentane. For example, component (B2) comprises at least 50 mol%, preferably at least 80 mol%, particularly preferably at least 95 mol% of 1,5-diamino-3-oxapentane, in each case based on the total amount of component (B2). Most preferably, component (B2) consists of 1,5-diamino-3-oxapentane.
[0128] Furthermore, component (B2) may contain further diamines. Suitable further diamines are known per se to the person skilled in the art, examples being butane-1,4-diamine, pentamethylenediamine or hexamethylenediamine.
[0129] For example, component (B2) comprises 1,5-diamino-3-oxapentane in the range of 50 to 99.9 mol % and hexamethylenediamine in the range of 0.1 to 50 mol %, in each case based on the total molar amount of component (B2).
[0130] The sum of the molar percentages of components (B1) and (B2) present in component (B) usually equals 100 mole %.
[0131] More preferably, component (B2) consists of 1,5-diamino-3-oxapentane, in which case component (B2) does not contain any further diamines.
[0132] It is therefore particularly preferred that component (B) consists of components (B1), i.e. adipic acid, and (B2), i.e. 1,5-diamino-3-oxapentane. Production of polymer film (P)
[0133] The polymer film (P) of the present invention is preferably prepared by the following steps: i) the following ingredients: (A) 60 to 95% by weight of at least one lactam (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine, (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing ii) extruding the at least one copolyamide prepared in step i) in molten form from a first extruder through a die to obtain a film of the at least one copolyamide in molten form; iii) cooling the film of at least one copolyamide in molten form obtained in step ii), whereby the at least one copolyamide solidifies to obtain a polymer film (P). The method includes:
[0134] The present invention therefore also relates to a method for the preparation of a polymer film (P) according to the invention, comprising the following steps: i) the following ingredients: (A) 60 to 95% by weight of at least one lactam, and (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine, (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing ii) extruding the at least one copolyamide prepared in step i) in molten form from a first extruder through a die to obtain a film of the at least one copolyamide in molten form; iii) cooling the film of at least one copolyamide in molten form obtained in step ii), whereby the at least one copolyamide solidifies to obtain a polymer film (P). The present invention provides a method comprising:
[0135] In step i), at least one copolyamide in molten form is provided in a first extruder.
[0136] "First extruder" means in the context of the present invention either exactly one first extruder or two or more first extruders. Usually, as many first extruders are used as there are first layers comprising at least one copolyamide that will be present in the polymer film (P).
[0137] If the polymer film (P) comprises, for example, exactly one first layer comprising at least one copolyamide, then exactly one first extruder is used. If the polymer film (P) comprises exactly two first layers comprising at least one copolyamide, then exactly two first extruders are used. If the polymer film (P) comprises exactly five first layers comprising at least one copolyamide, then exactly five first extruders are used.
[0138] For example, 1 to 11 first extruders are used, preferably 1 to 5 first extruders, more preferably 1 to 3 further extruders are used.
[0139] The above explanations and preferred conditions for the at least one copolyamide present in the polymer film (P) apply mutatis mutandis to the at least one copolyamide provided in step i).
[0140] According to the invention, at least one copolyamide is provided in molten form.
[0141] "In molten form" in the context of the present invention means that the at least one copolyamide is melted at a temperature above the melting temperature (T M(C) ) of the at least one copolyamide. Thus, "in molten form" means that the at least one copolyamide is prepared at a temperature above the melting temperature (T M(C) ) When the at least one copolyamide is in molten form, the at least one copolyamide is free-flowing.
[0142] By "free flowing" it is meant that the at least one copolyamide can be conveyed into the first extruder and the at least one copolyamide can be extruded from the first extruder.
[0143] For example, in each case, the temperature at which the at least one copolyamide is prepared is greater than the melting temperature (T M(C) ), the at least one copolyamide is provided in step i) at a temperature in the range of 190°C to 300°C, preferably in the range of 200°C to 280°C, particularly preferably in the range of 210°C to 270°C.
[0144] The at least one copolyamide can be provided in molten form in the first extruder by any method known to those skilled in the art.
[0145] For example, the at least one copolyamide can be fed to the first extruder in molten or solid form. If the at least one copolyamide is fed to the first extruder in solid form, it can be fed to the first extruder, for example, in the form of pellets and / or powder. The at least one copolyamide is then melted in the first extruder and is thus prepared in molten form in the first extruder. This embodiment is preferred.
[0146] It is further possible to polymerize components (A) and (B) directly in the first extruder, thereby providing at least one copolyamide in molten form in the first extruder. Methods for this purpose are known to the person skilled in the art.
[0147] In step ii) the at least one copolyamide in molten form is extruded from the first extruder through a die to obtain a film of the at least one copolyamide in molten form.
[0148] In the context of the present invention, a "die" means either exactly one die, or two or more dies. Exactly one die is preferred according to the present invention.
[0149] Suitable dies are all dies known to those skilled in the art that allow the extrusion of a film from at least one copolyamide in molten form, such dies being, for example, a ring die or a slot die.
[0150] Suitable ring and slot dies are known per se to those skilled in the art.
[0151] For example, when step i1), further described below, is carried out, in step ii) it is preferred that the at least one copolyamide in molten form from the first extruder is combined in a die, for example a ring die or a slot die, with at least one further polymer (FP) in molten form from a further extruder.
[0152] Specifically, in step ii), the at least one copolyamide in molten form from a first extruder is combined in a die with at least one further polymer (FP) in molten form from a further extruder, so that the film of the at least one copolyamide and the at least one further polymer (FP), in each case in molten form, obtained in step ii) comprises at least one first layer comprising the at least one copolyamide in molten form and also comprises at least one further layer comprising the at least one further polymer (FP) in molten form.
[0153] For example, the thickness of the film of the at least one copolyamide in the molten form is in the range from 5 μm to 1 mm, preferably in the range from 5 μm to 1 mm, particularly preferably in the range from 5 μm to 500 μm, very particularly preferably in the range from 5 μm to 100 μm and especially preferably in the range from 7.5 μm to 100 μm.
[0154] The film of at least one copolyamide in molten form can be, for example, a flat film or a tubular film: when a ring die is used as the die, a tubular film is generally obtained, when a slot die is used as the die, a flat film is obtained.
[0155] In step iii), the film of at least one copolyamide in molten form obtained in step ii) is cooled, whereby the at least one copolyamide solidifies to obtain a polymer film (P).
[0156] All methods known to those skilled in the art are suitable for cooling the film of at least one copolyamide in molten form. For example, the film of at least one copolyamide in molten form can be cooled by air or water cooling or by contact with a cold surface.
[0157] The film of the at least one copolyamide in molten form is, in step iii), for example, heated to a melting temperature (T M(C)) to obtain a polymer film (P). Preferably, the film of the at least one copolyamide in molten form is cooled in step iii) to a temperature below at least one glass transition temperature (T G(C) ) is cooled to a temperature lower than that of the
[0158] For example, the film of the at least one copolyamide in molten form is cooled in step iii) to a temperature in the range from 0 to 100° C., preferably in the range from 10 to 80° C., particularly preferably in the range from 15 to 70° C., the temperature to which the film of the at least one copolyamide in molten form is cooled being preferably less than the melting temperature (T M(C) ), preferably at least one glass transition temperature (T G(C) ) or less.
[0159] The present invention therefore also provides that in step (iii) the film of the at least one copolyamide in molten form is heated to a temperature above the melting temperature (T M(C) The method further comprises the steps of: (a) cooling the polymer film (P) to a temperature lower than the temperature at which the polymer film (P) is heated;
[0160] The above explanations and preferred conditions for the polymer film (P) of the present invention apply mutatis mutandis to the polymer film (P) obtained in step iii).
[0161] Steps ii) and iii) can be performed alternately or simultaneously.
[0162] Preferably, a further step i1) is carried out, in which at least one further polymer (FP) in molten form is fed to a further extruder.
[0163] In that case, the method for producing a polymer film (P) comprises the following steps: i) the following ingredients: (A) 60 to 95% by weight of at least one lactam (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine, (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing i1) providing at least one further polymer (FP) in molten form in a further extruder; ii) extruding the at least one copolyamide provided in step i) in molten form from a first extruder through a die and extruding the at least one further polymer (FP) provided in step i1) in molten form from a further extruder through a die to obtain a film of the at least one copolyamide and the at least one further polymer (FP), in each case in molten form; iii) cooling the film of the at least one copolyamide and of the at least one further polymer (FP), in each case in molten form, so that the at least one copolyamide and / or the at least one further polymer (FP) solidifies to give a polymer film (P). Includes.
[0164] In step i1) at least one further polymer (FP) in molten form is provided in a further extruder.
[0165] By "further extruder" in the context of the present invention is meant either exactly one further extruder or two or more further extruders. Two or more further extruders are preferred.
[0166] Preferably, the same number of further extruders as the number of further layers comprising at least one further polymer (FP) to be present in the polymer film (P) are used, for example 1 to 13 further extruders are used, preferably 1 to 11 further extruders, particularly preferably 1 to 7 further extruders are used.
[0167] If the polymer film (P) comprises, for example, exactly one additional layer comprising at least one additional polymer (FP), then exactly one additional extruder is used. If the polymer film (P) comprises exactly two additional layers comprising at least one additional polymer (FP), then exactly two additional extruders are used. If the polymer film (P) comprises exactly five additional layers comprising at least one additional polymer (FP), then exactly five additional extruders are used.
[0168] The above statements and preferences for the at least one further polymer (FP) optionally present in the polymer film (P) apply mutatis mutandis to the at least one further polymer (FP).
[0169] According to the invention, the at least one further polymer (FP) is provided in step i1) in molten form. "In molten form" means that the at least one further polymer (FP) is heated to a temperature below the melting temperature (T M(FP) ) of the at least one further polymer (FP). Thus, "in molten form" means that the at least one further polymer (FP) is prepared at a temperature above the melting temperature (T M(FP) ) When the at least one further polymer (FP) is in molten form, the at least one further polymer (FP) becomes free-flowing.
[0170] By "free flowing" it is meant that at least one further polymer (FP) can be conveyed within the further extruder and at least one further polymer (FP) can be extruded from the further extruder.
[0171] For example, in each case, the temperature at which the at least one further polymer (FP) is provided is preferably greater than the melting temperature (T M(FP) ), the at least one further polymer (FP) is provided in step i1) at a temperature in the range of 120 to 350°C, preferably in the range of 130 to 300°C, particularly preferably in the range of 140 to 250°C.
[0172] At least one further polymer (FP) may be provided in molten form in the further extruder by any method known to a person skilled in the art.
[0173] For example, the at least one further polymer (FP) can be fed to the further extruder in molten form or in solid form. If the at least one further polymer (FP) is fed to the further extruder in solid form, it can be fed to the further extruder, for example, in the form of pellets and / or powder. The at least one further polymer (FP) is then melted in the further extruder and is thus prepared in molten form in the further extruder.
[0174] Step i1) is usually carried out simultaneously with step i).
[0175] The above explanations and preferred conditions for steps i), ii) and iii) when step i1) is not performed apply mutatis mutandis to steps i), ii) and iii) when step i1) is performed.
[0176] The film of at least one copolyamide and at least one further polymer (FP), in each case in molten form, obtained in step ii) comprises at least one copolyamide in at least one first layer and at least one further polymer (FP) in at least one further layer. Typically, the film obtained in step ii) comprises a number of first layers comprising at least one copolyamide in molten form equal to the number of first extruders used in step i) and a number of further layers comprising at least one further polymer (FP) in molten form equal to the number of further extruders used in step i1).
[0177] Once step i1) has been carried out, it will be apparent that the polymer film (P) obtained in step iii) is a multilayer film.
[0178] Preferably, the polymer film (P) is stretched. The polymer film (P) can be stretched after step iii). It is also possible to stretch the polymer film (P) during step iii), i.e. during cooling of the film of at least one copolyamide and optionally at least one further polymer (FP).
[0179] Therefore, the present invention also provides a method in which the following steps are further performed: (iv) stretching the polymer film (P) to obtain a stretched polymer film (SP).
[0180] Steps iii) and iv) can be performed alternately or simultaneously.
[0181] When the polymer film (P) is stretched, the polymer chains of the at least one copolyamide may align and the crystallinity of the at least one copolyamide may increase.
[0182] Furthermore, the polymer chains of the at least one further polymer (FP) present in the polymer film (P) may also become aligned during the stretching operation, which may also increase the crystallinity of the at least one further polymer (FP).
[0183] Stretching can be accomplished by any method known to those skilled in the art.
[0184] For example, the polymer film (P) can be stretched by leading it over at least one roller, preferably a roller system, or by expanding the width of the polymer film (P). If the polymer film (P) is obtained in the form of a tube, it is also possible to stretch the polymer film (P) by blowing air into the tube of the polymer film (P). A combination of methods is of course also possible.
[0185] When the polymer film (P) is guided over at least one roller, preferably a roller system, it is stretched in the extrusion direction, i.e. in the direction of its length, whereas when the polymer film (P) is stretched in its width, it is stretched perpendicular to the extrusion direction.
[0186] When the polymer film (P) is stretched by being guided over at least one roller, preferably a roller system, the polymer chains of the at least one copolyamide and optionally the at least one further polymer (FP) are aligned parallel to the stretching direction.
[0187] The resulting stretched polymer film (SP) is uniaxially oriented if the film is stretched only in its length direction. Similarly, the resulting stretched polymer film (SP) is uniaxially oriented if the polymer film (P) is elongated by stretching only in its width direction. Again, the polymer chains of the at least one copolyamide and of the optional at least one further polymer (FP) are aligned parallel to the stretching direction.
[0188] By "uniaxially oriented" it is meant that the polymer chains are aligned essentially in one direction.
[0189] When the polymer film (P) is stretched by being guided over a roller system and its width is further extended, the polymer chains of the at least one copolyamide and of the optional at least one further polymer (FP) are aligned parallel to both directions in which they are stretched, and the resulting stretched polymer film (SP) is then biaxially oriented.
[0190] By "biaxially oriented" it is meant that the polymer chains are essentially aligned in two different directions, preferably at right angles to each other.
[0191] When the polymer film (P) is obtained in the form of a tube, the polymer film (P) is stretched by blowing air into the tube of the polymer film (P), so that the resulting stretched polymer film (SP) is uniaxially oriented.
[0192] Thus, by combining the above-mentioned methods for stretching a polymer film (P), the polymer film (P) is obtained, for example, in the form of a tube, which is stretched by blowing air into the tube of the polymer film (P) and is simultaneously led over a roller system, which also stretches it, so that the resulting stretched polymer film (SP) is then biaxially oriented.
[0193] The polymer film (P) typically has a glass transition temperature (T G(C) ) and the melting temperature (T M(C) If the polymer film (P) is a multilayer film, the polymer film (P) is stretched at a temperature lower than the melting temperature (T M(FP) ), particularly preferably below the melting temperature of at least one further polymer (FP) which melts at the lowest temperature.
[0194] The polymer film (P) of the present invention can be produced, for example, by the cast method, the blow method, the biaxially oriented polyamide film method (BOPA method) or the multi-blow method.
[0195] The invention therefore also provides a polymer film (P) produced by the cast process, the blown process, the biaxially oriented polyamide film process or the multi-blow process.
[0196] The cast method, the blow method, the biaxially oriented polyamide film method and the multi-blow method are known per se to those skilled in the art. Typically, in these methods, the polymer film (P) is stretched, so that a stretched polymer film (P) is obtained.
[0197] The casting method for producing the polymer film (P) preferably comprises the following steps ic) to iv-c): ic) the following ingredients: (A) 60 to 95% by weight of at least one lactam (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are, in each case, based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing ii-c) extruding the at least one copolyamide prepared in molten form in step ic) from the first extruder through a die to obtain a film of the at least one copolyamide in molten form, iii-c) cooling the film of at least one copolyamide obtained in molten form in step ii-c), whereby the at least one copolyamide solidifies to obtain a polymer film (P), iv-c) stretching the polymer film (P) obtained in step iii-c) by directing it over at least one roller, preferably over a roller system, to obtain a stretched polymer film (SP).
[0198] The above explanations and preferred conditions for steps i) to iii) of the process for producing the polymer film (P) apply mutatis mutandis to steps ic) to iii-c) of the casting process.
[0199] The die used in step ii-c) in the casting process is typically a slot die. The film of at least one copolyamide obtained in molten form in step ii-c) is therefore preferably a flat film, so that the polymer film (P) obtained in step iii-c) is preferably a flat film, as is the stretched polymer film (SP) obtained in step iv-c).
[0200] In the casting method, steps iii-c) and iv-c) can be carried out alternately or simultaneously. In the casting method, steps iii-c) and iv-c) are preferably carried out simultaneously. It is particularly preferred that steps iii-c) and iv-c) are carried out simultaneously with and immediately after step ii-c).
[0201] It is also preferred that in the casting process at least one roller, preferably the roller system, used in step iv-c) is cooled during step iv-c).
[0202] The blowing process for producing the polymer film (P) preferably comprises the following steps ib) to iv-b): ib) the following ingredients: (A) 60 to 95% by weight of at least one lactam (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are in each case based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing ii-b) extruding the at least one copolyamide prepared in molten form in step ib) from the first extruder through a die, which is a ring die, to obtain a tubular film of the at least one copolyamide in molten form, iii-b) cooling the tubular film of at least one copolyamide in molten form obtained in step ii-b), whereby the at least one copolyamide solidifies to obtain a polymer film (P), iv-b) Stretching the polymer film (P) obtained in step iii-b) by blowing air through the tube of polymer film (P) to obtain a stretched polymer film (SP).
[0203] The above explanations and preferred conditions for steps i) to iii) of the process for producing the polymer film (P) apply mutatis mutandis to steps ib) to iii-b) of the blowing process.
[0204] The die used in step ii-b) of the blowing process is preferably a stack dye, a helical distributor dye, or a mixed form thereof, which are known to the skilled person and described, for example, in Kirk Cantor's "Blown Film Extrusion", 2nd edition, Carl Hanser Verlag, Munich 2011.
[0205] Steps iii-b) and iv-b) can be carried out simultaneously or alternately during the blowing process. In the blowing process, steps iii-b) and iv-b) are preferably carried out simultaneously.
[0206] It will be clear that, when steps iii-b) and iv-b) are carried out simultaneously in the blowing process, in step iii-b) the tubular film of at least one copolyamide in molten form obtained in step ii-b) is cooled and simultaneously stretched by blowing air through it to obtain a stretched polymer film (SP).
[0207] The biaxially oriented polyamide film method for producing the polymer film (P) preferably comprises the following steps io) to iv-o): io) the following ingredients: (A) 60 to 95% by weight of at least one lactam (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are in each case based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing ii-o) extruding the at least one copolyamide prepared in molten form in step io) from the first extruder through a die to obtain a film of the at least one copolyamide in molten form, iii-o) cooling the film of at least one copolyamide in molten form obtained in step ii-o), whereby the at least one copolyamide solidifies to obtain a polymer film (P), iv-o) Stretching the polymer film (P) obtained in step iii-o). By guiding the polymer film (P) over at least one roller, preferably a roller system, to increase its width, a stretched polymer film (SP) is obtained.
[0208] The above explanations and preferred conditions for steps i) to iii) of the process for producing the polymer film (P) apply mutatis mutandis to steps io) to iii-o) of the biaxially oriented polyamide film process.
[0209] The die used in step ii-o) in the biaxially oriented polyamide film process is typically a slot die. The film of at least one copolyamide in molten form obtained in step ii-o) is therefore preferably a flat film, so that the polymer film (P) obtained in step iii-o) is preferably a flat film, as is the stretched polymer film (SP) obtained in step iv-o).
[0210] In the biaxially oriented polyamide film process, steps iii-o) and iv-o) can be carried out alternately or simultaneously, preferably steps iii-o) and iv-o) are carried out alternately. Particularly preferably, in the biaxially oriented polyamide film process, steps iii-o) and iv-o) are carried out alternately, and the polymer film (P) obtained in step iii-o) is heated before step iv-o). Here, the polymer film (P) is heated to at least one glass transition temperature (T G(C) ) and the melting temperature (T M(C) In that case, the polymer film (P) is preferably stretched in step iv-o) at the temperature to which it is heated before step iv-o).
[0211] The multi-blow process for producing the polymer film (P) preferably comprises the following steps im) to iv-m): im) the following ingredients: (A) 60 to 95% by weight of at least one lactam, and (B) 5 to 40% by weight of a monomer mixture (M) comprising: (B1) At least one C4-C 12 Dicarboxylic acids and (B2) at least one diamine (wherein component (B2) comprises 1,5-diamino-3-oxapentane, and the weight percentages of components (A) and (B) are in each case based on the sum of the weight percentages of components (A) and (B)). Providing in a first extruder, in molten form, at least one copolyamide produced by polymerizing ii-m) extruding the at least one copolyamide prepared in molten form in step im) from the first extruder through a die, which is a ring die, to obtain a tubular film of the at least one copolyamide in molten form; iii-m) cooling the tubular film of at least one copolyamide in molten form obtained in step ii-m), whereby the at least one copolyamide solidifies to obtain a polymer film (P); iv-m) Stretching the polymer film (P) obtained in step iii-m) by blowing air into the tube of polymer film (P) and simultaneously directing the polymer film (P) over at least one roller, preferably a roller system, to obtain a stretched polymer film (SP).
[0212] The explanations and preferred conditions given above for steps i) to iii) of the process for producing the polymer film (P) apply mutatis mutandis to steps im) to iii-m) of the multi-blow process.
[0213] Preferably, the tubular film of at least one copolyamide in molten form is cooled in a water bath in step iii-m).
[0214] In the multi-blow process, steps iii-m) and iv-m) can be carried out alternately or simultaneously, preferably steps iii-m) and iv-m) are carried out alternately. Particularly preferably, steps iii-m) and iv-m) are carried out alternately, and the polymer film (P) obtained in step iii-m) is heated before step iv-m). Here, the polymer film (P) is heated before step iv-m) to at least one glass transition temperature (T G(C) ) and the melting temperature (T M(C) In that case, the polymer film (P) is preferably stretched in step iv-m) at the temperature to which it is heated before step iv-m).
[0215] It will be clear that in the cast process, the blow process, the biaxially oriented polyamide film process and the multi-blow process, step i1), in which at least one further polymer (FP) is provided in molten form in a further extruder, can also optionally be carried out, in which case, according to step ii) of the process for producing a polymer film (P), in steps ii-c), ii-b), ii-o) and ii-m), a film of the at least one copolyamide and the at least one further polymer (FP) is obtained in each case in molten form, and that, according to step iii) of the process for producing a polymer film (P), this film is cooled in steps iii-c), iii-b), iii-o) and iii-m).
[0216] The explanations and preferred conditions given above for the optional step i1) of the process for producing the polymer film (P) apply mutatis mutandis to the optional step i1).
[0217] Preferably, step i1) is not carried out in the biaxially oriented polyamide film process, and therefore preferably, in the biaxially oriented polyamide film process, no further polymer (FP) is provided in a further extruder.
[0218] After being produced, the existing stretched polymer film (P) can be, for example, wound up. Methods for this purpose are known to those skilled in the art. If the stretched polymer film (SP) is tubular, such as in the blown and multi-blow processes, it can also be slit before winding up the tube. The slit film can then be wound up on one or more reels.
[0219] Use of polymer film (P) The polymer film (P) of the present invention can be used in all fields known to the person skilled in the art in which polymer films are used, in particular as packaging films.
[0220] The present invention therefore also provides the use of the polymer film (P) of the present invention as a packaging film.
[0221] The present invention will now be described in more detail with reference to examples. EXAMPLES
[0222] Molecular weights were determined by gel permeation chromatography against poly(methyl methacrylate) standards from Polymer Standard Services GmbH®, Mainz. The solvent was hexafluoro-2-propanol and the concentration of the polymer at the time of injection onto the styrene-divinylbenzene column was 1.5 mg / ml. The theoretical plate number was 20,000.
[0223] The viscosity numbers of the polyamides free of 1,5-diamino-3-oxapentane units were determined in accordance with EN ISO 307:2007+AMD 1:2013 in a 0.5% by weight solution in 96% by weight sulfuric acid at 25° C.
[0224] The viscosity numbers of polyamides containing 1,5-diamino-3-oxapentane units were determined at 25°C in a 0.5% by weight solution of phenol / o-dichlorobenzene in a weight ratio of 1:1 in a manner similar to that described in EN ISO 307:2007+Amd 1:2013.
[0225] The glass transition temperature and melting temperature were measured according to ISO 11357-1:2009, ISO 11357-2:2013, and ISO 11357-3:2011 by performing two heating runs and determining the glass transition temperature and melting temperature based on the second heating run.
[0226] To determine the proportion of adipic acid and 1,5-diamino-3-oxapentane in the copolyamide, the copolyamide was hydrolyzed in dilute hydrochloric acid (20%). This resulted in the protonation of the units derived from 1,5-diamino-3-oxapentane, with the chloride ion from the hydrochloric acid forming the counterion. This chloride ion was then exchanged for a hydroxide ion using an ion exchanger, liberating 1,5-diamino-3-oxapentane. The concentration of 1,5-diamino-3-oxapentane was then measured by titration with 0.1 molar hydrochloric acid, and the proportion of adipic acid and 1,5-diamino-3-oxapentane in the copolyamide was calculated therefrom.
[0227] The density was determined at a temperature of 25° C. in accordance with DIN EN ISO 1183-3.
[0228] The statistical distribution of the individual monomers in the copolyamide is 13 The carbonyl carbon atoms of caprolactam adjacent to 1,5-diamino-3-oxapentane were determined by C NMR by dissolving the sample in deuterated hexafluoro-2-propanol and assigning the following carbonyl carbon signals by 2D NMR: a.) the carbonyl carbon atom of caprolactam adjacent to 1,5-diamino-3-oxapentane is shifted to 183.6, b.) the carbonyl carbon atom of adipic acid adjacent to 1,5-diamino-3-oxapentane is shifted to 182.9, c.) the carbonyl carbon atom of caprolactam adjacent to caprolactam is shifted to 181.7, d.) the carbonyl carbon atom of adipic acid adjacent to caprolactam is shifted to 181.0. 13 C NMR signals were measured using a Bruker® AV 399 instrument.
[0229] Water vapor permeability and water vapor transmission rate were determined in duplicate measurements at 23° C. and 85% relative humidity according to ASTM F 1249 on a Permatran-W® model 3 / 33 instrument from MOCON®.
[0230] The Elmendorf tear resistance was measured in the extrusion direction (MD) and transversely thereto (TD) according to DIN ISO 6383-2:2004. Prior to the measurements, the films were conditioned according to standard climates for non-tropical countries as described in DIN EN ISO 291:2008. An 8 N pendulum weight was used in the Lorentzen&Wettre® tear tester.
[0231] The puncture resistance was measured using a metal spike with a diameter of 0.8 mm and a speed of 100 mm / min according to DIN EN 14477. Prior to the measurements, the films were conditioned according to standard climates for non-tropical countries as described in DIN EN ISO 291:2008.
[0232] Oxygen transmission rate and oxygen permeability were determined in duplicate measurements at 23° C. and 0% relative humidity according to ASTM F 1927 in an OX-TRAN® instrument.
[0233] The water permeability was measured using tubular film sections of 12 cm in length and 6 cm in width (see Figure 1, which shows the experimental setup for determining the water permeability). These were produced on a Weber blown film line with a nozzle diameter of 50 mm and an extruder length of 25 cm. First, the thickness of one side of the cross section of the tubular film was determined, and then one open end of the tubular section was heat sealed at 155 °C and the tubular section was cut to a length of 100 cm. 2 of distilled water and finally the other end of the tubular part was heat sealed at 155°C. To avoid damage to the heat seal joint (see Figure 1) and to measure the initial weight, both ends of the completely closed water-filled bag were attached to an aluminum cover. The weight loss at 23°C and 50% relative humidity was recorded every 24 hours for the first 3 days and then after 7 and 8 days by subtracting the current weight from the original weight.
[0234] The following polymers were used: polyamide A-1 Polyamide 6 manufactured by BASF SE®, sold under the trade name Ultramid® B40L, has a viscosity of 250 ml / g, a glass transition temperature of 57° C., a melting temperature of 220° C. and a density of 1.15 g / ml.
[0235] Copolyamides containing 1,5-diamino-3-oxapentane: C-1 A copolyamide of caprolactam, adipic acid, and 1,5-diamino-3-oxapentane was prepared in the following manner. 3230 g of caprolactam (component (A)), 237 g of 1,5-diamino-3-oxapentane (component (B2)), 333 g of adipic acid (component (B1)) and 190 g of water were mixed in a 7.8 l steel reactor and then purged 10 times with nitrogen. The vessel was then closed and heated to an external temperature of 260° C. within 40 minutes. At this point the internal pressure was 7 bar and the internal temperature was 208° C. The steel reactor was stirred under pressure for 50 minutes, then the pressure was released and the reactor was stirred for a further 2 hours and 45 minutes. During this time the internal temperature rose to 237° C. The vessel was then pressurized with 15 bar of N2, the valve was opened and the formed molten strands were pelletized in a water bath. The resulting pellets were extracted with boiling water under reflux for 16 hours and then dried at 70° C. under reduced pressure. The measured M W was 59 600 and the measured Mn was 24 000.
[0236] The pellets were then condensed for an additional 10 hours at 170° C. in a nitrogen stream. The viscosity number of the resulting copolyamide was 238 ml / g, the glass transition temperature was 47° C., and the melting temperature was 198° C. The proportion of 1,5-diamino-3-oxapentane.6 in the copolyamide was 15.5% by weight, based on the total weight of the copolyamide, and the density was 1.149 g / ml.
[0237] C-2 A copolyamide of caprolactam, adipic acid, and 1,5-diamino-3-oxapentane was prepared in the following manner. 3040 g of caprolactam (component (A)), 316 g of 1,5-diamino-3-oxapentane (component (B2)), 444 g of adipic acid (component (B1)) and 190 g of water were mixed in a 7.8 l steel reactor and purged 10 times with nitrogen. The vessel was then closed and heated to an external temperature of 260° C. within 45 minutes. At this point the internal pressure was 7 bar and the internal temperature was 207° C. The steel reactor was stirred under pressure for 40 minutes, then the pressure was released and the reactor was stirred for a further 2 hours and 30 minutes. During this time the internal temperature rose to 235° C. The vessel was then pressurized with 15 bar of N2, the valve was opened and the formed molten strands were pelletized in a water bath. The resulting pellets were extracted with boiling water under reflux for 16 hours and then dried at 70° C. under reduced pressure. The measured M W was 61 900 and the measured Mn was 25 600.
[0238] The pellets were then condensed for an additional 10 hours at 170° C. in a nitrogen stream. The resulting copolyamide had a viscosity number of 235 ml / g, a glass transition temperature of 45° C. and a melting temperature of 192° C. The proportion of 1,5-diamino-3-oxapentane.6 in the copolyamide was 20.3% by weight, based on the total weight of the copolyamide, and the density was 1.142 g / ml.
[0239] 13 In the C NMR spectrum, the relative integrals were 14.7% for signals a.), 4.7% for b.), 63.9% for c.), and 16.8% for d.).
[0240] C-3 A copolyamide of caprolactam, adipic acid, and 1,5-diamino-3-oxapentane was prepared in the following manner. 2850 g of caprolactam (component (A)), 395 g of 1,5-diamino-3-oxapentane (component (B2)), 555 g of adipic acid (component (B1)) and 190 g of water were mixed in a 7.8 l steel reactor and purged 10 times with nitrogen. The vessel was then closed and heated within 50 minutes to an external temperature of 260°C. At this point the internal pressure was 8 bar and the internal temperature was 205°C. The steel reactor was stirred under pressure for 35 minutes, then the pressure was released and the reactor was stirred for a further 2 hours and 15 minutes. During this time the internal temperature rose to 235°C. The vessel was then pressurized with 15 bar of N2, the valve was opened and the formed molten strands were pelletized in a water bath. The resulting pellets were extracted with boiling water under reflux for 16 hours and then dried at 70°C under reduced pressure. The measured M W was 58 400 and the measured Mn was 25 400.
[0241] The pellets were then further condensed at 170° C. for 13 hours in a nitrogen stream. The resulting copolyamide had a viscosity number of 237 ml / g, a glass transition temperature of 44° C. and a melting temperature of 186° C. The proportion of 1,5-diamino-3-oxapentane.6 in the copolyamide was 25.3% by weight based on the total weight of the copolyamide and the density was 1.152 g / ml.
[0242] 13 In the C NMR spectrum, the relative integrals were 19.3% for signals a.), 9.2% for b.), 53.8% for c.), and 17.8% for d.).
[0243] A copolyamide of C-4 caprolactam, adipic acid, and 1,5-diamino-3-oxapentane was prepared in the following manner. 2660 g of caprolactam (component (A)), 474 g of 1,5-diamino-3-oxapentane (component (B2)), 665 g of adipic acid (component (B1)) and 190 g of water were mixed in a 7.8 l steel reactor and purged 10 times with nitrogen. The vessel was then closed and heated within 15 minutes to an external temperature of 260°C. At this point the internal pressure was 1 bar and the internal temperature was 110°C. The steel reactor was stirred under pressure for 90 minutes, then the pressure was released and the reactor was stirred for a further 3 hours and 20 minutes. During this time the internal temperature rose to 237°C. The vessel was then pressurized with 15 bar of N2, the valve was opened and the formed molten strands were pelletized in a water bath. The resulting pellets were extracted with boiling water under reflux for 16 hours and then dried at 70°C under reduced pressure. The measured M W The measured Mn was 23,300.
[0244] The pellets were then further condensed at 170° C. for 13 hours in a nitrogen stream. The resulting copolyamide had a viscosity number of 231 ml / g, a glass transition temperature of 42° C. and a melting temperature of 179° C. The proportion of 1,5-diamino-3-oxapentane.6 in the copolyamide was 30.2% by weight based on the total weight of the copolyamide and the density was 1.154 g / ml.
[0245] Production of monofilms by the casting method: Monofilms of materials A-1, C-1, C-2, C-3, and C-4 were extruded in a Weber cast extrusion system equipped with a 30 mm diameter extruder screw at a throughput of 5 kg / h. The cooling roller was cooled to 20° C. The width of the films was 150 mm. The properties of the extruded film were as follows:
[0246] [Table 1]
[0247] The above examples show that films of copolyamides according to the invention have significantly increased water vapor permeability and tear propagation resistance compared to polyamide 6. The puncture resistance is slightly increased compared to polyamide 6 and the oxygen permeability is actually slightly lower for materials C-2, C-3 and C-4.
[0248] These copolyamides are therefore very well suited for packaging materials where it is intended that moisture escape from the packaging material.
[0249] Figure 2 shows the water permeability from sealed bags made with material A-1, with a film diameter of 26.73 μm, and material C-3, with a film diameter of 24.67 μm. The bag made with the inventive copolyamide C-3 had released all the water from its interior to the surrounding air after 8 days, while 82% of the water was still present in the bag made with material A-1. The two bags were stored next to each other at room temperature of 23°C and relative humidity of 50%.
Claims
1. Ingredients below: (A) 60 to 95% by weight of at least one lactam; and (B) 5 to 40% by weight of a monomer mixture (M) containing the following components: (B1) at least one C 4 ~C 12 dicarboxylic acids, and (B2) at least one diamine wherein component (B2) comprises 1,5-diamino-3-oxapentane, and said weight percentages of components (A) and (B) are based on the sum of said weight percentages of components (A) and (B), respectively. A copolyamide produced by polymerizing
2. 2. The copolyamide of claim 1, wherein component (A) is selected from the group consisting of 6-aminohexanolactam and 12-aminododecanolactam.
3. 3. The copolyamide of claim 1, wherein component (A) is 6-aminohexanolactam.
4. 4. Copolyamide according to claim 1 , wherein component (B) comprises in the range of 45 to 55 mol % of component (B1) and in the range of 45 to 55 mol % of component (B2), in each case based on the total molar amount of component (B).
5. 5. The copolyamide according to claim 1, wherein component (B1) is selected from the group consisting of butanedioic acid (succinic acid), pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), heptanedioic acid (pimelic acid), octanedioic acid (suberic acid), nonanedioic acid (azelaic acid), decanedioic acid (sebacic acid), undecanedioic acid, dodecanedioic acid, terephthalic acid, and isophthalic acid.
6. 6. Copolyamide according to claim 1, wherein component (B1) is hexanedioic acid (adipic acid).
7. Glass transition temperature (T G(c) ) and the glass transition temperature (T G(c) 7. The copolyamide according to claim 1, wherein the temperature is in the range of 30° C. to 70° C.
8. Melting temperature (T M(c) ) and said melting temperature (T M(c) 8. The copolyamide according to claim 1 , wherein the temperature (T) of the copolymer is in the range of 100° C. to 210° C.
9. A polymeric film (P) comprising at least one copolyamide according to at least one of the claims 1 to 8.
10. The polymer film (P) according to claim 9, wherein the thickness of the polymer film (P) is in the range of 5 μm to 100 μm.
11. 11. The polymer film (P) according to claim 9 or 10, wherein the polymer film (P) is produced by the cast process, the blow process, the multi-blow process or the biaxially oriented polyamide film process.
12. A process for producing a polymer film (P), comprising the steps of: i) providing at least one copolyamide according to at least one of claims 1 to 8 in molten form in an extruder; ii) extruding said at least one copolyamide provided in step i) in molten form from said first extruder through a die to obtain a film of at least one copolyamide in molten form; iii) cooling said film of said at least one copolyamide in molten form obtained in step ii), wherein said at least one copolyamide solidifies to obtain said polymer film (P). The method includes:
13. A method for producing a polymer film (P) according to claim 12, comprising the additional steps: (iv) Stretching the polymer film (P) to obtain a stretched polymer film (SP). The method includes:
14. 14. The method for producing a polymer film (P) according to claim 13, wherein steps (iii) and (iv) are carried out alternately or simultaneously.
15. Use of a polymer film (P) according to any one of claims 9 to 11 as a packaging film.
Citation Information
Patent Citations
Manufacture of polyamide sheet product
JP1990073858A
Production of polyamide containing 2,5-bis(aminomethyl)furan
JP2018520242A
Polymer film containing a copolyamide of a diamine, a dimer acid and a lactam
JP2019529638A
Process for the production of elastic copolyamides
DE2846596A1
Process for the preparation of polyamide sheets
EP0352562A2