High remanence neodymium iron boron magnet and its manufacturing method and application
A neodymium iron boron magnet with controlled elemental compositions and optimized manufacturing processes achieves high remanence and coercive force, addressing process limitations and resource imbalances to enhance magnetic stability and efficiency.
Patent Information
- Application Number
- JP2024518537
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-22
- Filing Date
- 2022-09-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-09-22
AI Technical Summary
Existing neodymium iron boron magnets face challenges in achieving high remanence and coercive force due to process difficulties, equipment precision limitations, and imbalances in heavy rare earth resources, leading to poor demagnetization resistance and inconsistent magnetic properties.
A neodymium iron boron magnet with controlled compositions of R, T, B, M1, and M2 elements, along with a manufacturing process involving smelting, rapid cooling, milling, press forming, and multiple sintering stages, to optimize grain boundary phases and enhance magnetic properties.
The magnet achieves high remanence (Br ≥ 1.44T) and coercive force (Hcj ≥ 1100kA/m) with excellent squareness (≥0.95), enabling stable magnetic performance and efficient motor operation with reduced volume and cost.
Smart Images

Figure 2024536834000001 
Figure 2024536834000002 
Figure 2024536834000003
Abstract
Description
Detailed Description of the Invention
[0001] [Priority and related applications] This application claims priority to a prior application, bearing patent application number 202111107088.3 and entitled "High remanence neodymium iron boron magnet and its manufacturing method and application," filed with the State Intellectual Property Office of the People's Republic of China on September 22, 2021. The above prior application is hereby incorporated by reference in its entirety.
[0002] [Technical field] The present invention belongs to the field of neodymium-iron-boron magnets, and more particularly to a neodymium-iron-boron based sintered magnet and its manufacturing method and applications.
[0003] [Background technology] Neodymium-iron-boron sintered magnets, as the fourth generation permanent magnet material, are known as the "king of magnetism" due to their excellent magnetic properties and are widely used in many fields such as automobiles, wind power generation, compressors, elevators and industrial automation.
[0004] Since the beginning of the 21st century, magnetic steel has attracted increasing attention for its improvement in coercivity performance. In particular, due to an imbalance in the supply of heavy rare earth resources, which are in relatively scarce stocks, and the cost issues caused by the rapid rise in raw material prices, many scholars and companies have been conducting research into techniques such as grain refinement and grain boundary diffusion to maintain and further improve coercivity performance, in order to ensure the demagnetization resistance of magnetic steel at operating temperatures, on the premise of reducing the amount of heavy rare earth used.
[0005] With the rise of the new energy vehicle market and new policies for high-efficiency, energy-saving home appliances, motor miniaturization and high efficiency indicators have become new points of interest. In order to ensure that motors are as small as possible and that the output power of the motors is maintained or even improved, the magnetic steel, which is the core of the motor, needs to have high energy density, i.e., high residual magnetism.
[0006] Theoretically, the limit remanence of pure neodymium iron boron magnets is 1.61T, and currently, the maximum remanence obtained under laboratory conditions is 1.56T, but due to process difficulties, equipment precision, and other reasons, it is far from mass production. At the same time, the mainstream remanence range of magnetic steels used in fields such as new energy automobiles and energy-saving home appliances is between 1.10 and 1.40T, and if the remanence can be further increased, it can effectively promote the demand for miniaturization and high efficiency levels of motors.
[0007] Patent CN111724985A In the present study, an alloy with a low B composition (0.80-0.93wt%) is smelted to have a certain amount of transition metal phase (R6T13M) to produce a sintered magnet (or a diffused magnet), and the sintered magnet (or the diffused magnet) is then subjected to a heat treatment at a temperature of 400°C to 600°C for 10 seconds to 30 minutes, so that the magnet has high remanence and high Hcj at the same time, and the remanence can reach 1.41T. The use of a low B composition produces a relatively wide R6T13M phase at the grain boundary, but due to the requirements of the theoretical formula for the remanence of NdFeB magnets, the main phase volume ratio is reduced and its Br is inevitably reduced. In addition, the R6T13M phase in the grain boundary is useful for improving Hcj, but the stability of the grain boundary phase is relatively low, and the difficulty of controlling the equipment process is highly required, and the perpendicularity of the magnet is easily variable and cannot be stably made larger than 0.95, which directly affects the high temperature demagnetization resistance of the motor.
[0008] Patent CN107424699AThe alloy is smelted with a low B composition (0.94wt%), alloy sheets with a columnar crystal ratio of 95% or more are produced, which are then processed in a rotary hydrogen crushing furnace and jet-milled powder with a size of 3.75-3.9μm is produced using high-pressure nitrogen gas, enabling the production of ultra-high performance NdFeB magnets with Br of 1.44-1.48T and Hcj of 14-16kOe. By controlling the columnar crystal ratio of the alloy flakes, optimizing the HD production process, controlling the particle size range of the jet-milled powder, and further matching it with the sintering process, magnets with high Br and high Hcj can be obtained. However, the RE content is extremely low, and there is no sufficient Nd-rich phase to uniformly surround the main phase crystal grains during sintering and promote sintering. At the same time, there is no grain boundary phase such as Zr or Ti borides, which makes it easy for the crystal grains to grow abnormally, and the magnet crystal grains are non-uniform in size, resulting in a poor squareness. Although it has high Br and Hcj, the areas of abnormal grain growth are extremely prone to reverse magnetization, deteriorating the demagnetization resistance of the magnet.
[0009] Summary of the Invention In order to solve the above technical problems, the present invention proposes a high remanence NdFeB magnet and its manufacturing method and application.
[0010] The present invention provides a neodymium iron boron magnet, the magnet having crystal grains mainly composed of an RTB type compound and a grain boundary phase, the neodymium iron boron magnet being: R is 28wt% or more and 30wt% or less, T is 63wt% or more and 70wt% or less, B is 0.98wt% or more and 1.05wt% or less, M1 is greater than 0 wt% and less than or equal to 0.3 wt%; M2 is 0.04 wt% or more and 0.15 wt% or less, R represents a rare earth element, and is Nd, or Nd and at least one selected from the rare earth elements Pr, La, Ce, Dy, Tb, and Ho; T is selected from Fe and / or Co, in which Fe accounts for 99 wt% or more of the total amount of T; M1 is selected from Cu and Ga, and Ga accounts for 75 wt% or more of the total amount of M1; M2 is at least one selected from Zr, Ti and Nb.
[0011] Preferably, M2 is selected from Ti.
[0012] According to an embodiment of the present invention, in the raw materials for producing the above-mentioned neodymium iron boron magnet, the atomic numbers of elements further satisfy the following condition.
[0013] 2.15≦[R] / ([B]-2[M2])≦2.35
[0014] In the above, [R] is the atomic percentage of R, [B] is the atomic percentage of B, and [M2] is the atomic percentage of M2. In the present invention, the atomic percentage means [the number of a certain atom] / [the total number of each atom in the raw material].
[0015] Illustratively, [R] / ([B]-2[M2]) is 2.15, 2.2, 2.24, 2.29, and 2.3.
[0016] According to an embodiment of the present invention, when R is at least one selected from Nd and rare earth elements Pr, La, Ce, Dy, Thb, and Ho, the total mass of heavy rare earth elements such as Dy, Thb, and Ho accounts for 1 wt% or less of the mass of the magnet, and preferably 0.5 wt% or less.
[0017] According to an embodiment of the present invention, the magnet has the following magnetic properties: (1) Perpendicularity ≧ 0.95, for example 0.95, 0.96, 0.97, 0.98, 0.99; (2) Br ≧ 1.44T, for example 1.45T, 1.46T, 1.47T, 1.48T, 1.49T, 1.5T; (3) Hcj≧1100kA / m, for example, 1100kA / m, 1110kA / m, 1120kA / m, 1130kA / m, 1140kA / m, 1150kA / m, 1160kA / m, 1170kA / m, 1180kA / m, 1190kA / m, 1200kA / m.
[0018] In the present invention, the content of each element in the manufacturing raw material is strictly limited, specifically, The magnetic polarization strength of the RTB-based main phase crystal grains made of rare earth elements such as Pr, Dy, Tb, and Ho is lower than that of Nd, which significantly reduces the Br of the magnet and ensures a high Br of the magnet, while at the same time increasing the Hcj of the magnet by using a small amount of heavy rare earth elements such as Dy, Tb, and Ho. If the R in the magnet is too high, the neodymium-rich phase of the magnet increases and Br decreases, and if the R is too low, a uniform and continuous Nd-rich phase cannot be formed in the magnet for magnetic insulation of the main phase crystal grains, causing a rapid deterioration in the Hcj and squareness of the magnet.
[0019] Co occupies the position of Fe in the main phase crystal grains, and the atomic magnetic moment of Co is smaller than that of Fe, so adding Co reduces the Br of the magnet. Therefore, Fe is controlled to account for 99% or more of the total T, and at the same time, by controlling the other components and optimizing the process, the corrosion resistance and temperature resistance of Co in the magnet are supplemented and improved.
[0020] The conventional technology produces high-performance NdFeB magnets with low B (≦0.95wt%) and improves the Hcj of the magnet by increasing the thickness of the grain boundary phase through the formation of RT-Ga type grain boundary phase, but as the grain boundary phase becomes thicker, the volume ratio of the main phase crystal grains is inevitably reduced, and the Br performance of the magnet is significantly reduced. The present invention increases the volume ratio of the main phase crystal grains by controlling the B content, and improves the Br of the magnet. When the B content is too low, the ratio of the formed B-rich phase or Nd-rich phase is relatively high and the volume ratio of the main phase crystal grains is small, so the Br of the magnet is relatively low, and when the B content is too high, the volume ratio of the B-rich phase becomes significantly high, which significantly reduces the magnetic properties.
[0021] M1 is mainly concentrated in the grain boundary phase, improving the structure of the grain boundary phase and greatly improving Hcj. If the magnet does not contain Cu and Ga, the main phase crystal grains and B-rich phase of the magnet will be relatively coarse, greatly reducing the magnetic properties of the magnet. If the content of Cu and Ga in the magnet is too high, it will inhibit the growth of crystal grains, and at the same time, the grain boundary phase will become thick, the volume ratio of the main phase crystal grains will decrease, and the Br of the magnet will decrease. When the Ga content of the present invention is reached, it can significantly improve the Hcj of the magnet, and has a significant optimization effect on the magnet temperature coefficient, avoiding the impact of low Co content on the temperature resistance of the magnet.
[0022] M2 and B form A2B type compounds, which exist in the grain boundary phase and play a role in inhibiting the abnormal growth of magnet crystal grains. If the content of M2 is too low, the existence of A2B type compounds cannot be effectively formed, so the abnormal growth of the main phase crystal grains of the magnet cannot be inhibited; if the content of M2 is too high, the A2B type compounds exist as grain boundary phases, which reduces the volume ratio of the main phase crystal grains, and the magnet cannot obtain high Br.
[0023] The present invention further provides a method for producing the above-mentioned NdFeB magnet, comprising: (a) a smelting step of melting raw materials for producing the NdFeB magnet at high temperature, casting the materials, and forming an alloy sheet after secondary cooling; (b) a milling step of pulverizing the alloy sheet to form an alloy powder; (c) a press molding step of press molding the alloy powder under the action of a magnetic field to obtain a billet; and (d) a sintering step of sintering the billet at high temperature.
[0024] According to an embodiment of the present invention, the (a) smelting step specifically includes fully melting the raw materials for manufacturing the NdFeB magnet into alloy molten steel in a vacuum or inert gas atmosphere, then rapidly cooling to form an alloy sheet, and further secondary cooling, and the interval between the secondary cooling and the rapid cooling does not exceed 10s, and the cooling rate of the secondary cooling is 5 to 20°C / s. Preferably, the melting is performed by medium frequency induction heating in a vacuum induction smelting furnace. In the present invention, the rapid cooling can be performed by any rapid cooling method commonly used in the technical field as long as the desired alloy sheet can be obtained. Exemplarily, the rapid cooling is performed using a quench roll.
[0025] In the present invention, the secondary cooling can be performed by selecting a cooling method and a cooling device commonly used in the art. Exemplarily, the secondary cooling is performed by using any one of a low-temperature inert gas spray, a water-cooled disk, or other types of cooling devices.
[0026] Preferably, the cooling rate of the secondary cooling is 5 to 20° C. / s.
[0027] Preferably, the alloy sheet has a thickness of 0.15 to 0.45 mm.
[0028] According to an embodiment of the present invention, the milling step (b) includes coarse grinding and fine grinding.
[0029] Preferably, the coarse grinding is selected from hydrogrinding and / or medium grinding.
[0030] Preferably, the pulverization is performed by a jet mill. Preferably, the jet mill is performed in an inert gas atmosphere. Preferably, the inert gas is selected from nitrogen gas, helium gas, and the like.
[0031] In the present invention, the above-mentioned hydro-grinding, medium grinding or jet milling can be carried out using operations known in the art.
[0032] Preferably, it is obtained after the above-mentioned fine grinding and by screening, such as grading wheel screening.
[0033] Preferably, the grain size SMD of the alloy powder is between 2.0-3.4 μm, and X90 / X10≦4.5, where SMD is the area average grain size, the smaller the SMD, the smaller the grain size of the powder particles, and the larger the SMD, the larger the grain size of the powder particles, X90 represents the grain size value when the cumulative distribution percentage reaches 90%, that is, all the grains are equal to or smaller than this grain size, and the number of grains larger than this grain size value is 0, and X10 represents the cumulative distribution percentage when 10 %, that is, the particle size of all particles is equal to or smaller than this particle size value, and the number of particles larger than this particle size value is 0. Here, X90 / X10 represents the particle size distribution of the powder, and the smaller X90 / X10 means that the particle size distribution of the powder is more concentrated.
[0034] Preferably, a lubricant should be added during pulverization, and preferably both before and after jet milling. Adding a lubricant before jet milling can improve the flowability of the powder, and improve the flowability and uniformity of the powder during jet milling, while adding a lubricant after jet milling can also improve the uniformity and flowability of the powder, facilitating uniform powder filling and pressing.
[0035] Preferably, the lubricant is selected from reagents known in the art and amounts known in the art so that the powder can be mixed sufficiently and uniformly and easily molded. Exemplarily, the lubricant is selected from organic solvents such as lipids or alcohols that are easily volatile, for example, zinc stearate. Exemplarily, the amount of the lubricant added is 0.1 to 1 wt% of the total mass of the raw materials.
[0036] Preferably, further mixing is required after adding the lubricant, and the mixing time is preferably 3 to 6 hours.
[0037] Mixing according to the present invention can be carried out using methods known in the art, such as, for example, mixing in a mixer.
[0038] According to an embodiment of the present invention, the press-molding step (c) specifically includes press-molding the alloy powder under the action of a magnetic field to obtain a billet.
[0039] Preferably, the pressing is carried out in a press die cavity.
[0040] Preferably, before press molding, it is necessary to perform alignment magnetization under a magnetic field strength of 2 T and then mold the material.
[0041] Preferably, after press molding, the material is demagnetized by applying an inverse magnetic field.
[0042] Preferably, the compacted billet can be further treated in a cold isostatic press to further increase the billet density.
[0043] According to an embodiment of the present invention, the sintering step (d) includes a first sintering, a first cooling, a second sintering, and a second cooling. The sintering step in the present invention can be performed using a method known in the art. Exemplarily, the billet is sintered in a sintering furnace.
[0044] Preferably, the sintering step is carried out in a vacuum atmosphere. Preferably, the degree of vacuum during heating is 10-1 Pa or less.
[0045] Preferably, the sintering temperature in the first sintering is 1000 to 1050° C., and the temperature retention time in the first sintering is 240 to 360 minutes.
[0046] Preferably, the second sintering temperature is 30 to 70°C higher than the first sintering temperature, and is preferably 1030 to 1100°C.
[0047] Preferably, the warming time for the second sintering is 270 to 360 minutes.
[0048] Preferably, both the first and second cooling steps are performed at temperatures below 200°C.
[0049] According to an embodiment of the present invention, the sintering step further includes an ageing treatment performed after the second cooling.
[0050] Preferably, the ageing treatment is selected from a primary ageing treatment or a secondary ageing treatment.
[0051] Preferably, the conditions for the primary aging treatment are that the aging treatment temperature is between 500 and 700° C. and the heat retention time is between 240 and 420 minutes.
[0052] Preferably, the secondary aging treatment includes a first aging treatment in which the temperature is increased to 800-950°C and the temperature is maintained for 180-300 min, and a second aging treatment in which the temperature is increased to between 450-600°C after cooling to 150°C or lower and the temperature is maintained for 240-360 min.
[0053] According to an embodiment of the present invention, after the sintering step, a diffusion treatment can also be performed.
[0054] Preferably, the diffusion treatment includes applying a diffusion material to the magnet surface, and performing a vacuum high temperature diffusion treatment, a diffusion cooling and a diffusion aging treatment.
[0055] Preferably, the diffusion material is selected from pure metals of Dy and / or Tb, or alloys such as hydrides, oxides, hydroxides, fluorides, etc. of Dy and / or Tb.
[0056] Preferably, the diffusion treatment can be carried out by using a method such as vacuum deposition, magnetron sputtering, coating or embedding.
[0057] Preferably, the temperature of the high-temperature diffusion is 850 to 950° C., and the time of the high-temperature diffusion is 10 to 30 hours.
[0058] Preferably, the diffusion cooling temperature is less than 100°C.
[0059] Preferably, the temperature of the diffusion aging treatment is 450 to 600° C., and the time of the diffusion aging treatment is 4 to 8 hours.
[0060] According to embodiments of the present invention, the billet may also be machined to a target size after the sintering process and before the diffusion process.
[0061] The present invention requires strict restriction of the conditions of each process in the magnet manufacturing method, specifically, when the alloy molten steel is rapidly cooled, take the rapid cooling by the chill roll as an example, the alloy sheet on the roll surface of the chill roll will form nucleation points, and the nucleation points will be used as the starting point to form and grow crystal grains. The alloy sheet will fall off the chill roll, and its temperature will drop from the melting temperature to about 800℃, in this case, the crystal grains will grow gradually, so it is necessary to carry out secondary cooling in a timely manner to reduce the temperature of the alloy sheet. If the time interval of secondary cooling is too long, the main phase crystal grains on the alloy sheet will continue to grow, and the temperature of the alloy sheet will diverge unevenly, resulting in secondary crystals. The existence of these secondary crystals will cause the main phase crystal grains to have poor uniformity in grain size, which will lead to poor squareness of the magnet. If the cooling rate is too slow, a large amount of B-rich phase will be formed in the grain boundary phase surrounding the main phase crystal grains, and the B-rich phase formed at this time cannot be effectively removed or reduced in processes such as milling and sintering, and the magnetic properties will inevitably deteriorate rapidly. If the cooling rate is too fast, the alloy sheet will be cooled too quickly, the growth of the main phase crystal grains will stop, and they will not be able to melt and absorb the surrounding grain boundary phase and B-rich phase to grow further, and the volume ratio will be relatively small, resulting in a decrease in the Br of the magnet.
[0062] As can be seen from the above, since the content of R in the raw material for magnet manufacturing is relatively small, in addition to the existence of binary and ternary grain boundary phases between the main phase grains on the alloy sheet, some of the main phase grains are in direct contact with each other, and the bonding strength between such directly contacting main phase grains is extremely high. If the grain size of the alloy powder is too small, the alloy powder particles will break with the grain boundary phase as the main breaking area, and at the same time, internal breakage of the main phase grains will occur to achieve the target powder grain size, and such broken powder will have irregular size and surface condition, and it is easy to form reverse magnetization points in the contact areas with the adjacent grains and grain boundary phases after sintering, which indicates that the magnet has a low squareness and is easy to be demagnetized under the action of high temperature or other external magnetic fields. If the grain size of the powder is too large, the grain boundary phase cannot be fully detached from the main phase grains, so the Nd-rich phase that is melted and attached to the main phase grains during sintering will grow, and there will be no enough Nd-rich phase to wrap the main phase grains, and the Hcj of the magnet will be greatly reduced. When the particle size distribution X90 / X10 of the powder is within the range of the present invention, a magnet with uniform and consistent particle size can be obtained, with relatively high Br and Hcj. If the particle size distribution X90 / X10 is too large, the crystal grain sizes of the magnet will be significantly different, and the fine powder will easily aggregate and melt to form triangular grain boundary phases, and the adjacent coarse powder will melt to form large crystal grains, all of which will have a significant impact on the squareness of the magnet.
[0063] At the same time, the present invention uses the secondary sintering process to greatly improve the magnet performance and effectively suppress the abnormal growth of magnet crystal grains. In the NdFeB magnet manufacturing method of the present invention, the second sintering temperature is higher than the first sintering temperature, and the first sintering is performed at a relatively low temperature, which can improve the density of the magnet, but some gaps still exist, and the abnormal growth of the main phase crystal grains is avoided; the second sintering temperature is relatively significantly higher than the first sintering temperature, which can promote sufficient growth of the main phase crystal grains, but does not cause the abnormal growth of the main phase crystal grains to rapidly deteriorate the magnetic properties. If the temperature difference between the two sintering temperatures is too low, the primary sintering temperature is relatively high, the crystal grain arrangement is relatively dense, and the relatively low secondary sintering temperature cannot fully reconstruct and optimize the crystal grain structure of the magnet, so that relatively high magnetic properties cannot be obtained. If the temperature difference between the two sintering temperatures is too large, the primary sintering temperature is relatively low, the gaps are relatively large, and the secondary sintering temperature is too high, which causes abnormal growth of the crystal grains in some areas, resulting in deterioration of the magnet performance.
[0064] The present invention further provides an application of the above magnet in the field of motors.
[0065] The present invention further provides a motor including the above magnet.
[0066] The present invention further provides applications of the above motor, preferably, the above motor can be applied to new energy vehicles and energy-saving home appliances.
[0067] [Beneficial Effects] In the NdFeB magnet of the present invention, by adjusting the ratios of elements such as B, Cu, Ga, RE, and Ti, a relatively high volume ratio of main phase crystal grains can be obtained and the ratio of the B-rich phase in the grain boundary phase can be effectively suppressed. By adding transition metal elements M1 (e.g. Ga) and M2 (e.g. Ti), the structure of the grain boundary phase is optimized and adjusted, giving the magnet a relatively high Br, and simultaneously providing excellent Hcj and squareness performance.
[0068] In the present invention, the content of B is higher than that of a general NdFeB sintered magnet. When a general NdFeB magnet has both Br and Hcj performance, [R] / ([B]-2[M2]) is slightly greater than 2.35, but is greater than 2.5, and the B-rich phase is relatively small or absent. In the present invention, the ratio is set between 2.15 and 2.35, so that more B-rich phase is theoretically formed compared to a general NdFeB magnet. However, within the ratio range of this relational formula, the volume ratio of the main phase crystal grains of the magnet can be increased in accordance with the secondary cooling in the manufacturing method of the present invention, and the excessive formation of the B-rich phase can be suppressed, ensuring the magnet Br while at the same time having excellent Hcj and squareness index.
[0069] The magnet of the present invention uses very small amounts of heavy rare earth elements such as Dy / Tb, or even does not use any of them, yet has high remanence and coercivity, and the magnet has a squareness of ≧0.95. The manufacturing process is simple, and mass production is stable.
[0070] When a magnet is manufactured using the manufacturing method of the present invention, it has high remanence, Br≧1.44T, and very high energy density. When applied to a motor, it can effectively improve the power output per unit volume and effectively reduce the volume of the motor, saving the material loss of other parts of the motor, and playing an important role in reducing the size and cost of the motor.
[0071] [Mode for carrying out the invention] The technical solution of the present invention will be described in more detail below with reference to specific examples. It should be understood that the following examples are merely illustrative and explanatory of the present invention and should not be construed as limiting the scope of the claims of the present invention. Any technology realized based on the above content of the present invention is included in the scope of the claims of the present invention.
[0072] Unless otherwise specified, all materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0073] In the following examples, atomic percentage means [number of a certain atom] / [total number of each atom in the raw material], where M1 is selected from Cu and Ga, M2 is at least one selected from Zr, Ti, and Nb, and R is at least one selected from Nd and rare earth elements Pr, La, Ce, Dy, Tb, and Ho.
[0074] [Examples 1 to 4] (1) The raw materials were mixed according to the target composition of the magnet in Table 1, and a Nd-Fe-B alloy sheet was produced by a melt spinning casting process. The alloy sheet was cooled by a quenching roll and dropped off, and then secondary cooling was performed by injecting low-temperature argon gas. By adjusting the flow rate and temperature of the low-temperature argon gas, the alloy sheet was obtained by secondary cooling at a cooling rate of 10°C / s. The alloy sheet was dropped onto a water-cooled disk and collected, thereby producing an alloy sheet with a thickness of 0.15 to 0.45 mm.
[0075] [Table 1]
[0076] (2) The alloy sheet was coarsely crushed by hydrogen crushing process to obtain powder, and zinc stearate, the mass of which was 0.1wt% of the raw material, was added to the powder as a lubricant and mixed for 60min. The mixed material was finely crushed in a fluidized bed jet mill, and nitrogen gas was used as the polishing gas to obtain jet mill powder with the target particle size SMD=2.5μm by adjusting the equipment parameters such as the rotation speed of the grading wheel and the polishing pressure.
[0077] (3) Zinc stearate, the mass of which is 0.2 wt% of the raw materials, is further added as a lubricant to the jet mill powder of the target particle size produced, and after thorough mixing, it is pressed under a magnetization magnetic field strength of 2 T to form a billet, and the billet is further densified by oil cold isostatic pressing treatment.
[0078] (4) The billet was placed in a sintering furnace and subjected to secondary sintering treatment in a vacuum atmosphere. The sintering heat retention time for both cycles was 270 min. When the sintering cooling time was below 80°C, the material was heated to 890°C and kept at that temperature for 240 min. After cooling, the material was subjected to secondary aging, and the aging temperature was adjusted to the optimum value according to the composition. The aging heat retention time was 280 min. The specific sintering aging regime is shown in Table 2.
[0079] [Table 2]
[0080] The magnets after sintering and aging treatment were processed into standard sample columns with a diameter of 10 mm and a height of 10 mm, and the magnet performance was measured using a BH analyzer. The specific magnetic property measurement results are shown in Table 3.
[0081] [Table 3]
[0082] As can be seen from the results in Table 3, when the composition of each element is within the control range, the magnet has relatively high remanence and coercivity, while at the same time ensuring a squareness of ≥ 0.95, which ensures that the magnet can provide a stable power output when the motor is running.
[0083] [Comparative Examples 1-2] The raw materials were blended according to the target composition of the magnet in Table 4, and a NdFeB alloy sheet was produced by a melt spinning casting process. The alloy sheet was cooled by a quenching roll and dropped off, and then secondary cooling was performed by injecting low-temperature argon gas. By adjusting the flow rate and temperature of the low-temperature argon gas, the alloy sheet was secondary cooled at a cooling rate of 10°C / s to obtain an alloy sheet. The alloy sheet was dropped onto a water-cooled disk and collected to obtain an alloy sheet.
[0084] Comparative Example 3 The raw materials were blended according to the target composition of the magnet in Table 4, and a NdFeB alloy sheet was produced by a melt spinning casting process. The alloy sheet was quenched by a quench roll and then directly dropped onto a water-cooled disk for cooling and recovery.
[0085] Comparative Example 4 The raw materials were blended according to the target composition of the magnet in Table 4, and a NdFeB alloy sheet was produced by a melt spinning casting process. The alloy sheet was quenched by a quench roll and then directly dropped onto a water-cooled disk for cooling and recovery.
[0086] [Table 4]
[0087] The alloy sheets obtained in Comparative Examples 1 to 4 were prepared into jet mill powders with a target SMD of 2.5 μm by the same process as in the Examples, and then pressed and sintered and aged. The specific process parameters are shown in Table 5.
[0088] [Table 5]
[0089] The magnets produced in Comparative Examples 1 to 4 were processed into standard sample columns with a diameter of 10 mm and a height of 10 mm, and the magnet performance was measured using a BH analyzer. Specific magnetic property measurement results are shown in Table 6.
[0090] [Table 6]
[0091] As can be seen from Comparative Example 1, when the ratio of [R], [B], and [M2] exceeds 2.35, Hcj is slightly improved, but Br is obviously reduced, and the squareness is less than 0.95, so the demagnetization resistance fluctuates and the motor cannot output a stable magnetic field during high-speed operation.
[0092] Since the ratio relationship between [Cu] and [Ga] in Comparative Example 2 is much smaller than 0.75, the Br and Hcj of the magnet are both significantly lower than those of the Examples, and it is not possible to simultaneously possess high remanence and high coercivity.
[0093] The composition of the target magnet in Comparative Example 3 is the same as that of Example 1, but the alloy sheet is not subjected to secondary cooling in the smelting process using the method claimed in the present patent. As can be seen from Table 3, when the secondary cooling of the alloy sheet is eliminated, the alloy sheet experiences significant grain growth and increases in thickness. When jet mill polishing is performed, jet milled powder with the target SMD is obtained, but the particle size distribution (X90 / X10) significantly deteriorates, the ratio of coarse powder and fine powder increases, the powder uniformity is low, and in the sintering process, only primary sintering is performed and no secondary sintering process is performed, so the remanence and coercivity of the magnet are both significantly reduced.
[0094] As can be seen from Comparative Example 4, when the ratio relationship of [Cu] and [Ga] is less than 0.75 and the secondary cooling and secondary sintering processes described in the present invention are not used, the Hcj is obviously reduced and the squareness is far lower than 0.95, so that the demagnetization resistance fluctuates and the motor cannot stably output a magnetic field when operating at high speed.
[0095] Example 5 The magnet after sintering and aging in Example 1 was taken and processed into a sheet product with a length of 20 mm, a width of 20 mm and a thickness of 5 mm, and a thin film of metallic Dy was added to the magnet surface by a dip coating process, and then the magnet was subjected to a diffusion treatment at 900°C for 15 hours, and after the diffusion temperature was cooled to less than 100°C, the magnet was further heated to 500°C and subjected to an aging treatment for 5 hours. The magnetic properties and composition of the final magnet were measured. The final composition and magnetic property results are shown in Tables 9 and 10.
[0096] [Table 7]
[0097] [Table 8]
[0098] As can be seen from the above results, the coercive force of the magnet after diffusion is significantly improved, and Br does not obviously decrease, so the magnet of the present invention can also be used as a diffusion base material.
[0099] The exemplary embodiments of the present invention have been described above. However, the present invention is not limited to the above embodiments. Any modifications, equivalent replacements, improvements, etc. made by those skilled in the art without departing from the spirit and principles of the present invention should be included within the scope of the claims of the present invention.
Claims
1. A neodymium iron boron magnet, The neodymium iron boron magnet has crystal grains having an R-T-B type compound as a main structure and a grain boundary phase, R of 28 wt% or more and 30 wt% or less; T of 63 wt% or more and 70 wt% or less; 0.98 wt% or more and 1.05 wt% or less of B; M1 is greater than 0 wt% and less than or equal to 0.3 wt%; M2 is 0.04 wt% or more and 0.15 wt% or less; R represents a rare earth element, and is Nd, or Nd and at least one selected from the rare earth elements Pr, La, Ce, Dy, Tb, and Ho; T is selected from Fe and / or Co, in which Fe accounts for 99 wt % or more of the total amount of T; M1 is selected from Cu and Ga, and Ga accounts for 75 wt % or more of the total amount of M1; M2 is at least one selected from Zr, Ti, and Nb; In the manufacturing raw materials of the neodymium iron boron magnet, the atomic number of the elements further satisfies the following conditions: 2.15≦[R] / ([B]-2[M2])≦2.35, Wherein, [R] is the atomic percentage of R, [B] is the atomic percentage of B, and [M2] is the atomic percentage of M2; When R is at least one selected from Nd and rare earth elements Pr, La, Ce, Dy, Tb, and Ho, the total mass of heavy rare earth elements such as Dy, Tb, and Ho is 1 wt % or less of the mass of the magnet, The magnet is (4) Perpendicularity ≧ 0.95; (5) Br≧1.44T, (6) Having magnetic properties of Hcj≧1100 kA / m; A neodymium iron boron magnet characterized by:
2. The total mass of heavy rare earth elements such as Dy, Tb, and Ho is 0.5 wt % or less of the mass of the magnet, Preferably, M2 is selected from Ti; 2. The neodymium iron boron magnet according to claim 1 .
3. (a) a smelting step of melting the raw materials for manufacturing the NdFeB magnet at a high temperature, casting the raw materials, and forming an alloy sheet after secondary cooling; (b) a milling step of pulverizing the alloy sheet to form an alloy powder; and (c) a press forming step of press forming the alloy powder under the action of a magnetic field to obtain a billet. (d) sintering the billet at a high temperature.
3. The method for producing a neodymium iron boron magnet according to claim 1 or 2.
4. The (a) smelting step specifically includes: fully melting the raw materials for producing the NdFeB magnet into alloy molten steel in a vacuum or inert gas atmosphere, then rapidly cooling to form an alloy sheet, and then secondary cooling; the interval between the secondary cooling and the rapid cooling is not more than 10 seconds, and the cooling rate of the secondary cooling is 5 to 20°C / s; The method according to claim 3 .
5. The rapid cooling is performed using a rapid cooling roll, Preferably, the secondary cooling is performed using any one of a cold inert gas spray, a water-cooled disk, or other type of cooling device; Preferably, the cooling rate of the secondary cooling is preferably 5 to 20 ° C / s, Preferably, the thickness of the alloy sheet is 0.15 to 0.45 mm. The method according to claim 3 or 4.
6. The (b) milling step includes coarse grinding and fine grinding, Preferably, the coarse grinding is selected from hydrogrinding and / or medium grinding, Preferably, the pulverization is performed by a jet mill, preferably, the jet mill is performed in an inert gas atmosphere, preferably, the inert gas is selected from nitrogen gas, helium gas, etc.; Preferably, after said milling, also obtained by screening, such as grading wheel screening, Preferably, the grain size SMD of the alloy powder is between 2.0 and 3.4 μm and X90 / X10≦4.5; Preferably, a lubricant needs to be added during fine grinding, preferably both before and after the jet mill, and preferably the lubricant is selected from easily volatile organic solvents such as lipids or alcohols, and illustratively the amount of the lubricant added is 0.1 to 1 wt % of the total mass of the raw materials; Preferably, further mixing is required after adding the lubricant, and the mixing time is preferably 3 to 6 hours. Preferably, the (c) press molding step specifically includes press molding the alloy powder under the action of a magnetic field to obtain a billet, Preferably, before press molding, the material needs to be aligned and magnetized under a magnetic field strength of 2 T and then molded. Preferably, after press molding, a reverse magnetic field is applied to demagnetize the material, Preferably, the compacted billet can be further treated by cold isostatic pressing to further increase the billet density. The method according to any one of claims 3 to 5.
7. The (d) sintering step includes a first sintering, a first cooling, a second sintering, and a second cooling, Preferably, the sintering process is carried out in a vacuum atmosphere, and preferably, the degree of vacuum is 10-1 Pa or less when heating; Preferably, the sintering temperature of the first sintering is 1000 to 1050° C., and the warming time of the first sintering is 240 to 360 min. Preferably, the second sintering temperature is 30 to 70° C. higher than the first sintering temperature, preferably 1030 to 1100° C.; Preferably, the second sintering is performed for a period of 270 to 360 minutes. Preferably, the first and second cooling steps are both less than 200° C. Preferably, the sintering step further comprises an ageing treatment performed after the second cooling, Preferably, the aging treatment is selected from a primary aging treatment or a secondary aging treatment, Preferably, the conditions of the primary aging treatment are that the aging treatment temperature is between 500 and 700° C. and the heat retention time is between 240 and 420 min. Preferably, the secondary aging treatment includes: performing a first aging treatment by increasing the temperature to 800 to 950° C. and a heat-retention time of 180 to 300 min; and performing a second aging treatment by increasing the temperature to between 450 to 600° C. and a heat-retention time of 240 to 360 min after cooling to 150° C. or less; Preferably, after the sintering step, a diffusion treatment may be carried out. Preferably, the diffusion treatment includes applying a diffusion material to a magnet surface, and performing a vacuum high-temperature diffusion treatment, a diffusion cooling and a diffusion aging treatment; Preferably, the diffusion material is selected from pure metals of Dy and / or Tb or alloys such as hydrides, oxides, hydroxides, fluorides of Dy and / or Tb; Preferably, the diffusion treatment can be carried out by using a method such as vacuum deposition, magnetron sputtering, coating or embedding, Preferably, the temperature of the high-temperature diffusion is 850-950° C., and the time of the high-temperature diffusion is 10-30 h; Preferably, the diffusion cooling temperature is less than 100° C. Preferably, the temperature of the diffusion aging treatment is 450 to 600 ° C, and the time of the diffusion aging treatment is 4 to 8 h. The method according to any one of claims 3 to 6.
8. Application of the magnet according to claims 1 to 2 in the field of motors.
9. A motor comprising the magnet according to claim 1 or 2.
10. Preferably, the motor is applicable to new energy vehicles and energy-saving home appliances; Application of the motor according to claim 9.
Citation Information
Patent Citations
Neodymium-iron-boron permanent magnet and preparation method and application thereof
CN113223807A
Production method for r-t-b-based rear earth sintered magnetic alloy and production method for r-t-b-based rear earth sintered magnet
JP2016017203A
R-t-b-based permanent magnet
JP2019050284A
PROCESS FOR PRODUCING RFeB-BASED SINTERED MAGNET
WO2016111346A1
R-t-b sintered magnet