Composition for electrochromic element having light transmittance, high flexibility, and high moisture resistance, and method for manufacturing electrochromic member

The electrochromic element composition with a polymer resin, plasticizer, and electrochromic substances addresses electrolyte leakage issues, enhancing light transmittance and flexibility, suitable for diverse applications.

JP2024536986AActive Publication Date: 2024-10-10KOREA UNIV OF TECH & EDUCATION IND UNIV COOPERATION FOUND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024514129
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-14
Filing Date
2021-12-08
Publication Date
2024-10-10
Estimated Expiration
2041-12-08

AI Technical Summary

Technical Problem

Conventional electrochromic elements face issues with electrolyte leakage and require additional protective layers to prevent water vaporization, limiting their use in flexible displays.

Method used

A composition for electrochromic elements comprising a light-transmitting polymer resin, plasticizer, and electrochromic substances like diheptylviologen dihexafluorophosphate or ethylviologen dibis(trifluoromethanesulfonyl)imide, along with an ionic liquid, is used to enhance light transmittance, flexibility, and durability.

Benefits of technology

The composition achieves improved light transmittance, elasticity, and durability, enabling applications in various fields with a simple manufacturing method that reduces costs and increases production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536986000001_ABST
    Figure 2024536986000001_ABST
Patent Text Reader

Abstract

The present invention relates to a composition for an electrochromic element having improved light transmittance and elasticity, and a method for producing an electrochromic member. The composition for an electrochromic device according to an embodiment of the present invention includes a light-transmitting polymer resin, a plasticizer, and an electrochromic material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for an electrochromic element having optical transparency, high flexibility, and high moisture resistance, and a method for producing an electrochromic member. [Background technology]

[0002] The electrochromic element contains an electrochromic material and changes color depending on the voltage applied from the outside. Various materials such as polymer compounds and metal oxides are used for the electrochromic material, and the color changes reversibly depending on the voltage applied to the electrodes.

[0003] Recently, the application of such color-changing elements has been expanding, for example, to smart window systems that block outside views and sunlight, and to automotive glass that displays information such as maps and text.

[0004] Conventional electrochromic devices use liquid electrochromic materials, which causes electrolyte leakage, limiting their use as flexible displays.

[0005] Recently, a solidified water-based electrolyte has been developed, but this requires the addition of a protective layer to prevent the water from easily evaporating. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Korean Patent No. 10-2078481 Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a composition for an electrochromic element and a method for producing an electrochromic member having improved light transmittance and elasticity.

[0008] It also has a long life and excellent durability.

[0009] In addition, the flexibility and stretchability of the material make it applicable to a variety of fields.

[0010] Furthermore, the manufacturing method is simple, which makes it possible to increase production efficiency and reduce manufacturing costs. [Means for solving the problem]

[0011] The composition for an electrochromic device according to an embodiment of the present invention includes a light-transmitting polymer resin, a plasticizer, and an electrochromic material.

[0012] The electrochromic material may be diheptyl viologen dihexafluorophosphate, and the content of the electrochromic material may be 5 to 20 parts by weight based on 100 parts by weight of the polymer resin.

[0013] The electrochromic material may be represented by the following Chemical Formula 1.

[0014] [ka]

[0015] The composition may further include an ionic liquid having a content of 100 to 200 parts by weight based on 100 parts by weight of the polymer resin.

[0016] The electrochromic material may be ethyl viologen dibis(trifluoromethanesulfonyl)imide, and the content of the electrochromic material may be 5 to 14 parts by weight based on 100 parts by weight of the polymer resin.

[0017] The ethyl viologen dibis(trifluoromethanesulfonyl)imide can be represented by the following Chemical Formula 2.

[0018] [ka]

[0019] The electrochromic element according to an embodiment of the present invention includes a first electrode, a second electrode, and an electrochromic element layer that changes color in response to a voltage applied between the first electrode and the second electrode, and the electrochromic element layer includes the composition for electrochromic elements described above.

[0020] A method for manufacturing an electrochromic member according to an embodiment of the present invention includes the steps of dissolving a polymer resin, a plasticizer, an ionic liquid, and an electrochromic material in a solvent to prepare a mixed solution, and removing the solvent from the mixed solution.

[0021] The electrochromic substance may be diheptyl viologen dihexafluorophosphate, and a method for preparing the electrochromic substance may include preparing a solution of 1,1'-diheptyl-4,4'-bipyridinium dibromide in a solvent, and adding NH4PF6 to the solution.

[0022] The electrochromic material may be ethyl viologen dibis(trifluoromethanesulfonyl)imide, and a method for preparing the electrochromic material may include preparing a solution of ethyl viologen dibromide in a solvent, and adding lithium bis(trifluoromethanesulfonyl)imide to the solution. Effect of the Invention

[0023] The composition for electrochromic element and the method for manufacturing an electrochromic member according to the embodiments of the present invention may have improved light transmittance and elasticity.

[0024] It also has a long life and excellent durability.

[0025] In addition, the flexibility and stretchability of the material make it applicable to a variety of fields.

[0026] Furthermore, the manufacturing method is simple, which makes it possible to increase production efficiency and reduce manufacturing costs. [Brief description of the drawings]

[0027] [Figure 1] FIG. 13 shows the results of cyclic voltammetry measurements when the electrochromic substances are DHV[PF6]2, DBV[PF6]2, and DEV[PF6]2. [Diagram 2] FIG. 13 is a diagram showing the measurement results of light absorptance when the electrochromic materials are DHV[PF6]2, DBV[PF6]2, and DEV[PF6]2. [Diagram 3] The photographs show the degree of color development depending on the electric potential when the electrochromic materials are DHV[PF6]2, DBV[PF6]2, and DEV[PF6]2. [Figure 4] FIG. 13 is a diagram showing experimental results of light transmittance when the electrochromic material is DHV[PF6]2, DBV[PF6]2, or DEV[PF6]2. [Diagram 5] FIG. 1 shows the optical density vs. charge density profile for electrochromic materials DHV[PF6]2, DBV[PF6]2, and DEV[PF6]2. [Figure 6] FIG. 1 shows the results of repeated coloring / bleaching cycle experiments when the electrochromic materials are DHV[PF6]2, DBV[PF6]2, and DEV[PF6]2. [Figure 7] FIG. 1 is a Nyquist diagram showing impedance experiment results when the electrochromic material is EV[TFSI]2. [Figure 8] FIG. 1 shows the tensile strength-strain measurements where the electrochromic material is EV[TFSI]2. [Figure 9] FIG. 1 shows the results of a compressive load test where the electrochromic material is EV[TFSI]2. [Figure 10] FIG. 1 shows the results of an evaporation test where the electrochromic material is EV[TFSI]2. [Figure 11] FIG. 1 shows the results of cyclic voltammetry measurements in which the electrochromic material is EV[TFSI]2. [Figure 12] FIG. 1 shows the measurement results of the light absorptance when the electrochromic material is EV[TFSI]2. [Figure 13] FIG. 13 shows the experimental results of light transmittance when the electrochromic material is EV[TFSI]2. [Figure 14] FIG. 1 shows optical density versus charge density profile where the electrochromic material is EV[TFSI]2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. However, the embodiments of the present invention may be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the relevant technical field. Therefore, the shapes and sizes of elements in the drawings may be exaggerated for clearer explanation, and elements represented by the same reference numerals in the drawings are the same elements. Furthermore, the same reference numerals are used throughout the drawings for parts having similar functions and actions. In addition, throughout the specification, "including" a certain element means that it may further include other elements, rather than excluding other elements, unless otherwise specified to the contrary.

[0029] Composition for electrochromic elements The composition for an electrochromic device according to an embodiment of the present invention includes a light-transmitting polymer resin, a plasticizer, and an electrochromic material.

[0030] The polymer resin forms a basic body from a composition for an electrochromic element. The polymer resin may have light transmittance, flexibility, and elasticity when cured with a plasticizer. To this end, the polymer resin may be at least one of polyvinyl chloride (PVC), polytetrafluoroethylene (PTFE), polyurethane (PU), polymethyl methacrylate (PMMA), polydimethylsiloxane (PDMS), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyethylene oxide (PEO), polyimide (PI), and polyethylene terephthalate (PET). In particular, the use of polyvinyl chloride (PVC) can provide high light transmittance, flexibility, and elasticity.

[0031] A plasticizer is a material that plasticizes a polymer resin. The plasticizer is not particularly limited, but may be DBA (dibutyl adipate). DBA may be represented by the following Chemical Formula 3.

[0032] [ka]

[0033] The content of the plasticizer may be 700 to 1200 parts by weight, preferably 800 to 1000 parts by weight, based on 100 parts by weight of the polymer resin. If the content of the plasticizer is too low, crystals may easily form in the manufactured color-changing element member, and if the content of the plasticizer is too high, mechanical properties may be reduced.

[0034] The electrochromic material is a material that changes the wavelength of absorption and color depending on the voltage applied from the outside. In the embodiment of the present invention, the electrochromic material may be preferably diheptyl viologen dihexafluorophosphate or ethyl viologen dibis(trifluoromethanesulfonyl)imide.

[0035] The diheptyl viologen dihexafluorophosphate is represented by DHV[PF6]2 and is represented by the following formula 4. The diheptyl viologen dihexafluorophosphate can realize a blue or cyan color when a voltage is applied. By limiting the electrochromic material in this way, it is possible to accurately realize a color by controlling the light transmittance according to the voltage while maintaining high light transmittance of the electrochromic element layer.

[0036] [ka]

[0037] The ethyl viologen dibis(trifluoromethanesulfonyl)imide is represented by EV[TFSI]2 and is represented by the following formula 5. The ethyl viologen dibis(trifluoromethanesulfonyl)imide can realize a blue or cyan color when a voltage is applied. By limiting the electrochromic material in this way, it is possible to accurately realize a color by controlling the light transmittance according to the voltage while maintaining high light transmittance of the electrochromic element layer.

[0038] [ka]

[0039] The content of the electrochromic material may be 5 to 20 parts by weight based on 100 parts by weight of the polymer resin. If the electrochromic material is diheptyl viologen dihexafluorophosphate, the content of the electrochromic material may be preferably 14 to 17 parts by weight.

[0040] When the electrochromic material is ethyl viologen dibis(trifluoromethanesulfonyl)imide, the content of the electrochromic material may be preferably 8 to 13.5 parts by weight, more preferably 11 to 13.5 parts by weight. If the content of the electrochromic material is too low, it is difficult to control the light transmittance, and the color may not be accurately realized, whereas if the content is too high, crystals are generated in the electrochromic layer, resulting in non-uniform color change.

[0041] In one embodiment, the composition for electrochromic device may further include an ionic liquid. Ionic liquids are generally substances that can improve the movement of ions and electrons while being maintained in a non-volatile liquid state at temperatures below 100° C. Various ionic liquids may be used, but preferably 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide (EMIM-TFSI) may be used. By limiting the ionic liquid in this way, the light transmittance of the electrochromic device layer may be kept high. The EMIM-TFSI may be represented by the following Chemical Formula 6.

[0042] [ka]

[0043] The content of the ionic liquid may be 100 to 200 parts by weight, preferably 150 to 170 parts by weight, based on 100 parts by weight of the polymer resin. If the content of the ionic liquid is too high, the light transmittance may decrease.

[0044] In an embodiment, the composition for an electrochromic device may further include an anode redox compound, which may be any one of ferrocene and dimethylferrocene, and is preferably dimethylferrocene. The dimethylferrocene may be represented by the following Formula 7:

[0045] [ka]

[0046] The content of the anode redox compound may be 1 to 5 parts by weight, preferably 1 to 7 parts by weight, based on 100 parts by weight of the polymer resin.

[0047] Electrochromic element The electrochromic element according to an embodiment of the present invention includes a first electrode, a second electrode, and an electrochromic element layer that changes color in response to a voltage applied between the first electrode and the second electrode, and the electrochromic element layer includes the composition for electrochromic elements described above.

[0048] The first and second electrodes are not particularly limited and may be made of materials commonly used in electrical devices, but may be made of ITO glass or ITO-PEN, etc., because they have optical transparency, flexibility, and stretchability.

[0049] The electrochromic element layer may include the composition for electrochromic element described above, and may be prepared in an appropriate size and thickness by the preparation method described below.

[0050] Manufacturing method of electrochromic member A method for manufacturing an electrochromic member according to an embodiment of the present invention includes the steps of dissolving a polymer resin, a plasticizer, an ionic liquid, and an electrochromic material in a solvent to prepare a mixed solution, and removing the solvent from the mixed solution.

[0051] The polymer resin, the plasticizer, and the ionic liquid mixed in the step of preparing the mixed solution are the same as those described above.

[0052] In this step, if the electrochromic material is diheptyl viologen dihexafluorophosphate, the method for preparing the electrochromic material may include preparing a solution of 1,1'-diheptyl-4,4'-bipyridinium dibromide in a solvent, and adding NH4PF6 to the solution. The 1,1'-diheptyl-4,4'-bipyridinium dibromide may be represented by DHV(Br)2.

[0053] The solvent is a liquid capable of dissolving 1,1'-diheptyl-4,4'-bipyridinium dibromide, preferably water. In this step, 1,1'-diheptyl-4,4'-bipyridinium dibromide is added to water and stirred to completely dissolve.

[0054] The step of adding NH4PF6 to the solution may be carried out by slowly dripping NH4PF6 onto the 1,1'-diheptyl-4,4'-bipyridinium dibromide solution.

[0055] Then, the reaction can be carried out at room temperature to produce DHV[PF6]2. Then, the solvent can be removed, washed and dried to finally produce DHV[PF6]2.

[0056] In this step, if the electrochromic material is ethyl viologen dibis(trifluoromethanesulfonyl)imide, the electrochromic material can be prepared by preparing a solution of ethyl viologen dibromide in a solvent, and adding lithium bis(trifluoromethanesulfonyl)imide to the solution. The ethyl viologen dibromide is represented by EV(Br)2 and is represented by the following formula 8.

[0057] [ka]

[0058] The solvent is a liquid capable of dissolving ethyl viologen dibromide, preferably water. In this step, ethyl viologen dibromide is added to water and stirred to completely dissolve.

[0059] The step of adding lithium bis(trifluoromethanesulfonyl)imide may be carried out by slowly dropping lithium bis(trifluoromethanesulfonyl)imide onto the ethyl viologen dibromide solution. The lithium bis(trifluoromethanesulfonyl)imide is represented by LiTFSI and is represented by the following formula 9:

[0060] [ka]

[0061] Then, the reaction can be carried out at room temperature to produce EV[TFSI]2, which can then be finally produced by removing the solvent, washing and drying.

[0062] In the step of preparing the mixed solution, the solvent used may be a polar organic solvent, which can easily dissolve polymer resins such as PVC. The polar organic solvent may be any one of dioxane, tetrahydrofuran (THF), acetone, dimethylsulfoxide (DMSO), dimethylformamide (DMF), and 1-methyl-2-pyrrolidone (NMP).

[0063] The content of the plasticizer added in this step may be 700 to 1200 parts by weight, the content of the ionic liquid may be 100 to 200 parts by weight, and the content of the electrochromic material may be 5 to 20 parts by weight, preferably 5 to 14 parts by weight, based on 100 parts by weight of the polymer resin. Also, an anode redox compound having a content of 1 to 7 parts by weight, preferably 1 to 5 parts by weight, based on 100 parts by weight of the polymer resin may be further added.

[0064] After this step, a step of removing the solvent is performed. This step can be performed by leaving the solution in which various materials are mixed at room temperature for a long period of time, or using a dryer if necessary. This step can also be performed on a film or mold to produce a desired shape and thickness.

[0065] Manufacturing example: Electrochromic material DHV[PF 6 ] 2 , DBV[PF 6 ] 2 , DEV[PF 6 ] 2 Manufacturing To prepare the electrochromic material DHV[PF6]2, 0.2g of DHV(Br)2 manufactured by TCI was dissolved in 40ml of water, and then 0.19g of NH4PF6 was dissolved in another 40ml of water. Next, the aqueous solution of NH4PF6 was added dropwise to the aqueous solution of DHV(Br)2. The mixed solution was then left at 25°C for 24 hours to produce DHV[PF6]2. The mixed solution was filtered under reduced pressure, washed with distilled water, and then dried in a vacuum oven at 80°C for 24 hours.

[0066] To prepare the electrochromic material DBV[PF6]2, 0.2 g of DBV(Br)2 (benzyl viologen dichloride) manufactured by Alfa Aeser was dissolved in 40 ml of water, and 0.2389 g of NH4PF6 was added dropwise to the solution so that the molar ratio of DBV(Br)2 to NH4PF6 was 1:3. The mixed solution was then left at 25°C for 24 hours to produce DBV[PF6]2. The mixed solution was filtered under reduced pressure, washed with distilled water, and then dried at 80°C for 24 hours in a vacuum oven.

[0067] To prepare the electrochromic material DEV[PF6]2, 0.2 g of DEV(Br)2 (1,1'-diethyl-4,4'-bipyridinium dibromide) was dissolved in 40 ml of water, and 0.34 g of NH4PF6 was added dropwise to the solution. The mixture was then left at 25°C for 24 hours to produce DEV[PF6]2. The mixture was filtered under reduced pressure, washed with distilled water, and then dried at 80°C for 24 hours in a vacuum oven.

[0068] Manufacturing example: Electrochromic material EV [TFSI] 2 Manufacturing 0.2 g of EV(Br)2 was dissolved in 40 ml of water, and 0.34 g of LiTFSI was dissolved in another 40 ml of water. The solution containing LiTFSI was added dropwise to the solution containing EV(Br)2 so that the molar ratio of EV(Br)2 to LiTFSI was 1:3. The mixed solution was then left at 25°C for 24 hours to produce EV[TFSI]2. The mixed solution was filtered under reduced pressure, washed with distilled water, and then dried at 80°C for 24 hours in a vacuum oven.

[0069] Manufacturing example: DHV[PF 6 ] 2 , DBV[PF 6 ] 2 , DEV[PF 6 ] 2 Manufacturing electrochromic materials using Example 1 0.3424g of PVC (Scientific Polymer Products) as a polymer resin, 3.0816g of DBA (TCI) as a plasticizer, 0.5478g of EMIMTFSI (io-li-tec) as an ionic liquid, 0.0333g of DHV[PF6]2 (previously prepared) as an electrochromic material, and 0.0111g of dimethylferrocene (TCI) as an anode redox compound were mixed in THF as a solvent. Next, the mixed solution was poured into a glass dish and dried by evaporating the solvent at room temperature for 3 days.

[0070] Example 2 The same procedure as in Example 1 was repeated except that 0.0416 g of DHV[PF6]2 and 0.0138 g of dimethylferrocene were used.

[0071] Example 3 The same procedure as in Example 1 was repeated except that 0.0499 g of DHV[PF6]2 and 0.0166 g of dimethylferrocene were used.

[0072] Example 4 The same procedure as in Example 1 was repeated except that 0.0583 g of DHV[PF6]2 and 0.0194 g of dimethylferrocene were used.

[0073] Comparative Example 1 The same procedure as in Example 1 was carried out to prepare the product, except that 0.0325 g of DBV[PF6]2 (previously prepared) and 0.0111 g of dimethylferrocene were used instead of DHV[PF6]2.

[0074] Comparative Example 2 The same procedure as in Example 2 was carried out to prepare the product, except that 0.0406 g of DBV[PF6]2 (previously prepared) and 0.0138 g of dimethylferrocene were used instead of DHV[PF6]2.

[0075] Comparative Example 3 The same procedure as in Example 1 was carried out to prepare the product, except that 0.0487 g of DBV[PF6]2 (previously prepared) and 0.0166 g of dimethylferrocene were used instead of DHV[PF6]2 in Example 3.

[0076] Comparative Example 4 The same procedure as in Example 1 was carried out to prepare the product, except that 0.0130 g of DEV[PF6]2 (previously prepared) and 0.0055 g of dimethylferrocene were used instead of DHV[PF6]2.

[0077] Comparative Example 5 The same procedure as in Comparative Example 4 was repeated except that 0.0196 g of DEV[PF6]2 and 0.008 g of dimethylferrocene were used.

[0078] Comparative Example 6 The same procedure as in Comparative Example 4 was repeated except that 0.0261 g of DEV[PF6]2 and 0.0111 g of dimethylferrocene were used.

[0079] Manufacturing example: EV[TFSI] 2 Manufacturing of electrochromic elements using Example 5 0.3424g of PVC (Scientific Polymer Products) as a polymer resin, 3.0816g of DBA (TCI) as a plasticizer, 0.5478g of EMIMTFSI (io-li-tec) as an ionic liquid, 0.02g of EV[TFSI]2 (previously prepared) as an electrochromic material, and 0.0055g of dimethylferrocene (TCI) as an anode redox compound were mixed in 25ml of THF as a solvent. Next, the mixed solution was poured into a glass dish and dried by evaporating the solvent at room temperature for 3 days.

[0080] Example 6 The same procedure as in Example 1 was repeated except that 0.03 g of EV[TFSI]2 and 0.0083 g of dimethylferrocene were used.

[0081] Example 7 The same procedure as in Example 1 was repeated except that 0.04 g of EV[TFSI]2 and 0.0111 g of dimethylferrocene were used.

[0082] Example 8 The same procedure as in Example 1 was repeated except that 0.045 g of EV[TFSI]2 and 0.01244 g of dimethylferrocene were used.

[0083] Comparative Example 7 The same procedure as in Example 1 was repeated except that 0.050 g of EV[TFSI]2 and 0.01383 g of dimethylferrocene were used.

[0084] Comparative Example 8 The preparation was carried out in the same manner as in Example 1, except that EV[TFSI]2 was not added.

[0085] Manufacturing example: Manufacturing of electrochromic elements The electrochromic member prepared above was placed on ITO glass, and a spacer having a thickness of 100 μm was placed on the edge of the electrochromic member, and then the top was covered with another ITO glass. The electrochromic elements thus prepared were defined as Examples D1 to D4 corresponding to Examples 1 to 4, Examples E5 to E8 corresponding to Examples 5 to 8, Comparative Examples D1 to D6 corresponding to Comparative Examples 1 to 6, and Comparative Examples E7 and E8 corresponding to Comparative Examples 7 and 8.

[0086] Experimental example: Visual inspection Examples 1 to 8 and Comparative Examples 1 to 8 were visually inspected to check for any abnormalities. In the cases of Comparative Examples 3, 6, and 7, it was confirmed that crystals had formed inside.

[0087] Experimental Example: Cyclic Voltammetry Measurement (1) 20mVs using a potential tester (biologics, SP240) -1Current / potential curves were obtained by cyclic voltammetry for Examples D1 to D4 and Comparative Examples D1 to D6 under the above conditions. Figure 1 shows the results of this experiment. Referring to Figure 1, it can be seen that the changes in current are clearer in Examples D1 to D4 than in the Comparative Examples, and particularly clearer in Examples D3 and D4.

[0088] Experimental example: Measuring light absorption rate For Example D4, Comparative Example D2, and Comparative Example D5, a UV-Vis Spectrometer (Perkin Elmer, Lambda 465) was used to measure in the range of 400 to 800 nm. FIG. 2(a) shows the experimental results of Example D4, FIG. 2(b) shows the experimental results of Comparative Example D2, and FIG. 2(c) shows the experimental results of Comparative Example D5. Referring to FIG. 2, it can be seen that in the case of Example D4, the absorptance at a wavelength of 606 nm is the highest, and the light absorptance is adjusted depending on the applied voltage. In the case of the comparative example, the light absorptance is higher around 606 nm than other wavelengths, but the difference in absorption amount is not as large as in the examples.

[0089] Experimental example: Color expression experiment A voltage of 0V to -1.4V was applied to Example D4, Comparative Example D2, and Comparative Example D5, and the change in hue was observed. Figure 3 shows the results of this experiment. Referring to Figure 3, in the case of Example D4, the control of the hue depending on the applied voltage was the most obvious, and it was a darker blue color than the comparative examples.

[0090] Experimental example: Light transmittance experiment (1) The degree of transmission of light with a wavelength of 606 nm was measured for Examples D1 to D4 and Comparative Examples D1 to D6. In this case, the change in light transmittance was observed while coloring and bleaching were performed by applying and cutting off a voltage. Figure 4 shows the results of this experiment. Referring to Figure 4, the Examples showed a larger change in light transmittance than the Comparative Examples, and among the Examples, Examples D3 and D4 showed a larger change in light transmittance than the other Examples.

[0091] Experimental Example: Optical Density vs. Charge Density Analysis (1) The relationship between optical density and charge density was analyzed for Examples D1 to D4 and Comparative Examples D1 to D6 under conditions of 606 nm and -1.0 V to determine the coloring efficiency (η). Figure 8 shows the results of this experiment. Referring to Figure 5, it can be seen that the Examples have a higher coloring efficiency (η) than the Comparative Examples, and in particular, Examples 6 to 8 have a larger increase in coloring efficiency (η), but among the Examples, Examples D3 to D4 have the higher efficiency.

[0092] Experimental example: Light transmittance experiment using repeated coloring and bleaching cycles Voltage was repeatedly applied to Example D4 and Comparative Examples D2 and D5 to repeat coloring and bleaching, and the degree of transmission of light with a wavelength of 606 nm was measured for 40,000 seconds. At this time, the change in light transmittance was observed while coloring and bleaching were performed by applying and cutting off the voltage. Figure 6 shows the results of this experiment, where (a) is the result of Example D4, (b) is the result of Comparative Example D2, and (c) is the result of Comparative Example D5. Referring to Figure 6, it can be seen that the light transmittance of Example D4 remained constant during the cycle period, but the light transmittance of Comparative Examples D2 and D5 decreased.

[0093] Experimental example: Measurement of impedance characteristics The electrochromic members prepared in Examples 5 to 8 and Comparative Example 8 were placed between platinum electrodes, and impedance spectra were measured using an impedance spectrometer. Figure 7 is a Nyquist diagram showing the results of this experiment. Referring to Figure 7, it can be seen that there is no significant difference in characteristics between Example 5 and Comparative Example 8, and that the characteristics of Example 8 are improved compared to Comparative Example 8.

[0094] Experimental example: Tensile strength-strain measurement Measurements were performed on Examples 5 to 8 and Comparative Example 8 using a universal testing machine (UTM, Tinius Olsen, H5KT) in accordance with ASTM D638 type V. Figure 8 shows the experimental results. Referring to Figure 8, it can be seen that the Examples have significantly higher tensile strength than Comparative Example 8, and in particular, Examples 6 to 8 are even more excellent.

[0095] Experimental example: Compression load test Examples 5 to 8 and Comparative Example 8 were cut to a thickness of 3 mm and a width and length of 10 mm, and were subjected to compression at a speed of 10 mm / min using a compression load tester. Figure 9 shows the results of this experiment. Referring to Figure 9, it can be seen that the Examples have superior compression characteristics compared to Comparative Example 8.

[0096] Experimental example: Evaporation test Examples 5 to 8 and Comparative Example 8 were cut to a certain size, and the weights of the corresponding samples were measured while maintaining them at room temperature for 30 days under conditions of 20 to 27°C and 19 to 40% RH. Figure 10 shows the results of this experiment. Referring to Figure 10, it can be seen that there was no change in weight even when the content of the electrochromic material increased.

[0097] Experimental Example: Cyclic Voltammetry Measurement (2) 20mVs using a potential tester (biologics, SP240) -1 Current / potential curves were obtained by cyclic voltammetry for Examples E5 to E8 under the conditions shown in Figure 11. The experimental results are shown in Figure 11. It can be seen that the higher the content of the electrochromic material, the clearer the change in current.

[0098] Experimental example: Measuring light absorption rate For Example E8, a UV-Vis Spectrometer (Perkin Elmer, Lambda 465) was used to measure in the range of 400 to 800 nm. Figure 12 shows the results of this experiment. Referring to Figure 12, it can be seen that the absorptance is highest for a wavelength of 606 nm, and that the light absorptance is adjusted depending on the applied voltage.

[0099] Experimental example: Light transmittance experiment (2) The degree of transmission of light with a wavelength of 606 nm was measured for Examples E5 to E8. In this case, the change in light transmittance was observed while coloring and bleaching were performed by applying and cutting off a voltage. Figure 13 shows the results of this experiment. Referring to Figure 13, it can be seen that the higher the content of the electrochromic material, the greater the change in light transmittance, and in particular, the change in light transmittance of Examples E7 and E8 was very excellent.

[0100] Experimental Example: Optical Density vs. Charge Density Analysis (2) The relationship between optical density and charge density was analyzed for Examples E5 to E8 at 606 nm and -1.0 V to determine the coloring efficiency (η). Figure 14 shows the results of this experiment. Referring to Figure 14, it can be seen that the higher the content of the electrochromic material, the higher the coloring efficiency (η), and the increase in coloring efficiency (η) is particularly noticeable in Examples E6 to E8.

[0101] The present invention is not limited by the above-described embodiments and the accompanying drawings, but is limited by the appended claims. Therefore, various substitutions, modifications, and changes can be made by a person skilled in the art without departing from the technical spirit of the present invention as set forth in the claims, and such modifications and changes are also within the scope of the present invention.

Claims

1. A light-transmitting polymer resin; A plasticizer; and an electrochromic substance.

2. 2. The composition for an electrochromic device according to claim 1, wherein the electrochromic material is diheptyl viologen dihexafluorophosphate, and the content of the electrochromic material is 5 to 20 parts by weight based on 100 parts by weight of the polymer resin.

3. The electrochromic material is represented by the following formula 1: 【Chemistry 1】 The composition for electrochromic devices according to claim 1 .

4. 2. The composition for electrochromic device according to claim 1, wherein the electrochromic material is ethyl viologen dibis(trifluoromethanesulfonyl)imide, and the content of the electrochromic material is 5 to 14 parts by weight based on 100 parts by weight of the polymer resin.

5. The electrochromic material is represented by the following formula 2: 【Chemistry 2】 The composition for electrochromic devices according to claim 1 .

6. 2. The composition for an electrochromic device according to claim 1, further comprising an ionic liquid having a content of 100 to 200 parts by weight based on 100 parts by weight of the polymer resin.

7. 2. The composition for an electrochromic device according to claim 1, further comprising an anode redox compound in an amount of 1 to 7 parts by weight based on 100 parts by weight of the polymer resin.

8. A first electrode; A second electrode; An electrochromic element comprising: an electrochromic element layer that changes color in response to a voltage applied by the first electrode and the second electrode, the electrochromic element layer comprising the composition for electrochromic elements according to claim 1 .

9. dissolving a polymer resin, a plasticizer, an ionic liquid, and an electrochromic material in a solvent to prepare a mixed solution; and removing the solvent from the mixed solution.

10. The electrochromic material is diheptyl viologen dihexafluorophosphate, and the electrochromic material is prepared by the following method: preparing a solution of 1,1'-diheptyl-4,4'-bipyridinium dibromide in a solvent; and The solution was diluted with NH 4 P.F. 6 and a step of adding:

11. The electrochromic material is ethyl viologen dibis(trifluoromethanesulfonyl)imide, and the electrochromic material is prepared by the following method: preparing a solution of ethyl viologen dibromide in a solvent; and and adding lithium bis(trifluoromethanesulfonyl)imide to the solution.

12. In the step of preparing the mixed solution, The content of the plasticizer is 700 to 1200 parts by weight based on 100 parts by weight of the polymer resin, The content of the ionic liquid is 100 to 200 parts by weight, 10. The method of claim 9, wherein the content of the electrochromic material is 5 to 20 parts by weight based on 100 parts by weight of the polymer resin.

13. In the step of preparing the mixed solution, 10. The method of claim 9, further comprising adding an anode redox compound having a content of 1 to 7 parts by weight based on 100 parts by weight of the polymer resin.

Citation Information

Patent Citations

  • Viologen-based electrochromic compositions which can be formulated and applied at room temperature

    US20110003070A1

  • Thermoplastic electrochromic materials

    US20110147680A1

  • Electrochromic devices, and method for manufacturing the same

    KR102078481B1