Polyimide film containing graphene nanoplates and method for producing same

A polyimide film with optimized dianhydrides and diamines, combined with graphene nanoplatelets, addresses the dielectric inefficiencies of conventional films, providing superior insulation and moisture resistance for high-frequency communication.

JP2024537041AActive Publication Date: 2024-10-10PI ADVANCED MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024519123
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-29
Publication Date
2024-10-10
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

Conventional polyimide films exhibit inadequate dielectric properties, particularly high dielectric constants and dielectric loss factors, which hinder high-frequency, high-speed communication in flexible thin circuit boards, and are susceptible to moisture-induced degradation.

Method used

A polyimide film composition incorporating specific dianhydrides (BTDA, BPDA, PMDA) and diamines (m-tolidine, PPD) with graphene nanoplatelets, optimized for a specific content ratio and properties, to achieve a dielectric constant of 4.0 to 7.0 and a dielectric loss factor of 0.01 or less.

Benefits of technology

The resulting polyimide film maintains excellent dielectric properties, ensuring insulation and minimizing signal transmission delay even at high frequencies, while resisting moisture absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537041000001
    Figure 2024537041000001
  • Figure 2024537041000002
    Figure 2024537041000002
  • Figure 2024537041000003
    Figure 2024537041000003
Patent Text Reader

Abstract

The present invention provides a polyimide film containing 0.5 to 2.5 wt % of graphene nanoplatelets, which is obtained by subjecting a polyamic acid solution containing a dianhydride component including benzophenonetetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride (BPDA), and pyromellitic dianhydride (PMDA) and a diamine component including m-tolidine and paraphenylenediamine (PPD) to an imidization reaction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyimide film containing graphene nanoplates and having excellent dielectric properties, and a method for producing the same. [Background technology]

[0002] Polyimide (PI) is a polymeric material based on imide rings, which have extremely excellent chemical stability along with a rigid aromatic main chain, and has the highest levels of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials.

[0003] In particular, due to its excellent electrical properties such as excellent insulating properties, i.e., low dielectric constant, it has been in the spotlight as a highly functional polymer material in the electrical, electronic and optical fields. 2. Description of the Related Art Recently, as electronic products become lighter and smaller, highly integrated and flexible thin circuit boards have been actively developed. Such thin circuit boards tend to have a structure in which a circuit containing metal foil is formed on a polyimide film, which has excellent heat resistance, low temperature resistance and insulating properties and is easily flexible. Flexible metal clad laminates are mainly used for such thin circuit boards, and an example is Flexible Copper Clad Laminate (FCCL), which uses a thin copper plate as the metal foil. Polyimide is also sometimes used as a protective film or insulating film for thin circuit boards.

[0004] Meanwhile, as electronic devices are increasingly being equipped with a variety of functions, there is a demand for faster computing and communication speeds. To meet this demand, thin circuit boards capable of high-speed communication at high frequencies have been developed. To realize high-frequency and high-speed communication, insulators with high impedance that can maintain electrical insulation even at high frequencies are required. Since impedance is inversely proportional to the frequency and dielectric constant (Dk) formed in the insulator, the dielectric constant must be as low as possible to maintain insulation even at high frequencies. However, in the case of ordinary polyimide, the dielectric properties are not excellent enough to maintain sufficient insulation for high frequency communication. In addition, the lower the dielectric properties of the insulator, the less undesirable stray capacitance and noise can be generated in thin circuit boards, and the greater the likelihood of communication delays being eliminated. Therefore, the low dielectric properties of polyimide are recognized as the most important factor in the performance of thin circuit boards.

[0005] In particular, in the case of high frequency communication, dielectric loss through polyimide is inevitable. The dielectric dissipation factor (Df) refers to the degree of electrical energy loss in a thin circuit board and is closely related to the signal transmission delay that determines the communication speed. Therefore, keeping the dielectric dissipation factor of polyimide as low as possible is recognized as an important factor for the performance of thin circuit boards. In addition, the more moisture a polyimide film contains, the larger its dielectric constant becomes, and the higher its dielectric loss factor becomes. Although polyimide film is suitable as a material for thin circuit boards due to its excellent inherent properties, it is relatively vulnerable to moisture due to its polar imide group, which can cause a deterioration in its insulating properties. Therefore, there is a need to develop a polyimide film with dielectric properties that maintains the mechanical properties specific to polyimide at a certain level. Recently, as transmission speeds have become faster, a method of absorbing energy by attaching a terminator to the end of the circuit has been applied to solve the problem of reflected signals disturbing the rising time part and hindering semiconductor operation. To apply this absorption method, the impedance of the terminator and the impedance of the transmission circuit must be the same. At this time, since the impedance value of the terminator resistor is fixed, it is necessary to adjust the impedance of the circuit on the printed circuit board (PCB). In other words, as the trend toward miniaturization of electronic devices leads to thinner insulation thickness and therefore lower impedance, the dielectric constant must be made higher than that of conventional polyimide films (Dk: 3.5) to match the impedance value of the prescribed terminator resistor. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Korean Patent Publication No. 10-2015-0069318 Summary of the Invention [Problem to be solved by the invention]

[0007] In order to solve the above problems, an object of the present invention is to provide a polyimide film having excellent dielectric properties and a method for producing the same. Therefore, a substantial object of the present invention is to provide specific embodiments thereof. [Means for solving the problem]

[0008] To achieve the above object, one embodiment of the present invention provides a polyimide film containing 0.5 to 2.5 wt % graphene nanoplatelets, which is obtained by imidizing a polyamic acid solution containing a dianhydride component including benzophenonetetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride (BPDA), and pyromellitic dianhydride (PMDA) and a diamine component including m-tolidine and paraphenylenediamine (PPD).

[0009] Based on 100 mol % of the total content of the diamine components, the content of m-tolidine may be from 20 mol % to 40 mol % and the content of paraphenylenediamine may be from 60 mol % to 80 mol %.

[0010] In addition, based on 100 mol% of the total content of the dianhydride acid components, the content of benzophenone tetracarboxylic dianhydride may be 20 mol% or more and 45 mol% or less, the content of biphenyl tetracarboxylic dianhydride may be 20 mol% or more and 45 mol% or less, and the content of pyromellitic dianhydride may be 20 mol% or more and 45 mol% or less.

[0011] The graphene nanoplates have an average thickness of 6 to 8 nm, an average particle size of 5 to 25 μm, and a specific surface area of ​​120 to 150 m. 2 / g.

[0012] Meanwhile, the polyimide film may have a dielectric constant of 4.0 or more and 7.0 or less, and a dielectric loss factor of 0.01 or less.

[0013] Another embodiment of the present invention is a method for producing a benzophenone tetracarboxylic dianhydride comprising the steps of: The present invention provides a method for producing a polyimide film, the method including: (a) polymerizing a dianhydride component including biphenyltetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride (BPDA), and pyromellitic dianhydride (PMDA) with a diamine component including m-tolidine and paraphenylenediamine (PPD) in an organic solvent to produce a polyamic acid; (b) adding graphene nanoplates to the polyamic acid and mixing them; and (c) imidizing the polyamic acid including the graphene nanoplates.

[0014] Yet another embodiment of the present invention provides a multilayer film including the polyimide film, a flexible metal foil laminate including the polyimide film and an electrically conductive metal foil, and an electronic device including the flexible metal foil laminate. Effect of the Invention

[0015] As described above, the present invention provides a polyimide film having excellent dielectric properties through a polyimide film having specific components and a specific composition ratio and a manufacturing method thereof, and the polyimide film can be usefully applied to various fields requiring such properties, particularly electronic parts such as flexible metal foil laminates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the embodiments of the present invention will be described in more detail in the order of "polyimide film" and "method for producing polyimide film" according to the present invention.

[0017] Prior to this, the terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that is consistent with the technical idea of ​​the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to explain his / her invention in the best possible manner. Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not fully represent the technical ideas of the present invention, and therefore various equivalents and modifications that can replace them may exist at the time of this application.

[0018] In this specification, the singular includes the plural unless the context clearly dictates otherwise. In this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.

[0019] When an amount, concentration, or other value or parameter is given herein as a range, a preferred range, or a list of upper preferred values ​​and lower preferred values, it should be understood that this specifically discloses all ranges formed by any pair of any upper range value or preferred value and any lower range value or preferred value, whether or not a range is otherwise disclosed. Where a range of numerical values ​​is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited by the specific values ​​recited when defining a range.

[0020] As used herein, "dianhydride" is intended to include precursors or derivatives thereof, which may not technically be dianhydrides, but which nevertheless react with diamines to form polyamic acids, which can then be converted back to polyimides. can be done.

[0021] As used herein, "diamine" is intended to include precursors or derivatives thereof, which may not technically be diamines, but which nevertheless react with dianhydrides to form polyamic acids, which can be converted back to polyimides.

[0022] In this specification, when a numerical range is indicated as "a to b" or "a~b," "to" and "~" are defined as ≧a and ≦b.

[0023] The polyimide film according to the present invention is obtained by imidizing a polyamic acid solution containing a dianhydride component including benzophenonetetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) and a diamine component including m-tolidine and paraphenylenediamine (PPD), and may contain 0.5 to 2.5 wt % of graphene nanoplatelets.

[0024] Based on 100 mol % of the total content of the diamine components, the content of m-tolidine may be from 20 mol % to 40 mol % and the content of paraphenylenediamine may be from 60 mol % to 80 mol %. In particular, m-tolidine has a methyl group that is particularly hydrophobic, and contributes to the low moisture absorption properties of the polyimide film.

[0025] Based on 100 mol% of the total content of the dianhydride acid components, the content of benzophenone tetracarboxylic dianhydride may be 20 mol% or more and 45 mol% or less, the content of biphenyl tetracarboxylic dianhydride may be 20 mol% or more and 45 mol% or less, and the content of pyromellitic dianhydride may be 20 mol% or more and 45 mol% or less.

[0026] The polyimide chain derived from the biphenyltetracarboxylic dianhydride of the present invention has a structure named charge transfer complex (CTC), i.e., a regular linear structure in which the electron donor and the electron acceptor are located close to each other, thereby enhancing the intermolecular interaction. In addition, benzophenone tetracarboxylic dianhydride, which has a carbonyl group, also contributes to the expression of CTCs, similar to biphenyl tetracarboxylic dianhydride. This structure has the effect of preventing hydrogen bonding with moisture, which has an effect of lowering the moisture absorption rate, thereby maximizing the effect of lowering the moisture absorption of the polyimide film.

[0027] In one specific example, the dianhydride acid component may further include a pyromellitic dianhydride, which is a dianhydride acid component having a relatively rigid structure and is preferred in that it can impart appropriate elasticity to the polyimide film. In order for the polyimide film to simultaneously satisfy the appropriate elasticity and moisture absorption rate, the content ratio of the dianhydride is particularly important. For example, as the content ratio of biphenyltetracarboxylic dianhydride decreases, it becomes difficult to expect a low moisture absorption rate due to the CTC structure.

[0028] In addition, biphenyltetracarboxylic dianhydride and benzophenonetetracarboxylic dianhydride contain two benzene rings that correspond to the aromatic moiety, whereas pyromelitic dianhydride contains one benzene ring that corresponds to the aromatic moiety.

[0029] In the dianhydride acid component, an increase in the pyromellitic dianhydride content can be understood as an increase in the imide groups in the molecule when the same molecular weight is used as a standard, and this can be understood as an increase in the proportion of imide groups originating from the pyromellitic dianhydride in the polyimide polymer chain relative to the imide groups originating from biphenyltetracarboxylic dianhydride and benzophenonetetracarboxylic dianhydride. In other words, an increase in the pyromellitic dianhydride content can be regarded as a relative increase in imide groups with respect to the entire polyimide film, which makes it difficult to expect a low moisture absorption rate. Conversely, if the content ratio of the pyromellitic dianhydride is decreased, the components having a relatively rigid structure are decreased, and the elasticity of the polyimide film may decrease below a desired level.

[0030] For this reason, if the content of the biphenyltetracarboxylic dianhydride and the benzophenonetetracarboxylic dianhydride exceeds the above range, or the content of the pyromellitic dianhydride is below the above range, the mechanical properties of the polyimide film are deteriorated, and it is not possible to ensure a level of heat resistance appropriate for producing a flexible metal foil laminate. Conversely, if the content of the biphenyltetracarboxylic dianhydride and the benzophenonetetracarboxylic dianhydride is below the above range, or the content of the pyromellitic dianhydride is above the above range, it is difficult to achieve appropriate levels of dielectric constant, dielectric loss factor and moisture absorption rate, which is not preferable.

[0031] Meanwhile, the graphene nanoplates have an average thickness of 6 to 8 nm, an average particle size of 5 to 25 μm, and a specific surface area of ​​120 to 150 m. 2 / g. The graphene nanoplates have relatively excellent dispersibility compared to other carbon nano materials, and when added to a polyimide film, the graphene nanoplates can minimize the decrease in the dielectric loss factor of the polyimide film.

[0032] In an embodiment, the polyimide film may have a dielectric constant of 4.0 to 7.0 and a dielectric loss factor of 0.01 or less. The dielectric constant may preferably be 4.5 or more, and more preferably 5.0 or more.

[0033] In this regard, polyimide films that satisfy both the dielectric constant (Dk) and dielectric loss factor (Df) can be used as insulating films for flexible metal foil laminates. Even if the manufactured flexible metal foil laminates are used as electrical signal transmission circuits that transmit signals at high frequencies of 10 GHz or more, the insulation safety can be ensured and signal transmission delay can be minimized.

[0034] In the present invention, the polyamic acid can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the dianhydride component to polymerize the mixture; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and then the remaining dianhydride component is added, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (4) A method in which a dianhydride component is placed in a solvent, a portion of a diamine compound is mixed in a ratio of 95 to 105 mol % relative to the reactive components, and then another dianhydride component is added, followed by the remaining diamine component, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (5) A method of forming a first composition by reacting a part of a diamine component and a part of a dianhydride acid component in a solvent so that one of them is in an excess amount, and forming a second composition by reacting a part of a diamine component and a part of a dianhydride acid component in another solvent so that one of them is in an excess amount, and then mixing the first and second compositions to complete polymerization, in which if the diamine component is in excess when the first composition is formed, the dianhydride acid component is in excess in the second composition, and if the dianhydride acid component is in excess in the first composition, the diamine component is in excess in the second composition, and the first and second compositions are mixed to polymerize so that the total amount of diamine components and dianhydride acid components used in these reactions are substantially equimolar.

[0035] However, the polymerization method is not limited to the above example, and it goes without saying that any known method can be used to produce the polyamic acid.

[0036] In one specific example, the method for producing a polyimide film according to the present invention includes: (a) preparing a polyamic acid by polymerizing a dianhydride component including benzophenone tetracarboxylic dianhydride (BTDA), biphenyl tetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) and a diamine component including m-tolidine and paraphenylenediamine (PPD) in an organic solvent; (b) adding and mixing graphene nanoplates into the polyamic acid; and (c) imidizing the polyamic acid including the graphene nanoplates.

[0037] Based on 100 mol% of the total content of the diamine components, the content of m-tolidine may be 20 mol% or more and 40 mol% or less, the content of paraphenylenediamine may be 60 mol% or more and 80 mol% or less, and based on 100 mol% of the total content of the dianhydride acid components, the content of benzophenone tetracarboxylic dianhydride may be 20 mol% or more and 45 mol% or less, the content of biphenyl tetracarboxylic dianhydride may be 20 mol% or more and 45 mol% or less, and the content of pyromellitic dianhydride may be 20 mol% or more and 45 mol% or less.

[0038] In the present invention, the polymerization method of the polyamic acid may be defined as a random polymerization method, and the polyimide film prepared from the polyamic acid of the present invention prepared in the above-mentioned process may be preferably used in terms of maximizing the effect of the present invention having excellent dielectric properties.

[0039] However, in the above polymerization method, the length of the repeating unit in the polymer chain is relatively short, so that there is a limit to the excellent properties of the polyimide chain derived from the dianhydride acid component. Therefore, the polymerization method of the polyamic acid particularly preferably used in the present invention may be a block polymerization method.

[0040] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited. Any solvent that dissolves the carboxylic acid may be used, but an amide-based solvent is preferred. Specifically, the solvent may be an organic polar solvent, and more specifically, may be an aprotic polar solvent, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as necessary. In one example, the solvent that can be particularly preferably used is N,N-dimethylformamide or N,N-dimethylacetamide.

[0041] In the polyamic acid production process, a filler may be added for the purpose of improving various properties of the film, such as sliding properties, thermal conductivity, corona resistance, Knoop hardness, etc. The filler to be added is not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.

[0042] The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm. If the particle size is below this range, it becomes difficult to obtain the modifying effect, whereas if it exceeds this range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced.

[0043] The amount of the filler to be added is not particularly limited and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, per 100 parts by weight of polyimide. If the amount of the filler added is less than this range, the filler is unlikely to have a modifying effect, and if it exceeds this range, the mechanical properties of the film may be significantly damaged. The method of adding the filler is not particularly limited, and any known method may be used.

[0044] In the production method of the present invention, the polyimide film can be produced by a thermal imidization method or a chemical imidization method. It can also be produced by a hybrid imidization method in which thermal imidization and chemical imidization are carried out simultaneously.

[0045] The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared drier. The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600° C., specifically, 200 to 500° C., more specifically, 300 to 500° C.

[0046] However, even during the process of forming the gel film, a portion of the amic acid (about 0.1 mol % to 10 mol %) can be imidized, and for this purpose, the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which can also be included in the category of the thermal imidization method. In the case of the chemical imidization method, a polyimide film can be prepared using a dehydrating agent and an imidization agent according to methods well known in the art. As an example of the composite imidization method, a dehydrating agent and an imidization agent are added to a polyamic acid solution, which is then heated at 80 to 200°C, preferably 100 to 180°C, partially cured and dried, and then heated at 200 to 400°C for 5 to 400 seconds to produce a polyimide film.

[0047] The polyimide film of the present invention produced by the above-mentioned production method may have a dielectric constant of 4.0 or more and 7.0 or less, and a dielectric loss factor of 0.01 or less.

[0048] The present invention provides a multilayer film comprising the aforementioned polyimide film, and a flexible metal foil laminate comprising the aforementioned polyimide film and an electrically conductive metal foil.

[0049] The multilayer film may include a thermoplastic resin layer, in particular a thermoplastic polyimide resin layer.

[0050] The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment applications, the metal foil may be, for example, copper or copper alloy, stainless steel or its alloy, nickel or nickel alloy (including alloy 42), aluminum or aluminum alloy. In general soft metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and can be preferably used in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer. In the present invention, the thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient function depending on the application.

[0051] The flexible metal foil laminate according to the present invention may have a structure in which a metal foil is laminated on one side of the polyimide film, or an adhesive layer containing a thermoplastic polyimide is added to one side of the polyimide film, and the metal foil is laminated in a state of being attached to the adhesive layer.

[0052] The present invention also provides an electronic component including the flexible metal foil laminate as an electrical signal transmission circuit, the electrical signal transmission circuit being an electronic component that transmits signals at a high frequency of at least 2 GHz, particularly at least 5 GHz, more particularly at least 10 GHz. The electronic component may be, for example, but is not limited to, a communication circuit for a mobile terminal, a communication circuit for a computer, or a communication circuit for an aerospace application. EXAMPLES

[0053] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention. However, these examples are presented only as examples of the present invention and do not define the scope of the invention.

[0054] <Production Example> DMF was added to a 500 ml reactor equipped with a stirrer and nitrogen inlet / outlet tubes while injecting nitrogen, and the temperature of the reactor was set to 30° C. or less. Then, m-tolidine and paraphenylenediamine as diamine components, and benzophenone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride and pyromellitic dianhydride as dianhydride components were added, and it was confirmed that they were completely dissolved. The content of m-tolidine was 34 mol % and the content of p-phenylenediamine was 66 mol % based on 100 mol % of the total content of the diamine components. The content of biphenyltetracarboxylic dianhydride was 33 mol %, the content of biphenyltetracarboxylic dianhydride was 32 mol %, and the content of pyromellitic dianhydride was 35 mol %. Thereafter, the temperature of the reactor was raised to 40° C. under a nitrogen atmosphere, and stirring was continued for 120 minutes to produce polyamic acid. The graphene nanoplates were added to the polyamic acid thus prepared and then stirred. A catalyst and a dehydrating agent were added to the final polyamic acid thus prepared, and the mixture was rotated at a high speed of 1,500 rpm or more to remove air bubbles, and then the mixture was applied to a glass substrate using a spin coater. Then, the gel film was prepared by drying at 120°C for 30 minutes under a nitrogen atmosphere, and the temperature was increased to 450°C at a rate of 2°C / min, and heat-treated at 450°C for 60 minutes. The gel film was then cooled again at a rate of 2°C / min to 30°C to obtain a final polyimide film, which was then peeled off from the glass substrate by dipping in distilled water. The thickness of the polyimide film was 15 μm. The thickness of the polyimide film was measured using an Anritsu Electric Film Thickness Tester.

[0055] <Examples 1 and 2 and Comparative Examples 1 to 5> The graphene nanoplate content was adjusted as shown in Table 1 by the same method as described above.

[0056] [Table 1]

[0057] <Experimental Example>Evaluation of dielectric constant and dielectric loss factor As shown in Table 1, the dielectric constant and dielectric loss factor of the polyimide films prepared in Examples 1 and 2 and Comparative Examples 1 to 5 were measured. (1) Measurement of dielectric constant The dielectric constant (Dk) was measured at 10 GHz using a Keysight SPDR measuring instrument. (2) Measurement of dielectric loss factor The dielectric loss factor (Df) was measured using an Agilent 4294A resistance meter by leaving the soft metal foil laminate for 72 hours.

[0058] As shown in Table 1, the polyimide films prepared according to the embodiments of the present invention satisfied all the conditions that the dielectric constant was 4.0 or more and 7.0 or less, and the dielectric loss factor was 0.01 or less. The polyimide films of Comparative Examples 1 and 2, which contained no graphene nanoplates or only a small amount (0.1 wt %) of graphene nanoplates, had a dielectric constant of less than 4.0. In addition, Comparative Examples 3 to 5, which contained an excessive amount (3 wt % or more) of graphene nanoplates, had a dielectric constant exceeding 7.0, and in particular, Comparative Examples 4 and 5 also had a dielectric loss factor exceeding 0.01. Therefore, it can be seen that the dielectric constant and dielectric loss factor are at desired levels only within the range of the graphene nanoplate content according to the embodiment. Such results are achieved by the components and composition ratios specified herein, and it is understood that the content of each component plays a decisive role. In contrast, the polyimide films of Comparative Examples 1 and 2, which have components different from those of the Examples, are expected to be difficult to use in electronic components in which signal transmission is performed at high frequencies in the gigahertz range, since they have lower dielectric constants and dielectric loss factors than the polyimide films of the Examples. The present invention has been described above with reference to examples thereof. However, a person having ordinary knowledge in the field to which the present invention pertains will be able to make various applications and modifications within the scope of the present invention based on the above content. [Industrial Applicability]

[0059] As described above, the present invention provides a polyimide film having excellent dielectric properties through a polyimide film having specific components and a specific composition ratio and a manufacturing method thereof, and the polyimide film can be usefully applied to various fields requiring such properties, particularly electronic parts such as flexible metal foil laminates.

Claims

1. The polyamic acid solution is obtained by imidizing a dianhydride component including benzophenonetetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) and a diamine component including m-tolidine and paraphenylenediamine (PPD), Contains 0.5 to 2.5 wt.% graphene nanoplatelets; Polyimide film.

2. the content of m-tolidine is 20 mol % or more and 40 mol % or less, and the content of p-phenylenediamine is 60 mol % or more and 80 mol % or less, based on 100 mol % of the total content of the diamine components; The polyimide film according to claim 1 .

3. The content of benzophenone tetracarboxylic dianhydride is 20 mol % or more and 45 mol % or less based on 100 mol % of the total content of the dianhydride acid components, The content of biphenyltetracarboxylic dianhydride is 20 mol % or more and 45 mol % or less, 2. The polyimide film according to claim 1, wherein the content of the pyromellitic dianhydride is from 20 mol % to 45 mol %.

4. The graphene nanoplates have an average thickness of 6 to 8 nm; The average particle size is 5 to 25 μm. Specific surface area is 120 to 150 m 2 / g, The polyimide film according to claim 1 .

5. The dielectric constant is 4.0 or more and 7.0 or less, The dielectric loss factor is 0.01 or less. The polyimide film according to claim 1 .

6. (a) preparing a polyamic acid by polymerizing a dianhydride component including benzophenonetetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) and a diamine component including m-tolidine and paraphenylenediamine (PPD) in an organic solvent; (b) adding and mixing graphene nanoplates into the polyamic acid; and (c) imidizing the polyamic acid containing the graphene nanoplates; A method for producing a polyimide film.

7. the content of m-tolidine is from 20 mol % to 40 mol % and the content of p-phenylenediamine is from 60 mol % to 80 mol % based on 100 mol % of the total content of the diamine components; The content of benzophenone tetracarboxylic dianhydride is 20 mol % or more and 45 mol % or less based on 100 mol % of the total content of the dianhydride acid components, The content of biphenyltetracarboxylic dianhydride is 20 mol % or more and 45 mol % or less, The method for producing a polyimide film according to claim 6, wherein the content of the pyromellitic dianhydride is from 20 mol % to 45 mol %.

8. The dielectric constant of the polyimide film is 4.0 or more and 7.0 or less, The dielectric loss factor is 0.01 or less. The method for producing a polyimide film according to claim 6 .

9. The polyimide film according to any one of claims 1 to 5 is included. Multilayer film.

10. A laminate comprising the polyimide film according to any one of claims 1 to 5 and an electrically conductive metal foil. Flexible metal foil laminate.

11. The flexible metal foil laminate according to claim 10, Electronic components.

Citation Information

Patent Citations

  • Graphene modified polyimide-based composite and preparation method thereof

    CN102911360A

  • Multilayer polyimide film and method for manufacturing multilayer polyimide film

    JP2017177601A

  • High heat resistance, low dielectric polyimide film and method for producing the same

    JP2023500716A

  • Apparatus for assisting driving of a host vehicle and method therof

    KR1020220148378A

  • Highly heat-resistant and low dialectric-polyimide film and method for producing same

    US20220396667A1