Thermoplastic polyurethane powder and 3D molded body formed from said powder
The use of TPU powder from expanded TPU with specific particle and density characteristics addresses the challenge of producing lightweight 3D printed parts with high resilience and mechanical strength, suitable for automotive and footwear components.
Patent Information
- Application Number
- JP2024522511
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-15
- Filing Date
- 2022-10-07
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing 3D printing technologies using thermoplastic polyurethane powders face challenges in producing lightweight parts with high impact resilience and good mechanical properties, particularly for automotive and footwear applications.
Development of thermoplastic polyurethane (TPU) powder derived from expanded TPU, with an average particle diameter of 1 mm or less, and a bulk density of 1 g/cm³ or less, which can be used to create 3D products with low density and high resilience through processes like selective laser sintering.
The TPU powder enables the production of 3D molded bodies with densities as low as 0.55 g/cm³ and impact resilience of at least 35%, along with excellent mechanical properties, suitable for applications such as soles, outerwear, and footwear.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic polyurethane powder, a 3D body formed from the powder, and a method for forming the 3D body. [Background technology]
[0002] 3D printing techniques using thermoplastic powders, such as selective laser sintering (SLS), multi-jet fusion (MJF), and selective heat sintering (SHS), are used for rapid prototyping and rapid manufacturing processes. Thermoplastic polyurethane powder is a type of 3D printable material and is widely used in footwear, protective gear, and consumer applications. To obtain lightweight 3D printed parts, it is necessary to extend 3D printed parts from prototyping to end-use parts, especially in the automotive and footwear industries. However, it is difficult to obtain 3D printed parts with low density, high resilience, and good mechanical properties. Therefore, there is a strong demand for the development of material types with low density, high resilience, and excellent performance for the successful 3D printing process. Summary of the Invention [Problem to be solved by the invention]
[0003] One object of the present invention is to provide a thermoplastic polyurethane (TPU) powder derived from an expanded TPU and / or a molded part thereof, the TPU powder of the present invention can be used to prepare 3D products with low density and high resilience.
[0004] Another object of the present invention is to provide a powder composition comprising the TPU powder of the present invention and at least one auxiliary agent.
[0005] A further object of the present invention is to provide a method for preparing a 3D molded body comprising using the TPU powder of the present invention.
[0006] It is a further object of the present invention to provide a 3D molded body formed from the TPU powder of the present invention. [Means for solving the problem]
[0007] Surprisingly, it has been found that the above objectives can be achieved by the following embodiments: 1. Thermoplastic polyurethane (TPU) powder derived from expanded TPU and / or its molded parts, the average particle size D50 of which is 1 mm or less.
[0008] 2. The TPU powder according to item 1, wherein the average particle size D50 of the TPU powder is in the range of 1 μm to 1 mm.
[0009] 3. The TPU powder according to item 1 or 2, wherein the average particle size D50 of the TPU powder is in the range of 5 to 800 μm, preferably 10 to 500 μm.
[0010] 4. The bulk density of the TPU powder is 1 g / cm 3 Less than 0.8 g / cm 3 or less than 0.6g / cm 3 4. The TPU powder according to any of items 1 to 3, wherein
[0011] 5. The TPU powder according to any of items 1 to 4, wherein the TPU powder is derived from expanded TPU pellets or molded parts thereof or residual expanded TPU or reclaimed expanded TPU, or a mixture thereof.
[0012] 6. Use of an expanded TPU and / or a molded part thereof for producing a TPU powder according to any of items 1 to 5.
[0013] 7. A method for preparing a TPU powder according to any of items 1 to 5, comprising atomizing the expanded TPU and / or a molded part thereof.
[0014] 8. A powder composition comprising the TPU powder according to any of items 1 to 5 and at least one adjuvant preferably selected from fillers, flow agents and pigments.
[0015] 9. Use of the TPU powder according to any one of items 1 to 5 or the powder composition according to item 8 for preparing a 3D molded body.
[0016] 10. A method for preparing a 3D molded body, comprising using a TPU powder according to any of items 1 to 5 or a composition according to item 8.
[0017] 11. The method according to item 10, comprising the steps of: a) adding a TPU powder according to any of items 1 to 5 or a composition according to item 8 to a molding mixture, and b) Producing molded articles by selectively bonding powders The method includes:
[0018] 12. The method according to claim 11, wherein the molded body produced in step b) is produced by a process of building a three-dimensional object layer-by-layer by selectively bonding parts of a powder onto other parts of a powder.
[0019] 13. The method according to claim 11 or 12, wherein selectively bonding comprises selective laser sintering, selective inhibition of powder bonding, multi-jet fusion, rapid sintering, 3D printing, or a microwave process.
[0020] 14. A 3D molded body formed from the TPU powder according to any of items 1 to 5 or from the composition according to item 8.
[0021] 15. The 3D molded body according to item 14, wherein the 3D molded body includes a sole, outerwear, fabric, footwear, toys, mats, tires, hoses, gloves and seals.
[0022] 16. The 3D shaped body according to any one of items 14 or 15, having a density of 1 g / cm 3 Less than 0.95 g / cm 3 Less than or equal to 0.9 g / cm 3 The following is a 3D molded body.
[0023] 17. The 3D shaped body according to any of items 14 to 16, wherein the rebound resilience according to ASTM D2632 is at least 35%, preferably at least 40%, more preferably at least 42%.
[0024] 18. The 3D shaped body according to any of items 14 to 17, wherein its elongation at break according to ISO 527-21 / A15 2012 is at least 50%, preferably at least 80%, more preferably at least 100% or at least 120%.
[0025] The TPU powder of the present invention can be used to prepare 3D products with low density, high resilience and good mechanical properties, and the TPU powder of the present invention can be obtained from a wide range of sources, in particular from reclaimed and residual expanded TPU, and the TPU powder and 3D products of the present invention can be easily recycled. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 shows a photograph of the printed part of Example C. [Diagram 2] FIG. 2 shows a photograph of the remaining expanded TPU molded part. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The undefined articles "a," "an," and "the" refer to one or more of the species designated by the term that follows the article.
[0028] In the context of this disclosure, any specific values recited for a characteristic (including the specific values recited in a range as endpoints) may be recombined to form new ranges.
[0029] One aspect of the invention relates to a thermoplastic polyurethane (TPU) powder derived from an expanded TPU, the powder having a mean particle size D50 of 1 mm or less.
[0030] TPU powder According to the present invention, the average particle size D50 of the TPU powder is from 1 μm to 1 mm, for example, 1 μm, 5 μm, 10 μm, 20 μm, 50 μm, 80 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm or 1 mm, preferably 1 to 800 μm, 5 to 600 μm, 10 to 500 μm, 10 to 400 μm, It can be in the range of 10 to 250 μm, or 20 to 800 μm, 20 to 600 μm, 20 to 400 μm, 20 to 250 μm, or 30 to 800 μm, 30 to 600 μm, 30 to 400 μm, 30 to 250 μm, or 40 to 800 μm, 40 to 600 μm, 40 to 400 μm, 40 to 250 μm, or 50 to 800 μm, 50 to 600 μm, 50 to 400 μm, or 50 to 250 μm.
[0031] The average particle size D50 can be tested according to ISO13320-1.
[0032] In one embodiment, the TPU powder has a bulk density of 1 g / cm 3 For example, 0.01 g / cm 3 , 0.05g / cm 3 , 0.1g / cm 3 , 0.15g / cm 3 , 0.2g / cm 3 , 0.3g / cm 3 , 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 , 0.9g / cm3 , or 1g / cm 3 , preferably 0.8 g / cm 3 or less than 0.6g / cm 3 or less than 0.5g / cm 3 In one embodiment, the bulk density of the TPU powder is 0.01 g / cm 3 ~1g / cm 3 , 0.05g / cm 3 ~0.9g / cm 3 , 0.05g / cm 3 ~0.7g / cm 3 , 0.05g / cm 3 ~0.65g / cm 3 , or 0.1 g / cm 3 ~0.6g / cm 3 The range may be:
[0033] The bulk density of the TPU powder can be tested according to ISO1068.
[0034] According to the present invention, the TPU powder is derived from expanded TPU and / or its molded parts. The expanded TPU and its molded parts can have a wide range of sources. For example, they can be selected from expanded TPU pellets (e.g., microspheres), molded parts of expanded TPU (e.g., molded parts of expanded TPU pellets), residual expanded TPU, recycled expanded TPU, or a mixture thereof.
[0035] According to one embodiment, the TPU powder of the present invention is derived from, in particular produced by comminuted (e.g., grinding) expanded TPU and / or molded parts thereof, such as expanded TPU pellets (e.g., microspheres), residual expanded TPU, reclaimed expanded TPU, molded parts of expanded TPU, or mixtures thereof.
[0036] TPUs and their preparation methods are well known. For example, TPUs can be prepared via the reaction of (a) an isocyanate with (b) a compound reactive towards isocyanates and having a molar mass of 500 to 10,000, and optionally (c) a chain extender having a molar mass of 50 to 499, optionally in the presence of (d) a catalyst and / or (e) conventional auxiliaries and / or conventional additives.
[0037] The components (a) isocyanate, (b) compound reactive towards isocyanate, (c) chain extender are individually or collectively referred to as forming components. The forming components, including catalysts and / or conventional auxiliaries and / or additives, are also referred to as starting materials.
[0038] According to the present invention, the TPU is at least 0.1 × 10 6 g / mol, preferably at least 0.4×10 6 g / mol, specifically 0.6×10 6 It is preferred to prepare TPUs with a weight average molecular weight of more than 0.8×10 g / mol. The upper limit of the weight average molecular weight of the TPU is generally determined by processability and the desired property spectrum. The number average molecular weight of the TPU is preferably less than 0.8×10 6 The average molecular weights given above for the TPU and forming components (a) and (b) can be determined by gel permeation chromatography.
[0039] As organic isocyanates (a), aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates are preferred, more preferably trimethylene, tetramethylene, pentamethylene, hexamethylene, heptamethylene and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethylbutylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4-bis(isocyanatomethyl)cyclohexane and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), paraphenylene 2,4-diisocyanate (PPDI), tetramethylene diisocyanate, ... Preference is given to using tramethylene xylene 2,4-diisocyanate (TMXDI), dicyclohexylmethane 4,4'-, 2,4'- and 2,2'-diisocyanate (H12MDI), hexamethylene 1,6-diisocyanate (HDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate, (MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), diphenylmethane diisocyanate, 3,3'-dimethylbiphenyl diisocyanate, diphenylmethane 1,2-diisocyanate and / or phenylene diisocyanate.
[0040] Preference is given to using the isocyanates diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), hexamethylene 1,6-diisocyanate (HDI) and dicyclohexylmethane 4,4'-, 2,4'- and 2,2'-diisocyanate (H12MDI), particularly preferably diphenylmethane 4,4'-diisocyanate (4,4'-MDI).
[0041] As the compound (b) reactive to isocyanate, 500 g / mol to 8×10 3g / mol, preferably 0.7×10 3 g / mol ~ 6.0 x 10 3 g / mol, specifically 0.8×10 3 g / mol ~ 4.0 x 10 3 Those with molecular weights in the g / mol range are preferred.
[0042] The compound (b) reactive towards isocyanates has, on a statistical average, at least 1.8 and not more than 3.0 Zerewitinoff active hydrogen atoms, this number is also called the functionality of the compound (b) reactive towards isocyanates, which gives the theoretical molar amount of isocyanate-reactive groups of the molecule calculated per molecule. The functionality is preferably in the range of 1.8 to 2.6, more preferably in the range of 1.9 to 2.2, and especially 2.
[0043] The compound reactive towards isocyanates is a substance or mixture of substances which are substantially linear and reactive towards isocyanates, and which mixture meets the aforementioned requirements.
[0044] These long chain compounds are used in a molar ratio of 1 equivalent mol % to 80 equivalent mol % based on the isocyanate group content of the polyisocyanate.
[0045] The compound (b) which is reactive towards isocyanates preferably has reactive groups selected from hydroxyl, amino, mercapto or carboxyl groups. Hydroxyl groups are preferred. The compound (b) which is reactive towards isocyanates is particularly preferably selected from the group consisting of polyesterols, polyetherols and polycarbonate diols, which are summarized under the term "polyols".
[0046] Also preferred are polyester diols, preferably polycaprolactones, and / or polyether polyols, preferably polyether diols, more preferably those based on ethylene oxide, propylene oxide and / or butylene oxide, preferably polypropylene glycol. One particularly preferred polyether is polytetrahydrofuran (PTHF), especially polyetherol.
[0047] Particular preference is given to polyols selected from the following group: copolyesters based on adipic acid, succinic acid, pentanedioic acid, sebacic acid or mixtures thereof and mixtures of 1,2-ethanediol and 1,4-butanediol, copolyesters based on adipic acid, succinic acid, pentanedioic acid, sebacic acid or mixtures thereof and mixtures of 1,4-butanediol and 1,6-hexanediol, polyesters based on adipic acid, succinic acid, pentanedioic acid, sebacic acid or mixtures thereof and 3-methylpentane-1,5-diol and / or polytetramethylene glycol (polytetrahydrofuran, PTHF).
[0048] It is particularly preferable to use copolyesters based on adipic acid and mixtures of 1,2-ethanediol and 1,4-butanediol, or copolyesters based on adipic acid and 1,4-butanediol and 1,6-hexanediol, or polyesters based on adipic acid and polytetramethylene glycol (polytetrahydrofuran PTHF) or mixtures thereof.
[0049] Very particular preference is given to using polyesters based on adipic acid and polytetramethylene glycol (PTHF) or mixtures thereof as polyols.
[0050] In a preferred embodiment, chain extenders (c) are used, which are preferably aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds having a molecular weight between 50 g / mol and 499 g / mol and preferably having two isocyanate-reactive groups, also referred to as functional groups.
[0051] The chain extender (c) is preferably at least one chain extender selected from the group consisting of 1,2-ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanediol, 1,4-dimethanolcyclohexane and neopentyl glycol. Chain extenders selected from the group consisting of 1,2-ethylene glycol, 1,3-propanediol, 1,4-butanediol and 1,6-hexanediol are particularly preferred.
[0052] Very particularly preferred chain extenders are 1,4-butanediol, 1,6-hexanediol and ethanediol.
[0053] In a preferred embodiment, catalysts (d) are used together with the forming components. These are in particular catalysts which promote the reaction between the NCO groups of the isocyanates (a) and the hydroxyl groups of the compounds (b) which are reactive towards isocyanates and, if used, the chain extenders (c). Preferred catalysts are tertiary amines, in particular triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 2-(dimethylaminoethoxy)ethanol, diazabicyclo[2.2.2]octane. In another preferred embodiment, the catalyst is an organometallic compound, for example a titanate ester, an iron compound, preferably iron(III) acetylacetonate, a tin compound, preferably of a carboxylic acid, particularly preferably tin diacetate, tin dioctoate, tin dilaurate or a dialkyltin salt, more preferably dibutyltin diacetate, dibutyltin dilaurate, or a bismuth salt of a carboxylic acid, preferably bismuth decanoate.
[0054] Particularly preferred catalysts are tin dioctoate, bismuth decanoate, and titanic acid esters. The catalyst (d) is preferably used in an amount of 0.0001 to 0.1 parts by mass, or 0.001 to 0.05 parts by mass, per 100 parts by mass of the isocyanate-reactive compound (b). Apart from the catalyst (d), conventional auxiliaries (e) can also be added to the forming components (a)-(c). Examples include surface-active substances, fillers, flame retardants, nucleating agents, oxidation inhibitors, lubricants and release aids, dyes and pigments, optionally stabilizers, preferably stabilizers against hydrolysis, light, heat or discolouration, inorganic and / or organic fillers and / or plasticizers.
[0055] In one embodiment, the TPU is contacted with a blowing agent.
[0056] In principle, expanded TPU pellets can be produced by directly or indirectly via a suspension or extrusion process, by expanding the expandable TPU pellets in a pressure pre-expander with steam or hot air.
[0057] In the suspension process, the TPU in pellet form is heated above the softening point of the pellets together with water, suspending agent and blowing agent in a closed reactor. This causes the polymer pellets to be impregnated with the blowing agent. The hot suspension is then allowed to cool, the particles solidify containing the blowing agent and the reactor is depressurized. The (expandable) pellets thus obtained, containing the blowing agent, are expanded by heating to give expanded pellets. Alternatively, the hot suspension can be suddenly depressurized without cooling (explosion-expansion process), in which case the softened pellets containing the blowing agent are immediately expanded to give expanded pellets.
[0058] In the extrusion process, the TPU is mixed with a blowing agent introduced into the extruder while being melted in the extruder. The mixture containing the blowing agent is extruded and pelletized under conditions of pressure and temperature such that the TPU pellets do not foam (expand). An example of a method used for this purpose is underwater pelletization, operated at a water pressure of more than 2 bar. This results in expandable pellets containing the blowing agent, which are expanded by subsequent heating to obtain expanded pellets. Alternatively, the mixture can be extruded at atmospheric pressure and pelletized. In this process, the molten extrudate is expanded, and the product obtained by pelletization is expanded pellets.
[0059] The TPU can be used in the form of commercially available pellets, powder, granules, or any other form. It is advantageous to use pellets. An example of a suitable form is what is known as pellets, with a preferred average diameter of 0.2 to 10 mm, in particular 0.5 to 5 mm. These mainly cylindrical or round pellets are produced via extrusion of the TPU and optionally other additives, discharge from the extruder, optional cooling, and pelletization. For cylindrical pellets, the length is preferably 0.2 to 10 mm, in particular 0.5 to 5 mm. The pellets can also have a lamellar shape. The average diameter of the thermoplastic polyurethane including the blowing agent is preferably 0.2 to 10 mm.
[0060] As a function of the process used, the preferred blowing agent can be varied if appropriate. In the case of suspension processes, the blowing agent used preferably comprises an organic liquid or an inorganic gas, or a mixture thereof. Liquids that can be used include halogenated hydrocarbons, but saturated aliphatic hydrocarbons, especially those having 3 to 8 carbon atoms, are preferred. Suitable inorganic gases are nitrogen, air, ammonia, or carbon dioxide.
[0061] In the production via extrusion process, the blowing agent used preferably comprises a volatile organic compound having a boiling point of −25 to 150° C. at atmospheric pressure of 1013 mbar, in particular −10 to 125° C. Hydrocarbons (preferably free of halogens) are suitable, in particular C 4~10-alkanes, such as the isomers of butane, the isomers of pentane, the isomers of hexane, the isomers of heptane and the isomers of octane, particularly preferably sec-pentane. Other suitable blowing agents are bulkier compounds, such as alcohols, ketones, esters, ethers and organic carbonates.
[0062] The blowing agent is preferably halogen-free, although halogenated hydrocarbons may also be used. However, this does not preclude the use of a very small proportion of halogen-containing blowing agents in the blowing agent mixture. It is, of course, also possible to use mixtures of the aforementioned blowing agents.
[0063] The amount of the foaming agent is preferably 0.1 to 40 parts by mass, particularly preferably 0.5 to 35 parts by mass, and particularly preferably 1 to 30 parts by mass, based on 100 parts by mass of the TPU used.
[0064] When the expandable TPU pellets are obtained, they can be expanded in a known manner to obtain expanded TPU pellets. The expansion is generally carried out by heating the expandable pellets in a conventional expansion apparatus, for example with hot air or superheated steam, known as a pressure pre-expander, for example of the type normally used for processing expandable polystyrene (EPS). It is preferable to expand the pellets at a temperature at which the pellets soften (softening range), particularly preferably at a temperature between 100 and 140°C.
[0065] The bulk density of the expanded TPU pellets can be between 10 and 600 g / l, and preferably between 15 and 300 g / l.
[0066] The average diameter of the expanded TPU pellets is usually in the range of 0.2 to 20 mm, preferably 0.5 to 15 mm, and in particular 1 to 12 mm. In the case of non-spherical, e.g. elongated or cylindrical, pellets, the diameter refers to the longest dimension.
[0067] The TPU powder according to the invention can be obtained by atomization of expanded TPU pellets and / or molded parts thereof.
[0068] In one embodiment, the expanded TPU is a reclaimed expanded TPU, a residual expanded TPU, a molded part of an expanded TPU, or a mixture thereof.
[0069] The regenerated expanded TPU can be made into a shaped article, such as a sole. The regenerated expanded TPU can be granulated to obtain the TPU powder according to the present invention. Before granulation, the regenerated expanded TPU can be washed and / or separated from foreign matter.
[0070] The TPU powder of the present invention allows the preparation (for example by 3D printing) of 3D molded bodies with low density, high resilience, preferably good mechanical properties, especially breaking elongation.The details of the density, resilience and mechanical properties of the 3D molded bodies are as follows for the 3D molded bodies of the present invention.
[0071] composition One aspect of the invention relates to a powder composition comprising the TPU powder according to the invention and at least one auxiliary agent, which may be chosen from fillers, flow agents and pigments.
[0072] The flow agent may be selected from the group consisting of silica, fumed silica, precipitated silica, colloidal silica, hydrophobic / hydrophilic silica and mixtures thereof.
[0073] The fluidizing agent of the present invention has a median particle size of 5 nm to 200 μm. The median particle size of the fluidizing agent is preferably 10 nm to 150 μm, and particularly preferably 100 nm to 100 μm.
[0074] The fluidizing agent is 20 to 600 m 2 The fluidizing agent preferably has a specific surface area of 40 to 550 m 2 / g, particularly preferably 60 to 500m 2 / g, and more preferably 60 to 450 m 2 / g.
[0075] The amount of the flow agent in the composition can be 0 to 5 mass%, 0.01 to 5 mass%, 0.01 to 3 mass%, 0.01 to 2 mass%, 0.05 to 5 mass%, 0.05 to 3 mass%, 0.05 to 2 mass%, 0.1 to 5 mass%, 0.1 to 3 mass%, or 0.1 to 2 mass%, relative to the total mass of the composition.
[0076] Examples of fillers include glass microspheres, glass fibers, and carbon fibers.
[0077] As other auxiliary agents, preferred examples include surface active substances, nucleating agents, lubricating waxes, dyes, catalysts, UV absorbers and stabilizers, such as stabilizers against oxidation, hydrolysis, light, heat or discoloration. As hydrolysis inhibitors, oligomeric and / or polymeric aliphatic or aromatic carbodiimides are preferred. In order to stabilize the 3D printed object of the present invention against aging and harmful environmental effects, in a preferred embodiment, stabilizers are added to the system.
[0078] In the case where the composition of the present invention is exposed to thermo-oxidative damage during use, in a preferred embodiment, antioxidant is added.Phenol antioxidant is preferred.Phenol antioxidant, such as Irganox® 1010 from BASF SE, is shown in Plastics Additive Handbook, 5th edition, H. Zweifel, ed., Hanser Publishers, Munich, 2001, pages 98-107, 116 and 121.
[0079] When the composition of the present invention is exposed to UV light, it is preferable to additionally stabilize the composition with a UV absorber. UV absorbers are generally known as molecules that absorb high-energy UV light and dissipate energy. Conventional UV absorbers used in industry belong to the groups of, for example, cinnamic acid esters, diphenylcyanoacrylates, formamidines, benzylidene malonates, diaryl butadienes, triazines and benzotriazoles. Examples of commercially available UV absorbers can be found in Plastics Additive Handbook, 5th edition, H. Zweifel, ed, Hanser Publishers, Munich, 2001, pages 116-122.
[0080] Further details regarding the abovementioned auxiliaries can be found in the specialist literature, for example in Plastics Additive Handbook, 5th Edition, H. Zweifel, ed., Hanser Publishers, Munich, 2001.
[0081] The total amount of the at least one auxiliary agent can be in the range of 0 to 60% by weight, preferably 0 to 40% by weight, 0 to 20% by weight, 0 to 10% by weight, 0 to 5% by weight, or 0.01 to 60% by weight, 0.05 to 40% by weight, or 0.1 to 20% by weight, relative to the total weight of the composition.
[0082] Method for preparing 3D bodies In a further aspect, the present invention relates to a method for preparing a 3D moulded body comprising using the TPU powder according to the invention or the composition according to the invention.
[0083] In one embodiment, the method comprises: a) adding the inventive TPU powder or the inventive composition to a molding mixture, and b) Producing a compact by selectively bonding the powder. Includes.
[0084] In one embodiment, the compact produced in step b) is produced by a process of building a three-dimensional object layer by layer by selectively bonding a portion of a powder onto another portion of a powder. In a preferred embodiment, the selective bonding comprises selective laser sintering, selective inhibition of powder bonding, multi-jet fusion, rapid sintering, 3D printing, or microwave processes.
[0085] According to the present invention, selectively bonding includes selective laser sintering, selective inhibition of powder bonding, multi-jet fusion, rapid sintering, 3D printing, or microwave processes, in particular by 3D printing.
[0086] After step (b) is completed, the part can be separated from the excess powder to obtain the final 3D body.
[0087] According to the present invention, the excess powder can be reused for printing as is.
[0088] 3D molded object In a further aspect, the present invention relates to a 3D molded body formed from the TPU powder of the present invention or from the composition of the present invention. According to one embodiment, the 3D molded objects include soles, outerwear, fabrics, footwear, toys, mats, tires, hoses, gloves and seals.
[0089] The 3D moulded bodies of the present invention have low density, high resilience and preferably good mechanical properties, in particular elongation at break.
[0090] In a preferred embodiment, the density of the 3D molded body of the present invention is less than 1 g / cm 3 For example, 0.95 g / cm 3 , 0.9g / cm 3 , 0.85g / cm 3 , 0.8g / cm 3 , 0.78g / cm 3 , 0.76g / cm 3 , 0.74g / cm 3 , 0.72g / cm 3, 0.70g / cm 3 , 0.68g / cm 3 , 0.66g / cm 3 , 0.64g / cm 3 , 0.62g / cm 3 , 0.6g / cm 3 , 0.58g / cm 3 , 0.56g / cm 3 or 0.55g / cm 3 Preferably, the density of the 3D molded body of the present invention is 0.95 g / cm 3 Below, 0.9g / cm 3 Below, 0.8g / cm 3 Below, 0.78g / cm 3 , 0.76g / cm 3 Below, 0.74g / cm 3 or less than 0.72 g / cm 3 Preferably, the density of the 3D molded body of the present invention is 0.1 to 1 g / cm 3 , 0.1~0.9g / cm 3 , 0.1~0.8g / cm 3 , 0.2~0.8g / cm 3 , 0.3~0.8g / cm 3 , 0.4~0.8g / cm 3 , 0.5~0.8g / cm 3 , 0.6~0.78g / cm 3 , or 0.62 to 0.76 g / cm 3 The range is.
[0091] Density can be tested according to ASTM D792.
[0092] In a preferred embodiment, the resilience of the 3D molded body of the present invention according to ASTM D2632 is at least 35%, for example 36%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, or 65%, 70%, or 80%, preferably at least 38%, at least 40%, at least 42%, at least 45%, or at least 48%. In a preferred embodiment, the resilience of the 3D molded body of the present invention is in the range of 35% to 80%, 35% to 70%, 35% to 65%, 38% to 62%, 40% to 60%, or 42% to 60%.
[0093] In a preferred embodiment, the breaking elongation of the 3D shaped body of the invention according to ISO527-21 / A15 2012 is at least 50%, preferably 80%, for example 100%, 120%, 140%, 150%, 180%, 200%, 220%, 250%, 280%, 300%, 400%, 500% or 600%, preferably at least 100%, or at least 120%. In a preferred embodiment, the breaking elongation of the 3D shaped body of the invention is in the range of 50% to 600%, 80% to 600%, 80% to 550%, 100% to 550%.
[0094] In a preferred embodiment, the 3D shaped body of the present invention has a hardness (Shore A) according to ASTM D2240-15 of A40 to A72, for example A44, A46, A48, A50, A52, A55, A60, A65, A68, A70 or A72, preferably A44 to A72.
[0095] The tensile strength of the 3D molded body of the present invention according to ISO527-21 / A15 2012 is 1 MPa or more, for example 1.2 MPa, 1.3 MPa, 1.4 MPa, 1.5 MPa, 1.8 MPa, 2.0 MPa, 2.2 MPa, 2.5 MPa, 2.8 MPa, 3.0 MPa, 3.2 MPa, 3.5 MPa, 4 MPa, 4.5 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, or 15 MPa. In a preferred embodiment, the tensile strength of the 3D molded body of the present invention is in the range of 1 to 15 MPa, or 1.2 to 12 MPa. EXAMPLES
[0096] material - Thermoplastic polyurethane powder (TPU-1): Prepared by grinding BASF expanded TPU130U pellets (BASF commercial product: Infinergy X1125-130U, bulk density of pellets is 0.12-0.14 g / cm 3 The average pellet mass was 26 mg and the average pore size was 130 μm. The average powder particle size D50 was 160 μm and the bulk density of the powder was 0.18 g / cm 3 The TPU-1 powder was prepared by cryogenic grinding at −196° C. and a grinding speed of 100 m / s (linear velocity) and sieving to the required size.
[0097] - Thermoplastic polyurethane powder (TPU-2): Infinergy32-100U10 (bulk density of pellets of Infinergy32-100U10 is 0.085~0.135g / cm 3 The powder was prepared by grinding the remainder of an expanded TPU molded part (shown in FIG. 2) prepared by pulverizing the remaining ... 3 The grinding procedure was similar to that of TPU-1 powder.
[0098] Thermoplastic polyurethane powder (TPU-3): Prepared by grinding expanded TPU130U pellets from BASF (BASF commercial product: Infinergy X1125-130U, bulk density of pellets is 0.12-0.14 g / cm 3 The average mass of the pellets was 26 mg, and the average pore size was 130 μm. The average particle size D50 of the powder was 80 μm, and the bulk density of the powder was 0.25 g / cm 3 The grinding procedure was similar to that of TPU-1 powder.
[0099] -TPU88A: BASF Ultrasint TPU88A powder for 3D printing. The TPU powder was prepared by grinding TPU pellets. Bulk density of TPU88A: 0.6 g / cm3, average particle size D50 of TPU88A: 80 μm.
[0100] - Superplasticizer: Wacker HDKN20 amorphous silica (BET: 175-225m 2 / g), Cabot ENERSIL 2030 fumed silica (BET: 175-225m 2 / g).
[0101] method -All samples were printed on a Farsoon HT251SLS 3D printer. - Tensile strength and elongation at break were measured with a Zwick Z050 at a speed of 6 mm / min (in accordance with ISO 527-21 / A15 2012). - Rebound resilience was tested according to ASTM D2632. -Hardness was determined in accordance with ASTM D2240-15 using an ASKER DUROMETER (Type A). -Density was investigated according to ASTM D792. -The average particle size D50 of the powders was tested according to ISO 13320-1 with a Beckerman Coulter LS13 320 Lase Diffraction Particle Size Analyzeer. -The bulk density of TPU powder was tested according to ISO1068.
[0102] Examples A, B, C, D, E and Comparative Example 1 The powders of Example A and Comparative Example 1 shown in Table 1 were used as they were. The powder compositions of Examples B, C, D and E were prepared by blending the powders of the components shown in Table 1. The blending experiments were carried out in an HTS-5 high-speed mixer from Dongguan Huanxin Machinery Co., Ltd. Each component was weighted according to the mass percentage shown in Table 1. The powders were mixed at 1400 rpm for 60 seconds to obtain the powder compositions, and the total mass of each composition was 5000 g.
[0103] [Table 1]
[0104] Example 2 - 3D Printing The powders or powder compositions of Examples A, B, C, D, E and Comparative Example 1 were printed on a Farsoon HT251 selective laser sintering 3D printer. In a typical printing process, the powders or powder compositions were loaded into the feed chamber of the printer. For all printing processes, the printing parameters needed to be adjusted according to different types of powders and their cracking or warping phenomena during the printing process. The detailed printing parameters are shown in Table 2.
[0105] Post-treatment process: After the printing process was completed and the printed object was cooled, the build chamber was removed from the printer and transferred to a cleaning station, where the printed object was separated from the excess powder to obtain the final 3D printed object.
[0106] [Table 2]
[0107] A photograph of a print sample prepared from the powder composition of Example C is shown in FIG.
[0108] The tensile strength, breaking elongation, hardness, rebound resilience and density of the printed samples are summarized in Table 3.
[0109] [Table 3]
[0110] The printed samples or molded parts thereof based on the expanded TPU powder (Examples A, B, C, D and E) showed significantly lower density and higher resilience than the printed sample based on the powder from TPU (Comparative Example 1).
Claims
1. Thermoplastic polyurethane (TPU) powder derived from expanded TPU and / or molded parts thereof, having an average particle size D50 of 1 mm or less.
2. 2. The TPU powder according to claim 1, having an average particle size D50 in the range of 1 μm to 1 mm.
3. 3. The TPU powder according to claim 1 or 2, having an average particle size D50 in the range of 5 to 800 μm, preferably 10 to 500 μm.
4. Bulk density is 1 g / cm 3 Less than 0.8 g / cm 3 or less than 0.6 g / cm 3 3. The TPU powder according to claim 1, wherein:
5. 3. The TPU powder according to claim 1 or 2, derived from expanded TPU pellets or molded parts thereof or residual expanded TPU or reclaimed expanded TPU, or a mixture thereof.
6. 3. Use of the expanded TPU and / or its molded parts for producing the TPU powder according to claim 1 or 2.
7. 3. A method for preparing the TPU powder according to claim 1 or 2, comprising atomizing the expanded TPU and / or its molded parts.
8. 10. A powder composition comprising the TPU powder according to claim 1 and at least one adjuvant, preferably chosen from fillers, flow agents and pigments.
9. 10. Use of the TPU powder according to claim 1 or the powder composition according to claim 8 for preparing a 3D moulded body.
10. 9. A method for preparing a 3D moulded body comprising using the TPU powder according to claim 1 or the composition according to claim 8.
11. The following steps: a) adding the TPU powder according to claim 1 or the composition according to claim 8 to a molding mixture, and b) Producing a molded article by selectively bonding the powder. The method of claim 10, comprising:
12. 12. The method of claim 11, wherein the compact produced in step b) is produced by a process of building a three-dimensional object layer-by-layer by selectively bonding portions of a powder onto other portions of a powder.
13. 12. The method of claim 11, wherein selectively bonding comprises selective laser sintering, selective inhibition of powder bonding, multi-jet fusion, rapid sintering, 3D printing, or microwave processes.
14. 9. A 3D moulded body formed from the TPU powder of claim 1 or the composition of claim 8.
15. 15. The 3D molded body of claim 14, including soles, outerwear, fabrics, footwear, toys, mats, tires, hoses, gloves and seals.
16. Density is 1 g / cm 3 Less than 0.95 g / cm 3 or less, more preferably 0.9 g / cm 3 15. The 3D molded body according to claim 14, wherein:
17. 15. The 3D moulded body according to claim 14, having a rebound resilience according to ASTM D2632 of at least 35%, preferably at least 40%, more preferably at least 42%.
18. 15. The 3D moulded body according to claim 14, having an elongation at break according to ISO 527-21 / A15 2012 of at least 50%, preferably at least 80%, more preferably at least 100% or at least 120%.