Method for promoting phase separation in polymer solutions and method for preparing olefin polymers
By applying perturbations within specific Reynolds number ranges, the method addresses energy inefficiencies in polymer solution phase separation, achieving faster and more cost-effective phase separation.
Patent Information
- Application Number
- JP2024525086
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for liquid-liquid phase separation of polymer solutions in solution polymerization processes are energy-intensive and costly, with high energy consumption and inefficient phase separation due to reliance on standing time and inadequate perturbation techniques.
Applying perturbations to polymer solutions within specific Reynolds number ranges (0.2 to 30) through heat treatment and mechanical means, such as shear forces, to facilitate phase separation into clear and concentrated liquid phases, reducing energy and material consumption.
The method significantly reduces phase separation time and energy/material consumption by up to 40% compared to conventional techniques, enhancing phase separation efficiency.
Smart Images

Figure 2024537473000001_ABST
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field] The present invention is in the field of polymer preparation and relates to a method for promoting phase separation of a polymer solution, as well as a corresponding method for phase separation of a polymer solution and a method for preparing an olefin polymer.
[0002] [Background technology] Solution polymerization process occupies an important position in the polymer material industry. This process can be used to manufacture various products including fibers, rubber, plastics, elastomers, coatings and adhesives. However, the separation of polymers in the polymer solution produced by solution polymerization is more complicated than other processes. Currently, it is common to pass steam through the polymer solution to decompose and remove catalyst residues, and then separate the polymer through a condensation stripping operation, which finally removes the solvent, unreacted monomers, residual small amounts of water and other volatile components, and the polymer is made into a porous small particle product for subsequent drying treatment, while the solvent is recovered in a recovery device for recycling.
[0003] In the prior art, there are also processes that use liquid-liquid separation to separate polymer solutions. Polymer solutions can exhibit the phenomenon of lower critical solution temperature (LCST), also known as the minimum cosolubility temperature. When the temperature of a homogeneous polymer solution is increased and reaches a certain temperature point, it forms two liquid phases, called a clear liquid phase and a concentrated liquid phase. The concentrated liquid phase contains most of the polymer, and the clear liquid phase contains only a small amount of polymer.
[0004] CN107614541A discloses a continuous solution polymerization process, in which the polymer solution can be heated or cooled to a temperature within 50°C of the solvent's critical temperature, after which the polymer solution passes through a pressure relief valve into a liquid-liquid separator, and the process can reduce or increase the pressure of the polymer solution to within 50 psig of the critical pressure, separating the polymer solution into two liquid phases. The upper dilute phase contains very little polymer, while the lower concentrated phase is concentrated with polymer, reducing the energy required for subsequent solvent separation.
[0005] Summary of the Invention The object of the present invention is to overcome the limitations of the prior art when carrying out liquid-liquid phase separation of polymers in a polymer solution, and the drawbacks of high energy consumption and high cost, and to provide a novel method useful for promoting phase separation of a polymer solution, a method for phase separation of a polymer solution, and a method for preparing an olefin polymer.
[0006] In order to achieve the above object, according to a first aspect of the present invention, there is provided a method for promoting phase separation of a polymer solution, comprising applying a perturbation to the polymer solution in a phase separation apparatus for liquid-liquid phase separation of the polymer solution into a clear liquid phase and a concentrated liquid phase, such that the Reynolds number at any location in the polymer solution except for the boundary layer is greater than 0.2 and less than a critical Reynolds value, the critical Reynolds value being in the range of 1 to 30. Thus, in an exemplary embodiment, the method comprises subjecting at least a portion of the polymer solution to a heat treatment under a flow such that the polymer solution is separated into a clear liquid phase and a concentrated liquid phase, wherein the Reynolds number of the flow of the polymer solution is in the range of 0.2 to 30.
[0007] Without being limited to known theories, the inventors have found that phase separation of a polymer solution can be promoted by making the polymer solution satisfy the specific Reynolds number requirement proposed in the present invention. However, in practical operation, the requirement of a specific Reynolds number needs to take into account the influence of factors such as boundary layers. The boundary layer has a meaning well known in the art, and generally refers to the presence of a fluid layer having a large velocity gradient due to the influence of a solid boundary in the vicinity of the interface between a solid and a fluid (such as the wall surface of a phase separation device). The distance from the interface to the point where the flow velocity does not change is called the boundary layer thickness, the region beyond the boundary layer thickness is called the mainstream region, and the flow velocity in the mainstream region is called the mainstream velocity. According to the Blasius equation, the boundary layer thickness is expressed by Re -1 / 2 Since the boundary layer thickness is proportional to the velocity, a person skilled in the art can specifically determine the boundary layer thickness for each case. In the present invention, the point where the velocity reaches 0.99 times the main velocity is used as the upper limit of the boundary layer thickness.
[0008] Thus, taking into account the effects of the boundary layer, in one embodiment of the present invention, in the phase separation device, from a macroscopic perspective, at least 75% by volume of the polymer solution meets the specific Reynolds number requirement of the present invention, preferably at least 85%, at least 90%, at least 95%, at least 98%, at least 99%, at least 99.5%, or even if the effects of the boundary layer are small, substantially the entire polymer solution meets the specific Reynolds number requirement of the present invention.
[0009] Preferably, the polymer solution is thermally perturbed by heat treatment and / or mechanically perturbed by mechanical means.
[0010] Preferably, the perturbation is applied in the phase separation apparatus before the polymer solution enters the phase separation apparatus and / or while the polymer solution is being fed into the phase separation apparatus.
[0011] Preferably, at least a portion of the polymer solution is subjected to mechanical perturbation by the action of a shear force, for example, the heat treatment is carried out under the action of a shear force τ, so that the polymer solution is separated into a clear liquid phase and a concentrated liquid phase, where the shear force τ satisfies the following formula: 0.3×μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 ×ρ) Preferably, the following formula is satisfied: 5×μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 ×ρ) (I) where μ is the viscosity of the polymer solution before phase separation, in Pa s. D is the diameter of the phase separation vessel in m; ρ is the density of the polymer solution before phase separation, in kg / m 3 It is.
[0012] Preferably, τ satisfies the following formula: 20×μ 2 / (D 2 ×ρ)<τ<120×μ 2 / (D 2 ×ρ) (II).
[0013] Preferably, the mechanical perturbation is applied by stirring.
[0014] Preferably, the mechanical perturbation is applied during or after the heat treatment.
[0015] Preferably, the perturbation is applied by one or more of the following methods: A heat treatment is performed before the phase separation device, and one or more mechanical perturbations are applied selected from the following: a mechanical perturbation is applied in a heat treatment device before the phase separation device, a mechanical perturbation is applied in a pipe that conveys the polymer solution to the phase separation device, a mechanical perturbation is applied during the process of feeding the polymer solution into the phase separation device, and a mechanical perturbation is applied in the phase separation device; and A heat treatment is carried out in the phase separator, and a mechanical perturbation is applied in the phase separator.
[0016] Preferably, the entire polymer solution is heat treated under shear force.
[0017] Preferably, the heat treatment of the polymer solution is carried out under stirring.
[0018] Preferably, the polymer solution is a polymer solution obtained by a solution polymerization process.
[0019] Preferably, the polymer concentration in the polymer solution is 5 to 20 wt %, more preferably 6 to 15 wt %.
[0020] Preferably, the polymer in the polymer solution is selected from one or more of plastics, rubbers, and thermoplastic elastomers.
[0021] Preferably, the plastic is selected from one or more of polyethylene, polypropylene, polybutylene, copolymers of ethylene and one or more alpha-olefins, and copolymers of propylene and one or more alpha-olefins.
[0022] Preferably, the rubber is selected from one or more of butadiene-styrene rubber, butadiene rubber, isoprene rubber, and styrene-isoprene rubber.
[0023] Preferably, the thermoplastic elastomer is selected from one or more of copolymers of ethylene and one or more α-olefins, copolymers of propylene and one or more α-olefins, and copolymers of ethylene and one or more cyclic olefins, copolymers of ethylene and one or more cyclic olefins, copolymers of ethylene and one or more α-olefins and optionally a non-conjugated diene, butene-ethylene copolymers, styrene-butadiene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers.
[0024] Preferably, the solvent in the polymer solution is selected from one or more of C5 to C10 linear or branched alkanes, C5 to C10 cycloalkanes, and C6 to C20 aromatic hydrocarbons.
[0025] Preferably, the solvent in the polymer solution is selected from one or more of n-pentane, isopentane, cyclopentane, n-hexane, isohexane, cyclohexane, methylcyclohexane, n-heptane, 2-methylheptane, n-octane, isooctane, mixed octanes, benzene, toluene, o-xylene, m-xylene and p-xylene.
[0026] According to one embodiment of the present invention, for the heat treatment performed in the phase separation apparatus, the heat treatment temperature is preferably within the range of the lower critical solution temperature of the polymer solution ±50°C, and more preferably, the heat treatment temperature is within the range of the lower critical solution temperature of the polymer solution -50°C.
[0027] More preferably, the polymer solution is subjected to heat treatment under stirring in a phase separator.
[0028] Preferably, the heat treatment temperature is 100 to 300° C. and the heat treatment pressure is 10 to 50 bar.
[0029] Preferably, the polymer concentration in the clear liquid phase is less than 1 wt % and the polymer concentration in the concentrated liquid phase is 8 to 50 wt %; Preferably, the polymer concentration in the concentrated liquid phase is 1.35 times or more, more preferably 1.8 times or more, and even more preferably 2.0 times or more, the polymer concentration in the polymer solution.
[0030] According to a second aspect of the present invention there is provided a method for phase separation of a polymer solution, the method comprising the steps of: 1) promoting phase separation of a polymer solution by the method for promoting phase separation of a polymer solution according to the present invention; 2) Separating the clear liquid phase from the concentrated liquid phase.
[0031] According to a third aspect of the present invention there is provided a method for preparing an olefin polymer, the method comprising the steps of: (A) providing a catalyst system into a polymerization reactor and contacting it with one or more olefin monomers and, optionally, hydrogen to polymerize olefins to obtain a polymerization reaction mixture; (B) The phase separation of the polymerization reaction mixture in step A is carried out by the method for phase separation of a polymer solution of the present invention.
[0032] Compared with the prior art, the present invention has the following features: By performing heat treatment under specific Reynolds number conditions, the present invention can lower the temperature for phase separation of the solution and shorten the time for phase separation of the solution, compared to conventional techniques in which phase separation is performed only by heat treatment. The material and energy consumption of the entire process are reduced by approximately 20 to 40%, respectively, compared to conventional techniques.
[0033] [Figure Description] The drawings are used to provide further understanding of the present invention and constitute a part of this specification. Together with the following specific embodiments, the drawings are used to explain the present invention but are not intended to limit the present invention. In the drawings, FIG. 1 is a schematic diagram of the spiral coil of the spiral coil heat exchanger used in Examples II.1 to II.12.
[0034] FIG. 2 is a schematic diagram of the pipeline structure of the Chinese knot heat exchanger used in Examples II.13 to II.15.
[0035] FIG. 3 is a schematic diagram of the internal pipe arrangement of the tubular heat exchanger used in Comparative Examples II.1-2.
[0036] Detailed Description of the Invention The end points of the ranges and any values disclosed herein are not limited to the exact ranges or values, but these ranges or values are understood to include the values approaching such ranges or values.For numerical ranges, the end points of each range, the end points of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges.These numerical ranges are considered to be specifically disclosed herein.
[0037] In the prior art, when the purpose is to separate the phases of a polymer solution, it is generally believed that sufficient settling is one of the important conditions for phase separation. However, after thorough research, the present inventors have found that for the separation of a polymer solution, for example, the separation of rubber or polyolefin elastomers, adding and maintaining a proper perturbation in the solution is more conducive to achieving phase separation. Without being bound by known theories, it is believed that in the case of polymers, a proper perturbation is beneficial for the polymer chains to fully extend, thereby causing faster and clearer stratification. If the perturbation is too weak, problems such as slow stratification or poor stratification effect may occur, and if the perturbation is too strong, problems such as destruction of the phase interface may occur.
[0038] Therefore, after thorough research, the "appropriate" perturbation can be defined by the Reynolds number, based on the fact that the "Reynolds number" is known in the art as a dimensionless value that characterizes the fluid flow state. Specifically, the inventors have found through data statistics that when the Reynolds number of a polymer solution is greater than 0.2, the system may be deformed and prone to phase separation. However, as the Reynolds number of a polymer solution continues to increase, a critical value is reached at which phase interface collapse occurs. In the present invention, this critical value is called the "critical Reynolds value". After further thorough research and detailed statistics, it has been found that the "appropriate" perturbation can be defined by the Reynolds number, based on the fact that ... based on the fact that the Reynolds number of a polymer solution continues to increase, a critical value is reached at which phase interface collapse occurs. In the present invention, this critical value is called the "critical Reynolds value". For thermoplastic elastomers selected from copolymers, copolymers of ethylene, α-olefins and one or more cyclic olefins, copolymers of ethylene, α-olefins and optionally non-conjugated dienes, butene-ethylene copolymers, styrene-butadiene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers, such as ethylene propylene rubber (EPR), polybutadiene rubber (PB), propylene-based elastomers (PBE) or polyolefin-based elastomers (POE), the critical Reynolds value is considered to be in the range of 1 to 30.
[0039] Thus, the present invention provides a method for promoting phase separation of a polymer solution, the method comprising applying a perturbation to a phase separation device for liquid-liquid phase separation of the polymer solution into a clear liquid phase and a concentrated liquid phase such that the Reynolds number at any location in the polymer solution is greater than 0.2 and less than a critical Reynolds value, the critical Reynolds value being in the range of 1 to 30. Thus, in an exemplary embodiment, the method comprises subjecting at least a portion of the polymer solution to a heat treatment under a flow such that the polymer solution is separated into a clear liquid phase and a concentrated liquid phase, wherein the Reynolds number of the flow of the polymer solution is between 0.2 and 30.
[0040] According to one embodiment of the invention, the Reynolds number anywhere in the polymer solution is increased by perturbation to greater than 0.5, or greater than 1. According to one embodiment of the invention, the critical Reynolds value is less than or equal to 20, or less than or equal to 10.
[0041] According to one embodiment of the present invention, the polymer solution is thermally perturbed by heat treatment and / or mechanically perturbed by mechanical means.
[0042] According to one embodiment of the invention, the perturbation is applied in the phase separation device, the perturbation is applied before the polymer solution enters the phase separation device, and / or the perturbation is applied while feeding the polymer solution into the phase separation device.
[0043] According to one embodiment of the present invention, no depressurization step is included before the polymer solution enters the phase separation device, and the polymer solution does not experience significant depressurization in the phase separation device. For example, the pressure of the polymer solution in the phase separation device does not decrease or decreases by 20% or less, preferably by 10% or less, and in some cases, the polymer solution of the present invention may be subjected to a suitable pressure increase before entering the phase separation device and / or in the phase separation device as appropriate, as long as it still meets the requirements of the present invention, especially the requirements regarding the Reynolds number and the critical Reynolds number. Preferably, the pressure of the polymer solution in the phase separation device at steady state decreases by 20% or less compared to the pressure at the outlet of the reactor used for the polymerization reaction of the polymer solution. For example, the pressure of the polymer solution in the phase separation device at steady state may be substantially equal to the pressure at the outlet of the reactor used for the polymerization reaction of the polymer solution.
[0044] In the present invention, the method of phase-separating a part of the polymer solution may be, for example, applying a shear force to the polymer solution, so that the Reynolds number of the flow of the polymer solution becomes 0.2 or more and 30 or less.
[0045] Preferably, the Reynolds number of the flow of the polymer solution is in the range of 0.2 to 30. Specific examples of the Reynolds number of the polymer solution include the following: 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9 ...8, 3.9, 3.1, 3.1, 3.2, 3.3, 3.4, 3.5, 3.7, 3.9, 3.1, 3.2, 3.3, 3.4, 3.5, 3.8, 3.9, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 3.1, 3.2, 3.3, 3.4, 3.5, 3.9, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3. 9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6 .5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0, 15.5, 16.0, 1 6.5, 17.0, 17.5, 18.0, 18.5, 19.0, 19.5, 20.0, 20.5, 21.0, 21.5, 22.0, 22.5, 23.0, 23.5, 24.0, 24.5, 25.0, 25.5, 26.0, 26.5, 27.0, 27.5, 28.0, 28.5, 29.0, 29.5, 30.0 etc.
[0046] In the present invention, it is preferred to apply thermal perturbation to the polymer solution, for example by heat treatment. On the basis of thermal perturbation, the present invention preferably further applies mechanical perturbation to the polymer solution. According to one embodiment of the present invention, mechanical perturbation is carried out during or after heat treatment. Therefore, in one embodiment, it is preferred for the present invention that no mechanical perturbation is carried out before heat treatment.
[0047] Thus, the implementation of mechanical perturbations during heat treatment can be carried out as follows: - carrying out a heat treatment in a phase separator and applying a mechanical perturbation in said phase separator; and In the present case, the mechanical perturbation after the heat treatment can be carried out as follows: - carrying out a heat treatment prior to phase separation and carrying out one or more mechanical perturbations selected from: applying a mechanical perturbation in a heat treatment device prior to a phase separation device, applying a mechanical perturbation in a pipe conveying the polymer solution to a phase separation device, applying a mechanical perturbation while feeding the polymer solution into a phase separation device, and applying a mechanical perturbation within the phase separation device.
[0048] For embodiments in which mechanical perturbation is applied after heat treatment, the various mechanical perturbations exemplified above can be combined with each other. For example, for the purposes of the present invention, perturbation can be performed in one or more of the following ways: (1) performing a heat treatment prior to the phase separation device and applying a mechanical perturbation in the pipeline conveying the polymer solution to the phase separation device; (2) performing a heat treatment prior to the phase separation device and applying a mechanical perturbation while feeding the polymer solution into the phase separation device; (3) Heat treatment is performed before the phase separator and mechanical perturbation is applied within the phase separator; (4) performing a heat treatment before the phase separation device, applying a mechanical perturbation while feeding the polymer solution into the phase separation device, and applying a mechanical perturbation in the phase separation device; (5) Heat treatment is performed before the phase separator, and mechanical perturbation is applied in the equipment where heat treatment is performed before the phase separator.
[0049] According to one embodiment of the present invention, the heat treatment before the phase separator is carried out by a heat exchanger and / or by applying jacket heating to the pipes connected to the phase separator. For the purposes of the present invention, any suitable combination of different heat treatment means before the phase separator can be carried out.
[0050] According to one embodiment of the present invention, a mechanical perturbation is applied during the feeding of the polymer solution into the phase separation device by feeding the polymer solution through a nozzle or distributor. For the purposes of the present invention, any suitable combination of different mechanical perturbations applied during the feeding process of the phase separation device can be implemented.
[0051] According to one embodiment of the present invention, the heat treatment in the phase separation device is performed by jacket heating and / or built-in heating coils. For the purposes of the present invention, various heat treatment means in the phase separation device can be implemented in any suitable combination.
[0052] According to one embodiment of the present invention, the mechanical perturbation is applied in the phase separation device by applying stirring, providing baffles or providing other stationary parts. For the purposes of the present invention, various means of applying mechanical perturbation in the phase separation device may be combined as appropriate.
[0053] According to one embodiment of the present invention, the mechanical perturbation is applied by placing a component such as a coil / Chinese knot in the device for performing a heat treatment prior to the phase separation device. For the purposes of the present invention, any suitable combination of different means of applying mechanical perturbation in the device for performing a heat treatment prior to the phase separation device can be implemented.
[0054] For the purposes of the present invention, the various heat treatment means before the phase separation apparatus, the various mechanical perturbations applied during the supply to the phase separation apparatus, the various heat treatment means within the phase separation apparatus, the various mechanical perturbations applied within the phase separation apparatus, and the means of applying various mechanical perturbations within the equipment for performing the heat treatment before the phase separation apparatus may be implemented in any suitable combination as long as the mechanical perturbations are applied during or after the heat treatment, so that, within the phase separation apparatus, the Reynolds number at any location in the polymer solution is greater than 0.2 and less than the critical Reynolds value, and the critical Reynolds value is in the range of 1 to 30.
[0055] In an exemplary embodiment, the heat treatment is performed in a phase separation device, and the mechanical perturbation is applied in the phase separation device. Preferably, at least a portion of the polymer solution is mechanically disturbed by the action of a shear force τ, for example, the heat treatment is performed under the action of a specific shear force of the present invention, so that the polymer solution is separated into a clear liquid phase and a concentrated liquid phase, and the shear force τ satisfies the following formula: 0.3×μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 ×ρ) Preferably, the following formula is satisfied: 5×μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 ×ρ) (I) where μ is the viscosity of the polymer solution before phase separation, in Pa s. D is the diameter of the phase separation vessel in m; ρ is the density of the polymer solution before phase separation, in kg / m 3 It is.
[0056] According to the present invention, by performing heat treatment under the action of shear force, it is possible to lower the temperature for phase separation of the solution, shorten the time for phase separation of the solution, and significantly reduce the amount of material and energy consumed, compared to conventional techniques in which phase separation is only performed during heat treatment.
[0057] From the viewpoint of further reducing the phase separation time, the material consumption, and the energy consumption, preferably, τ satisfies the following formula: 1×μ 2 / (D 2 ×ρ)<τ<800×μ 2 / (D 2 ×ρ); more preferably, τ satisfies the following formula: 5×μ 2 / (D 2 ×ρ)<τ<600×μ 2 / (D 2 ×ρ); more preferably, τ satisfies the following formula: 10×μ 2 / (D 2 ×ρ)<τ<400×μ 2 / (D 2 ×ρ); more preferably, τ satisfies the following formula: 15×μ 2 / (D 2 ×ρ)<τ<200×μ 2 / (D 2 ×ρ); more preferably, τ satisfies the following formula: 20×μ 2 / (D 2 ×ρ)<τ<120×μ 2 / (D 2 ×ρ).
[0058] According to the present invention, at least a part of the polymer solution is subjected to heat treatment under the action of the specific shear force of the present invention, and preferably, the entire polymer solution is subjected to heat treatment under the action of the specific shear force of the present invention. That is, a part of the polymer solution can be heat treated under the action of the specific shear force of the present invention, or the entire polymer solution can be heat treated under the action of the specific shear force of the present invention. By heat treating the entire polymer solution under the action of a shear force, the phase separation time can be further shortened, and the material consumption and energy consumption can be further reduced.
[0059] According to the present invention, the shear force satisfies the above formula. 2 / (D 2 If the shear force is less than 1000 × μ, the polymer chains cannot be sufficiently stretched due to insufficient perturbation, resulting in slower interlayer separation or poor interlayer separation effect. 2 / (D 2 × ρ), the perturbation is too strong and the phase boundary is destroyed.
[0060] According to the present invention, the shear force can be achieved by equipment that can generate shear force generally in the art, preferably an agitator. That is, the heat treatment of the polymer solution is preferably carried out under stirring. The agitator may be any type of agitator, preferably one or more of a paddle agitator, an anchor agitator, a helical ribbon agitator and a gate agitator. One or more agitators may be used.
[0061] Furthermore, the agitator can be inserted into the phase separation vessel in a central top insertion type, an eccentric top insertion type, a bottom insertion type, a side insertion type, an oblique insertion type, etc. Examples of the seal form of the agitator include a mechanical seal, a packing seal, a magnetic seal, etc.
[0062] In a preferred embodiment of the present invention, one or more baffles or guide tubes can be disposed in the phase separation vessel to enhance the stirring effect.
[0063] In another exemplary embodiment, heat treatment is performed before the phase separation device, and mechanical perturbation is applied in the device for performing heat treatment before the phase separation device, so that the polymer solution is kept in a state of being disturbed and heated while being fed into the phase separation tank.Preferably, for example, the polymer solution is conveyed to a heat exchanger having a heating function and capable of disturbing the flow of the polymer solution, and then heat treatment is performed before the phase separation device, and then the polymer solution is sent to the phase separation tank for separation.
[0064] As in the above heat exchanger, it is preferable to provide a protrusion capable of disturbing the flow of the liquid in the pipe of the polymer solution flow path in the heat exchanger. Such a protrusion may have a rod-like, plate-like, disk-like, cylindrical or other shape, for example, a crushing rod, a baffle, or the like, and may be fixed to the pipe joint at any angle and in any manner.
[0065] The heat exchanger can also be a Chinese knot heat exchanger and / or a spiral coil heat exchanger having a complex structure in the heat exchanger. By using the Chinese knot heat exchanger and / or the spiral coil heat exchanger, the polymer solution can be sufficiently stirred and heated while being fed into the phase separation tank, so that the time for phase separation of the solution can be shortened, and the material and energy consumption of the entire process can be reduced.
[0066] According to one embodiment of the present invention, the heat exchanger with heating function is a Chinese knot heat exchanger equipped with a "Chinese knot" type pipe joint, in which the polymer solution passes through the "shell" layer, and the heat medium such as steam or hot oil passes through the "pipe" layer.
[0067] The Chinese knot heat exchanger with "Chinese knot" type pipe joints refers to the following: the internal pipes of the heat exchanger are bent in the shell in the manner of Chinese knots into multiple Chinese knots, and the angle of the pipes at the bent parts can be appropriately selected, for example, can be 45 degrees or 135 degrees.
[0068] Preferably, the internal pipe of the Chinese knot heat exchanger is bent into a plurality of Chinese knots, more preferably into 1 to 5 Chinese knots, and even more preferably into 2 to 3 Chinese knots.
[0069] Examples of Chinese knot numbers include: 1, 2, 3, 4, 5, etc.
[0070] According to one embodiment of the present invention, the heat exchanger with heating function is a spiral coil heat exchanger equipped with a spiral disk pipe joint, in which the polymer solution passes through the "shell" layer, and the heat medium such as steam or hot oil passes through the "pipe" layer.
[0071] Preferably, the pipe of the spiral coil heat exchanger is spirally bent to form a plurality of spirals, more preferably 3 to 20 spirals, even more preferably 4 to 15 spirals, and even more preferably 5 to 10 spirals.
[0072] Examples of spiral numbers include: 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, etc.
[0073] The heat treatment before the phase separation device allows the temperature of the polymer solution when fed into the phase separation tank to be the temperature of phase separation. The temperature of phase separation can be, for example, in the range of the lower critical solution temperature of the polymer solution ±50°C, more preferably, the temperature of phase separation is in the range of the lower critical solution temperature of the polymer solution ±30°C, and even more preferably, the temperature of phase separation is in the range of the lower critical solution temperature of the polymer solution ±20°C.
[0074] Specifically, the heat treatment makes it possible to adjust the temperature of the polymer solution to 100 to 300°C, preferably 110 to 250°C, and more preferably 120 to 200°C when it is supplied into the phase separation tank.
[0075] According to the present invention, the polymer solution can be various polymer solutions commonly used in the art for thermal treatment phase separation, for example, the polymer solution can be a polymer solution obtained by a solution polymerization process, such as a homogeneous liquid polymerization system contained in a reactor, or a polymer solution obtained by dissolving a polymer in a liquid, such as an inert solvent or one or more monomers or their blends, and preferably a polymer solution obtained by a solution polymerization process.
[0076] According to the present invention, the solution polymerization process is a polymerization reaction carried out in a solution state by dissolving a monomer in a suitable solvent and adding an initiator (or catalyst) as generally used in the art. The catalyst can be, for example, a Ziegler-Natta catalyst, a transition metal single-site or multi-site catalyst, a rare earth metal catalyst, etc. The catalyst can be dissolved in a solvent or suspended in a solvent. In some embodiments, the catalyst can be used in combination with an electron donor. In other embodiments, the catalyst needs to be used in combination with a cocatalyst such as a boron-containing compound and / or an aluminum alkyl and / or a methylaluminoxane.
[0077] According to the present invention, the solution polymerization temperature can be varied in a wide range, preferably between 45° C. and 200° C. The solution polymerization pressure can be varied in a wide range, preferably between 0.5 and 15 MPa. The solution polymerization process can be batch, semi-continuous or continuous.
[0078] According to the present invention, the polymer concentration in the polymer solution can be changed within a wider range, preferably, the polymer concentration in the polymer solution is 5-20 wt%, more preferably, the polymer concentration in the polymer solution is 6-15 wt%.
[0079] According to the present invention, preferably the polymer in the polymer solution is selected from one or more of plastics, rubbers and thermoplastic elastomers.
[0080] The plastic may be selected, for example, from one or more of polyethylene, polypropylene, polybutylene, copolymers of ethylene and one or more alpha-olefins, and copolymers of propylene and one or more alpha-olefins.
[0081] The rubber may be selected from, for example, one or more of butadiene-styrene rubber, butadiene rubber, isoprene rubber, and styrene-isoprene rubber.
[0082] The thermoplastic elastomer may be selected, for example, from one or more of copolymers of ethylene and one or more α-olefins, copolymers of propylene and one or more α-olefins, copolymers of ethylene and one or more cyclic olefins, copolymers of ethylene, α-olefins and one or more cyclic olefins, copolymers of ethylene, α-olefins and optionally non-conjugated dienes, butene-ethylene copolymers, styrene-butadiene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers.
[0083] Copolymers of ethylene and one or more α-olefins refer to ethylene-based copolymers having a viscosity of about 0.85 to 0.915 g / cm 3 (as determined according to ASTM D4703, Method B and ASTM D1505). The ethylene-based copolymers described herein are copolymers that contain at least about 50% by weight of units derived from ethylene and higher α-olefins, such as propylene, 1-butene, 1-hexene, 1-octene, and the like.
[0084] Copolymers of propylene and one or more α-olefins refer to propylene-based copolymers. The propylene-based copolymers described herein are copolymers that contain at least about 50 wt.% of units derived from propylene and units derived from ethylene, or copolymers that contain at least about 50 wt.% of units derived from propylene and units derived from higher α-olefins, such as 1-butene, 1-hexene, and 1-octene.
[0085] In a preferred embodiment of the invention, the copolymer of ethylene and one or more α-olefins is an EPR, an ethylene-1-butene copolymer elastomer or an ethylene-1-octene copolymer elastomer.
[0086] According to the present invention, preferably, the solvent in the polymer solution is selected from one or more of C5-C10 linear or branched alkanes, C5-C10 cycloalkanes, and C6-C20 aromatic hydrocarbons, and more preferably, the solvent in the polymer solution is selected from one or more of n-pentane, isopentane, cyclopentane, n-hexane, isohexane, cyclohexane, methylcyclohexane, n-heptane, 2-methylheptane, n-octane, isooctane, mixed octanes, benzene, toluene, o-xylene, m-xylene, and p-xylene.
[0087] In some preferred embodiments of the present invention, a metallocene catalyst and a boron-containing compound and / or a methylaluminoxane compound are used as a catalyst system, optionally an alkylaluminum is used as a scavenger, the solution polymerization is carried out in an alkane such as isopentane, n-pentane, n-hexane, cyclohexane and isohexane, and the prepared polymer is a polymer solution of an ethylene-α-olefin copolymer, a propylene-α-olefin copolymer, or an ethylene-propylene and optionally a non-conjugated diene copolymer. In a more preferred embodiment, a metallocene catalyst and a boron-containing compound are used as a catalyst system, optionally an alkylaluminum is used as a scavenger, the solution polymerization is carried out in an alkane such as isopentane, n-pentane or n-hexane, and the prepared polymer is a polymer solution of an ethylene-α-olefin copolymer. In another more preferred embodiment, a metallocene catalyst and a boron-containing compound are used as the catalyst system, an alkylaluminum is used as the scavenger, the solution polymerization is carried out in an alkane such as isopentane, n-pentane or n-hexane, and the prepared polymer is a polymer solution of a propylene-α-olefin copolymer.
[0088] In some preferred embodiments, a nonmetallocene catalyst and a boron-containing compound and / or a methylaluminoxane compound are used as the catalyst system, optionally an alkylaluminum is used as a scavenger, the solution polymerization is carried out in an alkane such as isopentane, n-pentane, n-hexane, cyclohexane, and isohexane, and the prepared polymer is a polymer solution of an ethylene-α-olefin copolymer, a propylene-α-olefin copolymer, and an ethylene-propylene and optionally a non-conjugated diene copolymer. In a more preferred embodiment, a nonmetallocene catalyst, a boron-containing compound, and a methylaluminoxane are used as the catalyst system, the solution polymerization is carried out in an alkane such as isopentane, n-pentane, and n-hexane, and the prepared polymer is a polymer solution of an ethylene-propylene and a non-conjugated diene copolymer.
[0089] In a specific embodiment of the invention, the polymer in the polymer solution is a polyolefin elastomer and the solvent in the polymer solution is a mixture of cyclohexane and n-hexane.
[0090] In another specific embodiment of the present invention, the polymer in the polymer solution is a polyolefin elastomer and the solvent in the polymer solution is a mixture of cyclohexane and n-hexane.
[0091] In another specific embodiment of the present invention, the polymer in the polymer solution is a polyolefin elastomer and the solvent in the polymer solution is n-pentane.
[0092] In another specific embodiment of the present invention, the polymer in the polymer solution is a polyolefin elastomer and the solvent in the polymer solution is isopentane.
[0093] In another specific embodiment of the present invention, the polymer in the polymer solution is a propylene-based elastomer and the solvent in the polymer solution is n-pentane.
[0094] In another specific embodiment of the present invention, the polymer in the polymer solution is a propylene-based elastomer and the solvent in the polymer solution is isopentane.
[0095] In another specific embodiment of the present invention, the polymer in the polymer solution is polybutadiene rubber and the solvent in the polymer solution is a mixture of cyclohexane and n-hexane.
[0096] In another specific embodiment of the present invention, the polymer in the polymer solution is ethylene propylene rubber and the solvent in the polymer solution is a mixture of cyclohexane and n-hexane.
[0097] According to the embodiment of the present invention in which the heat treatment is performed in a phase separation apparatus and the mechanical perturbation is applied in the phase separation apparatus, the temperature of the heat treatment may be in the range of the lower critical solution temperature of the polymer solution ±50°C, and preferably, the temperature of the heat treatment is in the range of the lower critical solution temperature of the polymer solution -50°C.
[0098] In the present invention, the temperature at which the solution separates is lowered by performing heat treatment under the action of shear force, as compared with the prior art in which phase separation is performed only by heat treatment. Therefore, in the present invention, heat treatment can be performed at a temperature equal to or lower than the lower critical solution temperature of the polymer solution, shortening the time for phase separation of the polymer solution and reducing the consumption of materials and energy.
[0099] The heat treatment temperature may be, for example, within a range of the lower critical solution temperature of the polymer solution ±50°C, preferably within a range of the lower critical solution temperature of the polymer solution -50°C, more preferably within a range of the lower critical solution temperature of the polymer solution -30°C, and even more preferably within a range of the lower critical solution temperature of the polymer solution -20°C.
[0100] For the purposes of the present invention, the term "a range of ±50°C of the lower critical solution temperature of the polymer solution" refers to a range of -50°C of the lower critical solution temperature of the polymer solution to +50°C of the lower critical solution temperature of the polymer solution, the term "a range of -50°C of the lower critical solution temperature of the polymer solution" refers to a range of -50°C of the lower critical solution temperature of the polymer solution to the lower critical solution temperature of the polymer solution, the term "a range of -30°C of the lower critical solution temperature of the polymer solution" refers to a range of -30°C of the lower critical solution temperature of the polymer solution to the lower critical solution temperature of the polymer solution, and the term "a range of -20°C of the lower critical solution temperature of the polymer solution" refers to a range of -20°C of the lower critical solution temperature of the polymer solution to the lower critical solution temperature of the polymer solution. Since the type of a specific polymer solution is different, the lower critical solution temperature of a specific polymer solution is also different. Therefore, the range is different depending on the type of polymer solution.
[0101] The "lower critical solution temperature of a polymer solution" is well known in the art and can be determined, for example, by a turbidity method. For details, see Wu Qi, "Polymer Solution", Higher Education Press, 2021, pp. 424-431.
[0102] According to an embodiment of the present invention in which heat treatment is performed in a phase separation apparatus and mechanical perturbation is applied in the phase separation apparatus, the heat treatment in the phase separation apparatus can be performed in a vessel capable of performing heat treatment phase separation generally in the art. For example, the phase separation vessel may be a sealed vessel capable of withstanding high temperature and pressure, such as a vertical vessel, a horizontal vessel, a rectangular vessel, etc., and the header may have a flat header, an elliptical header, a cone bottom, etc., and may or may not have a jacket through which a heat transfer medium such as hot oil or steam passes.
[0103] According to the above-mentioned embodiment, the temperature and pressure of the heat treatment in the phase separation apparatus can be selected according to the lower critical solution temperature of the polymer solution, but generally, the heat treatment temperature can be 100 to 300° C., and the heat treatment pressure can be 2 to 50 bar. The heat treatment temperature is more preferably 120 to 280° C., and even more preferably 120 to 180° C., and the heat treatment pressure is more preferably 3 to 20 bar, and even more preferably 3 to 10 bar.
[0104] According to this embodiment, preferably, after carrying out the phase separation according to the invention, the polymer concentration in the clear liquid phase is less than 1 wt %, and the polymer concentration in the concentrated liquid phase is 8-50 wt %.
[0105] Specifically, the polymer concentration in the concentrated liquid phase is more than 1.35 times, more preferably more than 1.8 times, even more preferably more than 2.0 times, even more preferably less than 10 times, more preferably less than 5 times, even more preferably less than 4 times, even more preferably less than 3.5 times the polymer concentration in the polymer solution.
[0106] According to an embodiment of the present invention in which heat treatment is performed before the phase separation apparatus and mechanical perturbation is applied in the apparatus for heat treatment before the phase separation apparatus, the temperature and pressure of phase separation can be selected according to the lower critical solution temperature of the polymer solution, but usually, the temperature of phase separation can be 100 to 300 ° C, and the pressure of phase separation can be 2 to 50 bar. Moreover, the temperature of phase separation is more preferably 120 to 280 ° C, more preferably 120 to 180 ° C, and the pressure of phase separation is more preferably 3 to 20 bar, more preferably 3 to 10 bar. Furthermore, the time of phase separation is preferably within 60 minutes, more preferably 5 to 45 minutes, more preferably 7 to 30 minutes.
[0107] According to this embodiment, preferably, after carrying out the phase separation according to the present invention, the polymer concentration in the clear liquid phase is less than 1 wt%, more preferably less than 0.5 wt%, and the polymer concentration in the concentrated liquid phase is 10 wt%, preferably more than 15 wt%, more preferably more than 18 wt%, and even more preferably 25 to 50 wt%.
[0108] The present invention also provides a method for phase separation of a polymer solution, the method comprising the steps of: 1) promoting phase separation of a polymer solution by using the method for promoting phase separation of a polymer solution according to the present invention; 2) Separating the clear liquid phase from the concentrated liquid phase.
[0109] According to the present invention, the separation method is not particularly limited, and various methods commonly used in the art for separating a clear liquid phase from a concentrated liquid phase can be adopted, and will not be described in detail in this specification.
[0110] According to yet another aspect of the present invention, there is provided a method for preparing an olefin polymer, the method comprising the steps of: (A) providing a catalyst system into a polymerization reactor and contacting it with one or more olefin monomers and, optionally, hydrogen to polymerize olefins to obtain a polymerization reaction mixture; (B) The polymerization reaction mixture of step A is phase-separated by using the method for phase separation of a polymer solution of the present invention.
[0111] According to the preparation method of the present invention, the method further comprises the steps of: recovering a concentrated liquid phase from the phase-separated solution obtained in step B, and devolatilizing the concentrated liquid phase to obtain a polymer.
[0112] The main improvement of the method for preparing an olefin polymer of the present invention is to carry out phase separation of the polymerization reaction mixture obtained by the polymerization reaction. As the monomers, solvents, post-treatment methods and conditions used in the polymerization, various monomers, solvents, post-treatment methods and conditions generally used in this field can be used.
[0113] For example, olefin monomers can include ethylene, propylene, butylene, pentene, octene, butadiene, isoprene, styrene, and the like.
[0114] In a preferred embodiment of the present invention, step A comprises feeding the catalyst system to a polymerization reactor and contacting it with one or more olefinic ethylene and / or propylene monomers, optionally one or more comonomers, and optionally hydrogen to carry out polymerization of olefins and obtain a polymerization mixture.
[0115] Examples of such comonomers include 1-butene, 1-hexene, 1-octene, and the like.
[0116] Examples of such olefin polymers include one or more of the plastics, rubbers, and thermoplastic elastomers listed above.
[0117] According to the present invention, by performing heat treatment under specific Reynolds number conditions, it is possible to lower the phase separation temperature of the solution, shorten the phase separation time of the solution, and reduce the material consumption and energy consumption of the entire process by about 20 to 40%, respectively, compared to the conventional technology in which phase separation is only performed during heat treatment.
[0118] [Example] The present invention will be described in detail below through examples, but the present invention is not limited to the following examples.
[0119] Unless otherwise specified, the operations and processing methods involved in the present invention are conventional methods in the art.
[0120] Unless otherwise specified, the instruments used in the present invention are conventional instruments in the art.
[0121] Unless otherwise specified, all materials used were commercially available.
[0122] In the examples and comparative examples, ethylene propylene rubber (EPR), polybutadiene rubber (PB), propylene-based elastomer (PBE) or polyolefin-based elastomer (POE) are used as examples, and the solvents are n-pentane (nPN), isopentane (iPN), n-hexane (nHX), and a mixture of cyclohexane and n-hexane (HX, the weight percentage of n-hexane is 80%).
[0123] where POE is an ethylene / octene copolymer prepared using (tert-butylamido)dimethyl(1,2,3,4,5-η)-1,5,6,7-tetrahydro-2-methylindenylsilanetitanium(II) 1,3-pentadiene metal complex (prepared according to USP 5,965,756) and tris(pentafluorophenyl)borane cocatalyst and triisobutylaluminum scavenger in a molar ratio of Ti:B:Al of 1:3:1, and the density of POE is 0.868 g / cm 3 The weight average molecular weight is 130,000, the molecular weight distribution is 2.0, and the ethylene mass fraction is 60 to 62%.
[0124] PBE is a propylene / ethylene copolymer prepared by using dimethylsilylbis(5,6,7,8-tetrahydro-2,5,5,8,8-pentamethylbenzindenyl)dimethylhafnium (prepared according to US60 / 586465) with commercially available triphenylcarbonium tetrakis(pentafluorophenyl)boron compound and triisobutylaluminum scavenger in a molar ratio of Hf:B:Al of 1:2:1; the density of PBE is 0.87 g / cm. 3 The weight average molecular weight is 120,000, the molecular weight distribution is 2.1, and the ethylene mass fraction is 12 to 15%.
[0125] EPR is an ethylene / propylene copolymer prepared using bis((2-oxy-3-(dibenzo-1H-pyrrol-1-yl)-5-(methyl)phenyl)-2-phenoxy)-1,3-propanediylzirconium(IV) dichloride (prepared according to CN102786619B) and commercially available methylaluminoxane solution in a molar ratio of Zr:B:Al of 1:2:1; the density of EPR is 0.87 g / cm. 3 The weight average molecular weight is 120,000 and the molecular weight distribution is 2.1.
[0126] For the preparation method of PB, reference can be made to Example 1 of CN1093375A, and a polybutadiene rubber with a weight average molecular weight of 390,000 and a molecular weight distribution of 3.8 can be obtained.
[0127] In the following example, the amount of paste entering the heating tank with stirring paddles is 3.1 L. The dynamic equipment that provides the shear force is a four-blade inclined paddle mixer with a blade inclination angle of 45 degrees and a blade diameter of 0.05 m. The heating tank is a phase separation vessel, and uses thermal oil in the jacket for heating, with an inner diameter of 0.15 m.
[0128] Examples I.1 to 17 and Comparative Examples I.1 to 4 The polymer solution was transported to the phase separation heating tank by a gear pump. When the pressure in the phase separation heating tank rose to a specified pressure, the polymer solution was started to be heated and stirred. When the temperature reached 110°C or higher, the temperature was held for 10 minutes for every 5°C rise due to heating to observe whether there was a tendency for phase separation, and the pressure was kept constant during heating. Timing was started when the temperature reached the point where phase separation occurred, and the time was calculated. After phase separation was completed, samples were taken from the top and bottom, and poured into ethanol three times the amount of the sample. The precipitated polymer was removed and baked at 80°C for 24 hours, after which the weight was measured and the concentration of the paste was calculated.
[0129] The Reynolds number was calculated as follows: - The density of the polymer solution was measured as follows: a 100 ml pressure-resistant steel cylinder was used to take the sample and the weight was measured. After the weight measurement, the weight of the empty cylinder was subtracted to obtain the weight of the polymer solution, and then the weight of the polymer solution was divided by the volume of the cylinder to obtain the density of the polymer solution. The viscosity and shear rate of the polymer solution under the experimental conditions were measured with a rotational rheometer HAAKE RS6000 (Thermo Fisher Scientific, USA).
[0130] - The Reynolds number Re is calculated by the formula Re=d 2 × N × ρ / μ, where D is the diameter of the agitator (m) and N is the rotation speed (s -1 ), μ is the viscosity of the polymer solution before phase separation (Pa s), and ρ is the density of the polymer solution before phase separation (kg / m 3 The shear force τ was calculated by the formula τ = μ × Vs, where μ is the viscosity of the polymer solution before phase separation (Pa s) and Vs is the shear rate (s -1 ) and Vs = π × d × μ / (1 / 2 × (Dd)).
[0131] The conditions of the examples are shown in Table 1. The operation steps of the comparative examples were almost the same as those of the examples, except for the stirring. The conditions of the comparative examples are also shown in Table 1.
[0132] [Table 1]
[0133] Comparing Examples I.1 to I.17 with Comparative Examples I.1 to I.2, the Reynolds number is in the range of 0.2 to 30, and the shear force is 0.3 × μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 × ρ), the time for phase separation of the solution is shortened, and the material and energy consumption of the entire process are significantly reduced, compared to the conventional technique in which phase separation is performed only by heat treatment.
[0134] Comparing Examples I.1 to I.3 with Comparative Example I.1, and comparing Examples with Comparative Example I.2, the Reynolds number is in the range of 0.2 to 30, and the shear force is 0.3 × μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 × ρ), not only is the time for phase separation of the solution shortened, but the material and energy consumption of the entire process is significantly reduced, and the polymer concentration in the concentrated phase is increased, compared to the conventional technology in which phase separation is performed only by heat treatment.
[0135] Comparing Example I.11 with Comparative Example I.3, the Reynolds number is in the range of 0.2 to 30, and the shear force is 0.3 × μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 × ρ), not only is the time for phase separation of the solution shorter, but the material and energy consumption of the entire process is significantly reduced, and the concentration of the concentrated phase polymer is increased, compared to when the shear stress and Reynolds number are not within the above ranges.
[0136] Comparing Example I.16 with Comparative Example I.4, the Reynolds number is in the range of 0.2 to 30, and the shear force is 0.3 × μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 × ρ) the polymer solution can undergo phase separation in a relatively short time, whereas when the shear stress and Reynolds number exceed these ranges, the polymer solution cannot undergo phase separation.
[0137] From the above, it can be seen that the method proposed by the present invention can lower the phase separation temperature and shorten the phase separation time during the phase separation of the polymer solution, thereby reducing the energy consumption and steam consumption compared with the prior art, greatly reducing the production cost, and increasing the polymer concentration in the concentrated phase.
[0138] Examples II.1 to II.12 The polymer solution was fed into a spiral coil heat exchanger (heat exchanger shell size is φ159mm×500mm, BEM type, built-in spiral coil is as shown in Fig. 1, total length of spiral pipe in heat exchanger is 2m, pipe diameter is 2mm, number of spirals is 5) and heat exchange was performed (polymer solution passes through shell side, heat transfer oil passes through pipe side as heat transfer medium). After heat exchange, polymer solution was sent to phase separation tank for phase separation. The polymer and its concentration, solvent of polymer solution, outlet temperature of heat exchanger, phase separation condition, polymer concentration of clear phase, and polymer concentration of concentrated phase are shown in Table 1.
[0139] The Reynolds number was calculated as follows: - The density of the polymer solution was measured as follows: a 100 ml pressure-resistant steel cylinder was used to take the sample and the weight was measured. After the weight measurement, the weight of the empty cylinder was subtracted to obtain the weight of the polymer solution, and this weight was divided by the volume of the cylinder to obtain the density of the polymer solution. The viscosity of the polymer solution under the experimental conditions was measured with a rotational rheometer HAAKE RS6000 (Thermo Fisher Scientific, USA).
[0140] - The Reynolds number Re is calculated by the formula Re=ρvd / μ, where d is the characteristic length (m), which means the shortest radial distance through which the fluid flows under static perturbation. μ is the viscosity of the polymer solution before phase separation (Pa s). ρ is the density of the polymer solution before phase separation (kg / m 3 ) v is the flow velocity of the polymer solution (m / s).
[0141] Examples II.13 to 15 The polymer solution was fed into a Chinese knot heat exchanger (heat exchanger shell size is φ159mm×500mm, BEM type, built-in Chinese knot pipeline is as shown in Fig. 2, total pipe length in the heat exchanger is 2.7m, pipe is bent in the shell to make two Chinese knots in the manner of Chinese knot, pipe angle of the bent part is 45 degrees or 135 degrees, pipe diameter is 2mm) and heat exchange was performed (polymer solution passes through the shell side, heat transfer oil passes through the pipe side as heat transfer medium). After heat exchange, the polymer solution was sent to the phase separation tank and phase separation was performed. The polymer and its concentration, solvent of the polymer solution, outlet temperature of the heat exchanger, phase separation conditions, polymer concentration in the clear phase, and polymer concentration in the concentrated phase are shown in Table 1.
[0142] Examples II.16-17 These examples were carried out according to the protocol of Example II.1, except that the spiral coil heat exchanger had a heat exchanger shell size of φ159 mm × 800 mm, BEM type, the total length of the spiral pipe in the heat exchanger was 4 m, the pipe diameter was 2 mm, and the number of spirals was 10. The polymers and their concentrations, the solvent of the polymer solution, the outlet temperature of the heat exchanger, the phase separation conditions, the polymer concentrations in the clear phase, and the polymer concentrations in the concentrated phase are shown in Table 1.
[0143] Examples II.18-19 These examples were carried out according to the protocol of Example II.13, except that the heat exchanger shell size of the Chinese knot heat exchanger was φ159mm×800mm, it had a BEM type, Chinese knot pipeline built in, the total length of the pipe in the heat exchanger was 4.2m, the pipe was bent inside the shell in the manner of Chinese knot to make three Chinese knots, the angle of the pipe in the bent part was 45° or 135°, and the diameter of the pipe was 2mm. The polymer and its concentration, the solvent of the polymer solution, the outlet temperature of the heat exchanger, the phase separation conditions, the polymer concentration in the clear phase, and the polymer concentration in the concentrated phase are shown in Table 1.
[0144] In the above examples, the method for measuring the time of phase separation was as follows: The polymer concentration and phase separation time were measured by starting the measurement from the time the mixture entered the phase separation tank and calculating the time. After the phase separation was completed, samples were taken from the top and bottom, and poured into ethanol in an amount three times the amount of the sample. The precipitated polymer was removed and baked at 80°C for 24 hours, after which the weight was measured and the concentration of the paste was calculated.
[0145] [Table 2]
[0146] From Examples II.1-15, it can be seen that the temperature of phase separation of the solution is reduced, the time of phase separation of the solution is within 35 minutes, and the residence time of the polymer at high temperature until the catalyst is deactivated can be effectively avoided. From Examples II.16-17, it can be seen that increasing the length of the spiral pipe and the number of spirals can further shorten the time of phase separation and further increase the polymer concentration in the concentrated phase. From Examples II.1, 8-19, it can be seen that increasing the total length of the pipe and the number of Chinese knots can further shorten the time of phase separation and further increase the polymer concentration in the concentrated phase.
[0147] Examples II.20 to 25 The polymer solution was fed into a tubular heat exchanger (heat exchanger shell size is φ159mm×500mm, BEM type, the arrangement of built-in pipes is as shown in Figure 3, the pipes in the heat exchanger are arranged in one pass, each pipe is 500mm long and 20mm in diameter) to carry out heat exchange (polymer solution passes through the pipe side, and heat transfer oil as heat transfer medium passes through the shell side). After heat exchange, the polymer solution was sent to a phase separation tank, where phase separation was carried out through a pipe with five sets of baffles (4.5mm×3mm) symmetrically installed inside. The polymer and its concentration, the solvent of the polymer solution, the outlet temperature of the heat exchanger, the phase separation conditions, the polymer concentration in the clear phase, and the polymer concentration in the concentrated phase are shown in Table II.2.
[0148] The Reynolds number Re was determined in the same manner as in Examples II.1 to II.19.
[0149] [Table 3]
[0150] From Examples II.20-25, it can be seen that the time for phase separation of the solution is within 45 minutes, thereby shortening the residence time of the polymer at high temperature.
[0151] Although the preferred embodiments of the present invention have been described in detail above, the present invention is not limited to the specific contents of the above embodiments. Within the scope of the technical idea of the present invention, various simple modifications can be made to the technical solutions of the present invention, and all of these simple modifications belong to the protection scope of the present invention.
[0152] Furthermore, it should be noted that each of the specific technical features described in the above specific embodiments can be combined in any suitable manner unless there is a contradiction. In order to avoid unnecessary repetition, various possible combinations will not be described further in this specification. In addition, as long as it is not contrary to the concept of the present invention, any combination of various embodiments of the present invention is also possible, and they should also be considered as the disclosure of the present invention. [Brief description of the drawings]
[0153] [Figure 1] FIG. 1 is a schematic diagram of the spiral coil of the spiral coil heat exchanger used in Examples II.1 to II.12. [Diagram 2] FIG. 1 is a schematic diagram of the pipeline structure of the Chinese knot heat exchanger used in Examples II.13 to 15. [Diagram 3] FIG. 1 is a schematic diagram of the internal pipe arrangement of the tubular heat exchanger used in Comparative Examples II.1-2.
Claims
1. A method for promoting phase separation of a polymer solution, comprising: in a phase separation apparatus for liquid-liquid phase separation of a polymer solution into a clear liquid phase and a concentrated liquid phase, disturbance is applied to the polymer solution so that the Reynolds number at any location except for a boundary layer in the polymer solution is greater than 0.2 and smaller than a critical Reynolds value, the critical Reynolds value being in the range of 1 to 30.
2. 2. The method of claim 1, wherein the polymer solution is perturbed such that the Reynolds number anywhere in the polymer solution is greater than 0.5, or greater than 1, and / or the critical Reynolds value is 20 or less, or 10 or less, and the critical Reynolds value is 2.5 or more, or 3 or more, or 4.5 or more.
3. The method of claim 1 , wherein the polymer solution is thermally disturbed by heat treatment and / or mechanically disturbed by mechanical means.
4. 4. The method of claim 1, wherein the agitation is added in the phase separation apparatus, the agitation is added before the polymer solution enters the phase separation apparatus, and / or the agitation is added while feeding the polymer solution into the phase separation apparatus.
5. 5. The method according to any one of claims 1 to 4, wherein no depressurization step is included before the polymer solution enters the phase separation apparatus and the polymer solution does not experience significant depressurization in the phase separation apparatus, e.g. the pressure of the polymer solution in the phase separation apparatus does not decrease or decreases by no more than 20%, preferably no more than 10%, e.g. the pressure of the polymer solution in the phase separation apparatus at steady state decreases by no more than 20% compared to the pressure at the outlet of the reactor used for the polymerization reaction of the polymer solution.
6. The polymer solution is thermally disturbed by a heat treatment, the temperature of the heat treatment is within a range of the lower critical solution temperature of the polymer solution ±50° C., and the pressure of the heat treatment is 10 to 50 bar; A method according to any one of claims 1 to 5, wherein said heat treatment preferably results in a temperature of the polymer solution in said phase separation apparatus of from 100 to 300°C, preferably from 110 to 250°C, more preferably from 120 to 200°C.
7. A mechanical perturbation is applied to some or all of the polymer solution by applying a shear force τ, the shear force τ satisfying the following equation: 5×μ 2 / (D 2 ×ρ)<τ<1000×μ 2 / (D 2 ×ρ) (I) where μ is the viscosity of the polymer solution before phase separation, in Pa s; D is the hydraulic diameter in meters; ρ is the density of the polymer solution before phase separation, in kg / m 3 and Preferably, τ satisfies the following formula: 20×μ 2 / (D 2 ×ρ) < τ < 120 × μ 2 / (D 2 ×ρ) (II).
8. The method of claim 7 , wherein the mechanical perturbation is applied by stirring.
9. 10. The method of claim 8, wherein the phase separation device is provided with one or more internal components for enhancing turbulence.
10. 10. The method of claim 9, wherein the internal components for enhancing turbulence are baffles and / or guide tubes.
11. The method of claim 6 , wherein a mechanical perturbation is performed during or after the heat treatment.
12. 12. The method of claim 11, wherein the perturbation is applied by one or more of the following methods: performing a heat treatment prior to the phase separation device and applying one or more mechanical perturbations selected from: applying a mechanical perturbation in a heat treatment device prior to the phase separation device, applying a mechanical perturbation in a pipe conveying the polymer solution to the phase separation device, applying a mechanical perturbation while feeding the polymer solution into the phase separation device, and applying a mechanical perturbation within the phase separation device; and Carrying out a heat treatment in the phase separator and applying a mechanical perturbation in the phase separator.
13. 13. The method of claim 12, wherein the perturbation is applied by one or more of the following methods: (1) carrying out a heat treatment prior to the phase separation device and applying a mechanical perturbation in the pipe conveying the polymer solution to the phase separation device; (2) performing a heat treatment before the phase separation device and applying a mechanical perturbation while feeding the polymer solution into the phase separation device; (3) Heat treatment before the phase separator and mechanical perturbation in the phase separator; (4) performing a heat treatment before the phase separation device, applying a mechanical perturbation while feeding the polymer solution into the phase separation device, and applying a mechanical perturbation in the phase separation device; (5) Heat treatment is performed before the phase separator, and mechanical perturbation is applied in the equipment where heat treatment is performed before the phase separator.
14. 14. The method according to claim 12 or 13, wherein the heat treatment prior to the phase separation device is carried out by means of a heat exchanger and / or by applying jacket heating to the pipes connected to the phase separation device.
15. 14. The method according to claim 12 or 13, wherein applying a mechanical perturbation while feeding the polymer solution into the phase separation device is performed by feeding the polymer solution through a nozzle or distributor.
16. 14. The method according to claim 12 or 13, wherein the heat treatment in the phase separation device is performed by means of jacket heating and / or built-in heating coils.
17. 14. The method according to claim 12 or 13, wherein applying mechanical perturbation in the phase separation device is performed by applying stirring, providing baffles or providing other stationary parts.
18. 14. The method according to claim 12 or 13, wherein the mechanical perturbation is applied by placing a part such as a coil / Chinese knot in an apparatus for carrying out a heat treatment prior to the phase separation apparatus.
19. The method according to claim 12 or 13, wherein the polymer solution is transported to a heat exchanger having a heating function and capable of disturbing the flow of the polymer solution to carry out a heat treatment, and then sent to a phase separation device to carry out phase separation.
20. 20. The method according to claim 19, wherein protrusions capable of disturbing the flow of the liquid are provided in the pipe of the polymer solution flow path upstream of the phase separation device.
21. 20. The method according to claim 18, wherein the pipes of the polymer solution flow path in the heat exchanger are provided with protrusions capable of disturbing the flow of the liquid.
22. The heat exchanger is a Chinese knot heat exchanger and / or a spiral coil heat exchanger; Preferably, the internal pipe of the Chinese knot heat exchanger is bent to form a plurality of Chinese knots, more preferably 1 to 5 Chinese knots; A method according to claim 19 or 20, wherein preferably the pipe of the spiral coil heat exchanger is spirally bent to form a plurality of spirals, more preferably between 3 and 20 spirals.
23. The method according to any one of claims 1 to 22, wherein said polymer solution is obtained by a solution polymerization process, and the polymer concentration in said polymer solution is 5-20 wt%, preferably 6-15 wt%.
24. the polymer in the polymer solution is selected from one or more of plastics, rubbers, and thermoplastic elastomers; Preferably, the plastic is selected from one or more of polyethylene, polypropylene, polybutylene, copolymers of ethylene and one or more α-olefins, and copolymers of propylene and one or more α-olefins; Preferably, the rubber is selected from one or more of butadiene-styrene rubber, butadiene rubber, isoprene rubber, and styrene-isoprene rubber; 24. The method according to any one of claims 1 to 23, wherein the thermoplastic elastomer is selected from one or more of copolymers of ethylene and one or more α-olefins, copolymers of propylene and one or more α-olefins, and copolymers of ethylene and one or more cyclic olefins, copolymers of ethylene and one or more cyclic olefins, copolymers of ethylene and one or more α-olefins and optionally a non-conjugated diene, butene-ethylene copolymers, styrene-butadiene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers.
25. the solvent in the polymer solution is selected from one or more of C5 to C10 linear or branched alkanes, C5 to C10 cycloalkanes, and C6 to C20 aromatic hydrocarbons; 25. The method of any one of claims 1 to 24, wherein the solvent in the polymer solution is selected from one or more of n-pentane, isopentane, cyclopentane, n-hexane, isohexane, cyclohexane, methylcyclohexane, n-heptane, 2-methylheptane, n-octane, isooctane, mixed octanes, benzene, toluene, o-xylene, m-xylene and p-xylene.
26. 26. The process according to any one of claims 1 to 25, wherein the polymer concentration in the clear liquid phase is less than 1 wt % and the polymer concentration in the concentrated liquid phase is 8 to 50 wt %, preferably 10 to 35 wt %, more preferably 15 to 31 wt %.
27. 27. The method of claim 26, wherein the polymer concentration in the concentrated liquid phase is greater than 1.35 times, more preferably greater than 1.8 times, and even more preferably greater than 2.0 times, the polymer concentration in the polymer solution.
28. A method for phase separation of a polymer solution, comprising the steps of: 1) promoting phase separation of a polymer solution using the method according to any one of claims 1 to 27; 2) Separating the clear liquid phase from the concentrated liquid phase.
29. A method for preparing an olefin polymer, comprising the steps of: (A) providing a catalyst system into a polymerization reactor and contacting it with one or more olefin monomers and, optionally, hydrogen to polymerize olefins to obtain a polymerization reaction mixture; (B) The phase separation of the polymerization reaction mixture of step A is carried out by the method for phase separation of a polymer solution according to claim 28, to obtain a clear liquid phase and a concentrated liquid phase.
30. 30. The process according to claim 29, further comprising the steps of: A concentrated liquid phase is recovered from the phase-separated solution obtained in step B, and the concentrated liquid phase is subjected to devolatilization to obtain a polymer.
Citation Information
Patent Citations
Disposing method of molded foam
JP2003003010A
Method for the production of a polypropylene blend
US20020128394A1