Sintered Zirconia Beads

Sintered zirconia beads with a controlled composition address the limitations of existing grinding media by providing improved wear resistance and strength for efficient wet dispersion and micro-grinding.

JP2024538598AInactive Publication Date: 2024-10-23SAINT GOBAIN CENT DE RES & DEVS & DETUD EUROEN
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024519127
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-28
Filing Date
2022-09-26
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing grinding media, such as glass and metal beads, face issues of wear resistance, contamination, and high energy consumption, while ceramic beads have composition-specific production methods that are not interchangeable, limiting their effectiveness in modern high-speed mills.

Method used

Sintered zirconia beads with a specific chemical composition of ZrO2 + HfO2 + Y2O3 + CeO2, with controlled monoclinic zirconia content and stabilizing phases, offering improved abrasion resistance and strength for grinding applications.

Benefits of technology

The sintered zirconia beads exhibit enhanced wear resistance and strength, making them suitable for wet dispersion and micro-grinding, reducing energy consumption and equipment stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538598000003
    Figure 2024538598000003
  • Figure 2024538598000001
    Figure 2024538598000001
  • Figure 2024538598000002
    Figure 2024538598000002
Patent Text Reader

Abstract

Sintered beads, wherein the sintered beads have the following chemical composition as a mass percentage based on oxides: ZrO2 + HfO2 + Y2O3 + CeO2: the remainder up to 100%; 0% ≤ Al2O3 ≤ 1.5%; CaO ≤ 2%; Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO: ≤ 5%; As a molar percentage based on the total of ZrO2, HfO2, Y2O3 and CeO2, 1.3% ≤ Y2O3 ≤ 2.5%, and 0.1% ≤ CeO2 ≤ 1.7% the contents of Y2O3 and CeO2, and the following crystal phases as a mass percentage based on the crystal phase, with respect to a total of 100%: Stabilized zirconia: the remainder up to 100%; Monoclinic zirconia: ≤ 15%; Crystal phases other than stabilized zirconia and monoclinic zirconia: < 7% having provided that Y2O3 < 1.8%, provided that 0.5% ≤ CeO2, and / or 0.9% < CeO2 ≤ 1.7%, and / or 10% < monoclinic zirconia ≤ 15% being the said sintered beads.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to sintered zirconia beads, a method for making these beads, and the use of these beads as grinding media or as a wet dispersion agent or for surface treatment. [Background technology]

[0002] The paint, ink, dye, magnetic lacquer and pesticide industries use beads for dispersion and homogenization of liquid and solid components.

[0003] In the minerals industry, beads are used to finely grind materials that may have previously been dry ground via conventional processes, particularly calcium carbonate, titanium dioxide, gypsum, kaolin, and iron ore.

[0004] In the field of microgrinding, rounded grain sand, glass beads, metal beads and ceramic beads are known. Rounded grain sand, such as Ottawa sand, is a natural, inexpensive product, but is not suitable for modern pressurized high-speed grinding mills because it is brittle, has low density, is variable in quality, and is abrasive to equipment. The widely used glass beads have better strength, less abrasiveness and are available in a wider diameter range. Metal beads, especially steel beads, are less inert towards the products undergoing treatment, cause, among other things, contamination of mineral fillers and greying of paints, are excessively dense and require special grinding machines, which, among other things, involve high energy consumption, significant heat and high mechanical stresses on the equipment. Ceramic beads have better strength, higher density, and greater chemical inertness than glass beads.

[0005] The beads are conventionally sized from 0.005 to 10 mm.

[0006] The following can be identified: Fused ceramic beads, which are generally obtained by melting a ceramic component, forming spherical droplets from the molten material, and then solidifying the droplets; and Sintered ceramic beads, which are generally obtained by cold forming of ceramic powder followed by solidification of said powder by firing at high temperature.

[0007] Unlike sintered beads, sintered beads usually contain a very abundant intergranular glass phase that fills the network of crystalline grains. Therefore, the problems that sintered beads and fused beads face in their respective applications, as well as the technical solutions adopted to solve said problems, are generally different. Moreover, due to significant differences between the manufacturing methods, compositions developed for manufacturing fused beads are in principle not suitable for the manufacture of sintered beads and vice versa. Summary of the Invention [Problem to be solved by the invention]

[0008] There is a continuing need for sintered zirconia beads having improved wear resistance, particularly for milling applications.

[0009] One object of the present invention is to address, at least in part, this need. [Means for solving the problem]

[0010] The Applicant's International Patent Application No. PCT / EP2021 / 058816, filed on April 2, 2021, claims sintered beads, The following chemical composition as mass percentages based on oxides: ZrO2+HfO2+Y2O3+CeO2: remainder to 100%; 0%≦Al2O3≦1.5%; CaO≦2%; Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO: ≤ 5%; As molar percentages based on the total of ZrO2, HfO2, Y2O3 and CeO2, 1.8% ≤ Y2O3 ≤ 2.5% and 1.8% ≤ Y2O3 ≤ 2.5% and 0.1% ≤ CeO2 ≤ 0.9%, Y2O3 and CeO2 contents, and As mass percentages based on the crystal phase, for a total of 100%, the following crystal phases: Stabilized zirconia: the remainder up to 100%; Monoclinic zirconia: ≤ 10%; Crystal phases other than stabilized zirconia and monoclinic zirconia: < 7% Relates to the above sintered beads having the same.

[0011] The reason is that the inventors have found that these types of beads exhibit improved wear resistance, particularly under hydrothermal conditions. However, complementary detailed studies have shown that these beads also have excellent wear resistance in the following cases: 1.3% ≤ Y2O3 < 1.8%, provided that 0.5% ≤ CeO2 ≤ 1.8%, and / or 0.9% < CeO2 ≤ 1.8%, and / or 10% < monoclinic zirconia ≤ 15%.

[0012] Therefore, the present invention is a sintered bead, wherein the sintered bead has As mass percentages based on the oxides, the following chemical composition: ZrO2 + HfO2 + Y2O3 + CeO2: the remainder up to 100%; 0% ≤ Al2O3 ≤ 1.5%; CaO ≤ 2%; Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO: ≤ 5% As molar percentages based on the total of ZrO2, HfO2, Y2O3 and CeO2,[[]] 1.3% ≤ Y2O3 ≤ 2.5%, particularly 1.3% ≤ Y2O3 < 1.8%, and 0.1% ≤ CeO2 ≤ 1.8%, particularly 0.5% ≤ CeO2 ≤ 1.8%, particularly 0.9% < CeO2 ≤ 1.8%, preferably CeO2 ≤ 1.7% is, the contents of Y2O3 and CeO2, and as mass percentages based on the crystal phase, with respect to a total of 100%, the following crystal phases: Stabilized zirconia: the remainder up to 100%; Monoclinic zirconia: ≤ 15%; Crystal phases other than stabilized zirconia and monoclinic zirconia: < 7% has, provided that Y2O3 < 1.8%, provided that 0.5% ≤ CeO2, preferably 0.8% ≤ CeO2, and / or 0.9% < CeO2 ≤ 1.8%, preferably CeO2 ≤ 1.7%, and / or 10% < monoclinic zirconia ≤ 15% is, for the above sintered beads.

[0013] As shown in more detail in the remainder of the detailed description of the present invention, unexpectedly, the inventors have found that not only in the complementary composition ranges thus defined, but also in the ranges defined in International Application No. PCT / EP2021 / 058816, sintered zirconia beads exhibiting excellent strength during grinding can be obtained by having the content of monoclinic zirconia be more than 10% and 15% or less.

[0014] Accordingly, the sintered zirconia beads according to the present invention are particularly well - suited for wet dispersion and subjecting to micronization.

[0015] In a first preferred main embodiment, the present invention is a sintered bead, having the following chemical composition as mass percentages based on oxides: ZrO2 + HfO2 + Y2O3 + CeO2: the remainder up to 100%; 0% ≤ Al2O3 ≤ 1.5%; CaO ≤ 2%; Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3, and CaO: ≤ 5%; As a molar percentage based on the total of ZrO2, HfO2, Y2O3, and CeO2, 1.3% ≤ Y2O3 < 1.8% and 0.5% ≤ CeO2 ≤ 1.8%, preferably 0.5% ≤ CeO2 ≤ 1.7%, preferably 0.8% ≤ CeO2 ≤ 1.7% The contents of Y2O3 and CeO2, and, As a mass percentage based on the crystal phase, with respect to a total of 100%, the following crystal phases: Stabilized zirconia: The remainder up to 100%; Monoclinic zirconia: ≤ 15%, preferably ≤ 10%; Crystal phases other than stabilized zirconia and monoclinic zirconia: < 7% Having, Regarding the above sintered beads.

[0016] In a second preferred main embodiment, the present invention is a sintered bead, With the following chemical composition as a mass percentage based on the oxides: ZrO2 + HfO2 + Y2O3 + CeO2: The remainder up to 100%; 0% ≤ Al2O3 ≤ 1.5%; CaO ≤ 2%; Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3, and CaO: ≤ 5%; As a molar percentage based on the total of ZrO2, HfO2, Y2O3, and CeO2, 1.3% ≤ Y2O3 ≤ 2.5%, and 0.9% < CeO2 ≤ 1.8%, preferably 0.9% < CeO2 ≤ 1.7% The contents of Y2O3 and CeO2, and, As a mass percentage based on the crystal phase, with respect to a total of 100%, the following crystal phases: Stabilized zirconia: The remainder up to 100%; Monoclinic zirconia: ≤ 15%, preferably ≤ 10%; Crystalline phases other than stabilized zirconia and monoclinic zirconia: <7% having Regarding the sintered beads.

[0017] FIG. 1 shows a composition range 10 of International Patent Application No. PCT / EP2021 / 058816 and a complementary composition range 12 according to the first and second main embodiments of the present invention.

[0018] In a third main embodiment, the present invention provides sintered beads, comprising: The following chemical composition as mass percentages based on oxides: ZrO2+HfO2+Y2O3+CeO2: remainder to 100%; 0%≦Al2O3≦1.5%; CaO≦2%; Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO: ≦5%; As a mole percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, 1.3%≦Y2O3≦2.5%, and 0.1% <CeO2≦1.8% The content of Y2O3 and CeO2 is having However, when Y2O3<1.8%, 0.5%≦CeO2; and The following crystalline phases are present, based on the mass percentage of said crystalline phases, relative to a total of 100%: Stabilized zirconia: remainder up to 100%; 10%<monoclinic zirconia≦15%; Crystalline phases other than stabilized zirconia and monoclinic zirconia: <7% having Regarding the sintered beads.

[0019] Insofar as optional features of International Patent Application No. PCT / EP2021 / 058816 are technically compatible with the main embodiment, such features are also optionally applied to this embodiment.

[0020] Regardless of the main embodiment, the sintered zirconia beads according to the invention may have one or more of the following optional characteristics, provided that these characteristics are in accordance with the main embodiment: the sintered beads are composed of more than 99% of their mass oxides; the content of Y2O3, as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, is less than 2.4%, preferably less than 2.2%, preferably less than 2.0%, preferably less than 1.9%, preferably 1.8%, preferably 1.7% or less, and / or preferably 1.4% or more; The content of Y2O3 is, as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, 1.3% or more, preferably 1.4% or more, and less than 1.8%, preferably 1.7% or less; The content of CeO2 is, as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, 0.6% or more, preferably 0.7% or more, preferably 0.8% or more, and 1.7% or less, preferably 1.6% or less, preferably 1.5% or less; the content of Al2O3, expressed as a mass percentage based on said oxide, is 0.2% or more and 1.2% or less, preferably 0.8% or less, or less than 0.1%; the content of CaO, expressed as a mass percentage based on said oxide, is less than 1.0% or more than 0.2%; the total content of oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO, expressed as a percentage by mass based on said oxides, is less than 2%; As a mass percentage based on the total amount of said crystalline phase: The content of said monoclinic zirconia is not more than 10%, preferably not more than 8%, preferably not more than 5%; the total content of crystalline phases other than said stabilized zirconia and monoclinic zirconia is less than 5%; the mass of the amorphous phase, as a mass percentage relative to the mass of the beads, is substantially zero; the stabilized zirconia is substantially exclusively in the form of quadratic zirconia; The stabilized zirconia is stabilized with Y2O3 and CeO2; The sintered beads have an average grain size of less than 2 μm and / or have a grain size distribution with a standard deviation of less than 0.20 μm; The sintered beads have an average grain size of less than 0.6 μm and / or have a grain size distribution with a standard deviation of less than 0.15 μm.

[0021] These optional features described above are preferred for the third main embodiment, except as regards the composition of the sintered beads.

[0022] In particular, in the third main embodiment, the sintered zirconia beads according to the invention may also have one or more of the following optional and preferred features: the content of Y2O3, expressed as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, is 1.9% or more, preferably 2% or more, and / or preferably 2.4% or less, preferably 2.2% or less; the content of CeO2, as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, is equal to or greater than 0.2%, preferably equal to or greater than 0.3%, preferably equal to or greater than 0.4%, and / or is less than 0.8%, preferably less than 0.7%, preferably less than 0.6%; the sintered beads consist of more than 98%, preferably more than 99%, preferably more than 99.5%, preferably more than 99.9% of their mass of oxides; the content of Al2O3, expressed as a mass percentage based on said oxide, is greater than or equal to 0.2%, preferably greater than or equal to 0.25%, and preferably greater than or equal to 1.2%, preferably less than or equal to 1%, preferably less than or equal to 0.8%, or less than 0.1%; the content of CaO, expressed as a mass percentage based on said oxide, is less than 1.0% or more than 0.2%; The total content of oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO, expressed as a mass percentage based on said oxides, is less than 4%, preferably less than 3%, preferably less than 2%, preferably less than 1%, preferably less than 0.8%, preferably less than 0.5%.

[0023] The present invention also relates to a bead powder comprising more than 90%, preferably more than 95%, preferably substantially 100%, by weight of beads according to the invention.

[0024] The invention also relates to a device selected from suspensions, grinders and surface treatment equipment, said device comprising a powder of beads according to the invention.

[0025] The present invention also provides a method for producing sintered zirconia beads according to the present invention, comprising the steps of: a) preparing a particle mixture having a median size of less than 2 μm and a composition suitable for obtaining sintered zirconia beads according to the invention based on the results of step g); b) optionally drying the particle mixture; c) preparing a starting material from the optionally dried particle mixture; d) forming the starting material into the form of green beads; e) optionally, a washing step; f) optionally drying; g) sintering at a sintering temperature above 1300°C to obtain sintered beads. The method further comprises the steps of:

[0026] The manufacturing method according to the invention may also have one or more of the following optional features: In step a), the one or more starting material powders introduced into the particle mixture are milled, preferably co-milled, In step a), the particle mixture has a median size of less than 0.5 μm and / or a ratio (D 90 -D 10 ) / D50 having In step a), no starting materials other than the zirconia powder at least partially stabilized with Y2O3, ceria and corundum are intentionally introduced into the particle mixture; One or more of the powders of the particle mixture are at least partially replaced with an equivalent powder that provides the same composition, with the same crystallographic phases, in the same amounts in the beads.

[0027] The optional and preferred features listed above with respect to the sintered beads and with respect to the composition of these beads are also optional and preferred features of the particle mixture used in step a) for producing the beads.

[0028] The invention finally relates to the use of the bead powder according to the invention, in particular the bead powder produced by the process according to the invention, as grinding medium, more in particular as grinding medium for wet grinding, as wet dispersant or for surface treatment.

[0029] definition

[0030] The sum of oxide contents (ie a formula in which these contents are linked by a "+" sign) does not imply that the two oxides linked by this "+" sign are necessarily present simultaneously.

[0031] The term "particles" refers to the individualized solid products in a powder.

[0032] The words "powder" and "particle mixture" are conventionally synonymous. For the sake of clarity, the term "particle mixture" in the present description denotes the powder produced in step a) of the method according to the invention.

[0033] Conventionally, the term "sintering" refers to the solidification of green particles (granular aggregates) by heat treatment above 1100°C, possibly accompanied by partial or total melting of some (but not all) of the constituents of the green particles.

[0034] A "grain" of a sintered zirconia bead consists of particles of a particle mixture that have been agglomerated by sintering. Thus, a sintered bead according to the invention consists of an aggregate of multiple grains that have been joined by sintering. The bead may also contain an amorphous phase.

[0035] The term "bead" means a particle having a sphericity, i.e. the ratio between its smallest Ferret diameter and its largest Ferret diameter, greater than 0.6, regardless of the manner in which this sphericity is obtained. Preferably, beads according to the invention have a sphericity greater than 0.7.

[0036] The "size" of a bead refers to its smallest Feret diameter.

[0037] "Percentile" 10 of a powder or particle mixture (D 10 ), 50(D 50 ) and 90 (D 90 (denoted as D ) refer to the particle sizes corresponding to percentages equal to 10%, 50% and 90% by weight, respectively, on the cumulative particle size distribution curve of the powder or the particle mixture, said particle sizes being ranked in ascending order. Thus, according to this definition, 10% by weight of the particles in the powder or particle mixture are D 10 and 90% by weight of the particles are smaller than D 10 That's it. The percentiles can be determined, for example, using a laser granulometer.

[0038] The "median size" of a particle powder or particle mixture is the 50th percentile, or D 50 The median size is therefore used to separate the particles or mixture of particles of a powder into first and second populations of equal mass, each of which contains only particles having a size equal to or greater than the median size, or less than the median size, respectively.

[0039] The "average size" of the grains in the sintered beads is the size measured by using the "average linear intercept" method. This type of measurement is described in ASTM standard E1382.

[0040] The term "sintered beads" means solid beads obtained by sintering green beads.

[0041] "Other oxides" are preferably "impurities", i.e. unavoidable oxides inevitably introduced into the starting material. In particular, oxides of sodium and other alkali metals are impurities. Examples that may be mentioned include Na2O or KO. Hafnium oxide is, however, not considered an impurity. A total impurity content of less than 5% is considered not to substantially modify the results obtained.

[0042] In the context of this patent application, HfO2 is considered not to be chemically dissociated from ZrO2. Therefore, in the chemical composition of the zirconia-containing product, "ZrO2" or "ZrO2 + HfO2" refers to the total content of these two oxides. According to the present invention, HfO2 is not intentionally added to the starting material. Therefore, HfO2 refers only to trace amounts of hafnium oxide, since this oxide is always naturally present in zirconia sources, generally in contents less than 2%.

[0043] For clarity, the terms "ZrO2" (or "ZrO2+HfO2") and "Al2O3" are used to refer to the content of these oxides in the composition, and "zirconia" and "corundum" refer to the crystalline phases of these oxides, consisting of ZrO2+HfO2 and Al2O3, respectively. However, these oxides may also exist in other phases. The term "zirconia" conventionally includes a small amount of hafnia phase, which cannot be distinguished by X-ray diffraction.

[0044] The term "stabilized zirconia" refers to a combination of quadratic and cubic zirconia.

[0045] The term "at least partially stabilized zirconia" means partially stabilized zirconia or fully stabilized zirconia. Partially stabilized zirconia is zirconia that contains monoclinic zirconia and has a monoclinic zirconia content of less than 50% as a mass percentage based on the total amount of crystalline phases, with other phases present being tetragonal and / or cubic phases. CeO2 and Y2O3 act to stabilize the zirconia, but may also be present outside the zirconia.

[0046] The term "powder of a compound" means a powder comprising more than 95% by weight of particles comprising more than 90% by weight of the compound. Thus, a corundum powder comprises more than 95% by weight of particles comprising more than 90% by weight of corundum. A "tetragonal zirconia powder" comprises more than 95% by weight of particles comprising more than 90% by weight of tetragonal zirconia. A "stabilized zirconia powder" comprises more than 95% by weight of particles comprising more than 90% by weight of stabilized zirconia.

[0047] The term "precursor" of an oxide means one or more constituents capable of providing said oxide during the sintering step of the manufacturing method according to the invention. For example, aluminum hydroxide is a precursor of alumina.

[0048] An amount of a precursor of an oxide is said to be "equivalent" to an amount of said oxide if it results in said amount of said oxide during sintering.

[0049] The specific surface area is calculated by the BET (Brunauer Emmett Teller) method described in the Journal of the American Chemical Society, 60 (1938), pages 309 to 316.

[0050] The term "absolute density" of a sintered zirconia product, in particular of a sintered bead, means the absolute density AD calculated by using the following formula (1): AD=100 / [(x / 3.987)+(100-x) / ADz] (1) where x is the alumina content in mass percentage; ADz is the absolute density of the zirconia stabilized with Y2O3 and CeO2, calculated by dividing the mass of a zirconia unit cell by the volume of the unit cell, and the zirconia is considered to be stabilized only in the tetragonal phase. The volume of the unit cell is calculated by using cell parameters determined by X-ray diffraction. The mass of the unit cell is equal to the sum of the masses of the Zr, O, Y and Ce elements present in the unit cell, and all of the Y2O3 and CeO2 are considered to stabilize the zirconia.

[0051] The term "bulk density" of a sintered product, in particular of sintered beads, conventionally means the ratio equal to the mass of the sintered product divided by the volume occupied by the sintered product, which can be measured by imbibition according to the principle of Archimedes' thrust.

[0052] The term "relative density" of a sintered product, in particular of a sintered bead, means the ratio equal to the apparent density divided by the absolute density, expressed as a percentage.

[0053] Unless otherwise stated, all averages are arithmetic means.

[0054] Unless otherwise stated, all percentages are mass percentages on an oxide basis.

[0055] The words "include", "having" and "comprise" are to be construed in an open-ended manner.

[0056] All the characteristics of the beads can be measured according to the protocols described in the examples.

[0057] Other features and advantages of the present invention will become apparent from a reading of the following detailed description and a review of the accompanying drawings. [Brief description of the drawings]

[0058] [Figure 1] FIG. 1 is a graph representing composition ranges according to the first and second main embodiments of the present invention, from International Patent Application No. PCT / EP2021 / 058816, in which the x-axis represents the Y2O3 content and the y-axis represents the CeO2 content as a mole percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0059] Sintered Zirconia Beads

[0060] The sintered zirconia beads according to the present invention should be noted with respect to their composition.

[0061] Surprisingly, and without being able to be theoretically explained, the inventors have discovered that the simultaneous presence of Y2O3 and CeO2 in the contents indicated in the present invention makes it possible to achieve excellent resistance during grinding.

[0062] The sintered zirconia beads according to the invention preferably consist of more than 98% of their mass of oxides, preferably more than 99%, preferably more than 99.5%, preferably more than 99.9%. Preferably, the sintered zirconia beads according to the invention consist substantially entirely of oxides.

[0063] Preferably, the sintered zirconia beads according to the present invention have a Y2O3 content, expressed as a mole percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, of greater than or equal to 1.4% and / or preferably less than 2.4%, preferably less than 2.2%, preferably less than 2.0%, preferably less than 1.9%, preferably less than 1.8%, preferably less than 1.7%.

[0064] Preferably, the sintered zirconia beads according to the present invention have a Y2O3 content, expressed as a mole percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, of 1.3% or more, preferably 1.4% or more, and less than 1.8%, preferably less than 1.7%.

[0065] Preferably, the sintered zirconia beads according to the present invention have a CeO2 content, expressed as a mole percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, of 0.6% or more, preferably 0.7% or more, preferably 0.8% or more, and / or preferably 1.7% or less, preferably less than 1.6%, preferably 1.5% or less.

[0066] Preferably, the sintered zirconia beads according to the present invention have a Y2O3 content, as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2, of 1.4% or more and / or preferably less than 2.4%, preferably less than 2.2%, preferably less than 2.0%, preferably less than 1.9%, preferably less than 1.8%, preferably less than 1.7%, and a CeO2 content of 0.6% or more, preferably 0.7% or more, preferably 0.8% or more, and / or preferably 1.7% or less, preferably 1.6% or less, preferably 1.5% or less. Advantageously, the sintered zirconia beads have excellent resistance to wear during grinding.

[0067] In a preferred embodiment, the sintered zirconia beads according to the invention have an Al2O3 content, expressed as a mass percentage based on the oxide, of 0.2% or more, preferably 0.25% or more and preferably 1.2% or less, preferably 1% or less, preferably 0.8% or less.

[0068] However, tests have shown that the presence of Al2O3 is not essential. In one embodiment, the sintered zirconia beads according to the invention have an Al2O3 content, expressed as a mass percentage based on the oxide, of less than 0.1%, less than 0.005%, less than 0.003%, less than 0.002%, or substantially zero.

[0069] Preferably, the sintered beads according to the invention have a CaO content, expressed as a mass percentage based on the oxide, of less than 1.5%, preferably less than 1.0%.

[0070] In one embodiment, the sintered zirconia beads according to the invention have a CaO content, expressed as a mass percentage based on the oxide, of more than 0.1%, preferably more than 0.2%, preferably more than 0.3%.

[0071] Preferably, the sintered beads according to the invention have a total content of oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO of less than 4%, preferably less than 3%, preferably less than 2%, preferably less than 1%, preferably less than 0.8%, preferably less than 0.5%, based on the mass percentage of said oxides. Preferably, in the sintered zirconia beads according to the invention, said oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO are impurities.

[0072] Preferably, in the sintered zirconia beads according to the present invention, any oxide other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO is present in an amount of less than 2.0%, preferably less than 1.5%, preferably less than 1.0%, preferably less than 0.8%, preferably less than 0.5%, preferably less than 0.3%.

[0073] The sintered zirconia beads according to the invention preferably have a content of monoclinic zirconia, expressed as a mass percentage based on the total amount of crystalline phases, of less than 10%, preferably less than 8%, preferably less than 5%, preferably essentially zero.

[0074] The sintered zirconia beads according to the invention preferably have a total content of crystalline phases other than stabilized zirconia and monoclinic zirconia of less than 6%, preferably less than 5%, or even less than 4%, as a mass percentage based on the total amount of crystalline phases.

[0075] In the sintered zirconia beads according to the invention, the zirconia is stabilized with Y2O3 and CeO2. Preferably, the stabilized zirconia is present substantially exclusively in the form of tetragonal zirconia.

[0076] Preferably, in the sintered beads of zirconia according to the invention, the mass of amorphous phase, i.e. vitreous, expressed as a mass percentage relative to the mass of the beads, is less than 7%, preferably less than 5%, preferably essentially zero.

[0077] The sintered zirconia beads according to the invention have an average grain size of less than 2 μm, preferably less than 1.5 μm, preferably less than 1 μm, preferably less than 0.9 μm, preferably less than 0.8 μm, preferably less than 0.6 μm, preferably less than 0.5 μm, and preferably greater than 0.1 μm, preferably greater than 0.15 μm. Advantageously, resistance during grinding is improved.

[0078] Preferably, the sintered zirconia beads according to the present invention have a grain size distribution with a standard deviation of less than 0.20 μm, preferably less than 0.15 μm, preferably less than 0.1 μm.

[0079] In a preferred embodiment, the sintered zirconia beads according to the present invention have: The following chemical composition, expressed as mass percentages based on the oxides: ZrO2+HfO2+Y2O3+CeO2: remainder to 100%; 0%≦Al2O3≦1.5%, wherein the Al2O3 content is preferably ≧0.2%, preferably ≧0.25% and preferably ≦1.2%, preferably ≦1%, preferably ≦0.8%; CaO≦2%, where the CaO content is preferably less than 1.5%, preferably less than 1.0%, Oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO, i.e. "other oxides", ≦5%, where the content of "other oxides" is preferably less than 4%, preferably less than 3%, preferably less than 2%, preferably less than 1%, more preferably less than 0.8%, preferably less than 0.5%; Y2O3 and CeO2 contents, as mole percentages based on the sum of ZrO2, HfO2, Y2O3 and CeO2, the Y2O3 content is equal to or greater than 1.3%, preferably equal to or greater than 1.4%, and equal to or less than 1.8%, preferably equal to or less than 1.7%, and the CeO2 content is equal to or greater than 0.6%, preferably equal to or greater than 0.7%, preferably equal to or greater than 0.8%, and equal to or less than 1.7%, preferably equal to or less than 1.6%, preferably equal to or less than 1.5%, The following crystalline phases are present in the mass percentage based on the crystalline phase, relative to the total of 100%: Stabilized zirconia: the remainder up to 100%, where the stabilized zirconia is stabilized with Y2O3 and CeO2 and is preferably present substantially exclusively in the form of tetragonal zirconia; Monoclinic zirconia≦15%, wherein the content of monoclinic zirconia is preferably 10% or less, preferably 8% or less, preferably 5% or less, preferably substantially zero; Crystal phases other than stabilized zirconia and monoclinic zirconia, i.e. "other crystalline phases": <7%, where the content of other crystalline phases is preferably less than 5%, preferably substantially zero; and A mass of amorphous phase, expressed as a mass percentage relative to the mass of the sintered zirconia beads, of less than 7%, preferably less than 5%, preferably substantially zero.

[0080] In the above preferred embodiment, the sintered zirconia beads preferably have an average grain size of less than 2 μm, preferably less than 1.5 μm, preferably less than 1 μm, preferably less than 0.9 μm, preferably less than 0.8 μm, preferably less than 0.6 μm, preferably less than 0.5 μm, and preferably greater than 0.1 μm, preferably greater than 0.15 μm.

[0081] Preferably, the sintered zirconia beads according to the present invention have a relative density of more than 99%, preferably more than 99.5%, preferably more than 99.6%, preferably more than 99.7%, preferably more than 99.8%, preferably more than 99.9%, where the absolute density is calculated according to the method already described.

[0082] The sintered zirconia beads according to the invention preferably have a size less than 10 mm, preferably less than 2.5 mm and / or more than 0.005 mm, preferably more than 0.01 mm, preferably more than 0.02 mm, preferably more than 0.03 mm.

[0083] The sintered zirconia beads according to the present invention preferably have a sphericity greater than 0.7, preferably greater than 0.8, preferably greater than 0.85, or even greater than 0.9.

[0084] The sintered zirconia beads according to the present invention can be produced by using the production method according to the present invention.

[0085] Method for producing sintered zirconia beads

[0086] To produce sintered zirconia beads according to the present invention, steps a) to g) described above and detailed below may be carried out.

[0087] In step a), a particle mixture having a median size of less than 2 μm is prepared, the composition of which is adapted in a manner known per se so that the sintered zirconia beads have a composition according to the invention.

[0088] The starting material powders are intimately mixed.

[0089] The starting powders can be individually milled or preferably co-milled so that the resulting particle mixture has a median size of less than 2 μm, preferably less than 1.5 μm, preferably less than 1 μm, preferably less than 0.8 μm, preferably less than 0.6 μm, preferably less than 0.5 μm, preferably less than 0.4 μm, preferably less than 0.3 μm, and / or preferably greater than 0.05 μm. The milling can be wet milling. Milling or co-milling can also be used to obtain an intimate mixture.

[0090] Preferably, the particle mixture has a ratio (D 90 -D 10 ) / D 50 has.

[0091] Y2O3 and CeO2 are known stabilizers for zirconia. In the particle mixture, they may or may not stabilize the zirconia. However, in accordance with the present invention, the particle mixture should result in sintered zirconia beads in accordance with the present invention.

[0092] In the particle mixture, the zirconia is preferably at least partially stabilized with Y2O3. Preferably, then, CeO2 ceria powder is used as the CeO2 source. In the above embodiment, the zirconia powder is at least partially stabilized with Y2O3 and has a 0.5m 2 / g, preferably 1m 2 / g, preferably 1.5m 2 / g and / or 20m 2 / g, preferably less than 18m 2 / g, preferably less than 15m 2 / g. Advantageously, the optional grinding, generally in suspension, is thereby facilitated. Furthermore, the sintering temperature of step f) can be reduced. In the above embodiment, in the zirconia powder at least partially stabilized with Y2O3, the zirconia is present substantially exclusively in tetragonal form.

[0093] Ceria and / or yttria and / or zirconia precursors may also be used in the particle mixture.

[0094] The ceria and / or the ceria precursor, and / or the yttria and / or the yttria precursor, may be partially or completely incorporated into the particle mixture in the form of a powder, i.e., separate from the zirconia, so that the zirconia is at least partially stabilized after sintering. In this embodiment, the yttria powder median size and / or the yttria precursor median size and / or the ceria powder median size and / or the ceria precursor median size are preferably less than 1 μm, preferably less than 0.5 μm, more preferably less than 0.3 μm. Advantageously, the stabilization efficiency of the zirconia is thereby improved during sintering.

[0095] In one embodiment, the particle mixture comprises particles in which stabilized or unstabilized zirconia and yttria and / or ceria are intimately mixed. Such intimate mixtures can be obtained, for example, by coprecipitation, pyrohydrolysis or spraying, and optionally solidified by heat treatment. In the particle mixture, the yttria and / or ceria can be replaced by an equivalent amount of one or more precursors.

[0096] Preferably, the particle mixture does not include any yttria precursors.

[0097] Preferably, the particle mixture does not include any ceria precursors.

[0098] Preferably, the particle mixture does not include any zirconia precursors.

[0099] Preferably, the particle mixture does not include any monoclinic zirconia powder.

[0100] Preferably, for the first and second main embodiments and insofar as these features are compatible with these embodiments, the Y2O3 content, expressed as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2 present in the particle mixture, is greater than or equal to 1.4% and / or preferably less than or equal to 2.4%, preferably less than 2.2%, preferably less than 2.0%, preferably less than 1.9%, preferably less than 1.8%, or preferably less than or equal to 1.7%.

[0101] Preferably, for the first and second main embodiments, and insofar as these features are compatible with these embodiments, the Y2O3 content, expressed as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2 present in the particle mixture, is greater than or equal to 1.3%, preferably greater than or equal to 1.4%, and less than 1.8%, preferably less than or equal to 1.7%.

[0102] Preferably, for the first and second main embodiments and insofar as these features are compatible with these embodiments, the CeO2 content, expressed as a molar percentage based on the sum of ZrO2, HfO2, YO3 and CeO2 present in the particle mixture, is 0.6% or more, preferably 0.7% or more, preferably 0.8% or more, and / or 1.7% or less, 1.6% or less, preferably 1.5% or less.

[0103] Preferably, for the first and second main embodiments and in so far as these features are compatible with these embodiments, the Y2O3 content, as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2 present in the particle mixture, is 1.4% or more and / or preferably 2.4% or less, preferably less than 2.2%, preferably less than 2.0%, preferably less than 1.9%, preferably less than 1.8%, preferably 1.7% or less, and the CeO2 content is 0.6% or more, preferably 0.7% or more, preferably 0.8% or more and / or preferably 1.7% or less, preferably 1.6% or less, preferably 1.5% or less. Advantageously, the sintered zirconia beads obtained from the particle mixture have excellent resistance during grinding.

[0104] Preferably, for the first and second main embodiments, and in so far as these features are compatible with these embodiments, the Y2O3 content, expressed as a molar percentage based on the sum of ZrO2, HfO2, Y2O3 and CeO2 present in the particle mixture, is equal to or greater than 1.3%, preferably equal to or greater than 1.4% and less than 1.8%, preferably equal to or less than 1.7%, and the CeO2 content is equal to or greater than 0.6%, preferably equal to or greater than 0.7%, preferably equal to or greater than 0.8%, and preferably equal to or less than 1.7%, preferably equal to or less than 1.6%, preferably equal to or less than 1.5%.

[0105] In a preferred embodiment, the particle mixture comprises alumina powder in an amount of 0.2% or more, preferably 0.25% or more and preferably 1.2% or less, preferably 1% or less, preferably 0.8% or less, as a mass percentage based on the mass of the particle mixture. Advantageously, this improves the sinterability of the particle mixture. The alumina can be completely or partially replaced with an equivalent amount of precursor. Preferably, the particle mixture does not comprise any alumina precursor. More preferably, the alumina is essentially present in the form of corundum, which preferably has a median diameter of less than 5 μm, preferably less than 3 μm, preferably less than 1 μm.

[0106] However, tests have shown that the presence of alumina is not essential. In one embodiment, the alumina content can be less than 0.1%, less than 0.05%, less than 0.03%, less than 0.01%, or substantially zero, in particular as a mass percentage based on the mass of the particle mixture.

[0107] In one embodiment, the particle mixture comprises: Zirconia at least partially stabilized with Y2O3; Celia, corundum Contains powder.

[0108] The powders providing the oxides are preferably selected so that the total content of oxides other than ZrO2, HfO2, Y2O3, CeO2, Al2O3 and CaO, expressed as a mass percentage based on the oxides, is less than 5%.

[0109] Preferably, no starting materials other than powders of Y2O3, ceria, and zirconia at least partially stabilized with corundum are intentionally introduced into the particle mixture, and other oxides present are impurities.

[0110] Preferably, the powders used have a median size of less than 5 μm, preferably less than 3 μm, preferably less than 2 μm, preferably less than 1 μm, preferably less than 0.7 μm, preferably less than 0.6 μm, preferably less than 0.5 μm, preferably less than 0.4 μm or even less than 0.3 μm, respectively.

[0111] Regardless of the embodiment, one or more of the powders of the particle mixtures described above may be at least partially replaced with an equivalent powder, i.e. a powder that results in the same amount of the same constituents (same composition, same crystallographic phases) in the beads during the manufacture of the beads according to the invention.

[0112] In optional step b), the particle mixture, especially if it was obtained by wet grinding or if at least one starting material powder was obtained by wet grinding, can be dried, for example in an oven or by spraying. Preferably, the temperature and / or duration of the drying step are adapted so that the residual moisture content of the particle mixture is less than 2%, or even less than 1.5%.

[0113] In step c), the starting materials, including the particle mixture obtained at the end of step a) or at the end of step b), and optionally a solvent, preferably water, are preferably prepared at room temperature, the amount of which is adapted to the formation method of step d).

[0114] As known to those skilled in the art, the starting materials are adapted to the formation method of step d).

[0115] In particular, the forming may result from a gelation process. To this end, a solvent, preferably water, is preferably added to the starting material to produce a suspension.

[0116] The suspension preferably has a solids content by mass of 50% to 70%.

[0117] The suspension may also include one or more of the following components: a dispersant in an amount of 0 to 10%, as a mass percentage based on the solids; a surface tension modifier in an amount of 0 to 3%, expressed as a mass percentage based on the solids; A gelling agent, or "gellant," in an amount of 0-2%, as a mass percentage based on the solids.

[0118] Dispersants, surface tension modifiers and gelling agents are well known to those skilled in the art.

[0119] Examples that may be mentioned are: As dispersants, the family of sodium or ammonium polymethacrylates, the family of sodium or ammonium polyacrylates, the family of citrates, e.g. ammonium, the family of sodium phosphates, and the family of carbonates, As a surface tension adjusting agent, an organic solvent such as an aliphatic alcohol, Natural polysaccharides as gelling agents Includes:

[0120] The particle mixture is preferably added to a mixture of water and dispersants / deflocculants in a ball mill. After stirring, water in which the gelling agent has already been dissolved is added to obtain a suspension.

[0121] When the forming is carried out by extrusion, a thermoplastic or thermosetting polymer may be added to the starting materials, which preferably do not contain any solvent.

[0122] In step d) any known conventional forming process for the production of sintered beads can be carried out.

[0123] Among these processes, Granulation processes, for example using granulators, fluid bed granulators or granulation discs; Gelling process, Injection molding or extrusion processes, and Pressurized Process may be mentioned.

[0124] In the gelation process, droplets of the above-mentioned suspension are obtained by flowing the suspension through a calibrated orifice, which causes the droplets exiting the orifice to fall into a bath of gelling solution (an electrolyte adapted to react with the gelling agent), where they harden after regaining a substantially spherical shape.

[0125] In an optional step e), the green beads obtained in the previous step are washed, for example with water.

[0126] In optional step f), the optionally washed green beads are dried, for example in an oven.

[0127] In step g), the optionally washed and / or dried green beads are sintered. Preferably, the sintering is carried out in air, preferably in an electric furnace, preferably at atmospheric pressure.

[0128] The sintering in step g) is preferably carried out at a temperature above 1330°C, preferably above 1350°C and preferably below 1600°C, preferably below 1550°C, preferably below 1500°C, preferably 1450°C.

[0129] The holding time in the stationary temperature stage is preferably more than 1 hour and / or preferably less than 10 hours, preferably less than 7 hours, preferably less than 5 hours, preferably less than 3 hours. Preferably the sintering time is between 1 and 3 hours.

[0130] The resulting sintered zirconia beads preferably have a minimum diameter greater than 0.005 mm, preferably greater than 0.1 mm, preferably greater than 0.15 mm, and less than 10 mm, preferably less than 5 mm, preferably less than 2.5 mm.

[0131] The sintered zirconia beads according to the invention are particularly well suited as an agent for grinding, in particular for wet grinding, or as an agent for wet dispersion. The invention therefore also relates to the use of the beads according to the invention or of a powder of beads produced according to the process according to the invention as an agent for grinding, in particular for wet grinding, or as an agent for wet dispersion.

[0132] The properties of the sintered zirconia beads according to the invention, and their ease of production, make them suitable for other applications, especially for surface treatments (especially by spraying the sintered beads according to the invention).

[0133] The present invention therefore also relates to a device selected from suspension equipment, crushers and surface treatment equipment, said device comprising a powder of beads according to the invention.

[0134] Working Example

[0135] Measurement Protocol

[0136] The following methods can be used to characterize the sintered beads or mixtures of sintered beads in particular according to the invention.

[0137] To determine the sphericity of the beads, the minimum and maximum Feret diameters are measured with a Camsizer XT machine sold by the company Horiba.

[0138] Quantification of the crystalline phases present in the sintered beads is carried out directly on the beads, which are attached to the self-adhesive carbon pellets, so that the surface of the pellets is covered with the maximum amount of beads.

[0139] The crystalline phases present in the sintered beads are measured by X-ray diffraction, for example using a Panalytical X'Pert PRO diffractometer equipped with a copper XD tube. The diffraction patterns are acquired using this instrument over an angular range 2θ of 5° to 100°, with a step size of 0.017° and a counting time of 150 sec / step. The front optics include a fixed 1 / 4° programmable divergence slit, a 0.04 rad Soller slit, a mask equal to 10 mm and a fixed 1 / 2° anti-divergence slit. The sample is rotated around itself to limit the preferred orientation. The rear optics include a fixed 1 / 4° programmable anti-divergence slit, a 0.04 rad Soller slit and a Ni filter.

[0140] The diffraction patterns are then qualitatively analyzed using EVA software and the ICDD2016 database.

[0141] Once the phases present are highlighted, the diffraction patterns are quantitatively analyzed by the Rietveld refinement method using High Score Plus software according to the following strategy: Refinement of the background signal is performed using the "Processing" function, "Background determination", with the following selections: "Bending factor" at 0 and "Grain size" at 40. Conventionally, the highlighted ICDD sheets of quantifiable present phases are selected and therefore taken into account in the refinement. Next, an automatic refinement is performed by selecting a pre-determined background signal with "Use available background" and by selecting the "Auto:Options phase fit-default Rietveld" mode. Then, manual refinement of the "B global" parameters of all the selected phases is performed simultaneously. Finally, a simultaneous manual refinement of the Caglioti W parameters of the tetragonal and cubic zirconia phases is performed if the automatic function did not do so. In this case, "W" is selected for the zirconia phase and the refinement is performed again. Results are retained only if the "goodness of fit" parameter of the second refinement is lower than that of the first refinement.

[0142] The amount of amorphous phase present in the sintered beads is measured by X-ray diffraction, for example using a Panalytical X'Pert PRO diffractometer equipped with a copper XD tube. The diffraction pattern is obtained using this device in the same way as the determination of the crystalline phases present in the beads, the analyzed sample being in powder form. The applied method consists in adding a known amount of a completely crystalline standard, in this case zinc oxide ZnO powder, in an amount equal to 20% based on the mass of a sample of zinc oxide and ground sintered beads. The maximum size of the zinc oxide powder is 1 μm and the sintered beads are ground to obtain a maximum powder size of less than 40 μm.

[0143] A maximum ZnO particle size is entered into the High Score Plus software to limit microabsorption effects.

[0144] The content of the amorphous phase as a percentage is calculated using the following formula, where Q ZnO is the amount of ZnO determined from the diffraction pattern: Amorphous phase content = 100*(100 / (100-20))*(1-(20 / Q ZnO )).

[0145] For example, Q ZnO is equal to 22%, the content of amorphous phase is equal to 100×(100 / (100−20))×(1−(20 / 22))=11.4%.

[0146] The bulk density of the sintered beads is measured by hydrostatic weighing.

[0147] The unit cell parameters required to calculate the absolute density of at least partially stabilized zirconia are determined by X-ray diffraction using a Bruker D8 Endeavor machine on the surface of the sample to be characterized (the sample is not ground into a powder). The parameters required for obtaining the diffraction pattern are identical to the parameters used for obtaining the diffraction pattern required for the quantification of the crystalline phases.

[0148] The unit cell parameters a and c were determined using a pseudo-Voigt profile (with npr=5) after refinement of the diffraction pattern using Fullprof software available at https: / / www.ill.eu / sites / fullprof / , and the refined parameters were the displacement of the sample using the "SyCos" function, Lorentzian / Gaussian fraction of pseudo-Voigt function using the "Shape 1" function, Half-width parameters U, V, W, Skewness parameters using the 'Asy1' and 'Asy2' functions, Baseline point and the space group of the partially substituted tetragonal zirconia unit cell, P 42 / nmc (137), is considered to be identical to the space group of the unsubstituted tetragonal zirconia unit cell.

[0149] The chemical analysis of the sintered beads is measured by Inductively Coupled Plasma (ICP) spectroscopy for elements whose content does not exceed 0.5%. To determine the content of other elements, a droplet of the sintered bead material to be analyzed is made by melting the material, and then a chemical analysis is carried out by X-ray fluorescence.

[0150] The average grain size of the sintered beads is measured by the "average linear intercept" method. This type of method is described in ASTM standard E1382. According to this standard, analysis lines are drawn on the image of the sintered beads, and then along each analysis line, the length, known as the "intercept", between two consecutive grain boundaries that intersect the analysis line is measured.

[0151] The average length "l'" of the segments "I" is then determined.

[0152] The sections are determined from images obtained by scanning electron microscopy of sintered bead samples, the cross sections of which have previously been polished to mirror quality and then thermally etched at 50° C. below the sintering temperature to expose the grain boundaries. The magnification used to take the images is chosen to visualize approximately 100 grains in one image. Five images are taken per sintered bead.

[0153] The average grain size "d" of the sintered beads is given by the relationship: d = 1.56 x l', which is taken from formula (13) in the paper "Average Grain Size in Polycrystalline Ceramics" by MI Mendelson, J. Am. Ceram. Soc. Vol. 52, No. 8, pages 443-446.

[0154] The standard deviation of the grain size distribution is 1.56 times the standard deviation of the intercept distribution "l".

[0155] The specific surface area of ​​a powder or particle mixture is measured by the BET (Brunauer Emmett Teller) method described in the Journal of the American Chemical Society, 60 (1938), pages 309 to 316.

[0156] The 10th, 50th and 90th percentiles of the powders and particle mixtures are conventionally measured using a LA950V2 model laser granulometer sold by Horiba.

[0157] To determine the "planetary wear" rate, 20 ml (volume measured using a graduated cylinder) of test beads with a size between 0.9 and 1.1 mm are weighed (mass m0) and introduced into one of four bowls of a Retsch brand PM400 rapid planetary mill, each with a capacity of 125 ml, lined with dense sintered alumina. 50 2.2 g of 100 μm SiO2 (having a SiC content of 0.1 g / g) and 40 ml of water are added to the same bowl already containing the beads. The bowl is closed and rotated at 400 rpm for 1.5 hours with the direction of rotation reversed every minute (planetary motion). The contents of the bowl are then washed on a 100 μm sieve to remove residual silicon carbide and any material removed by abrasion during grinding. After sieving on the 100 μm sieve, the beads are dried in an oven at 100° C. for 3 hours and then weighed (mass m1). The beads (mass m1) are reintroduced into one of the bowls with the SiC suspension (same concentration and amount as before) and undergo a new grinding cycle identical to the previous one. The contents of the bowl are then washed on a 100 μm sieve to remove residual silicon carbide and any material removed by abrasion during grinding. After sieving through a 100 μm sieve, the beads are dried in an oven at 100° C. for 3 hours and then weighed (mass m2). The beads (mass m2) are reintroduced into one of the bowls with the SiC suspension (same concentration and amount as before) and undergo a new grinding cycle identical to the previous one. The contents of the bowls are then washed on a 100 μm sieve to remove residual silicon carbide and any material removed by abrasion during grinding. After sieving through a 100 μm sieve, the beads are dried in an oven at 100° C. for 3 hours and then weighed (mass m3).

[0158] The planetary wear (PW) is expressed as a percentage (%) and is equal to the mass loss of the beads relative to the initial mass of the beads, i.e. 100(m2-m3) / (m2), and the PW results are given in Table 2 below.

[0159] Manufacturing Protocol

[0160] The sintered beads were prepared using: 10m 2 yttriated zirconia powder (for example 1) containing a molar Y2O3 content of 2.5% with a specific surface area of ​​about 1.0 μm / g and a median diameter of less than 0.3 μm; 10m 2 yttria-loaded zirconia powder (for Example 2) with a molar content of 3% Y2O3 having a specific surface area of ​​about 1000 nm / g and a median diameter of less than 0.3 μm; 10m 2 yttria-loaded zirconia powder (for examples 3-5) with a molar content of 2% Y2O3 having a specific surface area of ​​about 100 nm / g and a median diameter of less than 0.3 μm; 10m 2 yttria-loaded zirconia powder (for examples 3-5) containing 1% Y2O3 molar content, with a specific surface area of ​​about 1.0 μm / g and a median diameter of less than 0.3 μm; CeO2 ceria powder having a purity of more than 99% and a median diameter of less than 10 μm (for Examples 3 to 5); Alumina powder having a purity of greater than 99% and a median diameter of less than 0.5 μm (for Examples 1 to 5).

[0161] Table 1 below summarizes the example particle mixtures obtained in step a).

[0162] [Table 1]

[0163] In step a), the various powders were mixed and then wet co-milled until a particle mixture with a median size of less than 0.3 μm was obtained.

[0164] Then, in step b), the particle mixture was dried.

[0165] Then, in step c), a starting material consisting of an aqueous suspension containing, for each example, 1% of a carboxylic ester dispersant, 3% of a carboxylic dispersant and 0.4% of a gelling agent, i.e. a polysaccharide of the alginic acid family, as percentages by mass based on solids, was prepared from the dry particle mixture obtained based on the results of step b). A ball mill was used for this preparation in order to obtain a good homogeneity of the starting material. First, a solution containing the gelling agent was formed. The particle mixture and the dispersant were added successively to water. Then, the solution containing the gelling agent was added. The mixture thus obtained was stirred for 8 hours. The particle size was checked using a laser granulometer model LA950V2 sold by the company Horiba (median diameter <0.3 μm), and then a certain amount of water was added to obtain an aqueous suspension with a solids content of 68% and a viscosity of less than 5000 centipoise, measured using a Brookfield viscometer with LV3 spindle at a speed equal to 20 rpm. The pH of the suspension was then approximately 9 after optional adjustment with a strong base.

[0166] In step d), the suspension was passed through a calibrated hole at a flow rate to obtain beads of size about 1 mm for these examples after sintering. Droplets of the suspension were allowed to fall into an electrolyte (divalent cation salt) based gelling bath to react with the gelling agent.

[0167] The raw beads were collected, washed with water in step e) and then dried at 80° C. in step f) to remove moisture.

[0168] Then, in step g), the beads were transferred to a sintering furnace where they were sintered in the following cycle: Heat up to 500°C at 100°C / hour, 500℃ for 2 hours, Heat at 100℃ / hour to 1425℃, 1425℃ for 2 hours, The temperature is reduced by natural cooling.

[0169] result

[0170] The results obtained are collated in Table 2 below.

[0171] [Table 2]

[0172] The sintered beads of this example consist substantially entirely of oxides, with an amorphous phase in an amount of less than 5% by weight.

[0173] The bead powder of this example has an average sphericity of greater than 0.9.

[0174] Example 2 outside the invention is representative of the prior art and is provided as a basis for comparison with Example 3 according to the invention, the total molar Y2O3+CeO2 content of the two examples being substantially identical.

[0175] Example 1 outside the invention is provided as a basis for comparison with Example 4 according to the invention, the total molar Y2O3+CeO2 content of the two examples being substantially identical.

[0176] Comparing Example 2 outside the invention with Example 3 according to the invention, the beads according to Example 3 show a planetary ball mill wear rate PW that is 11.8% lower than the beads of Example 2.

[0177] Comparing Example 1 outside the invention with Example 4 according to the invention, the beads according to Example 1 show a 12.5% ​​lower planetary ball mill wear rate PW than the beads of Example 4.

[0178] Comparing Example 2 outside the invention with Example 5 according to the invention, the beads according to Example 5 exhibited a planetary ball mill wear rate PW that was 11.8% lower than the beads of Example 2, which have a molar content of Y2O3+CeO2 of 3% and 3.73%, respectively, based on the molar content of ZrO2+HfO2+Y2O3+CeO2.

[0179] As can now be seen, the present invention provides sintered zirconia beads that exhibit significant planetary ball mill wear rates PW.

[0180] However, it will be understood that the present invention is not limited to only the embodiments described above.

Claims

1. 1. A sintered bead, comprising: The following chemical composition, as mass percentages based on oxides: ZrO 2 + HfO 2 +Y 2 O 3 +CeO 2 : Remaining to 100%; 0%≦Al 2 THE 3 ≦1.5%; CaO≦2%; ZrO 2 , HfO 2 , Y 2 O 3 , CEO 2 , Al 2 O 3 and oxides other than CaO: ≦5%; ZrO 2 , HfO 2 , Y 2 O 3 and CeO 2 As a mole percentage based on the sum of 1.3%≦Y 2 O 3 ≦2.5%, and 0.1%≦CeO 2 ≦1.7% Y 2 O 3 and CeO 2 The content of, The following crystalline phases are present, based on the mass percentage of the crystalline phase, relative to a total of 100%: Stabilized zirconia: balance to 100%; Monoclinic zirconia: ≦15%; Crystalline phases other than stabilized zirconia and monoclinic zirconia: <7% having however, Y 2 O 3 <1.8%, but 0.5% or less CeO 2 and / or 0.9% < CeO 2 ≦1.7%, and / or 10% < Monoclinic zirconia ≦ 15% That is, The sintered beads.

2. The above Y 2 O 3 The content is ZrO 2 , HfO 2 , Y 2 O 3 and CeO 2 2. The sintered bead of claim 1, wherein the molar percentage based on the sum of

3. The above Y 2 O 3 The content is ZrO 2 , HfO 2 , Y 2 O 3 and CeO 2 3. The sintered beads according to claim 1 or 2, wherein the molar percentage based on the sum of the above is 1.8% or less.

4. The sintered beads consist of more than 99% by mass of oxides, and / or the sintered beads The above Y 2 O 3 The content is ZrO 2 , HfO 2 , Y 2 O 3 and CeO 2 and / or The CeO 2 The content is ZrO 2 , HfO 2 , Y 2 O 3 and CeO 2 and / or The Al 2 O 3 The content, expressed as a mass percentage based on the oxide, is 0.2% or more and 1.2% or less, and / or the CaO content is less than 1.0% or more than 0.2%, expressed as a percentage by mass based on the oxide, and / or ZrO 2 , HfO 2 , Y 2 O 3 , CEO 2 , Al 2 O 3 and the total content of oxides other than CaO is less than 2%, expressed as a mass percentage based on the oxides; Sintered beads according to any one of claims 1 to 3.

5. The CeO 2 The content is ZrO 2 , HfO 2 , Y 2 O 3 and CeO 2 and / or The Al 2 O 3 The content is 0.8% or less as a mass percentage based on the oxide; 5. The sintered bead of claim 4.

6. In the sintered beads, as a mass percentage based on the total amount of the crystalline phase, The content of monoclinic zirconia is 10% or less, and / or The total content of crystalline phases other than the stabilized zirconia and monoclinic zirconia is less than 5%. Sintered beads according to any one of claims 1 to 5.

7. 7. Sintered beads according to any one of claims 1 to 6, wherein the mass of the amorphous phase, as a mass percentage relative to the mass of the bead, is substantially zero.

8. In the sintered beads, the stabilized zirconia is present substantially only in the form of quadratic zirconia and / or the stabilized zirconia is 2 O 3 and CeO 2 8. Sintered beads according to claim 1, which are stabilized with

9. Sintered beads according to any one of claims 1 to 8, having an average grain size of less than 2 µm and / or having a grain size distribution with a standard deviation of 0.20 µm.

10. 10. The sintered beads of claim 9 having an average grain size of less than 0.6 μm and / or having a grain size distribution with a standard deviation of less than 0.15 μm.

11. A powder comprising beads according to any one of claims 1 to 10 in a mass percentage of more than 90%.

12. A device selected from a suspension device, a grinder, and a surface treatment machine, said device comprising a powder of beads according to any one of claims 11.

13. A method for producing sintered beads according to any one of claims 1 to 10, comprising the steps of: a) preparing a particle mixture having a median size of less than 2 μm and a composition suitable for obtaining sintered beads according to any one of claims 1 to 10 based on the outcome of step g), b) optionally drying the particle mixture; c) preparing a starting material from the optionally dried particle mixture; d) forming the starting material into the form of green beads; e) optionally, washing; f) optionally drying; g) sintering at a sintering temperature above 1300°C to obtain sintered beads. The method comprises the successive steps of:

14. The method according to claim 13, wherein in step a) one or more starting material powders introduced into the particle mixture are co-milled.

15. In step a), the particle mixture has a median diameter of less than 0.5 μm and / or a ratio (D 90 -D 10 ) / D 50 15. The method of claim 13 or 14, comprising:

16. In step a), Y 2 O 3 16. The method according to claim 13, wherein no starting materials other than the zirconia powder at least partially stabilized with ceria and corundum are intentionally introduced into the particle mixture.

17. 17. The method according to any one of claims 13 to 16, wherein one or more of the powders of the particle mixture are at least partially replaced with an equivalent powder that provides the same composition, with the same crystallographic phases, in the same amounts in the beads.

Citation Information

Patent Citations

  • Thermal shock strength and hot water stability zirconia base ceramics

    JP1988151670A

  • Partially stabilized zinc oxide spherical body and method of manufacturing the same

    JP2004315246A

  • ZrO2 SINTERED COMPACT AND ITS MANUFACTURING METHOD, MEMBER OF CRUSHER, AND CRUSHER

    JP2006298711A

  • Sintered products based on alumina and zirconia

    JP2012528782A

  • Sintered zirconia balls

    JP2023524381A