Method for producing auxiliary cementitious material, and auxiliary cementitious material produced therefrom

By pre-carbonating cementitious materials with CO2 to form supplementary cementitious materials, the method addresses the high energy consumption and emissions of Portland cement production, enhancing hydraulic performance and reducing emissions by up to 30%.

JP2024538709AInactive Publication Date: 2024-10-23SOLIDIA TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024520950
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-07
Filing Date
2022-10-06
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The production of ordinary Portland cement is a highly energy-intensive process and a significant source of greenhouse gas emissions, contributing to approximately 8% of total CO2 emissions globally, necessitating a method to integrate carbon capture into the cement manufacturing process to reduce environmental impact.

Method used

A method involving carbonation-assisted cementitious materials is developed, where carbonatable materials are pre-carbonated with CO2 to form supplementary cementitious materials (SCMs) that can be integrated into traditional hydraulic concrete materials, reducing the clinker factor and incorporating carbon capture, using various carbonation processes such as slurry, cyclic, and high-temperature carbonation.

Benefits of technology

This approach enhances hydraulic performance by increasing CO2 absorption rates and reduces the environmental footprint of cement production, achieving up to 30% lower emissions compared to traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538709000001_ABST
    Figure 2024538709000001_ABST
Patent Text Reader

Abstract

A method of preparing a carbonation-assisted cementitious material includes carbonating a carbonatable mixture to obtain a first carbonated cementitious material, grinding the first carbonated cementitious material, and carbonating the ground mixture to obtain a carbonation-assisted cementitious material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit of priority to U.S. Provisional Application No. 63 / 253,343, filed October 7, 2021, pursuant to 35 U.S.C. § 119, the entire contents of which are incorporated by reference as if fully set forth herein.

[0002] (Technical field) The present application is directed to the preparation of ground carbonation-assisted cementitious materials with enhanced carbon dioxide absorption rates. [Background technology]

[0003] Where a document, act, or article of knowledge is referenced or discussed in this specification, such reference or discussion is not an admission that that document, act, article of knowledge, or any combination thereof, was publicly available, well known, part of the general knowledge at the priority date, or otherwise constitutes prior art under any applicable statutory provision or is known to be relevant to any attempt to solve any problem to which this specification pertains.

[0004] The production of ordinary Portland cement (OPC) is a very energy-intensive process and a major source of greenhouse gas emissions. The cement sector is the third largest industrial energy consumer and the second largest CO2 emitter in total industrial CO2 emissions. Global cement production reached 4.1 Gt in 2019 and is estimated to contribute about 8% of total anthropogenic CO2 emissions.

[0005] In an attempt to combat climate change, member states of the United Nations Framework Convention on Climate Change (UNFCC) agreed through the Paris Agreement adopted in December 2015 to reduce CO2 emissions by 20% to 25% by 2030. This corresponds to a target of reducing one gigaton of CO2 annually. Under this agreement, the UNFCC agreed to limit the rise in global temperature to within 2 degrees Celsius by the end of this century. To achieve this goal, the World Business Council for Sustainable Development (WBCSD) Cement Sustainability Initiative (CSI) has created a roadmap called "Low Carbon Transition in the Cement Industry" (WBCSD-CSI). The roadmap identified four carbon emission reduction levers in the global cement industry. The first lever is to improve energy efficiency by retrofitting existing facilities to improve their energy performance. The second is to switch to alternative fuels with lower carbon dioxide emissions. For example, biomass and waste materials can be used in cement kilns to offset the consumption of carbon-intensive fossil fuels. The third is to reduce the clinker coefficient or clinker-to-cement ratio. Finally, the WBCSD-CSI proposes using emerging innovative technologies, such as integrating carbon capture into the cement manufacturing process.

[0006] Therefore, there is a need for improved cement production that reduces CO2 emissions and mitigates the global effects of climate change. This disclosure attempts to address these issues identified by the EPA and UNFCC by developing a method to integrate carbon capture into the cement manufacturing process.

[0007] For example, Solidia Technologies Inc. has developed a low CO2 emission clinker that reduces CO2 emissions by 30%. However, there is a need to integrate such materials into conventional hydraulic concrete materials to reduce the clinker factor of hydraulic cements such as ordinary portland cement (OPC) and to further increase the positive environmental potential of using such low CO2 emission materials as supplementary cementitious materials (SCMs) in concrete. Although certain aspects of the prior art have been discussed to facilitate disclosure of the present invention, applicants are not in any way disclaiming these technical aspects, and it is believed that the claimed invention may include or include one or more of the prior art aspects discussed herein. Summary of the Invention

[0008] It has been discovered that the present invention overcomes the above-mentioned shortcomings and provides certain advantages. For example, the method and composition of the present invention provide a novel approach to pre-carbonate a carbonatable clinker, preferably but not exclusively a low CO2 emission clinker, before adding it to a hydraulic cement as a supplementary cementitious material (SCM), providing a double environmental benefit by both reducing the clinker coefficient of conventional hydraulic cement and incorporating carbon capture into the production of cement or concrete materials. Various exemplary methods for preparing SCM, including slurry process, cyclic carbonation process, non-slurry carbonation process (semi-wet carbonation process) and high temperature carbonation process, are described in U.S. Provisional Application Nos. 63 / 151,971 and 63 / 217,590, and corresponding U.S. Patent Application Nos. 17 / 675,777 and 17 / 855,576, the contents of which are incorporated by reference as if fully set forth herein.

[0009] An exemplary embodiment is directed to a method of preparing a carbonation-assisted cementitious material, the method including adding water to a carbonatable material to form a carbonatable mixture, the carbonatable mixture having a water content of about 0.1% to about 99.9%, stirring or agitating the carbonatable mixture for about 1 minute to about 24 hours, carbonating the carbonatable mixture to obtain a first carbonated cementitious material, grinding the first carbonated cementitious material for about 0.1 minutes to about 60 minutes to obtain a ground mixture, and carbonating the ground mixture for about 1 minute to about 24 hours, the carbonating the carbonatable mixture and the ground mixture including flowing a gas containing about 5% to about 100% carbon dioxide by volume, respectively, and maintaining a temperature of about 1° C. to about 99° C. to obtain a carbonation-assisted cementitious material. The carbonation and grinding steps may be repeated up to 10 times as necessary to maximize the absorption rate of CO2.

[0010] Another exemplary embodiment is directed to a method of forming a cement or concrete, the method including forming a carbonation-assisted cementitious material by any of the methods described herein; combining the carbonation-assisted cementitious material with a hydraulic cement composition to form a cementitious material mixture, the cementitious material mixture comprising about 1% to about 99% by weight of the carbonation-assisted cementitious material based on the total weight of solids in the mixture; and reacting the cementitious material mixture with water to form the cement or concrete.

[0011] These and other features of the invention will now be described with reference to the drawings of specific embodiments which are intended to be illustrative, not limiting, of the invention. [Brief description of the drawings]

[0012] [Figure 1] 1 depicts measurements of mortar flow for mixtures of ASTM sand in accordance with ASTM C778 and supplemental cementitious materials prepared using the grinding method according to an exemplary embodiment, measured at 20% replacement of ordinary Portland cement (OPC) having a water-to-cement ratio (w / c) of 0.485. [Diagram 2] 13 depicts the SAI of ground supplemental cementitious material according to an exemplary embodiment measured at 20% replacement of OPC having a w / c of ​​0.485 after 7 days and 28 days, respectively. [Diagram 3] 1 shows the CO2 absorption rates of the examples and comparative examples of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Further aspects, features and advantages of the present invention will become apparent from the detailed description below. It should be understood that the various individual aspects and features of the present invention described herein can be combined in any number of any one or more of the individual aspects or features to form the embodiments of the present invention that are specifically contemplated and encompassed by the present invention. Furthermore, any feature described in the claims can be combined with any other feature described in the claims in any number or combination. Such combinations are also expressly contemplated as being encompassed by the present invention.

[0014] As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0015] As used herein, "about" is a term of approximation and is intended to include slight variations in the literally recited quantities, as would be understood by one of ordinary skill in the art. Such variations include, for example, standard deviations associated with techniques commonly used to measure the amounts of components or ingredients of alloys or composites, or other properties and characteristics. All values ​​characterized by the above modifier "about" are also intended to include the exact numerical values ​​disclosed herein. Additionally, all ranges include the upper and lower limits.

[0016] Any composition described herein, unless expressly indicated otherwise, is intended to encompass compositions consisting of, consisting essentially of, or even comprising the various components identified herein.

[0017] As used herein, reference to a numerical range of a variable is intended to convey that the variable can be equal to any value within that range, and to all subranges contained within the broader range. Thus, the variable can be equal to any integer value within the numerical range, including the end points of the range. By way of example, a variable described as having a value between 0 and 10 can be 0, 4, 2 to 6, 2.75, 3.19 to 4.47, etc.

[0018] In this specification and claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. As used herein, unless specifically indicated otherwise, the word "or" is used in the "inclusive" sense of "and / or" and not in the "exclusive" sense of "either / or."

[0019] Unless otherwise indicated, each of the individual features or embodiments herein may be combined without restriction with any other individual features or embodiments described herein, and such combinations are specifically contemplated within the scope of the present invention, regardless of whether they are explicitly described as combinations herein.

[0020] Technical and scientific terms used herein have the meanings commonly understood by one of ordinary skill in the art to which this description pertains, unless otherwise defined. Reference is made herein to various methodologies and materials known to those skilled in the art.

[0021] The base material used to form the supplemental cementitious material of the present invention is not particularly limited as long as it is carbonizable. As used herein, the term "carbonatable" refers to a material that can react with carbon dioxide and sequester carbon dioxide under conditions described herein or equivalent conditions. Carbonatable materials can be naturally occurring materials or can be synthesized from precursor materials.

[0022] In an exemplary embodiment, the carbonatable material may include municipal solid waste (MSW). As used herein, MSW is defined as waste generated by households and businesses, including food, kitchen waste, green waste, paper waste, glass, bottles, cans, metal, plastic, fabric, clothing, batteries, tires, building debris, construction and demolition waste, soil, rocks, rubble, electronics, computer equipment, paint, chemicals, light bulbs and fluorescent lights, fertilizer, medical waste, and the like. As defined in the present invention, MSW also includes sewage sludge, which contains undigested food residues, mucus, bacteria, urea, chloride, sodium ions, potassium ions, creatinine, other dissolved ions, inorganic and organic compounds, and water. MSW in various forms contains CO2 and water in a more concentrated form than pure water and carbon dioxide. For example, the carbon content of municipal solid waste in one large trash can is equivalent to at least 15,000 pounds of carbon dioxide and 700 gallons of water. Unlike pure water and CO2, no refrigeration or preservatives are required for long-term storage of MSW. Additionally, minimal transportation is required to bring the MSW to the digestion site.

[0023] An exemplary embodiment of the present application is directed to a method of preparing a carbonation-assisted cementitious material, the method including adding water to a carbonatable material to form a carbonatable mixture, the water content of the mixture being between about 0.1% and about 99.99% by weight; stirring or agitating the carbonatable mixture for between about 1 minute and 24 hours; carbonating the carbonatable mixture to obtain a first carbonated cementitious material; grinding the first carbonated cementitious material for between about 0.1 minutes and about 10 minutes to obtain a ground mixture; carbonating by flowing a gas comprising between about 5% and about 100% by volume of carbon dioxide through the ground mixture for between about 1 minute and 24 hours, respectively, through the mixture and the ground mixture; and heating to between about 1° C. and about 99° C. and maintaining the temperature to obtain a carbonation-assisted cementitious material.

[0024] The carbonatable material may include a water content in an amount having any value falling within any of these recited ranges, such as about 0.1% to about 99.99%, about 0.1% to about 90%, about 0.1% to about 80%, about 0.1% to about 70%, about 0.1%, about 0.1% to about 50%, about 0.1% to about 40%, about 0.1% to about 30%, about 0.1% to about 20%, about 0.1% to about 10%, etc., and 0.1%, 1.0%, 0.5% to 10%, 0.5% to 90%, 10.5%, 6.75% to 9.25%, etc. The water content value may be equal to any integer value or values ​​within the above numerical ranges, including the range endpoints.

[0025] The carbonatable mixture may be agitated or stirred for about 1 minute to about 15 hours, about 5 minutes to about 14 hours, about 10 minutes to about 13 hours, about 15 minutes to about 12 hours, about 20 minutes to about 11 hours, about 30 minutes to about 10 hours, about 1 hour to about 9.5 hours, about 1.5 hours to about 8 hours, about 2 hours to about 7.5 hours, about 2.5 hours to about 7 hours, about 3 hours to about 6.5 hours, about 3.5 hours to about 6 hours, about 4 hours to about 5.5 hours, about 4.5 hours to about 5 hours, etc. The agitation or stirring time may be equal to any integer value or multiple values ​​within the above numerical ranges, including the endpoints of these ranges.

[0026] The order of each step in the above method is not particularly limited, and stirring or agitation and carbonation may be performed simultaneously, or stirring or agitation and carbonation may be performed successively.

[0027] In an exemplary embodiment, the methods described herein further include a plurality of carbonation cycles alternating with the plurality of grinding cycles, wherein the duration of each of the plurality of carbonation cycles and each of the plurality of grinding cycles may be as described herein.

[0028] In another exemplary embodiment, the process may further include steaming the ground mixture prior to carbonating the ground mixture, where the steaming includes exposing the ground mixture to vapor or steam at a temperature of about 20° C. to about 200° C., about 40° C. to about 180° C., about 60° C. to about 160° C., about 80° C. to about 140° C., about 100° C. to about 120° C., etc. The temperature may be equal to any integer value or values ​​within the above numerical ranges, including the endpoints of these ranges. The steaming of the ground mixture may occur simultaneously with or prior to carbonating the ground mixture, and multiple steaming steps may be used in conjunction with multiple grinding steps.

[0029] In another exemplary embodiment, the process includes drying the carbonation-assisted cementitious material at a temperature of about 50° C. to about 150° C., about 53° C. to about 140° C., about 56° C. to about 130° C., about 60° C. to about 120° C., etc., for about 5 hours to about 25 hours, about 5 hours to about 24 hours, about 6 hours to about 24 hours, etc., and / or drying the carbonatable mixture at a temperature of about 0.05 inches to about 1.5 inches, about 0.1 inches to about 1 inch, about 0.15 inches to about 0.95 inches, about 0.2 inches to about 0.9 inches, about 0.25 inches to about 0.85 inches, about 0.3 inches to about 0.8 inches, about 0.35 inches, etc., prior to subjecting the carbonatable mixture to a carbonation cycle. The method may further include spreading the mixture into a layer having a thickness of about 0.75 inches, about 0.4 inches to about 0.7 inches, about 0.45 inches to about 0.65 inches, about 0.5 inches to about 0.6 inches, etc., and / or deagglomerating the mixture, and / or rewetting and stirring or agitating the carbonatable mixture after each of a plurality of carbonation cycles, and / or grinding the carbonation-assisted cementitious material, and / or wetting the gas including carbon dioxide prior to providing the gas during a plurality of carbonation cycles, wherein wetting the gas comprises bubbling the gas in hot water. The values ​​of the numerical ranges above may be equal to any integer value or multiple values ​​in the numerical ranges above, including the end points of these ranges.

[0030] The average particle size (d50) of the carbonation-assisted cementitious cement after completion of multiple grinding cycles can be about 1 μm to about 25 μm, about 2 μm to about 25 μm, about 4 μm to about 24 μm, about 6 μm to about 24 μm, about 7 μm to about 23 μm, about 8 μm to about 22 μm, about 9 μm to about 21 μm, about 10 μm to about 20 μm, etc. The average particle size (d50) can be equal to any integer value or multiple values ​​in the above numerical ranges, including the endpoints of these ranges. The particle sizes described in this application are measured using a laser diffraction particle size analyzer.

[0031] The BET surface area of ​​the carbonation-assisted cementitious material prepared according to the method described herein is about 5 m 2 / g ~ approx. 25m 2 / g, approx. 5m 2 / g~about 20m 2 / g, approx. 5m 2 / g ~ approx. 18m 2 / g, approx. 5m 2 / g ~ approx. 15m 2 / g, approx. 6m 2 / g ~ approx. 15m 2 / g, about 7m 2 / g ~ approx. 15m 2 / g, approx. 8m 2 / g ~ approx. 15m 2 / g, approx. 9m 2 / g ~ approx. 15m 2 / g, etc. The BET surface area may be equal to any integer value or values ​​within the numerical ranges recited above, including the endpoints of these ranges. The nitrogen adsorption method is used to measure the BET surface area as described in this application.

[0032] The gas used for carbonation may contain about 5% to about 100% by volume, about 10% to about 100% by volume, about 20% to about 100% by volume, about 30% to about 100% by volume, about 40% to about 100% by volume, about 50% to about 100% by volume, about 60% to about 100% by volume, about 70% to about 100% by volume, about 80% to about 100% by volume, about 90% to about 100% by volume. The carbon dioxide content may be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0033] The gas comprising carbon dioxide may be obtained from flue gas. However, the gas comprising carbon dioxide is not limited thereto and any suitable gas source comprising carbon dioxide may be used. For example, many industrial gas suppliers provide tanked carbon dioxide gas, compressed carbon dioxide gas, liquid carbon dioxide in various purities. Alternatively, carbon dioxide may be recovered as a by-product from any suitable industrial process. As used herein, carbon dioxide sources from by-products of industrial processes are generally referred to as "flue gas". The flue gas may undergo further processing, such as purification, as necessary, before being introduced into the carbonatable material. As a non-limiting example, carbon dioxide may be recovered from cement plants, power plants, and the like.

[0034] The flow rate of the gas, including carbon dioxide, as measured by a gas flow meter or calibrated valve may be from about 1 L / min to about 10 L / min, from about 1.5 L / min to about 9 L / min, from about 2 L / min to about 8 L / min, from about 2.5 L / min to about 7 L / min, from about 3 L / min to about 6 L / min, etc., per kilogram of carbonatable material. The flow rate may be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0035] The carbonation process may include flowing the carbon dioxide for about 0.5 hours to about 24 hours, about 1 hour to about 24 hours, about 1.5 hours to about 20 hours, about 2 hours to about 15 hours, about 5 hours to about 10 hours, about 4 hours to about 6 hours, etc. The time for flowing the gas can be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0036] The gas comprising carbon dioxide may be flowed over the carbonatable material at a temperature of about 1° C. to about 99° C., about 5° C. to about 90° C., about 10° C. to about 85° C., about 20° C. to about 80° C., about 30° C. to about 70° C., etc. The temperature may be equal to any integer value or value within these ranges, including the endpoints of these ranges.

[0037] One or more additives may be added to the carbonatable material, for example, polycarboxylic ethers (PCEs), dispersants such as sugars, set retarders such as sugars, citric acid and its salts, carbonation enhancing additives such as acetic acid and its salts, vinegar, etc.

[0038] The multiple milling cycles may be carried out using any suitable equipment, including but not limited to a ball mill, a vertical roller mill, a belt roller mill, a granulator, a hammer mill, an attrition mill, a grinding roller, a peeling roller mill, an air swept roller mill, or combinations thereof.

[0039] The predetermined temperature of the carbonate material can be about 50° C. to about 150° C., about 55° C. to about 145° C., about 60° C. to about 140° C., about 65° C. to about 130° C., about 70° C. to about 120° C., about 75° C. to about 125° C., about 85° C. to about 115° C., etc. The temperature can be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0040] The starting liquid to solids ratio (L / S) of the mixture including the carbonatable material and water can be from about 0.01 to about 2.5, from about 0.01 to about 2.0, from about 0.02 to about 1.5, from about 0.03 to about 1.0, from about 0.04 to about 0.09, from about 0.05 to about 0.8, from about 0.05 to about 0.6, from about 0.05 to about 0.45, from about 0.1 to about 0.25, etc. The L / S ratio can be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0041] The CO2 uptake of the carbonation-assisted cementitious material prepared using this method can be about 5% to about 40%, about 8% to about 35%, about 10% to about 30%, about 12% to about 25%, about 14% to about 20%, about 16% to about 18%, where the CO2 uptake is measured as the percentage change in mass of the cement after carbonation. The carbon dioxide uptake can be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0042] In accordance with an exemplary embodiment of the present invention, a carbonatable material can be prepared by mixing a first raw material having a first concentration of M and reacting it with a second raw material having a second concentration of Me to produce a carbonatable material having the general formula M a Me b O c , M a Me b (OH) d , M a Me b O c (OH) d , or M a Me b O c (OH) d (H2O) ewherein M is at least one metal capable of reacting to form a carbonate salt, and Me is at least one element capable of forming an oxide during the carbonation reaction.

[0043] As described, M in the first raw material has the general formula M a Me b O c , M a Me b (OH) d , M a Me b O c (OH) d , or M a Me b O c (OH) d (H2O) e The first raw material may include any metal that can become carbonate when present in a synthetic formulation having a first concentration of M. For example, M may be any alkaline earth element, preferably calcium and / or magnesium. The first raw material may be any mineral and / or by-product having a first concentration of M.

[0044] As described, Me in the second feedstock has the general formula M a Me b O c , M a Me b (OH) d , M a Me b O c (OH) d , or M a Me b O c (OH) d (H2O) eThe second raw material may include any element that can form an oxide by hydrothermal disproportionation reaction when present in a synthetic formulation having the above formula. For example, Me may be silicon, titanium, aluminum, phosphorus, vanadium, tungsten, molybdenum, gallium, manganese, zirconium, germanium, copper, niobium, cobalt, lead, iron, indium, arsenic, sulfur, and / or tantalum. In a preferred embodiment, Me includes silicon. The second raw material may be any one or more minerals and / or by-products having a second concentration of Me.

[0045] According to an exemplary embodiment of the present invention, the first and second concentrations of the first and second raw materials are prepared by mixing the first and second raw materials in a predetermined ratio to form a mixture of the general formula M a Me b O c , M a Me b (OH) d , M a Me b O c (OH) d , or M a Me b O c (OH) d (H2O) e and the resulting composite formulation may undergo a carbonation reaction. In one or more exemplary embodiments, the composite formulation may have an a:b ratio between about 2.5:1 and about 0.167:1 undergoes a carbonation reaction. The composite formulation may have an O concentration of c, where c is 3 or greater. In other embodiments, the composite formulation may have an OH concentration of d, where d is 1 or greater. In further embodiments, the composite formulation may also have an HO concentration of e, where e is 0 or greater.

[0046] The synthetic formulation reacts with carbon dioxide in a carbonation process whereby M reacts to form a carbonate phase and Me reacts to form an oxide phase by hydrothermal disproportionation.

[0047] In one example, M in the first feedstock contains a significant concentration of calcium, and Me in the second feedstock contains a significant concentration of silicon. In an exemplary embodiment, the first feedstock can contain an amount of M such as about 30% to about 60%, and the second feedstock can contain an amount of Me such as about 30% to about 60%. The carbon dioxide absorption rate can be equal to any integer value or value within these ranges, including the endpoints of these ranges.

[0048] Thus, for example, a first raw material may be or may include limestone having a first concentration of calcium. A second raw material may be or may include shale having a second concentration of silicon. The first and second raw materials are then mixed and reacted in a predetermined ratio to produce a compound of the general formula (Ca w M x ) a (Si y Me z ) b O c , (Ca w M x ) a (Si y ,Me z ) b (OH) d , or (Ca w M x ) a (Si y ,Me z ) b O c (OH) d (H2O) eThe reaction product includes at least one synthetic blend having a ratio of a:b, where M may include one or more additional metals other than calcium that may react to form carbonates, and Me may include one or more elements other than silicon that may form oxides during the carbonation reaction. The limestone and shale in this example may be mixed in a ratio a:b such that the resulting synthetic blend can undergo a carbonation reaction as explained above. The resulting synthetic blend may be, for example, wollastonite, CaSiO3, with an a:b ratio of 1:1. However, for synthetic blends where M is primarily calcium and Me is primarily silicon, an a:b ratio of about 2.5:1 to about 0.167:1 is believed to be capable of undergoing a carbonation reaction, since outside this range greenhouse gas emissions may not be reduced, energy consumption may not be achieved, and sufficient carbonation may not occur. For example, if the a:b ratio is greater than 2.5:1, the blend will be rich in M, requiring more energy and more CO2 emissions. On the other hand, if the a:b ratio is less than 0.167:1, the mixture will be rich in Me and insufficient carbonation may not occur.

[0049] In another example, M in the first raw material contains significant concentrations of calcium and magnesium. Thus, for example, the first raw material can be or include dolomite having a first concentration of calcium, and the composite formulation can be represented by the general formula (Mg u Ca v M w ) a (Si y ,Me z ) b O c or (Mg u Ca v M w ) a (Si y Me z ) b (OH) dwhere M may include one or more additional metals other than calcium and magnesium that may react to form carbonates, and Me may include one or more elements other than silicon that may form oxides during the carbonation reaction. In another example, Me in the first feedstock includes significant concentrations of silicon and aluminum, and the synthetic formulation has the general formula (Ca v M w ) a (Al x S y ,Me z ) b O c or (Ca v M w ) a (Al x S y ,Me z ) b (OH) d , (Ca v M w ) a (Al x S y ,Me z ) b O c (OH) d or (Ca v M w ) a (Al x S y ,Me z ) b O c (OH) d (H2O) e has.

[0050] Compared to Portland cement having an a:b ratio of about 2.5:1, the exemplary composite mix of the present invention results in reduced CO2 emissions and requires less energy to form the composite mix, as described in more detail below. The reduced CO2 emissions and lower energy requirements are achieved for several reasons. First, less raw material such as limestone is used compared to an equivalent amount of Portland cement, so less CaCO3 is converted. Also, because less raw material is used, less heat (energy) is required to decompose the raw materials and cause the carbonation reaction.

[0051] Other specific examples of carbonatable materials consistent with the above are described in U.S. Pat. No. 9,216,926, U.S. Provisional Application No. 63 / 151,971, and corresponding U.S. patent application Ser. No. 17 / 675,777, which are hereby incorporated by reference in their entireties.

[0052] According to further embodiments, the carbonatable material comprises, consists essentially of, or consists of various calcium silicates. The molar ratio of element Ca to element Si in the composition is from about 0.8 to about 1.2. The composition is composed of a blend of discrete crystalline calcium silicate phases selected from one or more of CS (wollastonite or pseudowollastonite), C3S2 (rankinite), and C2S (belite or larnite or bredigit) at about 30% or more by weight of the total phases. The calcium silicate composition is characterized by having about 30% or less metal oxides of Al, Fe, and Mg based on the total oxide weight, and being suitable for carbonation with CO2 at temperatures between about 30°C and about 95°C, or between about 30°C and about 70°C to form CaCO3 with a mass gain of about 10% or more. The calcium silicate composition may also include a small amount of C3S (alite, Ca3SiO5). The C2S phase present within the calcium silicate composition may be either the α-Ca2SiO4, β-Ca2SiO4 or γ-Ca2SiO4 polymorphs, or combinations thereof. The calcium silicate composition may also contain small amounts of residual CaO (lime) and SiO2 (silica).

[0053] In addition to the crystalline phases described above, calcium silicate compositions may contain amorphous (non-crystalline) calcium silicate phases. The amorphous phases may further contain Al, Fe, Mg ions and other impurity ions present in the raw materials. Each of these crystalline and amorphous calcium silicate phases is suitable for carbonation with CO2. Calcium silicate compositions may also contain small amounts of residual CaO (lime) and SiO2 (silica).

[0054] Each of these crystalline and amorphous calcium silicate phases is suitable for carbonation with CO2.

[0055] Calcium silicate compositions also have the general formula (Ca,Na,K)2[(Mg,Fe 2+ , Fe 3+ It may contain significant amounts of inert phases such as melilite-type minerals (melilite, gehlenite, or kermanite) having the general formula Ca(Al,Fe)O 3+ )2O5) ferrite type minerals (ferrite, brownmillerite, or C4AF). In certain embodiments, the calcium silicate composition is composed exclusively of an amorphous phase. In certain embodiments, the calcium silicate comprises exclusively a crystalline phase. In certain embodiments, some of the calcium silicate composition is present in an amorphous phase and some in a crystalline phase.

[0056] Each of these calcium silicate phases is suitable for carbonation with CO2. Hereinafter, the discrete calcium silicate phases suitable for carbonation are referred to as reactive phases. The reactive phases may be present in any suitable amount in the composition. In certain preferred embodiments, the reactive phase is present at about 50% by weight or greater.

[0057] The various reaction phases may comprise any suitable portion of the total reaction phase. In certain preferred embodiments, the CS reaction phase is present at about 10 to about 60 wt%, C3S2 at about 5 to 50 wt%, C2S at about 5 wt% to 60 wt%, and C at about 0 wt% to 3 wt%. The amount of the CS reaction phase can be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0058] In certain embodiments, the reaction phase comprises, by weight of the total phase, for example, about 40% or more, about 45% or more, about 50% or more, about 55% or more, about 60% or more, about 65% or more, about 70% or more, about 75% or more, about 80% or more, about 85% or more, about 90% or more, about 95% or more, etc., of calcium silicate-based amorphous phase. It is noted that the amorphous phase may further incorporate impurity ions present in the raw materials. The percentage of amorphous phase may be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0059] It is to be understood that the calcium silicate compositions, phases and methods disclosed herein can be employed to use magnesium silicate phases in place of or in addition to calcium silicate phases. As used herein, the term "magnesium silicate" refers to, for example, Mg2SiO4 (also known as "forsterite") and Mg3SiO4. 10 It refers to naturally occurring minerals or synthetic materials composed of one or more of a group of magnesium-silicon containing compounds including (OH)2 (also known as "talc") and CaMgSiO4 (also known as "monticellite"), each of which may contain one or more other metal ions and oxides (e.g., calcium, aluminum, iron or manganese oxides), or blends thereof, or may contain calcium silicate in natural or synthetic forms in amounts ranging from trace amounts (1%) to about 50% or more by weight.

[0060] Other specific examples of carbonatable calcium silicate materials consistent with the above are described in US Pat. No. 10,173,927, the entirety of which is incorporated herein by reference.

[0061] Additionally, the cementitious material may include calcium silicate, calcium carbonate, and amorphous silica. The amorphous silica content may be about 5% to about 50%, about 8% to about 45%, about 8% to about 40%, about 9% to about 40%, about 10% to about 40%, about 20% to about 40%, and the amorphous silica reacts with calcium hydroxide to form a calcium silicate hydrate gel. The amorphous silica content may be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges.

[0062] The cement or concrete described herein may include multiple bonding elements, each bonding element including a core (non-carbonated cement), a first layer rich in silica at least partially covering the periphery of the core, and a second layer rich in calcium carbonate and / or magnesium carbonate at least partially covering the periphery of the first layer. As used herein, the terms "rich in silica" and "rich in calcium carbonate and / or magnesium carbonate" may mean that the silica and calcium carbonate and / or magnesium carbonate content, respectively, is greater than 50% by weight or volume of the total mass or volume of the components of the respective layer.

[0063] The silica-rich first layer may include amorphous silica. The amount of amorphous silica in the silica-rich layer may be greater than the amount of amorphous silica in a cement or concrete prepared without curing the mixture in a Ca(OH)2 solution.

[0064] The silica-rich layer further reacts with Ca(OH)2 produced by ordinary Portland cement (OPC) hydration to form additional CSH (pozzolanic reaction), and calcium carbonate from the auxiliary cementitious materials reacts with OPC to form monocarbonate.

[0065] The carbonatable material may include calcium silicate having a molar ratio of element Ca to element Si of about 0.5 to about 1.5, about 0.6 to about 1.4, about 0.7 to about 1.3, about 0.8 to about 1.2, about 0.9 to about 1.1, etc. The molar ratio may be equal to any integer value or value within these ranges, including the endpoints of these ranges.

[0066] The carbonatable material may comprise a blend of discrete crystalline calcium silicate phases selected from one or more of CS (wollastonite or pseudowollastonite), C3S2 (rankinite) and C2S (belite or larnite or breathite), preferably at about 20% or more, about 25% or more, about 30% or more, about 35% or more, about 40% or more, about 45% or more, about 50% or more, about 55% or more, about 60% or more, about 65% or more, about 70% or more, about 75% or more, about 80% or more, about 85% or more, about 90% or more, etc., by weight of all phases, and may be about 99% or less, about 98% or less, about 97% or less, about 96% or less, about 95% or less, etc. The blend of discrete crystalline calcium silicate phases may include about 50% or less, about 45% or less, about 40% or less, about 35% or less, about 30% or less, about 25% or less, about 20% or less, about 15% or less, about 10% or less, about 5% or less, etc., of metal oxides of Al, Fe and Mg based on total oxide mass. The amount of the blend of discrete crystalline calcium silicate phases may be equal to any integer value or value within these ranges, including the endpoints of these ranges. The carbonateable material may further include an amorphous calcium silicate phase.

[0067] Other non-limiting examples of supplemental cementitious materials consistent with the above, their methods of manufacture, and their incorporation into ordinary Portland cement and the like, are described in U.S. Provisional Application No. 63 / 217,574 and corresponding U.S. Patent Application No. 17 / 854,778, which are hereby incorporated by reference in their entireties.

[0068] Additionally, the above pozzolanic reactions include the term "pozzolans," which broadly encompasses siliceous or alumino-siliceous and aluminous materials that do not have intrinsic cementitious properties but can chemically react (or be activated) with calcium hydroxide in the presence of water to form cementitious compounds. Pozzolanic materials are also referred to as activatable amorphous phases. Historically, natural materials containing volcanic glass components were used in combination with hydrated lime to create mortars that were essential to ancient building practices. In modern times, many pozzolanic materials are used in combination with hydraulic cements. These include materials such as fly ash, ground granulated blast furnace slag (GGBFS), silica fume, organic incineration residues (such as rice husk ash), reactive metakaolin (calcined clay), calcined shale, volcanic ash, pumice, and diatomaceous earth.

[0069] A reduction in the volumetric CO2 emissions of concrete products is made possible in many applications by the use of such pozzolans, which include a range of natural materials and industrial by-products that have the ability to partially replace Portland cement in concrete while contributing to the strength of the final concrete component. These materials can replace significant amounts of Portland cement, in some cases up to 80%, due to their contribution to the strength of the material.

[0070] The pozzolanic reaction in a typical hydraulic cement system is simply the reaction of portlandite (Ca(OH)2) with silicic acid (H4SiO4), supplied by the hydraulic cement component. This reaction generally produces a compound called calcium silicate hydrate (CSH), commonly written as CaH2SiO4·2H2O. In practice, the CSH phase can have a wide variety of Ca / Si molar ratios and a wide variety of crystal water contents. Further details of the pozzolanic reaction are described in U.S. Pat. No. 10,662,116, which is incorporated herein by reference in its entirety.

[0071] Another exemplary embodiment is directed to a method for forming a cement or concrete, the method including forming a carbonation-assisted cementitious material according to any of the exemplary methods described herein, combining the carbonation-assisted cementitious material with a hydraulic cement composition to form a mixture, the mixture including about 1% to about 99% by weight of the carbonation-assisted cementitious material based on the total weight of solids in the mixture, and reacting the mixture with water to form the cement or concrete. The mixture may include about 20% to about 35% by weight of the carbonation-assisted cementitious material based on the total weight of solids in the mixture. The amounts of the various components of the mixture may be equal to any integer value or value within these ranges, including the endpoints of these ranges. The hydraulic cement may include one or more of ordinary portland cement (OPC), calcium sulfoaluminate cement (CSA), belite cement, or other calcium-based hydraulic materials. The method may further include adding aggregate to the mixture, the aggregate may be coarse aggregate and / or fine aggregate. The resulting cement or concrete may be suitable for a variety of applications including, but not limited to, foundations, roadbeds, sidewalks, building slabs, pavers, CMUs, wet cast tiles, split retaining walls, hollow core slabs, and other cast and precast applications. The resulting cement or concrete may also be suitable for use in preparing mortars suitable for masonry applications.

[0072] Other non-limiting examples of carbonateable calcium silicate materials, and additional details of supplemental cementitious materials and their incorporation into conventional Portland cement and the like consistent with the above, are described in U.S. Provisional Application No. 63 / 151,971 and corresponding patent application Ser. No. 17 / 675,777, which are hereby incorporated by reference in their entireties.

[0073] The strength activity index (SAI) of the cement or concrete prepared using any of the methods described herein can be at least about 50%, about 50% to about 150%, about 55% to about 145%, 60% to about 140%, about 65% to about 135%, about 70% to about 130%, about 75% to about 120%, etc., where the SAI is measured at 20% replacement of OPC in the mortar mixture according to ASTM C618. The strength activity index is the ratio of the compressive strength of the cement or concrete containing about 20% by weight of a carbonation-assisted cementitious material to the compressive strength of the cement or concrete containing about 0% by weight of a carbonation-assisted cementitious material, based on the total weight of solids in the mixture. The strength activity index can be equal to any integer value or values ​​within these ranges, including the endpoints of these ranges. The strength activity index of a cement or concrete measured 28 days or more after the cement or concrete is formed may be higher than the strength activity index of a cement or concrete measured 7 days or less after the cement or concrete is formed. The strength activity index of a cement or concrete produced with a carbonation-assisted cementitious material after grinding is higher than the strength activity index of a cement or concrete produced with a carbonation-assisted cementitious material without grinding.

[0074] When the carbonated cementitious material is ground for about 5 minutes to about 10 minutes, the strength activity index of the cement or concrete measured about 7 days after the formation of the cement or concrete is about 5% to about 20%, about 6% to about 18%, about 7% to about 16%, about 7.5% to about 14%, about 8% to about 13%, about 8.5% to about 13%, about 9% to about 12%, etc., higher than the strength activity index of the cement or concrete measured about 7 days after the formation of the cement or concrete without grinding the carbonated cementitious material.

[0075] As the results of the examples of this application show, intermediate grinding, whereby the carbonated cementitious material is ground prior to further carbonation, not only increases the rate of CO2 uptake, but also activates the amorphous silica in the silica-rich layer and promotes the pozzolanic reaction between the silica-rich layer and Ca(OH)2 produced by hydration of Ordinary Portland Cement (OPC) to form additional CSH, resulting in a cement or concrete with an unexpectedly high strength activity index that is maintained and / or increased over time.

[0076] The principles of the present invention, as well as certain illustrative features and embodiments thereof, will now be illustrated with reference to the following non-limiting examples. EXAMPLES

[0077] Material Processing - Steam Treatment

[0078] An example of material processing is steaming. In this method, a steamer is preheated to a predetermined temperature ranging from 30°C to 90°C. A sample containing 10.0 g of carbonatable powder material and 2.0 g of tap water (L / S ratio = 0.20) is kneaded in a ziplock plastic bag for about 1 min to mix well, then a small piece of the mixture is quickly placed in an aluminum pan with a known tare. The pan is placed on a metal tray with a cone placed on it and set in the steamer. Steaming is performed at a temperature of 68°C and a pressure of 3 psi CO2. Carbonation time is 60 min with a fan speed of 400 rpm. The sample is dried overnight at 80°C.

[0079] Material Processing - Mixing

[0080] Another example of material processing involves mixing. In this method, 250 g of carbonate powder (solid) is ground in a planetary ball mill for 5 minutes and mixed with 582.5 g of tap water to prepare a mixture with an L / S ratio of 2.33. The mixture is stirred at 400 rpm with a Rushton impeller under 100% CO2 with a flow rate of 1552 mL / min at a temperature of 60 °C for 1 hour. At the end of the carbonation process, the slurry is filtered through a membrane and the wet cake is dried at 80 °C overnight.

[0081] Grinding effect of Solidia SCM

[0082] Carbonated Solidia SCM was produced using a slurry carbonation process and dried to produce dry Solidia SCM. Six batches of such SCM were produced and characterized. All six batches produced were blended at a third-party blending facility (Empire Blending "EB") to avoid batch-to-batch variations that would affect performance evaluation. The blended materials of Examples 1-3 were ground in a Retch planetary ball mill for 1, 5, and 10 minutes, respectively, and the mortar performance of the blended materials was subsequently measured. Table 1 shows the particle size distribution and surface area measured using the BET method for the pre-ground blended materials (EB1, Comparative Example 1) and the ground blended materials of Examples 1-3.

[0083] [Table 1]

[0084] As shown in Table 1, grinding produces very fine material with a corresponding increase in BET surface area.

[0085] Table 2 summarizes the mortar fluidity and compressive strength performance at 20% replacement (water-to-cement ratio of 0.485) of ordinary Portland cement (OPC) (20% EB1 blend, Comparative Example 2) and 20% EB1 ground for 1, 5 and 10 minutes (Examples 4-6, respectively). The flow data measured according to ASTM C230 are shown in Figure 1 and the SAI data measured according to ASTM C618 are shown in Figure 2.

[0086] [Table 2]

[0087] As shown in Table 2, grinding the supplementary cementitious materials for 5 min did not further increase the water demand, and the strength activity index increased by about 10% upon grinding. The CO2 uptake rates of these materials were measured with a calcium meter and are shown in Table 3 and Figure 3.

[0088] [Table 3]

[0089] As shown in Figure 3, when multiple grinding cycles are performed, the CO2 absorption rate increases significantly. For example, as shown in Table 3, after multiple grinding cycles with a total carbonation time of 75 minutes, the CO2 absorption rate increases by about 125%.

[0090] The results shown in Table 3 and Figure 3 indicate that grinding between carbonation steps increases the CO2 absorption rate in a short period of time. For example, as shown in Table 3 (Examples 12 and 13), grinding for 5 minutes achieves an increase in CO2 absorption rate of about 5%.

[0091] As explained above, the carbonated SCM used in these examples was made using a slurry carbonation process. In this process, a slurry of carbonatable material and water was dried in a tray. Further details of the slurry process are described in U.S. Provisional Application No. 63 / 151,971 and corresponding U.S. Application No. 17 / 675,777, the contents of which are incorporated by reference as if fully set forth herein. The dried powder was further milled for 1, 5, and 10 minutes. The intact dried and milled materials were replaced with 20 wt% OPC in the mortar mix to evaluate the effect of milling on flow and strength development. Table 2 shows the flow performance of the milled EB samples. As also shown in Table 2 (Example 5), the 7-day Strength Activity Index (SAI) increases substantially from about 90% (20% EB without milling) to about 98% after 1 minute of milling, and exceeds 100% after 5 minutes or more of milling.

[0092] Materials characterization

[0093] The particle size distribution and surface area of ​​the materials are measured using laser diffraction and BET methods for the initial and processed materials, respectively. The particle size and surface area measurements are shown in Table 1. The properties of the SCM prepared using the slurry method are also shown in Table 1 (Comparative Example 1).

[0094] Mortar performance - flow measurement

[0095] The flow of mortar (a mixture of ASTM sand and cementitious material) was measured at 20% (w / c 0.485) replacement level of OPC with ASTM C109 ratio of cement to sand. The flow of the crushed material is shown in Figure 1. No increase in water demand was observed at replacement levels of 20%, 35%, and 50%, which are comparable to the flow rate of 100% OPC mortar.

[0096] Mortar performance - Compressive strength

[0097] The mortars made for flow were also cast for compressive strength measurements. Figure 2 shows the Strength Activity Index (SAI) of the mortars. SAI is the ratio of the compressive strength of SCM mortar with 20% replacement to the compressive strength of 100% OPC mortar. All mortar cubes were cast in a temperature and humidity controlled environment.

[0098] Solidia SCM produced by the carbonation process described in this application, which includes at least one grinding cycle, had a much lower surface area than SCM produced using a slurry process. Grinding the material improved the strength activity index at 28 days. Despite the lower surface area, the strength activity index of the ground material was comparable to the SCM produced using the slurry process.

[0099] Since various modifications can be made to the above-mentioned method and composition without departing from the scope of the present invention, all matters contained in the above description are intended to be interpreted as illustrative and not limiting. Numerical values ​​expressing amounts of ingredients, components, reaction conditions, and the like used herein are interpreted as encompassing the exact numerical values ​​specified herein, and are interpreted in all cases as modified by the term "about". Notwithstanding the numerical ranges and parameters described, the broad scope of the subject matter described herein is approximate, and the numerical values ​​described are indicated as precisely as possible. However, any numerical value may inherently contain certain errors or imprecision, as evidenced by the standard deviation found in each measuring technique. None of the features described herein should be interpreted as invoking the 6th paragraph of Section 112 of the U.S. Patent Act, unless the term "means" is explicitly used.

Claims

1. 1. A method for preparing a carbonation-assisted cementitious material, the method comprising: adding water to the carbonatable materials to form a carbonatable mixture, the mixture having a water content of about 0.1% to about 99.99% by weight; agitating or stirring the carbonatable mixture for about 1 minute to about 24 hours; carbonating the carbonatable mixture to obtain a first carbonated cementitious material; grinding the first carbonated cementitious material for about 0.1 minutes to about 60 minutes to obtain a ground mixture; carbonating the ground mixture for about 1 minute to about 24 hours to obtain a carbonated assisted cementitious material; Including, 11. The method of preparing a carbonation assisted cementitious material, wherein carbonating the carbonatable mixture and the ground mixture comprises flowing a gas comprising about 5% to about 100% by volume carbon dioxide through the carbonatable mixture and the ground mixture, respectively, and maintaining a temperature of about 1° C. to about 99° C. to obtain the carbonation assisted cementitious material.

2. The method of claim 1 , wherein the water content of the carbonatable mixture is from about 0.1% to about 90% by weight.

3. The method of claim 1 , wherein the method includes multiple carbonation cycles alternating with multiple grinding and wetting cycles.

4. 10. The method of claim 1, further comprising steaming the ground mixture prior to carbonating the ground mixture, the steaming comprising exposing the ground mixture to vapor or steam at a temperature of about 20° C. to about 200° C.

5. 10. The method of claim 1, further comprising drying the carbonation-assisted cementitious material at a temperature of from about 20° C. to about 500° C. for from about 1 minute to about 24 hours.

6. The method of claim 1 further comprising the step of deagglomerating the mixture.

7. The method of claim 1 further comprising obtaining a gas comprising carbon dioxide from the exhaust gas.

8. 2. The method of claim 1, wherein the grinding is carried out in a mill selected from a ball mill, a vertical roller mill, a belt roller mill, a granulator, a hammer mill, an attrition mill, a grinding roller, a peeling roller mill, an air swept roller mill, or a combination thereof.

9. 10. The method of claim 1, further comprising the step of humidifying the gas prior to carbonation, wherein humidifying the gas comprises bubbling the gas in hot water.

10. 10. The method of claim 1, wherein the flow rate of the gas comprising carbon dioxide is from about 1 L / min / Kg to about 6 L / min / Kg per kilogram of carbonatable material.

11. The method of claim 1 , wherein flowing the gas comprising carbon dioxide occurs for a period of from about 1 minute to about 24 hours.

12. 2. The method of claim 1, wherein the carbonation assisted cementitious material has an average particle size (d50) of from about 1 μm to about 25 μm.

13. The BET surface area of ​​the carbonation-assisted cementitious material is about 5 m 2 / g ~ approx. 25m 2 The method of claim 1, wherein the molecular weight is 1 / g.

14. 10. The method of claim 1, wherein the carbonation assisted cementitious material has a carbon dioxide absorption rate of about 5% to about 40%.

15. The carbonatable material has the general formula M a Me b O c , M. a Me b (OH) d , M. a Me b O c (OH) d , or M a Me b O c (OH) d ・(H 2 O) e wherein M is at least one metal capable of reacting to form a carbonate and Me is at least one element capable of forming an oxide during a carbonation reaction.

16. 16. The method of claim 15, wherein M is calcium and / or magnesium.

17. 16. The method of claim 15, wherein Me is silicon, titanium, aluminum, phosphorus, vanadium, tungsten, molybdenum, gallium, manganese, zirconium, germanium, copper, niobium, cobalt, lead, iron, indium, arsenic, sulfur, and / or tantalum.

18. 16. The method of claim 15, wherein the ratio of a:b is from about 2.5:1 to about 0.167:1, c is 3 or greater, d is 1 or greater, and e is 0 or greater.

19. The method of claim 1 , wherein the carbonatable material comprises calcium silicate having a molar ratio of element Ca to element Si of about 0.8 to about 3.

0.

20. The carbonatable material is CS (wollastonite or pseudowollastonite), C 3 S 2 (rankinite), and C 2 20. The method of claim 19, comprising a blend of discrete crystalline calcium silicate phases selected from one or more of: S (Belite or Larnite or Bredigit) at 30% or more by weight of total phases, and metal oxides of Al, Fe, and Mg at 30% or less by total oxide weight.

21. 20. The method of claim 19, wherein the carbonatable material comprises calcium silicate hydrate (C-S-H), recycled concrete, municipal waste, mine tailings, or mixtures thereof.

22. The method of claim 15 , wherein the carbonatable material further comprises an amorphous calcium silicate phase.

23. 1. A method of forming cement or concrete, the method comprising: forming a carbonation-assisted cementitious material according to the method of claim 1; combining the carbonation supplemented cementitious material with a hydraulic cement composition to form a cementitious material mixture, the cementitious material mixture comprising from about 1% to about 99% by weight of the carbonation supplemented cementitious material, based on the total weight of solids in the mixture; reacting the cementitious material mixture with water to form the cement or concrete; 23. A method of forming cement or concrete comprising:

24. 24. The method of claim 23, wherein the cementitious material mixture comprises about 20% to about 35% by weight of carbonation-assisted cementitious material, based on the total weight of solids in the mixture.

25. 24. The method of claim 23, wherein the hydraulic cement composition comprises one or more of ordinary portland cement (OPC), calcium sulfoaluminate cement (CSA), belite cement, or other calcium-based hydraulic material.

26. 24. The method of claim 23, further comprising adding aggregate to the cementitious material mixture.

27. the cement or concrete has a strength activity index of about 75% to about 120%; 24. The method of claim 23, wherein the strength activity index is the ratio of the compressive strength of the cement or concrete containing about 20% by weight of the carbonation assisted cementitious material to the compressive strength of the cement or concrete containing about 0% by weight of the carbonation assisted cementitious material, based on the total weight of solids in the mixture.

28. grinding the first carbonated cementitious material for about 5 minutes to about 60 minutes; a strength activity index of the cement or concrete obtained after grinding the first carbonated cementitious material is about 7% to about 15% higher than a strength activity index of the cement or concrete obtained without grinding, when measured 7 days after formation of the respective cement or concrete; 24. The method of claim 23, wherein the strength activity index is the ratio of the compressive strength of the cement or concrete containing about 20% by weight of the carbonation assisted cementitious material to the compressive strength of the cement or concrete containing about 0% by weight of the carbonation assisted cementitious material, based on the total weight of solids in the mixture.

29. 29. The method of claim 28, wherein the strength activity index of the cement or concrete obtained after grinding the first carbonated cementitious material for about 5 minutes to about 10 minutes is about 8.5% to about 13% higher than the strength activity index of the cement or concrete obtained without grinding, when measured 7 days after formation of the respective cement or concrete.

30. the strength activity index of the cement or concrete measured 28 days after the formation of the cement or concrete is higher than the strength activity index of the cement or concrete measured 7 days after the formation of the cement or concrete; 24. The method of claim 23, wherein the strength activity index is the ratio of the compressive strength of a cement or concrete containing about 20 wt.% of the carbonation assisted cementitious material to the compressive strength of a cement or concrete containing about 0 wt.% of the carbonation assisted cementitious material, based on the total weight of solids in the mixture.