Negative electrode sheet, secondary battery, battery module, battery pack, and power consuming device

The combination of graphite, hard carbon, and a ferroelectric coating in the negative electrode sheet addresses limitations in energy density and charging rates, improving the performance of secondary batteries by enhancing ion storage and preventing dendrite formation.

JP2024539121AActive Publication Date: 2024-10-28CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024523554
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-07-05
Publication Date
2024-10-28
Estimated Expiration
2042-07-05

AI Technical Summary

Technical Problem

Existing negative electrode active materials in secondary batteries, such as graphite and hard carbon, face limitations in energy density, high-rate charging, and cycle life due to issues like dendrite formation and inefficient ion storage.

Method used

A negative electrode sheet design featuring a first layer of graphite, a second layer of hard carbon, and a functional coating layer with a ferroelectric material is used, which enhances ion deposition control and suppresses dendrite growth, improving charging rates and cycle life.

Benefits of technology

The design achieves high energy density, high-rate charging capability, and extended cycle life by optimizing ion storage and preventing dendrite formation, thereby enhancing the performance of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present application provides a negative electrode sheet, a secondary battery, a battery module, a battery pack, and a power consumption device. The negative electrode sheet includes a negative electrode current collector, and a first negative electrode film layer, a second negative electrode film layer, and a functional coating layer, which are sequentially provided on at least one surface of the negative electrode current collector, the functional coating layer including a ferroelectric material, the second negative electrode film layer including a second negative electrode active material including hard carbon, and the first negative electrode film layer including a first negative electrode active material including graphite. The negative electrode sheet according to the present application allows the secondary battery to achieve both a high charge rate and a long cycle life on the premise of having a high energy density.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of batteries, and in particular to a negative electrode sheet, a secondary battery, a battery module, a battery pack, and a power consuming device. [Background technology]

[0002] In recent years, secondary batteries have been widely used in many fields, such as energy storage power systems such as hydroelectric, thermal, wind and solar power plants, as well as electric tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and many other fields. With the application and popularity of secondary batteries, the requirements for the energy density, cycle performance and high-rate charging performance of secondary batteries are becoming increasingly higher. As an important component of secondary batteries, the negative electrode active material has a certain degree of influence on the performance of secondary batteries. Graphite is one of the most commonly used negative electrode active materials in secondary batteries, and has the advantages of small polarization and high cycle stability, but its theoretical capacity per gram is only 372mAh / g. At present, the performance of commercial graphite has been developed to its limit, and the room for improvement of its reversible capacity per gram and energy density is very limited. At the same time, the layer spacing of graphite is small, and its high-rate charging performance has also been developed to its limit. Hard carbon, as a new negative electrode active material, can realize rapid insertion and desorption of active ions during the charge and discharge process of secondary batteries, and has a very broad future development potential. However, the compaction degree and initial coulombic efficiency of commercial hard carbon are low, and there is a limit to improving the energy density of secondary batteries. Summary of the Invention

[0003] An object of the present application is to provide a negative electrode sheet, a secondary battery, a battery module, a battery pack, and a power consuming device that achieve both a high charge rate and a long cycle life, on the premise that the secondary battery has a high energy density.

[0004] A first aspect of the present application provides a negative electrode sheet including a negative electrode current collector, and a first negative electrode film layer, a second negative electrode film layer, and a functional coating layer, which are sequentially provided on at least one surface of the negative electrode current collector, wherein the functional coating layer includes a ferroelectric material, the second negative electrode film layer includes a second negative electrode active material including hard carbon, and the first negative electrode film layer includes a first negative electrode active material including graphite.

[0005] In the negative electrode sheet of the present application, a first negative electrode film layer containing graphite and a second negative electrode film layer containing hard carbon are sequentially provided on the surface of the negative electrode current collector to perform a combination design, thereby compensating for the defects of graphite and hard carbon and highlighting their respective advantages. A larger layer spacing of the hard carbon can provide a higher charging rate. The first coulombic efficiency of the hard carbon can be compensated for by interposing graphite between the hard carbon and the negative electrode current collector. In addition, since the insertion potential of the active ions into the hard carbon micropore structure is about 0V, which is close to the deposition potential of the active ions on the graphite surface, the micropore structure of the hard carbon cannot function sufficiently as an active ion storage site. However, the inventors of the present application unexpectedly found that the above problem can be solved by providing a functional coating layer containing a ferroelectric material on the surface of the negative electrode sheet. The ferroelectric material can control the deposition method of the active ions to highlight the advantage of the large capacity of the microporous structure of the hard carbon, and can also suppress the active ions from being reduced and continuously precipitated on the graphite surface, thereby improving the cycle life of the secondary battery. Therefore, the secondary battery using the negative electrode sheet of the present application has a long cycle life, can be charged at a high rate, has a high output voltage, and has a high energy density.

[0006] In any embodiment of the present application, the thickness of the functional coating layer is H 1 The thickness of the second negative electrode film layer is H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet is H 1 / (H 2+H 3 ) is 0.01 to 0.15, and is selectably 0.01 to 0.08. This improves the overall performance of the secondary battery, and enables charging at a high rate with a high energy density to be achieved.

[0007] In any embodiment of the present application, the thickness of the functional coating layer is H 1 μm, H 1 is 2 to 10, and is selectable from 4 to 6. This improves the overall performance of the secondary battery, and enables charging at a high rate with a high energy density to be achieved.

[0008] In any embodiment of the present application, the thickness of the second negative electrode film layer is H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet is H 2 / H 3 is 0.10 to 5, and optionally 0.5 to 4. This allows the second negative electrode film layer and the first negative electrode film layer to exhibit a better synergistic effect.

[0009] In any embodiment of the present application, the volume average particle diameter Dv50 of the ferroelectric material is d 1 μm, and d 1 is equal to or less than 1, and is selectable between 0.05 and 0.8. This improves the overall performance of the secondary battery, enables high-rate charging with high energy density, and reduces production costs.

[0010] In any embodiment of the present application, the volume average particle diameter Dv50 of the second negative electrode active material is d 2 μm, and the volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 2 / d 3is 0.1 to 1, and optionally 0.2 to 0.8. In this case, it is advantageous that the second negative electrode film layer improves the high-rate charging ability of the secondary battery, and the first negative electrode film layer fully exerts the effect of improving the initial coulombic efficiency and cycle life of the secondary battery, thereby improving the overall performance of the secondary battery and realizing high-rate charging with high energy density.

[0011] In any embodiment of the present application, the mass percentage of the ferroelectric material in the functional coating layer is W1, and based on the total mass of the functional coating layer, W1 is 70%-95%, optionally 80%-95%, so that the overall performance of the secondary battery is better and high-rate charging with high energy density can be realized.

[0012] In any embodiment of the present application, the mass percentage of hard carbon in the second negative electrode film layer is W2, and based on the total mass of the second negative electrode film layer, W2 is 68% or more, and optionally 90% to 98%, which is advantageous for the secondary battery to have a higher charge rate.

[0013] In any embodiment of the present application, the mass percentage of graphite in the first negative electrode film layer is W3, and based on the total mass of the first negative electrode film layer, W3 is 78% or more, optionally 90% to 98%, which is advantageous for the secondary battery to have a higher initial coulombic efficiency and a longer cycle life.

[0014] In any embodiment of the present application, the volume average particle diameter Dv50 of the second negative electrode active material is d 2 μm, and d 2 is 3 to 11, and selectively 3 to 7. This is advantageous for improving the capacity and energy density of the secondary battery.

[0015] In any embodiment of the present application, the particle size distribution index (Dv90-Dv10) / Dv50 of the second negative electrode active material is 1 and α 1is 0.6 to 5, and is selectable from 1 to 4. This is advantageous for improving the high rate charging capability and charge / discharge efficiency of the secondary battery.

[0016] In any embodiment of the present application, the specific surface area of ​​the second negative electrode active material is 3 m 2 / g~7m 2 / g, selectable 4m 2 / g~6m 2 This is advantageous for improving the high rate charging capability of the secondary battery.

[0017] In any embodiment of the present application, the powder compaction density of the second negative electrode active material at 20000 N is 0.9 g / cm 3 ~1.3g / cm 3 and can be selected from 1g / cm 3 ~1.2g / cm 3 This is advantageous for improving the energy density of the secondary battery.

[0018] In any embodiment of the present application, the second negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the proportion of primary particles in the second negative electrode active material is 90% to 100%, which is advantageous for improving the high-rate charging capability of the secondary battery.

[0019] In any embodiment of the present application, the volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 3 is 9 to 18, and selectively 11 to 15. This is advantageous in that the secondary battery has high initial coulombic efficiency, high energy density, and long cycle life.

[0020] In any embodiment of the present application, the particle size distribution index (Dv90-Dv10) / Dv50 of the first negative electrode active material is α 2 and α 2 is 0.2 to 5, and optionally 0.3 to 4. This is advantageous for improving the cycle performance of the secondary battery.

[0021] In any embodiment of the present application, the specific surface area of ​​the first negative electrode active material is 0.6 m 2 / g~1.5m 2 / g, selectable 0.8m 2 / g~1.4m 2 This is advantageous for improving the cycle performance of the secondary battery.

[0022] In any embodiment of the present application, the powder compaction density of the first negative electrode active material at 20000 N is 1.4 g / cm 3 ~1.85g / cm 3 and selectable, 1.6g / cm 3 ~1.75g / cm 3 This is advantageous for improving the energy density of the secondary battery.

[0023] In any embodiment of the present application, the graphitization degree of the first negative electrode active material is 91% to 95%, and optionally 92% to 94%, which is advantageous for improving the cycle life of the secondary battery.

[0024] In any embodiment of the present application, the first negative electrode active material includes artificial graphite, natural graphite, or a combination thereof, and optionally, the surface of the artificial graphite has a carbon coating layer, which is advantageous for improving the cycle performance and high-rate charging ability of the secondary battery.

[0025] In any embodiment of the present application, the first negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the quantity ratio of the secondary particles in the first negative electrode active material is 80% to 100%, which is advantageous for improving the cycle performance, storage performance, and high-rate charging ability of the secondary battery.

[0026] In any embodiment of the present application, the dielectric constant of the ferroelectric material is 50 or more, and optionally 50-100,000.

[0027] In any embodiment of the present application, the ferroelectric material may include one or more combinations selected from inorganic ferroelectric materials and organic ferroelectric materials, and optionally the inorganic ferroelectric material may include one or more combinations selected from perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layered structure compounds, lithium niobate, lithium tantalate, lead metaniobate, and barium lithium lead niobate, and optionally the organic ferroelectric material may include one or more combinations selected from vinylidene fluoride homopolymer or copolymer, 2,5-dibromo-3,6-dihydroxy-p-benzoquinone, phenazine-chloranilic acid, and croconic acid.

[0028] In any embodiment of the present application, the functional coating layer further comprises an adhesive and / or a dispersing agent, optionally the adhesive comprises one or a combination of one or more selected from styrene butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan, and optionally the dispersing agent comprises sodium carboxymethyl cellulose.

[0029] A second aspect of the present application provides a secondary battery including the negative electrode sheet of the first aspect of the present application.

[0030] A third aspect of the present application provides a battery module including the secondary battery of the second aspect of the present application.

[0031] A fourth aspect of the present application provides a battery pack including one of the secondary batteries according to the second aspect of the present application and the battery modules according to the third aspect.

[0032] A fifth aspect of the present application provides a power consuming device including at least one of the secondary battery of the second aspect of the present application, the battery module of the third aspect, and the battery pack of the fourth aspect.

[0033] A secondary battery using the negative electrode sheet of the present application has a long cycle life, can be charged at a high rate, has a high output voltage, and has a high energy density. The battery module, battery pack, and power consumption device of the present application include the secondary battery of the present application, and therefore have at least the same advantages as the secondary battery. [Brief description of the drawings]

[0034] In order to more clearly describe the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can also obtain other drawings based on the drawings without creative efforts. [Figure 1] FIG. 1 is a schematic diagram of an embodiment of a negative electrode sheet according to the present application. [Diagram 2] FIG. 1 is a schematic diagram of an embodiment of a secondary battery according to the present application. [Diagram 3] 3 is an exploded schematic view of the embodiment of the secondary battery of FIG. 2. [Figure 4] FIG. 1 is a schematic diagram of an embodiment of a battery module according to the present application. [Diagram 5] 1 is a schematic diagram of an embodiment of a battery pack according to the present application. [Figure 6] 6 is an exploded schematic view of the embodiment of the battery pack shown in FIG. 5. [Figure 7] 1 is a schematic diagram of an embodiment of a power consuming device including a secondary battery of the present application as a power source.

[0035] In the drawings, which are not necessarily drawn to scale, the reference symbols are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 case, 52 electrode assembly, 53 cover plate, 10 negative electrode sheet, 101 functional coating layer, 102 second negative electrode film layer, 103 first negative electrode film layer, 104 negative electrode current collector. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Hereinafter, the embodiments specifically disclosing the negative electrode sheet, secondary battery, battery module, battery pack, and power consumption device of the present application will be described in detail with reference to the drawings as appropriate. However, unnecessary detailed description may be omitted. For example, detailed description of already well-known matters and duplicated description of substantially the same configuration may be omitted. This is to avoid the following description becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. Note that the attached drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0037] The "ranges" disclosed herein are defined in the form of lower and upper limits, where a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits specifically define the boundaries of the range. Ranges defined in this manner may or may not include the endpoints and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, by reciting ranges of 60-120 and 80-110 for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. Also, by reciting minimum range values ​​1 and 2 and maximum range values ​​3, 4 and 5, the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 are all contemplated. In this application, unless otherwise stated, a numerical range "a-b" refers to a contraction of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 and 5" are listed in this specification, and "0 to 5" is an abbreviated expression of combinations of these numerical values. In addition, when a parameter is expressed as an integer of 2 or more, this is equivalent to disclosing that the parameter is an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0038] Unless otherwise stated, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure content of the present application.

[0039] Unless otherwise stated, all technical features and optional technical features of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure content of the present application.

[0040] Unless otherwise stated, all steps in the present application may be performed in sequence, may be performed randomly, and are preferably performed in sequence. For example, when the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed in sequence, and may also include steps (b) and (a) performed in sequence. For example, when it is mentioned that the method further includes step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), may include steps (a), (c), and (b), and may further include steps (c), (a), and (b), etc.

[0041] Unless otherwise stated, the terms "comprising" and "including" referred to in this application may be open ended or closed ended. For example, "comprising" and "including" indicate that the term may comprise or include other components not further recited, or may comprise or include only the recited components.

[0042] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or A and B are both true (or exist).

[0043] As used herein, the terms "plurality" and "multiple types" refer to two or more than two types.

[0044] In this application, the terms "primary particle" and "secondary particle" have the meanings well known in the art. A primary particle refers to a particle that is not in an aggregated state, and a secondary particle refers to a particle in an aggregated state in which two or more primary particles are aggregated. Primary particles and secondary particles can be easily distinguished from each other by taking SEM images using a scanning electron microscope.

[0045] Hard carbon means carbon that is difficult to graphitize, and is difficult to graphitize even at high temperatures of 2500°C or higher. Hard carbon is usually obtained by pyrolyzing a precursor such as a polymer. In the pyrolysis process, the structure in which carbon atoms in the precursor are crosslinked with each other inhibits the growth of the carbon layer in the planar direction, so that the hard carbon structure contains many microcrystals with a disordered graphite-like structure (abbreviated as graphite microcrystals). The structure of hard carbon is complex, and in addition to graphite microcrystals, it includes defect structures (e.g., surface defects, lattice defects, etc.) and micropore structures (e.g., open pore structures, closed pore structures, etc.). Therefore, active ions are inserted and removed from hard carbon at various angles, so that secondary batteries have excellent high-rate charging capabilities, and hard carbon has unique advantages, especially in the field of power batteries. Compared with graphite, the spacing between the crystal plane layers of hard carbon (002) is larger, so that the structure of hard carbon is more stable during charging and discharging, and no obvious volume expansion and contraction effects occur.

[0046] Hard carbon has many defect structures, which catalyze the decomposition of the electrolyte to form a thick solid electrolyte interface (SEI) film, which increases the irreversible loss of active ions. In addition, the surface of hard carbon has a sparse porous structure, which easily adsorbs moisture and oxygen gas in the air to form various CH functional groups on the surface, and these functional groups react with active ions, further increasing the irreversible loss of active ions. Therefore, compared with graphite, hard carbon has a lower initial coulombic efficiency and poor cycle performance, for example, the initial coulombic efficiency is usually less than 80%, and the advantage of its high capacity cannot be fully exerted.

[0047] The inventors of the present application have conducted extensive research to provide a novel negative electrode sheet that can improve the capacity of hard carbon and provide a secondary battery with a high energy density, while also providing improved high-rate charging capability and cycle life. Negative electrode sheet

[0048] Specifically, an embodiment of the present application provides a negative electrode sheet, which includes a negative electrode current collector, and a first negative electrode film layer, a second negative electrode film layer, and a functional coating layer sequentially provided on at least one surface of the negative electrode current collector, the functional coating layer including a ferroelectric material, the second negative electrode film layer including a second negative electrode active material including hard carbon, and the first negative electrode film layer including a first negative electrode active material including graphite.

[0049] Graphite has the advantages of high initial coulombic efficiency and high cycle stability, but has limited charging ability at high rates. Hard carbon has the advantages of high insertion and desorption rates of active ions, so it has excellent charging ability at high rates, but its initial coulombic efficiency is low and its capacity decay is fast, so that the actual capacity of the secondary battery is poor. The inventors of the present application discovered in the course of actual research that the defects of graphite and hard carbon can be compensated for by combining graphite and hard carbon in two layers by sequentially providing them on the surface of the negative electrode current collector. By providing graphite close to the negative electrode current collector, the initial coulombic efficiency of the hard carbon can be compensated for, and by providing the hard carbon away from the negative electrode current collector, more active ions can be inserted into the negative electrode more quickly, thereby improving the charging ability at high rates of the negative electrode sheet and the secondary battery.

[0050] However, in the course of further research, the inventors of the present application discovered that when graphite and hard carbon are sequentially provided on the surface of the negative electrode current collector to form a two-layer combination, the effect of improving the high-rate charging capacity and energy density of the secondary battery is not obvious. After extensive research, the inventors discovered that the possible cause is that the formation of "dendrites" during charging of the secondary battery, especially in the final stage of charging, is a factor that affects the improvement of the high-rate charging capacity and energy density of the secondary battery.

[0051] During the charging process of a secondary battery, if an abnormal situation occurs, such as a lack of space for inserting negative electrode active ions, the resistance to inserting active ions into the negative electrode is too large, and the active ions are too fast to detach from the positive electrode but cannot be inserted into the negative electrode in equal amounts, the active ions that are not inserted into the negative electrode can only obtain electrons on the surface of the negative electrode, and precipitate as a simple metal, forming "dendrites". Therefore, the problem with "dendrites" becomes more serious as the charging rate of the secondary battery increases. The formed dendrites not only reduce the performance of the secondary battery, for example by shortening the cycle life, but also, in serious cases, form sharp shapes to pierce the separator and cause a short circuit in the battery, which may cause catastrophic results such as combustion and explosion, thereby increasing the safety risk of the secondary battery. In addition, the dendrites that continue to accumulate fall off the surface of the negative electrode and lose electrical contact with the negative electrode current collector, and are no longer able to participate in the charge / discharge reaction and capacity contribution, and the energy density of the secondary battery is also reduced.

[0052] After the graphite and hard carbon are sequentially placed on the surface of the negative electrode current collector to form a two-layer combination, in the initial charging stage of the secondary battery, the active ions are first adsorbed on the surface defects and lattice defects of the hard carbon, this process corresponds to the "high potential slope region" in the charge and discharge curve of the hard carbon, at this time the negative electrode potential is usually between -2V and -0.1V, as the charging continues, the active ions are inserted between the layers of the graphite microcrystals of the hard carbon, and the graphite-like insertion behavior occurs, this process corresponds to the "low potential plateau region" in the charge and discharge curve of the hard carbon, at this time the negative electrode potential is usually between -0.1V and 0V. Since the hard carbon has a more abundant micropore structure, during the secondary charging, when the negative electrode potential drops to about 0V, the active ions are further stored in the micropore structure of the hard carbon, providing extra active ion storage sites, improving the capacity performance and initial coulombic efficiency of the hard carbon, and the longer the discharge plateau in the low potential plateau region, the higher the corresponding reversible capacity of the hard carbon and the better the capacity performance. However, the potential of the low potential plateau region of hard carbon is close to the dendrite formation potential of the graphite surface layer, both of which are about 0 V, so in order to prevent the formation of dendrites, the capacity of the low potential plateau region of hard carbon is limited, and the micropore structure of hard carbon cannot function sufficiently as an active ion storage site, and at the same time, in order to prevent the formation of dendrites, the cutoff voltage of the negative electrode is usually set high, which reduces the output voltage of the entire secondary battery and further reduces the energy density of the secondary battery. Therefore, when graphite and hard carbon are provided in this order on the surface of the negative electrode current collector to form a two-layer combination, there is a limit to the effect of improving the high-rate charging ability, energy density, and / or cycle life of the secondary battery.

[0053] In the negative electrode sheet of the present application, a first negative electrode film layer containing graphite and a second negative electrode film layer containing hard carbon are sequentially arranged on the surface of a negative electrode current collector, and a functional coating layer containing a ferroelectric material is further arranged on the surface of the second negative electrode film layer. The ferroelectric material has a spontaneous polarization phenomenon, and when electrons accumulate on the surface of the dendrite, the ferroelectric material is influenced by an electric field and causes spontaneous polarization, so that the center of the positive charge of the ferroelectric material moves to the electron accumulation region and surrounds the electron accumulation region, and at the same time, the center of the positive charge of the ferroelectric material becomes positively charged, which repels the polarity of the positively charged active ions on the surface of the dendrite, balances the electron density, and reduces the concentration of active ions, thereby suppressing the continued growth of the dendrite in the direction perpendicular to the electrode sheet.

[0054] Therefore, in the negative electrode sheet of the present application, a first negative electrode film layer containing graphite and a second negative electrode film layer containing hard carbon are sequentially provided on the surface of the negative electrode current collector to perform a combination design, thereby compensating for the defects of graphite and hard carbon and highlighting their respective advantages. A larger layer spacing of hard carbon can provide a higher charging rate. The first coulombic efficiency of hard carbon can be compensated for by interposing graphite between the hard carbon and the negative electrode current collector. In addition, since the insertion potential of active ions into the micropore structure of hard carbon is about 0V, which is close to the deposition potential of active ions on the graphite surface, the micropore structure of hard carbon cannot function sufficiently as an active ion storage site. However, the inventors of the present application unexpectedly found that the above problem can be solved by providing a functional coating layer containing a ferroelectric material on the surface of the negative electrode sheet. By controlling the deposition method of active ions, the ferroelectric material can highlight the large capacity advantage of the microporous structure of hard carbon, and can also suppress the active ions from being reduced and continuously precipitated on the graphite surface, thereby improving the cycle life of the secondary battery.

[0055] Specifically, in the early stage of charging the secondary battery, active ions are rapidly adsorbed on the surface defects and lattice defects of the hard carbon, so that the negative electrode sheet has high dynamic performance. In the later stage of charging the secondary battery, the overpotential can be precisely controlled under the action of the functional coating layer, so that a large amount of active ions can be stored in the micropore structure of the hard carbon, the length of the low potential plateau region can be increased, and the reversible capacity of the secondary battery can be increased, thereby improving the high rate charging ability and energy density of the secondary battery. In addition, in the overpotential, the functional coating layer generates a reverse electric field, which reduces the concentration of active ions and inhibits the dendrites from continuing to grow in the direction perpendicular to the electrode sheet, thereby improving the safety and cycle performance of the secondary battery.

[0056] Therefore, a secondary battery using the negative electrode sheet of the present application has a long cycle life, and can be charged at a high rate, has a high output voltage, and further has a high energy density.

[0057] In some embodiments, optionally, the dielectric constant of the ferroelectric material is greater than or equal to 50. The higher the dielectric constant of the ferroelectric material, the greater the effect of inhibiting dendrites from continuing to grow in the direction perpendicular to the pole sheet, but the effect does not always increase, and at the same time, the higher the dielectric constant, the higher the requirements for the preparation process of the ferroelectric material, which also increases the production cost.

[0058] In some embodiments, the dielectric constant of the ferroelectric material may be optionally between 50 and 100,000, e.g., between 50 and 50,000, between 50 and 25,000, between 50 and 10,000, between 50 and 5,000, between 50 and 4,000, between 50 and 3,000, between 50 and 2,000, between 100 and 100,000, between 100 and 50,000, between 100 and 25,000, It may be 100 to 10,000, 100 to 5,000, 100 to 4,000, 100 to 3,000, 100 to 2,000, 200 to 100,000, 200 to 50,000, 200 to 25,000, 200 to 10,000, 200 to 5,000, 200 to 4,000, 200 to 3,000, 200 to 2,000, or 200 to 1,000.

[0059] In this application, the dielectric constant of a ferroelectric material refers to the dielectric constant at room temperature (25±5°C), and has a meaning well known in the art, and can be tested by devices and methods well known in the art. For example, after preparing a circular sample of a ferroelectric material, an LCR meter is used to test the capacitance C, and the dielectric constant ε is calculated by the formula: ε=(C×d) / (ε 0 × A), where C is capacitance in Farads (F), d is thickness of the sample in cm, and A is area of ​​the sample in cm. 2 and ε 0 denotes the vacuum dielectric constant, and ε 0 =8.854×10 -14 F / cm. In this application, the test conditions may be 1KHz, 1.0V, 25±5℃. The test standard may be in accordance with GB / T 11297.11-2015. When preparing samples, reference may be made to Chinese patent application CN114217139A.

[0060] In some embodiments, the ferroelectric material may include one or a combination of inorganic ferroelectric materials, organic ferroelectric materials, or optionally, inorganic ferroelectric materials.

[0061] In some embodiments, optionally, the inorganic ferroelectric material may be a perovskite structure oxide, a tungsten bronze type compound, a bismuth oxide type layered structure compound, lithium niobate (LiNbO 3 ), lithium tantalate (LiTaO 3 ), lead metaniobate, and one or more combinations selected from lead barium lithium niobate. More optionally, the inorganic ferroelectric material is selected from perovskite structure oxides.

[0062] Optionally, the perovskite structure oxide may have the molecular formula Ba 1-x A x Ti 1-y B y O 3 . A may include one or more combinations selected from Pb, Sr, Ca, K, Na, and Cd, and B may include one or more combinations selected from Sn, Hf, Zr, Ce, Nb, and Th, where 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1. For example, the perovskite structure oxide may be BaTiO 3 , Ba 1-x1 Sr x1 TiO 3 (0 ≦ x1 ≦ 1), SrTiO 3 , PbTiO 3 , PbZr y1 Ti 1-y1 O 3 (0 ≦ y1 ≦ 1), BaZr y2 Ti 1-y2 O 3 (0 < y2 < 1), KNbO 3 , NaNbO 3 , and may include one or more combinations selected therefrom.

[0063] Optionally, the tungsten bronze type compound may have the molecular formula M z WO 3 . M may include one or more combinations selected from Na, K, Rb, and Cs, and 0 < z < 1. For example, the tungsten bronze type compound may be Na z1 WO 3(0 < z1 < 1), K z2 WO 3 It may include one or more combinations selected from (0 < z2 < 1).

[0064] Optionally, the bismuth oxide type layered structure compound has a molecular formula (Bi 2 O 2 )(C n-1 D n O 3n+1 ). C may include one or more combinations selected from Na, K, Ba, Sr, Pb, Ca, Ln, and Bi, D may include one or more combinations selected from Zr, Cr, Nb, Ta, Mo, W, Fe, Ti, and V, and 2 ≤ n ≤ 5. For example, the bismuth oxide type layered structure compound may be SrBi 2 Nb 2 O 9 , SrBi 2 Ta 2 O 9 , SrBi 2 Nb 2 O 9 , Bi 4 Ti 3 O 12 or a combination of one or more of them.

[0065] In some embodiments, the organic ferroelectric material may include one or more combinations selected from vinylidene fluoride homopolymer or copolymer, 2,5-dibromo-3,6-dihydroxy p-benzoquinone, phenazine-chloranilic acid, and croconic acid.

[0066] In some embodiments, the thickness of the functional coating layer is H 1 μm, the thickness of the second negative electrode film layer is H 2 μm, the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet satisfies H 1 / (H 2 + H 3 ) being 0.01 to 0.15, and optionally, 0.01 to 0.08.

[0067] In further investigation, the inventors found that the thickness H 1 μm, the thickness H of the second negative electrode film layer 2 μm and the thickness H of the first negative electrode film layer 3 μm is H 1 / (H 2 +H 3 ) is 0.01 to 0.15, the overall performance of the secondary battery is better, and high-rate charging can be realized with high energy density. In addition, the following situation can be effectively avoided. When the thickness of the functional coating layer is low and the total thickness of the first negative electrode film layer and the second negative electrode film layer is high, the reverse electric field strength by the functional coating layer is insufficient, and it is not possible to balance the electron density and inhibit the continued growth of dendrites in the direction perpendicular to the electrode sheet. As a result, when the output voltage of the secondary battery is increased to improve the energy density, the safety risk of the secondary battery increases, and when the output voltage of the secondary battery is reduced to reduce the safety risk of the secondary battery, the micropore structure of the hard carbon cannot function sufficiently as an active ion storage site. When the thickness of the functional coating layer is high and the total thickness of the first negative electrode film layer and the second negative electrode film layer is low, the functional coating layer does not have electrochemical activity and cannot contribute to the capacity, so it occupies a lot of volume space and mass parts, which affects the energy density of the secondary battery.

[0068] In some embodiments, the functional coating layer has a thickness of H 1 μm, H 1is 2-10, and optionally 4-6. When the thickness of the functional coating layer is within an appropriate range, the overall performance of the secondary battery is better, and high-rate charging with high energy density can be realized. In addition, the following situations can be effectively avoided. When the functional coating layer is thin, the reverse electric field strength is insufficient, and it is not possible to balance the electron density and inhibit the continued growth of dendrites in the direction perpendicular to the electrode sheet, which increases the safety risk of the secondary battery when increasing the output voltage of the secondary battery to improve the energy density, and the micropore structure of the hard carbon cannot function sufficiently as an active ion storage site when reducing the output voltage of the secondary battery to reduce the safety risk of the secondary battery. When the functional coating layer is thick, it does not have electrochemical activity and cannot contribute to the capacity, so it occupies a lot of volume space and mass parts, which affects the energy density of the secondary battery.

[0069] In some embodiments, the second negative electrode layer has a thickness of H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet is H 2 / H 3 is 0.10 to 5, and can be selected from 0.5 to 4.

[0070] In further investigation, the inventors found that the thickness H of the first negative electrode film layer 3 Thickness H of the second negative electrode layer in μm 2It has been found that when the μm ratio is within an appropriate range, the second negative electrode film layer and the first negative electrode film layer can exert a better synergistic effect. The second negative electrode film layer mainly bears the pressure of high-rate charging, ensuring that the secondary battery has a high charging rate, while the first negative electrode film layer mainly provides a long cycle life, while ensuring a high initial coulombic efficiency, so that the overall performance of the secondary battery is better and high-rate charging can be realized on the basis of high energy density. In addition, the following situation can be effectively avoided: When the second negative electrode film layer is thin and the first negative electrode film layer is thick, during the charging process, the pressure of high-rate charging shared by the hard carbon in the second negative electrode film layer is less, in this case, the graphite in the first negative electrode film layer still plays a leading role, and the effect of improving the charging rate of the secondary battery is not obvious. When the second negative electrode film layer is thick and the first negative electrode film layer is thin, the hard carbon surface contains a large amount of inactive functional groups, which increases the irreversible consumption of active ions, which may affect the initial coulombic efficiency of the secondary battery and also reduce the cycle life of the secondary battery.

[0071] In some embodiments, the second negative electrode film layer has a thickness of H 2 μm, H 2 is 10 to 120, optionally 35 to 110, and more preferably 40 to 100. If the thickness of the second negative electrode film layer is within an appropriate range, it is advantageous for the secondary battery to have a high charge rate.

[0072] In some embodiments, the first negative electrode film layer has a thickness of H 3 μm, H 3 is 20 to 100, optionally 25 to 70, and more preferably 28 to 60. When the thickness of the first negative electrode film layer is within an appropriate range, it is advantageous for the secondary battery to have a high initial coulombic efficiency and a long cycle life.

[0073] The functional coating layer comprises a ferroelectric material. In some embodiments, the mass percentage of the ferroelectric material in the functional coating layer is W1, based on the total mass of the functional coating layer, W1 being 70%-95%, optionally 80%-95%.

[0074] In further study, the inventors found that when the content of the ferroelectric material is within an appropriate range, the overall performance of the secondary battery is better, and a high rate of charging can be realized with a high energy density. In addition, the following situations can be effectively avoided. When the content of the ferroelectric material is low, the reverse electric field strength is insufficient, and it may not be possible to balance the electron density and inhibit the continued growth of dendrites in the direction perpendicular to the electrode sheet, which increases the safety risk of the secondary battery when increasing the output voltage of the secondary battery to improve the energy density, and the micropore structure of the hard carbon cannot fully function as an active ion storage site when reducing the output voltage of the secondary battery to reduce the safety risk of the secondary battery. When the content of the ferroelectric material is high, the content of other components (e.g., adhesive) in the functional coating layer is low, which causes the functional coating layer to have poor adhesion with the second negative electrode film layer and is easily detached from the second negative electrode film layer.

[0075] In some embodiments, the functional coating layer may further include an adhesive to bond the ferroelectric materials together and to bond the functional coating layer to the second negative electrode film layer. Optionally, the adhesive may include one or more combinations selected from styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0076] In some embodiments, the functional coating layer may further include other auxiliary agents, for example, a dispersing agent, such as sodium carboxymethylcellulose (CMC).

[0077] The second negative electrode film layer includes a second negative electrode active material, and the second negative electrode active material includes hard carbon. Optionally, the mass percentage of the hard carbon in the second negative electrode active material is 70% to 100%, and optionally 80% to 98%, based on the total mass of the second negative electrode active material. This is advantageous in that the second negative electrode film layer contains a lot of hard carbon, and the secondary battery has a higher charge rate. In some embodiments, the second negative electrode active material may include only hard carbon, and in some other embodiments, the second negative electrode active material may further include other negative electrode active materials other than hard carbon, such as graphite, soft carbon, mesocarbon microbeads, silicon-based materials, tin-based materials, etc., and optionally, the mass percentage of the other negative electrode active materials in the second negative electrode active material is 30% or less, and more preferably 20% or less, based on the total mass of the second negative electrode active material.

[0078] In some embodiments, the mass percentage of hard carbon in the second negative electrode film layer is W2, and based on the total mass of the second negative electrode film layer, W2 is 68% or more, optionally 90% to 98%. When the content of hard carbon is within a suitable range, it is advantageous for the secondary battery to have a higher charge rate.

[0079] In some embodiments, the second negative electrode film layer may further include a conductive agent, which plays a role in collecting microcurrent between the second negative electrode active material (e.g., hard carbon), reducing the contact resistance of the electrode, accelerating the electron transfer rate, and at the same time reducing polarization, thereby improving the charge and discharge efficiency of the secondary battery. For example, the conductive agent may include one or more combinations selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, based on the total mass of the second negative electrode film layer, the mass percentage of the conductive agent is 5% or less.

[0080] In some embodiments, the second negative electrode membrane layer may further include an adhesive to bond the second negative electrode active materials together, to bond the second negative electrode membrane layer to the functional coating layer, and to bond the second negative electrode membrane layer to the first negative electrode membrane layer. For example, the adhesive may include one or more combinations selected from styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the adhesive is 5% or less based on the total mass of the second negative electrode membrane layer.

[0081] In some embodiments, the second negative electrode membrane layer may further include other additives. For example, the other additives may include a thickener, such as sodium carboxymethylcellulose (CMC), a PTC thermistor material, etc. In some embodiments, based on the total mass of the second negative electrode membrane layer, the mass percentage of the other additives is 2% or less.

[0082] The first negative electrode film layer includes a first negative electrode active material including graphite. Optionally, the mass percentage of the graphite in the first negative electrode active material is 80% to 100%, and optionally 90% to 98%, based on the total mass of the first negative electrode active material. This is advantageous in that the first negative electrode film layer contains a lot of graphite, and the secondary battery has a higher initial coulombic efficiency and a longer cycle life. In some embodiments, the first negative electrode active material may include only graphite, and in some other embodiments, the first negative electrode active material may further include other negative electrode active materials other than graphite, such as hard carbon, soft carbon, mesocarbon microbeads, silicon-based materials, tin-based materials, etc., and optionally, the mass percentage of the other negative electrode active materials in the first negative electrode active material is 20% or less, and more preferably 10% or less, based on the total mass of the first negative electrode active material.

[0083] In some embodiments, the mass percentage of graphite in the first negative electrode film layer is W3, and W3 is 78% or more, optionally 90% to 98%, based on the total mass of the first negative electrode film layer. When the graphite content is within a suitable range, it is advantageous for the secondary battery to have a higher initial coulombic efficiency and a longer cycle life.

[0084] In some embodiments, the first negative electrode film layer may further include a conductive agent, which plays a role in collecting microcurrent between the first negative electrode active material (e.g., graphite), reducing the contact resistance of the electrode, accelerating the electron transfer speed, and at the same time reducing polarization, thereby improving the charge and discharge efficiency of the secondary battery. For example, the conductive agent may include one or a combination of a plurality of materials selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the conductive agent is 5% or less, based on the total mass of the first negative electrode film layer.

[0085] In some embodiments, the first negative electrode film layer may further include an adhesive to bond the first negative electrode active materials together, to bond the first negative electrode film layer and the second negative electrode film layer, and to bond the first negative electrode film layer and the negative electrode current collector. For example, the adhesive may include one or more combinations selected from styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the adhesive is 5% or less based on the total mass of the first negative electrode film layer.

[0086] In some embodiments, the first negative electrode membrane layer may further include other auxiliary agents. For example, the other auxiliary agents may include a thickener, such as sodium carboxymethylcellulose (CMC), a PTC thermistor material, etc. In some embodiments, based on the total mass of the first negative electrode membrane layer, the mass percentage of the other auxiliary agents is 2% or less.

[0087] In some embodiments, the volume average particle size Dv50 of the ferroelectric material is d 1 μm, and d 1 is 1 or less, and may be, for example, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, or 0.2 or less. 1 is 0.01 to 1, 0.02 to 1, 0.03 to 1, 0.04 to 1, 0.05 to 1, 0.06 to 1, 0.07 to 1, 0.08 to 1, 0.01 to 0.8, 0.02 to 0.8, 0.03 to 0.8, 0.04 to 0.8, 0.05 to 0.8, 0.06 to 0.8, 0.07 to 0.8, 0.08 to 0.8, 0.09 to 0.8, or 0.1 to 0.8.

[0088] When the Dv50 of the ferroelectric material is within an appropriate range, the overall performance of the secondary battery is better, high-rate charging can be realized with high energy density, and production costs can be reduced. In addition, the following situations can be effectively avoided. If the Dv50 of the ferroelectric material is large, the interference of the reverse electric field is large, which may not balance the electron density and inhibit the continued growth of dendrites in the direction perpendicular to the polar sheet, which increases the safety risk of the secondary battery when increasing the output voltage of the secondary battery to improve the energy density, and the micropore structure of the hard carbon cannot function fully as an active ion storage site when reducing the output voltage of the secondary battery to reduce the safety risk of the secondary battery. If the Dv50 of the ferroelectric material is small, the preparation process is complicated and the production cost increases.

[0089] In some embodiments, the second negative electrode active material has a volume average particle diameter Dv50 of d 2 μm, and the volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 2 / d 3 is 0.1 to 1, selectable from 0.2 to 0.8.

[0090] In the negative electrode sheet of the present application, the first negative electrode film layer adopts a first negative electrode active material with a large particle size, so that the compaction density of the first negative electrode film layer is higher, which is advantageous for the secondary battery to have a high initial coulombic efficiency, high energy density and long cycle life. In the negative electrode sheet of the present application, the second negative electrode film layer adopts a second negative electrode active material with a small particle size, so that its specific surface area is high, the contact area with the electrolyte is increased, and the liquid phase diffusion path and solid phase diffusion path of the active ion can be shortened. At the same time, the integrity of the channel structure of the second negative electrode film layer can be better maintained, which is advantageous for the secondary battery to have a higher charge rate. In addition, the particle size of the second negative electrode active material is small and its withstand voltage is higher, so that the micropore structure of the second negative electrode active material, especially the hard carbon, is better maintained, so that the micropore structure of the hard carbon can function fully as an active ion storage site, and the capacity and energy density of the secondary battery can be improved. At the same time, the compaction density of the second negative electrode film layer is low, and the electrolyte can quickly infiltrate into the first negative electrode film layer, which is advantageous for reducing the polarization of the negative electrode and improving the charge / discharge efficiency of the secondary battery.

[0091] In further studies, the inventors have found that the ratio d of the particle size of the second negative electrode active material to the particle size of the first negative electrode active material 2 / d 3 It has been discovered that when is within an appropriate range, it is advantageous for the second negative electrode film layer to fully exhibit the effect of improving the high-rate charging capability of the secondary battery and the effect of the first negative electrode film layer to fully exhibit the effect of improving the initial coulombic efficiency and cycle life of the secondary battery, thereby improving the overall performance of the secondary battery and realizing high-rate charging with high energy density.

[0092] In some embodiments, the second negative electrode active material has a volume average particle diameter Dv50 of d 2 μm, and d 2is 3 to 11, and optionally 3 to 9. When the particle size of the second negative electrode active material is within an appropriate range, the micropore structure is better maintained, so that the micropore structure of the hard carbon can function fully as an active ion storage site, and the capacity and energy density of the secondary battery can be improved. At the same time, when the particle size of the second negative electrode active material is within an appropriate range, the second negative electrode film layer has a smooth channel structure, which is advantageous for the electrolyte to smoothly pass through the channel structure of the second negative electrode film layer and quickly infiltrate into the first negative electrode film layer, thereby reducing the polarization of the negative electrode and improving the charge / discharge efficiency of the secondary battery.

[0093] In some embodiments, the particle size distribution index (Dv90-Dv10) / Dv50 of the second negative electrode active material is 1 and α 1 is 0.6 to 5, and optionally 1 to 4. When the particle size distribution index of the second negative electrode active material is within a suitable range, it is favorable for improving the processing performance of the second negative electrode film layer, and for the whole second negative electrode film layer to have high particle distribution uniformity and smooth channel structure, so that different regions of the second negative electrode film layer all have high active ion transport performance, which is favorable for further improving the high rate charging ability of the secondary battery, and at the same time, it is favorable for the electrolyte to quickly infiltrate into the first negative electrode film layer, which reduces the polarization of the negative electrode, and improves the charging and discharging efficiency of the secondary battery.

[0094] In some embodiments, the second negative electrode active material has a specific surface area of ​​3 m 2 / g~7m 2 / g, selectable 4m 2 / g~6m 2 / g. When the specific surface area of ​​the second negative electrode active material is within an appropriate range, the impedance of charge exchange can be reduced, and the second negative electrode film layer has a smoother channel structure, which results in higher active ion transport performance, thereby further improving the high-rate charging ability of the secondary battery. When the specific surface area of ​​the second negative electrode active material is within an appropriate range, the film formation efficiency of the SEI film is improved, the formation of an SEI film that is too thick is avoided, and irreversible consumption of active ions is reduced, thereby further improving the capacity exertion and cycle performance of the secondary battery.

[0095] In some embodiments, the powder compaction density of the second negative electrode active material at 20,000 N is 0.9 g / cm 3 ~1.3g / cm 3 and can be selected from 1g / cm 3 ~1.2g / cm 3 If the compaction degree of the powder of the second negative electrode active material is within an appropriate range, it is advantageous for improving the energy density of the secondary battery.

[0096] In some embodiments, the second negative electrode active material comprises primary particles, secondary particles, or a combination thereof, and optionally the proportion of primary particles in the second negative electrode active material is 90%-100%. When the second negative electrode active material comprises a suitable proportion of primary particles, it is advantageous for the second negative electrode membrane layer to have a short active ion transport path, which can further improve the high-rate charging capability of the secondary battery, and can also reduce the polarization of the negative electrode and the side reaction of the electrolyte, thereby further improving the cycle performance and storage performance of the secondary battery.

[0097] In some embodiments, the first negative electrode active material has a volume average particle diameter Dv50 of d 3 μm, and d 3 is 9 to 18, and optionally 11 to 15. When the particle size of the first negative electrode active material is within an appropriate range, it is advantageous for the first negative electrode film layer to have a high compaction ratio, so that the secondary battery has a high initial coulombic efficiency, a high energy density, and a long cycle life.

[0098] In some embodiments, the particle size distribution index (Dv90-Dv10) / Dv50 of the first negative electrode active material is 2 and α 2 is 0.2 to 5, and optionally 0.3 to 4. When the particle size distribution index of the first negative electrode active material is within a suitable range, it is favorable for improving the processing performance of the first negative electrode film layer, and for the entire first negative electrode film layer to have high particle distribution uniformity and smooth channel structure, so that different regions of the first negative electrode film layer all have high active ion transport performance, which is favorable for further improving the cycle performance of the secondary battery.

[0099] In some embodiments, the first negative electrode active material has a specific surface area of ​​0.6 m 2 / g~1.5m 2 / g, selectable 0.8m 2 / g~1.4m 2 When the specific surface area of ​​the first negative electrode active material is within an appropriate range, the impedance of charge exchange can be reduced, and the first negative electrode film layer has a smoother channel structure, which results in higher active ion transport performance, thereby further improving the cycle performance of the secondary battery.

[0100] In some embodiments, the powder compaction density of the first negative electrode active material at 20000 N is 1.4 g / cm 3 ~1.85g / cm 3 and selectable, 1.6g / cm 3 ~1.75g / cm 3 If the compaction degree of the powder of the first negative electrode active material is within an appropriate range, it is advantageous for improving the energy density of the secondary battery.

[0101] In some embodiments, the graphitization degree of the first negative electrode active material is 91% to 95%, and optionally 92% to 94%. If the graphitization degree of the first negative electrode active material is within an appropriate range, it is advantageous to improve the cycle performance of the secondary battery.

[0102] In some embodiments, the first negative electrode active material includes artificial graphite, natural graphite, or a combination thereof. Optionally, the mass percentage of the artificial graphite in the first negative electrode active material is 50% or more, and optionally 60% to 100%, based on the total mass of the first negative electrode active material. Optionally, the artificial graphite further has a carbon coating layer on a surface thereof, which can further reduce the impedance of charge transfer and improve the cycle performance and high rate charging capability of the secondary battery. Optionally, the carbon coating layer includes amorphous carbon.

[0103] In some embodiments, the first negative electrode active material comprises primary particles, secondary particles or a combination thereof, and optionally the quantity ratio of the secondary particles in the first negative electrode active material is 80%-100%. When the first negative electrode active material comprises a suitable proportion of secondary particles, its isotropy is improved, which is favorable for the first negative electrode film layer to have more active ion transport paths, thereby further improving the high-rate charging capability of the secondary battery; at the same time, the first negative electrode film layer has a high compaction ratio, which is favorable for improving the energy density of the secondary battery, and further improving the cycle performance and storage performance of the secondary battery by reducing the polarization of the negative electrode and the side reaction of the electrolyte.

[0104] In some embodiments, the negative electrode sheet has a compaction density of 1.4 g / cm 3 ~1.85g / cm 3 and selectable 1.6g / cm 3 ~1.75g / cm 3 If the compaction degree of the negative electrode sheet is within an appropriate range, it is advantageous for improving the high-rate charging capability, cycle performance, and energy density of the secondary battery.

[0105] In some embodiments, the negative electrode current collector may be a metal foil piece or a composite current collector. Examples of the metal foil piece include copper foil and copper alloy foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more combinations selected from copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, and the polymeric material base layer may include one or more combinations selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0106] The negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the first negative electrode film layer, the second negative electrode film layer and the functional coating layer may be provided on either or both of the two opposing surfaces of the negative electrode current collector.

[0107] In addition, the parameters of the first negative electrode film layer, the second negative electrode film layer and the functional coating layer provided in this application all refer to the parameter range of the coating layer on one side of the negative electrode current collector. When the first negative electrode film layer, the second negative electrode film layer and the functional coating layer are provided on two surfaces of the negative electrode current collector, if the parameters of the coating layer on either surface meet the provisions of this application, it is considered to be within the protection scope of this application.

[0108] The negative electrode sheet of the present application will be described below with reference to the drawings. FIG. 1 is a schematic diagram of an embodiment of a negative electrode sheet 10 of the present application. The negative electrode sheet 10 includes a negative electrode current collector 104, a first negative electrode film layer 103 provided on each of the two surfaces of the negative electrode current collector 104, a second negative electrode film layer 102 provided on the first negative electrode film layer 103, and a functional coating layer 101 provided on the second negative electrode film layer 102. Of course, the first negative electrode film layer 103, the second negative electrode film layer 102, and the functional coating layer 101 may be provided on only one surface of the negative electrode current collector 104.

[0109] In this application, the Dv90, Dv50, and Dv10 of the material have the meanings known in the art and can be measured by instruments and methods known in the art. For example, refer to the particle size distribution laser diffraction method of GB / T 19077-2016, and can be easily tested using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer of Malvern, UK. Dv90 is the particle size corresponding to the material cumulative volume distribution percentage reaching 90%, Dv50 is the particle size corresponding to the material cumulative volume distribution percentage reaching 50%, and Dv10 is the particle size corresponding to the material cumulative volume distribution percentage reaching 10%.

[0110] In this application, the specific surface area of ​​a material has a meaning well known in the art and can be measured by instruments and methods well known in the art. For example, the specific surface area can be tested by the nitrogen gas adsorption specific surface area analysis test method in accordance with GB / T 19587-2017 and calculated by the BET (Brunauer Emmett Teller) method. The nitrogen gas adsorption specific surface area analysis test can be performed by a specific surface area pore size analysis tester of the Tri-Star 3020 type manufactured by Micromeritics, USA.

[0111] In the present application, the graphitization degree of a material has a meaning known in the art and can be measured by an apparatus and method known in the art. For example, the graphitization degree of a material can be measured by an X-ray diffractometer (e.g., Bruker D8 Discover) with reference to JIS K 0131-1996 and JB / T 4220-2011. 002 After obtaining the formula g=(0.344-d 002 The graphitization degree of the material was calculated from d / (0.344-0.3354)×100%. 002 is the layer spacing of the (002) crystal plane in the crystal structure of the material, expressed in nanometers (nm).

[0112] In this application, the powder compaction of a material has a meaning known in the art and can be measured by instruments and methods known in the art. For example, it can be tested by an electronic pressure test machine (e.g., UTM7305 type) with reference to GB / T24533-2009. One exemplary test method is to weigh 1 g of material and measure the powder compaction with a base area of ​​1.327 cm. 2 The method includes the steps of placing the powder in a mold, pressurizing it to 2000 kg (equivalent to 20,000 N), holding the pressure for 30 seconds, releasing the pressure, holding for 10 s, and then recording and calculating the powder compaction density at the applied force of 20,000 N of the material.

[0113] In this application, the quantity ratio of primary particles and secondary particles can be measured by instruments and methods known in the art, such as scanning electron microscope. In order to ensure the accuracy of the test results, a number of different areas (e.g., 5 or more) can be randomly selected from the test sample to perform a scan test, and the percentage of the number of primary particles and secondary particles in each area to the number of total particles at a certain magnification (e.g., 1000 times or more) can be calculated, that is, the quantity ratio of primary particles and secondary particles in each area. In order to ensure the accuracy of the test results, the above test can be repeated using multiple test samples (e.g., 10 or more), and the average value of each test sample can be taken as the final test result. The test standard can refer to JY / T010-1996.

[0114] In this application, the thicknesses of the first negative electrode film layer, the second negative electrode film layer, and the functional coating layer have meanings known in the art and can be measured by instruments and methods known in the art, such as a scanning electron microscope (e.g., ZEISS Sigma300), which allows the boundary area between the functional coating layer and the second negative electrode film layer and the boundary area between the second negative electrode film layer and the first negative electrode film layer to be more accurately determined. One exemplary test method is to cut the negative electrode sheet into a test sample of a certain size (e.g., 2 cm x 2 cm), fix the negative electrode sheet to a sample stand with paraffin, place the sample stand in a sample holder, lock and fix it, turn on the power of an argon ion cross-section polishing device (e.g., IB-19500CP) to draw a vacuum (e.g., 10ー4 The method includes the steps of setting the argon gas flow rate (e.g., 0.15MPa) and voltage (e.g., 8KV) and polishing time (e.g., 2 hours), adjusting the sample stand to swing mode, and starting polishing. The test standard can refer to JY / T010-1996. In order to ensure the accuracy of the test results, a plurality of different areas (e.g., 5 or more) can be randomly selected from the test sample to perform a scan test, and the thicknesses of the first negative electrode film layer, the second negative electrode film layer, and the functional coating layer in the scale test area can be read at a certain magnification (e.g., 500 times or more). For the accuracy of the test, a plurality of test areas can be used for testing, and the average value can be used.

[0115] In this application, the compaction degree of the negative electrode sheet has a meaning known in the art and can be measured by devices and methods known in the art. Compaction degree of the negative electrode sheet = areal density of the negative electrode sheet / thickness of the coating layer on one side of the negative electrode current collector. The areal density of the negative electrode sheet has a meaning known in the art and can be measured by devices and methods known in the art. One exemplary test method is to apply a coating to a negative electrode sheet that is coated on one side and cold pressed (if the negative electrode sheet is coated on two sides, the coating layer on one side can be wiped off first) to an area of ​​S 1 The wafer is punched out into small wafers, weighed, and 1 The weight of the negative electrode current collector was measured and recorded as M. 0 The areal density of the negative electrode sheet is recorded as = (M 1 -M 0 ) / S 1 It is.

[0116] The first negative electrode active material, the second negative electrode active material, and the ferroelectric material may be sampled and tested for various parameters before application, or may be sampled and tested from the negative electrode sheet after cold pressing. When the test specimen is sampled from the cold-pressed negative electrode sheet, for example, the steps are as follows: (1) arbitrarily select a coating layer on one side of the negative electrode current collector that is cold-pressed, and sample the ferroelectric material (for example, a blade can be used to scrape off the powder for sampling), with the scraping depth not exceeding the boundary region between the functional coating layer and the second negative electrode film layer; and (2) sample the second negative electrode active material (for example, a blade can be used to scrape off the powder for sampling), with the scraping depth not exceeding the boundary region between the second negative electrode film layer and the first negative electrode film layer. During the cold pressing process, there may be an intermelted layer at the boundary region between the functional coating layer and the second negative electrode film layer. For the sake of test accuracy, when sampling the second negative electrode active material, the intermelted layer should first be scraped off, and then the second negative electrode active material should be sampled. (3) sampling the first negative electrode active material (for example, using a blade to scrape off the powder for sampling), and since there may be a mutual fusion layer at the boundary region between the second negative electrode film layer and the first negative electrode film layer during the cold pressing process, for the sake of test accuracy, when sampling the first negative electrode active material, first, scraping off the mutual fusion layer, and then scraping off the powder for the first negative electrode active material for sampling; (4) putting the collected ferroelectric material, the first negative electrode active material, and the second negative electrode active material into deionized water, respectively, followed by suction filtration and drying, and sintering the dried powder at a certain temperature and time (for example, 400°C, 2h) to remove adhesives, conductive agents, etc., to obtain a test sample by sampling. [Preparation method]

[0117] The method for preparing the negative electrode sheet of the present application is known. In some embodiments, the negative electrode sheet can be prepared by a method of dispersing a first negative electrode active material, a conductive agent, an adhesive, any other components, etc. in a solvent (e.g., deionized water) to form a first slurry, dispersing a second negative electrode active material, a conductive agent, an adhesive, any other components, etc. in a solvent (e.g., deionized water) to form a second slurry, dispersing a ferroelectric material, an adhesive, any other components, etc. in a solvent (e.g., deionized water) to form a third slurry, applying the first slurry to a negative electrode current collector and drying to form a first negative electrode film layer, applying the second slurry to the first negative electrode film layer and drying to form a second negative electrode film layer, applying the third slurry to the second negative electrode film layer, and obtaining a negative electrode sheet after steps such as drying and cold pressing. secondary battery

[0118] An embodiment of the present application further provides a secondary battery comprising the negative electrode sheet of the first aspect of the present application.

[0119] A secondary battery, also called a rechargeable battery or storage battery, is a battery that can continue to be used by activating the active material by charging after the battery is discharged. The secondary battery includes an electrode assembly and an electrolyte, and the electrode assembly usually includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is provided between the positive electrode sheet and the negative electrode sheet, and mainly serves to prevent short circuits between the positive electrode and the negative electrode, and at the same time, allows active ions to pass through. The electrolyte serves to conduct active ions between the positive electrode sheet and the negative electrode sheet. The secondary battery of the present application may be a lithium-containing secondary battery, and in particular may be a lithium-ion secondary battery. [Negative electrode sheet]

[0120] The negative electrode sheet used in the secondary battery of the present application is the negative electrode sheet according to any one of the embodiments of the first aspect of the present application. [Positive electrode sheet]

[0121] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, for example, the positive electrode current collector has two surfaces opposed to each other in a thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on one or both of the two opposed surfaces of the positive electrode current collector.

[0122] The positive electrode film layer includes a positive electrode active material, and the positive electrode active material can be a positive electrode active material for secondary batteries known in the art. For example, the positive electrode active material may include one or a combination of a plurality of types selected from lithium transition metal oxides, lithium-containing phosphates, and their modified compounds. Examples of lithium transition metal oxides include lithium cobalt oxides (e.g., LiCoO 2 ), lithium nickel oxide (e.g., LiNiO 2 ), lithium manganese oxide (e.g., LiMnPO 2 , LiMn 2 O 4 ), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 , LiNi 0.5 Co 0.25 Mn 0.25 O 2 , LiNi 0.6 Co 0.2 Mn 0.2 O 2 , LiNi 0.8 Co 0.1 Mn 0.1 O 2 ), lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05 O 2It may include one or more combinations selected from them and their respective modified compounds. Examples of the lithium-containing phosphate include lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and one or more combinations selected from their modified compounds.

[0123] In some embodiments, in order to further increase the energy density of the secondary battery, the positive electrode active material may include one or more combinations selected from the lithium transition metal oxides represented by Formula 1 and their modified compounds.

[0124] Li a Ni b Co c M d O e A f Formula 1

[0125] In Formula 1, 0.8 ≦ a ≦ 1.2, 0.5 ≦ b < 1, 0 < c < 1, 0 < d < 1, 1 ≦ e ≦ 2, 0 ≦ f ≦ 1, M may include one or more combinations selected from Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A may include one or more combinations selected from N, F, S, and Cl.

[0126] In the present application, the modified compound of each of the above positive electrode active materials may be obtained by performing doping modification and / or surface coating modification on the positive electrode active material.

[0127] In some embodiments, the positive electrode film layer may further include a conductive agent, which plays a role in collecting microcurrent between the positive electrode active material, reducing the contact resistance of the electrode, accelerating the electron transfer rate, reducing polarization, and improving the charge and discharge efficiency of the secondary battery. For example, the conductive agent may include one or more combinations selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the conductive agent is 5% or less based on the total mass of the positive electrode film layer.

[0128] In some embodiments, the positive electrode membrane layer may further include an adhesive to bond the positive electrode active materials together and to bond the positive electrode membrane layer and the positive electrode current collector. For example, the adhesive may include one or more combinations selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene ternary copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. In some embodiments, the mass percentage of the adhesive is 5% or less based on the total mass of the positive electrode membrane layer.

[0129] In some embodiments, the positive electrode current collector may be a metal foil piece or a composite current collector. Examples of the metal foil piece include aluminum foil or aluminum alloy foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more combinations selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, and the polymeric material base layer may include one or more combinations selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0130] The positive electrode membrane layer is usually formed by applying a positive electrode slurry to a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is usually formed by dispersing a positive electrode active material, a conductive agent, an adhesive, and any other components in a solvent and stirring the mixture uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP). [Electrolytes]

[0131] In the present application, the type of the electrolyte is not particularly limited and can be selected according to needs. For example, the electrolyte may be at least one selected from a solid electrolyte, a gel electrolyte, and a liquid electrolyte (i.e., an electrolytic solution).

[0132] In some embodiments, the electrolyte employs an electrolyte solution, the electrolyte solution including a lithium salt and a solvent.

[0133] As an example, the lithium salt may be lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ), lithium hexafluoroarsenate (LiAsF 6), lithium bisfluorosulfonylimide (LiFSI), lithium bistrifluoromethanesulfonylimide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB) and lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO 2 F 2 ), lithium difluorobisoxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP), or a combination of two or more of these.

[0134] By way of example, the organic solvent may comprise at least one or a combination of more than one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).

[0135] In some embodiments, the electrolyte may include an additive, such as an anode film-forming additive, a cathode film-forming additive, and may further include an additive that can improve certain performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature performance or low temperature performance of the battery, etc. [Separator]

[0136] In the present application, the type of the separator is not particularly limited, and any known porous structure separator having good chemical stability and mechanical stability can be selected.

[0137] In some embodiments, the separator may be made of at least one material selected from glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride, or a combination of multiple materials. The separator may be a single layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer may be the same or different.

[0138] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be prepared into an electrode assembly by a winding process or a stacking process.

[0139] In some embodiments, the secondary battery may include an exterior case that can be used to seal the electrode assembly and electrolyte.

[0140] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft package, such as a bag-type soft package. The material of the soft package may be one or a combination of plastics, such as polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0141] In the present application, the shape of the secondary battery is not particularly limited, and may be cylindrical, rectangular, or any other shape. For example, FIG. 2 shows a secondary battery 5 having a rectangular structure as an example.

[0142] In some embodiments, as shown in FIG. 3, the exterior may include a case 51 and a cover plate 53. The case 51 includes a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are surrounded to form a receiving chamber. The case 51 has an opening communicating with the receiving chamber, and the cover plate 53 covers the opening to close the receiving chamber. The positive electrode sheet, the negative electrode sheet and the separator can form an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is sealed in the receiving chamber. The electrode assembly 52 is infiltrated with an electrolyte. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted according to needs.

[0143] The method of preparing the secondary battery of the present application is known. In some embodiments, a secondary battery can be formed by assembling a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte. For example, a positive electrode sheet, a separator, and a negative electrode sheet can be formed into an electrode assembly by a winding process or a lamination process, and the electrode assembly can be placed in an outer casing, dried, and then an electrolyte can be injected, and a secondary battery can be obtained through processes such as vacuum sealing, standing, chemical formation, and shaping.

[0144] In some embodiments of the present application, the secondary battery of the present application may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, and the specific number may be adjusted according to the application and capacity of the battery module.

[0145] Fig. 4 is a schematic diagram of an example battery module 4. As shown in Fig. 4, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by a fastener.

[0146] Optionally, the battery module 4 further includes a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.

[0147] In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0148] 5 and 6 are schematic diagrams of an example battery pack 1. As shown in Fig. 5 and 6, the battery pack 1 may include a battery box and a plurality of battery modules 4 provided in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 is covered by the lower housing 3 to form an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner. power consumption equipment

[0149] The embodiment of the present application further provides a power consuming device including at least one of the secondary battery, battery module, and battery pack of the present application. The secondary battery, battery module, and battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may be, but is not limited to, a mobile device (e.g., mobile phone, laptop, etc.), an electric vehicle (e.g., pure electric vehicle, hybrid electric vehicle, plug-in hybrid electric vehicle, electric bicycle, electric scooter, electric golf cart, electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0150] The power consumption device can select a secondary battery, a battery module or a battery pack according to its usage demand.

[0151] 7 is a schematic diagram of an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, in which a battery pack or battery module can be employed to meet the high power and high energy density demands of the power consuming device.

[0152] Other examples of power consuming devices may be mobile phones, tablet computers, notebook computers, etc. Such power consuming devices are usually required to be thin and may employ secondary batteries as their power source. Working Example

[0153] The following examples are provided to more specifically describe the contents of the present application, and these examples are merely used for explanatory purposes, and it is obvious to those skilled in the art that various modifications and changes can be made within the scope of the contents of the present application.Unless otherwise specified, all parts, percentages, and ratios described in the following examples are calculated based on mass, and all reagents used in the examples can be purchased or synthesized according to conventional methods, and can be used directly without further processing.In addition, all devices used in the examples can be purchased. Example 1-1 Step (1): Preparation of negative electrode sheet S10: Preparation of artificial graphite

[0154] Raw coke powder, which is petroleum non-needle coke, is pretreated to remove impurities, then mixed with coal pitch and granulated to obtain secondary particles with a Dv50 of 10 μm. The granulated material is then placed in an Acheson graphitization furnace and graphitized at 3000°C for 24 hours to obtain graphite particles. The resulting graphite particles are mixed with petroleum pitch and carbonized at 1000°C for 15 hours to obtain artificial graphite. The artificial graphite has a Dv50 of 12 μm, a Dv90 of 20 μm, a Dv10 of 6.5 μm, a graphitization degree of 92%, and a specific surface area of ​​0.86 m. 2 / g, and the powder compaction density is 1.6g / cm 3 The morphology was that of secondary particles. S20: Preparation of hard carbon

[0155] The phenolic resin was heated at 500°C for 30 min to obtain a precursor, which was then crushed and heat-treated at 1200°C for 20 h under a nitrogen gas atmosphere and crushed again to obtain hard carbon. The hard carbon had a Dv50 of 5 μm, a Dv90 of 10 μm, a Dv10 of 2.5 μm, and a specific surface area of ​​5 m. 2 / g and had a primary particle morphology. S30: Preparation of first slurry

[0156] The artificial graphite prepared above, conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener were mixed in a mass ratio of 96.8:0.8:1.2:1.2, and then added to deionized water. The mixture was stirred with a vacuum mixer until the system became uniform, obtaining a first slurry with a solid content of 66%. S40: Preparation of second slurry

[0157] The hard carbon prepared above, conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener were mixed in a mass ratio of 95:1.5:3.1:0.4, and then added to deionized water. The mixture was stirred under the action of a vacuum stirrer until the system became uniform, obtaining a second slurry with a solid content of 66%. S50: Preparation of third slurry

[0158] Barium titanate (dielectric constant of 3000 or more) with Dv50 of 100 nm, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a dispersant were mixed in a mass ratio of 85:10:5, and then added to deionized water and stirred with a vacuum mixer until the system became uniform, obtaining a third slurry with a solid content of 40%. S60: Slurry application

[0159] The first slurry is applied to one surface of the copper foil, which is the negative electrode current collector, with a thickness of 8 μm, and dried to form a first negative electrode film layer. The second slurry is applied to the first negative electrode film layer and dried to form a second negative electrode film layer. The third slurry is applied to the second negative electrode film layer and dried to form a functional coating layer. The above steps are then repeated on the other surface of the copper foil, which is the negative electrode current collector, and after further processes such as cold pressing, a negative electrode sheet is obtained. The thickness of the first negative electrode film layer on one side of the negative electrode current collector was 59 μm, the thickness of the second negative electrode film layer was 82 μm, and the thickness of the functional coating layer was 2 μm. The compaction density of the negative electrode sheet was 1.55 g / cm 3 It was. Step (2): Preparation of the positive electrode sheet

[0160] Positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811), conductive carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive were mixed in a mass ratio of 98:1:1, and then added to the solvent NMP. The system was stirred until it became uniform using a vacuum stirrer to obtain a positive electrode slurry with a solid content of 75%. The positive electrode slurry was evenly applied to two surfaces of an aluminum foil with a thickness of 13 μm, dried at 90°C, and then cold pressed to obtain a positive electrode sheet with a positive electrode film layer on one side of the positive electrode current collector having a thickness of 114 μm. Step (3): Preparation of electrolyte

[0161] In an environment with a water content of less than 10 ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent, which was then thoroughly dried. 6 was dissolved in the above organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L. Step (4): Preparation of the separator

[0162] As the separator, a porous polyethylene film was used. Step (5): Preparation of secondary battery

[0163] The positive electrode sheet, separator, and negative electrode sheet were stacked in that order and rolled up to obtain an electrode assembly. The electrode assembly was placed in an exterior case and dried, after which an electrolyte was injected, and the assembly was vacuum sealed, left to stand, chemically formed, shaped, and other processes were carried out to obtain a secondary battery. Examples 1-2 to 1-7

[0164] A secondary battery was prepared in a similar manner to Example 1-1, except that the coating thickness of the third slurry in the preparation of the negative electrode sheet and the thickness of the functional coating layer obtained thereby were different. See Table 1 for specific parameters. Comparative Example 1-1

[0165] A secondary battery was prepared in a similar manner to Example 1-1, except that the third slurry was not applied in preparing the negative electrode sheet. Comparative Example 1-2

[0166] The secondary battery was prepared in a similar manner to Example 1-1, with the difference being that the third slurry was not applied in the preparation of the negative electrode sheet, and when applying the slurry, the second slurry was first applied to one surface of the copper foil having a thickness of 8 μm, which is the negative electrode current collector, and dried to form a first negative electrode film layer, and then the first slurry was applied to the first negative electrode film layer and dried to form a second negative electrode film layer, and then the above steps were repeated on the other surface of the copper foil, which is the negative electrode current collector, and then a negative electrode sheet was obtained through a process such as cold pressing. The thickness of the first negative electrode film layer on one side of the negative electrode current collector was 82 μm, and the thickness of the second negative electrode film layer was 59 μm. Comparative Example 1-3

[0167] A secondary battery was prepared in a similar manner to Example 1-1, except that the second and third slurries were not applied in preparing the negative electrode sheet.

[0168] The first slurry was applied to both surfaces of a negative electrode current collector made of copper foil with a thickness of 8 μm, and then dried and cold pressed to obtain a negative electrode sheet. The thickness of the negative electrode film layer on one side of the negative electrode current collector was 141 μm. Comparative Example 1-4

[0169] A secondary battery was prepared in a similar manner to Example 1-1, except that the first and third slurries were not applied in preparing the negative electrode sheet.

[0170] The second slurry was applied to both surfaces of a negative electrode current collector made of copper foil with a thickness of 8 μm, and then dried and cold pressed to obtain a negative electrode sheet. The thickness of the negative electrode film layer on one side of the negative electrode current collector was 141 μm. Comparative Examples 1-5

[0171] A secondary battery was prepared in a similar manner to Example 1-1, except that the negative electrode sheet preparation process was different.

[0172] S10 to S20 are the same as in Example 1-1. S30: Preparation of slurry

[0173] The artificial graphite and hard carbon prepared above, conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener were mixed in a mass ratio of 40:55:1.5:3.1:0.4, and then added to deionized water and stirred with a vacuum mixer until the system became uniform, obtaining a slurry with a solid content of 66%. S40: Slurry application

[0174] The slurry was applied to both surfaces of a negative electrode current collector made of copper foil with a thickness of 8 μm, and after drying, cold pressing, etc., a negative electrode sheet was obtained. The thickness of the negative electrode film layer on one side of the negative electrode current collector was 141 μm. Comparative Examples 1-6

[0175] A secondary battery was prepared in a similar manner to Example 1-1, except that the negative electrode sheet preparation process was different.

[0176] S10 to S30 are the same as in the first embodiment. S40: Preparation of second slurry

[0177] The hard carbon prepared above, barium titanate (Dv50 is 100 nm, dielectric constant is 3000 or more), conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener were mixed in a mass ratio of 93:1:1.5:3.1:0.4, and then added to deionized water and stirred with a vacuum stirrer until the system was uniform, obtaining a second slurry with a solid content of 66%. S50: Slurry application

[0178] The first slurry was applied to one surface of the 8 μm thick copper foil as the negative electrode current collector, and dried to form a first negative electrode film layer, the second slurry was applied to the first negative electrode film layer, and dried to form a second negative electrode film layer, and then the above steps were repeated on the other surface of the copper foil as the negative electrode current collector, and after further processes such as cold pressing, a negative electrode sheet was obtained. The thickness of the first negative electrode film layer on one side of the negative electrode current collector was 59 μm, and the thickness of the second negative electrode film layer was 82 μm. Test part (1) Maximum charging rate test

[0179] At 25 ° C., the secondary battery prepared above is fully discharged at a rate of 0.33 C, fully charged at a rate of 0.33 C, and then the fully charged secondary battery is left to stand for 5 min, and then fully discharged at a rate of 0.33 C. The discharge capacity obtained when the fully charged secondary battery is fully discharged at a rate of 0.33 C is the actual capacity of the secondary battery at a rate of 0.33 C, and is designated as C0. The secondary battery is fully charged at a rate of xC0 (a gradient charge rate, for example, 1C0, 1.1C0, 1.2C0, 1.3C0, 1.4C0, etc.), left to stand for 5 min, and then fully discharged at 1 C. After cycling 10 times in this manner, the secondary battery is fully charged at 1 C. When the secondary battery is disassembled and the lithium deposition status on the surface of the negative electrode sheet is observed, if lithium is not deposited on the surface of the negative electrode sheet, the charge rate is increased and measured again until lithium is deposited on the surface of the negative electrode sheet, and the maximum charge rate at which lithium is not deposited on the surface of the negative electrode sheet is recorded. The higher the maximum charge rate of the secondary battery, the better the charging ability at a large rate. (2) Energy density test

[0180] The secondary battery prepared above was fully charged at a rate of 0.33 C at 25° C., and then cycled three times to fully discharge at a rate of 0.33 C, and the discharge energy of the secondary battery was recorded. Energy density of secondary battery=discharge energy of secondary battery / mass of secondary battery. In each of the examples and comparative examples of the present application, the energy density of the secondary battery prepared in Comparative Example 1-1 is set to 100%, and the energy densities of the secondary batteries of the other examples and comparative examples are shown. (3) Cycle life test

[0181] At 25°C, the secondary battery prepared above was fully discharged at a rate of 1C, fully charged at a rate of 1C, and then the fully charged secondary battery was left to stand for 5 minutes, after which it was fully discharged at a rate of 1C. The discharge capacity C0 obtained when this was taken as the initial capacity of the secondary battery. The secondary battery was fully charged at a rate of 3C and fully discharged at a rate of 1C, and a charge-discharge cycle test was performed. The discharge capacity after each cycle was recorded until the discharge capacity of the secondary battery decayed to 80% of the initial capacity, and the number of cycles at this time indicates the cycle life of the secondary battery. It is expected that the higher the number of cycles of the secondary battery, the longer the cycle life will be.

[0182] [Table 1]

[0183] Summarizing the test results of Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-6, it was found that the secondary battery using the negative electrode sheet with the three-layer structure design of the present application had both a high charge rate and a long cycle life. The surface of the negative electrode current collector of Comparative Example 1-1 was provided with a graphite layer and a hard carbon layer in this order, but no functional coating layer was provided, so lithium was easily precipitated during the long-term charge / discharge cycle process of the secondary battery, affecting the cycle life of the secondary battery. The surface of the negative electrode current collector of Comparative Example 1-2 was provided with a hard carbon layer and a graphite layer in this order, but no functional coating layer was provided, so it was difficult for the secondary battery to achieve both a high charge rate and a long cycle life. In Comparative Example 1-3, the graphite layer was provided only on the surface of the negative electrode current collector, so the secondary battery had a long cycle life but was difficult to achieve a high charge rate. In Comparative Example 1-4, the hard carbon layer was provided only on the surface of the negative electrode current collector, so that the secondary battery could have a high charge rate, but it was difficult to have a long cycle life. In Comparative Example 1-5, the mixed layer of graphite and hard carbon was provided on the surface of the negative electrode current collector, so that the secondary battery had difficulty in achieving both a high charge rate and a long cycle life. Compared to Comparative Example 1-1, the hard carbon layer of Comparative Example 1-6 also contains barium titanate, but barium titanate has a poor effect of suppressing the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, and is therefore unlikely to clearly improve the charge rate and cycle life of the secondary battery.

[0184] To summarize the test results of Examples 1-1 to 1-7, it was found that the maximum charge rate and cycle life of the secondary battery both increased with an increase in the thickness of the functional coating layer. The possible reason is that the functional coating layer increases the reverse electric field strength, which increases the effect of suppressing the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, thereby improving the high-rate charge capacity and cycle performance of the secondary battery.

[0185] The test results of Examples 1-1 to 1-7 are summarized as follows: 1 / (H 2 +H 3 ) is smaller than 0.01, the functional coating layer is set to be small relative to the total thickness of the first negative electrode film layer and the second negative electrode film layer, and the effect of inhibiting the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet is not obvious, and therefore it has been found that the effect of improving the maximum charging rate of the secondary battery is not obvious.

[0186] The test results of Examples 1-6 and 1-7 are summarized as follows: 1 It was found that when the thickness is greater than 10, the functional coating layer does not sustainably increase its inhibitory effect on the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, and the maximum charge rate of the secondary battery does not sustainably increase. At the same time, the functional coating layer does not have electrochemical activity and cannot contribute to capacity, so that a thickness exceeding 10 μm significantly reduces the energy density of the secondary battery.

[0187] Next, the inventors investigated the effect of the mass percentage of the ferroelectric material in the functional coating layer on the performance of the secondary battery. The secondary batteries of Example 2-1 to Example 2-6 were prepared in a similar manner to Example 1-2, and the difference was that the mass percentage of the ferroelectric material in the functional coating layer was different.

[0188] [Table 2]

[0189] To summarize the test results of Examples 1-2, 2-1 to 2-6, it was found that when the thickness of the functional coating layer was fixed at 4 μm, the maximum charge rate and cycle life of the secondary battery both increased as the mass percentage of the ferroelectric material in the functional coating layer increased. The possible reason is that in this case, the reverse electric field strength of the functional coating layer increased, which increased the effect of suppressing the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, thereby improving both the high-rate charge capacity and cycle performance of the secondary battery.

[0190] To summarize the test results of Comparative Example 1-1 and Example 2-1, it was found that when the mass percentage of the ferroelectric material in the functional coating layer is small, the functional coating layer obtained thereby does not have a clear effect of inhibiting the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, and therefore the effect of improving the maximum charging rate of the secondary battery is not clear.

[0191] Summarizing the test results of Examples 2-5 and 2-6, it can be seen that when the mass percentage of the ferroelectric material in the functional coating layer exceeds 95%, the cycle performance of the secondary battery is significantly deteriorated. The possible reason is that the adhesive content in the functional coating layer is too low in this case, which may cause the functional coating layer to fall off from the surface of the second negative electrode film layer during the long-term charge-discharge cycle process of the secondary battery.

[0192] Next, the inventors investigated the effect of the volume average particle diameter Dv50 of the ferroelectric material in the functional coating layer on the performance of the secondary battery. The secondary batteries of Example 3-1 to Example 3-6 were prepared in a similar manner to Example 1-2, except that the volume average particle diameter Dv50 of the ferroelectric material in the functional coating layer was different.

[0193] [Table 3]

[0194] Summarizing the test results of Examples 1-2, 3-1 to 3-6, it can be seen that when the thickness of the functional coating layer is fixed at 4 μm and the mass percentage of the ferroelectric material is fixed at 85%, as the volume average particle diameter Dv50 of the ferroelectric material increases, the maximum charge rate and cycle life of the secondary battery both decrease. The possible reason is that as the volume average particle diameter Dv50 of the ferroelectric material increases, the interference of the reverse electric field increases, which deteriorates the effect of inhibiting the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, so that the maximum charge rate and cycle life of the secondary battery both decrease.

[0195] Next, the inventors investigated the influence of the thickness of the first negative electrode film layer and the thickness of the second negative electrode film layer on the performance of the secondary battery. The secondary batteries of Examples 4-1 to 4-7 were prepared in a similar manner to Example 1-2, except that the thicknesses of the first negative electrode film layer and the second negative electrode film layer were different.

[0196] [Table 4]

[0197] To summarize the test results of Examples 4-1 to 4-7, it was found that when the thickness of the second negative electrode film layer increases, the maximum charge rate of the secondary battery increases.

[0198] To summarize the test results of Examples 4-1 to 4-7, the thickness H of the second negative electrode film layer 2 μm and the thickness H of the first negative electrode film layer 3 μm is H 2 / H 3 It was found that when the condition of H is between 0.25 and 4, the secondary battery can achieve both a high maximum charge rate and a long cycle life. 2 / H 3 If is less than 0.25, the second negative electrode film layer is thin, and the effect of improving the maximum charge rate of the secondary battery is not obvious. 2 / H 3 When H is greater than 4, the second negative electrode film layer becomes thicker and the cycle performance of the hard carbon itself becomes poor, resulting in poor cycle performance of the secondary battery. 2 / H 3 It was found that when is greater than 4, the improvement in cycle life of the secondary battery is not obvious.

[0199] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely illustrative, and any embodiment having substantially the same configuration as the technical idea within the technical scope of the present application and having similar effects is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of can be applied to the embodiment within the scope of the present application, and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application.

Claims

1. The negative electrode current collector includes a first negative electrode film layer, a second negative electrode film layer, and a functional coating layer, which are sequentially provided on at least one surface of the negative electrode current collector; the functional coating layer comprises a ferroelectric material; the second negative electrode film layer includes a second negative electrode active material including hard carbon; The first negative electrode film layer includes a first negative electrode active material including graphite; Negative electrode sheet.

2. The thickness of the functional coating layer is H 1 μm, and the thickness of the second negative electrode film layer is H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet is H 1 / (H 2 +H 3 2. The negative electrode sheet according to claim 1, wherein the ratio of the saturation temperature to the surface tension temperature is 0.01 to 0.15, and optionally 0.01 to 0.

08.

3. The thickness of the functional coating layer is H 1 μm, and H 1 The negative electrode sheet according to claim 1 or 2, wherein is 2 to 10, optionally 4 to 6.

4. The thickness of the second negative electrode film layer is H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet is H 2 / H 3 The negative electrode sheet according to any one of claims 1 to 3, wherein is 0.10 to 5, and optionally 0.5 to 4.

5. The volume average particle diameter Dv50 of the ferroelectric material is d 1 μm, and d 1 The negative electrode sheet according to any one of claims 1 to 4, wherein is equal to or less than 1, and optionally is 0.05 to 0.

8.

6. The volume average particle diameter Dv50 of the second negative electrode active material is d 2 μm, and the volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 2 / d 3 The negative electrode sheet according to any one of claims 1 to 5, wherein is 0.1 to 1, and optionally is 0.2 to 0.

8.

7. The negative electrode sheet according to any one of claims 1 to 6, wherein the mass percentage of the ferroelectric material in the functional coating layer is W1, and based on the total mass of the functional coating layer, W1 is 70% to 95%, and optionally 80% to 95%.

8. The mass percentage of hard carbon in the second negative electrode film layer is W2, and based on the total mass of the second negative electrode film layer, W2 is 68% or more, optionally 90% to 98%; and / or The mass percentage of graphite in the first negative electrode film layer is W3, and based on the total mass of the first negative electrode film layer, W3 is 78% or more, optionally 90% to 98%. The negative electrode sheet according to any one of claims 1 to 7.

9. The negative electrode sheet according to any one of claims 1 to 8, wherein the second negative electrode active material satisfies at least one of the following conditions (1) to (5): (1) The volume average particle diameter Dv50 of the second negative electrode active material is d 2 μm, and d 2 is 3 to 11, selectable from 3 to 7. (2) The particle size distribution index (Dv90-Dv10) / Dv50 of the second negative electrode active material is α 1 and α 1 is between 0.6 and 5, selectable between 1 and 4. (3) The specific surface area of ​​the second negative electrode active material is 3 m 2 / g ~ 7m 2 / g, and optionally 4m 2 / g to 6m 2 / g. (4) The powder compaction density of the second negative electrode active material at 20000 N is 0.9 g / cm 3~1.3g / cm 3 and optionally 1 g / cm 3 ~1.2g / cm 3 It is. (5) The second negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the quantity ratio of the primary particles in the second negative electrode active material is 90% to 100%.

10. The negative electrode sheet according to any one of claims 1 to 9, wherein the first negative electrode active material satisfies at least one of the following conditions (1) to (7): (1) The volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 3 is 9-18, selectable from 11-15. (2) The particle size distribution index (Dv90-Dv10) / Dv50 of the first negative electrode active material is α 2 and α 2 is between 0.2 and 5, selectable between 0.3 and 4. (3) The specific surface area of ​​the first negative electrode active material is 0.6 m 2 / g to 1.5m 2 / g, and optionally 0.8m 2 / g to 1.4m 2 / g. (4) The powder compaction density of the first negative electrode active material at 20,000 N is 1.4 g / cm 3 ~1.85g / cm 3 and optionally 1.6 g / cm 3 ~1.75g / cm 3 It is. (5) The graphitization degree of the first negative electrode active material is 91% to 95%, and optionally 92% to 94%. (6) The first negative electrode active material includes artificial graphite, natural graphite, or a combination thereof, and optionally, a surface of the artificial graphite has a carbon coating layer. (7) The first negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the quantity ratio of the secondary particles in the first negative electrode active material is 80% to 100%.

11. The negative electrode sheet according to any one of claims 1 to 10, wherein the dielectric constant of the ferroelectric material is 50 or more, and optionally 50 to 100,000.

12. The ferroelectric material includes one or a combination of a plurality of ferroelectric materials selected from inorganic ferroelectric materials and organic ferroelectric materials; Optionally, the inorganic ferroelectric material comprises one or more combinations selected from perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layer structure compounds, lithium niobate, lithium tantalate, lead metaniobate, and lead barium lithium niobate; Optionally, the organic ferroelectric material may include one or more combinations selected from the group consisting of vinylidene fluoride homopolymer or copolymer, 2,5-dibromo-3,6-dihydroxy-p-benzoquinone, phenazine-chloranilic acid, and croconic acid. The negative electrode sheet according to any one of claims 1 to 11.

13. The functional coating layer further comprises an adhesive and / or a dispersant; Optionally, the adhesive comprises one or a combination of adhesives selected from styrene butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan; Optionally, the dispersant comprises sodium carboxymethylcellulose.

14. A secondary battery comprising the negative electrode sheet according to any one of claims 1 to 13.

15. A battery module comprising the secondary battery according to claim 14.

16. A battery pack comprising one of the secondary battery according to claim 14 and the battery module according to claim 15.

17. A power consuming device comprising at least one of the following: the secondary battery according to claim 14; the battery module according to claim 15; and the battery pack according to claim 16.

Citation Information

Patent Citations

  • Negative electrode plate and lithium ion battery

    CN114050231A

  • Negative electrode and nonaqueous electrolyte secondary battery using it

    JP2008059999A

  • Secondary battery

    JP2020109735A

  • Negative Electrode, Method For Preparing The Same And Electrochemical Device

    US20190190028A1

  • Negative electrode for all-solid-state secondary cell, method for manufacturing same, and all-solid-state secondary cell

    WO2021241423A1