Methods for wet atomic layer etching of copper.
The novel wet ALE process for copper etching using carboxylic acid-based ligands and ammonium hydroxide achieves atomic-level precision and selectivity, addressing the challenges of conventional etching methods by ensuring precise copper removal and uniformity in semiconductor manufacturing.
Patent Information
- Application Number
- JP2024524368
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-04-20
- Filing Date
- 2022-09-14
- Publication Date
- 2024-10-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional etching techniques for copper in semiconductor manufacturing lack atomic-level control and etch selectivity, particularly in sub-32 nm back-end-of-line (BEOL) Cu lines and sub-100 nm Cu bond pads, leading to issues such as flat areas near contact pads and inability to achieve sub-nanometer recess control.
A novel wet atomic layer etch (ALE) process using a complexing step with a carboxylic acid-based ligand in an organic solvent and a dissolution step with an aqueous solvent, such as ammonium hydroxide, to form and remove a self-limiting copper carboxylate layer, ensuring monolayer precision and selectivity.
The process provides atomic-level etch control and high selectivity, enabling precise copper removal without affecting underlying copper metal layers, suitable for sub-nanometer recess control in copper pad recesses and three-dimensional interconnects, reducing surface roughness and improving uniformity.
Smart Images

Figure 2024539246000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 277,443, entitled "Method for Wet Atomic Layer Etching of Copper," filed November 9, 2021, and U.S. Nonprovisional Patent Application No. 17 / 725,072, entitled "Method for Wet Atomic Layer Etching of Copper," filed April 20, 2022, the disclosures of which are expressly incorporated by reference in their entireties herein.
[0002] This application is related to commonly owned co-pending U.S. patent application Ser. No. 17 / 674,579, entitled "Methods for Wet Atomic Layer Etching of Ruthenium," filed Feb. 17, 2022, the disclosure of which is expressly incorporated by reference herein in its entirety. [Background technology]
[0003] This disclosure relates to semiconductor device manufacturing, and in particular to the etching and removal of metals, such as, but not limited to, copper (Cu) metal. During typical semiconductor fabrication, various metals formed on a substrate may be removed by patterned etching, chemical mechanical polishing, as well as other techniques. Various techniques are known for etching layers on a substrate, including plasma-based, or gas-phase (dry etching, or liquid-based (wet etching).
[0004] Wet etching involves dispensing a chemical solution onto the surface of a substrate or immersing the substrate in the chemical solution. Often the chemical solution contains a solvent, chemicals designed to react with materials on the substrate surface, and chemicals that facilitate dissolution of the reaction products. Exposure of the substrate surface to an etchant results in removal of material from the substrate. The composition and temperature of the etchant can control the etch rate, specificity, and remaining material on the substrate surface after etching.
[0005] As substrate feature geometries continue to shrink and the types of structures evolve, the challenges of etching substrates increase. One technique that has been utilized to address these challenges is atomic layer etching (ALE). ALE processes are generally known to involve the sequential removal of thin layers through one or more self-limiting reactions. For example, ALE typically refers to techniques that can etch with atomic precision, i.e., by removing only one or more monolayers of material. In general, ALE methods rely on the chemical modification of the surface to be etched, and the subsequent selective removal of the modified layer. Thus, ALE processes improve performance by separating the etching process into successive steps of surface modification and removal of the modified surface. Such processes often involve multiple cyclical successions of layer modification and etching steps. The modification step can modify the exposed surface, and the etching step can selectively remove the modified layer.
[0006] A variety of ALE processes are known, including plasma ALE, thermal ALE, and wet ALE techniques. Like all ALE processes, wet ALE is typically a cyclic process that selectively removes material from a surface using successive self-limiting reactions. However, unlike thermal and plasma ALE, the reactions used in wet ALE occur primarily in the liquid phase. Compared to other ALE processes, wet ALE is often desirable because it can be performed at (or near) room temperature and atmospheric pressure. In addition, the self-limiting nature of the wet ALE process leads to a smoothing of the surface during etching, rather than the roughness commonly seen during other etching processes.
[0007] The wet ALE process typically begins with a surface modification step, which exposes the material to a first solution to form a self-limiting modified surface layer. The modified surface layer can be formed by oxidation, reduction, ligand binding, or ligand exchange. Ideally, the modified surface layer is limited to the top monolayer of the material and acts as a passivation layer that prevents the modification reaction from proceeding any further. After the modified surface layer is formed, the wet ALE process can be followed by a dissolution step in which the modified surface layer is exposed to a second solution to selectively dissolve the modified surface layer. The dissolution step must selectively dissolve the modified surface layer without removing any of the underlying unmodified material. This selectivity can be achieved by using a different solvent in the dissolution step than that used in the surface modification step, by changing the pH, or by changing the concentration of other components in the second solution. The wet ALE cycle can be repeated until the desired or specified amount of etching is achieved.
[0008] Copper (Cu) metal is commonly used as an interconnect metal in integrated circuits. Copper / Cu hybrid junctions for three-dimensional interconnects (3DI) and fully aligned vias (FAV) rely on sub-nanometer control of copper pad recesses to form electrical contacts, which may be surrounded by dielectric materials, for example. In some conventional processes, the copper pad recess is achieved with chemical mechanical planarization (CMP). However, as feature sizes shrink, exposed copper and dielectric materials on the substrate surface tend to polish at the same rate, resulting in flat areas near the contact pads that severely limit the process window. Some hybrid junction and FAV process nodes are too small for CMP. For example, CMP cannot provide sub-nm copper recess control with good copper uniformity for FAV or sub-32 nm back-end-of-line (BEOL) Cu lines for sub-100 nm Cu bond pads.
[0009] Sequential etching techniques have also been utilized to etch metals such as copper. Known sequential etching techniques for etching metals often use an oxidizer (e.g., oxygen plasma, ozone, or hydrogen peroxide) in a self-limiting oxidation step to form an oxide on the exposed surface of the metal, and then perform an acid wet etch to selectively remove the oxide. While these known techniques provide a sequential hybrid or wet etching process, there is a lack of atomic layer control due to the strong oxidizer required to form the oxide in the self-limiting oxidation step. Thus, there is a need for an improved wet etching method for etching Cu metal that provides etch control at the atomic level while also achieving high etch selectivity to other materials exposed during the etching process. Summary of the Invention [Means for solving the problem]
[0010] The present disclosure provides a novel wet atomic layer etching (ALE) process for etching copper (Cu) metal. More specifically, the present disclosure provides various embodiments of methods utilizing novel etching chemistries for etching copper in a wet ALE process. By utilizing the novel etching chemistries disclosed herein in a repeated wet ALE process, the present disclosure provides highly selective etching of copper with monolayer precision.
[0011] In the present disclosure, a wet ALE process is provided for etching a copper metal layer formed on a substrate, the exposed surface of the copper metal layer comprising an oxidized copper surface layer (e.g., a copper oxide layer). The wet ALE process is a cyclic process including one or more ALE cycles, each ALE cycle including a complexing step and a dissolving step. In the complexing step, the surface of the substrate is exposed to a complexing solution including a complexing agent (e.g., a carboxylate-based ligand) dissolved in a first solvent. The complexing agent reacts with the oxidized copper surface layer to form a ligand-metal complex (e.g., a complex-bonded oxidized copper surface layer), which is insoluble in the first solvent.
[0012] After the ligand-metal complexes are formed, a dissolution step can be performed to selectively dissolve and remove the ligand-metal complexes without removing the underlying copper metal layer. In the dissolution step, the surface of the substrate is exposed to a dissolution solution that includes a reactant and an aqueous solvent. The reactant reacts with the ligand-metal complexes formed during the complexation step to form soluble species, which are dissolved in the aqueous solvent. By removing the ligand-metal complexes in the dissolution step, the underlying copper metal layer is exposed, which reacts with the aqueous solvent in the dissolution solution to reoxidize the underlying copper metal layer to form a new oxidized copper surface layer (e.g., a copper hydroxide layer), which can be used to form new ligand-metal complexes in the next ALE cycle. The complexation and dissolution steps can be repeated for one or more ALE cycles until the desired amount of copper metal is removed. A purge step can be performed between the complexation and dissolution steps to remove the complexation solution and the dissolution solution from the substrate surface, along with excess reactants and soluble species contained therein.
[0013] In the present disclosure, the complexing solution includes a carboxylic acid or other ligand dissolved in a first solvent (e.g., an organic solvent such as isopropyl alcohol, IPA, etc.), and the dissolving solution includes a base dissolved in an aqueous solution (e.g., ammonium hydroxide in deionized water, etc.). When a carboxylic acid is utilized in the complexing solution, the ligand-metal complex formed during the complexing step is a copper carboxylate layer that is insoluble in the first solvent used in the complexing solution, but soluble in the aqueous dissolving solution. In one embodiment, oxalic acid may be utilized in the complexing solution to form a copper oxalate layer on the unmodified copper metal layer. However, other carboxylic acids may also be utilized in the complexing solution to combine with the oxidized copper surface layer to form other copper carboxylate layers that are insoluble in the first solvent, but soluble in the aqueous dissolving solution.
[0014] When oxalic acid is utilized in the complexing solution, the oxalic acid reacts with the oxidized copper surface layer to form a copper oxalate layer on the underlying copper metal layer. In the present disclosure, the complexing solution may be provided to the substrate surface for a period of time necessary to form at least one monolayer of copper oxalate on the underlying copper metal layer. Copper oxalate is insoluble in most solvents, but is soluble in ammonium hydroxide solution by a ligand exchange mechanism. Thus, in some embodiments, the dissolution solution may include an aqueous ammonium hydroxide solution. The ammonium hydroxide contained in the dissolution solution selectively removes the copper oxalate layer to expose the copper metal layer underlying the copper oxalate layer. Once the copper oxalate layer is selectively removed, the aqueous solvent contained in the dissolution solution reoxidizes the exposed surface of the underlying copper metal layer to form a new oxidized copper surface layer (e.g., a copper hydroxy layer) on the underlying copper metal layer. Since metallic copper is also etched by ammonium hydroxide, the concentration of ammonium hydroxide used in the dissolution solution may be selected to provide good selectivity between the copper oxalate layer and the underlying copper metal layer. In some embodiments, a relatively low concentration (e.g., less than 10 mM) of ammonium hydroxide may be utilized in the dissolution solution to avoid etching the underlying copper metal layer and any oxidized copper surface layer formed thereon.
[0015] Cross-contamination of the complexing and dissolving solutions can result in successive etching processes, leading to increased surface roughness and poor uniformity. To avoid cross-contamination, a purge step may be performed between the complexing and dissolving steps to remove excess reactants from the substrate surface and prevent successive etching during the dissolving step. In some embodiments, a purge solution may be provided to the substrate surface after each of the complexing and dissolving steps to remove excess reactants and soluble species from the substrate surface.
[0016] As mentioned above and as further described herein, the present disclosure provides various embodiments of methods utilizing the novel etching chemistries disclosed herein for etching copper in a wet ALE process. It should be understood that the order of description of the different steps described herein is presented for ease of explanation. In general, the steps can be performed in any suitable order. In addition, although reference may be made in different places in the present disclosure to each of the different features, techniques, configurations, etc. described herein, it is intended that each of the concepts can be performed independently of each other or in combination with each other. Thus, the present invention can be embodied and viewed in many different ways.
[0017] According to one embodiment, an etching method for etching copper according to the present disclosure is provided herein. The method may generally begin by receiving a substrate having a copper metal layer formed thereon, with an oxidized copper surface layer of the copper metal layer exposed on the substrate surface. The method may then include exposing the substrate surface to a complexing solution including a carboxylic acid dissolved in an organic solvent. The carboxylic acid may react with the oxidized copper surface layer to form a carboxylate copper layer, which is insoluble in the organic solvent. The method may then include, following the formation of the carboxylate copper layer, removing the complexing solution from the substrate surface and exposing the substrate surface to a dissolving solution to selectively remove the carboxylate copper layer to expose the copper metal layer underlying the carboxylate copper layer. The dissolving solution may generally include a reactant and an aqueous solvent. The reactant may react with the carboxylate copper layer to form a soluble species that is dissolved by the aqueous solvent. The method may then include removing the dissolving solution and the soluble species from the substrate surface to etch the copper metal layer.
[0018] In some embodiments, the method may further include repeating the steps of exposing the substrate surface to a complexing solution, removing the complexing solution, exposing the substrate surface to a dissolving solution, and removing the dissolving solution for multiple cycles until a predetermined amount of copper metal is removed from the substrate. In some embodiments, removing the complexing solution and removing the dissolving solution may each include rinsing the substrate surface with a purge solution to remove excess reactants from the substrate surface and prevent the complexing solution and the dissolving solution from mixing.
[0019] A wide variety of etching chemicals may be used in the complexing solution and dissolving solution. In some embodiments, for example, the complexing solution may include: (a) a carboxylic acid, such as oxalic acid, mandelic acid, malic acid, maleic acid, or fumaric acid, and (b) an organic solvent, such as isopropyl alcohol (IPA) or other alcohols, diethyl ether ((C2H5)2O), acetonitrile (C2H3N), dimethyl sulfoxide (C2H6OS), ketones, or acetates. Other carboxylic acids and organic solvents may also be used in the complexing solution.
[0020] In some embodiments, the dissolution solution may include an aqueous base solution. The reactant included in the dissolution solution may be virtually any weak base. For example, the reactant may be ammonium hydroxide (NH4OH), potassium hydroxide (KOH), sodium hydroxide (NaOH), tetramethylammonium hydroxide (CH3)4NOH), potassium carbonate (K2CO3), or ammonium carbonate (NH4)2CO3). Other weak bases may also be included in the dissolution solution.
[0021] In one exemplary embodiment, the carboxylic acid contained in the complexing solution may be oxalic acid and the organic solvent contained in the complexing solution may be isopropyl alcohol (IPA). In one such embodiment, the oxalic acid may react with the oxidized copper surface layer to form a copper oxalate layer that is insoluble in IPA but soluble in the aqueous solvent contained in the dissolution solution.
[0022] In some embodiments, exposing the substrate surface to the complexing solution may include supplying the complexing solution to the substrate surface for a period of time necessary to form at least one monolayer of a copper carboxylate layer on the underlying copper metal layer. When the carboxylic acid is oxalic acid, the complexing solution may be supplied to the substrate surface for at least 5 seconds to form at least one monolayer of copper oxalate on the underlying copper metal layer.
[0023] After exposing the substrate surface to the dissolving solution to selectively remove the carboxylate copper layer and expose the underlying copper metal layer, the dissolving solution can re-oxidize the exposed surface of the underlying copper metal layer to form a new oxidized copper surface layer, but the dissolving solution does not etch the underlying copper metal layer or the new oxidized copper surface layer.
[0024] In one exemplary embodiment, the dissolution solution may include aqueous ammonium hydroxide (NH4OH). If aqueous ammonium hydroxide is utilized, after selectively removing the copper carboxylate layer, the concentration of ammonium hydroxide in the dissolution solution may be maintained below a level that would etch the underlying copper metal layer or the newly oxidized copper surface layer.
[0025] According to another embodiment, a method for etching copper using a wet atomic layer etching (ALE) process is provided herein in accordance with the present disclosure. The method may generally include: a) receiving a substrate having a copper (Cu) metal layer with an oxidized Cu surface layer formed thereon; b) exposing the oxidized Cu surface layer to a complexing solution containing a complexing agent to bond the complexing agent to the oxidized Cu surface layer and form a complexed oxidized Cu surface layer on the Cu metal layer; c) rinsing the substrate with a first purge solution to remove the complexing solution from the surface of the substrate; d) selectively removing the complexed oxidized Cu surface layer from the Cu metal layer by exposing the complexed oxidized Cu surface layer to a dissolving solution that dissolves the complexed oxidized Cu surface layer and forms a new oxidized Cu surface layer on the Cu metal layer; and e) rinsing the substrate with a second purge solution to remove the dissolving solution from the surface of the substrate to etch the Cu metal layer.
[0026] In one embodiment, the method may further include repeating steps b)-e) at least once to further etch the Cu metal layer. In some embodiments, steps b) and d) have no temporal overlap. In some embodiments, the substrate may have an exposed dielectric layer thereon that is not etched by steps b)-e).
[0027] As discussed above, a wide variety of etching chemistries may be used in the complexing solution and dissolving solution. In some embodiments, the complexing solution may include a complexing agent dissolved in an organic solvent. In one exemplary embodiment, the complexing agent may include oxalic acid dissolved in isopropyl alcohol (IPA). Other carboxylic acids and organic solvents may also be used in the complexing solution.
[0028] In some embodiments, the dissolution solution may include a basic aqueous solution. In one exemplary embodiment, the dissolution solution may include ammonium hydroxide (NH4OH) dissolved in an aqueous solvent. Other bases may be included in the dissolution solution. However, it is important that the dissolution solution does not etch the Cu metal layer or the newly oxidized Cu surface layer. The dissolution solution may include ammonium hydroxide (NH4OH), and after selectively removing the complex-bonded oxidized Cu surface layer, the concentration of ammonium hydroxide in the dissolution solution may be selected and maintained below a level that etches the Cu metal layer or the newly oxidized Cu surface layer.
[0029] It should be noted that this "Summary" does not specify all embodiments and / or inherently novel aspects of the invention described in this disclosure or claims. Instead, this "Summary" provides only a preliminary discussion of various embodiments and corresponding points of novelty over the prior art. For additional details and / or anticipated aspects of the invention and embodiments, the reader is directed to the "Description of Embodiments" section of this disclosure and corresponding figures, as further discussed below.
[0030] A more detailed understanding of the present invention and its advantages can be obtained by reference to the following description taken in conjunction with the accompanying drawings, in which like reference numerals indicate like features, and in which it should be noted, however, that the accompanying drawings depict only exemplary embodiments of the disclosed concepts, and therefore should not be considered as limiting the scope of the present invention, as the disclosed concepts may encompass other equally effective embodiments. [Brief description of the drawings]
[0031] [Figure 1] 1 illustrates an example of a cyclic wet atomic layer etching (ALE) process that can be used to etch copper according to the present disclosure. [Diagram 2] 2 is a graph of experimental results illustrating exemplary etch amounts (expressed in nanometers (nm)) as a function of the number of wet ALE cycles that may be achieved when using the wet ALE process shown in FIG. 1 to etch copper metal layers on various patterned coupons. [Diagram 3] 2 is a graph of experimental results showing the effect of changing the temperature of the dissolving solution (expressed in ° C.) on the copper etch rate (expressed in nm / cycle) when etching a patterned coupon containing 0.5 μm Cu pads with 1 μm pitch using the wet ALE process shown in FIG. [Figure 4] 1 is a schematic cross-sectional view of a copper-filled recessed feature in a dielectric film illustrating the amount of material removed and the convexity of the copper-filled recessed feature. [Diagram 5] 2 is a graph of experimental results showing copper convexity (expressed in nanometers (nm)) achieved as a function of wet ALE cycles when etching a patterned coupon containing 0.5 μm Cu pads with 1 μm pitch using the wet ALE process shown in FIG. [Figure 6] FIG. 2 is a graph of experimental results showing copper roughness (expressed in Rq (nm)) achieved as a function of wet ALE cycles when etching a patterned coupon containing 0.5 μm Cu pads with 1 μm pitch using the wet ALE process shown in FIG. 1 . [Figure 7] 2 is a graph of experimental results showing dielectric (e.g., TEOS) roughness achieved as a function of wet ALE cycles when etching a patterned coupon containing 0.5 μm Cu pads with 1 μm pitch using the wet ALE process shown in FIG. [Figure 8]1 is a graph of experimental results showing an exemplary amount of material removed (expressed in nm) after five etching cycles as a function of immersion time (expressed in seconds (s)) in a dissolving solution (e.g., NHOH). [Figure 9] 1 is a graph of experimental results showing an exemplary amount of material removed (expressed in nm) after five etching cycles as a function of immersion time (expressed in seconds (s)) in a complexing solution (e.g., oxalic acid). [Figure 10] FIG. 1 is a schematic diagram showing the formation of a monolayer of oxalic acid chemisorbed onto an oxidized copper surface layer. [Figure 11A] Illustrates common challenges (e.g., seams and keyholes in bonded wafers) encountered in three-dimensional interconnect (3DI) hybrid bonding processes when copper (Cu) metal features are recessed into dielectric layers using conventional etching techniques. [Figure 11B] Illustrates common challenges (e.g., seams and keyholes in bonded wafers) encountered in three-dimensional interconnect (3DI) hybrid bonding processes when copper (Cu) metal features are recessed into dielectric layers using conventional etching techniques. [Figure 12A] We show how the wet ALE process described herein for etching copper can be applied to a 3DI hybrid bonding process and utilized to eliminate seams and keyholes in bonded wafers. [Figure 12B] We show how the wet ALE process described herein for etching copper can be applied to a 3DI hybrid bonding process and utilized to eliminate seams and keyholes in bonded wafers. [Figure 13A] This paper presents common challenges encountered in fully self-aligned via (FSAV) processes. [Figure 13B] This paper presents common challenges encountered in fully self-aligned via (FSAV) processes. [Figure 13C]We show how the wet ALE process described herein for etching copper can be applied to a fully self-aligned via (FSAV) process. [Figure 14] FIG. 1 is a block diagram of an exemplary processing system in which the techniques described herein can be used to etch a copper metal layer. [Figure 15] FIG. 1 is a flow diagram illustrating one embodiment of a method utilizing the techniques described herein. [Figure 16] FIG. 11 is a flow diagram illustrating another embodiment of a method utilizing the techniques described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The present disclosure provides a novel wet atomic layer etching (ALE) process for etching copper (Cu) metal. More specifically, the present disclosure provides various embodiments of methods utilizing novel etching chemistries for etching copper in a repeated wet ALE process. By utilizing the novel etching chemistries disclosed herein in a repeated wet ALE process, the present disclosure provides highly selective etching of copper with monolayer precision.
[0033] The repeated wet ALE process described herein generally includes one or more ALE cycles, and each ALE cycle may include a complexing step and a dissolving step. In the complexing step, the copper metal layer having an oxidized copper surface layer is exposed to a complexing solution, the complexing solution including a complexing agent dissolved in a first solvent. In some embodiments, the complexing solution may include a carboxylic acid dissolved in an organic solvent. The carboxylic acid reacts with and bonds to the oxidized copper surface layer to form an insoluble carboxylate copper layer on the unmodified copper metal layer. After the carboxylate copper layer is formed, a dissolving step is performed to selectively remove the carboxylate copper layer from the underlying copper metal layer. For example, the carboxylate copper layer can be dissolved in a dissolving solution, the dissolving solution including a reactant dissolved in an aqueous solvent. The dissolving solution selectively removes the carboxylate copper layer without removing the unmodified copper metal layer underlying the carboxylate copper layer. By removing the copper carboxylate layer, an underlying copper metal layer is exposed, which can then react with the aqueous solvent in the dissolution solution to reoxidize the underlying copper metal layer to form a new oxidized copper surface layer, which can be used to form a new copper carboxylate layer in the next ALE cycle. The complexing and dissolution steps may be repeated for one or more ALE cycles until a desired amount of the copper metal layer is removed. A purging step is performed between the complexing and dissolution steps to remove excess reactants from the substrate surface and to prevent mixing of the complexing solution with the dissolution solution, thus preventing continued etching during the dissolution step.
[0034] The techniques described herein for etching copper can be utilized in a wide variety of applications. In some embodiments, for example, the wet ALE processes and methods disclosed herein can be used to etch copper pad recesses to form electrical contacts in three-dimensional interconnect (3DI) hybrid bond and fully aligned via (FAV) applications. The disclosed processes and methods offer several advantages over conventional methods commonly used to etch copper. For example, unlike conventional CMP techniques used to planarize copper pads, the wet ALE processes and methods disclosed herein provide sub-nanometer control of copper pad recesses with high selectivity to the dielectric material (e.g., silicon oxide) surrounding the copper pad. This makes the wet ALE processes and methods disclosed herein highly suitable as an adjunct to CMP, especially at small pad sizes.
[0035] Unlike conventional hybrid and wet etching processes commonly used to etch metals such as copper, the wet ALE process and method disclosed herein does not use a strong oxidizing agent to form an oxide on the exposed surface of the copper metal layer in a self-limiting oxidation step. Instead, the wet ALE process and method disclosed herein distributes a complexing solution onto the substrate surface for a predetermined time required to form at least one monolayer of carboxylic acid on the oxidized copper surface layer. The monolayer of carboxylic acid reacts with and bonds to the oxidized copper surface layer on the underlying copper metal layer to form a monolayer of copper carboxylate. The monolayer of copper carboxylate is then selectively removed in a subsequent dissolution step without removing the unmodified copper metal layer or the dielectric material surrounding the copper metal layer beneath the monolayer of copper carboxylate. As a result, the wet ALE process and method disclosed herein provides atomic level etch control of the copper carboxylate layer while also achieving high etch selectivity to other materials exposed during the etching process (e.g., dielectric materials, unmodified copper metal layer, and oxidized copper surface layer).
[0036] FIG 1 illustrates an example of a wet ALE process that may be used to etch copper in accordance with the present disclosure. More specifically, FIG 1 illustrates exemplary steps performed during one cycle of a wet ALE process that may be utilized to etch a copper metal layer in accordance with the present disclosure. As shown in FIG 1 and described in more detail below, the wet ALE process described herein is a cyclic process consisting of one or more ALE cycles, each ALE cycle including a complexing step 100, a first purging step 140, a dissolving step 150, and a second purging step 160.
[0037] In the process shown in FIG. 1, during the complexing step 100, the copper metal layer 105 surrounded by the dielectric material 110 contacts a complexing solution 125 to react with and bond to the oxidized copper surface layer 115 (e.g., copper oxide surface layer) of the copper metal layer 105. The complexing solution 125 used in the complexing step 100 may generally include a complexing agent 120 dissolved in a first solvent. In some embodiments, the complexing agent 120 may be a carboxylic acid and the first solvent may be an organic solvent. In one exemplary embodiment, the complexing agent 120 may be oxalic acid and the first solvent may be isopropyl alcohol (IPA). However, other complexing agents and solvents may be utilized, as described in more detail below.
[0038] During the complexation step 100 shown in Figure 1, the complexing agent 120 reacts with and binds to the oxidized copper surface layer 115 to form a ligand-metal complex 130. In some embodiments, the complexing agent 120 may include a carboxylate-based ligand (e.g., a carboxylic acid, such as but not limited to oxalic acid) that selectively binds to the oxidized copper surface layer 115 and causes the oxidized copper surface layer 115 to react with the carboxylate-based ligand to form an insoluble ligand-metal complex 130. When a carboxylate-based ligand is used, the ligand-metal complex 130 formed during the complexation step 100 is a copper carboxylate layer that is insoluble in the first solvent but is soluble in the subsequent dissolution step 150.
[0039] In some embodiments, the complexing solution 125 may be dispensed onto the substrate surface for a predetermined time necessary to form at least one monolayer of carboxylic acid on the oxidized copper surface layer 115. If oxalic acid is included in the complexing solution 125, multiple monolayers of oxalic acid may be formed on the oxidized copper surface layer 115 after a certain time. This is because oxalic acid has a high packing density and can form multiple monolayers on the oxidized copper surface layer 115 through hydrogen bonding (see, for example, FIG. 10). If the substrate surface is rinsed after the complexing step 100, the excess monolayer of oxalic acid may be removed from the oxidized copper surface layer 115, such that after rinsing, a single monolayer of oxalic acid remains on the oxidized copper surface layer 115.
[0040] After performing the complexation step 100 to form the ligand-metal complex 130 (e.g., a copper carboxylate layer), a first purge step 140 is performed to remove the complexation solution 125 from the substrate surface. In the first purge step 140, the substrate is rinsed with a first purge solution 135 to remove excess reactants from the substrate surface and / or to remove an extra monolayer of oxalic acid from the oxidized copper surface layer 115. The first purge solution 135 should not react with the ligand-metal complex 130 formed during the complexation step 100 or with the reagents present in the complexation solution 125. In some embodiments, the first purge solution 135 used during the first purge step 140 may use the same solvent (e.g., IPA) as used in the complexation solution 125. However, other solvents may be utilized, as described in more detail below. In some embodiments, the first purge step 140 may be long enough to completely remove all excess reactants from the substrate surface.
[0041] After the substrate is rinsed, a dissolving step 150 is performed to selectively remove the ligand-metal complexes 130 (e.g., copper carboxylate layer) formed during the complexing step 100. In the dissolving step 150, the substrate is exposed to a dissolving solution 145 to selectively remove or dissolve the ligand-metal complexes 130 without removing the unmodified copper metal layer 105 underlying the ligand-metal complexes 130 or the dielectric material 110 surrounding the copper metal layer 105. The dissolving solution 145 may generally include a reactant dissolved in an aqueous solvent (e.g., deionized water, etc.). In some embodiments, the reactant may be a base, such as ammonium hydroxide (NH4OH), and the aqueous solvent may be deionized water (DI H2O). As described in more detail below, other reactants and solvents may also be utilized. In order to selectively remove the ligand-metal complex 130, the ligand-metal complex 130 must be soluble and the unmodified copper metal layer 105 underlying the ligand-metal complex 130 must be insoluble in the dissolution solution 145. The solubility of the ligand-metal complex 130 allows it to be removed by dissolving it in the bulk dissolution solution 145. In some embodiments, the dissolution step 150 may continue until the ligand-metal complex 130 is completely dissolved.
[0042] The wet ALE process shown in FIG. 1 utilizes ligand binding followed by a dissolution method to selectively remove the ligand-metal complex 130 without removing the unmodified copper metal layer 105 underneath the ligand-metal complex 130. In the ligand binding followed by dissolution method, the ligand binding and dissolution steps do not have a time overlap. Instead, the ligand is dissolved in a liquid solvent in which the ligand-metal complex 130 is insoluble (e.g., an organic solvent used in the complexing solution 125, e.g., IPA). During the complexing step 100, the ligand dissolved in the liquid solvent reacts with the oxidized copper surface layer 115 to form an insoluble layer of the ligand-metal complex 130. This insoluble layer is dissolved in the subsequent dissolution step 150 when the substrate surface is exposed to a different liquid solvent in which the ligand-metal complex 130 is soluble (e.g., an aqueous solvent used in the dissolving solution 145, e.g., DI H2O). In methods where ligand binding is followed by dissolution, removal of the ligand-metal complex 130 (e.g., a copper carboxylate layer) is limited by the ligand packing density of the ligands on the surface. The ligand binding in the complexation step 100, and therefore the dissolution of the ligand-metal complex 130 in the dissolution step 150, is self-limiting.
[0043] By removing the ligand-metal complex 130 (e.g., a copper carboxylate layer) in a dissolution step 150, the underlying copper metal layer 105 is exposed to a dissolution solution 145. The exposed surface of the underlying copper metal layer 105 reacts with an aqueous solvent (e.g., DI H2O) in the dissolution solution 145 to re-oxidize the copper metal layer 105 and form a new oxidized copper surface layer 115 on the underlying copper metal layer 105.
[0044] Once the ligand-metal complex 130 (e.g., the copper carboxylate layer) has been dissolved in the dissolution solution 145 and a new oxidized copper surface layer 115 has been formed, a second purge step 160 may be performed to remove the dissolution solution 145 from the substrate surface, completing the wet ALE etch cycle shown in FIG. 1. In the second purge step 160, the substrate is rinsed with a second purge solution 165, which may be the same as or different from the first purge solution 135. In some embodiments, the second purge solution 165 may use the same solvent as that used in the complexing solution 125 (e.g., IPA). However, as will be described in more detail below, other solvents may also be utilized. The second purge step 160 may generally continue until the dissolution solution 145, and / or the reactants and soluble species contained therein, are completely removed from the substrate surface.
[0045] Embodiments of the present disclosure describe wet ALE of a copper (Cu) metal layer on a substrate. The wet ALE process described herein is a highly uniform cyclic etching process that provides atomic level Cu etch control while also achieving high etch selectivity over other materials, such as silicon oxide and other dielectric materials. As described above, the cyclic wet ALE process shown in FIG. 1 generally includes the steps of: a) receiving a substrate having a copper metal layer 105 with an oxidized copper surface layer 115 formed thereon; b) exposing the oxidized copper surface layer 115 to a complexing solution 125 containing a complexing agent 120 to bond the complexing agent 120 to the oxidized copper surface layer 115 and form a complexed oxidized copper surface layer (e.g., ligand-metal complex 130) on the copper metal layer 105; and c) rinsing the substrate with a first purge solution 135 to remove the complexing agent 120 from the copper metal layer 105. d) selectively removing the complexed oxidized copper surface layer from the copper metal layer 105 by exposing the complexed oxidized copper surface layer to a dissolving solution 145 that dissolves the complexed oxidized copper surface layer and forms a new oxidized copper surface layer 115 on the copper metal layer 105; and e) rinsing the substrate with a second purge solution 165 to remove the dissolving solution 145 from the surface of the substrate and etch the copper metal layer 105. In some embodiments, steps b)-e) may be repeated for one or more ALE cycles until a desired amount of the copper metal layer 105 is removed. It should be appreciated that the repeated wet ALE process illustrated in FIG. 1 is only one example of an etching process that may be used to etch copper in accordance with the present disclosure.
[0046] Wet ALE of copper metal requires the formation of a self-limiting passivation layer on the copper metal surface. This is achieved by exposing the oxidized copper metal surface layer to a first etching solution (i.e., complexing solution 125) that allows or causes a chemical reaction between chemical species in the solution and the oxidized copper metal surface layer. This passivation layer must be insoluble in the solution used for its formation, but appreciably soluble in the second etching solution (i.e., dissolving solution 145) used for its dissolution. The self-limiting passivation layer must be removed after its formation in every cycle. The second etching solution is used to selectively dissolve the passivation layer without etching the underlying unmodified copper metal layer.
[0047] Wet ALE offers numerous advantages over other etching techniques. One advantage of wet ALE is that it can be performed near room temperature and at atmospheric pressure. In addition, the self-limiting nature of the wet ALE process leads to a smoothing of the surface during etching, rather than the roughness typically seen when other etching techniques are used. The wet ALE process described herein for etching copper offers additional advantages as further described herein.
[0048] According to one embodiment, the wet ALE process described herein uses alternating solutions of oxalic acid (C2H2O4) in isopropyl alcohol (IPA) and ammonium hydroxide (NH4OH) in deionized water (DI H2O) to etch a copper (Cu) metal layer. As shown in FIG. 1 and described above, each etching cycle of the wet ALE process may include a complexing step 100, a first purge step 140, a dissolving step 150, and a second purge step 160. In one implementation, each etching cycle of the wet ALE process described herein for etching a copper metal layer may include a 5 second dispense of a complexing solution 125 containing oxalic acid, a 5 second IPA rinse, a 5 second dispense of a dissolving solution 145 containing ammonium hydroxide, and a 5 second IPA rinse. The etching cycle may be repeated at least once until the desired amount of etching of Cu metal is achieved. In some embodiments, the purge time between the complexing and dissolving steps may be reduced to, for example, 3 seconds.
[0049] As described above with reference to FIG. 1, the wet ALE process may generally begin by receiving a substrate having a copper metal layer 105 formed thereon, with an oxidized copper surface layer 115 of the copper metal layer 105 exposed on the substrate surface. The wet ALE process may then expose the substrate surface to a complexing solution 125 comprising a carboxylic acid dissolved in an organic solvent. In one exemplary embodiment, the complexing solution 125 may comprise about 50 mM oxalic acid (C2H2O4) dissolved in isopropyl alcohol (IPA). The oxalic acid in the complexing solution 125 complexes the oxidized copper surface layer 115, which resides on the copper metal layer 105 as copper oxide / hydroxide to form a monolayer of copper oxalate. As shown in FIG. 9 and described in more detail below, this complexing reaction rapidly forms a monolayer of copper oxalate after about 5 seconds. Thus, in one embodiment, the wet ALE process described herein may deliver the complexing solution 125 to the substrate surface for about 5 seconds to ensure that at least one monolayer of copper oxalate is formed on the underlying copper metal layer 105.
[0050] After forming the copper oxalate layer, the substrate is rinsed with IPA for about 5 seconds to remove the complexing solution 125 from the substrate surface before exposing the substrate surface to a diluted aqueous ammonium hydroxide (NH4OH) dissolving solution 145. To ensure that the dissolution of the copper oxalate layer is self-limiting, the NH4OH concentration must be low enough (e.g., less than 10 mM) so as not to etch the underlying copper metal layer 105, but high enough to efficiently dissolve the copper oxalate layer. In one exemplary embodiment, the dissolving solution 145 may include about 5 mM ammonium hydroxide (NH4OH) dissolved in deionized water (DI H2O). After dissolving the copper oxalate layer, the substrate may be rinsed again with IPA for about 5 seconds to remove the dissolving solution 145 from the substrate surface. The etching cycle may then be repeated multiple times until a desired amount of the copper metal layer 105 is removed.
[0051] The etch rate per cycle for patterned substrates / wafers etched using the wet ALE process described herein has been calculated from atomic force microscope (AFM) measurements to correspond to roughly the metal diameter of one copper (Cu) atom, and thus approximately one monolayer of copper is etched per cycle. Furthermore, the repeated wet ALE process described herein can be used to rapidly remove approximately 2-4 nm of copper without increasing the convexity of the etched copper features or adversely affecting the roughness of the dielectric material 110 or the copper metal layer 105 itself. This is illustrated in the graphs presented in Figures 5-7 and described in more detail below.
[0052] The present disclosure contemplates a wide variety of etching chemistries that may be used in the complexing solution 125 and dissolving solution 145 shown in FIG. 1. Exemplary etching chemistries for etching copper using the wet ALE process disclosed herein are detailed below. Mixing these solutions leads to sequential etching processes, loss of etch control, and roughness of the surface after etching, all of which negate the benefits of wet ALE. Therefore, purge steps 140 and 160 are performed in the wet ALE process shown in FIG. 1 to prevent direct contact between the complexing solution 125 and dissolving solution 145 on the substrate surface.
[0053] According to one embodiment of the present disclosure, in the complexing step 100, the oxidized copper surface layer 115 is exposed to a complexing solution 125 of oxalic acid dissolved in IPA to form a copper oxalate layer on the unmodified copper metal layer 105. According to other embodiments, in the complexing step 100, the oxalic acid may be replaced with other carboxylic acids. Any carboxylic acid that reacts with the oxidized copper surface layer 115 to form a corresponding copper carboxylate layer may be used, so long as the carboxylic acid is soluble in the first solvent (e.g., IPA) and the copper carboxylate layer is insoluble in the first solvent. For example, other carboxylic acids such as mandelic acid, malic acid, maleic acid, or fumaric acid may be utilized in the complexing solution 125 to form the corresponding copper carboxylate layer.
[0054] IPA is one example of a first solvent that may be used in the complexing solution 125 because of its widespread use and availability in the semiconductor industry, although many other solvents will work for this process. Examples of other organic solvents that may be used in the complexing solution 125 include diethyl ether ((C2H5)2O), acetonitrile (C2H3N), dimethyl sulfoxide (C2H6OS), as well as various alcohols (e.g., methanol, ethanol, amyl alcohol, and polyols), ketones (e.g., acetone, and methyl ethyl ketone), and acetates. This list is illustrative but not exhaustive. The only requirements for the first solvent are that (a) oxalic acid is soluble in the first solvent, (b) the copper oxalate layer formed during the complexing step 100 is insoluble in the first solvent, and (c) there is no reaction between the first solvent and copper metal.
[0055] According to one embodiment of the present disclosure, the copper oxalate layer (or other copper carboxylate layer) formed during the complexation process 100 is selectively removed by exposing the substrate surface to a dissolution solution 145 of ammonium hydroxide (NH4OH) dissolved in deionized water (DI H2O). According to other embodiments, the ammonium hydroxide may be replaced with another reactant that reacts with the copper oxalate layer (or other copper carboxylate layer) to form a soluble species. For example, a base such as potassium hydroxide (KOH), sodium hydroxide (NaOH), tetramethylammonium hydroxide ((CH3)4NOH), potassium carbonate (K2CO3), ammonium carbonate ((NH4)2CO3), or any other weak base may be used in the dissolution solution 145.
[0056] Deionized water (DI H2O) is one example of an aqueous solvent that may be used in dissolution solution 145, although other solvents may be used. For example, some metal carboxylates are soluble in high purity acetic acid as a solvent. The only requirements for the solvent used in dissolution solution 145 are that (a) the copper oxalate layer (or another copper carboxylate layer) is soluble in the solvent, and (b) the solvent reacts with the copper metal to reoxidize the exposed surface of the copper metal to form a new oxidized copper surface layer 115.
[0057] Mixing the complexing solution 125 containing oxalic acid and the dissolving solution 145 containing ammonium hydroxide leads to sequential etching processes, loss of etching control, and surface roughness. Therefore, to prevent direct contact of the two etching solutions on the copper surface, a solvent rinsing step (i.e., purging steps 140 and 160) is performed between the complexing and dissolving steps. This includes thoroughly rinsing the two solutions from small features that may be formed on the patterned substrate. According to one embodiment of the present disclosure, the substrate surface may be rinsed in IPA. However, other solvents may be used for this purpose. For example, in other embodiments, the substrate surface may instead be rinsed with other alcohols (e.g., methanol, ethanol, or amyl alcohol), acetates (e.g., ethyl acetate, or amyl acetate), acetone, or acetonitrile.
[0058] Etching experiments were performed using the preferred etching chemistry disclosed above on coupons cut from 300 mm silicon wafers containing a copper (Cu) metal layer deposited on one side. The different coupons contain different patterned areas of exposed copper metal. Specifically, the coupons used in the etching experiments include an unpatterned blanket coupon, a first patterned coupon containing 2 μm copper pads with a 3 μm pitch, a second patterned coupon containing 0.5 μm copper pads with a 1 μm pitch, and a third patterned coupon from a fully patterned wafer containing 0.5 μm copper pads with a 1 μm pitch. The etching recipe used to etch the coupons includes multiple wet ALE cycles, each cycle including a 5 second dispense of a complexing solution 125 containing oxalic acid, a 5 second IPA rinse, a 5 second dispense of a dissolving solution 145 containing dilute ammonium hydroxide, and a 5 second IPA rinse.
[0059] The total etch amount (nm) as a function of the number of wet ALE cycles for the different coupons mentioned above is illustrated in the graph 200 shown in FIG. 2. The linear etch amount behavior observed in FIG. 2 is characteristic of ALE and confirmed to be an etch rate of about 0.28 nm / cycle between 2 and 10 cycles, which roughly corresponds to the diameter of one copper atom (0.26 nm) and one monolayer of copper per ALE cycle. These results hold for both larger and smaller pad sizes (2 μm and 0.5 μm) up to 50 ALE cycles. The relatively high etch rate of 0.46 nm / cycle for the fully patterned wafer was confirmed to be due to the short purge time (e.g., 3 seconds) between exposures. Other experimental results using longer purge times (e.g., 5 seconds) resulted in about 0.25 nm / cycle for the fully patterned spinning disk.
[0060] Graph 300 in Figure 3 illustrates the effect of changing the temperature (°C) of the ammonium hydroxide solution on the etch rate (nm / cycle) of copper. As shown in Figure 3, when the etching solution was heated from 25°C to 70°C, the etch rate increased by about 0.004 nm / cycle / °C.
[0061] Further etching experiments were performed on substrates containing copper-filled recessed features in silicon dioxide (SiO2). FIG. 4 is a schematic cross-sectional view of a test sample 400 having a copper-filled recessed feature 405 in a dielectric film 410 (e.g., a SiO2 film such as TEOS) showing the amount of material removed during the etching experiment as well as the convexity of the copper-filled recessed feature 405 formed as a result of the etching. The convexity is the difference in thickness of the copper-filled recessed feature 405 measured at the center and the edge of the feature. As shown in FIG. 4, the etching cycle removed copper metal from the recessed feature, but the amount of copper removed varied from the center to the edge of the recessed feature, resulting in a convex recessed feature.
[0062] 5-7 show experimental results obtained after performing multiple cycles (e.g., 10) of the wet ALE process described herein on a patterned coupon containing 0.5 μm copper pads with a 1 μm pitch. Graph 500 shown in FIG. 5 shows the copper convexity (expressed in nanometers (nm)) achieved as a function of wet ALE cycles. Graph 600 shown in FIG. 6 shows the copper roughness (R q Graph 700 shown in FIG. 7 illustrates the dielectric (e.g., SiO2 film such as TEOS) roughness results achieved as a function of wet ALE cycles. As shown in FIGS. 5-7, the experimental results showed no significant effect on copper convexity (FIG. 5), copper roughness (FIG. 6), and dielectric roughness (FIG. 7) for at least 10 wet ALE cycles. The etching chemistry described herein and used to generate the experimental results did not remove the dielectric film in addition to preventing surface roughness.
[0063] Additional etching experiments were performed to determine the effect of NH4OH concentration in DI H2O on the etch selectivity between the copper oxalate layer and the underlying copper metal layer. During the etching experiments, selective removal of copper oxalate was observed at a NH4OH concentration of 5 mM, and uncontrolled etching of copper was observed at a NH4OH concentration of 50 mM. Further experiments using NH4OH at a concentration of 10 mM showed some pitting of the copper metal layer. Thus, according to one embodiment, the NH4OH concentration can be about 10 mM or less to avoid pitting. The experimental results indicate that NH4OH etches and dissolves the copper oxalate layer, but must be used at a relatively low concentration (e.g., 10 mM or less) to ensure that it does not etch metallic copper or the newly oxidized copper surface layer formed on the copper metal layer during the dissolution process when the copper oxalate layer is removed. This is a necessary condition to maintain the ALE of copper with good control over the etch rate.
[0064] A graph 800 depicting an exemplary amount of material removed (expressed in nm) after five etching cycles as a function of dissolution (e.g., NHOH) immersion time (expressed in seconds) is provided in Figure 8. As shown in Figure 8, for low NHOH concentrations (e.g., 10 mM or less), NHOH immersion times greater than about 5 seconds did not substantially increase the etch rate, indicating that at such low NHOH concentrations, NHOH selectively etches copper oxalate.
[0065] A graph 900 is provided in FIG. 9 depicting an exemplary amount of material removed (expressed in nm) after five etching cycles as a function of complexing solution (e.g., oxalic acid) immersion time (expressed in seconds). As shown in FIG. 9, immersion of at least 5 seconds of complexing solution was required to form a monolayer of oxalic acid on the substrate. If longer immersion times are used, multiple layers of oxalic acid may form on the substrate through hydrogen bonding. This is due to the high ligand packing density of oxalic acid and is shown diagrammatically in FIG. 10. According to one embodiment, as shown in FIG. 10, an IPA rinse step is performed after exposure to oxalic acid to remove any multiple layers of oxalic acid from the substrate surface, such that only a chemisorbed monolayer of oxalic acid is formed on the substrate surface.
[0066] 11A-11B illustrate common challenges encountered in three-dimensional interconnect (3DI) hybrid bonding processes after recessing copper (Cu) metal features into a dielectric layer using conventional etching techniques. More specifically, FIG. 11A illustrates a cross-sectional view 1100 of a copper metal feature 1105 recessed into a dielectric layer 1110 using conventional wet etching techniques. FIG. 11B illustrates a 3DI hybrid bonding process 1120 in which a top wafer 1130 having an etched copper metal surface and a bottom wafer 1140 having an etched copper metal surface are bonded together such that the etched copper metal surfaces face each other. As shown in FIGS. 11A and 11B, conventional etching methods result in a non-ideal etch profile 1115 (e.g., rough, rounded corners) due to poor etch selectivity between the dielectric layer 1110 (e.g., silicon dioxide, SiO2) and the copper metal feature 1105. When two wafers are bonded together using thermal processing, a non-ideal etch profile 1115 results in seams and keyholes 1150 at the bond interface. To avoid these issues, precise removal of approximately 2-5 nm of copper metal is required, where the copper metal removal is selective to the dielectric material (e.g., SiO2) surrounding the copper metal.
[0067] 12A-12B show how the wet ALE process described herein for etching copper metal can be applied to a 3DI hybrid bonding process and utilized to eliminate seams and keyholes in bonded wafers. More specifically, FIG. 12A shows a cross-sectional view 1200 of a copper metal feature 1205 recessed into a dielectric layer 1210 using the wet ALE technique described herein. FIG. 12B shows a 3DI hybrid bonding process 1220 in which a top wafer 1230 having an etched copper metal surface and a bottom wafer 1240 having an etched copper metal surface are bonded together such that the etched copper metal surfaces face each other. In FIG. 12A, a selective copper etching process is used to recess the copper metal feature 1205 downward from the top surface of the dielectric layer 1210. The wet ALE process described above can be used to provide the selective Cu etch shown in FIG. 12A. In Figure 12B, two wafers with recessed copper metal features 1205 are bonded together using a thermal treatment that reflows the copper metal. As shown in Figures 12A-12B, the wet ALE process described herein provides good etch selectivity between the dielectric layer 1210 (e.g., silicon dioxide, SiO2) and the copper metal features 1205, and therefore provides an ideal etch profile 1215 that eliminates seams and keyholes at the bonded interface when the two wafers are bonded together.
[0068] As mentioned above, the wet ALE process described herein allows for the removal of copper metal with atomic layer precision. In one embodiment, the wet ALE process described herein can be used to accurately remove approximately 2-5 nm of copper metal. The accurate removal of 2-5 nm of copper metal allows for the required wafer-to-wafer etch uniformity required for high volume semiconductor manufacturing of bonded interconnects. The wet ALE process described herein also results in precise recess depth and recess depth uniformity of the etched copper metal within the wafer, allowing for the formation of good Cu / Cu contacts using low thermal budgets during the heat treatment portion of the 3DI hybrid bonding process. Other requirements for the 3DI hybrid bonding process include minimal damage to the surface of the dielectric, minimal increase in dielectric surface roughness, and minimal corner rounding of the dielectric to avoid the formation of voids after the wafer bonding process. Additionally, the copper metal removal process used in the bonding process should preferably use corrosion resistant chemistries and minimize contamination of the process chamber with volatile copper-containing reaction products. The wet ALE process described herein for etching copper meets all of these requirements.
[0069] 13A and 13B illustrate a common problem encountered in a fully self-aligned via (FSAV) process. More specifically, FIG. 13A shows a schematic cross-sectional view of an FSAV 1300, where relocation errors between a copper metal feature 1305 (e.g., a copper-filled via) and a copper metal line 1315 result in degradation of the via-to-line distance if a copper metal etch-back process is not performed. FIG. 13B shows a schematic cross-sectional view of an FSAV 1320 where a copper metal feature 1305 in a dielectric layer 1310 has been etched back or recessed using a conventional etching technique, where an etch-stop material 1325 is formed. As shown in FIG. 13B, when a conventional etching technique is utilized, the etch-stop material 1325 is present at the line edges due to the high convexity of the etched copper metal feature 1305.
[0070] FIG. 13C illustrates how the wet ALE process described herein for etching copper can be applied to a fully self-aligned via (FSAV) process. More specifically, FIG. 13C illustrates a schematic cross-sectional view of an FSAV 1330 with an ideal via-line distance and surface profile after etching back or recessing a copper metal feature 1305 in a dielectric layer 1310 using a selective copper etching process according to an embodiment of the present disclosure. The wet ALE process described above can be used to provide the selective copper etching process shown in FIG. 13C for recessing the copper metal feature 1305 so that it is below the top surface of the dielectric layer 1310. In one embodiment, approximately 7-10 nm of copper metal can be accurately removed using the wet ALE process described herein, and such removal is selective to low-k dielectrics. This recessing (as shown in FIG. 13A) is necessary to reduce the effects of relocation errors and allows for the patterning of large vias. As mentioned above, the selective copper etch process described herein minimizes damage to the roughness and topography of the dielectric or copper surfaces, avoids corner rounding of the dielectric material (which can reduce the distance between copper metal lines), and avoids increased convexity of the copper surface (which can lead to subsequent etch non-uniformity and reliability concerns).
[0071] The wet ALE process described herein for etching copper can be accomplished using a variety of techniques. For example, the wet ALE process disclosed above may be performed by immersing a substrate having copper metal features formed thereon into a beaker of the respective etching solution. In this case, purging can be accomplished by either rinsing or immersing the substrate in an appropriate solvent bath. The wet ALE process disclosed above can also be performed in a wide variety of semiconductor processing systems. Although the wet ALE process can be accomplished using many different process chambers, tools, and equipment, the processing equipment used to perform the wet ALE process is preferably capable of operating at (or near) room temperature and at (or near) atmospheric pressure.
[0072] In one implementation, the wet ALE process described herein may be performed in a spin chamber. When a spin chamber is utilized, the etching solution is dispensed from a nozzle positioned above the substrate and dispersed by the rotational motion of the spin chuck on which the substrate is placed. After a set exposure time, the nozzle begins to dispense the next solution in the etching recipe. This process continues throughout the etching cycle, repeated as many cycles as necessary to remove the desired amount of metal. For high volume manufacturing, the dispensing of the etching solution and rinse can be performed using conventional tools, such as wet etching and rinsing tools.
[0073] FIG. 14 illustrates one embodiment of a processing system 1400 that may etch a copper metal layer on a surface of a substrate 1430 using the hybrid ALE technique described herein. As shown in FIG. 14, the processing system 1400 includes a process chamber 1410, which may be a pressure-controlled chamber in some embodiments. In the embodiment shown in FIG. 14, the process chamber 1410 is a spin chamber having a spinner 1420 (or spin chuck) configured to spin or rotate at a constant rotational speed. A substrate 1430 is held on the spinner 1420, for example, by electrostatic forces or vacuum pressure. In one example, the substrate 1430 may be a semiconductor wafer with a copper metal layer formed on or in the substrate 1430.
[0074] The processing system 1400 shown in FIG. 14 further includes a liquid nozzle 1440 disposed above the substrate 1430 for dispensing various etching solutions 1442 onto the substrate surface 1430. The etching solutions 1442 dispensed onto the surface of the substrate 1430 may generally include a complexing solution including a complexing agent (e.g., a carboxylic acid-based ligand) that bonds to the oxidized copper metal surface layer to form a ligand-metal complex (e.g., a copper carboxylate layer), and a dissolving solution that selectively removes the ligand-metal complex. A purge solution may also be dispensed onto the surface of the substrate 1430 between the complexing and dissolving steps to separate the complexing and dissolving solutions. Examples of complexing, dissolving, and purge solutions are described above.
[0075] 14, the etching solutions 1442 may be stored in a chemical supply system 1446, which may include one or more reservoirs for holding various etching solutions 1442 and a chemical injection manifold fluidly coupled to the process chamber 1410 via liquid supply lines 1444. In operation, the chemical supply system 1446 may selectively apply a desired chemical to the process chamber 1410 via the liquid supply lines 1444 and liquid nozzles 1440 disposed in the process chamber 1410. Thus, the chemical supply system 1446 may be used to distribute the etching solution 1442 onto the surface of the substrate 1430. The process chamber 1410 may further include a drain 1450 for removing the etching solution 1442 from the process chamber 1410.
[0076] The components of the processing system 1400 may be coupled to or controlled by a controller 1460, which may in turn be coupled to a corresponding memory storage unit and a user interface (not shown). Various processing operations may be performed via the user interface, and various processing recipes and operations may be stored in the memory storage unit. Thus, a given substrate 1430 may be processed in the process chamber 1410 according to a particular recipe. In some embodiments, a given substrate 1430 may be processed in the process chamber 1410 according to an etch recipe that utilizes the wet ALE techniques described herein for etching copper.
[0077] The controller 1460, shown in block diagram form in FIG. 14, can be implemented in a wide variety of ways. In one example, the controller 1460 can be a computer. In another example, the controller 1460 can include one or more programmable integrated circuits programmed to provide the functionality described herein. For example, one or more processors (e.g., microprocessors, microcontrollers, central processing units, etc.), programmable logic devices (e.g., complex programmable logic devices (CPLDs), field programmable gate arrays (FPGAs), etc.), and / or other programmable integrated circuits can be programmed with software or other programming instructions to achieve the functionality of a prescribed plasma process recipe. It is further noted that the software or other programming instructions can be stored in one or more non-transitory computer-readable media (e.g., memory storage devices, flash memory, dynamic random access memory (DRAM), reprogrammable storage devices, hard drives, floppy disks, DVDs, CD-ROMs, etc.) and that the software or other programming instructions, when executed by the programmable integrated circuit, cause the programmable integrated circuit to perform the processes, functions, and / or capabilities described herein. Other variations can also be implemented.
[0078] 14, a controller 1460 may be coupled to various components of the processing system 1400 to receive inputs from and provide outputs to the components. For example, the controller 1460 may be coupled to the process chamber 1410 to control the temperature and / or pressure therein, the spinner 1420 to control the rotational speed of the spinner 1420, and the chemical delivery system 1446 to control the various etching solutions 1442 that are dispensed onto the substrate 1430. The controller 1460 may control other processing system components not shown in FIG. 14, as known in the art.
[0079] In some embodiments, the controller 1460 may control various components of the processing system 1400 according to an etch recipe that utilizes the wet ALE techniques described herein for etching copper. For example, the controller 1460 may provide various control signals to the chemical delivery system 1446, which in turn cause the chemical delivery system 1446 to a) dispense a complexing solution onto the surface of the oxidized substrate 1430 to bind a complexing agent to the oxidized copper surface layer and form a complexed oxidized copper surface layer (e.g., a ligand-metal complex) on the copper metal layer, b) rinse the surface of the substrate 1430 with a first purge solution to remove the complexing solution 125 and any excess reactants from the surface of the substrate 1430, c) dispense a dissolving solution onto the surface of the substrate 1430 to selectively remove or dissolve the complexed oxidized copper surface layer from the copper metal layer and form a new oxidized copper surface layer on the copper metal layer, and d) rinse the substrate with a second purge solution to remove the dissolving solution from the surface of the substrate 1430. In some embodiments, the controller 1460 may provide control signals to the chemical delivery system 1446 in a cyclical manner such that steps a)-d) are repeated for one or more ALE cycles until a desired amount of copper metal is removed.
[0080] In some embodiments, the controller 1460 may control the temperature and / or pressure in the process chamber 1410. In some embodiments, the complexing, dissolving, and purging steps of the wet ALE processes described herein may be performed at approximately the same temperature and pressure. In one implementation, the complexing, dissolving, and purging steps may be performed at (or near) atmospheric pressure and room temperature, respectively. Performing the processing steps in the same process chamber at approximately the same temperature and pressure reduces cycle time and improves throughput of the wet ALE processes described herein by avoiding unnecessary chamber transitions and temperature / pressure changes.
[0081] However, it should be noted that the embodiments described herein are not strictly limited to only atmospheric pressure and room temperature, nor are they limited to any particular process chamber. In other embodiments, one or more of the complexing, dissolving, and purging steps described herein may be performed above atmospheric pressure as described above in a pressure vessel or at reduced pressure in a vacuum chamber. The etching solution may be dispensed in these environments as long as the vapor pressure of the liquid is lower than the chamber pressure. In these implementations, a spinner having a liquid dispensing nozzle is disposed in the pressure vessel or vacuum chamber. The temperature of the dispensed liquid may be raised to any temperature below the boiling point at the pressure of the process. In one implementation, the dissolving step may be performed at a temperature between 25° C. and 70° C. as shown in FIG. 3. Higher liquid temperatures may be used to increase the etch rate, as shown.
[0082] 15-16 illustrate an exemplary method utilizing the novel etching chemistries described herein for etching copper in a wet ALE process. It will be understood that the embodiments of FIGS. 15-16 are merely exemplary and that additional methods may utilize the techniques described herein. Additionally, additional steps may be added to the methods illustrated in FIGS. 15-16 as the process steps described are not intended to be exclusive. Additionally, the order of steps is not limited to the order shown in the figures as different orders may occur and / or various steps may be combined or performed simultaneously.
[0083] FIG. 15 illustrates one embodiment of a method 1500 of etching. The method 1500 illustrated in FIG. 15 may generally begin by receiving (at step 1510) a substrate having a copper metal layer formed thereon, with an oxidized copper surface layer of the copper metal layer exposed on the substrate surface. The method 1500 may then include exposing (at step 1520) the substrate surface to a complexing solution including a carboxylic acid dissolved in an organic solvent. The carboxylic acid may react with the oxidized copper surface layer to form a carboxylate copper layer, which is insoluble in the organic solvent. The method 1500 may then include removing the complexing solution from the substrate surface following the formation of the carboxylate copper layer (at step 1530) and exposing (at step 1540) the substrate surface to a dissolving solution to selectively remove the carboxylate copper layer to expose the copper metal layer underlying the carboxylate copper layer. The dissolving solution may generally include a reactant and an aqueous solvent. The reactant may react with the carboxylate copper layer to form a soluble species that is dissolved by the aqueous solvent. Method 1500 may then include removing (at 1550) the dissolving solution and soluble species from the substrate surface to etch the copper metal layer. In some embodiments, method 1500 may further include repeating the steps of exposing the substrate surface to the complexing solution, removing the complexing solution, exposing the substrate surface to the dissolving solution, and removing the dissolving solution for multiple cycles until a predetermined amount of copper metal is removed from the substrate.
[0084] Figure 16 illustrates one embodiment of a method 1600 that may be used to etch copper using a wet atomic layer etching (ALE) process. The method 1600 illustrated in Figure 16 generally includes a) receiving (at step 1610) a substrate having a copper (Cu) metal layer having an oxidized Cu surface layer formed thereon, b) exposing (at step 1620) the oxidized Cu surface layer to a complexing solution containing a complexing agent to bond the complexing agent to the oxidized Cu surface layer and form a complexed oxidized Cu surface layer on the Cu metal layer, and c) rinsing (at step 1630) the substrate with a first purge solution to remove the complexing agent from the surface of the substrate. removing the solution; d) selectively removing (at 1640) the complexed oxidized Cu surface layer from the Cu metal layer by exposing the complexed oxidized Cu surface layer to a dissolving solution that dissolves the complexed oxidized Cu surface layer and forms a new oxidized Cu surface layer on the Cu metal layer; and e) (at 1650) rinsing the substrate with a second purge solution to remove the dissolving solution from the surface of the substrate and to etch the Cu metal layer. In one embodiment, the method may further include repeating steps b)-e) at least once to further etch the Cu metal layer. In one example, the complexing agent may include oxalic acid and the dissolving solution may include ammonium hydroxide dissolved in an aqueous solvent.
[0085] It should be noted that references throughout this specification to "one embodiment" or "one embodiment" mean that a particular feature, structure, material, or characteristic described in connection with this embodiment is included in at least one embodiment of the invention, but do not mean that it is present in all embodiments. Thus, the appearance of "in one embodiment" or "in one embodiment" in various places throughout this specification does not necessarily refer to the same embodiment of the invention. Moreover, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments. In other embodiments, various additional layers and / or structures may be included and / or described features may be omitted.
[0086] As used herein, the term "substrate" refers to and includes a base material or structure on which a material is formed. It will be understood that a substrate may include a single material, multiple layers of different materials, one or more layers having regions of different materials or structures therein. These materials may include semiconductors, insulators, conductors, or combinations thereof. For example, the substrate may be a semiconductor substrate, a base semiconductor layer on a supporting structure, a metal electrode, or a semiconductor substrate having one or more layers, structures, or regions formed thereon. The substrate may be a conventional silicon substrate or other bulk substrate including a layer of semiconducting material. As used herein, the term "bulk substrate" refers to and includes silicon wafers, as well as silicon-on-insulator ("SOI") substrates such as silicon-on-sapphire ("SOS") substrates and silicon-on-glass ("SOG") substrates, epitaxial layers of silicon on a base semiconductor substrate, and other semiconductor or optoelectronic materials such as silicon germanium, germanium, gallium arsenide, gallium nitride, and indium phosphide. The substrate may be doped or undoped.
[0087] Systems and methods for processing a substrate are described in various embodiments. The substrate may include any material portion or structure of a device, particularly a semiconductor or other electronic device, and may be, for example, a base substrate structure, such as a semiconductor substrate, or a layer on or overlying the base substrate structure, such as a thin film. Thus, the substrate is not intended to be limited to any particular base structure, underlying layer, or overlying layer, patterned or unpatterned, but rather is intended to include any such layer or base structure, and any combination of layers and / or base structures.
[0088] Those skilled in the art will understand that the various embodiments may be practiced without one or more of the specific details, or with other alternative and / or additional methods, materials, or components. In other instances, well-known structural, material, or operational details have not been shown or described to avoid obscuring aspects of the various embodiments of the invention. Similarly, for purposes of explanation, specific numbers, materials, and configurations have been set forth to provide a thorough understanding of the invention. Nevertheless, the invention may be practiced without the specific details. Furthermore, it should be understood that the various embodiments shown in the figures are illustrative representations and are not necessarily drawn to scale.
[0089] Further modifications and alternative embodiments of the described system and method will be apparent to those skilled in the art upon review of this specification. It will therefore be understood that the described system and method are not limited by these exemplary configurations. It should be understood that the forms of the system and method shown and described herein should be construed as exemplary embodiments. Various modifications may be made in the implementation. Thus, while the wet ALE technique for etching copper is described herein with reference to specific embodiments, various modifications and changes can be made without departing from the scope of the disclosure. Thus, the specification and drawings should be regarded in an illustrative rather than a restrictive sense, and such modifications are intended to be included within the scope of the disclosure. Moreover, any benefits, advantages, or solutions to problems described herein with respect to specific embodiments are not intended to be construed as any or all of the essential, necessary, or essential features or elements of the claims.
Claims
1. 1. A method of etching, the method comprising: receiving a substrate having a copper metal layer formed thereon, the substrate having an oxidized copper surface layer of the copper metal layer exposed on a surface thereof; exposing the surface of the substrate to a complexing solution comprising a carboxylic acid dissolved in an organic solvent, the carboxylic acid reacting with the oxidized copper surface layer to form a copper carboxylate layer, the copper carboxylate layer being insoluble in the organic solvent; following formation of the copper carboxylate layer, removing the complexing solution from the surface of the substrate; exposing the surface of the substrate to a dissolution solution to selectively remove the copper carboxylate layer and expose the copper metal layer underlying the copper carboxylate layer, the dissolution solution comprising a reactant and an aqueous solvent, the reactant reacting with the copper carboxylate layer to form a soluble species that is dissolved by the aqueous solvent; removing the dissolving solution and the soluble species from the surface of the substrate and etching the copper metal layer; The method comprising:
2. moreover, exposing the surface of the substrate to the complexing solution; removing the complexing solution; exposing the surface of the substrate to the dissolving solution; repeating the step of removing the dissolving solution for multiple cycles until a predetermined amount of the copper metal layer is removed from the substrate; 2. The method of claim 1, comprising:
3. 2. The method of claim 1, wherein the carboxylic acid is oxalic acid, mandelic acid, malic acid, maleic acid, or fumaric acid.
4. The organic solvent is isopropyl alcohol (IPA) or another alcohol, diethyl ether (C 2 H 5 ) 2 O), acetonitrile (C 2 H 3 N), dimethyl sulfoxide (C 2 H 6 2. The method of claim 1, wherein the aryloxy group is a ketone, an acetate, or an aryloxy group.
5. the carboxylic acid is oxalic acid, the organic solvent is isopropyl alcohol (IPA), and the oxalic acid reacts with the oxidized copper surface layer to form a copper oxalate layer; 2. The method of claim 1, wherein the copper oxalate layer is insoluble in IPA but soluble in the aqueous solvent contained in the dissolution solution.
6. 2. The method of claim 1, wherein exposing the surface of the substrate to the complexing solution comprises providing the complexing solution to the surface of the substrate for a period of time necessary to form at least one monolayer of the copper carboxylate layer on the underlying copper metal layer.
7. 7. The method of claim 6, wherein the carboxylic acid is oxalic acid, and the complexing solution is applied to the surface of the substrate for at least 5 seconds to form at least one monolayer of copper oxalate on the underlying copper metal layer.
8. The method of claim 1 , wherein the reactant in the dissolution solution is a base.
9. The reactant in the solution is ammonium hydroxide (NH 4 3. The method of claim 1 , wherein
10. 10. The method of claim 1, wherein after selectively removing the carboxylate copper layer and exposing the underlying copper metal layer, the dissolving solution re-oxidizes the exposed surface of the underlying copper metal layer to form a new oxidized copper surface layer.
11. The method of claim 10 , wherein the dissolving solution does not etch the underlying copper metal layer or the newly oxidized copper surface layer.
12. The dissolution solution is aqueous ammonium hydroxide (NH 4 OH), 11. The method of claim 10, wherein after the step of selectively removing the copper carboxylate layer, the concentration of the ammonium hydroxide in the dissolving solution is maintained below a level that would etch the underlying copper metal layer or the newly oxidized copper surface layer.
13. 2. The method of claim 1 , wherein removing the complexing solution and removing the dissolving solution each comprise rinsing the surface of the substrate with a purge solution to remove excess reactants from the surface of the substrate, and preventing the complexing solution and the dissolving solution from mixing.
14. 1. A method for etching copper using a wet atomic layer etching (ALE) process, the method comprising: a) receiving a substrate having a copper (Cu) metal layer thereon having an oxidized Cu surface layer formed thereon; b) exposing the oxidized Cu surface layer to a complexing solution containing a complexing agent to bind the complexing agent to the oxidized Cu surface layer and form an oxidized Cu surface layer complexed to the Cu metal layer; c) rinsing the substrate with a first purge solution to remove the complexing solution from the surface of the substrate; d) selectively removing the complex-bonded oxidized Cu surface layer from the Cu metal layer by exposing the complex-bonded oxidized Cu surface layer to a dissolving solution, the dissolving solution dissolves the complex-bonded oxidized Cu surface layer and forms a new oxidized Cu surface layer on the Cu metal layer; e) rinsing the substrate with a second purge solution to remove the dissolving solution from the surface of the substrate and to etch the Cu metal layer; The method comprising:
15. The method of claim 14 , wherein steps a) and b) have no overlap in time.
16. 15. The method of claim 14, further comprising repeating steps b) through e) at least once to further etch the Cu metal layer.
17. The dissolution solution is aqueous ammonium hydroxide (NH 4 15. The method of claim 14 comprising:
18. The method of claim 14 , wherein the dissolving solution does not etch the Cu metal layer or the newly oxidized Cu surface layer.
19. The dissolving solution is ammonium hydroxide (NH 4 OH), 20. The method of claim 18, wherein after the step of selectively removing the complexed oxidized Cu surface layer, the concentration of the ammonium hydroxide in the dissolution solution is maintained below a level that would etch the Cu metal layer or the newly oxidized Cu surface layer.
20. The method of claim 14 , wherein the complexing agent is dissolved in an organic solvent.
21. 15. The method of claim 14, wherein the complexing agent comprises oxalic acid dissolved in isopropyl alcohol (IPA).
22. The method of claim 14, wherein the substrate further comprises an exposed dielectric layer, the dielectric layer not being etched by steps b) through e).
Citation Information
Patent Citations
Preparation of copper surface for improving bonding, composition used therein and product manufactured thereof
JP1999261215A
Method of manufacturing semiconductor device and apparatus for manufacturing the semiconductor device
JP2009004807A
Substrate processing device, substrate processing method, and chemicals
JP2021118351A