Quantum dot integrated plate, its manufacturing method and display device including same
The quantum dot integrated board optimizes refractive index and structure to enhance light utilization and reduce blue light output, addressing stability and cost issues in quantum dot optical plates, thereby improving brightness and reducing assembly costs across different display devices.
Patent Information
- Application Number
- JP2024515870
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-09
- Filing Date
- 2022-11-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-07
AI Technical Summary
Existing quantum dot optical plates face challenges with low stability due to factors like water, oxygen, and heat, and require complex combinations of materials and high costs for light conversion films, with limited utilization of blue light and high assembly costs.
A quantum dot integrated board with specific refractive index layers and fine structure patterns, including red and green quantum dot layers, enhances light utilization and reduces blue light output by optimizing the refractive index and structure design.
Improves brightness and reduces blue light output, eliminating the need for additional films, lowering costs, and increasing the application range of quantum dots in various display devices.
Smart Images

Figure 2024539541000001_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to China Patent Application No. 2021113169728, entitled "Quantum dot integrated plate, its manufacturing method, and display device including the same," filed with the China National Intellectual Property Administration on November 9, 2021. [Technical field]
[0002] The present application relates to the technical field of quantum dot optical plates, and in particular to a quantum dot integrated plate, a manufacturing method thereof, and a display device including the same. [Background technology]
[0003] Quantum dot materials have the characteristics of wide excitation spectrum, narrow emission spectrum, high color purity, and high light stability, so they are used in the field of display, effectively improving the color gamut of the device, making the display effect of the device more vivid and vivid. The quantum dot integrated plate can effectively apply the excellent optical performance of quantum dot materials to the traditional backlight display system, and can make the quantum dot high color gamut display technology cheaper and more popular. However, in the application process, the quantum dots are simultaneously affected by elements such as water, oxygen, and heat, so the stability of the quantum dots is low. At the same time, the difference in the backlight of different liquid crystal display devices (the display devices of TVs and computer displays commonly used in the market are mainly direct type and edge-light type, while devices such as notebook computers, Pads, and mobile phones mainly use edge-light type display devices) creates different demands for quantum dot devices.
[0004] However, the conventional technology has at least the following disadvantages: (1) a complex combination of optical board materials, optical films, and backlight light sources is required to realize the backlight light source required for a television; (2) the light emitted by the green quantum dots is absorbed by the red quantum dots, affecting the luminous efficiency of the quantum dot board material, thereby limiting the utilization rate of the quantum dot material for blue light; and (3) the assembly costs and film costs are high, resulting in high costs of using the quantum dot light conversion film.
[0005] CN111393578A discloses a wide color gamut composite film including a brightness enhancing layer and a diffusion layer. The brightness enhancing layer includes two parts, one is a brightness enhancing substrate layer, which is generally made of PET, and the other is a square prism structure that is closely arranged on the brightness enhancing substrate layer and has an isosceles trapezoidal cross section. The square prism is made of the high refractive index quantum dot UV resin, and the lower end surface of the square prism with a large area is connected to the brightness enhancing substrate layer, and the upper end surface parallel to the brightness enhancing substrate layer is connected to the bottom surface of the diffusion layer. This patent application improves the refractive index of the resin itself by adding a sulfur-containing acrylate monomer, and improves the compatibility of the high refractive index UV resin with the quantum dots and the stability of the quantum dots by utilizing the coordination between the sulfur element and the metal atom on the surface of the quantum dots. The high refractive index UV resin is used to manufacture a brightness enhancing structure of an oblique square prism containing quantum dots, thereby achieving both the functions of brightness improvement and color gamut improvement. In addition, the side of the square pillar is connected to the bottom of the diffusion film, which leads to higher adhesion, more integrated functions, and a thinner, lighter composite film with lower cost.
[0006] CN111650678A discloses a high brightness quantum dot film including a lower substrate, a first structure layer, a second structure layer and an upper substrate arranged in order from bottom to top, the upper end surface of the first structure layer and the lower end surface of the second structure layer are triangular prisms arranged in order, the first structure layer and the second structure layer are doped with two different color quantum dot materials, red and green, with a weight ratio of 1:1, respectively, and the refractive index of the first structure layer is greater than that of the second structure layer. By designing the prism structure and matching the refractive index difference between the two fine structure layers, the quantum dot film manufactured using the invention of this patent application can have an optical light collecting effect, and when used with a blue light LED backlight module, it can improve the color saturation and brightness of the LCD screen, and can achieve the purpose of wide color gamut and energy saving.
[0007] CN108303819A discloses a backlight and a manufacturing method thereof, a light guide plate and a manufacturing method thereof, and a display device, specifically, the refractive index t0 of the transparent adhesive satisfies t1≦t0≦t2, where t1 is the refractive index of the light guide plate, and t2 is the refractive index of the optical film layer. By filling a transparent adhesive between the optical film layer and the light guide plate body and ensuring that the refractive index of the transparent adhesive is equal to or greater than the refractive index of the light guide plate and equal to or less than the refractive index of the optical film layer, the light ray is always transmitted from an optically sparse medium to an optically dense medium during the process of entering the optical film layer from the light guide plate, which can effectively prevent a part of the light ray from being totally reflected during the transmission process, and improve the utilization rate of the light ray.
[0008] The above-mentioned prior art combines the characteristics of the wide color gamut output of quantum dot film and is partially related to the design of the propagation path of light through each layer structure, but it is desired to further improve the light utilization rate and blue light blocking effect. Summary of the Invention [Problem to be solved by the invention]
[0009] In order to overcome the drawbacks of the prior art that it is desirable to further improve the brightness and blue light blocking effect of quantum dot optical plates, the present application aims to provide a quantum dot integrated plate that can improve brightness while reducing blue light output and has a wide range of applications, a manufacturing method thereof, and a display device including the same. [Means for solving the problem]
[0010] In order to achieve the above object, a first aspect of the present invention includes a first optical transition layer, a first quantum dot layer, a second optical transition layer, and a second quantum dot layer, which are provided in this order, and the refractive indexes of the layers are t 第1光遷移層 <t 第1量子ドット層 , t 第2光遷移層 <t 第1量子ドット層 , t 第2光遷移層 <t 第2量子ドット層a first microstructure pattern is provided on a side of the first quantum dot layer adjacent to the second optical transition layer, and a second microstructure pattern is provided on a side of the second quantum dot layer away from the second optical transition layer, the first quantum dot layer containing a red quantum dot material, and the second quantum dot layer containing a green quantum dot material.
[0011] Preferably, the outer surface of the first microstructured pattern and the outer surface of the second microstructured pattern are each independently plate-shaped, arc-shaped, or a combination of both.
[0012] Preferably, the first fine structure pattern and the second fine structure pattern each independently include a vertex, and the angle of the vertex is within a range of 45° to 135°.
[0013] Preferably, the first microstructure pattern and the second microstructure pattern each have a plurality of repeating units, and each repeating unit independently satisfies the maximum width of 10 to 100 μm and the maximum height of 2 to 120 μm.
[0014] More preferably, the repeating unit of the first microstructure pattern and / or the second microstructure pattern satisfies the maximum width of 50 μm and the maximum height of 25 μm.
[0015] Preferably, the first microstructure pattern and the second microstructure pattern are each independently a prismatic structure.
[0016] Preferably, in the vertical propagation direction of a light beam, the included angle between the first microstructure pattern and the second microstructure pattern is 0 to 180°, preferably, the included angle is 45 to 135°, and most preferably, the included angle is 90°.
[0017] Preferably, the quantum dot integrating plate further includes a resin powder provided in the first optical transition layer.
[0018] Preferably, the content of the resin powder in the first optical transition layer is 1 to 50 wt %.
[0019] Preferably, the material of the resin powder is the same as the base material of the first quantum dot layer.
[0020] Preferably, the resin powder has an average particle size of 1 to 100 μm.
[0021] Preferably, the thickness of the first optical transition layer and the second optical transition layer is independently 10 to 500 μm, preferably 10 to 200 μm, and the thickness of the first quantum dot layer and the second quantum dot layer is independently 0.05 to 1.5 mm.
[0022] A second aspect of the present application is A step (1) of producing a first quantum dot sheet and a second quantum dot sheet; (2) forming a first microstructure pattern and a second microstructure pattern on one side of the first quantum dot sheet and one side of the second quantum dot sheet, respectively; Step (3): measuring the refractive index of the first quantum dot sheet and the second quantum dot sheet, selecting a photocurable adhesive or a pressure-sensitive adhesive to form a first optical transition layer and a second optical transition layer, and applying the photocurable adhesive or the pressure-sensitive adhesive to the other side of the first quantum dot sheet and the other side of the second quantum dot sheet, respectively; and (4) joining a side of the first quantum dot sheet on which a first microstructure pattern is formed and a side of the second quantum dot sheet on which a photocurable adhesive or a pressure-sensitive adhesive is applied to form a quantum dot integrated plate in which the refraction of light is variable.
[0023] Preferably, in step (1), the production of the first quantum dot sheet and the second quantum dot sheet each independently includes a step of mixing a quantum dot solution with a polymer material, followed by molding.
[0024] Preferably, in step (2), the first microstructure pattern and the second microstructure pattern are formed by pressing with a microstructure roller.
[0025] Preferably, the method further comprises the step of introducing a resin powder into the photocurable adhesive or pressure-sensitive adhesive applied to the first quantum dot sheet in step (3).
[0026] A third aspect of the present application provides a display device including the quantum dot integrated plate according to the first aspect.
[0027] Preferably, the display device comprises: a panel provided on the outer side of the second quantum dot layer of the quantum dot assembly plate; The quantum dot integrated plate further includes a diffusion plate or a light guide plate provided on a side of the quantum dot integrated plate away from the panel.
[0028] Preferably, when the display device is in a direct backlight mode, the thicknesses of the first quantum dot layer and the second quantum dot layer in the quantum dot integrated plate are each independently 0.5 to 1.5 mm, and when the display device is in an edge-light backlight mode, the thicknesses of the first quantum dot layer and the second quantum dot layer in the quantum dot integrated plate are each independently 0.05 to 0.5 mm. Effect of the Invention
[0029] According to the above-mentioned structural design, the present application provides an optical transition layer and designs the refractive index of each layer in the order of "small, large, small, large", thereby making better use of the fine structure of the quantum dot layer, improving or decreasing the probability of light refraction and reflection, thereby improving the utilization rate of light, improving the utilization rate of red and green quantum dot materials for blue light, improving the brightness value of the quantum dot board material, and reducing the output of blue light. Because of the sufficiently high brightness value, when a display device is constructed using the quantum dot integrated board of the present application, there is no need to use the diffusion film and brightness enhancement film in the construction of the conventional display device, and the cost of optical films and assembly costs can be significantly reduced.
[0030] The manufacturing method of the present application has high adaptability and simple process, and can manufacture quantum dot integrated plates with different thicknesses according to different display devices, thereby increasing the application range of quantum dots. The quantum dot integrated plates can be used in edge-lit display devices and direct-lit display devices, and the device terminals can be widely used in various terminals such as televisions, computer displays, notebook computers, pads, mobile phones, etc. [Brief description of the drawings]
[0031] [Figure 1] FIG. 2 is a front view of a specific embodiment of a quantum dot integrated plate according to the present application. [Diagram 2] FIG. 2 is a side view of FIG. [Diagram 3] 1 is a schematic diagram of light refraction in a microstructure pattern provided on a quantum dot integrated plate according to the present application. [Figure 4] 1 is a direct-type display device according to the present application. [Diagram 5] 1 is an edge-light type display device according to the present application. [Explanation of symbols]
[0032] 1-1st optical transition layer 2- First quantum dot layer 3-Second optical transition layer 4- Second quantum dot layer 5-Resin Powder A-Quantum dot integrated board 6-Panel 7-Diffuser 8-Light guide plate DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The range endpoints and any values disclosed herein are not limited to the exact ranges or values, and should be understood to include values close to these ranges or values. For numerical ranges, values between the endpoints of the ranges, between the endpoints of the ranges and the individual point values, and the individual point values can be combined with each other to form one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0034] As described above, the first aspect of the present application provides a quantum dot integrated plate, which includes a first optical transition layer 1, a first quantum dot layer 2, a second optical transition layer 3, and a second quantum dot layer 4, which are arranged in this order, as shown in FIG. 1 and FIG. 2. The refractive index of each layer is t 第1光遷移層 <t 第1量子ドット層 , t 第2光遷移層 <t 第1量子ドット層 , t 第2光遷移層 <t 第2量子ドット層 a first microstructure pattern is provided on a side of the first quantum dot layer 2 close to the second optical transition layer 3, and a second microstructure pattern is provided on a side of the second quantum dot layer 4 away from the second optical transition layer 3, the first quantum dot layer 2 contains a red quantum dot material, and the second quantum dot layer 4 contains a green quantum dot material.
[0035] In the course of research, the applicant of the present application discovered that by designing the structure of each of the above-mentioned layers of the present application, in particular by designing the refractive index of each layer in the order of "small, large, small, large" ("small" or "large" both refer to the adjacent layer), in accordance with the microstructure pattern provided corresponding to the quantum dot layer containing red and green quantum dot materials, the characteristics of the brightness enhancement structure and the quantum dot material can be fully exhibited. Specifically, the first quantum dot layer 2 can fully exert the light-collecting effect according to the first microstructure pattern provided thereon; and the transmission of the light from the first quantum dot layer 2 to the second optical transition layer 1 means that the light goes from an optically dense medium to an optically sparse medium, so that some of the light is repeatedly reflected within the first quantum dot layer 2, and the utilization rate of the light can be increased; at the same time, the transmission of the light from the first optical transition layer 1 to the first quantum dot layer 2 and the transmission from the second optical transition layer 3 to the second quantum dot layer 4 means that the light goes from an optically sparse medium to an optically dense medium, so that the light reflection phenomenon is reduced, the amount of light entering the quantum dot layer is increased, and the light loss is reduced; and due to this rule of change in the refractive index, the brightness of the quantum dot integrated plate is significantly improved.
[0036] Meanwhile, in a quantum dot diffuser plate generally containing a mixture of red and green quantum dots, blue light excites the red and green quantum dots at the same time, and red and green light are emitted. However, the green light of the quantum dots is absorbed by the red quantum dots and used to excite the red quantum dot material, so the performance of the green quantum dots cannot be maximized. Therefore, more green quantum dots and blue light must be used to achieve the same effect. At the same time, in the prior art, blue light generally passes directly through the quantum dot diffuser plate, and there is no reuse process of blue light in the first and second quantum dot sheets, so the utilization rate of blue light is low and a lot of blue light passes through the quantum dot diffuser plate. In the quantum dot integrated plate of the present application, the blue light first passes through the first quantum dot sheet containing red quantum dots, and its propagation path goes from an optically dense medium to an optically sparse medium, so that some of the blue light is repeatedly reflected in the first quantum dot sheet, and the blue light can fully excite the red quantum dots. When blue light and red light enter the second quantum dot sheet containing green quantum dots, some of the blue light and red light are repeatedly reflected within the second quantum dot sheet, and the red light does not excite the green quantum dots, so the blue light can fully excite the green quantum dots, thereby maximizing the performance of the green quantum dots, improving the utilization rate of blue light, and significantly reducing the output of blue light.
[0037] In the present application, the red quantum dot material and the green quantum dot material are both conventional quantum dot materials, which may be commercially available or may be prepared by conventional methods, and thus the description thereof is omitted here.
[0038] In this application, the "optical transition layer" may be understood to be a gradation transition layer in which the refractive index of light changes, and its function is, on the one hand, to increase the transmittance of light and reduce the light reflection phenomenon caused by the refractive index difference at the bonding point of the side of the quantum dot layer, and, on the other hand, to increase the angle change of the light in the optical transition layer and to play a certain diffusion and atomization effect on the light.
[0039] The present application does not specifically limit the materials of the first optical transition layer 1 and the second optical transition layer 3, as long as they satisfy the above-mentioned specific refractive index and are applicable to the optical plate. Non-limiting examples of the substrate of the optical transition layer may be selected from PMMA, PET, PC, MS, PP, PS, and PE.
[0040] In the present application, the specific selection of the refractive index of each layer may be made so long as it satisfies the above-mentioned refractive index rules and is advantageous for improving brightness and reducing blue light output. For example, it is preferable that the refractive indexes of the first quantum dot layer 2 and the second quantum dot layer 4 are each independently 1.3 to 1.7, and the refractive indexes of the first optical transition layer 1 and the second optical transition layer 3 are each independently 1 to 1.6, so that the above-mentioned refractive index rules are simultaneously satisfied.
[0041] The first quantum dot layer 2 and the second quantum dot layer 4 may have the same or different refractive indexes. The first optical transition layer 1 and the second optical transition layer 3 may have the same or different refractive indexes.
[0042] In the present application, the term "microstructure pattern" refers to a structure pattern having a micrometer size, which has a light-condensing effect on light rays. Specifically, for example, it may include four situations a to d of light ray propagation from left to right as shown in FIG. 3 , in which a) the light rays are totally reflected (TIR) as much as possible, and b) the light rays are totally reflected (TIR) as much as possible. + , e.g., total reflection within a microstructure unit in the same microstructure pattern); a. increase the amount of light that can be refracted; c. reduce the proportion of light loss; and d. reuse the refracted light (e.g., refracted in one microstructure unit and then re-used in the next microstructure unit). It can ensure the brightness improvement and reduce the blue light output by repeatedly reflecting some light in the corresponding quantum dot layer and improving the utilization rate of light.
[0043] In the present application, the specific shape of the microstructure pattern can be selected from a wide range of options, and may be, for example, a plate shape (e.g., a prism), an arc shape (e.g., a sphere or an ellipsoid), or a combination thereof, as long as it is advantageous for improving brightness and reducing blue light output.
[0044] More preferably, the first microstructure pattern and the second microstructure pattern each independently include a vertex, and the angle of the vertex is 45 to 135°. This preferred solution is favorable for multi-level reuse of light refracted at adjacent interfaces, thereby improving brightness and reducing blue light output.
[0045] In the present application, the angle of a vertex refers to the maximum angle at which the vertex is located. The vertex may be formed by at least two planes, at least one arcuate surface, or a combination of multiple planes and multiple arcuate surfaces, and the angle of the vertex refers to the maximum angle between any two surfaces that form the same vertex. For example, when the vertex is formed by one arcuate surface, the angle of the vertex is a taper angle.
[0046] More preferably, the angle of the apex of the second microstructure pattern is 70 to 110°, further preferably 80 to 100°, further preferably 90°. In this preferred solution, it is advantageous for improving brightness by multiple reflection or refraction of light rays, and for blue light to return to the second quantum dot layer by maximum reflection or refraction to act on the quantum dot material.
[0047] In a preferred embodiment of the present application, the first microstructure pattern and the second microstructure pattern each have a plurality of repeating units, and each repeating unit independently satisfies a maximum width of 10 to 100 μm and a maximum height of 2 to 120 μm.
[0048] Those skilled in the art can select the respective sizes of the corresponding repeat units of the first microstructure pattern and the second microstructure pattern from the standpoint of brightness enhancement and blue light blocking.
[0049] More preferably, the repeating unit of the first microstructure pattern and / or the second microstructure pattern satisfies a maximum width of 10 to 100 μm, further preferably 50 μm, and a maximum height of 10 to 70 μm, further preferably 25 μm. In this preferred solution, it is advantageous for improving brightness by multiple reflection or refraction of light rays, and for blue light to return to the second quantum dot layer by maximum reflection or refraction to act on the quantum dot material.
[0050] According to the present application, preferably, the first microstructure pattern and the second microstructure pattern are each independently a prism structure, the cross section of which is shown in FIG. 3, and the refraction and reflection state of which is shown in the direction of the arrow in FIG.
[0051] The first microstructured pattern and the second microstructured pattern may be the same or different.
[0052] Preferably, the angle between the first microstructure pattern and the second microstructure pattern in the vertical propagation direction of light (also referred to as the angle between two microstructures) is 0 to 180°, preferably the angle is 45 to 135°, and most preferably the angle is 90°. This preferred solution of the present application is advantageous for improving the utilization rate of light and reducing blue light.
[0053] In the present application, the "angle formed by the first microstructure pattern and the second microstructure pattern in the vertical propagation direction of a light ray" refers to the angle between a corresponding surface of the first microstructure pattern in the vertical direction and a corresponding surface of the second microstructure pattern in the vertical direction (or a surface on which an extension line of the surface is located) in the same vertical direction in which a light ray propagates. Note that the "surface" here means a flat surface or an arc surface.
[0054] According to the present application, preferably, as shown in Figures 1 and 2, the quantum dot integrated plate further includes a resin powder 5 disposed in the first optical transition layer 1. In this preferred solution, the resin powder 5 forms a certain roughness on the light incident surface of the first optical transition layer 1, and the light incident surface of the first optical transition layer 1 becomes rough, so that the specular reflection phenomenon can be reduced, which is favorable for increasing the amount of incident light, and is favorable for improving the brightness of the quantum dot integrated plate and the utilization rate of the red and green quantum dot materials for blue light. Meanwhile, when more blue light passes through the first optical transition layer 1 and enters the first quantum dot layer 2, the difference between the refractive index of the resin powder 5 and the refractive index of the adhesive changes the propagation angle of the light, causing the light to diverge at multiple angles, thereby achieving the effect of uniforming and diverging the light.
[0055] The resin powder 5 is dispersed and preferably uniformly distributed in the first optical transition layer 1, which is advantageous for uniformizing the light beam and promoting the use of multiple directions.
[0056] Preferably, the content of the resin powder 5 in the first optical transition layer is 1 to 50 wt %.
[0057] Preferably, the material of the resin powder 5 is the same as the base material of the first quantum dot layer 2. This preferred solution is advantageous to fully exert the brightness enhancement structure, and the refractive index change is better.
[0058] Those skilled in the art can select the particle size of the resin powder depending on the brightness and the propagation state of blue light.The average particle size of the resin powder 5 is preferably 1 to 100 μm.
[0059] In this application, "average particle size" means the average diameter.
[0060] According to the present application, the thickness of the first optical transition layer 1 and the second optical transition layer 3 is preferably 10 to 500 μm, more preferably 10 to 200 μm, and further preferably 10 to 100 μm, respectively and independently.
[0061] Preferably, the thickness of the first quantum dot layer 2 and the second quantum dot layer 4 is independently 0.05 to 1.5 mm.
[0062] Those skilled in the art can select the substrates of the first quantum dot layer 2 and the second quantum dot layer 4 according to the actual situation. Preferably, the first quantum dot layer 2 further includes a first polymer material, and the second quantum dot layer 4 further includes a second polymer material.
[0063] The first polymeric material and the second polymeric material may be the same or different, but preferably are the same. In the present application, there is no limitation on the specific type of the polymeric material, and it may be a polymeric material that is applicable to conventional optical plates in this field. Exemplarily, the polymeric material may be a resin material such as PE, PS, PMMA, PC, MS, PET, PP, etc.
[0064] In the corresponding quantum dot layer of the present application, those skilled in the art can select the ratio of the quantum dot material contained therein and the corresponding polymer material according to actual needs. Exemplarily, in the first quantum dot layer 2, the weight ratio of the red quantum dot material to the first polymer material may be 1:100-10000. Exemplarily, in the second quantum dot layer 4, the weight ratio of the blue quantum dot material to the second polymer material may be 1:100-10000.
[0065] A second aspect of the present application is A step (1) of producing a first quantum dot sheet and a second quantum dot sheet; (2) forming a first microstructure pattern and a second microstructure pattern on one side of the first quantum dot sheet and one side of the second quantum dot sheet, respectively; Step (3): measuring the refractive index of the first quantum dot sheet and the second quantum dot sheet, selecting a photocurable adhesive or a pressure-sensitive adhesive to form a first optical transition layer 1 and a second optical transition layer 3, and applying the photocurable adhesive or the pressure-sensitive adhesive to the other side of the first quantum dot sheet and the other side of the second quantum dot sheet, respectively; and (4) joining a side of the first quantum dot sheet on which a first microstructure pattern is formed and a side of the second quantum dot sheet on which a photocurable adhesive or a pressure-sensitive adhesive is applied to form a quantum dot integrated plate in which the refraction of light is variable.
[0066] The above-mentioned manufacturing method of the present application uses a photocurable adhesive or a pressure-sensitive adhesive to form the first optical transition layer 1 and the second optical transition layer 3, which can act synergistically with a specific refractive index design and microstructure pattern design, so that the manufactured quantum dot integrated plate can maximize the brightness improvement effect of light and the utilization effect of quantum dots on blue light, and can better improve the color gamut and reduce the output of blue light in accordance with the photoeffect properties of the quantum dot material.
[0067] In step (1), those skilled in the art can select a conventional method to manufacture the quantum dot layer according to their needs.
[0068] In a preferred embodiment, the first quantum dot sheet and the second quantum dot sheet are produced independently of each other by mixing a quantum dot solution with a polymer material and then performing a molding process.
[0069] In step (1), in the manufacture of the first quantum dot sheet, the corresponding quantum dot solution is a solution containing a red quantum dot material, and in the manufacture of the second quantum dot sheet, the corresponding quantum dot solution is a solution containing a green quantum dot material. The manufacture of these solutions is well known to those skilled in the art, and therefore will not be described here.
[0070] In the manufacture of the first quantum dot sheet and the second quantum dot sheet, the corresponding polymer materials are a first polymer material and a second polymer material, respectively.
[0071] According to the present application, the specific process of the above-mentioned molding includes molding manner and process parameters, which can be selected by those skilled in the art according to actual needs, and preferably, the above-mentioned molding is extrusion molding. The above-mentioned extrusion molding device can include a screw extruder.
[0072] More preferably, the extrusion is carried out at a temperature of 120 to 300°C.
[0073] In step (1) of the present application, the mixed material is stretched into a quantum dot sheet by the molding process to form the first quantum dot layer 2 and the second quantum dot layer 4 .
[0074] In step (2) of the present application, the first microstructure pattern and the second microstructure pattern can be formed by any conventional method as understood by those skilled in the art, for example, by direct inkjet printing, roll molding, additive manufacturing, etc.
[0075] Preferably, the first and second microstructured patterns are formed by pressing with a microstructured roller, this preferred solution makes the process simple and efficient.
[0076] The pressing conditions of the microstructure roller may be any conditions that allow the formation of a microstructure. For example, the formation of the microstructure by pressing the microstructure roller is performed under high temperature conditions.
[0077] In step (3) of the present application, the refractive indexes of the first quantum dot sheet and the second quantum dot sheet are measured according to the requirements that the refractive index should meet, and a photocurable adhesive or a pressure-sensitive adhesive is selected and applied to the other side of the first quantum dot sheet and the other side of the second quantum dot sheet, where the microstructure pattern and the applied adhesive are located on both sides of the quantum dot sheet, respectively.
[0078] In addition, the adhesive applied to the quantum dot sheet may be photocured (preferably UV cured) or pressed in an appropriate step according to the need for subsequent layer bonding to form a solid optical transition layer, as long as the first optical transition layer 1 and the second optical transition layer 3 can be finally formed. For example, if there is no need to later bond another layer to the applied adhesive, photocuring or pressing can be performed in step (3), and if there is a need to subsequently bond another layer, photocuring or pressing can be performed after bonding in a later step.
[0079] Preferably, the method further comprises the step of incorporating a resin powder 5 into the photocurable or pressure sensitive adhesive applied to the first quantum dot sheet in step (3).
[0080] It should be understood that the resin powder 5 is mixed into the light curable or pressure sensitive adhesive.
[0081] In step (4) of the present application, "the side of the first quantum dot sheet on which the first microstructure pattern is formed is joined to the side of the second quantum dot sheet on which the photocurable adhesive or pressure-sensitive adhesive is applied" means joining the surface of the first microstructure pattern on the first quantum dot sheet to the surface of the adhesive on the second quantum dot sheet. After the joining, a second optical transition layer 3 is formed between the first quantum dot sheet and the second quantum dot sheet through photocuring or pressure bonding.
[0082] In the present application, it should be understood that the amount of each raw material used should be such that it satisfies the structure and composition of each layer. The structure and composition of each layer are the same as those in the first embodiment, and therefore description thereof will be omitted here.
[0083] A third aspect of the present application provides a display device including the quantum dot integrated plate according to the first aspect.
[0084] The quantum dot integrated plate according to the present application can be applied to any type of conventional module, including, but not limited to, a normal direct type module (which generally includes a panel 6, a brightness enhancing film, a diffusion film, and a diffusion plate 7) and a normal edge-lit display device (which generally includes a panel 6, a brightness enhancing film, a diffusion film, and a light guide plate 8). The quantum dot integrated plate according to the present application can improve brightness and block blue light, and when used in a module, it does not require multiple components for improving brightness and blocking blue light, and can reduce the cost of the optical film and the assembly cost.
[0085] In a preferred embodiment, the display device is in a direct backlight mode, as shown in FIG. a panel 6 provided on the outer side of the second quantum dot layer 4 of the quantum dot assembly plate A; and a diffusion plate 7 provided on the side of the quantum dot integrating plate A away from the panel 6.
[0086] More preferably, the thickness of the first quantum dot layer and the second quantum dot layer in the quantum dot assembly plate A is independently 0.5 to 1.5 mm.
[0087] In another preferred embodiment, the display device is in an edge-lit backlight mode, as shown in FIG. a panel 6 provided on the outer side of the second quantum dot layer 4 of the quantum dot assembly plate A; and a light guide plate 8 provided on the side of the quantum dot integrating plate A away from the panel 6.
[0088] More preferably, the thickness of the first quantum dot layer and the second quantum dot layer in the quantum dot assembly plate A is independently 0.05 to 0.5 mm.
[0089] In the present application, there is no limitation on the specific type of the panel 6, and it may be, for example, a liquid crystal panel.
[0090] The present invention will now be described in more detail with reference to examples.
[0091] Example 1 The quantum dot integrated plate includes, in this order, a first optical transition layer 1, a PS first quantum dot layer 2, a second optical transition layer 3, and a PS second quantum dot layer 4. The first optical transition layer 1 is located below the first quantum dot layer 2, and the second optical transition layer 3 is located between the first quantum dot layer 2 and the second quantum dot layer 4. Both the first optical transition layer 1 and the second optical transition layer 3 are formed by curing an acrylic resin adhesive.
[0092] A specific method for producing the quantum dot integrated plate includes the following steps (1) to (3).
[0093] (1) The red and green quantum dot solutions are mixed with a polymer material PS, respectively, and then extruded at 200°C using a screw extruder to draw a quantum dot sheet. At the same time, a microstructured roller is used to press a microstructured pattern on one side of the sheet to produce a first quantum dot sheet containing red quantum dot material and a second quantum dot sheet containing green quantum dot material, i.e., a first quantum dot layer 2 having a first microstructured pattern and a second quantum dot layer 4 having a second microstructured pattern are obtained.
[0094] (2) A UV-curable adhesive is applied to the rear surface of the microstructure of the first quantum dot sheet, and after curing with UV light, a first optical transition layer 1 is formed on the first quantum dot sheet.
[0095] (3) An ultraviolet-curable adhesive is applied to the microstructured back surface of the second quantum dot sheet, and then the microstructured surface of the first quantum dot sheet and the microstructured back surface of the second quantum dot sheet are bonded with the applied ultraviolet-curable adhesive and cured with ultraviolet light. After that, a second optical transition layer 3 is formed between the first quantum dot sheet and the second quantum dot sheet, and a quantum dot integrated plate is finally produced.
[0096] Wherein, the first optical transition layer 1 has a refractive index of 1.49 and a thickness of 200 μm, the first quantum dot layer 2 has a refractive index of 1.52 and a thickness of 0.5 mm, the second optical transition layer 3 has a refractive index of 1.49 and a thickness of 200 μm, and the second quantum dot layer 4 has a refractive index of 1.52 and a thickness of 0.5 mm. The first and second microstructure patterns are both prism structures, and the repeating units of the microstructure patterns of the first quantum dot layer 2 and the second quantum dot layer 4 both have an apex angle of 45° and a maximum height of 120 μm, and the included angle between the first and second microstructure patterns in the vertical propagation direction of the light is 0°.
[0097] The quantum dot integrated plate manufactured in the embodiment was placed on a direct-type display device with the same blue light power, and a blue light illuminometer and a color analyzer were placed in the center of the board material to measure the blue light intensity and brightness. The blue light intensity and brightness of the original model optical plate were also measured and compared.
[0098] The original model optical plate is composed of a PET light diffusing layer, a PS red and green quantum dot layer and a PET brightness enhancing layer stacked in sequence. The refractive index of the light diffusing layer is 1.59, the refractive index of the quantum dot layer is 1.52, and the refractive index of the brightness enhancing layer is 1.59.
[0099] The measured luminance and blue light intensity data were compared with the original model and found to have a 2.56% increase in luminance and a 2.11% decrease in blue light intensity.
[0100] Example 2 This quantum dot integrated plate differs from that of Example 1 in that the maximum height of the second microstructure pattern is 25 μm.
[0101] The measured luminance and blue light intensity data were compared with the original model and found to have a 6.05% increase in luminance and a 5.15% decrease in blue light intensity.
[0102] Example 3 This quantum dot integrated plate differs from that of Example 1 in that the maximum height of the second microstructure pattern is 2 μm.
[0103] The measured luminance and blue light intensity data were compared with the original model and found to have a 2.48% increase in luminance and a 2.75% decrease in blue light intensity.
[0104] Example 4 This quantum dot integrated plate differs from that of Example 1 in that the maximum height of the first microstructure pattern is 25 μm.
[0105] The measured luminance and blue light intensity data were compared with the original model and found to have a 5.55% increase in luminance and a 4.42% decrease in blue light intensity.
[0106] Example 5 This quantum dot integrated plate differs from that of Example 4 in that the maximum height of the second microstructure pattern is 25 μm.
[0107] The measured luminance and blue light intensity data were compared with the original model and found to have a 9.41% increase in luminance and an 8.34% decrease in blue light intensity.
[0108] Example 6 This quantum dot integrated plate differs from that of Example 4 in that the maximum height of the second microstructure pattern is 2 μm.
[0109] The measured luminance and blue light intensity data were compared with the original model and found to have a 4.29% increase in luminance and a 4.01% decrease in blue light intensity.
[0110] Example 7 This quantum dot integrated plate differs from that of Example 1 in that the maximum height of the first microstructure pattern is 2 μm.
[0111] The measured luminance and blue light intensity data were compared with the original model and found to have a 2.01% increase in luminance and a 2.98% decrease in blue light intensity.
[0112] Example 8 This quantum dot integrated plate differs from that of Example 7 in that the maximum height of the second microstructure pattern is 25 μm.
[0113] The measured luminance and blue light intensity data were compared with the original model and found to have a 6.49% increase in luminance and a 5.25% decrease in blue light intensity.
[0114] Example 9 This quantum dot integrated plate differs from that of Example 7 in that the maximum height of the second microstructure pattern is 2 μm.
[0115] The measured luminance and blue light intensity data were compared with the original model and found to have a 2.62% increase in luminance and a 2.01% decrease in blue light intensity.
[0116] Example 10 This quantum dot integrated plate differs from that of Example 5 in that the angle formed between the first microstructure pattern and the second microstructure pattern in the vertical propagation direction of the light beam is 90°.
[0117] The measured luminance and blue light intensity data were compared with the original model and found to have a 13.49% increase in luminance and an 11.25% decrease in blue light intensity.
[0118] Example 11 This differs from the quantum dot integrated plate of Example 10 in that the angle between the first microstructure pattern and the second microstructure pattern in the vertical propagation direction of the light beam is 180°.
[0119] The measured luminance and blue light intensity data were compared with the original model and found to have a 9.62% increase in luminance and a 9.01% decrease in blue light intensity.
[0120] Example 12 This differs from the quantum dot integrated plate of Example 10 in that PS resin powder 5 is mixed into the first optical transition layer 1, the average particle size of the resin powder is 1 μm, and the amount of resin powder added to the first optical transition layer is 5 wt %.
[0121] The measured luminance and blue light intensity data were compared with the original model and found to have a 15.19% improvement in luminance and a 13.89% decrease in blue light intensity.
[0122] Example 13 This differs from the quantum dot integrated plate of Example 12 in that the amount of resin powder added to the first optical transition layer is 50 wt %.
[0123] The measured luminance and blue light intensity data were compared with the original model and found to have a 17.40% increase in luminance and a 14.45% decrease in blue light intensity.
[0124] Example 14 This quantum dot assembly plate differs from that of Example 12 in that the average particle size of the resin powder is 100 μm.
[0125] The measured luminance and blue light intensity data were compared with the original model and found to have a 15.77% increase in luminance and a 13.66% decrease in blue light intensity.
[0126] Example 15 This differs from the quantum dot integrated plate of Example 5 in that PS resin powder 5 is mixed into the first optical transition layer 1, the average particle size of the resin powder is 100 μm, and the amount of resin powder added to the first optical transition layer is 50 wt %.
[0127] The measured luminance and blue light intensity data were compared with the original model and found to have a 17.01% improvement in luminance and a 14.88% decrease in blue light intensity.
[0128] Comparative Example 1 It differs from the quantum dot integrated plate of Example 1 in that the refractive index of each layer is different, with the refractive index of the first optical transition layer 1 and the second optical transition layer 3 (both of which are 1.57) being higher than the refractive index of the first quantum dot layer 2 and the second quantum dot layer 4 (both of which are 1.52).
[0129] The measured luminance and blue light intensity data were compared with the original model and found to be reduced by 3.69% in luminance and 1.17% in blue light intensity.
[0130] Comparative Example 2 This differs from the quantum dot integrated plate of Example 1 in that the first and second fine structure patterns are not provided.
[0131] The measured luminance and blue light intensity data were compared with the original model and found to be reduced by 1.88% in luminance and 1.98% in blue light intensity.
[0132] As can be seen from the above examples and comparative examples, the quantum dot integrated plate having the specific structure of the present application, particularly the specific refractive index change and microstructure design, has a remarkable effect in terms of improving brightness and reducing blue light output.
[0133] Furthermore, as can be seen from multiple comparisons between Example 2 and Example 1 and Example 3, between Example 5 and Example 4 and Example 6, and between Example 8 and Example 7 and Example 9, if the maximum height of the first microstructure pattern or the second microstructure pattern is too large or too small, the improvement in brightness is relatively small, and the decrease in the intensity of blue light is relatively small. This is because if the maximum height of the first microstructure pattern or the second microstructure pattern is too large or too small, it is disadvantageous to the light ray returning to the second quantum dot layer by maximum reflection or refraction, which is disadvantageous to the improvement of brightness, and it is disadvantageous to the blue light returning to the second quantum dot layer by maximum reflection or refraction to interact with the blue light quantum dots, which is disadvantageous to the maximum utilization of blue light.
[0134] Moreover, as can be seen from the comparison between Example 10 and Example 11, the use of the preferred specific microstructure distribution solution of the present application can further improve the brightness and reduce the blue light output, because the two microstructure patterns form a suitable angle, which can promote the multi-level utilization of light and promote the full play of the properties of quantum dot material and the interaction with blue light.
[0135] Furthermore, as can be seen from the comparison between Example 10 and Example 12, the preferred solution of adding the resin powder 5 of the present invention can further improve the brightness and reduce the output of blue light. This is because the resin powder 5 can reduce the specular reflection phenomenon of the first optical transition layer 1 and increase the amount of blue light entering, while the resin powder 5 can further change the refractive index in the first optical transition layer 1, promoting the multi-angle and multi-directional divergence of the light when it enters the first quantum dot layer 2.
[0136] Furthermore, as can be seen from a comparison of Example 12 with Examples 13 and 14, and a comparison of Example 5 with Example 15, increasing the amount of resin powder 5 added is advantageous for improving brightness and reducing blue light output, and increasing the average particle size is advantageous for improving brightness.
Claims
1. The first optical transition layer, the first quantum dot layer, the second optical transition layer, and the second quantum dot layer are sequentially arranged, and the refractive index of each layer is t 第1光遷移層 <t 第1量子ドット層 , t 第2光遷移層 <t 第1量子ドット層 , t 第2光遷移層 <t 第2量子ドット層 a first microstructure pattern is provided on a side of the first quantum dot layer that is close to the second optical transition layer, and a second microstructure pattern is provided on a side of the second quantum dot layer that is away from the second optical transition layer, the first quantum dot layer containing a red quantum dot material, and the second quantum dot layer containing a green quantum dot material.
2. The quantum dot integrated plate according to claim 1 , wherein the outer surface of the first microstructure pattern and the outer surface of the second microstructure pattern are each independently plate-shaped, arc-shaped, or a combination of both.
3. The quantum dot integrated plate of claim 1, wherein the first microstructure pattern and the second microstructure pattern each independently include a vertex, and the angle of the vertex is between 45 and 135°.
4. The quantum dot integrated plate of claim 1, wherein the first microstructure pattern and the second microstructure pattern each have a plurality of repeating units, and each repeating unit independently satisfies a maximum width of 10 to 100 μm and a maximum height of 2 to 120 μm.
5. The quantum dot integrated plate according to claim 4 , wherein the repeating units of the first microstructure pattern and / or the second microstructure pattern each independently satisfy a maximum width of 50 μm and a maximum height of 25 μm.
6. The quantum dot integrated plate according to claim 1 , wherein the first microstructure pattern and the second microstructure pattern are each independently a prism structure.
7. 2. The quantum dot integrated plate according to claim 1, wherein an included angle between the first microstructure pattern and the second microstructure pattern in a vertical propagation direction of a light beam is 0 to 180 degrees.
8. 8. The quantum dot integrated plate according to claim 7, wherein the included angle is 45 to 135 degrees.
9. The quantum dot integrated plate according to claim 8 , wherein the included angle is 90°.
10. The quantum dot integrated plate according to any one of claims 1 to 9, further comprising a resin powder provided in the first optical transition layer.
11. The quantum dot integrated board according to claim 10, wherein the content of the resin powder in the first optical transition layer is 1 to 50 wt %.
12. The quantum dot integrated plate according to claim 10 , wherein the material of the resin powder is the same as that of the base material of the first quantum dot layer.
13. The quantum dot assembly board according to claim 10, wherein the resin powder has an average particle size of 1 to 100 μm.
14. The quantum dot integrated plate according to claim 1, wherein the thicknesses of the first optical transition layer and the second optical transition layer are each independently 10 to 500 μm, and the thicknesses of the first quantum dot layer and the second quantum dot layer are each independently 0.05 to 1.5 mm.
15. The quantum dot integrated plate according to claim 14, wherein the first optical transition layer and the second optical transition layer each have a thickness of 10 to 200 μm independently.
16. A method for producing a quantum dot integrated plate according to any one of claims 1 to 15, Step (1) of producing a first quantum dot sheet and a second quantum dot sheet; (2) forming a first microstructure pattern and a second microstructure pattern on one side of the first quantum dot sheet and one side of the second quantum dot sheet, respectively; Step (3): measuring the refractive index of the first quantum dot sheet and the second quantum dot sheet, selecting a photocurable adhesive or a pressure-sensitive adhesive to form a first optical transition layer and a second optical transition layer, and applying the photocurable adhesive or the pressure-sensitive adhesive to the other side of the first quantum dot sheet and the other side of the second quantum dot sheet, respectively; and (4) joining the side of the first quantum dot sheet on which a first microstructure pattern is formed and the side of the second quantum dot sheet on which a photocurable adhesive or a pressure-sensitive adhesive is applied to form a quantum dot integrated plate in which the refraction of light changes.
17. In step (1), the first quantum dot sheet and the second quantum dot sheet are produced independently of each other by mixing a quantum dot solution with a polymer material and then forming the mixture; And / or, in step (2), the first microstructure pattern and the second microstructure pattern are formed by pressing with a microstructure roller.
18. The method for manufacturing a quantum dot integrated plate according to claim 16 or 17, further comprising the step of introducing a resin powder into the photocurable adhesive or pressure-sensitive adhesive applied to the first quantum dot sheet in step (3).
19. A display device comprising the quantum dot integrated plate according to any one of claims 1 to 15.
20. a panel provided on the outer side of the second quantum dot layer of the quantum dot assembly plate; The display device according to claim 19 , further comprising a diffusion plate or a light guide plate provided on a side of the quantum dot integrated plate away from the panel.
21. The display device according to claim 19, wherein when the display device is in a direct backlight mode, the thicknesses of the first quantum dot layer and the second quantum dot layer in the quantum dot integrated plate are each independently 0.5 to 1.5 mm, and when the display device is in an edge-light backlight mode, the thicknesses of the first quantum dot layer and the second quantum dot layer in the quantum dot integrated plate are each independently 0.05 to 0.5 mm.
Citation Information
Patent Citations
Quantum dot color filter and preparation method, liquid crystal panel, and liquid crystal display device
CN106707610A
Optical member, backlight unit using the optical member and liquid crystal display device
JP2017173817A
Optical wavelength conversion composition, optical wavelength conversion member, optical wavelength conversion sheet, backlight device, and image display device
JP2018124411A
Remote controller with battery leakage prevention structure
KR102294222B1
Backlight modules
US20170175956A1