Heat Treated Aluminum Sheet and Manufacturing Process

A continuous heat treatment process for metal strips, including solution annealing, rapid cooling, and thermal spiking, addresses the challenge of producing thin gauge metal products with balanced strength and formability, enhancing production efficiency and suitability for automotive applications.

JP2024539637APending Publication Date: 2024-10-29NOVELIS INC(US)
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024522292
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2022-10-25
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Manufacturers face challenges in producing thin gauge metal products that balance good formability with high strength, particularly in automotive applications, as existing heat treatment processes are lengthy and complex, requiring batch aging and precise control, which limits production efficiency.

Method used

A continuous heat treatment process involving solution annealing, rapid cooling, and thermal spiking of metal strips at elevated temperatures, followed by coiling without batch aging, allowing for the production of metal strips with tailored properties suitable for automotive applications.

Benefits of technology

The process enables the production of metal strips with high strength and good formability, eliminating the need for batch aging and reducing production time, making it suitable for lightweight vehicle body panels and structural members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539637000001
    Figure 2024539637000001
  • Figure 2024539637000002
    Figure 2024539637000002
  • Figure 2024539637000003
    Figure 2024539637000003
Patent Text Reader

Abstract

Described herein is a continuous heat treatment process for metals, such as strips of heat treatable alloys, in which the metals are solutionized, rapidly cooled, heat spiked at high temperatures, and coiled. The continuous heat treatment process does not include or require a batch aging treatment.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 63 / 263,052, filed October 26, 2021, which is incorporated by reference herein in its entirety.

[0002] The present disclosure relates generally to metal processing, and more specifically to a continuous heat treatment process for metals in which a strip of a heat treatable alloy is solutionized, rapidly cooled, heat spiked, and coiled. [Background technology]

[0003] Manufacturers of metal articles are faced with the challenge of providing thin gauge materials that have both good formability and high strength after the article is formed and paint cured. As an example, the automotive industry requires such products for use in lightweight body panels or structural members to improve vehicle economy and fuel economy.

[0004] Heat treatable metals, such as heat treatable aluminum alloys, can achieve these objectives in some cases. Heat treatable alloys are generally alloys that contain soluble alloying components in amounts that exceed their room temperature solubility limits. These alloys can contain hardening elements (e.g., Mg, Si and / or Co) to provide hardening during aging, and potentially other elements such as Fe, Mn and possibly Cr to control formability and grain size. Such alloys can develop improved properties when subjected to working and / or heating and then a quenching step. Heat treatment of metals is conventionally done by precipitation hardening, which includes the steps of solution heat treatment and aging. In a solution heat treatment process, a metal strip, for example an aluminum alloy strip, is solutionized and cooled rapidly, with or without a heat spike depending on the product requirements. The purpose of the solutionizing procedure is to solutionize the alloying (solute) elements, ultimately strengthening the particular alloy. The purpose of the rapid cooling is to lock the solute elements and excess vacancies into the metal (e.g., aluminum) matrix of the metal strip. The purpose of the heat spike is to ensure that the coil is coiled between 60°C and 110°C and to eliminate the adverse effects of coil storage, where the material loses up to 40% of its potential strength gain during the paint bake. The heat treated metal strip can then undergo an aging procedure.

[0005] As an example, current processes for producing aged tempers involve a batch aging process in which coils in T4 temper are heated at 20°C / h to 50°C / h to high temperatures in the range of 120°C to 260°C, soaked for 1 hour or more, and cooled to room temperature. However, existing heat treating and batch aging processes require total cycle times and soak times longer than 8 hours (over 1 hour, often 4 to 6 hours), additional steps and complexities, and precise control of the heat treating process. Summary of the Invention

[0006] The term "embodiments" and similar terms are intended to refer broadly to all of the subject matter of the present disclosure and the following claims. Statements containing these terms should be understood to neither limit the subject matter described herein nor limit the meaning or scope of the following claims. The embodiments of the present disclosure addressed herein are defined by the following claims, not this Summary. This Summary is a broad overview of various aspects of the present disclosure and introduces some of the ideas that are further described in the Detailed Description section below. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to the entire specification of this disclosure, any or all drawings, and appropriate portions of each claim.

[0007] Certain aspects and features of the present disclosure relate to a continuous heat treatment process in which a metal strip is solutionized, rapidly cooled, heat spiked at an elevated temperature in the range of 120° C. to 300° C. (e.g., 200° C. to 250° C.), and coiled at a reel located at the end of a continuous line. In some aspects, the continuous heat treatment process and its constituent steps can be performed at a particular line speed, for example, a line speed of at least 10 meters / min (e.g., at least 40 meters / min; 10 meters / min to 100 meters / min, 40 meters / min to 100 meters / min, or 10 meters / min to 40 meters / min). In some aspects, the heat spike treatment can be performed in a relatively long reheat furnace, for example, a reheat furnace longer than 10 meters. In some aspects, only natural cooling (i.e., no cooling device is used) is performed between the heat spike and coiling, and the coiling is performed to maintain the line speed. In some embodiments, the cooling or natural cooling rate after the heat spike treatment is less than 10° C. / hour (e.g., less than 2° C. / hour), for example, to ambient temperature. Thus, in some embodiments, the coiling of the metal strip is performed at a relatively warm temperature, such as above 60° C., such as above 110° C., 70° C.-150° C., 70° C.-130° C., or 70° C.-110° C., 110° C.-150° C., 110° C.-130° C., or 110° C.-120° C. In certain embodiments, the disclosed process does not include or require a batch aging process to age harden the material.

[0008] The present disclosure allows for the production of products from the disclosed process with thin gauges that have both good formability and high strength using a continuous annealing line without the need for a batch aging process. The present disclosure is particularly beneficial in providing products with a tailored combination of properties and thus offering the possibility of downgauging or as a potential replacement for 5000 series aluminum alloys supplied in H1X, H2X and H3x tempers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Certain aspects and features of the present disclosure relate to a continuous heat treatment process in which a metal strip is solutionized, rapidly cooled, heat spiked (e.g., by hot air) at an elevated temperature in the range of 120° C. to 300° C., coiled, and cooled or naturally cooled (before and / or after coiling), for example at a rate of 5° C. / hour or less, preferably 2° C. / hour or less. In certain embodiments, the metal strip is a heat treatable alloy, for example a heat treatable aluminum alloy.

[0010] In certain embodiments, the heat spike temperature is maintained between 120° C. and 300° C. (e.g., between about 150° C. and 300° C.). The use of a higher temperature heat spike can induce the formation of clusters that act as nuclei to form hardened particles during subsequent coiling and coil cooling.

[0011] The present disclosure improves upon existing technology in part by eliminating the batch process entirely by using a reheat furnace to heat spike the metal strip to the desired temperature at the line speed before coiling. For example, a continuous annealing line can be used without the need for a batch aging process. The heat spike coil combined with coil cooling provides the proper conditions for age hardening. The use of heat spike and coiling at warm coiling temperatures to tailor various properties is accomplished by the present disclosure. The present disclosure is particularly beneficial in providing a product with a tailored combination of properties, thus offering the possibility of downgauging.

[0012] Although aspects and features of the present disclosure are described herein with respect to metal strip, such as continuously cast or uncoiled metal strip, the present disclosure may also be used with any suitable metal product processed on a continuous annealing line. Aspects and features of the present disclosure may be particularly suitable for any metal product having flat surfaces. Aspects and features of the present disclosure may be particularly suitable for any metal product having parallel or nearly parallel opposing surfaces (e.g., top and bottom surfaces). Nearly parallel may include parallel or within 1°, 2°, 3°, 4°, 5°, 6°, 7°, 8°, 9°, or 10° of parallel, or more.

[0013] Definitions and Explanations As used herein, the terms "invention," "the invention," "this invention," and "the present invention" are intended to refer broadly to all of the subject matter of this patent application and the claims that follow. Statements containing these terms should not be understood as limiting the subject matter described herein or the meaning or scope of the claims that follow.

[0014] Reference is made herein to alloys identified by AA numbers and other related designations, such as "series" or "7xxx." To understand the numbering systems most commonly used in naming and identifying aluminum and its alloys, please refer to "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingot," both published by The Aluminum Association.

[0015] As used herein, plate generally has a thickness of greater than about 15 mm. For example, plate can refer to aluminum products having a thickness of greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, or greater than about 100 mm.

[0016] As used herein, a shade (also referred to as a sheet plate) generally has a thickness of about 4 mm to about 15 mm. For example, the shade may have a thickness of about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm, or about 15 mm.

[0017] As used herein, sheet generally refers to an aluminum product having a thickness of less than about 4 mm. For example, the sheet can have a thickness of less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, or less than about 0.3 mm (e.g., about 0.2 mm).

[0018] As used herein, foil generally refers to a metal product having a thickness of less than about 0.2 mm. For example, the foil may have a thickness of less than about 0.2 mm, less than about 0.15 mm, less than about 0.10 mm, less than about 0.05 mm, less than about 0.04 mm, less than about 0.03 mm, less than about 0.02 mm, or less than about 0.01 mm (e.g., about 0.006 mm).

[0019] As used herein, direct chill (DC) and continuous casting are two methods of casting solid metal from liquid metal. In DC casting, liquid metal is poured into a mold with a retractable false bottom that can be withdrawn at the solidification rate of the liquid metal in the mold, often resulting in large, relatively thick ingots (e.g., 1500 mm wide x 500 mm thick x 5 m long). The ingots are processed, homogenized, hot rolled, cold rolled, and may or may not be annealed after hot rolling or before a final cold rolling pass, and / or heat treated, and otherwise finished before being coiled into a metal strip product that can be distributed to consumers of the metal strip product (e.g., automobile manufacturing facilities).

[0020] Continuous casting involves the continuous injection of molten metal into a casting cavity defined between a pair of moving, opposing casting surfaces and the withdrawal of a cast metal form (e.g., metal strip) from an outlet of the casting cavity. Continuous casting is desirable when the entire product can be prepared in a single, fully coupled process line. Such a fully coupled process line involves matching, or "interlocking," the speed of the continuous casting equipment to the speed of downstream processing equipment.

[0021] In this application, reference may be made to the temper or condition of the alloy. For an understanding of the most commonly used alloy temper descriptions, see American National Standards (ANSI) H35 on Alloy and Temper Designation Systems. The F condition or temper refers to the aluminum alloy as produced. The O condition or temper refers to the aluminum alloy after annealing. The Hxx condition or temper, also referred to herein as H temper, refers to the non-heat treatable aluminum alloy after cold rolling, with or without heat treatment (e.g., annealing). Suitable H tempers include tempers HX1, HX2, HX3, HX4, HX5, HX6, HX7, HX8, or HX9. The T1 condition or temper refers to the aluminum alloy that has been cooled from hot working and naturally aged (e.g., at room temperature). The T2 condition or temper refers to the aluminum alloy that has been cooled from hot working, cold worked, and naturally aged. The T3 condition or temper refers to an aluminum alloy that has been solution heat treated, cold worked, and naturally aged. The T4 condition or temper refers to an aluminum alloy that has been solution heat treated and naturally aged. The T5 condition or temper refers to an aluminum alloy that has been cooled from hot working and artificially aged (at high temperature). The T6 condition or temper refers to an aluminum alloy that has been solution heat treated and artificially aged. The T7 condition or temper refers to an aluminum alloy that has been solution heat treated and artificially overaged. The T8x condition or temper refers to an aluminum alloy that has been solution heat treated, cold worked, and artificially aged. The T9 condition or temper refers to an aluminum alloy that has been solution heat treated, artificially aged, and cold worked. The W condition or temper refers to an aluminum alloy after solution heat treatment.

[0022] As used herein, the meaning of "room temperature" can include a temperature of about 15° C. to about 30° C., e.g., about 15° C., about 16° C., about 17° C., about 18° C., about 19° C., about 20° C., about 21° C., about 22° C., about 23° C., about 24° C., about 25° C., about 26° C., about 27° C., about 28° C., about 29° C., or about 30° C. As used herein, the meaning of "ambient conditions" or "ambient environment" can include a temperature of about room temperature, a relative humidity of about 20% to about 100%, and an atmospheric pressure of about 975 millibars (mbar) to about 1050 mbar. For example, the relative humidity may be about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about It can be 1%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, or any value therebetween. For example, the air pressure can be about 975 mbar, about 980 mbar, about 985 mbar, about 990 mbar, about 995 mbar, about 1000 mbar, about 1005 mbar, about 1010 mbar, about 1015 mbar, about 1020 mbar, about 1025 mbar, about 1030 mbar, about 1035 mbar, about 1040 mbar, about 1045 mbar, about 1050 mbar, or any value therebetween.

[0023] Any range disclosed herein should be understood to include any and all subranges contained therein. For example, a range described as "1 to 10" should be considered to include any and all subranges between a minimum value of 1 and a maximum value of 10, inclusive. That is, all subranges begin with a minimum value of 1 or greater (e.g., 1 to 6.1) and end with a maximum value of 10 or less (e.g., 5.5 to 10). Unless otherwise indicated, when referring to a compositional amount of an element, the term "maximum" means that the element is optional and includes a 0% composition of that particular element. Unless otherwise indicated, all compositional percentages are weight percent (wt%).

[0024] As used herein, the meanings of "a," "an," and "the" include singular and plural references unless the context clearly dictates otherwise.

[0025] In this description, aluminum alloy products and their constituents may be described in terms of their elemental composition in weight percent (wt%), with the maximum wt% of the sum of all impurities in each alloy being 0.15%, with the balance being aluminum.

[0026] Incidental elements such as grain refiners and deoxidizers, or other additives may be present in the present invention and may themselves impart other properties without departing from or significantly altering the alloys described herein or the properties of the alloys described herein.

[0027] Metal Strip As described, the heat treatment process of the present disclosure can be carried out on metal strip, such as aluminum alloy strip. In certain embodiments, the metal strip described herein can be produced from metal casting, such as DC casting or continuous metal casting. After casting, in certain embodiments, the metal strip can be produced by homogenization, hot rolling, and / or cold rolling, and an optional annealing after hot rolling or before final cold rolling.

[0028] In certain aspects, the metal strip can be a metal sheet, shade, or foil. In certain aspects, the metal strip can be a sheet. For example, in one embodiment, the described process is used to produce a sheet having a gauge of 0.5 mm to 4.5 mm. In some such aspects, the metal strip can be an aluminum alloy sheet, such as a heat treatable aluminum alloy sheet. In some aspects, the metal strip can be selected from 2xxx, 6xxx, or 7xxx series aluminum alloy sheets. In some aspects, the metal strip is a 2xxx series aluminum alloy sheet. In some aspects, the metal strip is a 6xxx series aluminum alloy sheet. In some aspects, the metal strip is a 7xxx series aluminum alloy sheet. In certain aspects, the metal strip can be a shade. In some aspects, the metal strip can be an aluminum alloy shade, such as a heat treatable aluminum alloy shade. In some aspects, the metal strip can be selected from 2xxx, 6xxx, or 7xxx series aluminum alloy sheets. In some aspects, the metal strip is a 2xxx series aluminum alloy shade. In some embodiments, the metal strip is a 6xxx series aluminum alloy foil. In some embodiments, the metal strip is a 7xxx series aluminum alloy foil. In certain embodiments, the metal strip can be a foil. In some embodiments, the metal strip can be an aluminum alloy foil, such as a heat treatable aluminum alloy foil. In some embodiments, the metal strip can be selected from a 2xxx series, a 6xxx series, or a 7xxx series aluminum alloy foil. In some embodiments, the metal strip is a 2xxx series aluminum alloy foil. In some embodiments, the metal strip is a 6xxx series aluminum alloy foil. In some embodiments, the metal strip is a 7xxx series aluminum alloy foil.

[0029] In certain embodiments, the alloys exhibit high strength and high deformability. In some cases, the alloys exhibit increased strength after heat treatment without significant loss of deformability. The alloy properties are achieved, at least in part, due to the method of processing the alloys to produce the foils, sheets, or other products described above.

[0030] In some examples, the alloy may have the following elemental composition provided in Table 1. [Table 1]

[0031] In some examples, the alloy may have the following elemental composition provided in Table 2. [Table 2]

[0032] In other examples, the alloy may have the following elemental composition as provided in Table 3: [Table 3]

[0033] In one example, the aluminum alloy can have the following elemental composition shown in Table 4. In certain embodiments, the alloy is used to prepare aluminum foils and sheets. [Table 4]

[0034] In certain examples, the disclosed alloys include copper (Cu) in an amount of about 0.05% to about 1.2% (e.g., about 0.1% to about 1.2%, about 0.2% to about 1.1%, about 0.3% to about 1.0%, about 0.4% to about 1.0%, about 0.6% to about 1.1%, about 0.65% to about 0.9%, about 0.7% to about 1.0%, or about 0.6% to about 0.7%) based on the total weight of the alloy. For example, the alloy may be about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0.09%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.22%, about 0.23%, about 0.24%, about 0.25%, about 0.26%, about 0.27%, about 0.28%, about 0.29%, about 0.30%, about 0.32%, about 0.34%, about 0.36%, about 0.38%, about 0.39%, about 0.40%, about 0.41%, about 0.42%, about 0.43%, about 0.44%, about 0.45%, about 0.46%, about 0.47%, about 0.48%, about 0.49%, about 0.50%, about 0.51%, about 0.52%, about 0.53%, about 0.54%, about 0.55%, about 0.56%, about 0.57%, about 0.58%, about 0.59%, about 0.60%, about 0.61%, about 0.62%, about 0.63%, about 0.64%, about 0.65%, about 0.66%, about 0.67%, about 0.68%, about 0.69%, about 0.70%, about 0.71%, about 0.72%, about 0.73%, about 0.74%, about 0.75%, about 0.76%, about 0.77%, about 0.78%, about 0.79%, about 0.80%, about 0.31%, approx. 0.32%, approx. 0.33%, approx. 0.34%, approx. 0.35%, approx. 0.36%, approx. 0.37%, approx. 0.38%, approx. 0.39%, approx. 0.4%, approx. 0.41%, approx. 0.42%, approx. 0.43%, approx. 0.44%, approx. 0.45%, approx. 0.46%, approx. 0.47%, approx. 0.48%, approx. 0.49%, approx. 0.5%, approx. 0.51%, approx. 0.52%, approx. 0.53%, approx. 0.54%, approx. 0.55%, approx. 0.56%, approx. 0.57%, approx. 58%, 0.59%, 0.6%, 0.61%, 0.62%, 0.63%, 0.64%, 0.65%, 0.66%, 0.67%, 0.68%, 0.69%, 0.7%, 0.71%, 0.72%, 0.73%, 0.74%, 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.8%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85% , about 0.86%, about 0.87%, about 0.88%, about 0.89%, about 0.9%, about 0.9%, about 0.91%, about 0.92%, about 0.93%, about 0.94%, about 0.95%, about 0.96%, about 0.97%, about 0.98%, about 0.99%, about 1.0%, about 1.01%, about 1.02%, about 1.03%, about 1.04%, about 1.05%, about 1.06%, about 1.07%, about 1.08%, about 1.09%, about or about 1.1% Cu, all expressed as weight percent.

[0035] In certain examples, the disclosed alloys include silicon (Si) in an amount from about 0.6% to about 1.5% (e.g., from about 0.7% to about 1.3%, from about 0.8% to about 1.2%, from about 0.9% to about 1.1%, from about 0.6% to about 0.9%, from about 0.9% to about 1.1%, or from about 1.0% to about 1.1%) based on the total weight of the alloy. For example, the alloy may have an average molecular weight of about 0.6%, about 0.61%, about 0.62%, about 0.63%, about 0.64%, about 0.65%, about 0.66%, about 0.67%, about 0.68%, about 0.69%, about 0.7%, about 0.71%, about 0.72%, about 0.73%, about 0.74%, about 0.75%, about 0.76%, about 0.77%, about 0.78%, about 0.79%, about 0.8%, about 0.81%, about 0.82%, about 0.83%, about 0.84%, about 0.85%, about 0.86%, about 0.87%, about 0.88%, about 0.89%, about 10 ... %, about 0.86%, about 0.87%, about 0.88%, about 0.89%, about 0.9%, about 0.9%, about 0.91%, about 0.92%, about 0.93%, about 0.94%, about 0.95%, about 0.96%, about 0.97%, about 0.98%, about 0.99%, about 1.0%, about 1.01%, about 1.02%, about 1.03%, about 1.04%, about 1.05%, about 1.06%, about 1.07%, about 1.08%, about 1.09%, or about 1.1% Si, all expressed as weight percent.

[0036] In certain examples, the disclosed alloys include magnesium (Mg) in an amount of about 0.3% to about 1.3% (e.g., about 0.4% to about 1.25%, about 0.5% to about 1.2%, about 0.7% to about 1.1%, about 0.8% to about 1.25%, about 1.1% to about 1.25%, about 1.1% to about 1.2%, about 1.0% to about 1.2%, about 1.05% to about 1.3%, or about 1.15% to about 1.3%) based on the total weight of the alloy. For example, the alloy may be about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.71%, about 0.72%, about 0.73%, about 0.74%, about 0.75%, about 0.76%, about 0.77%, about 0.78%, about 0.79%, about 0.8%, about 0.81%, about 0.82%, about 0.83%, about 0.84%, about 0.85%, about 0.86%, about 0.87%, about 0.88%, about 0.89%, about 0.9%, about 0.91%, about 0.92%, about 0.93%, about 0.94%, about 0.95%, about 0.96%, about 0.97%, about 0.98%, about 0.99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 117%, about 118%, about 119%, about 120%, about 121%, about 122%, about 123%, about 124%, about 125%, about 126%, about 127%, about 128%, about 129%, about 130%, about 131%, about 132%, about 133%, about 134%, about 135%, about 136%, about 137%, about 138%, about 139%, about 140%, about 141%, about 142%, about 143%, about 144%, about 1 0.94%, about 0.95%, about 0.96%, about 0.97%, about 0.98%, about 0.99%, about 1.0%, about 1.01%, about 1.02%, about 1.03%, about 1.04%, about 1.05%, about 1.06%, about 1.07%, about 1.08%, about 1.09%, about 1.1%, about 1.11%, about 1.12%, about 1.13%, about 1.14%, about 1.15%, about 1.16%, about 1.17%, about 1.18%, about 1.19%, or about 1.2% Mg, all expressed as % by weight.

[0037] In certain embodiments, the alloy comprises chromium (Cr) in an amount up to about 0.25% (e.g., from about 0% to about 0.25%, from about 0.03% to about 0.06%, from about 0.03% to about 0.19%, or from about 0.06% to about 0.1%) based on the total weight of the alloy.For example, the alloy may be about 0.001%, about 0.002%, about 0.003%, about 0.004%, about 0.005%, about 0.006%, about 0.007%, about 0.008%, about 0.059%, about 0.01%, about 0.011%, about 0.012%, about 0.013%, about 0.014%, about 0.015%, about 0.016%, about 0.017%, about 0.018%, about 0.019%, about 0.02%, about 0.021%, about 0.022%, about 0.023%, about 0.024%, about 0.025%, about 0.026%, about 0.027%, about 0.028% ,approx. 0.029%,approx. 0.03%,approx. 0.031%,approx. 0.032%,approx. 0.033%,approx. 0.034%,approx. 0.035%,approx. 0.036%,approx. 0.037%,approx. 0.038%,approx. 0.039%,approx. 0.04%,approx. 0.041%,approx. 0.042%,approx. 0.043%,approx. 0.044%,approx. 0.045%,approx. 0.046%,approx. 0.047%,approx. 0.048%,approx. 0.049%,approx. 0.05%,approx. 0.051%,approx. 0.052%,approx. 0.053%,approx. 0.054%,approx. 0.055%,approx. 0.056%,approx. 0.057% ,approx. 0.058%,approx. 0.059%,approx. 0.06%,approx. 0.061%,approx. 0.062%,approx. 0.063%,approx. 0.064%,approx. 0.065%,approx. 0.066%,approx. 0.067%,approx. 0.068%,approx. 0.069%,approx. 0.07%,approx. 0.071%,approx. 0.072%,approx. 0.073%,approx. 0.074%,approx. 0.075%,approx. 0.076%,approx. 0.077%,approx. 0.078%,approx. 0.079%,approx. 0.08%,approx. 0.081%,approx. 0.082%,approx. 0.083%,approx. 0.084%,approx. 0.085%,approx. 0.086% , about 0.087%, about 0.088%, about 0.089%, about 0.09%, about 0.09%, about 0.091%, about 0.092%, about 0.093%, about 0.094%, about 0.095%, about 0.096%, about 0.097%, about 0.098%, about 0.099%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.22%, about 0.23%, about 0.24%, or about 0.25% Cr, all expressed as weight percent. In some cases, Cr is absent (i.e., 0%) in the alloy. In some instances, Cr can control grain structure and inhibit grain growth and recrystallization.Higher amounts of Cr can provide higher formability and improved bendability in the age temper.

[0038] In certain examples, the alloy can include manganese (Mn) in an amount of up to about 0.35% (e.g., between about 0% and about 0.35%, between about 0.05% and about 0.18%, between about 0.1% and about 0.35%, or between about 0.1% and about 0.3%) based on the total weight of the alloy.For example, the alloy may be about 0.001%, about 0.002%, about 0.003%, about 0.004%, about 0.005%, about 0.006%, about 0.007%, about 0.008%, about 0.059%, about 0.01%, about 0.011%, about 0.012%, about 0.013%, about 0.014%, about 0.015%, about 0.016%, about 0.017%, about 0.018%, about 0.019%, about 0.02%, about 0.021%, about 0.022%, about 0.023%, about 0.024%, about 0.025%, about 0.026%, about 0.027%, about 0.028%, about 0.029%, about 0.03%, about 0.031%, approx. 0.032%, approx. 0.033%, approx. 0.034%, approx. 0.035%, approx. 0.036%, approx. 0.037%, approx. 0.038%, approx. 0.039%, approx. 0.04%, approx. 0.041%, approx. 0.042%, approx. 0.043%, approx. 0.044%, approx. 0.045%, approx. 0.04 6%, approx. 0.047%, approx. 0.048%, approx. 0.049%, approx. 0.05%, approx. 0.051%, approx. 0.052%, approx. 0.053%, approx. 0.054%, approx. 0.055%, approx. 0.056%, approx. 0.057%, approx. 0.058%, approx. 0.059%, approx. 0.06%, approx. 0.061%, approx. 0 .062%, approx. 0.063%, approx. 0.064%, approx. 0.065%, approx. 0.066%, approx. 0.067%, approx. 0.068%, approx. 0.069%, approx. 0.07%, approx. 0.071%, approx. 0.072%, approx. 0.073%, approx. 0.074%, approx. 0.075%, approx. 0.076%, approx. 0.077 %, approx. 0.078%, approx. 0.079%, approx. 0.08%, approx. 0.081%, approx. 0.082%, approx. 0.083%, approx. 0.084%, approx. 0.085%, approx. 0.086%, approx. 0.087%, approx. 0.088%, approx. 0.089%, approx. 0.09%, approx. 0.091%, approx. 0.092%, approx. The composition may contain about 0.093%, about 0.094%, about 0.095%, about 0.096%, about 0.097%, about 0.098%, about 0.099%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.22%, about 0.23%, about 0.24%, about 0.25%, about 0.26%, about 0.27%, about 0.28%, about 0.29%, about 0.3%, about 0.31%, about 0.32%, about 0.33%, about 0.34%, or about 0.35% Mn.In some cases Mn is absent from the alloy (i.e. 0%). All expressed in weight percent.

[0039] In certain embodiments, the alloy also includes iron (Fe) in an amount between about 0.1% and about 0.35% (e.g., between about 0.1% and about 0.3%, between about 0.1% and about 0.25%, between about 0.18% and about 0.25%, between about 0.2% and about 0.21%, or between about 0.15% and about 0.22%) based on the total weight of the alloy. For example, the alloy may include about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.22%, about 0.23%, about 0.24%, about 0.25%, about 0.26%, about 0.27%, about 0.28%, about 0.29%, or about 0.30% Fe. In some cases, Fe is absent (i.e., 0%) in the alloy. All expressed in weight percent.

[0040] In certain embodiments, the alloy includes zirconium (Zr) in an amount up to about 0.25% (e.g., about 0% to about 0.2%, about 0.01% to about 0.25%, about 0.01% to about 0.15%, about 0.01% to about 0.1%, or about 0.02% to about 0.09%) based on the total weight of the alloy. For example, the alloy may include about 0.001%, about 0.002%, about 0.003%, about 0.004%, about 0.005%, about 0.006%, about 0.007%, about 0.008%, about 0.009%, about 0.01%, about 0.02%, about 0.03%, about 0.04%, about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0. ... %, about 0.09%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.22%, about 0.23%, about 0.24%, or about 0.25% Zr. In certain embodiments, Zr is absent (i.e., 0%) in the alloy. All expressed in weight percent. In some instances, Zr can control grain structure and prevent grain growth and recrystallization. Higher amounts of Zr can provide higher formability and improved bendability, even in T4 and aged tempers.

[0041] In certain embodiments, the alloys described herein include zinc (Zn) in an amount up to about 1.0% (e.g., about 0% to about 1.0%, about 0.001% to about 0.3%, about 0.005% to about 0.09%, about 0.004% to about 0.3%, about 0.03% to about 0.2%, or about 0.06% to about 0.1%) based on the total weight of the alloy.For example, the alloy may be about 0.001%, about 0.002%, about 0.003%, about 0.004%, about 0.005%, about 0.006%, about 0.007%, about 0.008%, about 0.009%, about 0.01%, about 0.011%, about 0.012%, about 0.013%, about 0.014%, about 0.015%, about 0.016%, about 0.017%, about 0.018%, about 0.019%, about 0.02%, about 0.021%, about 0.022%, about 0.023%, about 0.024%, about 0.025%, about 0.026%, about 0.027%, about 0.028%, about 0.029%, about 0.030%, about 0.031%, about 0.032%, about 0.033%, about 0.034%, about 0.035%, about 0.036%, about 0.037%, about 0.038%, about 0.039%, about 0.040%, about 0.041%, about 0.042%, about 0.043%, about 0.044%, about 0.045%, about 0.046%, about 0.047%, about 0.048%, about 0.049%, about 0.050%, about 0.050%, about 0.051%, about 0.052%, about 0.053%, about 0.054%, about 0.055%, about 0.056%, about 0.057%, about 0.058%, about 0.059%, about 0.060%, about 0.061%, about 0.062%, about .029%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.2%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.3%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35% ,approx. 0.36%,approx. 0.37%,approx. 0.38%,approx. 0.39%,approx. 0.4%,approx. 0.41%,approx. 0.42%,approx. 0.43%,approx. 0.44%,approx. 0.45%,approx. 0.46%,approx. 0.47%,approx. 0.48%,approx. 0.49%,approx. 0.50%,approx. 0.51%,approx. 0.52%,approx. 0.53%,approx. 0.54%,approx. 0.55%,approx. 0.56%,approx. 0.57%,approx. 0.58%,approx. 0.59%,approx. 0.6%,approx. 0.61%,approx. 0.62%,approx. 0.63%,approx. 0.64%,approx. 0.65%,approx. 0.66%,approx. 0.67%,approx. 0.68%,approx. 69%, about 0.7%, about 0.71%, about 0.72%, about 0.73%, about 0.74%, about 0.75%, about 0.76%, about 0.77%, about 0.78%, about 0.79%, about 0.8%, about 0.81%, about 0.82%, about 0.83%, about 0.84%, about 0.85%, about 0.86%, about 0.87%, about 0.88%, about 0.89%, about 0.90%, about 0.91%, about 0.92%, about 0.93%, about 0.94%, about 0.95%, about 0.96%, about 0.97%, about 0.98%, about 0.99%, or about 1.0% Zn. In some cases, Zn is absent (i.e., 0%) in the alloy. All expressed in weight percent.In certain embodiments, Zn can be beneficial to the forming, including bending and reducing bending anisotropy, of foil, sheet, and shade products.

[0042] In certain embodiments, the alloy comprises titanium (Ti) in an amount of up to about 0.3% (e.g., from about 0% to about 0.3%, from about 0.01% to about 0.25%, from about 0.05% to about 0.2%, or up to about 0.1%) based on the total weight of the alloy. For example, the alloy may be about 0.01%, about 0.011%, about 0.012%, about 0.013%, about 0.014%, about 0.015%, about 0.016%, about 0.017%, about 0.018%, about 0.019%, about 0.02%, about 0.025%, about 0.03%, about 0.035%, about 0.04%, about 0.045%, about 0.05%, about 0.055%, 0.06%, about 0.065%, about 0.07%, about 0.075%, about 0.08% , about 0.085%, about 0.09%, about 0.095%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.22%, about 0.23%, about 0.24%, about 0.25%, about 0.26%, about 0.27%, about 0.28%, about 0.29%, or about 0.3% Ti. In certain embodiments, Ti is absent (i.e., 0%) in the alloy. All expressed in weight percent.

[0043] In certain embodiments, the alloy includes nickel (Ni) in an amount of up to about 0.04% (e.g., 0% to about 0.02%, about 0.01% to about 0.03%, about 0.03% to about 0.04%) based on the total weight of the alloy. For example, the alloy includes about 0.001%, about 0.005%, about 0.01%, about 0.011%, about 0.012%, about 0.013%, about 0.014%, about 0.015%, about 0.016%, about 0.017%, about 0.018%, about 0.019%, about 0.02%, about 0.021%, about 0.022%, about 0.023%, about 0.024% , about 0.025%, about 0.026%, about 0.027%, about 0.028%, about 0.029%, about 0.03%, about 0.031%, about 0.032%, about 0.033%, about 0.034%, about 0.035%, about 0.036%, about 0.037%, about 0.038%, about 0.039%, or about 0.04% Ni. In certain embodiments, Ni is absent (i.e., 0%) in the alloy. All expressed in weight percent.

[0044] Optionally, the alloy composition may further include other trace elements, sometimes referred to as impurities, in amounts of about 0.05% or less, about 0.04% or less, about 0.03% or less, about 0.02% or less, or about 0.01% or less, respectively. These impurities may include, but are not limited to, V, Ga, Ca, Hf, Sr, Sc, Sn, or combinations thereof. Thus, V, Ga, Ca, Hf, Sr, Sc, or Sn may be present in the alloy in amounts of about 0.05% or less, about 0.04% or less, about 0.03% or less, about 0.02% or less, or about 0.01% or less. In certain embodiments, the sum of all impurities does not exceed about 0.15% (e.g., 0.1%). All expressed in weight percent. In certain embodiments, the remaining percentage of the alloy is aluminum.

[0045] Continuous Heat Treatment Process Certain aspects and features of the present disclosure relate to a continuous heat treatment process in which a metal strip is solutionized, rapidly cooled, heat spiked at an elevated temperature (e.g., a temperature in the range of 120° C. to 300° C.), and coiled, as described below. In certain embodiments, the metal strip is a heat treatable alloy, such as a heat treatable aluminum alloy. In certain embodiments, the heat spiked metal strip is cooled before or after coiling. In certain embodiments, the heat spiked metal strip is only allowed to cool naturally before or after coiling. In some embodiments, the coil can be cooled (e.g., using cooling fan(s)) after coiling at the end of the continuous heat treatment process. In certain embodiments, the metal strip itself can be prepared from scalping, homogenization, hot rolling, optionally batch annealing, and cold rolling of a cast ingot.

[0046] The continuous heat treatment process can be operated at a particular line speed. For example, the continuous heat treatment process can be operated at a line speed of more than 5 meters / min, e.g., more than 10 meters / min, more than 20 meters / min, more than 25 meters / min, more than 30 meters / min, more than 40 meters / min, more than 50 meters / min, more than 60 meters / min, more than 70 meters / min, more than 80 meters / min, more than 90 meters / min, more than 100 meters / min, 10 meters / min to 100 meters / min, 20 meters / min to 80 meters / min, 30 meters / min to 70 meters / min, or 40 meters / min to 60 meters / min.

[0047] solution treatment Solutionizing can provide a solution of the desired amounts of alloying elements present in a particular alloy (eg, aluminum in solid solution). In some embodiments, the solutionizing step can include heating the metal strip (e.g., a plate, a shade, a sheet, or a foil) from room temperature to a temperature of about 400°C to about 590°C (e.g., about 450°C to about 575°C, about 400°C to about 525°C, about 450°C to about 510°C, about 520°C to about 590°C, about 520°C to about 580°C, about 520°C to about 560°C, about 530°C to about 570°C, about 545°C to about 575°C, about 550°C to about 570°C, about 555°C to about 565°C, about 540°C to about 560°C, about 540°C to about 575°C, about 560°C to about 580°C, about 550°C to about 575°C, about 540°C, about 550°C, about 560°C, or about 570°C).

[0048] In certain embodiments, the strip can be immersed at temperature for a period of time. In certain aspects, the strip can be immersed for a period of time (e.g., up to about 5 minutes, from about 10 seconds to about 5 minutes, inclusive, from about 1 second to about 3 minutes, or from about 5 seconds to about 5 minutes). For example, the strip can be immersed at a temperature (e.g., from about 525° C. to about 590° C.) for less than 20 seconds, less than 25 seconds, less than 30 seconds, less than 35 seconds, less than 40 seconds, less than 45 seconds, less than 50 seconds, less than 55 seconds, less than 60 seconds, less than 65 seconds, less than 70 seconds, less than 75 seconds, less than 80 seconds, less than 85 seconds, less than 90 seconds, less than 95 seconds, less than 100 seconds, less than 105 seconds, less than 110 seconds, less than 115 seconds, less than 120 seconds, less than 125 seconds, less than 130 seconds, less than 135 seconds, less than 140 seconds, less than 145 seconds, or less than 150 seconds, or less than 5 minutes, or any time in between.

[0049] In certain aspects, the solutionizing can be carried out in a continuous process, such as a continuous heat treatment line. In some embodiments, the continuous process (e.g., a continuous heat treatment line) can have a particular line speed.

[0050] In certain embodiments, the solutionizing step is performed on the metal strip immediately after the hot rolling and / or cold rolling steps. In other embodiments, the solutionizing step is performed on the metal strip after the hot rolling and / or cold rolling steps (e.g., after more than 48 hours). In certain embodiments, the solutionizing step is performed after the annealing and cold rolling steps.

[0051] rapid cooling Without being bound by theory, the metal strip can be cooled very rapidly to lock the solute elements and excess vacancies into the metal (e.g., aluminum) matrix of the metal strip. Thus, in some embodiments, after solutionization, the metal strip can be cooled rapidly to reduce the temperature of the metal strip. In some embodiments, the transfer time from the solutionization furnace to the cooling medium is very short (e.g., less than 1 second, less than 2 seconds, less than 3 seconds, less than 5 seconds, less than 10 seconds, less than 15 seconds, less than 20 seconds, less than 25 seconds, less than 30 seconds, less than 35 seconds, less than 40 seconds, less than 45 seconds, less than 50 seconds, less than 55 seconds, less than 1 minute, less than 2 minutes, less than 3 minutes, less than 4 minutes, less than 5 minutes, or less than 10 minutes). The time of transfer of the solutionized metal starts from the moment the furnace door starts to open and proceeds to the point where the aluminum alloy is completely immersed and submerged. If the transfer time exceeds the prescribed time limit, incomplete solutionization can occur, which means non-uniform metallurgical and mechanical conditions of the particular alloy.

[0052] In certain embodiments, after solutionizing, the metal strip can be cooled in a rapid cooling step based on the gauge selected at a rate that can vary between about 1° C. / s and 400° C. / s. For example, the rate of rapid cooling can be about 50° C. / s to about 375° C. / s, about 60° C. / s to about 375° C. / s, about 70° C. / s to about 350° C. / s, about 80° C. / s to about 325° C. / s, about 90° C. / s to about 300° C. / s, about 100° C. / s to about 275° C. / s, about 125° C. / s to about 250° C. / s, about 150° C. / s to about 225° C. / s, about 175° C. / s to about 200° C. / s, about 10° C. / s to about 125° C. / s, or about 20° C. / s to about 125° C. / s. In some embodiments, the metal strip can be rapidly cooled to a temperature of less than 100°C, e.g., less than 90°C, less than 80°C, less than 70°C, less than 60°C, less than 50°C, less than 45°C, less than 40°C, less than 35°C, less than 30°C, less than 25°C, less than 20°C, less than 15°C, from about 20°C to about 80°C, from about 20°C to about 70°C, from about 20°C to about 60°C, from about 25°C to about 50°C, from about 25°C to about 40°C, to about 20°C, to about 25°C, to about 30°C, to about 35°C, to about 40°C, to about 45°C, or to about 50°C.

[0053] In certain embodiments, the metal strip can be rapidly cooled with a liquid (e.g., water) and / or gas, or another selected cooling medium. In certain embodiments, the metal strip is rapidly cooled with air. In certain embodiments, the metal strip can be rapidly cooled with water.

[0054] Thermal Spikes The metal strip can be subjected to a heat spike treatment at an elevated temperature. As described herein, the use of a higher heat spike temperature than previously disclosed in the art has helped achieve the unexpected advantages of the present disclosure. In some embodiments, the heat spike temperature (i.e., the peak temperature to which the metal strip is exposed, not necessarily the temperature of the metal strip itself) is in the range of about 100°C to about 300°C, e.g., about 120°C to about 300°C, about 150°C to about 300°C, about 170°C to about 280°C, about 180°C to about 270°C, about 190°C to about 260°C, about 200°C to about 250°C, about 210°C to about 250°C, about 220°C to about 250°C, about 220°C to about 240°C, about 200°C, about 210°C, about 220°C, about 230°C, about 240°C, or about 250°C. In some embodiments, the metal strip itself reaches within 100° C., e.g., within 90° C., within 80° C., within 70° C., within 60° C., within 50° C., within 40° C., within 30° C., within 20° C., within 10° C., within 5° C., or within 1° C., of the thermal spike temperature.

[0055] In some embodiments, the heat spike treatment is performed after the metal strip is solutionized and air cooled, hi some embodiments, the heat spike treatment can be performed at the same processing line speed as the solutionizing and rapid cooling, e.g., as part of a continuous heat treatment process.

[0056] Conventional 6XXX materials in T4 or T4P tempers contain numerous fine metastable clusters and zones uniformly distributed throughout the metal matrix. In conventional processes, during paint curing, some fine unstable clusters / zones redissolve into the metal matrix while others improve material strength by age hardening. The processes described herein allow alloy materials to exhibit improved aging response (hardness response). Without being bound by theory, it is believed that coiling and coil cooling after a thermal spike of 150°C-320°C, e.g., about 150°C-300°C, about 180°C-300°C, or about 150°C-225°C (e.g., in a long reheat furnace), form some of the clusters and zones, facilitating the precipitation process during coil cooling.

[0057] The period of time that the temperature is maintained at the peak heat spike temperature can range from 0 to any time practical in the circumstances. In some embodiments, the heat spike treatment is performed at the processing line speed of the continuous heat treatment process (e.g., in a long furnace). For example, the processing line speed and the heat spike treatment speed can be performed at a speed of about 1 meter / min to about 120 meters / min, e.g., about 2 meters / min to about 110 meters / min, about 5 meters / min to about 100 meters / min, about 10 meters / min to about 600 meters / min, about 20 meters / min to about 500 meters / min, about 25 meters / min to about 500 meters / min, about 30 meters / min to about 400 meters / min, about 40 meters / min to about 350 meters / min, about 50 meters / min to about 300 meters / min, or about 100 meters / min to about 250 meters / min. In practice, the period is typically from 0 up to about 5 minutes, e.g., from about 1 second to about 5 minutes, from about 2 seconds to about 4 minutes, from about 3 seconds to about 3 minutes, from about 5 seconds to about 2 minutes, from about 7 seconds to about 1 minute, or from about 10 seconds to about 30 seconds.

[0058] In some embodiments, the heating rate at which the thermal spike treatment is performed (i.e., the rate at which the temperature of the metal strip is increased) is from about 1° C. / min to about 50° C. / sec (e.g., from about 1° C. / sec to about 40° C. / sec, from about 2° C. / sec to about 40° C. / sec, from about 3° C. / sec to about 35° C. / sec, from about 3° C. / sec to about 30° C. / sec, from about 5° C. / sec to about 30° C. / sec, from about 10° C. / sec to about 25° C. / sec, or from about 2° C. / sec to about 10° C. / sec).

[0059] In some embodiments, the heat spike treatment is carried out in a reheat furnace, such as a continuous reheat furnace. In some embodiments, the heat spike treatment is carried out in a long reheat furnace. For example, the furnace can have an effective length (i.e., the length over which the metal strip is heated in a continuous process) of at least 10 meters, such as at least 20 meters, at least 25 meters, at least 30 meters, at least 40 meters, at least 50 meters, at least 60 meters, at least 70 meters, at least 80 meters, at least 90 meters, or at least 100 meters. Without being limiting of the disclosure, this can allow for increased line speeds and / or heat spike times.

[0060] Statute of Limitations In some embodiments, the metal strip is not subjected to an aging process, hi some embodiments, a thermal spike of the metal strip in combination with coiling the metal strip and / or cooling the metal strip can take the place of age hardening.

[0061] cooling In some embodiments, the metal strip can be cooled after the heat spike treatment. In some embodiments, this cooling can occur after coiling. In other embodiments, this cooling can occur before coiling. Also, in some embodiments, cooling can occur before and / or after coiling. For example, in some embodiments, the metal strip can be air-cooled, for example, using at least one fan. In some embodiments, the metal strip is only naturally cooled (e.g., during the passage of the strip between the heat spike treatment and coiling), meaning that there is no equipment or process used to cool the metal strip before coiling. For example, the metal strip may be exposed only to ambient conditions (e.g., at the line speed of a continuous heat treatment process) before coiling. In some embodiments, the metal strip is only naturally cooled after coiling. As described herein, natural cooling (e.g., only exposure to ambient conditions before cooling) is not included in the terms "cooling" or "cooled" as previously used in the art. In some embodiments, the cooling or natural cooling can be performed until the metal strip reaches ambient temperature.

[0062] In some embodiments, the metal strip and / or coiled metal strip can be cooled or naturally cooled at a rate of about 60° C. / hour or less (e.g., about 50° C. / hour or less, about 40° C. / hour or less, about 30° C. / hour or less, about 20° C. / hour or less, about 10° C. / hour or less, about 5° C. / hour or less, about 3° C. / hour or less, about 2.5° C. / hour or less, about 2° C. / hour or less, about 1.5° C. / hour or less, about 1° C. / hour or less, or about 0.8° C. / hour or less).

[0063] Method for preparing metal strip In certain embodiments, the disclosed metal (e.g., alloy) strip compositions are products of the disclosed methods. Without limiting the disclosure, alloy properties, such as aluminum alloy properties, are determined in part by the formation of the microstructure during preparation of the alloy. In certain embodiments, the preparation method for the alloy composition can affect or even determine whether the alloy has suitable properties for a desired application.

[0064] The metal (e.g., alloy) strip described herein can be cast into ingots using a casting process. For example, the casting process can include a direct chill (DC) casting process. In another example, the casting process can include a continuous casting process. The cast ingots can then undergo further processing steps. In one non-limiting example, the processing method includes scalping, homogenization, hot rolling, optional batch annealing, and cold rolling before the above-mentioned solutionizing, rapid cooling, heat spike treatment, and coiling, followed by cooling (e.g., fan cooling after coiling).

[0065] Homogenization In some embodiments, the homogenization step can include one-step homogenization or two-step homogenization. In one example of the homogenization step, an ingot prepared from an alloy composition described herein is heated to a peak metal temperature (PMT) of about or at least about 500°C (e.g., at least 520°C, at least 530°C, at least 540°C, at least 550°C, at least 560°C, at least 570°C, or at least 580°C). For example, the ingot can be heated to a temperature of about 520°C to about 580°C, about 530°C to about 575°C, about 535°C to about 570°C, about 540°C to about 565°C, about 545°C to about 560°C, about 530°C to about 560°C, or about 550°C to about 580°C. In some cases, the heating rate to the peak metal temperature can be about 100° C. / hour or less, 75° C. / hour or less, 50° C. / hour or less, 40° C. / hour or less, 30° C. / hour or less, 25° C. / hour or less, 20° C. / hour or less, 15° C. / hour or less, or 10° C. / hour or less. In other cases, the heating rate to the peak metal temperature can be about 10° C. / minute to about 100° C. / minute (e.g., about 10° C. / minute to about 90° C. / minute, about 10° C. / minute to about 70° C. / minute, about 10° C. / minute to about 60° C. / minute, about 20° C. / minute to about 90° C. / minute, about 30° C. / minute to about 80° C. / minute, about 40° C. / minute to about 70° C. / minute, or about 50° C. / minute to about 60° C. / minute).

[0066] The ingot is then soaked (i.e., held at the indicated temperature) for a period of time. According to one non-limiting example, the ingot is soaked for up to about 8 hours (e.g., from about 5 seconds to 8 hours, or from about 30 minutes to about 8 hours, inclusive). For example, the ingot can be soaked at a temperature of at least 500° C. for 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, or any time therebetween.

[0067] In another example of the homogenization step, a two-step homogenization is performed, in which an ingot prepared from an alloy composition described herein is heated to achieve a first temperature of about or at least about 480°C to about 520°C. For example, the ingot can be heated to a first temperature of about 480°C, 490°C, 500°C, 510°C, or 520°C. In certain embodiments, the heating rate to the first temperature can be about 10°C / min to about 100°C / min (e.g., about 10°C / min to about 90°C / min, about 10°C / min to about 70°C / min, about 10°C / min to about 60°C / min, about 20°C / min to about 90°C / min, about 30°C / min to about 80°C / min, about 40°C / min to about 70°C / min, or about 50°C / min to about 60°C / min). In other embodiments, the heating rate to the first temperature can be from about 10° C. / hour to about 100° C. / hour (e.g., from about 10° C. / hour to about 90° C. / hour, from about 10° C. / hour to about 70° C. / hour, from about 10° C. / hour to about 60° C. / hour, from about 20° C. / hour to about 90° C. / hour, from about 30° C. / hour to about 80° C. / hour, from about 40° C. / hour to about 70° C. / hour, or from about 50° C. / hour to about 60° C. / hour).

[0068] The ingot is then soaked for a period of time. In some cases, the ingot is soaked for up to about 6 hours (e.g., 5 seconds to 6 hours, or 30 minutes to 6 hours, inclusive). For example, the ingot can be soaked at a temperature of about 480° C. to about 520° C. for 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, or 6 hours, or any time therebetween.

[0069] In the second step of the two-step homogenization process, the ingot can be further heated from the first temperature to a second temperature greater than about 520°C (e.g., greater than 520°C, greater than 530°C, greater than 540°C, greater than 550°C, greater than 560°C, greater than 570°C, or greater than 580°C). For example, the ingot can be heated to a second temperature of about 520°C to about 580°C, about 530°C to about 575°C, about 535°C to about 570°C, about 540°C to about 565°C, about 545°C to about 560°C, about 530°C to about 560°C, or about 550°C to about 580°C. The heating rate to the second temperature can be about 10° C. / min to about 100° C. / min (e.g., about 20° C. / min to about 90° C. / min, about 30° C. / min to about 80° C. / min, about 10° C. / min to about 90° C. / min, about 10° C. / min to about 70° C. / min, about 10° C. / min to about 60° C. / min, about 40° C. / min to about 70° C. / min, or about 50° C. / min to about 60° C. / min).

[0070] In other embodiments, the heating rate to the second temperature can be from about 10° C. / hour to about 100° C. / hour (e.g., from about 10° C. / hour to about 90° C. / hour, from about 10° C. / hour to about 70° C. / hour, from about 10° C. / hour to about 60° C. / hour, from about 20° C. / hour to about 90° C. / hour, from about 30° C. / hour to about 80° C. / hour, from about 40° C. / hour to about 70° C. / hour, or from about 50° C. / hour to about 60° C. / hour).

[0071] The ingot is then soaked for a period of time. In some cases, the ingot is soaked for up to about 6 hours (e.g., 5 seconds to 6 hours, or 30 minutes to 6 hours, inclusive). For example, the ingot can be soaked at a temperature of about 520° C. to about 580° C. for 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, or 6 hours, or any time therebetween.

[0072] Hot rolling In some embodiments, the homogenization step can be followed by a hot rolling step. In certain cases, the ingot is laid down and hot rolled at an inlet temperature range of about 380°C to about 540°C. For example, the inlet temperature can be, for example, about 505°C, 510°C, 515°C, 520°C, 525°C, 530°C, 535°C, or 540°C. In certain cases, the hot rolling outlet temperature can be in the range of about 230°C to about 420°C (e.g., about 330°C to about 370°C). For example, the hot rolling exit temperature can be about 255°C, 260°C, 265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, or 380°C, and can be combined with any of the above entrance temperatures.

[0073] In certain cases, the ingot is hot rolled to about 2 mm to about 15 mm thickness gauge (e.g., about 5 mm to about 12 mm thickness gauge), which may be referred to as a sheath. For example, the ingot can be hot rolled to about 4 mm thickness gauge, about 5 mm thickness gauge, about 6 mm thickness gauge, about 7 mm thickness gauge, about 8 mm thickness gauge, about 9 mm thickness gauge, about 10 mm thickness gauge, about 11 mm thickness gauge, about 12 mm thickness gauge, about 13 mm thickness gauge, about 14 mm thickness gauge, or about 15 mm thickness gauge. In certain cases, the ingot can be hot rolled to a gauge greater than 15 mm thick (i.e., plate). In other cases, the ingot can be hot rolled to a gauge less than 4 mm (i.e., sheet). In some aspects, the hot rolled coil can be batch annealed before cold rolling in some cases. In certain embodiments, annealing can also occur after the first or second cold pass and before the final cold pass.

[0074] Cold rolling In some embodiments, the hot rolling step can be followed by a cold rolling step. In certain embodiments, the rolled product from the hot rolling step can be cold rolled into a sheet (e.g., less than about 4.0 mm). In certain embodiments, the rolled product is cold rolled to a thickness of 0.6 mm to 1.0 mm, 1.0 mm to 3.0 mm, or 3.0 mm to 4.0 mm. In certain embodiments, the alloy is cold rolled to about 3.5 mm or less, 3 mm or less, 2.5 mm or less, 2 mm or less, 1.5 mm or less, or 1 mm or less. For example, the rolled product can be cold rolled to about 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, or 3.0 mm.

[0075] The above-described process aspects can be used to produce metal strips as described above. Additionally, as described, the metal strips can be processed using the disclosed continuous heat treatment processes to produce heat treated articles. In some aspects, the entire process of producing the metal strip and heat treating the metal strip is continuous. The metal strips can then be subjected to the described heat treatment process. EXAMPLES

[0076] These illustrative examples are provided to introduce the reader to the general subject matter discussed herein and are not intended to limit the scope of the disclosed concepts. In the following sections, various additional features and examples are described with reference to the drawings, in which like numbers indicate like components. Also, directional descriptions are used to describe the exemplary embodiments, but as with the exemplary embodiments, should not be used to limit the disclosure. Elements included in the examples herein may not be drawn to scale.

[0077] Example 1 A direct chill cast ingot of an alloy containing 0.62 wt% Mg, 0.75 wt% Si, 0.21 wt% Cu, 0.13 wt% Mn, 0.2 wt% Fe and 0.02 wt% Ti was scalped, homogenized, hot and cold rolled to a final 0.9 mm gauge. The coiled cold rolled strip (Example 1) was solution heat treated at 540°C-575°C, rapidly cooled to below 50°C and thermally spiked in a furnace set at 220°C in a continuous process with the strip moving at 60 meters / min prior to coiling. There was no intentional cooling between the thermal spike and coiling at the end of the process (i.e. only natural). The strip was sampled prior to coiling at the flying shear position of the line and after cooling on the finishing line.

[0078] Samples taken before and after coiling were tested after a 6 day continuous annealing solution heat treatment ("CASH") using ASTM samples in as-is and paint bake conditions (2%+20 min at 185°C - referred to as T8X). Table 5 shows that the transverse yield strengths of sheet samples taken at flying shear and before coiling were 117 and 229 MPa for as-is and paint bake tempers, respectively, which are only slightly higher than typical values ​​expected from this alloy. However, the yield strength (YS) values ​​were higher for both tempers for the coil cooled samples, which is quite surprising since conventional products coiled at similar temperatures without a thermal spike do not exhibit such high properties. Such products are typically produced by subjecting the coil in the T4 temper to a separate batch aging heat treatment. Without being bound by theory, it is believed that the disclosed thermal spiking process accelerates the age hardening process during coil cooling.

[0079] [Table 5]

[0080] Examples 2 to 5 Direct chill cast ingots of four different alloys with compositions shown in Table 6 were scalped, homogenized, and hot and cold rolled to final gauge. The cold rolled strip in coils as in Example 1 was solution heat treated at 540°C-575°C, rapidly cooled to below 50°C, and thermally spiked in a furnace set at 250°C in a continuous process where the strip traveled at 60 meters / min prior to coiling at the end of the line. The strip was sampled prior to coiling at the flying shear position of the line and after cooling at the finishing line.

[0081] [Table 6]

[0082] Samples of Examples 2-5 taken before and after coiling were tested after several days in the cache in the as-is and T8X (2%+20min at 185°C) conditions, except for coiled Example 3, which was tested using the JIS samples and (2%+20min at 170°C) paint bake temper. Table 7 summarizes the tensile properties of the samples of Examples 2-5 taken at the flying shear and finishing lines. Table 7 shows that all four alloys exhibit significantly higher strength in the coil cooled samples as opposed to the flying shear samples before coil cooling, confirming the results of Example 1.

[0083] [Table 7]

[0084] Examples 6 to 8 Similar to Examples 2-5, three cold-rolled coils of alloy Ex.4 were solutionized on a continuous heat treatment line, heat-spiked in the range of 200-250°C, and coiled at the end of the line without any intentional cooling after the heat spike (i.e., only natural air cooling). Samples of Examples 6-8 obtained with a flying shear before coiling and coiled from the finishing line were tested in both as-is and T8X temper using ASTM samples. The results of this testing, as summarized in Table 8, show that the heat-spiked and coil-cooled samples exhibit higher strength compared to the flying shear samples, confirming the effect of the heat spike and the results of the previous examples.

[0085] The same coils of Examples 6-8 listed in Table 8 were re-solutioned in the same manner as the first, but with the reheaters set in automatic mode at 100°C and 150°C, respectively. The results from the re-solutioned coils are summarized in Table 9 and show that increasing the heat spike temperature results in higher strength, but the extent of the increase is less than that seen at >200°C. As shown in these results, the heat spike temperature has a significant effect on the strength of the coil-cooled samples. This observation indicates that with proper selection of alloys and heat temperatures, it is possible to produce different combinations of tensile properties without the need for an additional batch aging process.

[0086] [Table 8]

[0087] [Table 9]

[0088] Examples 9-10 The objectives of this test were firstly to investigate the effect of heating rate during a thermal spike with varying line speed (52m / min vs 41m / min) on the strength of AA6111 coils and secondly to compare the tensile properties of AA6111 with typical 5xxx alloys supplied in the H3X temper.

[0089] A pair of 2 mm gauge cold rolled coils (Examples 9 and 10) of AA6111 alloy containing 0.76 wt% Cu, 0.74 wt% Mg, 0.66 wt% Si, 0.27 wt% Fe and 0.74 wt% Mn were solutionized between 520-560°C, rapidly cooled below 50°C, thermally spiked in a furnace at 250°C and then coiled at the end of the continuous process. The coils of Examples 9 and 10 were heat treated at 52 meters / min and 41 meters / min, respectively. Samples were obtained from each coil on the finishing line and tested using ASTM samples in both the as-is and T8X tempers. The results of this testing are summarized in Table 10. Both coils processed at the two line speeds showed very similar properties in both T4 and T8X tempers, suggesting that there is no significant effect on tensile properties from changes in line speed ranging from 41 m / min to 52 m / min strip speed. The higher strength in the T4 temper could potentially be used for structural parts offering the possibility of downgauging or eliminating post-forming heat treatment.

[0090] [Table 10]

[0091] [Table 11]

[0092] Table 11 summarizes typical ASTM tensile properties for commonly used 5xxx alloys. YS, UTS and total elongation values ​​range from 190-290 MPa, 230 and 325 MPa, and 7-16%, respectively. The YS of the AA6111 coil in Table 10 is close to 5086-H34, and the total elongation is significantly higher. This suggests that the AA6111 material produced by the process described herein can replace 5086-H34 products while providing better total elongation. The same alloys can be produced at lower strengths by thermal spiking at lower temperatures to match the strength of other AA5xxx products. Different combinations of strengths can also be achieved by varying the alloy chemistry along with other process variables.

[0093] Thermal Spike AA6xxx does not exhibit any significant natural aging. This property provides a very attractive alternative to 5xxx products where high formability is required along with comparable strength and total elongation.

[0094] Example 11 Direct chilled cast ingots of AA6111 alloy containing 0.69 wt% Mg, 0.57 wt% Si, 0.51 wt% Cu, 0.19 wt% Mn, 0.23 wt% Fe and 0.01 wt% Ti were scalped, homogenized, hot and cold rolled to a final 2.3 mm gauge. The cold rolled strip in coils was solution heat treated between 525°C, rapidly cooled to below 50°C, thermally spiked in a furnace to heat the strip to about 190°C in a continuous process and uncoiled with a sidewall temperature of the coil width of about 135°C. The line speed was adjusted between 17-20 meters / min to ensure a strip temperature close to 190°C at the exit of the furnace. There was no intentional cooling between the thermal spike and coiling at the end of the process. The coil temperature was reduced from 135°C to 85°C at approximately 2.8°C / hr with further cooling to ambient at less than 2°C / hr. The coils were sampled 5 days after heat treatment and tested in as-is and in different paint bake tempers using ASTM samples.

[0095] Table 12 shows the average transverse ASTM tensile properties of sheet samples taken from the coil-cooled samples. The yield strength (YS) and ultimate tensile strength (UTS) of the coil-cooled samples were 277 MPa and 344 MPa, respectively, with a total elongation value of 17%. These properties are significantly different from AA6111 coils that are typically produced at coiling temperatures below 100°C, which typically exhibit a YS of 125 MPa, a UTS of 230 MPa, and a total elongation of 24%. The coil properties are characteristic of an aged temper obtained at 140°C for close to 50 hours of aging. Without wishing to be bound by theory, the thermal spike accelerates the hardening process during coil cooling. The alloys show a slight increase in strength when aged at high temperatures, with or without prestraining, as shown in Table 12. The thermal spike process produces coils that have strength at relatively short aging times and better elongation than would be expected from a typical batch annealing process, with an elongation of less than 14%.

[0096] [Table 12]

[0097] The foregoing description of embodiments, including the illustrated embodiment, has been presented only for purposes of illustration and description and is not intended to be exhaustive or limited to the precise form disclosed. Many modifications, adaptations and uses thereof will be apparent to those skilled in the art.

[0098] As used hereinafter, any reference to a series of embodiments should be understood disjunctively as a reference to each of those embodiments (e.g., "Embodiments 1-4" should be understood as "Embodiments 1, 2, 3, or 4").

[0099] Embodiment 1 is a process for producing a heat treated aluminum alloy, including casting metal strip; solutionizing the cast metal strip at a line speed to produce a solutionized metal strip; air cooling the solutionized metal strip to produce a cooled metal strip; heat spiking the cooled metal strip at a temperature between 150°C and 300°C continuously at a line speed to produce a heat spiked metal strip; and coiling the heat spiked metal strip to produce a coiled metal strip.

[0100] Embodiment 2 is the process of embodiment 1, further comprising cooling the heat spiked metal strip after the heat spike.

[0101] Embodiment 3 is the process of any of the embodiments, wherein cooling the heat-spiked metal strip comprises air-cooling the heat-spiked metal strip.

[0102] Embodiment 4 is the process of embodiment 1, where only natural cooling of the heat-spiked metal strip occurs between the heat spike and coiling.

[0103] Embodiment 5 is the process of any of the embodiments, wherein coiling the heat-spiked metal strip is performed continuously at the end of a continuous line.

[0104] Embodiment 6 is the process of any of the embodiments, wherein cooling the thermally spiked metal strip is at a rate of less than 10° C. / hour.

[0105] Embodiment 7 is the process of any of the embodiments, wherein cooling the thermally spiked metal strip is at a rate of less than 2° C. / hour.

[0106] Embodiment 8 is the process of any of the embodiments, wherein the coiling of the heat-spiked metal strip is at a temperature between 70 °C and 130 °C.

[0107] Embodiment 9 is the process of any of the embodiments, wherein coiling the heat-spiked metal strip is carried out at a temperature greater than 60° C.

[0108] Embodiment 10 is the process of any of the embodiments, wherein the line speed is at least 10 meters / minute.

[0109] Embodiment 11 is the process of any of the embodiments, wherein the line speed is from 10 meters / min to 120 meters / min.

[0110] Embodiment 12 is the process of any of the embodiments, wherein the thermal spike temperature is from 150°C to 280°C.

[0111] Embodiment 13 is the process of any of the embodiments, wherein the thermal spike temperature is from 200°C to 250°C.

[0112] Embodiment 14 is the process of any of the embodiments, wherein the casting of the metal strip comprises continuous casting.

[0113] Embodiment 15 is the process of any of the embodiments, wherein the casting of the metal strip comprises direct chill (DC casting).

[0114] Embodiment 16 is the process of any of the embodiments, further comprising homogenizing, hot rolling, and cold rolling the metal strip after casting and before solutionizing.

[0115] Embodiment 17 is the process of any of the embodiments, wherein the heat spiking of the cooled metal strip is carried out in a reheat furnace having a length of at least 12 meters.

[0116] Embodiment 18 is the process of any of the embodiments, wherein the solutionizing temperature is from about 480°C to about 590°C.

[0117] Embodiment 19 is the process of any of the embodiments, wherein air cooling the solutionized metal strip comprises cooling the solutionized metal strip to less than 50° C.

[0118] Embodiment 20 is a heat treated metal strip formed from the process according to any of the embodiments.

Claims

1. 1. A process for producing a heat treated aluminum alloy, comprising: Casting metal strip; solutionizing the cast metal strip at line speed to produce a solutionized metal strip; air cooling the solutionized metal strip to produce a cooled metal strip; heat spiking said cooled metal strip at a temperature of from 150° C. to 320° C. continuously at said line speed to produce a heat spiked metal strip; and coiling the heat spiked metal strip to produce a coiled metal strip.

2. The process of claim 1 further comprising cooling the coiled metal strip.

3. The process of claim 2 , wherein cooling the coiled metal strip comprises air cooling the thermally spiked metal strip.

4. 10. The process of claim 1, wherein only natural cooling of the heat-spiked metal strip occurs between the heat spike and coiling.

5. The process of claim 1 , wherein coiling the heat-spiked metal strip is performed continuously at the end of a continuous line.

6. 3. The process of claim 2, wherein the cooling of the coiled metal strip is at a rate of 10° C. / hour or less.

7. 2. The process of claim 1, wherein the coiling of the heat-spiked metal strip is at a temperature of from 110°C to 160°C.

8. 2. The process of claim 1, wherein the line speed is at least 10 meters / minute.

9. 2. The process of claim 1, wherein the line speed is from 10 meters / min to 120 meters / min.

10. 2. The process of claim 1, wherein the thermal spike temperature is from 150°C to 300°C.

11. 10. The process of claim 1, further comprising homogenizing, hot rolling, and cold rolling the metal strip prior to solutionizing.

12. 10. The process of claim 1, wherein the heat spiking of the cooled metal strip is carried out in a reheat furnace having a length of at least 12 meters.

13. The process of claim 1, wherein the solutionizing temperature is from about 480°C to about 590°C.

14. 2. The process of claim 1, wherein air cooling the solutionized metal strip comprises cooling the solutionized metal strip to less than 50°C.

15. 10. A heat treated metal strip formed from the process of claim 1.

Citation Information

Patent Citations

  • Heat treatment method for aluminum alloy sheet

    JP1998505131A

  • Method and apparatus for improving paint baking reaction and aging stability of aluminum sheet material, and products thereof

    JP2000503069A

  • Manufacturing method for aluminum alloy sheets

    JP2001513144A

  • A method for producing an aluminum alloy sheet with improved bending properties, and an aluminum alloy sheet produced by the same manufacturing method.

    JP2004527658A

  • Heat treatment process for aluminum alloy sheet

    JP2008106370A