Method for manufacturing sodium or potassium ion battery cells

A cost-effective manufacturing method for sodium or potassium ion batteries maintains the dehydrated phase of Prussian blue analogs within the cell casing, enhancing capacity and stability without requiring dry rooms, addressing the high costs and energy demands of conventional methods.

JP2024539669APending Publication Date: 2024-10-29ALTRIS AB
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024523166
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-20
Filing Date
2022-10-14
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Conventional methods for manufacturing sodium or potassium ion batteries using Prussian blue analogs require expensive dry rooms to prevent moisture exposure, which increases costs and energy demands.

Method used

A method involving a slurry of Prussian blue analog in a hydrated phase applied to a current collector, assembled with an anode and separator, then dried within the cell casing under controlled conditions to transition to a dehydrated phase, followed by electrolyte addition and sealing under inert conditions, all without the need for a dry room.

Benefits of technology

This method maintains the dehydrated phase of Prussian blue analog, preventing reversion and ensuring high capacity and stable cycling performance, while eliminating the need for costly dry rooms and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539669000001_ABST
    Figure 2024539669000001_ABST
Patent Text Reader

Abstract

The present disclosure generally relates to a method for producing a sodium or potassium ion battery that includes a Prussian blue analogue (PBA) as a positive electrode active material. The present disclosure also relates to a sodium or potassium ion battery produced by the method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure generally relates to a method for producing a sodium or potassium ion battery cell that includes a Prussian blue analogue (PBA) as an active cathode material. The present disclosure also relates to a sodium or potassium ion battery cell produced by the method. [Background technology]

[0002] Lithium-ion based batteries dominate the rechargeable battery market. However, this technology has drawbacks, at least due to the relatively scarce resources of lithium. Although superior to previous generations of secondary battery technology, lithium-ion based batteries are not considered environmentally friendly and are expensive from a recycling standpoint.

[0003] These shortcomings have triggered a search for alternatives to lithium-ion batteries. Sodium or potassium-ion batteries represent an attractive alternative and are also viable means of supporting renewable energy sources for the purposes of load leveling and excess energy storage.

[0004] The performance of a sodium or potassium ion battery depends heavily on the properties of the electrode materials.

[0005] A typical process for making an electrode, e.g., a cathode, is to mix an active material, e.g., in powder form, with a solvent, a conductive additive, and a binder to form a slurry. The slurry is then coated onto a current collector, such as a metal foil. The solvent is then removed by drying. The cathode is then assembled with an anode and any other components used to form a battery, such as a separator.

[0006] In conventional battery manufacturing, all steps of the process typically need to be carried out in a dry room, a room in which the moisture content of the air is controlled to a certain level. If a battery or any of its components is exposed to moisture during assembly, it can lead to degradation in quality, such as loss of charging capacity and overall performance.

[0007] Prussian blue analogue (PBA) cathode materials have stood out as promising cathode materials for use in sodium or potassium ion batteries. Prussian blue analogues have a unique crystal structure with an open three-dimensional framework and large interstitial voids, allowing them to store sodium (and potassium) ions.

[0008] Drying is particularly important when PBA is used as a cathode active material because any water present in the PBA structure must be removed in order for the material to fully utilize its capacity in a battery cell. The presence of water can adversely affect the electrochemical potential and cycling stability in battery cells containing PBA as the cathode material.

[0009] Therefore, it is essential to remove any water present in the PBA material when it is used in a final battery cell. However, once the water is removed from the PBA material, the PBA material still has a strong affinity for water. PBA is highly hygroscopic and can rapidly transition from anhydrous to hydrated upon exposure to air or moisture.

[0010] Therefore, the use of a dry room is an essential part of the process of preparing sodium or potassium ion batteries that utilize Prussian blue analog cathode materials.

[0011] However, there are various drawbacks associated with the use of dry rooms in battery manufacturing: First, dry rooms require high investment costs, and furthermore, energy demands are high due to temperature control and the large volumes of air that need to be dried.

[0012] Therefore, there is a need to provide an improved method for manufacturing sodium or potassium ion batteries that is simple, inexpensive, and does not require the use of a dry room. Summary of the Invention

[0013] In view of the above and other shortcomings of the prior art, it is an object of the present disclosure to provide improvements relating to sodium or potassium ion batteries, and in particular to providing a simple and inexpensive manufacturing method for producing such batteries.

[0014] According to a first aspect of the present disclosure, there is provided a method for producing a sodium or potassium ion battery, comprising the steps of: a) providing a slurry comprising a Prussian blue analogue, the Prussian blue analogue may be present in a first hydrated phase and a second dehydrated phase, the slurry comprising the first hydrated phase of the Prussian blue analogue; b) applying the slurry to a current collector to form a cathode; c) assembling the cathode with an anode and a separator to form an electrode stack; d) placing the electrode stack within a cell casing; e) drying the cell casing containing the electrode stack under conditions that allow the Prussian blue analogue to transform from the first hydrated phase to said second dehydrated phase; f) adding an electrolyte to the cell casing; and g) sealing the battery casing to form a battery cell, wherein steps f) and g) are performed under inert conditions.

[0015] The Prussian blue analogue (PBA) may be present in a hydrated, i.e., hydrated, phase or in a dehydrated, i.e., anhydrous, phase from which water has been removed. The inventors have found that a method for producing a sodium or potassium ion battery cell can be significantly improved if the conversion of the first hydrated phase of the Prussian blue analogue to a second dehydrated phase is carried out as late as possible in the process, i.e., if the drying step is carried out as late as possible.

[0016] In the first hydrated phase of the Prussian blue analog, the material has a monoclinic crystal structure. The PBA material is generally present in its monoclinic structure in the slurry and in the steps preceding the drying step.

[0017] In the second, dehydrated phase, the PBA material has a rhombohedral crystal structure. In battery applications, the dehydrated rhombohedral phase of PBA is desirably utilized to maximize the energy density and cycling stability of the battery cell.

[0018] In the transition from the first phase to the second phase, the crystal lattice of the monoclinic structure is distorted and undergoes a significant change in volume. The phase transition is associated with a substantial increase in sensitivity to moisture. The dehydrated rhombohedral structure of Prussian blue analogues is highly susceptible to reverting to the first hydrated phase, i.e., the monoclinic structure. However, such reversion is undesirable, as it can significantly damage the PBA structure, rendering the material unsuitable for use in battery cells. Furthermore, significant amounts of sodium or potassium can be lost during such reversion.

[0019] It is therefore important that the PBA material, after transitioning to the second dehydration phase, remain in this phase, i.e., maintain its rhombohedral crystal structure, throughout the remaining steps of the process, which is accomplished by the methods of the present disclosure.

[0020] By carrying out the process steps a) to g) in order, adding electrolyte and sealing the casing under inert conditions, the Prussian blue analogue is maintained in a second dehydrated phase throughout process steps f) and g).

[0021] The slurry containing the Prussian blue analogue is typically an aqueous slurry, so that the Prussian blue analogue is maintained in the first hydrated phase in the slurry.

[0022] Steps a) to d) of the method of the present disclosure may be carried out at ambient conditions.

[0023] Preferably, the Prussian blue analogue is present in a first hydrated phase in steps a) to d) of the method.

[0024] The inventors have found that it is desirable to keep the Prussian blue analogue in the first hydration phase until the drying step (step e), i.e. until the phase transition occurs, in this way undesirable transitions between the first and second phases are avoided and only one phase transition takes place (during the drying step).

[0025] This allows the steps preceding the drying step (step e) to be carried out under ambient conditions, which is a considerable advantage compared to conventional battery manufacturing techniques, which typically require all method steps to be carried out in a dry room.

[0026] Thus, the steps of providing a PBA slurry (step a), applying the slurry to a current collector (step b), assembling the cathode with additional cell components (step c), and placing the electrode stack within a cell casing (step d) can be performed at ambient conditions. During these stages of the process, the PBA material is less sensitive because it has not yet been converted to the second dehydrated phase.

[0027] The inventors have also tested and compared scenarios in which the drying step is performed after the assembly step (step c) but before placement of the electrode stack into the battery casing (step d), but all remaining steps are similar. Results from these tests demonstrate that the order of the method steps significantly impacts the capacity of the formed battery cells. Material performance is significantly affected by the conditions under which the materials are processed and handled.

[0028] With the disclosed method, significant improvements in capacity and cycling performance have been observed, with even very brief exposure to ambient atmosphere (as in the comparative test where the assembly was placed in a casing after a drying step) resulting in impaired battery cell performance.

[0029] The method of the present disclosure does not require the use of a dry room during any step of the battery manufacturing, thus providing a simple and cost-effective method.

[0030] In an exemplary embodiment, step f) of adding the electrolyte and step g) of sealing the cell casing are carried out in the same apparatus.

[0031] This is beneficial to prevent unwanted exposure to moisture and air during transport of the electrode stack.

[0032] In an exemplary embodiment, the drying step e) is performed in a chamber connected to or contained within the device.

[0033] Therefore, transfer of the dry cell stack to the electrolyte injection apparatus is performed under inert conditions, which prevents undesirable exposure to moisture and air.

[0034] In an exemplary embodiment, drying step e) is carried out at a temperature ranging from 110° C. to 250° C., preferably from 120° C. to 200° C., for at least 4 hours, preferably at least 10 hours.

[0035] These drying conditions are suitable for enabling the phase transition of the Prussian blue analog from the first hydrated phase to the second dehydrated phase of PBA. These drying conditions enable the removal of any water present in the first phase of the PBA material and any water potentially present in any other part of the battery cell. Further, these drying conditions do not adversely affect the PBA structure or other components of the battery cell.

[0036] In some embodiments, the drying step e) is performed under vacuum.

[0037] It is desirable to utilize vacuum as the drying process can be carried out at a lower temperature and the drying time can be shortened.

[0038] In an exemplary embodiment, the Prussian blue analog has the formula, A a M b [M’ c (CN)6] d wherein A is sodium or potassium, 1 < a ≦ 2, M and M’ are transition metals, preferably selected from iron and / or manganese, 0 < b < 2, 1 < c < 2, and 1 < d < 2.

[0039] In an embodiment, the Prussian blue analog is Prussian white and has the formula, A a Fe[Fe(CN)6] where A is sodium or potassium, 1.8 < a ≦ 2, preferably 1.9 < a ≦ 2.

[0040] Prussian white is associated with high battery capacity and an improvement in the storage ability of sodium (and potassium) ions. Prussian white is also environmentally friendly and can be manufactured at low cost.

[0041] In an exemplary embodiment, the battery casing is a pouch cell or a cylindrical cell.

[0042] Typically, the casing is a pouch cell.

[0043] The pouch cells may be formed of a flexible material, such as foil, so the battery casing is flexible, lightweight, and can be made into a variety of sizes and shapes.

[0044] The sealed battery casing seals around the battery cells and acts as a barrier to the transmission of any air or moisture into or out of the battery cells.

[0045] In an embodiment, the step of providing a slurry may include mixing a Prussian blue analog in powder form with a conductive additive and a binder.

[0046] The process of applying the slurry to the current collector is carried out at a rate of 5 mg / cm 2 ~30mg / cm 2 , preferably 10 mg / cm 2 ~20mg / cm 2 The method may include coating the slurry onto a current collector at a coating weight of about 1000 g / m.

[0047] The thickness of the coating on the current collector can vary depending on the particular application and purpose. For example, the thickness of the PBA coating can range from 50 μm to 500 μm, such as from 100 μm to 250 μm.

[0048] The electrodes can then be cut to the desired shape by techniques well known in the art.

[0049] The cathode may be assembled with the anode by stacking or winding the electrode with a separator.

[0050] According to another aspect, there is provided a sodium or potassium ion battery cell manufactured according to the above method.

[0051] The battery cell is Na + / 4.0V or more for Na or K + 3. The electrochemical cycling curves may have no voltage plateau above 4.15 V vs. / K.

[0052] The absence of voltage plateaus above 4 V (Na+ / Na) and 4.15 (K+ / K), respectively, is indicative of the removal of water from the battery cell and the presence of the PBA material in a second, dehydrated phase. Such battery cells exhibit stable behavior upon subsequent charging and discharging and have high initial coulombic efficiency. The absence of voltage plateaus above 4 V (Na+ / Na) and 4.15 (K+ / K), respectively, is indicative of the removal of water from the battery cell and the presence of the PBA material in a second, dehydrated phase.

[0053] Preferably, the battery cell is a Na + Between 3.2 and 3.9 V vs. Na, or K + 1 V vs. / K, and the electrochemical cycling curves are devoid of additional voltage plateau(s).

[0054] The presence of one clear voltage plateau within the above range indicates that the battery cell is devoid of water and no side reactions caused by water or moisture occur.

[0055] Further features and advantages of the present disclosure will become apparent upon review of the appended claims and the following description. Those skilled in the art will appreciate that different features of the present disclosure can be combined to create embodiments other than those described below without departing from the scope of the present disclosure.

[0056] The various aspects of the present disclosure, including its particular features and advantages, will be readily understood from the following detailed description and the accompanying drawings. [Brief description of the drawings]

[0057] [Figure 1] FIG. 1 shows a schematic diagram of the steps of the method of the present disclosure. [Diagram 2] FIG. 2 illustrates a schematic of a sodium or potassium ion battery according to an exemplary embodiment of the present disclosure. [Figure 3a]FIG. 3a shows cycle data for a sodium-ion battery cell manufactured according to a method in which the battery cell was dried before being inserted into a battery casing. [Figure 3b] FIG. 3b shows cycle data for a sodium-ion battery cell manufactured according to an exemplary embodiment of the method of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0058] The present disclosure will now be described more fully hereinafter with reference to the accompanying drawings, in which presently preferred embodiments of the disclosure are shown. However, the present disclosure may be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are provided for thoroughness and completeness, so as to fully convey the scope of the present disclosure to those skilled in the art.

[0059] FIG. 1a generally outlines the steps of a method (100) for manufacturing a sodium or potassium ion battery cell of the present disclosure.

[0060] The method comprises: a) providing a slurry comprising a Prussian blue analogue, the Prussian blue analogue may be present in a first hydrated phase and a second dehydrated phase, the slurry comprising the first hydrated phase of the Prussian blue analogue (step 101); b) applying the slurry to a current collector to form a cathode (step 102); c) assembling the cathode with the anode and a separator to form an electrode stack (step 103); d) placing the electrode stack within a cell casing (step 104); e) drying the cell casing containing the electrode stack under conditions that allow the Prussian blue analog to convert from the first hydrated phase to said second dehydrated phase (step 105); f) adding an electrolyte to the cell casing (step 106); and g) sealing the battery casing to form a battery cell (step 107), wherein steps f) and g) are performed under inert conditions.

[0061] An important feature of the disclosed method is that the electrode stack within the cell casing is dried and not allowed any exposure to moisture or air during steps subsequent to the drying step.

[0062] Thus, undesirable reversion between the first and second phases of the PBA material, which can result in expansion and damage to the material, is prevented.

[0063] The inventors have found that the battery cells manufactured according to the method of the present disclosure have significantly improved capacity and cycling performance, resulting in battery cells with stable cycling performance and avoiding undesirable side reactions due to air exposure (see Example 2).

[0064] The step of providing a slurry (Step 101) may include mixing a Prussian blue analog in powder form with a conductive additive and a binder.

[0065] The mixing may be performed by stirring and / or mixing for at least 1 hour. Prior to applying the slurry to the current collector, the mixing may be performed in an inert atmosphere to remove any potential air bubbles in the slurry.

[0066] The conductive additive may be any type of conductive additive known to those skilled in the art, for example, various types of carbon compounds such as super P, C65, C45, carbon black such as Ketjen Black may be utilized.

[0067] The binder is not limited to a specific binder, and may be, for example, alginate, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), or polyvinylidene fluoride (PVdF).

[0068] Prussian blue analogue (PBA) powder can be prepared by means known in the art.

[0069] The slurry containing the Prussian blue analogue is typically an aqueous slurry, and thus the Prussian blue analogue is present in a first hydrated phase in the slurry.

[0070] The step (102) of applying the slurry to the current collector is carried out at a concentration of 5 mg / cm 2 ~30mg / cm 2 , preferably 10 mg / cm 2 ~20 mg / cm 2 The method may include coating the slurry onto a current collector at a coating weight of about 1000 g / m.

[0071] The slurry is preferably evenly applied to at least one side of a current collector, which is typically a metal foil or sheet.

[0072] The current collector may be coated on one or both sides. When both sides are coated, the coating weight can be increased. For example, the coating weight can be 30 to 50 mg / cm. 2 may be also possible.

[0073] The coating process is not limited to a particular coating technique and can utilize any means for coating the slurry onto the current collector, such as slot die coating. Preferably, the coating is evenly distributed on at least one side of the current collector.

[0074] The thickness of the coating on the current collector can vary depending on the particular application and purpose. For example, the thickness of the PBA coating can range from 50 μm to 500 μm, such as from 100 μm to 250 μm.

[0075] The coated active PBA material may then be pressed and compressed onto the current collector, for example by calendaring using a roller press calendar, so that a consistent thickness and density of the coating can be achieved.

[0076] The electrode can then be cut to the desired shape by techniques well known in the art, for example, any type of slitting machine can be utilized.

[0077] In step 103, the cathode is assembled with the anode by stacking or winding the electrodes with a separator. Any technique known in the art can be utilized.

[0078] The battery cells are then placed into a battery casing (step 104).

[0079] In an embodiment, the battery casing is a cylindrical cell or a pouch cell.

[0080] The battery casing can vary depending on the intended use and preference. The battery casing seals around the battery cells and acts as a barrier to the transmission of any air or moisture into or out of the battery cells.

[0081] Preferably, the battery casing is a pouch cell, in other words, the battery casing may be in the form of a pouch made of a flexible material, such as foil, so that the casing is flexible, lightweight, and can be made into a variety of sizes and shapes.

[0082] For example, the pouch cell may include a polymer-coated metal foil. The metal foil may include a polymer coating on one or both sides of the metal foil.

[0083] When the electrode stack is inserted into the pouch cell, the pouch cell may be partially sealed.

[0084] As mentioned above, process steps a)-d) (shown as 101-104 in FIG. 1) may be carried out at ambient conditions. Steps a)-d) may be carried out at room temperature.

[0085] As used herein, "ambient conditions" refers to the general air temperature and relative humidity at which the process is carried out. Steps a) through d) may be carried out at relative humidity (RH) levels related to room temperature (e.g., 40-60% RH). The process is not limited to any particular requirements or equipment for these first steps of the method.

[0086] The cell casing is then dried (step 105) under conditions that allow the PBA material to transform into a second, dehydrated phase.

[0087] For example, the drying step may be carried out at a temperature ranging from 110° C. to 250° C., preferably from 120° C. to 200° C., for at least 4 hours, preferably at least 10 hours.

[0088] Thus, sodium or potassium ion batteries with improved capacity and cycling performance can be obtained, and these drying conditions do not adversely affect the PBA structure.

[0089] Preferably, the drying step is carried out under vacuum (pressure lower than ambient pressure) in order to allow for lower temperatures to be utilized during drying. Vacuum allows drying to be carried out at temperatures in the range of about 110-160°C.

[0090] The drying process is 10 -3 It can be carried out at a pressure of up to 100 mbar. For example, the pressure may be 0.01 to 1 mbar.

[0091] However, the pressure is highly dependent on the temperature utilized in the drying process, and therefore may vary depending on the temperature used during drying.

[0092] The drying step is important to ensure removal of any water present in the active PBA material, as well as any water potentially present in any other parts of the battery cell.

[0093] By dehydrated PBA material, it is meant that the PBA material does not contain water that would affect the electrochemical behavior of a battery cell containing the PBA material. This can be evidenced by the absence of voltage plateaus in the electrochemical cycling curves above 4 V for Na+ / Na and above 4.15 V for K+ / K. Such voltage plateaus are associated with water extraction and are an indication that the PBA has not fully transitioned from the first hydrated phase to the second dehydrated phase.

[0094] As used herein, "Na + / Na vs. 4 V, or K + The term "there is no voltage plateau above 4.15 V vs. Na / K" means that there is no additional capacity after 4 V and 4.15 V, respectively. + / >4V for Na or K + There is no moisture-induced response above 4.15 V vs. / K. This is shown by the vertical upward trend in the electrochemical cycling curves in Figure 3b. The anodes used for electrochemical cycling tests are typically carbon-based anodes (hard carbon).

[0095] The presence of water or side reactions caused by water or moisture may be + / Na > 4V or K + / K. This can also be evidenced by the presence of two or more voltage plateaus in the electrochemical cycling curves.

[0096] The battery cell is Na + Between 3.2 and 3.9 V vs. Na, or K +1 V vs. / K, and the electrochemical cycling curve is devoid of additional voltage plateau(s).

[0097] Therefore, a water-free, stable and high-performance battery cell is realized.

[0098] An important advantage of the disclosed method is that no dry room is required at any step of the battery manufacturing, therefore the method is simple and associated with low cost.

[0099] The method further includes adding an electrolyte to the battery cell after the drying step, where the electrolyte is added under inert conditions (step 106).

[0100] As used herein, the term "inert conditions" refers to an atmosphere free of oxygen and water. Preferably, a glove box, i.e., an air- and moisture-free closed chamber, is utilized. The glove box may include sealed gloves for electrolyte injection. The glove box may be filled with argon (Ar) gas.

[0101] Preferably, the electrolyte is a non-aqueous electrolyte. The non-aqueous electrolyte prevents water from interfering with the PBA-coated cathode. Furthermore, the non-aqueous electrolyte provides a larger potential window compared to aqueous electrolytes. Also, since the battery cell is dry and the PBA is dehydrated, there is substantially no water in the active PBA material or in the battery cell that may interfere with the non-aqueous electrolyte.

[0102] The present disclosure is not limited to the use of any particular non-aqueous electrolyte. Non-aqueous electrolytes typically include a solvent or blend of solvents and at least one dissolved salt.

[0103] For example, the non-aqueous electrolyte may include, for example, ethylene carbonate, diethyl carbonate, dimethyl carbonate, and / or any mixture thereof. The non-aqueous electrolyte may include a salt, such as sodium hexafluorophosphate (NaPF6) or sodium tetrafluoroborate (NABF4). The non-aqueous electrolyte may also include an additive.

[0104] In an embodiment, the non-aqueous electrolyte includes an alkali metal bis(oxalato)borate salt, and the alkali metal ion is sodium (Na + ), and potassium (K + Such a non-aqueous electrolyte is fluorine-free, environmentally friendly, safe, and has high ionic conductivity and electrochemical stability.

[0105] The cell casing is then sealed under inert conditions (step 107).

[0106] Step f) of adding the electrolyte and step g) of sealing the cell casing may be carried out in the same apparatus, for example using a glove box.

[0107] The drying step d) may be carried out in a chamber connected to or contained within the device.

[0108] For example, the drying step may be carried out in a chamber, forming a separate compartment of the apparatus.

[0109] In an embodiment, step f) of adding electrolyte and step g) of sealing the cell casing are carried out in the same glove box. The drying step may be carried out in a transfer chamber, also called antechamber, connected to or forming part of the glove box. The transfer chamber may be equipped with means for applying a vacuum.

[0110] After drying in the antechamber, the cell casings may be transferred to different compartments of the device for electrolyte injection and sealing.

[0111] After step e) of the method, the step of transferring the battery casing to the electrolyte injection device is carried out under inert conditions. Accordingly, the battery casing is not exposed to any moisture or air, and the PBA material is kept in its second dehydrated phase.

[0112] In an exemplary embodiment, the Prussian blue analog has the formula, A a M b [M’ c (CN)6] d wherein A is sodium or potassium, 1 < a ≦ 2, M and M’ are transition metals, preferably selected from iron and / or manganese, 0 < b < 2, 1 < c < 2, and 1 < d < 2.

[0113] In an embodiment, the Prussian blue analog is Prussian white and has the formula, A a Fe[Fe(CN)6] wherein A is sodium or potassium, 1.8 < a ≦ 2, preferably 1.9 < a ≦ 2.

[0114] Prussian white is associated with high battery capacity and an improved ability to store sodium (and potassium) ions. Prussian white is also environmentally friendly and can be manufactured at low cost.

[0115] In embodiments where the Prussian blue analog is a Prussian white material, this material can be prepared according to the method described in International Publication No. WO 2018 / 056890, which was assigned to Altris AB.

[0116] According to another aspect, a sodium or potassium ion battery cell manufactured according to the aforementioned method is provided.

[0117] 2 shows the general principle of a sodium or potassium ion battery 200, which utilizes sodium or potassium ions 201 as charge carriers. The battery stores energy in chemical bonds at the negative electrode, or anode 202. When the battery 200 is charged, the Na + Or K + Ions 201 are forced to deintercalate from the positive electrode, i.e., cathode 203, and migrate towards the anode 202. During discharge, the process is reversed. When the circuit is completed, electrons move back from the anode 202 to the cathode 203, and Na + Or K + The ions 201 move back to the cathode 203. During battery discharge, oxidation occurs at the anode 202 while reduction occurs at the cathode 203, as shown in Figure 2. Current flow is determined by the potential difference between the cathode 203 and the anode 202, the cell voltage.

[0118] The two electrodes are separated by a separator 205 , which is wetted with an electrolyte 204 .

[0119] As used herein, the term "battery" means a device that contains one or more battery cells.

[0120] A "battery cell" contains a positive electrode, or cathode, a negative electrode, or anode, and a separator. In a battery cell, chemical energy is converted to electricity by reduction and oxidation (redox) reactions at the electrodes.

[0121] The cathode 203 utilized in the sodium or potassium ion batteries of the present disclosure includes a current collector coated with the Prussian blue analog material described above.

[0122] The negative electrode material, i.e., anode 202, is not particularly limited as long as it is a material capable of storing / releasing sodium or potassium ions. Examples include metal composite oxides, sodium metal, sodium alloys, silicon, silicon-based alloys, tin-based alloys, bismuth-based alloys, metal oxides, conductive polymers, Na-Co-Ni-based materials, hard carbon, etc. The anode may be a metal foil coated with an active anode material.

[0123] The battery cell may further comprise a separator 205 to prevent electrical shorts between the negative and positive electrodes and to provide mechanical stability to the cell. The separator material may be any chemically stable, electrically insulating material, such as a polymer film typically made from polypropylene, polyethylene, or combinations thereof. The separator is preferably thermally stable at temperatures ranging up to 250° C.

[0124] Example 1: Drying on the outside of the casing A prototype Prussian White cell was laminated with a heat-resistant separator and a high mass loading electrode. A carbon-based anode, i.e., hard carbon, was utilized. The laminated prototype was placed in a high vacuum (2×10) oven to remove any water from the electrode. -2 The electrode stack was then dried at 150°C under 100 psi (< 300 mBar) for 12 hours. After drying was completed, the cell stack was transferred from the oven to a pouch cell casing for electrolyte injection and sealing. This operation involved exposing the electrode stack to ambient conditions for a short period (< 3 minutes) followed by a drying step at 120°C for 1-3 hours.

[0125] The cycling data in Figure 3a shows that the electrode stack contains both the anhydrous phase of Prussian White and the hydrated phase of Prussian White, i.e., both rhombohedral and monoclinic structures. This is clearly evidenced by the 4 volt plateau that appears at the end of charge and is associated with the extraction of water from the cathode. The water content in the cell caused gassing in the cell and discharging was not possible.

[0126] Example 2: Drying inside the casing A prototype Prussian White cell was stacked with a separator and a high mass loading electrode. A carbon-based anode, i.e., hard carbon, was utilized. The stacked prototype was transferred to a pouch cell casing and subjected to high vacuum (2×10) to remove any water from the electrode. -2 The cells were dried at 150° C. under a pressure of less than 1000 mBar for 12 hours. After drying was completed, the cell stack was injected with electrolyte and sealed without exposure to the ambient atmosphere. This operation is possible because the casing with the electrode stack does not require an assembly step before injection and sealing.

[0127] The cycling data in Figure 3b show that the electrode stack contains only the anhydrous, i.e., rhombohedral, phase of Prussian white. This is clearly evidenced by the absence of the 4 volt plateau that appears at the end of charge and is associated with the extraction of water from the cathode. The absence of water allowed the cell to be cycled with an initial coulombic efficiency of over 85% and stable behavior during subsequent charge and discharge.

[0128] In summary, the material is dry and cycles without side reactions.

[0129] The terms, definitions, and embodiments of all aspects of this disclosure apply mutatis mutandis to the other aspects of this disclosure.

[0130] Although the present disclosure has been described with reference to specific exemplary embodiments thereof, many different alterations, modifications and the like will become apparent to those skilled in the art.

[0131] Variations to the disclosed embodiments can be understood and effected by those skilled in the art in practicing the present disclosure, from a study of the drawings, the disclosure, and the appended claims. Moreover, in the claims, the word "comprising" does not exclude other elements or steps, and the indefinite article "a" or "an" does not exclude a plurality.

Claims

1. 1. A method for producing a sodium or potassium ion battery cell comprising the steps of: a) providing a slurry comprising a Prussian blue analogue, the Prussian blue analogue may be present in a first hydrated phase and a second dehydrated phase, the slurry comprising the first hydrated phase of the Prussian blue analogue; b) applying the slurry to a current collector to form a cathode; c) assembling the cathode with an anode and a separator to form an electrode stack; d) placing the electrode stack within a cell casing; e) drying the cell casing containing the electrode stack under conditions that allow the Prussian blue analog to transform from the first hydrated phase to the second dehydrated phase; f) adding an electrolyte to the cell casing; g) sealing the battery casing to form a battery cell; Including, The method, wherein steps f) and g) are carried out under inert conditions.

2. 2. The method of claim 1, wherein the Prussian blue analogue is maintained in the second dehydration phase throughout steps f) and g) of the method.

3. The method according to claim 1 or claim 2, wherein steps a) to d) of the method are carried out at ambient conditions.

4. The method according to any one of claims 1 to 3, wherein the Prussian blue analogue is present in the first hydrated phase in steps a) to d) of the method.

5. The method according to any one of claims 1 to 4, wherein said step f) of adding the electrolyte and said step g) of sealing the cell casing are carried out in the same apparatus.

6. The method of claim 5 , wherein the drying step e) is performed in a chamber connected to or contained within the device.

7. The method according to any one of the preceding claims, wherein the drying step e) is carried out at a temperature in the range of from 110°C to 250°C, preferably from 120°C to 200°C, for at least 4 hours, preferably at least 10 hours.

8. The method according to any one of claims 1 to 7, wherein the drying step e) is carried out under vacuum.

9. The Prussian blue analog has the formula: a M b [M' c (CN) 6 ] d wherein A is sodium or potassium, 1<a≦2, M and M′ are transition metals, preferably selected from iron and / or manganese, 0<b<2, 1<c<2, and 1<d<2.

10. The Prussian blue analog is Prussian white, and has the formula: a Fe[Fe(CN) 6 10. The method according to claim 1, wherein A is sodium or potassium and 1.8<a≦2, preferably 1.9<a≦2.

11. The method of any one of claims 1 to 10, wherein the battery casing is a pouch cell.

12. 12. The method according to any one of claims 1 to 11, wherein the step of providing a slurry comprises mixing the Prussian blue analogue in powder form with at least a conductive additive and a binder.

13. The step of applying the slurry to a current collector has a thickness of 5 mg / cm 2 ~30mg / cm 2 , preferably 10 mg / cm 2 ~20mg / cm 2 The method of any one of claims 1 to 12, comprising coating the slurry onto the current collector at a coating weight of

14. A sodium or potassium ion battery cell produced according to the method of any one of claims 1 to 13.

15. The battery cell is + / 4.0 V or more against Na, or K + 15. The sodium or potassium ion battery cell of claim 14, having an electrochemical cycling curve with no voltage plateau above 4.15 V vs. / K.

16. The battery cell is + / Na between 3.2 and 3.9 V, or K + 16. The sodium or potassium ion battery cell of claim 14 or claim 15, having an electrochemical cycling curve exhibiting one voltage plateau between 3.9 and 4.1 V vs. / K, the electrochemical cycling curve lacking additional voltage plateaus.

Citation Information

Patent Citations

  • A method for modifying Prussian blue and its analogues and a sodium ion battery

    CN109065883A

  • Prussian blue positive electrode material, sodium ion battery and preparation method and application thereof

    CN111377462A

  • An electrolyte solution comprising an alkali metal bis (oxalato)borate salt

    EP3783720A1

  • Method for producing sodium iron(II)-hexacyanoferrate(II) materials.

    JP2019529329A

  • Optimization of electrochemical cell

    US10978743B1