Method for preparing precursor materials for Li-containing cathode active materials

The method addresses the issues of high chloride content and gas emissions in Li-containing cathode active material production by enhancing the bulk density and homogeneity of mixed metal oxides through spray pyrolysis and spray drying, ensuring a high-quality precursor for battery production.

JP2024539972AActive Publication Date: 2024-10-31UMICORE(BE)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024524709
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-10-20
Publication Date
2024-10-31
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing methods for preparing Li-containing cathode active materials using spray pyrolysis result in high Cl content, low furnace capacity, and the generation of polluting gases like NO and NO2, making them unsuitable for industrial production.

Method used

A method involving spray pyrolysis of an aqueous solution to form mixed metal oxides, followed by spray drying and washing to increase bulk density, reduce chloride content, and improve homogeneity, using inexpensive and soluble salts, and incorporating size reduction steps to enhance the precursor material's properties.

Benefits of technology

The method significantly increases the furnace capacity and reduces environmental pollution by minimizing chloride content and gas emissions, resulting in a high-quality precursor material suitable for battery production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539972000001_ABST
    Figure 2024539972000001_ABST
Patent Text Reader

Abstract

1. A method for preparing a precursor material for a Li-containing cathode active material for a battery, the method comprising a spray pyrolysis step of decomposing droplets of an aqueous solution in a heated chamber to produce a metal oxide, wherein the metal oxide is either a mixed metal oxide comprising the elements Ni and one or both of the elements Co and Mn, and the aqueous solution is a mixed solution of a salt of Ni and a salt of Co and / or Mn, or the metal oxide is Ni oxide and the aqueous solution is a solution of a salt of Ni, the method comprising a spray drying step of spray drying an aqueous slurry comprising the metal oxide to form the precursor material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for preparing a precursor material for a Li-containing cathode active material, i.e., a positive electrode active material, and to the Li-containing cathode active material from said precursor. [Background technology]

[0002] Generally, Li-containing cathode active materials are prepared by first making precursors of Co and / or Ni and / or Mn and / or Al and then reacting such precursors with a lithium source in a furnace.

[0003] The precursors are typically single-element inorganic compounds or mixtures of single-element or multi-element inorganic compounds of the elements Co and / or Ni and / or Mn and / or Al, such as oxides, hydroxides or carbonates. The precursors themselves typically contain no or only very small amounts of Li.

[0004] A good precursor in an industrial context should not only have properties that allow the preparation of a good quality final product, but should also be cheap to produce and lend itself to cheap further manufacturing steps.

[0005] It is known to prepare mixed Ni-Co-Mn oxides as precursors for Li-containing cathode active materials using spray pyrolysis from mixed chloride solutions, see Frohlich et al., New large-scale production route for synthesis of lithium nickel manganese cobalt oxide, J Solid State Electrochem, 21, 3403-3410 (2017).

[0006] From WO 2019 / 185349 it is also known to use spray pyrolysis to prepare mixed Ni-Co-Mn oxides.

[0007] However, such known mixed oxides have drawbacks, in particular they lead to a relatively high Cl content in the final Li-containing cathode active material and, due to their low density, lead to a low furnace capacity for the subsequent reaction step with a Li source.

[0008] LiMn can be used as a Li-containing cathode active material 2 O 4 It is also known to use spray pyrolysis from a mixed nitrate solution containing Li, followed by spray drying, to prepare spherical LiMn. This is reported by TANIGUCHI et al. in "Synthesis of spherical LiMn 2 O 4 "Microparticles by a combination of spray pyrolysis and drying method", POWDER.TECHNOLOGY, Vol. 181, No. 3, January 29, 2008, pp. 228-236.

[0009] However, this produces gaseous NO and NO as decomposition products. 2 Generates NO and NO 2 This is undesirable because NO is a highly polluting gas in the atmosphere, causing both smog and acid rain. Therefore, such a process involves the extraction of NO and NO from the gases resulting from pyrolysis. 2 This requires very elaborate and expensive removal of the

[0010] It is also known to use spray pyrolysis from a mixed chloride solution containing Li, followed by spray drying, to prepare lithiated metal oxides that can be used directly as Li-containing cathode active materials. This is disclosed in CN104934572. However, such a method results in a high Cl content in the final product, making the product less suitable for use in batteries. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2019 / 185349 [Patent Document 2] China Patent Application Publication No. 104934572 [Non-patent literature]

[0012] [Non-Patent Document 1] Frohlich et al., “New large-scale production route for synthesis of lithium nickel manganese cobalt oxide”, J Solid State Electrochem, 21, 3403–3410 (2017) [Non-Patent Document 2] TANIGUCHI et al., “Synthesis of spherical LiMn2O4 microparticles by a combination of spray pyrolysis and drying method”, POWDER.TECHNOLOGY, Vol. 181, No. 3, January 29, 2008, p. 228-236 Summary of the Invention [Means for solving the problem]

[0013] The present invention aims to avoid and / or reduce these and other disadvantages and therefore provides a method for preparing a precursor material for a Li-containing cathode active material for a battery, the method comprising a spray pyrolysis step in which droplets of an aqueous solution are decomposed in a heated chamber to produce a metal oxide, the method comprising a spray drying step in which an aqueous slurry comprising said metal oxide is spray-dried, either directly from the spray pyrolysis step or after one or more intermediate processing steps, to form a precursor material, the metal oxide having the following characteristics: 1) The metal oxide is a mixed metal oxide containing Ni and one or both of Co and Mn, and the aqueous solution is a mixed solution of a Ni salt and a Co and / or Mn salt; 2) The metal oxide is Ni oxide, and the aqueous solution is a solution of a Ni salt; 3) the metal oxide is an Mn oxide and the aqueous solution is a solution of a salt of Mn.

[0014] In chemistry, a mixed oxide is the name for an oxide compound that contains cations of two or more chemical elements or cations of a single element in several oxidation states.

[0015] The first option in this definition is intended herein.

[0016] Alternatively, a mixed metal oxide may be defined as a metal oxide in which each particle of the metal oxide contains all of the metal elements present in the metal oxide.

[0017] As mixed metal oxides, only oxide compounds containing cations of two or more different metal elements are considered, not mixtures of single metal oxides.

[0018] By mixed salt solution is meant a solution in which salts of different metal elements are present in the same solvent, whether or not an explicit mixing step has taken place.

[0019] Various embodiments according to the present invention are disclosed in the claims and in this specification. The embodiments and examples described in the claims and in this specification can be freely combined with each other, unless expressly specified otherwise. Throughout this specification, when any numerical range is provided, the range also includes the endpoints, unless expressly specified otherwise.

[0020] The present invention relates to the following preferred embodiments.

[0021] The spray drying process significantly increases the bulk density of the metal oxides, thereby improving the capacity of the furnace used to react the precursor materials with Li.

[0022] In a preferred variant, the salt or salts are chlorides. They are cheaply available, highly soluble, and can be easily recycled.

[0023] In a preferred variant, the method includes a slurry preparation step in which particles of the metal oxide, either directly from the spray pyrolysis step, or after one or more intermediate processing steps, are mixed with water to prepare an aqueous slurry.

[0024] In a preferred variant, the method includes a washing step in which a mixture of metal oxide and water is prepared, either directly from the spray pyrolysis step or after one or more intermediate processing steps, in a ratio (weight of water) / (weight of metal oxide) of at least 0.1, preferably at least 0.5, and this mixture is filtered, centrifuged or decanted to recover the metal oxide, whereby the washing step is carried out before the slurry preparation step.

[0025] In this washing step, residual anions in the metal oxide, especially chloride, can be removed since they are soluble in water. Those skilled in the art will appreciate that the amount of water used will depend on the anion content desired after the washing step.

[0026] In a preferred variant, the method includes a size reduction step in which the metal oxide undergoes particle size reduction, either directly from the spray pyrolysis step or after one or more intermediate processing steps, which size reduction step is carried out before the spray drying step.

[0027] This improves the homogeneity of the precursor material produced and also allows for increased capacity of the spray drying process.

[0028] In a preferred variant, the size reduction step is carried out on the metal oxide wetted with water. This avoids intermediate drying of the metal oxide if there is a preceding wet step, such as the washing step mentioned above. It also reduces the generation of dust.

[0029] In a preferred variant, the median particle size D50 of the metal oxide particles in the aqueous slurry is between 10 nm and 1000 nm, so that the metal oxide content obtainable in the aqueous slurry may be optimal.

[0030] In a preferred variation, the precursor material comprises spherical particles and the precursor material has a density of at least 1.0 g / cm 3 , preferably at least 1.3 g / cm 3 , more preferably at least 1.4 g / cm 3 Spherical particles have a circularity ratio of at least 0.5 when viewed in cross-sectional images under a microscope. It is calculated as the ratio between the area of ​​the particle and the area of ​​the disk with the largest diameter of the particle.

[0031] The spherical particles preferably have a median particle size D50 of at least 2 μm and at most 50 μm to provide a good balance between ease of handling and rate of reaction with Li in subsequent processing steps.

[0032] The metal oxide preferably has a molar content of Mn y, a molar content of Co z, a molar content of Ni b and a molar content of A a, where A is any metal element other than Li, Ni, Mn and Co, 0.20≦b / (y+z+b+a)≦1.00, for example 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, or 0.90; 0≦y / (y+z+b+a)≦0.80, for example 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70; 0≦z / (y+z+b+a)≦0.60, for example 0.10, 0.20, 0.30, 0.40, or 0.50; and 0≦a / (y+z+b+a)≦0.10, for example 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, or 0.09.

[0033] More preferably, 0.30≦b / (y+z+b+a)≦1.00, and even more preferably, 0.45≦b / (y+z+b+a)≦1.00.

[0034] More preferably, the metal oxide is a mixed metal oxide, where 0.30≦b / (y+z+b+a)≦0.95 and 0.04≦z / (y+z+b+a)≦0.60, and even more preferably 0.45≦b / (y+z+b+a)≦0.90 and 0.04≦z / (y+z+b+a)≦0.35. [Brief description of the drawings]

[0035] [Figure 1] This is a CS-SEM image of EX1.2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] In the following detailed description, preferred embodiments are described to enable the practice of the invention. Although the invention is described with reference to these specific preferred embodiments, it will be understood that the invention is not limited to these preferred embodiments. The invention includes numerous alternatives, modifications, and equivalents that will be apparent from consideration of the following detailed description and the accompanying drawings.

[0037] A) CS-SEM (cross-sectional scanning electron microscope) analysis Cross sections of the transition metal oxide precursors described herein, i.e., precursor materials, are prepared by an ion beam cross section polishing (CP) instrument, JEOL (IB-0920CP), which uses argon gas as the beam source.

[0038] To prepare the test specimen, a small amount of transition metal oxide precursor powder is mixed with the resin and hardener, and then the mixture is heated on a hot plate for 10 minutes. After heating, it is placed in the ion beam instrument for cutting and the settings are adjusted to the standard procedure of a voltage of 6.5 kV for a duration of 3 hours.

[0039] The morphology of the transition metal oxide precursors was analyzed by scanning electron microscopy (SEM) technique. The measurements were performed using a JEOL JSM 7100F (https: / / www.jeolbenelux.com / JEOL-BV-News / jsm-7100f-thermal-field-emission-electron-microscope) at 25 °C with a resolution of 9.6 × 10 -5 The experiment was carried out under a high vacuum environment of 10 Pa.

[0040] B) Particle size analysis The particle size distribution (PSD) of the transition metal oxide precursor powders, i.e. precursor materials, was measured by laser diffraction particle size analysis using a Malvern Mastersizer 3000 equipped with a Hydro MV wet dispersion accessory (https: / / www.malvernpanalytical.com / en / products / product-range / mastersizer-range / mastersizer-3000#overview) after dispersing each powder sample in aqueous media. Sufficient sonication and stirring were applied and appropriate surfactants were introduced to improve the dispersion of the powders. The median particle size D50 is defined as the particle size at 50% of the cumulative volume % distribution obtained from the Malvern Mastersizer 3000 measurement with Hydro MV.

[0041] C) Bulk density The bulk density of the precursor material powder is determined by measuring the mass of the powder flowing into a graduated cylinder having a specific volume. The precursor bulk density is calculated according to the following formula:

[0042]

number

[0043] D) Carbon analyzer The carbon content of the positive electrode active material powder is measured by an Emia-Expert carbon / sulfur analyzer manufactured by Horiba, Ltd. 1 g of the example or comparative example is placed in a ceramic crucible in a high-frequency induction electric furnace. 1.5 g of tungsten and 0.3 g of tin as promoters are added into the crucible. The powder is heated at a programmable temperature where the gases produced during combustion are then analyzed by an infrared detector. CO 2 and CO analysis to determine carbon concentration.

[0044] E) ICP analysis The amount of metal elements, e.g., Ni, Mn, and Co, in the precursor is measured by Inductively Coupled Plasma (ICP) method using Agilent ICP720-ES (Agilent Technologies). 2 grams of powder sample is dissolved in 10 mL of high-purity hydrochloric acid (at least 37 wt% HCl with respect to the total weight of the solution) in an Erlenmeyer flask. The flask is covered with glass and heated on a hot plate at 380 °C until the precursor is completely dissolved. After cooling to room temperature, the solution in the Erlenmeyer flask is poured into a 250 mL volumetric flask. The volumetric flask is then filled with deionized water up to the 250 mL mark, followed by thorough homogenization. An appropriate amount of the solution is removed with a pipette and transferred to a 250 mL volumetric flask for the second dilution, and the volumetric flask is filled with internal standard and 10% hydrochloric acid up to the 250 mL mark, followed by homogenization. Finally, this 50 mL solution is used for ICP measurement.

[0045] The invention is further illustrated by the following (non-limiting) examples.

[0046] Example 1.1: Mixed Metal Oxides The precursor product was obtained by a spray pyrolysis and spray drying process carried out as follows. 1) Preparation of Feed Solution: NiCl in water at a total concentration of 110 g / L with Ni, Mn, and Co in a Ni:Mn:Co ratio of 0.6:0.2:0.2. 2 , MnCl 2 , and CoCI 2A mixed feed solution was prepared containing the solutions. 2) Spray pyrolysis: The feed solution was sprayed in the form of droplets into a heated chamber at 650 °C to decompose the salts and form mixed metal oxide powders. The chamber volume was approximately 8.8 m 3 and the feed rate was 30 L / hr. 3) Washing: The mixed metal oxide powder was washed with water (25 wt. % solids) followed by filtration to reduce the chloride content. 4) Slurry formulation: A slurry was prepared by mixing the washed product from step 3) with a dispersant (Dolapix CA, Zschimmer & Schwarz, DE) to have 70 wt. % solids in water and 2 wt. % dispersant. 5) Wet bead mill: The prepared slurry was wet bead milled with a specific milling energy of 1300 kWh / T. The milling media was 1 mm diameter Y-stabilized ZrO 2 The beads were (YSZ). The D50 of the ground particles was 0.28 μm. 6) Spray drying: The milled slurry was spray dried through a two fluid nozzle with an inlet temperature of 170° C. and an outlet temperature of 100° C. The product of this step was a precursor powder labeled EX1.1.

[0047] EX1.1 powder has a density of 1.8g / cm for the total powder weight. 3 and a carbon content of 0.7% by weight.

[0048] The intermediate product after step 2 is 0.31 g / cm 3 The bulk density was 1.01 g / g.

[0049] Example 1.2: Heated mixed metal oxide EX1.1 was heated in a furnace at 500 °C for 5 h under oxygen atmosphere to produce EX1.2 powder with a D50 of 12.6 μm. A CS-SEM image of the EX1.2 particles is shown in Figure 1. The carbon content was 0.012 wt% based on the total weight of EX1.2.

[0050] Example 1.3: Mixed Metal-Containing Positive Electrode Active Material EX1.3 was obtained by solid-state reaction between a lithium source and a transition metal-based precursor, carried out as follows. 1) Mixing: Precursor powder EX1.2 and LiOH as lithium source were homogeneously mixed in an industrial blending device with a lithium to metal Me (Li / Me) ratio of 1.05 to obtain mixtures (Me=Ni, Mn, Co). 2) Heating: The mixture from step 1) was heated at 840° C. for 15 hours under oxygen atmosphere. The heated powder was crushed, classified and sieved to obtain the lithiated product labeled EX1.3.

[0051] Example 2.1: Nickel oxide The feed solution in step 1) is NiCl 2 EX2.1 was prepared according to the same method as EX1.1, except that it only contained 1.5 g / cm. The D50 of the ground particles was 0.25 μm. EX2.1 was prepared according to the same method as EX1.1, except that it only contained 1.5 g / cm. 3 The NiO precursor powder has a bulk density of

[0052] Example 2.2: Heated Nickel Oxide EX2.1 was heated in a furnace at 500° C. for 5 hours under oxygen atmosphere to produce EX2.2 powder with a D50 of 12.0 μm. The carbon content was 0.015 wt% based on the total weight of EX2.2.

[0053] Example 2.3: Nickel-containing positive electrode active material EX2.3 was obtained by solid-state reaction between a lithium source and a transition metal-based precursor, carried out as follows. 1) Mixing: Precursor powder EX2.2 and LiOH as lithium source are homogeneously mixed in an industrial blending device with a lithium to metal Me (Li / Me) ratio of 1.05 to obtain a mixture (Me=Ni, Mn, Co). 2) Heating: The mixture from step 1) was heated at 750° C. for 15 hours under oxygen atmosphere. The heated powder was crushed, classified and sieved to obtain the lithiated product labeled EX2.3.

Claims

1. 1. A method for preparing a precursor material for a Li-containing cathode active material for a battery, comprising: a spray pyrolysis step in which droplets of an aqueous solution are decomposed in a heated chamber to produce metal oxides; The metal oxide is a mixed metal oxide containing the element Ni and one or both of the elements Co and Mn, and the aqueous solution is a mixed solution of a salt of Ni and a salt of Co and / or Mn. Or the metal oxide is Ni oxide and the aqueous solution is a solution of a Ni salt; or the metal oxide is a Mn oxide and the aqueous solution is a solution of a Mn salt, The method further comprising a drying step of drying the aqueous slurry comprising the metal oxide to form the precursor material.

2. The method of claim 1 , wherein the drying step is a spray drying step in which the aqueous slurry is spray dried to form the precursor material.

3. 3. The method according to claim 1 or 2, wherein the metal oxide is a mixed metal oxide comprising the element Ni and one or both of the elements Co and Mn, and the aqueous solution is a mixed solution of a salt of Ni and a salt of Co and / or Mn.

4. A method according to any one of claims 1 to 3, characterized in that the salt or salts are chlorides.

5. A method according to any one of claims 1 to 4, wherein the precursor material is heated at a temperature of at least 300°C and at most 1000°C to produce a heat-treated precursor material.

6. 6. The method according to any one of claims 1 to 5, wherein the method comprises a washing step in which a mixture of the metal oxide and water is prepared in a ratio (weight of water) / (weight of metal oxide) of at least 0.1, and this mixture is filtered, centrifuged or decanted to recover the metal oxide, whereby the washing step is performed before the slurry preparation step.

7. The method according to any one of claims 1 to 6, wherein the method comprises a size reduction step in which the metal oxide undergoes particle size reduction, the size reduction step being carried out before the spray drying step.

8. 8. The method of claim 7, wherein the size reduction step is carried out on a water-wet metal oxide.

9. A method according to any one of claims 1 to 8, wherein the concentration of said metal oxide in said aqueous slurry is at least 30% by weight.

10. 10. The method of any one of claims 1 to 9, wherein the metal oxide particles in the aqueous slurry have a first particle size distribution as determined by laser diffraction with a median particle size D50, the first particle size distribution having a first D50 of up to 0.60 μm.

11. The precursor material comprises spherical particles and has a density of at least 1.0 g / cm 3 The method according to any one of claims 1 to 10, having a bulk density of

12. 12. The method of any one of claims 1 to 11, wherein the spherical particles have a second particle size distribution determined by laser diffraction, the second particle size distribution having a second D50 of at least 2 μm.

13. 13. The method of any one of claims 1 to 12, wherein the spherical particles have a second particle size distribution determined by laser diffraction, the second particle size distribution having a second D50 of up to 25 μm.

14. the metal oxide has a molar content y of Mn, a molar content z of Co, a molar content b of Ni, and a molar content a of A, where A is any metal element other than Li, Ni, Mn, and Co; 0.20≦b / (y+z+b+a)≦1.00, 0≦y / (y+z+b+a)≦0.80, 0≦z / (y+z+b+a)≦0.60, and 14. The method according to any one of claims 1 to 13, wherein 0≦a / (y+z+b+a)≦0.

10.

15. 15. The method according to any one of claims 1 to 14, wherein the metal oxide has a molar content y of Mn, a molar content z of Co, a molar content b of Ni and a molar content a of A, where A is any metallic element other than Li, Ni, Mn and Co, and 0.30≦b / (y+z+b+a)≦0.95 and 0.05≦(y+z+a) / (y+z+b+a)≦0.70.

Citation Information

Patent Citations

  • Manufacture of positive electrode material for lithium cell

    JP1998134811A

  • Positive electrode active material for lithium battery and battery using it for positive electrode

    JP1999185755A

  • Method for preparing a positive electrode material for a rechargeable lithium-ion battery

    JP2021517721A

  • Preparation method for Li(Ni-Co-Al)O2 / TiO2 composite cathode material

    CN104934572A

  • Methods for preparing positive electrode material for rechargeable lithium ion batteries

    WO2019185349A1